Ceramic circuit board and semiconductor device using same

The ceramic circuit board's innovative design with an inclined metal plate and controlled bonding layer properties addresses resin peeling issues, enhancing thermal cycle resistance and adhesion to ensure semiconductor device reliability.

JP7581476B2Active Publication Date: 2024-11-12NITERRA MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023500804
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-17
Filing Date
2022-02-10
Publication Date
2024-11-12
Estimated Expiration
2042-02-10

AI Technical Summary

Technical Problem

Resin peeling occurs at the contact surface between the mold resin and the ceramic circuit board as semiconductor devices generate increasing heat, compromising the reliability of the semiconductor device.

Method used

A ceramic circuit board design with specific structural and material properties, including an inclined metal plate side surface, a protruding bonding layer, controlled Vickers hardness ratio, and a defined angle and area ratio, enhances the bonding layer's stress relaxation and adhesion, preventing resin peeling.

Benefits of technology

The design improves the thermal cycle resistance and resin adhesion, ensuring the reliability of semiconductor devices by preventing resin peeling and maintaining structural integrity under thermal stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581476000005
    Figure 0007581476000005
  • Figure 0007581476000006
    Figure 0007581476000006
  • Figure 0007581476000007
    Figure 0007581476000007
Patent Text Reader

Abstract

The present invention is a ceramic circuit board obtained by joining a ceramic board and a metal plate with a joining layer therebetween, and when the ceramic circuit board is observed in a cross-section from the thickness direction and lateral direction of the ceramic circuit board, a side surface of the metal plate has an inclined shape, and the joining layer has a joining-layer protruding section which protrudes 20-150[µm] from an edge where the joining layer is in contact with the side surface of the metal plate. Furthermore, the shape and Vickers hardness of the side surface of the metal plate is controlled. The ceramic board is preferably a silicon nitride board.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiments described below generally relate to a ceramic circuit board and a semiconductor device using the same. [Background technology]

[0002] Ceramic circuit boards are used as circuit boards on which semiconductor elements are mounted. Examples of ceramic boards include alumina boards, aluminium nitride boards, and silicon nitride boards. Copper and aluminum boards are used as metal plates bonded to ceramic boards. As semiconductor elements become more powerful, their junction temperatures are rising. For this reason, there is a demand for ceramic circuit boards to have improved TCT characteristics (thermal cycle resistance characteristics).

[0003] For example, International Publication No. 2017 / 056360 (Patent Document 1) describes providing a gradient structure on the side surface of a copper plate and optimizing the size of the protruding portion of the bonding layer. In Patent Document 1, excellent TCT characteristics are obtained. In particular, it is considered preferable to optimize the size of the protruding portion of the bonding layer. In Patent Document 1, excellent TCT characteristics are obtained.

[0004] Ceramic circuit boards become semiconductor devices when semiconductor elements are mounted on a metal plate. The metal plate on the side that does not have semiconductor elements mounted is joined to a heat sink base. Wire bonding and leads are also attached as necessary. The semiconductor elements are then molded with resin to protect them. Methods such as potting and transfer molding are used for resin molding. The molded resin is formed by solidifying the resin, and serves to protect the semiconductor elements. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2017 / 056360 Summary of the Invention [Problem to be solved by the invention]

[0006] When resin was molded into a semiconductor device using the ceramic circuit board of Patent Document 1, the phenomenon of resin peeling was observed in some cases. As the performance of semiconductor elements improves, the amount of heat generated increases. It was found that this makes it easier for resin peeling to occur at the contact surface between the molding resin and the ceramic circuit board.

[0007] The present invention is intended to address such problems, and to provide a ceramic circuit board capable of suppressing peeling of the molding resin. [Means for solving the problem]

[0008] A ceramic circuit board according to an embodiment, in which a ceramic substrate and a metal plate are bonded together via a bonding layer, has the following characteristics when the ceramic circuit board is observed in a cross section consisting of a thickness direction and a lateral direction of the ceramic circuit board. (1) The side of the metal plate has a sloped shape. (2) The bonding layer has a bonding layer protruding portion that protrudes by 20 μm or more and 150 μm or less from the edge where the bonding layer meets the side of the metal plate. (3) When the end portion is defined as point A, the side of the metal plate 20 μm inward from point A is defined as point B, and the surface of the protruding portion of the bonding layer 20 μm outward from point A is defined as point C, the angle ∠BAC is 110° or greater. (4) The average Vickers hardness of ten points in the region between a lateral line passing through point B and the interface of the metal plate and the bonding layer is Hm. (5) If the average Vickers hardness of 10 points in the bonding layer is Hb, then 300>Hm>Hb and Hm / Hb<2. (6) The ratio R of the area in which components of the bonding layer other than the components of the metal plate exist within the region is 5% or more and 20% or less.

[0009] That is, it is preferable that the requirements of the above features (1) to (6) are satisfied in a cross section consisting of the thickness direction and each side direction of the ceramic circuit board (when the planar shape of the ceramic circuit board is rectangular, each side direction is each of two perpendicular side directions). When a metal plate is bonded only to the front surface of the ceramic circuit board, only the metal plate and bonding layer on the front surface need to satisfy the requirements of the above features (1) to (6). When metal plates are bonded to both sides of the ceramic circuit board, the metal plates and bonding layers on both sides need to satisfy the requirements of the above features (1) to (6). [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a cross-sectional view taken along line II of a first example of a ceramic circuit board according to an embodiment. [Diagram 2] FIG. 2A is a side view showing an outline of a ceramic circuit board according to an embodiment, and FIG. 2B is a top view showing an outline of a ceramic circuit board according to an embodiment. [Diagram 3] 1 is a side view showing an example of a semiconductor device according to an embodiment; [Figure 4] FIG. 4 is a side view for explaining measurement of voltage resistance characteristics. [Diagram 5] FIG. 2 is a cross-sectional view showing a second example of a ceramic circuit board according to an embodiment. [Figure 6] FIG. 2 is a cross-sectional view showing a third example of a ceramic circuit board according to an embodiment. Embodiment

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of a ceramic circuit board and a semiconductor device using the same will be described in detail with reference to the drawings.

[0012] A ceramic circuit board according to an embodiment, in which a ceramic substrate and a metal plate are bonded together via a bonding layer, has the following characteristics when the ceramic circuit board is observed in a cross section consisting of a thickness direction and a lateral direction of the ceramic circuit board. (1) The side of the metal plate has a sloped shape. (2) The bonding layer has a bonding layer protruding portion that protrudes by 20 μm or more and 150 μm or less from the edge where the bonding layer meets the side of the metal plate. (3) When the end portion is defined as point A, the side of the metal plate 20 μm inward from point A is defined as point B, and the surface of the protruding portion of the bonding layer 20 μm outward from point A is defined as point C, the angle ∠BAC is 110° or greater. (4) The average Vickers hardness of ten points in the region between a lateral line passing through point B and the interface of the metal plate and the bonding layer is Hm. (5) If the average Vickers hardness of 10 points in the bonding layer is Hb, then 300>Hm>Hb and Hm / Hb<2. (6) The ratio R of the area in which components of the bonding layer other than the components of the metal plate exist within the region is 5% or more and 20% or less.

[0013] That is, it is preferable that the requirements of the above features (1) to (6) are satisfied in a cross section consisting of the thickness direction and each side direction of the ceramic circuit board (when the planar shape of the ceramic circuit board is rectangular, each side direction is each of two perpendicular side directions). When a metal plate is bonded only to the front surface of the ceramic circuit board, only the metal plate and bonding layer on the front surface need to satisfy the requirements of the above features (1) to (6). When metal plates are bonded to both sides of the ceramic circuit board, the metal plates and bonding layers on both sides need to satisfy the requirements of the above features (1) to (6).

[0014] 1, 2(A) and 2(B) are cross-sectional views showing the details of the ceramic circuit board according to the embodiment. In the figures, 1 is a ceramic circuit board, 2 is a ceramic substrate, 3 is a metal plate, 4 is a bonding layer, 5 is a region M and 6 is a metal plate. Note that although FIG. 1 is a cross-sectional view of FIG. 2(B) along line II, the bonding layer 4 and the back metal plate 6 on the back side of the ceramic circuit substrate 2 are omitted in FIG. 1. Also, the lateral directions of the ceramic substrate 2 are defined as the x-axis direction and the y-axis direction, and the depth direction of the ceramic substrate 2 is defined as the z-axis direction.

[0015] FIG. 1 illustrates an example of the side shape of the metal plate 3 on the front side of the ceramic circuit board 1 (the metal plate 6 on the rear side is not illustrated). Also, FIGS. 2(A) and (B) show the structure of the ceramic circuit board 1 having two metal plates 3 on the front side and one metal plate 6 on the rear side. The metal plate 3 on the front side is sometimes called the front metal plate because it is used as a circuit. Also, the metal plate 6 on the rear side is sometimes called the rear metal plate because it is used as a heat sink. The ceramic circuit board 1 according to the embodiment is not limited to such a structure. For example, there may be three or more front metal plates 3. Also, the rear metal plate 6 may have a circuit shape. Hereinafter, a case where the metal plates 3 and 6 are bonded to both sides of the ceramic circuit board 1 will be described as an example.

[0016] First, the ceramic substrate 2 is preferably one selected from a silicon nitride substrate, an aluminum nitride substrate, an alumina substrate, and an aluminium nitride substrate. The aluminium nitride substrate is a ceramic sintered body made of a mixture of alumina and zirconia.

[0017] When the ceramic substrate 2 is a silicon nitride substrate, the silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more. The silicon nitride substrate also preferably has a thermal conductivity of 80 W / m·K or more. By increasing the strength of the silicon nitride substrate, the substrate thickness can be reduced. For this reason, the silicon nitride substrate preferably has a three-point bending strength of 600 MPa or more, and more preferably 700 MPa or more. The silicon nitride substrate can be reduced in thickness to 0.40 mm or less, and even 0.30 mm or less.

[0018] Furthermore, when the ceramic substrate 2 is an aluminum nitride substrate, the three-point bending strength of the aluminum nitride substrate is about 300 to 450 MPa. On the other hand, the thermal conductivity of the aluminum nitride substrate is 160 W / m K or more. Since the aluminum nitride substrate has low strength, the substrate thickness is preferably 0.60 mm or more.

[0019] When the ceramic substrate 2 is an aluminum oxide substrate, the three-point bending strength of the aluminum oxide substrate is about 300 to 450 MPa, but it is inexpensive.When the ceramic substrate 2 is an alumina substrate, the three-point bending strength of the alumina substrate is high at about 550 MPa, but its thermal conductivity is about 30 to 50 W / m K.

[0020] It is preferable that the ceramic substrate 2 is a silicon nitride substrate. The silicon nitride substrate has high strength and can be made thin.

[0021] The metal plates 3 and 6 may be one or more selected from a copper plate, a copper alloy plate, an aluminum plate, and an aluminum alloy plate. The metal plates 3 and 6 are preferably copper plates. The metal plates 3 and 6 are preferably oxygen-free copper plates. As shown in JIS-H-3100, oxygen-free copper has a copper purity of 99.96 mass% or more. The thermal conductivity of copper is about 400 W / m·K, and the thermal conductivity of aluminum is about 240 W / m·K. Copper has a higher thermal conductivity than aluminum, so heat dissipation is improved. The aluminum plate is preferably pure aluminum. Pure aluminum is shown in JIS-H-4000. The ISO corresponding to JIS-H-3100 is ISO1337 (1980), etc. The ISO corresponding to JIS-H-4000 is ISO209-1 (1989), etc.

[0022] Moreover, the thickness of the metal plates 3, 6 is preferably 0.3 [mm] or more. By making the metal plates 3, 6 thicker, the heat dissipation can be improved. Also, the current carrying capacity can be increased. For this reason, the thickness of the metal plates 3, 6 is preferably 0.3 [mm] or more, and further preferably 0.6 [mm] or more. Furthermore, the upper limit of the thickness of the metal plates 3, 6 is not particularly limited, but is preferably 5 [mm] or less. If it exceeds 5 [mm], it may be difficult to control the inclined shape of the side surface of the metal plates 3, 6. Furthermore, from the viewpoint of heat dissipation, it is preferable to use a copper plate having a thickness of 0.3 [mm] or more as the metal plates 3, 6. Furthermore, it is preferable that both the front copper plate as the front metal plate 3 and the back copper plate as the back metal plate 6 have a thickness of 0.3 [mm] or more.

[0023] The ceramic substrate 2, the front metal plate 3, and the back metal plate 6 are each bonded via a bonding layer 4. The bonding layer 4 has a bonding layer protruding portion 4a that protrudes from an end portion (a dot in the cross-sectional view shown in FIG. 1) where the side surface of the front metal plate 3 and the bonding layer 4 are in contact.

[0024] The protruding length of the bonding layer protruding portion 4a (hereinafter simply referred to as "length") is 20 [μm] or more and 150 [μm] or less. The length of the bonding layer protruding portion 4a is measured using an arbitrary cross section of the ceramic circuit board 1. The cross section is observed with a SEM (scanning electron microscope). The magnification of the SEM photograph is 500 times. The length of the bonding layer protruding portion 4a is obtained using the SEM photograph. The length of the bonding layer protruding portion 4a is obtained based on the contact point between the bonding layer 4 and the front metal plate 3 and the contact point between the end of the bonding layer protruding portion 4a and the ceramic substrate 2. The same applies to the back metal plate 6 as to the front metal plate 3. The contact point between the bonding layer 4 and the front metal plate 3 is set as reference 1, and the contact point between the end of the bonding layer protruding portion 4a and the ceramic substrate 2 is set as reference 2. A vertical line (a line extending in the z-axis direction) is drawn from reference 1 and reference 2, and the horizontal distance between the vertical lines (the distance in the x-axis direction or the y-axis direction) is the length of the bonding layer protruding portion 4a. Even if the side surface of the front metal plate 3 has a metal coating, the measurement is based on the side surface of the front metal plate 3 itself. The metal coating can be, for example, metal plating.

[0025] If the length of the bonding layer protrusion 4a is 20 μm or more and 150 μm or less, the TCT characteristics can be improved. Part 4a If the length is less than 20 μm, the stress relaxation effect at the joint end is insufficient. If the length is longer than 150 μm, no further effect can be obtained. If the joint layer protrusion 4a is too long, it may be difficult to narrow the pitch between adjacent front metal sheets 3 (or back metal sheets 6). Therefore, the length of the joint layer protrusion 4a is preferably 20 μm or more and 150 μm or less, and more preferably 20 μm or more and 80 μm or less. More preferably, it is 30 μm or more and 60 μm or less. The thickness of the bonding layer protruding portion 4a may be uniform, or may be gradually thinner toward the tip.

[0026] In addition, when the end portion (a point in the cross-sectional view shown in Figure 1) where the side of the front metal plate 3 and the bonding layer 4 contact is defined as point A, the side of the front metal plate 3 20 μm away in the x-axis direction inward from point A (i.e., in the positive x-axis direction shown in Figure 1) is defined as point B, and the contact point on the surface of the bonding layer protruding portion 4a 20 μm away in the x-axis direction inward from point A (i.e., in the negative x-axis direction shown in Figure 1) is defined as point C, the angle ∠BAC is 110° or more.

[0027] The measurements of points A, B, and C are made using a cross-sectional SEM photograph. In the SEM photograph, the point where the side of the front metal plate 3 and the bonding layer 4 meet is defined as point A. The side of the front metal plate 3, which is 20 μm inward from point A in the x-axis direction, is defined as point B. Also, the contact point of the top surface of the protruding portion 4a of the bonding layer, which is 20 μm outward from point A in the x-axis direction, is defined as point C. Points B and A are connected by a straight line. Similarly, points A and C are connected by a straight line. The angle formed by each straight line is defined as angle ∠BAC. The angle formed by the straight line BA, which connects points B and A, and the straight line AC, which connects points A and C, is the angle ∠BAC. Also, the angle ∠BAC refers to the angle made on the upper side of Figure 1. By making the angle ∠BAC 110° or more, the stress on the bonding layer protruding portion 4a can be reduced. This means that there is a sufficient angle in a small region of 20μm from the contact point A. In addition, when the resin is molded, the adhesion between the side surface of the front metal plate 3 and the molded resin 8 can be improved.

[0028] If the angle ∠BAC is less than 110°, the angle of the metal plate side is steep. Also, if the bonding layer protrusion 4a becomes thicker toward the outside, the angle ∠BAC becomes smaller. With such a shape, the stress on the bonding layer protrusion 4a becomes large. Also, a gap is likely to occur between the side of the front metal plate 3 and the molded resin 8.

[0029] Furthermore, although there is no particular upper limit to the angle ∠BAC, it is preferable that it is 180° or less. If it is greater than 180°, the side of the front metal plate 3 will be too inclined, and the area for mounting the semiconductor element 7 (shown in FIG. 3) may become small. Also, when the angle ∠BAC exceeds 180°, there is a case where the bonding layer protruding portion 4a is long and becomes thinner toward the tip. If the bonding layer protruding portion 4a becomes long, the adjacent front metal plates 3 (or back It may be difficult to narrow the pitch between the metal plates 6. For this reason, the angle ∠BAC is preferably 110° or more and 180° or less, and more preferably 130° or more and 160° or less.

[0030] As shown in FIG. 1, the side of the front metal plate 3 may have an inclined shape that widens in the negative direction of the z axis, but as shown in FIG. 5, the side of the front metal plate 3 may have an arc shape that widens in the positive and negative directions of the z axis. By making the angle ∠BAC 110° or more and making the side of the front metal plate 3 arc-shaped, it is possible to achieve both stress relaxation and an increase in the mounting area of ​​the semiconductor element 7 (shown in FIG. 3). In addition, it is possible to suppress peeling of the molding resin when the resin is molded. FIG. 5 shows a second example of a ceramic circuit board 1 in which at least one side of the metal plates 3 and 6, for example, the side of the front metal plate 3, has an arc shape. Also, FIG. 6 shows a third example of a ceramic circuit board 1 in which the connection between the side of the front metal plate 3 and the surface has an R shape. 5 and 6 are cross-sectional views taken along line II in FIG. 2(B), but in FIGS. 5 and 6, the bonding layer 4 and the rear metal plate 6 on the rear side of the ceramic circuit board 2 are omitted.

[0031] As shown in Fig. 5, when the side surface of the front metal plate 3 has an arc shape, the surface of the front metal plate 3 is extended in the x-axis direction and the y-axis direction, respectively. This increases the flat surface on the surface of the front metal plate 3, making it possible to increase the mounting area for the semiconductor element 7. On the other hand, when the connection portion between the side surface and the front surface of the front metal plate 3 has an R shape as shown in Fig. 6, the flat surface on the front surface of the front metal plate 3 and the back surface of the back metal plate 6 becomes smaller, making it impossible to increase the mounting area.

[0032] In addition, when viewed in the above-mentioned cross-sectional SEM photograph (500x), the side surface of the front metal plate 3 shown in Fig. 5 may have slight irregularities. If the upper end of the side surface of the front metal plate 3 shown in Fig. 5 extends outward, it is called an arc shape.

[0033] Returning to the explanation of Figure 1, the area between the plane that passes through point B and is parallel to the plane (xy plane) of ceramic substrate 2 and the interface between front metal plate 3 and bonding layer 4 is defined as region M. The average Vickers hardness of 10 points in region M is Hm, the average Vickers hardness of 10 points in bonding layer 4 is Hb, 300>Hm>Hb and Hm / Hb<2, and the ratio R of the area in region M where components of bonding layer 4 other than components of front metal plate 3 exist is 5% or more and 20% or less.

[0034] Region M is the region between a line in the x-axis direction passing through point B and the interface between the front metal plate 3 and the bonding layer 4. In addition, the interface between the front metal plate 3 and the bonding layer 4 is a region where components other than the front metal plate 3 are 8 mass% or more.

[0035] For example, when a copper plate is used as the front metal plate 3, the interface between the copper plate and the bonding layer 4 is determined as the location where the concentration of components other than copper in the copper plate reaches 8 [mass%]. When there are two or more components other than the front metal plate 3, the interface between the copper plate and the bonding layer 4 is determined as the location where the total concentration reaches 8 [mass%]. The interface between the front metal plate 3 and the bonding layer 4 is measured by point analysis using SEM-EDX (energy dispersive X-ray spectroscopy).

[0036] The average value of the Vickers hardness at 10 points in the region M is defined as Hm, and the average value of the Vickers hardness at 10 points in the bonding layer 4 is defined as Hb. Measurement of Vickers Hardness teeth According to JIS-Z-2244(2009) cormorantThe specimen is taken from any cross section of the ceramic circuit board 1. The surface roughness Ra of the specimen measurement surface is 1 μm or less. If necessary, the specimen measurement surface may be polished. The test force (F) used is 9.807 N. The Vickers hardness may be measured by nanoindentation. The measurement method using the nanoindentation method is as described in Patent Document 1. The ISO corresponding to JIS-Z-2244 is ISO6507.

[0037] The Vickers hardness is measured at any 10 points in the region M, and the average value is defined as Hm. Similarly, the average value of the Vickers hardness at any 10 points in the bonding layer is defined as Hb.

[0038] In addition, it satisfies 300>Hm>Hb and Hm / Hb<2. 300>Hm>Hb indicates that Hm and Hb are less than 300 Vickers hardness. It also indicates that the Vickers hardness Hb of the bonding layer 4 is lower than the Vickers hardness Hm of the region M. In addition, Hm / Hb<2 indicates that the Vickers hardness Hm of the region M is less than twice the Vickers hardness Hb of the bonding layer 4. This indicates that the difference in hardness between the region M and the bonding layer 4 is small. This makes it possible to reduce the stress generated in the protruding portion 4a of the bonding layer. In addition, it is possible to suppress peeling of the resin when molding with resin. This is because the amount of deformation accompanying the deformation of the molding resin 8 (shown in FIG. 3) can be reduced.

[0039] The Vickers hardness Hb of the bonding layer 4 is preferably not less than 90 and not more than 200. When Hb is within the range of not less than 90 and not more than 200, it becomes easier to control the relationship between Hm and Hb.

[0040] In addition, the components of the bonding layer 4 other than the components of the front metal plate 3 in the region M are preferably one or more selected from Ag (silver), Ti (titanium), Sn (tin), In (indium), Zr (zirconium), Al (aluminum), Si (silicon), C (carbon), and Mg (magnesium). The components of the bonding layer 4 other than the components of the front metal plate 3 in the region M refer to components of the bonding layer 4 that are different from the front metal plate 3. In other words, it indicates that the bonding layer 4 contains one or more elements selected from Ag, Ti, Sn, In, Zr, Al, Si, C, and Mg. Note that point C when calculating the angle ∠BAC is represented as point C. Carbon in the bonding layer 4 is represented as C.

[0041] As described later, a heating and bonding process is performed when bonding the ceramic substrate 2 and the front metal plate 3 via the bonding layer 4. The components of the bonding layer 4 diffuse into the front metal plate 3 by heating. This allows Hm and Hb to be controlled. As described above, the interface between the front metal plate 3 and the bonding layer 4 is a region where components other than the front metal plate 3 account for 8% by mass. It is preferable that region M contains a total of 1% by mass or more of one or more elements selected from Ag, Ti, Sn, In, Zr, Al, Si, C, and Mg.

[0042] Furthermore, the ratio R of the area in region M where components of bonding layer 4 other than the components of front metal plate 3 are present is 5% or more and 20% or less. In order to control the Vickers hardness of region M, it is effective to control the ratio of the area where components of bonding layer 4 other than the components of front metal plate 3 are present in region M. The components of bonding layer 4 other than the components of front metal plate 3 in region M are one or more selected from Ag, Ti, Sn, In, Zr, Al, Si, C, and Mg.

[0043] The ratio R within region M is measured using area analysis by SEM-EDX. Area analysis is also called surface analysis. In any cross section of ceramic circuit board 1, the measurement region is region M, 50 μm wide × 20 μm thick. The 50 μm width is the width direction of region M. The 20 μm thickness is the range 20 μm into the bonding layer side, based on the line in the x-axis direction that passes through point B used when determining region M.

[0044] When the ratio R is within the range of 5% to 20%, Hm and Hb can be controlled. In addition, by distributing bonding layer components other than the metal plate components in the region M, the reliability of the bond can be improved. The ratio R can be measured at any one location. In other words, it is preferable that the ratio R is within the range of 5% to 20%, regardless of where in the region M is measured.

[0045] The ceramic circuit board 1 as described above can improve the TCT characteristics. In addition, it can suppress the peeling of the resin when molding the resin. Therefore, it is suitable for a semiconductor device in which a semiconductor element is mounted on the ceramic circuit board 1.

[0046] FIG. 3 shows an example of a semiconductor device according to an embodiment. In the figure, 1 is a ceramic circuit board, 7 is a semiconductor element, 8 is a molded resin, and 10 is a semiconductor device. FIG. 3 shows an example in which one semiconductor element is mounted, but two or more may be mounted. Although not shown, a lead frame, wire bonding, screw fastening structure, etc. may also be provided. Also, an example in which resin is molded over the entire semiconductor device 10 to form the molded resin 8 has been shown, but resin may also be molded over only the surface on which the semiconductor element 7 is mounted to form the molded resin 8.

[0047] The ceramic circuit board 1 according to the embodiment has excellent TCT characteristics. In addition, the mold resin 8 on the side surfaces of the metal plates 3 and 6 does not easily peel off. This improves the reliability of the semiconductor device 10 including the mold resin 8.

[0048] Next, a method for manufacturing the ceramic circuit board 1 according to the embodiment will be described. The method for manufacturing the ceramic circuit board 1 according to the embodiment is not limited as long as it has the above-mentioned configuration, but the following method can be mentioned as a method for obtaining the ceramic circuit board 1 with a good yield.

[0049] First, prepare a ceramic substrate 2. The ceramic substrate 2 is preferably one selected from a silicon nitride substrate, an aluminum nitride substrate, an alumina substrate, and an alumina substrate. Furthermore, the ceramic substrate 2 is preferably a silicon nitride substrate having a thermal conductivity of 80 [W / m K] or more. Furthermore, the silicon nitride substrate preferably has a three-point bending strength of 600 [MPa] or more. By increasing the strength of the silicon nitride substrate, the substrate thickness can be reduced. Next, the metal plates 3 and 6 are prepared. The metal plates 3 and 6 are preferably copper plates or aluminum plates. The copper plates are preferably oxygen-free copper plates. The aluminum plates are preferably pure aluminum plates. The metal plates 3 and 6 preferably have a thickness of 0.3 mm or more.

[0050] Next, a brazing material that will become the bonding layer 4 is prepared. When a copper plate is used as the bonding layer 4, it is preferable that the brazing material contains Ag (silver) or Cu (copper) as the main component and Ti (titanium). Brazing material containing Ti is called an active metal brazing material. In the active metal brazing material, Ti reacts with the ceramic substrate 2 to form a reaction layer, thereby improving the bonding strength. If the ceramic substrate 2 is a nitride-based ceramic substrate, the reaction layer will be mainly composed of titanium nitride. Nitride-based ceramic substrates include silicon nitride substrates and aluminum nitride substrates. Also, if the ceramic substrate 2 is an oxide-based ceramic substrate, the reaction layer will be mainly composed of titanium oxide. Oxide-based ceramic substrates include aluminum oxide. M These include nium substrates and arginine substrates.

[0051] The brazing material composition preferably contains Ag (silver) at 0% by mass to 60% by mass, Cu (copper) at 15% by mass to 85% by mass, and Ti (titanium) or TiH2 (titanium hydride) at 1% by mass to 15% by mass. When both Ti and TiH2 are used, the total is within the range of 1% by mass to 15% by mass. When both Ag and Cu are used, Ag is preferably 20-60% by mass and Cu is preferably 15-40% by mass.

[0052] The brazing material composition may contain one or both of Sn (tin) and In (indium) in an amount of 1% by mass to 50% by mass, if necessary. The content of Ti or TiH2 is preferably 1% by mass to 15% by mass, more preferably 1% by mass to 6% by mass. If necessary, C (carbon) may be contained in an amount of 0.1% by mass to 2% by mass. If necessary, one or more selected from Zr, Al, Si, and Mg may be contained in an amount of 0.1% by mass to 5% by mass.

[0053] The ratio of the brazing material composition is calculated with the total of the mixed raw materials being 100 [mass %]. For example, if it is composed of three types of materials, Ag, Cu, and Ti, then Ag+Cu+Ti=100 [mass %]. Also, if it is composed of four types of materials, Ag, Cu, TiH2, and In, then Ag+Cu+TiH2+In=100 [mass %]. Also, if it is composed of five types of materials, Ag, Cu, Ti, Sn, and C, then Ag+Cu+Ti+Sn+C=100 [mass %].

[0054] When an aluminum plate is used, the brazing material is preferably mainly composed of Al (aluminum) and contains Si (silicon) or Mg (magnesium). The Si content is preferably in the range of 0.1 [mass%] to 20 [mass%]. The Mg content is preferably in the range of 0.1 [mass%] to 20 [mass%]. Both Si and Mg may be contained. The ratio of the brazing material composition is calculated based on the total of the mixed raw materials being 100 [mass%]. For example, when the brazing material is composed of two types of materials, Al and Si, Al+Si=100 [mass%]. When the brazing material is composed of three types of materials, Al, Si, and Mg, Al+Si+Mg=100 [mass%].

[0055] After mixing the brazing material components, a binder and the like are added to prepare a brazing material paste. The brazing material paste is applied onto a ceramic substrate, and a front metal plate 3 is placed on it. When joining metal plates 3 and 6 to both sides of the ceramic substrate 2, respectively, the brazing material paste is applied to both sides of the ceramic substrate 2, and then the metal plates 3 and 6 are placed on it. This process makes it possible to prepare a laminate of the ceramic substrate 2, the brazing material paste, and the metal plates 3 and 6. In addition, it is preferable that the length and width of the ceramic substrate 2 and the metal plates 3 and 6 in the laminate state are approximately the same. "Almost the same" means that they are within a range of ±2 mm.

[0056] The thickness of the brazing paste applied is preferably 10 μm or more and 60 μm or less. After the brazing paste is applied to the ceramic substrate 2, a drying process is preferably performed. The drying process is a heat treatment within a range of 40°C or more and 80°C or less. If the drying temperature is low, the binder components and the solvent components may not be sufficiently removed. If the drying temperature is high, the brazing material may be oxidized. By performing the drying process, the contact between the brazing material components and the front metal plate 3 can be made uniform.

[0057] This can improve the uniformity of the diffusion state of the brazing material components. Note that the binder components remaining in the drying process can be removed during the temperature increase process of the heat bonding process.

[0058] Next, a heat bonding step is performed. The heating temperature is preferably within the range of 600°C to 960°C. The atmosphere is preferably a vacuum or an inert gas. -3 [Pa] or less. Examples of inert gas include nitrogen gas and argon gas. "In nitrogen" refers to an atmosphere with a nitrogen content of 80% or more by volume.

[0059] In addition, in the heat bonding step, a load is preferably applied to the laminate. The load is preferably in the range of 500 [Pa] to 2000 [Pa]. This allows the brazing material components to diffuse in appropriate amounts into the metal plates and become homogenous.

[0060] In addition, it is preferable to set the cooling rate after the heat bonding process to 5°C / min or more. By increasing the cooling rate, the brazing material can be solidified quickly. This allows the Vickers hardness of the bonding layer 4 to be uniform.

[0061] Furthermore, the front metal plate 3 preferably has a number of triple points between metal crystal particles in a unit area of ​​1 mm × 1 mm that is within a range of 20 to 150. The number of triple points is determined by observing the surface of the front metal plate 3 with a metallurgical microscope. When it is difficult to confirm the metal crystal particles, the surface of the front metal plate 3 may be etched. Furthermore, if the front metal plate 3 is a copper plate, the triple points will be between copper crystal particles. If the front metal plate 3 is an aluminum plate, the triple points will be between aluminum crystal particles.

[0062] A triple junction between metal crystal particles is more likely to be a route for the diffusion of the brazing material than a route between two metal crystal particles. By increasing the number of triple junctions, the route for the diffusion of the brazing material can be made into a complex maze. This allows the amount of diffusion to be controlled. The number of triple junctions of the metal plate is the number of triple junctions of the front metal plate 3 after bonding. By performing the heat bonding process, the crystal particles of the front metal plate 3 grow. If the number of triple junctions after bonding is within the above range, the diffusion route of the brazing material can be controlled. If the number of triple junctions between metal crystal particles is less than 20 in a unit area of ​​1 [mm] × 1 [mm], the number of triple junctions is small, so the diffusion route is smooth. If the diffusion becomes smooth, the amount of diffusion may increase. Also, if the number of triple junctions exceeds 150, the diffusion route becomes complex, but the diffusion route itself increases, so the amount of diffusion may increase. If the amount of diffusion increases, the ratio R is more likely to exceed 20 [%]. For this reason, the metal plates 3 and 6 preferably have 20 to 150 triple points between metal crystal grains, and more preferably 30 to 100, per unit area of ​​1 mm×1 mm.

[0063] Through the above steps, a bonded body of the ceramic substrate 2 and the front metal plate 3 is produced. Next, a process of imparting a circuit shape to the front metal plate 3 is performed. It is preferable to use an etching process to impart the circuit shape. The etching process includes a process of etching the front metal plate 3 and a process of etching the bonding layer. The process of etching the front metal plate 3 makes it possible to control the circuit shape and the shape of the side surface of the front metal plate 3. Furthermore, the process of etching the bonding layer 4 makes it possible to control the size of the protruding portion 4a of the bonding layer. Laser processing and honing processing are also effective for the process of imparting the circuit shape.

[0064] Through the above steps, a ceramic circuit board 1 including the metal plates 3 and 6 (or only the front metal plate 3) can be manufactured. Furthermore, a semiconductor element 7 is mounted on the ceramic circuit board 1 to form a semiconductor device 10. Furthermore, if necessary, a lead frame or wire bonding is joined to the ceramic circuit board 1.

[0065] Also, a molding process using resin or gel is carried out as necessary. Molding using resin means sealing by solidifying resin. Molding using gel means sealing with a jelly-like resin. In this embodiment, a description will be given of a case where molding using resin is adopted, but molding using gel may be adopted instead of molding using resin. The molding resin 8 molded using resin has the role of protecting the semiconductor elements and wiring. Also, the molding resin 8 is table It is possible to suppress electrical conduction and discharge between metal plates and between front and back metal plates. Meanwhile, the junction temperature is increasing with the high performance of the semiconductor element 7. Accordingly, the amount of heat transferred to the metal plates 3 and 6 is increasing. There is a difference in thermal expansion coefficient between the ceramic substrate 2, the bonding layer protruding portion 4a, and the metal plates 3 and 6. Therefore, the stress caused by the difference in thermal expansion is large near the bonding layer protruding portion. The ceramic circuit substrate 1 according to the embodiment can prevent resin peeling because the angle ∠BAC and the like are controlled. In other words, it is suitable for the ceramic circuit substrate 1 to be molded with resin.

[0066] Examples of methods used in resin molding processes include methods using resins and methods using gels. Examples of resins include epoxy resins, polyester resins, and silicone resins. Examples of molding methods include transfer molding and compression molding.

[0067] (Example) (Examples 1 to 10, Comparative Examples 1 to 4) Silicon nitride substrates and aridil substrates were prepared as the ceramic substrates 2 according to Examples 1 to 10 and the ceramic substrates according to Comparative Examples 1 to 4. The silicon nitride substrates had a thermal conductivity of 90 [W / m K] and a three-point bending strength of 650 [MPa]. The aridil substrates had a thermal conductivity of 25 [W / m K] and a three-point bending strength of 550 [MPa]. The metal plates were oxygen-free copper (Cu) and pure aluminum (Al). The brazing filler metals shown in Table 1 were also prepared.

[0068] [Table 1] TIFF0007581476000001.tif61170

[0069] The brazing material was made into a paste and applied to the ceramic substrate. A metal plate was placed on top of the paste. The joining conditions are shown in Table 2. By the above method, a bonded body was produced in which a front metal plate and a back metal plate were bonded to both sides of a ceramic substrate. The ceramic substrate and the metal plates had the same length and width. The combination of ceramic substrate, brazing material, front metal plate, and back metal plate is as shown in Table 2.

[0070] [Table 2] TIFF0007581476000002.tif195170

[0071] The resulting bonded body was subjected to an etching process. Through this process, the length of the bonding layer protrusion and the angle ∠BAC were adjusted. This resulted in the production of a ceramic circuit board. In addition, the length of the bonding layer protrusion and the angle ∠BAC of the front copper plate and the back copper plate were made the same.

[0072] An arbitrary cross section of the obtained ceramic circuit board was observed by SEM. The length of the protruding part of the bonding layer and the angle ∠BAC were measured by SEM photographs. The nanoindentation method was also used to examine the area M and the Vickers hardness of the bonding layer. The ratio R was also measured by SEM-EDX. The results are shown in Table 3.

[0073] [Table 3] TIFF0007581476000003.tif141170

[0074] As can be seen from Table 3, in the ceramic circuit boards of Examples 1 to 10, when the length of the bonding layer protruding portion was 20 μm or more and 150 μm or less, the angle ∠BAC was 110° or more, 300>Hm>Hb, Hm / Hb<2, and the ratio R was within the range of 5% or more and 20% or less.

[0075] On the other hand, in Comparative Example 1, the hardness Hm exceeded 300. In Comparative Example 2, the angle ∠BAC was less than 110°. In Comparative Example 2, the length of the protruding portion of the bonding layer was less than 20 μm. In Comparative Example 4, the ratio R exceeded 20%.

[0076] In addition, in Examples 1 to 10 and Comparative Examples 1 to 3, the number of triple points between metal crystal particles in a unit area of ​​1 [mm] × 1 [mm] on the surface of the metal plate was within a range of 20 to 150. In Comparative Example 4, the number of triple points between metal crystal particles in a unit area of ​​1 [mm] × 1 [mm] was within a range of 2 to 12.

[0077] Next, the TCT characteristics and voltage resistance characteristics of the ceramic circuit board were measured. First, the two front metal plates were shorted by wire bonding. Next, as shown in Figure 4, the potential of each of the front and back metal plates was externally measured, and a molded resin was formed by the transfer molding method. The TCT characteristics of the molded resin were evaluated. The TCT conditions were -40[℃] x 30 minutes → room temperature x 10 minutes → 250[℃] x 30 minutes → room temperature x 10 minutes, with one cycle consisting of these conditions. The TCT tests were performed for 1000 and 3000 cycles.

[0078] After the TCT test, the peeling rate due to cracks between the metal plate and the ceramics was measured using ultrasonic testing (SAT). The peeling rate includes both the peeling of the metal plate and the resin of the mold resin.

[0079] In addition, the withstand voltage between the front and back copper plates was evaluated by applying AC 50 [Hz] for 60 [sec]. The withstand voltage was measured using samples after 3000 cycles of TCT. The withstand voltage evaluation started with the application of a voltage of 500 [V], and after each voltage passed the withstand voltage evaluation, the voltage was increased in steps of 500 [V]. This was continued until dielectric breakdown occurred, and the maximum voltage value at which dielectric breakdown did not occur was taken as the withstand voltage value. The results are shown in Table 4.

[0080] [Table 4] TIFF0007581476000004.tif147170

[0081] As can be seen from Table 4, there was no significant difference after 1000 cycles, but there was a significant difference after 3000 cycles. Therefore, it was found that the ceramic circuit boards according to Examples 1 to 10 have excellent reliability even when equipped with a resin mold. In contrast, peeling of the resin was confirmed in many places in the boards according to Comparative Examples 1 to 4.

[0082] As described above, according to the ceramic circuit board 1 and the semiconductor device 10 using the same, peeling of the molding resin 8 can be suppressed.

[0083] Although several embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. Modifications of these embodiments are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other.

Claims

1. In a ceramic circuit board in which a ceramic substrate and a metal plate are bonded via a bonding layer, The metal plate is any one of Cu, Al, and alloys containing these metals, When the ceramic circuit board is observed at a cross section consisting of a thickness direction and a lateral direction of the ceramic circuit board, The side surface of the metal plate has an inclined shape, The bonding layer has a bonding layer protruding portion that protrudes from an end where the side surface of the metal plate and the bonding layer are in contact with each other by 20 [μm] to 150 [μm], When the end portion is defined as point A, the side surface of the metal plate that is 20 μm inward from point A in the lateral direction is defined as point B, and the surface of the protruding portion of the bonding layer that is 20 μm outward from point A in the lateral direction is defined as point C, an angle ∠BAC is 110° or more, When an average value of Vickers hardness at 10 points in a region M between the lateral line passing through the point B and the interface between the metal plate and the bonding layer is Hm, and an average value of Vickers hardness at 10 points in the bonding layer is Hb, 300>Hm>Hb and Hm / Hb<2; A ceramic circuit board, characterized in that the ratio R of the area within the region M where components of the bonding layer other than components of the metal plate are present is 5% or more and 20% or less.

2. 2. The ceramic circuit board according to claim 1, wherein the length of the protruding portion of the bonding layer is within a range of 20 [μm] to 80 [μm].

3. 3. The ceramic circuit board according to claim 1, wherein the metal plate has a thickness of 0.3 mm or more.

4. A ceramic circuit board as described in any one of claims 1 to 3, characterized in that the components of the bonding layer other than the components of the metal plate in the region M are one or more selected from Ag, Ti, Sn, In, Zr, Al, Si, C, and Mg.

5. 5. The ceramic circuit board according to claim 1, wherein the ceramic substrate is a silicon nitride substrate having a thermal conductivity of 80 [W / mK] or more.

6. 6. The ceramic circuit board according to claim 1, wherein the bonding layer has a Vickers hardness Hb of 90 or more and 200 or less.

7. 7. The ceramic circuit board according to claim 1, wherein the number of triple points between metal crystal grains in a unit area of ​​1 [mm] × 1 [mm] on the surface of the metal plate is in the range of 20 to 150.

8. A semiconductor device comprising the ceramic circuit board according to any one of claims 1 to 7 and a semiconductor element mounted on the ceramic circuit board.

9. 9. The semiconductor device according to claim 8, wherein the semiconductor device is molded with a resin or a gel.

Citation Information

Patent Citations

  • Ceramic-metal joined body

    JP1994048851A

  • Ceramic-metal joined body

    JP1994048852A

  • Circuit substrate, heat dissipation module and semiconductor component

    JP2005005404A

  • Ceramic copper circuit board and semiconductor device employing same

    WO2013094213A1

  • Circuit substrate and semiconductor device

    WO2017056360A1