Optical glass and glass assembly or optical element made therefrom, and optical instrument
Optimized optical glass compositions with controlled ratios of specific cations enhance chemical stability and refractive index, addressing the issues of prior art glasses, achieving high performance and cost-effectiveness.
Patent Information
- Application Number
- JP2023113611
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-27
- Filing Date
- 2023-07-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-08-22
AI Technical Summary
Optical glasses in the prior art suffer from poor chemical stability, low refractive index, and high manufacturing costs, which affect the performance and lifespan of optical instruments.
Optical glass compositions optimized with specific ratios of Si, B, La, Gd, Y, Zr, Nb, Ti, Zn, W, and R cations, along with controlled ratios of (Nb + Ti + W)/Y, (La + Gd)/Y, (Si + B)/Y, and other components, achieving a refractive index of 1.99 to 2.01 and Abbe number of 28 to 31, with improved chemical stability and reduced alkali metal content.
The solution provides optical glasses with excellent chemical stability, high refractive index, and low production costs, ensuring grade 2 or higher acid and water resistance, and maintaining optical properties.
Smart Images

Figure 0007581435000001 
Figure 0007581435000002 
Figure 0007581435000003
Abstract
Description
[Technical field]
[0001] The present invention belongs to the technical field of glass, in particular optical glass, glass assemblies or optical elements made therefrom, and optical instruments. [Background technology]
[0002] The chemical stability of optical glass refers to the corrosion resistance of the polished surface of the optical component to various corrosive media that it comes into contact with during processing, storage, and use. If the chemical stability of the optical glass is poor, the corrosion resistance of the optical component will be reduced, and irregular dot-like or flaky black spots will be generated on the optical component, resulting in substandard performance and function of the optical instrument, which will seriously affect the service life of the optical instrument. In the prior art, the content of alkali metal oxides in the glass is mainly adjusted to improve its chemical stability. However, the optical glass obtained by this method has the problems of low refractive index and high manufacturing cost.
[0003] Therefore, providing an optical glass having excellent chemical stability, high refractive index, and low manufacturing cost has become a problem to be urgently solved by those skilled in the art. Summary of the Invention
[0004] A first object of the present invention is to provide an optical glass that solves the problems in the prior art, such as poor chemical stability, low refractive index, and high manufacturing cost.
[0005] A second object of the present invention is to provide a glass assembly made from optical glass.
[0006] A third object of the present invention is to provide an optical element made from optical glass.
[0007] A fourth object of the present invention is to provide an optical instrument containing the optical element.
[0008] The technical solutions of the present invention to achieve the objectives are as follows:
[0009] Optical glass contains 1 to 10% Si by mol%. 4+ and 25-40% B 3+ and 20-40% La 3+ and 0-15% Gd 3+ and Y greater than 0 but less than 10% 3+ and 1-10% Zr 4+ and 1-12% Nb 5+ and 8-25% Ti 4+ and 0-10% W 6+ It contains (Nb 5+ +Ti 4+ +W 6+ ) / Y 3+ is 26~46.
[0010] 0-8% Zn 2+ and 0-10% R 2+ and 0-10% R + It contains R 2+ Ba 2+ , Sr 2+ , Ca 2+ , and Mg 2+ and R + Li + , Na + , and K + One or more of the following:
[0011] Optical glass contains 1 to 10% Si by mol%. 4+ and 25-40% B 3+ and 20-40% La 3+ and 0-15% Gd 3+ and Y greater than 0 but less than 10% 3+ and 1-10% Zr 4+ and 1-12% Nb 5+ and 8-25% Ti 4+ and 0-8% Zn 2+ and 0-10% W 6+ and 0-10% R 2+ and 0-10% R + It contains (Nb 5++Ti 4+ +W 6+ ) / Y 3+ is 26 to 46, and R 2+ Ba 2+ , Sr 2+ , Ca 2+ , or Mg 2+ and R + Li + , Na + , K + One or more of the following:
[0012] In addition, all components meet one or more of the following six conditions:
[0013] 1)(Nb 5+ +Ti 4+ +W 6+ ) / Y 3+ is 26~40.
[0014] 2)(La 3+ +Gd 3+ ) / Y 3+ is 39 to 65.
[0015] 3)(Si 4+ +B 3+ ) / Y 3+ is 36 to 69.
[0016] 4)Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.02 to 0.4.
[0017] 5)(Si 4+ +Zr 4+ ) / (Nb 5+ +Ti 4+ ) is 0.06~2.
[0018] 6) La 3+ / (Si 4+ +Zr 4+ ) is 1.5 to 15.
[0019] In addition, Si 4+ 3-9% and / or B3+ 26-35% and / or La 3+ 25-35% and / or Gd 3+ is 0-10%, and / or Y 3+ 0.1 to 5% and / or Zr 4+ 1-8% and / or Nb 5+ 2-10% and / or Ti 4+ 10-20% and / or Zn 2+ 0.1 to 5% and / or W 6+ is 0-5%, and / or R 2+ is 0-5%, and / or R + is 0 to 5%, and R 2+ Ba 2+ , Sr 2+ , Ca 2+ , and Mg 2+ and R + Li + , Na + , and K + One or more of the following:
[0020] In addition, all components meet one or more of the following six conditions:
[0021] 1)(Nb 5+ +Ti 4+ +W 6+ ) / Y 3+ is 28~35.
[0022] 2)(La 3+ +Gd 3+ ) / Y 3+ is 40 to 60.
[0023] 3)(Si 4+ +B 3+ ) / Y 3+ is between 40 and 65.
[0024] 4)Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.05 to 0.3.
[0025] 5)(Si 4++Zr 4+ ) / (Nb 5+ +Ti 4+ ) is between 0.08 and 1.
[0026] 6) La 3+ / (Si 4+ +Zr 4+ ) is between 2 and 10.
[0027] In addition, Si 4+ is 4-8%, and / or B 3+ 27-32% and / or La 3+ 26-33% and / or Gd 3+ is 1-8%, and / or Y 3+ 0.3-3% and / or Zr 4+ 2-6% and / or Nb 5+ 3-8% and / or Ti 4+ 14-20% and / or Zn 2+ is 1-4%.
[0028] In addition, all components meet one or more of the following five conditions:
[0029] 1)(La 3+ +Gd 3+ ) / Y 3+ is 42-55.
[0030] 2)(Si 4+ +B 3+ ) / Y 3+ is 45-58.
[0031] 3)Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.08 to 0.21.
[0032] 4)(Si 4+ +Zr 4+ ) / (Nb 5+ +Ti 4+ ) is 0.1 to 0.52.
[0033] 5) La 3+ / (Si 4+ +Zr 4+ ) is 2.42~8.
[0034] In addition, W 6+ and / or R 2+ and / or R + Does not include.
[0035] Furthermore, the glass has a refractive index (nd) of 1.99-2.01 and an Abbe number (vd) of 28-31.
[0036] Furthermore, the acid resistance (D A ) is grade 2 or more, preferably grade 1, and the water resistance (D W ) is grade 2 or higher, preferably 1.
[0037] The glass assembly is made from the optical glass.
[0038] The optical element is made from the optical glass or the glass assembly.
[0039] The optical instrument contains the optical element.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] The present invention has the advantages of scientific design, rational formation, excellent chemical stability, high refractive index, and low production cost.
[0042] According to the present invention, an optical glass having excellent chemical stability, a refractive index of 1.99 to 2.01, and an Abbe number of 28 to 31 is obtained by reducing the content of alkali metals or by eliminating alkali metals and by using various components and (Nb 5+ +Ti 4+ +W 6+ ) / Y 3+ This is achieved by optimizing the ratio of β-methyl-1-pyridine, thereby satisfying the high requirements for chemical stability and refractive index of optical glass. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] In the specification, unless the content of all components is specifically stated, the content of cationic components is expressed as a percentage of the total moles of all cations, and the content of anionic components is expressed as a percentage of the total moles of all anions. Also, in the following specification, references below or above a given value include the given value.
[0044] It should be noted that the ionic valence of each component is not different from other ionic valences and is a standard value for convenience. The ionic valences of all components present in optical glass have other possibilities in addition to the standard value. For example, Si exists in the glass in the form of an ionic valence of 4, and therefore, as a representative example in this specification, "Si 4+ ", however, Si may have other ionic valence states and are within the scope of the present invention.
[0045] B of the present invention 3+ The oxide is a glass network forming component, which is a component necessary for forming glass, and has the effect of maintaining stability and meltability, lowering the liquidus temperature, and realizing low dispersion of the glass. 3+ If the content is lower than 25%, the crystallization stability of the glass is low. 3+ If the content is higher than 40%, the liquidus temperature of the glass increases and the chemical stability decreases, so the range of the content in the present invention is defined as 25 to 40%, preferably 26 to 35%, and more preferably 27 to 32%.
[0046] Si in the present invention 4+ The oxide is a glass network forming component and can be introduced to improve the crystallization resistance and high temperature viscosity of the glass. If the content exceeds 10%, the glass conversion temperature increases, the glass melting property decreases, and the glass chemical stability tends to deteriorate. Therefore, the content range in the present invention is defined as 1-10%, preferably 3-9%, and more preferably 4-8%.
[0047] The rare earth ion oxide of the present invention fills mainly the network voids of the glass as a network modifying oxide, so that the glass structure becomes more compact. 3+ , Gd 3+ , and Y 3+ Contains:
[0048] The La of the present invention 3+ can improve the chemical stability, mechanical strength, and refractive index of glass, and reduce the partial dispersion ratio of glass. However, if its content exceeds 40%, the crystallization resistance of glass is obviously reduced. If its content is less than 20%, the chemical stability of glass is reduced. Therefore, the range of its content in the present invention is defined as 20 to 40%, preferably 25 to 35%, and more preferably 26 to 33%.
[0049] The present invention relates to Gd 3+ Gd can improve the refractive index of glass, and has the effect of improving the crystallization resistance and chemical stability. However, the cost of its raw material is high, and if its content is higher than 15%, the devitrification resistance of glass decreases and the density of glass increases. 3+ The content is defined as 0 to 15%, preferably 0 to 10%, and more preferably 1 to 8%.
[0050] The Y of the present invention 3+ Y can improve the melting property of glass, and can improve the crystallization resistance and chemical stability of glass. If its content is higher than 10%, the chemical stability and crystallization resistance of glass will decrease. Therefore, the Y in the present invention 3+ The upper limit of the range of the content is 10%, preferably 8%, more preferably 5%, more preferably 3%, and even more preferably 1%. 3+ The lower limit of the content is preferably greater than 0, more preferably 0.1%, more preferably 0.3%, and even more preferably 0.5%.
[0051] After much research, the inventors discovered that La 3+, Gd 3+ , and Y 3+ It was discovered that the coexistence of (La) has the effect of improving the crystallization resistance and chemical stability of glass. 3+ +Gd 3+ ) / Y 3+ When the value of La is 39 to 65, preferably 40 to 60, the glass has excellent chemical stability. 3+ +Gd 3+ ) / Y 3+ When the viscosity is 42 to 55, the acid resistance and water resistance of the glass can reach grade 2 or more, preferably grade 1.
[0052] According to the research findings, the inventors 4+ +B 3+ The total amount of Y 3+ It has been found that a proportional relationship between (Si 4+ +B 3+ ) / Y 3+ When the value is in the range of 36 to 69, the glass obtains the necessary optical properties and has excellent crystallization resistance. The range is preferably 40 to 65, and more preferably 45 to 58, so that crystallization does not easily occur during manufacturing and pressing.
[0053] According to the present invention, Si 4+ It has been found that when there is a proportional relationship between the amount of Si and the total amount of rare earth ions, a glass with good crystallization resistance can be obtained. 4+ / (La 3+ +Gd 3+ +Y 3+ If the value of ) is greater than 0.4, the crystallization resistance is reduced. If the value is less than 0.02, the chemical stability is deteriorated. Therefore, Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is defined as being in the range of 0.02 to 0.4, preferably 0.05 to 0.3, and more preferably 0.08 to 0.21.
[0054] According to the present invention, Zn 2+has the effect of improving the meltability, chemical stability and crystallization resistance of glass, and lowering the glass conversion temperature. 2+ If the content is higher than 8%, its crystallization property is deteriorated, the dispersion is increased, and the refractive index requirement cannot be met. 2+ The content range is defined as 0 to 8%, preferably 0.1 to 5%, and more preferably 1 to 4%.
[0055] According to the present invention, Zr 4+ Zr can improve the chemical stability of glass. 4+ When the content of Zn is 1-10%, the glass has a suitable refractive index and thermal expansion coefficient, and excellent chemical stability and crystallization resistance. When the content is higher than 10%, the liquidus temperature of the glass increases and the glass transmittance decreases. When the content is less than 1%, the crystallization resistance decreases and the refractive index requirement cannot be met. According to the present invention, Zn 2+ The content range is defined as 1 to 10%, preferably 1 to 8%, and more preferably 2 to 6%.
[0056] After much research, the inventors discovered that Si 4+ and Zr 4+ The total amount of La 3+ It was found that the proportional relationship between La and the chemical stability of glass can be improved. 3+ / (Si 4+ +Zr 4+ If the value of La is less than 1.5, the chemical stability of the glass is deteriorated. If the value exceeds 15, the crystallization resistance is deteriorated and the refractive index requirement cannot be met. 3+ / (Si 4+ +Zr 4+ ) is preferably 2 to 10, and more preferably 2.42 to 8.
[0057] According to the present invention, Nb 5+Nb has the effect of improving the refractive index of glass, increasing the dispersion, and increasing the chemical stability of glass. If its content is higher than 12%, the short-wave transmittance of the glass in the visible range is reduced, and the glass is obviously colored. If its content is less than 1%, the refractive index requirement is not met, and the chemical stability is reduced. According to the present invention, Nb 5+ The content range is defined as 1 to 12%, preferably 2 to 10%, and more preferably 3 to 8%.
[0058] According to the present invention, Ti 4+ Ti participates in the formation of a glass network and has the effect of improving the refractive index and chemical stability of the glass. 4+ When the content of Ti is 8-25%, the glass has good chemical stability and can improve the refractive index. When the content is higher than 25%, the short-wave transmittance of the glass in the visible range is reduced, and the glass is obviously colored; when the content is lower than 8%, the refractive index requirement cannot be met, and the chemical stability is reduced. According to the present invention, Ti 4+ The content range is defined as 8 to 25%, preferably 10 to 20%, and more preferably 14 to 20%.
[0059] After much research, the inventors discovered that Si 4+ and Zr 4+ The total amount of Nb 5+ and Ti 4+ It was found that the proportional relationship between the total amount of (Si 4+ +Zr 4+ ) / (Nb 5+ +Ti 4+ ) ratio is in the range of 0.06 to 2, (Si 4+ +Zr 4+ ) / (Nb 5+ +Ti 4+ It has been discovered that when the ratio of (a) to (b) is preferably 0.08 to 1, and more preferably 0.1 to 0.52, the glass forming stability and crystallization resistance are excellent.
[0060] According to the present invention, W6+ has the effect of improving the refractive index of glass. However, if its content is higher than 10%, the chemical stability, transmittance, and crystallization resistance of the glass are all deteriorated. Therefore, its content range is 0 to 10%, preferably 0 to 5%, and more preferably it is not included.
[0061] After extensive research, the inventors found that Nb 5+ , Ti 4+ , and W 6+ The total amount of Y 3+ It was found that when there is a proportional relationship between Nb 5+ +Ti 4+ +W 6+ ) / Y 3+ If the ratio is less than 26, the crystallization resistance is reduced. If the ratio is more than 46, the chemical stability is reduced. Therefore, the range of the ratio is defined as 26 to 46, preferably 26 to 40, and more preferably 28 to 35.
[0062] According to the present invention, Li + It can increase the melting property of glass and reduce the conversion temperature. If its content is higher than 10%, the refractive index of glass cannot reach the design requirement, so its upper limit is controlled at 10%.
[0063] According to the present invention, Na + and K + Both have the effect of improving glass melting property. + and K + If the content is greater than 10%, the glass refractive index cannot reach the requirement. Therefore, Na + and K + The content is defined as 10% or less of each.
[0064] According to the present invention, Li + , Na + , and K +Li is an alkali metal ion, which can adjust the optical data of the glass, improve the melting effect of the glass, and make the glass have a low conversion temperature. + +Na + +K + When the total amount of Li is less than 10%, the glass has high chemical stability and can meet the refractive index requirements. When the value exceeds 10%, the crystallization resistance of the glass decreases. Therefore, Li + +Na + +K + is defined as 0 to 10%, preferably 0 to 5%, and more preferably not included.
[0065] According to the present invention, Ba 2+ It has the effect of increasing the refractive index of glass and improving the transmittance of glass. If its content is more than 10%, both the chemical stability and crystallization resistance of glass deteriorate. Therefore, its content range is 0 to 10%, preferably 0 to 5%, and more preferably it is not included.
[0066] According to the present invention, Sr 2+ can effectively adjust the refractive index and Abbe number of the glass. In addition, its raw material cost is high. If its content is more than 10%, both the chemical stability and crystallization resistance of the glass will deteriorate. Therefore, its content range is 0-10%, preferably 0-5%, and more preferably it is not included.
[0067] According to the present invention, Ca 2+ can reduce the Abbe number and specific gravity of the glass. However, if its content is more than 10%, the crystallization resistance of the glass decreases. Therefore, its content range is 0 to 10%, preferably 0 to 5%, and more preferably it is not included.
[0068] According to the present invention, Mg 2+can improve the chemical stability of glass. However, if its content is too high, the refractive index of the glass will not meet the requirements, and the crystallization characteristics and chemical stability will be reduced. Therefore, its content range is 0-10%, preferably 0-5%, and more preferably it is not included.
[0069] According to the present invention, Ba 2+ , Sr 2+ , Ca 2+ , and Mg 2+ Ba is an alkaline earth metal ion that can adjust the refractive index of the glass and reduce the high-temperature viscosity of the glass. 2+ , Sr 2+ , Ca 2+ , and Mg 2+ The total amount of (Ba 2+ +Sr 2+ +Ca 2+ +Mg 2+ When the value of Ba is greater than 10%, the chemical stability and crystallization resistance of the glass are obviously deteriorated. 2+ +Sr 2+ +Ca 2+ +Mg 2+ ) is defined to be 0-10%, preferably 0-5%, and more preferably not included.
[0070] According to the present invention, the main anion is O 2- Without affecting the properties of the optical glass provided by the present invention, F - and Cl - Other anions such as O may be present to some extent. 2- The content is 95% or more, preferably 98% or more, and more preferably 100%.
[0071] The refractive index (nd) of the optical glass provided by the present invention is in the range of 1.99 to 2.01. The Abbe number (vd) of the glass provided by the present invention is in the range of 28 to 31, preferably in the range of 28 to 30.
[0072] The method for analyzing the crystallization resistance of glass provided by the present invention includes the following steps: cut a sample glass into a specification of 20×20×10 mm, put it into a muffle furnace at a temperature of Tg+230℃ for 30 minutes, take it out and put it into a warm cotton for annealing, and visually observe the surface crystallization after cooling.
[0073] According to the present invention, the chemical stability of the glass provided by the present invention is water resistance D W and acid resistance D A The water resistance (D W ) is grade 2 or higher, preferably grade 1. A ) is grade 2 or higher, preferably grade 1.
[0074] The following paragraphs further describe the present invention in combination with the embodiments. The methods provided by the present invention include, but are not limited to, the following embodiments.
[0075] Example 1 The embodiment provides a method for producing optical glass provided by the present invention. The various optical glasses of Glass No. 1 to 33 are obtained by using carbonate, nitrate, hydroxide, oxide, and boric acid as raw materials, proportionally weighing all raw materials according to the composition of the optical glass, uniformly mixing them to obtain a mixed raw material, putting the mixed raw material into a platinum crucible, heating it to 1,250 to 1,450°C, clarifying it, and stirring it for 3 to 5 hours to obtain a uniform molten glass, and then pouring the molten glass into a preheated mold and finally keeping it at 600 to 700°C for 2 to 4 hours.
[0076] Example 2 The embodiments provide a method for analyzing the properties of the optical glass provided by the present invention, in particular:
[0077] The refractive index (nd) is analyzed according to the method specified in GB / T7962.1-2010.
[0078] The Abbe number (vd) is analyzed according to the method specified in GB / T7962.1-2010.
[0079] The test method for the crystallization resistance performance of glass includes the following steps: Cut the sample glass to the specifications of 20x20x10mm, put it into a muffle furnace at a temperature of Tg+230℃, and keep it warm for 30 minutes. After taking it out, put it into a warm cotton for annealing, and visually observe the surface crystallization after cooling. "A" indicates no obvious crystallization, and "B" indicates obvious crystallization.
[0080] Water resistance (D W ) is analyzed according to the test methods specified in GB / T17129.
[0081] Acid resistance (D A ) is analyzed according to the test methods specified in GB / T17129.
[0082] Example 3 The embodiments provide compositions and properties of optical glasses, the details of which are shown in the table below. [Table 1] [Table 2] [Table 3] [Table 4]
[0083] Example 4 The embodiment provides a method for producing glass assembly members using the optical glass provided by the present invention. The optical glass in Tables 1 to 4 is cut to a predetermined size, and a release agent of boron nitride powder is uniformly applied to the surface, and then heated and softened, and press-molded into assembly members for various lenses and prisms, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0084] Example 5 An embodiment provides a method of making an optical element using the glass assembly provided by the present invention.
[0085] The optical assemblies produced by the method of embodiment 4 are annealed to reduce and fine-tune the internal distortion of the glass, so that the optical properties, such as the refractive index, are set to the desired values. Each assembly is then ground and polished to form various lenses and prisms, such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. An anti-reflective film may be coated on the surface of the resulting optical element.
[0086] Example 6 Optical Instrument Embodiments
[0087] The optical components or optical elements are formed by optical design or by one or more optical elements, which may be used in imaging devices, sensors, microscopes, medical technology, digital projection, communication, optical communication technology / information transmission, optics / illumination in the automotive field, photolithography, excimer lasers, wafers, computer chips, integrated circuits, and electronic devices containing such circuits and chips.
[0088] The embodiment is merely one of the preferred embodiments of the present invention and should not be used to limit the protection scope of the present invention. However, all modifications or refinements that have no substantial meaning based on the main design idea and spirit of the present invention should be included in the protection scope of the present invention if they solve the technical problems consistent with one of the present invention.
Claims
1. 1 to 10% Si by mol% 4+ and 25-35% B 3+ and 20-40% La 3+ and 0-15% Gd 3+ and Y is greater than 0 but less than 10% 3+ and 1 to 10% Zr 4+ and 1 to 12% Nb 5+ and 8 to 25% Ti 4+ And 0 to 10% W 6+ and (Si 4+ +B 3+ ) / Y 3+ is 36 to 66.67, and (Nb 5+ + Ti 4+ +W 6+ ) / Y 3+ The optical glass is characterized in that
2. In addition, 0 to 8% Zn 2+ and 0 to 10% R 2+ and 0 to 10% R + and R 2+ Ba 2+ , Sr 2+ , Ca 2+ , or Mg 2+ and R + Li + , Na + , K + 2. The optical glass according to claim 1, characterized in that the optical glass is one or more of the following:
3. 1 to 10% Si by mol% 4+ and 25-35% B 3+ and 20-40% La 3+ and 0-15% Gd 3+ and Y is greater than 0 but less than 10% 3+ and 1 to 10% Zr 4+ and 1 to 12% Nb 5+ and 8 to 25% Ti 4+ and 0-8% Zn 2+ And 0 to 10% W 6+ and 0 to 10% R 2+ and 0 to 10% R + and (Si 4+ +B 3+ ) / Y 3+ is 36 to 66.67; (Nb 5+ + Ti 4+ +W 6+ ) / Y 3+ is 26 to 46, and R 2+ Ba 2+ , Sr 2+ , Ca 2+ , Mg 2+ and R + Li + , Na + , K + The optical glass is characterized by being one or more of the above.
4. The optical glass according to any one of claims 1 to 3, characterized in that all of the components satisfy one or more of the following six conditions: 1) (Nb 5+ + Ti 4+ +W 6+ ) / Y 3+ is 26 to 40, 2) (La 3+ +Gd 3+ ) / Y 3+ is 39 to 65, 3) (Si 4+ +B 3+ ) / Y 3+ is 36.02 to 66.67, 4) Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.02 to 0.4; 5) (Si 4+ + Zr 4+ ) / (Nb 5+ + Ti 4+ ) is 0.06 to 2; 6) La 3+ / (Si 4+ + Zr 4+ ) is 1.5 to 15.
5. S 4+ 3 to 9%, and / or B 3+ 26 to 35%, and / or La 3+ 25-35% and / or Gd 3+ is 0 to 10%, and / or Y 3+ and / or Zr 4+ and / or Nb 5+ and / or Ti 4+ and / or Zn 2+ and / or W 6+ is 0 to 5%, and / or R 2+ is 0 to 5%, and / or R + is 0 to 5%, and R 2+ Ba 2+ , Sr 2+ , Ca 2+ , Mg 2+ and R + Li + , Na + , K + 4. The optical glass according to claim 1, wherein the optical glass has one or more of the following properties:
6. The optical glass according to any one of claims 1 to 3, characterized in that all of the components satisfy one or more of the following six conditions: 1) (Nb 5+ + Ti 4+ +W 6+ ) / Y 3+ is 28 to 35, 2) (La 3+ +Gd 3+ ) / Y 3+ is 40 to 60, 3) (Si 4+ +B 3+ ) / Y 3+ is 40 to 65, 4) Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.05 to 0.3; 5) (Si 4+ + Zr 4+ ) / (Nb 5+ + Ti 4+ ) is 0.08 to 1; 6) La 3+ / (Si 4+ + Zr 4+ ) is 2 to 10.
7. S 4+ is 4 to 8%, and / or B 3+ 27 to 32%, and / or La 3+ 26-33% and / or Gd 3+ is 1 to 8%, and / or Y 3+ and / or Zr 4+ and / or Nb 5+ and / or Ti 4+ and / or Zn 2+ The optical glass according to any one of claims 1 to 3, characterized in that
8. The optical glass according to any one of claims 1 to 3, characterized in that all of the components satisfy one or more of the following five conditions: 1) (La 3+ +Gd 3+ ) / Y 3+ is 42 to 55, 2) (Si 4+ +B 3+ ) / Y 3+ is 45 to 58, 3) Si 4+ / (La 3+ +Gd 3+ +Y 3+ ) is 0.08 to 0.21; 4) (Si 4+ + Zr 4+ ) / (Nb 5+ + Ti 4+ ) is 0.1 to 0.52; 5) La 3+ / (Si 4+ + Zr 4+ ) is 2.42 to 8.
9. W 6+ and / or R 2+ and / or R + 4. The optical glass according to claim 1, which is free of
10. 4. The optical glass according to claim 1, wherein the refractive index (nd) of the glass is 1.99-2.01 and the Abbe number (vd) is 28-31.
11. The acid resistance of the glass (D A ) is grade 2 or more, and the water resistance (D W 4. The optical glass according to claim 1, wherein the optical fiber has a refractive index of 2 or higher.
12. The optical glass of claim 11, wherein the acid resistance (D A ) of said glass is Class 1 and the water resistance (D W ) of said glass is Class 1.
13. A glass assembly member, characterized in that it is made from the optical glass according to any one of claims 1 to 12.
14. An optical element, characterized in that it is produced from the optical glass according to any one of claims 1 to 12 or the glass assembly according to claim 13.
15. An optical instrument comprising the optical element according to claim 14.
Citation Information
Patent Citations
Optical glass
CN102745894A
Optical glass
JP2010030879A
Optical glass, preform, and optical element
JP2012162448A
Optical glass
JP2015074572A
Optical glass, and optical element and optical device prepared with optical glass
JP2016117598A