CLEANING METHOD, SEMICONDUCTOR DEVICE MANUFACTURING METHOD, SUBSTRATE PROCESSING APPARATUS AND PROGRAM
By dividing the processing chamber into zones with controlled temperature differences and managing gas flow, the cleaning method ensures uniformity in substrate processing, addressing non-uniformity issues in film thickness and film formation post-cleaning.
Patent Information
- Application Number
- JP2023506611
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-17
AI Technical Summary
The film forming process in semiconductor manufacturing often results in non-uniform cleaning of the processing chamber, leading to variations in film thickness on substrates due to uneven deposition and removal of film-forming materials.
The processing chamber is divided into multiple zones with controlled temperature differences and gas flow directions, and a cleaning method is employed where the temperature difference between zones is managed to ensure uniform cleaning by adjusting the cleaning gas supply and heating patterns.
This approach achieves nearly uniform processing of each substrate by controlling the cleaning process, reducing film thickness variations and suppressing the film thickness drop phenomenon post-cleaning, thereby ensuring consistent film formation.
Smart Images

Figure 0007581484000001 
Figure 0007581484000002 
Figure 0007581484000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a cleaning method, a manufacturing method for a semiconductor device, a substrate processing apparatus, and a program. [Background technology]
[0002] As one step in the manufacturing process of a semiconductor device, a film formation process is performed in which a source gas and a reactive gas are supplied to a substrate in a processing chamber to form a film on the substrate. When the film formation process is performed, deposits containing a film-forming material may adhere to the inner surface of the processing chamber. For this reason, a method is known in which, after the film formation process, a cleaning gas is supplied to the processing chamber in which the substrate is processed to clean the inside of the processing chamber (see, for example, JP 2007-13205 A and JP 2012-216696 A). Summary of the Invention
[0003] Incidentally, in the film forming process after cleaning, the processing may become non-uniform for each substrate.
[0004] An object of the present disclosure is to provide a technique that can make processing for each substrate more uniform in a substrate processing step after cleaning. [Means for solving the problem]
[0005] According to one aspect of the present disclosure, A method for cleaning a processing chamber for performing a film formation process on a substrate, comprising the steps of: a heating step of dividing a processing chamber into which a cleaning gas is supplied into three or more zones in a gas flow direction, and heating the processing chamber so that a temperature difference between a zone located on the upstream side in the gas flow direction in the processing chamber and a zone adjacent to the zone is larger than a temperature difference between a zone located on the downstream side in the gas flow direction and a zone adjacent to the zone; a supply step of supplying the cleaning gas into the processing chamber after the heating step; A cleaning method is provided comprising: Effect of the Invention
[0006] According to the present disclosure, in a substrate processing step after cleaning, processing for each substrate can be made more uniform. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic configuration diagram of a substrate processing apparatus according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing a flow of a cleaning gas in the processing furnace shown in FIG. [Diagram 3] 2 is a diagram showing a state in which a cleaning gas is supplied into a processing chamber from a second nozzle in the processing furnace shown in FIG. 1. FIG. [Figure 4] FIG. 2 is a diagram illustrating a configuration of a control unit of the substrate processing apparatus according to an embodiment of the present disclosure. [Diagram 5] FIG. 1 is a flow diagram of a substrate processing process according to an embodiment of the present disclosure. [Figure 6] 13 is a graph showing the relationship between the accumulated film thickness and the film thickness fluctuation rate in a processing chamber in a substrate processing apparatus of a comparative example. [Figure 7] 11 is a graph showing the relationship between the accumulated film thickness and the film thickness fluctuation rate in a processing chamber in the substrate processing apparatus of the embodiment. [Figure 8] 13 is a vertical cross-sectional view of a processing furnace included in a substrate processing apparatus according to another embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. Note that all drawings used in the following description are schematic, and the dimensional relationships, ratios, etc. of each element shown in the drawings do not necessarily match the actual ones. Furthermore, the dimensional relationships, ratios, etc. of each element between multiple drawings do not necessarily match.
[0009] <Substrate processing equipment> 1 is a diagram showing a substrate processing apparatus 10 according to the present embodiment. The substrate processing apparatus 10 is used for manufacturing semiconductor devices. Specifically, the substrate processing apparatus 10 according to the present embodiment is configured as a batch-type vertical heat processing apparatus.
[0010] 1, the substrate processing apparatus 10 of this embodiment includes a processing furnace 20. The processing furnace 20 includes a processing chamber 30, a processing gas supply system 40, a cleaning gas supply system 50, a heater 60 as a heating unit, and a controller 70 as a control unit.
[0011] (Processing room) 1, the processing furnace 20 includes a reaction tube 32 serving as a processing vessel. The reaction tube 32 is installed in the processing furnace 20 with the vertical direction of the processing furnace 20 as the axial direction (i.e., the tube axial direction). The reaction tube 32 includes an inner tube 34 and an outer tube 36.
[0012] The inner tube 34 is formed in a tubular shape (cylindrical shape in this embodiment). The internal space of the inner tube 34 constitutes the processing chamber 30. The processing chamber 30 processes wafers 200 as substrates. The processing chamber 30 is configured to be able to accommodate a boat 148, which is an example of a substrate holder capable of holding the wafers 200 in a horizontal position and aligned vertically in multiple stages by the boat 148 described below.
[0013] The inner tube 34 is made of a heat-resistant material, such as quartz (SiO 2 ), silicon carbide (SiC), etc.
[0014] The outer pipe 36 is formed in a tubular shape (cylindrical shape in this embodiment) with a closed upper end. The outer pipe 36 is disposed radially outside the inner pipe 34 so as to surround the inner pipe 34. The outer pipe 36 is also disposed concentrically with the inner pipe 34. As shown in FIG. 1, a gap is formed between the inner pipe 34 and the outer pipe 36.
[0015] The outer tube 36 is made of a heat-resistant material, such as quartz (SiO 2 ), silicon carbide (SiC), etc. In the present embodiment, the inner tube 34 and the outer tube 36 are formed of the same heat-resistant material, but the present disclosure is not limited to this configuration.
[0016] A manifold 38 is provided below the outer tube 36 and concentrically with the outer tube 36. The manifold 38 is formed in a cylindrical shape with an open upper end and a closed lower end. The manifold 38 engages with the inner tube 34 and the outer tube 36 to support the inner tube 34 and the outer tube 36. Examples of materials constituting the manifold 38 include metal materials such as nickel alloys and stainless steel, and heat-resistant materials such as quartz and SiC. An O-ring (not shown) is provided between the manifold 38 and the outer tube 36 as a sealing member. The manifold 38 is supported by a support (not shown) of the processing furnace 20, so that the reaction tube 32 is installed vertically with the up-down direction as the axial direction.
[0017] (Processing gas supply system) The process gas supply system 40 is configured to supply a process gas (source gas) into the process chamber. The process gas supply system 40 includes a first process gas supply system 42 and a second process gas supply system 44.
[0018] The first process gas supply system 42 is composed of at least a nozzle 80 serving as a first gas supply nozzle, a gas supply pipe 90, a valve 100, an MFC 110, and a valve 120, all of which are shown in Fig. 1. Note that a nozzle 81 serving as a second gas supply nozzle, a gas supply pipe 91, a valve 101, an MFC 111, and a valve 121, all of which are shown in Fig. 1, may be added to the first process gas supply system 42. Furthermore, a first process gas supply source 130 may be added to the first process gas supply system 42.
[0019] The nozzle 80 is connected to the peripheral wall of the manifold 38 and communicates with the inside of the processing chamber 30. Therefore, a first processing gas is supplied into the processing chamber 30 through the nozzle 80. A gas supply pipe 90 is connected to the upstream end of the nozzle 80 in the flow direction of the first processing gas. The gas supply pipe 90 is provided with a first processing gas supply source 130, a valve 120, an MFC (mass flow controller) 110 as a gas flow rate controller, and a valve 100, in this order from the upstream side in the flow direction of the first processing gas. The nozzle 80 is an example of a first nozzle of the present disclosure.
[0020] The nozzle 81 penetrates the peripheral wall of the manifold 38, extends from the lower side to the upper side of the processing chamber 30, and communicates with the inside of the processing chamber 30. Specifically, the nozzle 81 is L-shaped, extending horizontally through the peripheral wall of the manifold 38, bending midway, and extending from the lower side to the upper side of the processing chamber 30 along the axial direction of the reaction tube 32. In addition, as shown in FIG. 3, a vertical portion 81A of the nozzle 81 extending from the lower side to the upper side of the processing chamber 30 is provided with a plurality of injection ports 81B spaced apart in the extending direction of the vertical portion 81A (in the axial direction of the reaction tube 32 in this embodiment). The first processing gas supplied to the nozzle 81 is supplied into the processing chamber 30 from the plurality of injection ports 81B. Here, the injection port 81B is formed in the vertical portion 81A at least in the portion corresponding to the middle zone 30B and the upper zone 30A in the processing chamber 30, and therefore the first processing gas can be directly supplied to the middle zone 30B and the upper zone 30A of the processing chamber 30. A gas supply pipe 91 is connected to the upstream end of the nozzle 81 in the flow direction of the first processing gas. The gas supply pipe 91 is provided with a first processing gas supply source 130, a valve 121, a MFC (mass flow controller) 111 as a gas flow rate controller, and a valve 101 in this order from the upstream side in the flow direction of the first processing gas. The nozzle 81 is an example of the second nozzle of the present disclosure. It is not necessarily required to provide the nozzle 81 in the present disclosure. By providing the nozzle 81 and supplying the first processing gas from the nozzle 81, the processing uniformity for each wafer 200 can be improved.
[0021] The MFC 110, the valves 100 and 120, and the MFC 111, the valves 101 and 121 are each electrically connected to a controller 70 (see FIG. 4) which will be described later. The controller 70 is configured to control the MFC 110, the valves 100 and 120, and the MFC 111, the valves 101 and 121, respectively, so that the flow rates of the first process gas supplied into the process chamber 30 are each predetermined flow rates at predetermined timings.
[0022] 1, the second process gas supply system 44 is composed of at least a nozzle 82 serving as a first gas supply nozzle, a gas supply pipe 92, a valve 102, an MFC 112, and a valve 122. In addition, a nozzle 83 serving as a second gas supply nozzle, a gas supply pipe 93, a valve 103, an MFC 113, and a valve 123 may be added to the second process gas supply system 44. Furthermore, a second process gas supply source 131 may be added to the second process gas supply system 44.
[0023] The nozzle 82 is connected to the peripheral wall of the manifold 38 and communicates with the inside of the processing chamber 30. Therefore, the second processing gas is supplied into the processing chamber 30 through the nozzle 82. A gas supply pipe 92 is connected to the upstream end of the nozzle 82 in the flow direction of the second processing gas. The gas supply pipe 92 is provided with, in this order from the upstream side in the flow direction of the second processing gas, a second processing gas supply source 131, a valve 122, an MFC (mass flow controller) 112 as a gas flow rate controller, and a valve 102. The nozzle 82 is an example of a first nozzle of the present disclosure.
[0024] The nozzle 83 penetrates the peripheral wall of the manifold 38, extends from the lower side to the upper side of the processing chamber 30, and communicates with the inside of the processing chamber 30. Specifically, the nozzle 83 is L-shaped, extending horizontally through the peripheral wall of the manifold 38, bending midway, and extending from the lower side to the upper side of the processing chamber 30 along the axial direction of the reaction tube 32. In addition, as shown in FIG. 3, a vertical portion 83A of the nozzle 83 extending from the lower side to the upper side of the processing chamber 30 is provided with a plurality of injection ports 83B spaced apart in the extending direction of the vertical portion 83A (in the axial direction of the reaction tube 32 in this embodiment). The second processing gas supplied to the nozzle 83 is supplied into the processing chamber 30 from the plurality of injection ports 83B. Here, since the injection ports 83B are formed in the vertical portion 83A at least in portions corresponding to the middle zone 30B and the upper zone 30A in the processing chamber 30, the first processing gas can be directly supplied to the middle zone 30B and the upper zone 30A of the processing chamber 30. A gas supply pipe 93 is connected to the upstream end of the nozzle 83 in the flow direction of the second processing gas. The gas supply pipe 93 is provided with a second processing gas supply source 131, a valve 123, an MFC (mass flow controller) 113 as a gas flow rate controller, and a valve 103 in this order from the upstream side in the flow direction of the second processing gas. The nozzle 83 is an example of a second nozzle in the present disclosure. In the present disclosure, the nozzle 83 is not necessarily required. By providing the nozzle 83 and supplying the second process gas from the nozzle 83, it is possible to improve the process uniformity for each wafer 200.
[0025] The MFC 112, the valve 102, and the valve 122, and the MFC 113, the valve 103, and the valve 123 are each electrically connected to a controller 70 (see FIG. 4). The controller 70 is configured to control the MFC 112, the valve 102, and the valve 122, and the MFC 113, the valve 103, and the valve 123, respectively, so that the flow rate of the second process gas supplied into the process chamber 30 becomes a predetermined flow rate at a predetermined timing.
[0026] (Cleaning gas supply system) The cleaning gas supply system 50 is configured to supply a cleaning gas into the processing chamber 30. The cleaning gas supply system 50 includes a first cleaning gas supply system 52 and a second cleaning gas supply system 54, as shown in FIG.
[0027] The first cleaning gas supply system 52 mainly includes a nozzle 80, a gas supply pipe 94, a valve 104, an MFC 114, and a valve 124. A nozzle 81, a gas supply pipe 95, a valve 105, an MFC 115, and a valve 125 may also be added to the first cleaning gas supply system 52. Furthermore, a cleaning gas supply source 132 may also be added to the first cleaning gas supply system 52.
[0028] 1, a gas supply pipe 94 for supplying a cleaning gas into the processing chamber 30 is connected between the valve 100 and the nozzle 80 of the gas supply pipe 90. In the gas supply pipe 94, a cleaning gas supply source 132, a valve 124, an MFC (mass flow controller) 114 as a gas flow rate controller, and a valve 104 are provided in this order from the upstream side in the flow direction of the cleaning gas.
[0029] A gas supply pipe 95 for supplying a cleaning gas into the processing chamber 30 is connected between the valve 101 and the nozzle 81 of the gas supply pipe 91. In the gas supply pipe 95, a cleaning gas supply source 132, a valve 125, an MFC (mass flow controller) 115 as a gas flow rate controller, and a valve 105 are provided in this order from the upstream side in the flow direction of the cleaning gas.
[0030] The MFC 114, the valves 104 and 124, and the MFC 115, the valves 105 and 125 are each electrically connected to a controller 70 (see FIG. 4). The controller 70 is configured to control the MFC 114, the valves 104 and 124, and the MFC 115, the valves 105 and 125, respectively, so that the flow rates of the cleaning gas supplied into the processing chamber 30 are each predetermined flow rates at predetermined timings.
[0031] The second cleaning gas supply system 54 is composed of at least a nozzle 82, a gas supply pipe 96, a valve 106, an MFC 116, and a valve 126. A nozzle 83, a gas supply pipe 97, a valve 107, an MFC 117, and a valve 127 may also be added to the second cleaning gas supply system 54. Furthermore, a cleaning gas supply source 132 may also be added to the second cleaning gas supply system 54.
[0032] 1, a gas supply pipe 96 for supplying a cleaning gas into the processing chamber 30 is connected between the valve 102 of the gas supply pipe 92 and the nozzle 82. The gas supply pipe 96 is provided with a cleaning gas supply source 132, a valve 126, an MFC (mass flow controller) 116 as a gas flow rate controller, and a valve 106 in this order from the upstream side in the flow direction of the cleaning gas.
[0033] A gas supply pipe 97 for supplying a cleaning gas into the processing chamber 30 is connected between the valve 103 and the nozzle 83 of the gas supply pipe 93. The gas supply pipe 97 is provided with a cleaning gas supply source 132, a valve 127, an MFC (mass flow controller) 117 as a gas flow rate controller, and a valve 107 in this order from the upstream side in the flow direction of the cleaning gas.
[0034] The MFC 116, the valves 106 and 126, and the MFC 117, the valves 107 and 127 are each electrically connected to a controller 70 (see FIG. 4). The controller 70 is configured to control the MFC 116, the valves 106 and 126, and the MFC 117, the valves 107 and 127, respectively, so that the flow rates of the cleaning gas supplied into the processing chamber 30 are each predetermined flow rates at predetermined timings.
[0035] With this configuration, the cleaning gas is supplied from the upstream side (lower side) of the processing chamber 30 to the downstream side (upper side).
[0036] In this embodiment, one cleaning gas supply source is used for multiple cleaning gas supply systems, but the present disclosure is not limited to this configuration, and one cleaning gas supply source may be used for each cleaning gas supply system.
[0037] (Inert gas supply system) The processing furnace 20 also includes an inert gas supply system 58. The inert gas supply system 58 is configured to supply an inert gas into the processing chamber 30.
[0038] The inert gas supply system 58 is composed of at least a nozzle 82, a gas supply pipe 98, a valve 108, an MFC 118, and a valve 128. A nozzle 83, a gas supply pipe 99, a valve 109, an MFC 119, and a valve 129 may be added to the inert gas supply system 58. Furthermore, an inert gas supply source 133 may be added to the inert gas supply system 58.
[0039] 1, a gas supply pipe 98 for supplying an inert gas into the processing chamber 30 is connected between the valve 102 and the nozzle 82 of the gas supply pipe 92. In the gas supply pipe 98, an inert gas supply source 133, a valve 128, an MFC (mass flow controller) 118 as a gas flow rate controller, and a valve 108 are provided in this order from the upstream side in the flow direction of the inert gas.
[0040] A gas supply pipe 99 for supplying an inert gas into the processing chamber 30 is connected between the valve 103 and the nozzle 83 of the gas supply pipe 93. The gas supply pipe 99 is provided with an inert gas supply source 133, a valve 129, an MFC (mass flow controller) 119 as a gas flow rate controller, and a valve 109 in this order from the upstream side in the flow direction of the inert gas.
[0041] The MFC 118, the valves 108 and 128, and the MFC 119, the valves 109 and 129 are each electrically connected to a controller 70 (see FIG. 4). The controller 70 is configured to control the MFC 118, the valves 108 and 128, and the MFC 119, the valves 109 and 129, respectively, so that the flow rates of the cleaning gas supplied into the processing chamber 30 are predetermined flow rates at predetermined timings.
[0042] The inert gas is, for example, nitrogen (N 2 ) gas may also be used.
[0043] (Exhaust system) 1, the processing furnace 20 includes an exhaust system 140. The exhaust system 140 is configured to exhaust the atmosphere inside the processing chamber 30. The exhaust system 140 is mainly configured with an exhaust pipe 141, a pressure sensor 142, an APC valve 143, and a vacuum pump 144.
[0044] The exhaust pipe 141 is connected to the peripheral wall of the manifold 38. In addition, the exhaust pipe 141 is disposed at the lower end of the cylindrical space 37 formed by the gap between the inner pipe 34 and the outer pipe 36, and communicates with the cylindrical space 37. With this configuration, the exhaust pipe 141 is adapted to exhaust the atmosphere in the processing chamber 30 via the cylindrical space 37.
[0045] On the opposite side of the exhaust pipe 141 from the side connected to the manifold 38, a vacuum pump 144 as a vacuum exhaust device is provided via a pressure sensor 142 as a pressure detector and an APC valve 143 as a pressure adjustment device.
[0046] The vacuum pump 144 is configured to evacuate the processing chamber 30 so that the pressure inside the processing chamber 30 becomes a predetermined pressure (vacuum degree). A controller 70 is electrically connected to the APC valve 143 and the pressure sensor 142. The controller 70 is configured to control the APC valve 143 at a desired timing based on pressure information detected by the pressure sensor 142 so that the pressure inside the processing chamber 30 becomes the desired pressure.
[0047] With the above-mentioned configuration, the first process gas supplied from the first process gas supply system, the second process gas supplied from the second process gas supply system, the cleaning gas supplied from the cleaning gas supply system, and the inert gas supplied from the inert gas supply system each rise in the internal space of the inner tube 34 (inside the process chamber 30), flow from the upper end opening of the inner tube 34 into the cylindrical space 37, flow down the cylindrical space 37, and then are exhausted from the exhaust pipe 141 (see FIG. 2).
[0048] Below the manifold 38, a seal cap 146 is provided as a furnace port cover capable of air-tightly closing the lower end opening of the manifold 38. The seal cap 146 is adapted to be brought into contact with the lower end of the manifold 38 from below in the vertical direction. The seal cap 146 is formed in a disk shape. Examples of materials that form the seal cap 146 include metal materials such as stainless steel. An O-ring (not shown) is provided on the upper surface of the seal cap 146 as a seal member that comes into contact with the lower end of the manifold 38.
[0049] A support stand 149 that supports the boat 148 is provided on the seal cap 146. The support stand 149 is made of a heat-resistant material. Examples of materials that can be used to make the support stand 149 include quartz and silicon carbide (SiC). The support stand 149 functions as a heat insulating section that makes it difficult for heat from the heater 60 to be transmitted to the manifold 38 side.
[0050] As described above, the boat 148 is configured to be able to hold multiple wafers 200 in multiple stages in a horizontal position with their centers aligned. The boat 148 is made of a heat-resistant material such as quartz or silicon carbide.
[0051] Further, a rotation mechanism (not shown) for rotating the boat 148 and a boat elevator (not shown) for raising and lowering the boat 148 are provided below the seal cap 146. The rotation mechanism can rotate the boat 148 within the processing chamber 30 by a rotational action. Furthermore, the boat elevator can move the boat 148 in and out of the processing chamber 30 by a raising and lowering action.
[0052] (heater) The heater 60 as a heating unit is formed in a tubular shape (cylindrical shape in this embodiment) and is disposed radially outside the reaction tube 32 so as to surround the reaction tube 32. The heater 60 is also disposed concentrically with the reaction tube 32.
[0053] As shown in FIG. 1, the heater 60 is configured to divide the inside of the processing chamber 30 into three or more zones in the gas flow direction of the cleaning gas, and to heat each zone individually. Specifically, the heater 60 in this embodiment is divided into three in the axial direction, which are heater section 60A, heater section 60B, and heater section 60C from the top. These heater sections 60A, 60B, and 60C are individually controlled by the controller 70. Specifically, the controller 70 is configured to adjust the heating temperature of each heater section by controlling the power supply to each heater wire provided in each heater section (for example, by controlling the on / off of a thyristor). The range heated by the heater section 60A of the processing chamber 30 is the upper zone 30A of the processing chamber 30, the range heated by the heater section 60B of the processing chamber 30 is the middle zone 30B of the processing chamber 30, and the range heated by the heater section 60C of the processing chamber 30 is the lower zone 30C of the processing chamber 30. The upper zone 30A is a zone located downstream in the flow direction of the cleaning gas in the processing chamber 30, the middle zone 30B is a zone located midstream in the flow direction of the cleaning gas in the processing chamber 30, and the lower zone 30C is a zone located upstream in the flow direction of the cleaning gas in the processing chamber 30. Here, the downstream side in the gas flow direction in the processing chamber 30 means the side close to the exhaust system that exhausts the atmosphere in the processing chamber 30, and the upstream side in the gas flow direction means the opposite side to the downstream side. In addition, the midstream side in the gas flow direction means the vicinity of the middle between the downstream side and the upstream side. In other words, the upstream side, midstream side, and downstream side of the gas flow do not have to coincide with the position of each zone of the heater 60.
[0054] 1, in the cylindrical space 37, temperature sensors are installed as temperature detectors for detecting the temperature inside the reaction tube 32. Specifically, a temperature sensor 62A is installed in a range of the cylindrical space 37 heated by the heater part 60A, a temperature sensor 62B is installed in a range of the cylindrical space 37 heated by the heater part 60B, and a temperature sensor 62C is installed in a range of the cylindrical space 37 heated by the heater part 60C.
[0055] A controller 70 is electrically connected to the heater parts 60A, 60B, 60C, temperature sensors 62A, 62B, and 62C. The controller 70 is configured to control the power supply to each heater part of the heater 60 at a desired timing based on temperature information detected by each temperature sensor so that the temperature inside the processing chamber 30 has a desired temperature distribution.
[0056] (controller) The controller 70 is configured as a computer. This computer includes a central processing unit (CPU) 121A, a random access memory (RAM) 121B, a storage device 73, and an I / O port 74, as shown in FIG.
[0057] The RAM 72, the storage device 73, and the I / O port 74 are configured to be able to exchange data with the CPU 71 via an internal bus 75. The controller 70 is connected to an input / output device 76 configured as, for example, a touch panel.
[0058] The storage device 73 is composed of, for example, a flash memory, a HDD (Hard Disk Drive), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe describing the procedure and conditions of substrate processing (to be described later), etc. are readably stored in the storage device 73.
[0059] A process recipe is a combination of procedures in a substrate processing step, which will be described later, that are executed by the controller 70 to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, and the like will be collectively referred to simply as a program.
[0060] In this disclosure, when the word "program" is used, it may include only a process recipe, only a control program, or both. The RAM 72 is configured as a memory area (work area) in which programs and data read by the CPU 71 are temporarily stored.
[0061] Connected to the I / O port 74 are valves 100-109, MFCs (mass flow controllers) 110-119, valves 120-129, a pressure sensor 142, an APC valve 143, a vacuum pump 144, heater sections 60A-60C of the heater 60, each temperature sensor 62A-62C, a rotation mechanism not shown, a boat elevator not shown, etc.
[0062] The CPU 71 is configured to read and execute a control program from the storage device 73, and also to read a process recipe from the storage device 73 in response to an input of an operation command from the input / output device .
[0063] The CPU 71 is configured to be able to control the flow rate adjustment operation of various gases by the MFCs 110-119, the opening and closing operations of the valves 100-109 and the valves 110-119, and the opening and closing operation of the APC valve 143, in accordance with the contents of the read process recipe. The CPU 71 is also configured to be able to control the pressure adjustment operation by the APC valve 143 based on the pressure sensor 142, the start and stop of the vacuum pump 144, and the temperature adjustment operation of the heater 60 (each of the heater sections 60A-60C) based on each of the temperature sensors 62A-62C. The CPU 71 is also configured to be able to control the rotation and rotation speed adjustment operation of the boat 148 by the boat rotation mechanism, the raising and lowering operation of the boat 148 by the boat elevator, etc.
[0064] The controller 70 is not limited to being configured as a dedicated computer, and may be configured as a general-purpose computer. For example, the controller 70 of this embodiment can be configured by preparing an external storage device 77 storing the above-mentioned program, and installing the program in a general-purpose computer using this external storage device 77. Examples of the external storage device include a magnetic disk such as a hard disk, an optical disk such as a CD, a magneto-optical disk such as an MO, and a semiconductor memory such as a USB memory.
[0065] However, the means for supplying the program to the computer is not limited to supplying it via the external storage device 77. For example, the program may be supplied without going through the external storage device 77 by using a communication means such as the Internet or a dedicated line. The storage device 73 and the external storage device 77 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. When the term recording medium is used in this disclosure, it may include only the storage device 73 alone, only the external storage device 77 alone, or both.
[0066] The controller 70 of this embodiment is configured to control the heater parts 60A-60C of the heater 60 to heat the inside of the processing chamber 30 so that the temperature difference (T2) between the zone (lower zone 30C) located on the upstream side in the gas flow direction in the processing chamber 30 and the zone (middle zone 30B) adjacent thereto becomes larger than the temperature difference (T1) between the zone (upper zone 30A) located on the downstream side in the gas flow direction and the zone (middle zone 30B) adjacent thereto. The controller 70 is configured to control the cleaning gas supply system 50 to supply a cleaning gas into the processing chamber 30 while maintaining the temperature state (T2>T1) in the heated processing chamber 30.
[0067] <Substrate processing process> Next, as one step in the manufacturing process of a semiconductor device, a substrate processing step in which a film formation process is performed to form a film on the wafer 200, a cleaning process as a removal process to remove a film-forming material attached to the inner surface of the processing chamber 30, and a pre-coating process to form a film of a predetermined thickness on the inner surface of the processing chamber 30 are performed in this order will be described with reference to Fig. 5. In the following description, the operation of each part constituting the substrate processing apparatus 10 is controlled by a controller 70.
[0068] (Carry-in process) In the loading step S210, the wafers 200 are loaded into the processing chamber 30. More specifically, first, a plurality of wafers 200 are loaded into the boat 148 (wafer charge). Then, as shown in Fig. 1, the boat 148 holding the plurality of wafers 200 is elevated by a boat elevator (not shown) and loaded into the processing chamber 30 (boat load). In this state, the seal cap 146 seals the lower end of the manifold 38 via an O-ring (not shown).
[0069] When the loading step S210 is performed, an inert gas (nitrogen gas in this embodiment) is supplied into the processing chamber 30 to purge the processing chamber 30. Specifically, by opening the valves 108 and 128, the inert gas supplied from the inert gas supply source 133 to the gas supply pipe 98 is controlled to a predetermined flow rate by the MFC 118, and then supplied from the nozzle 82 through the gas supply pipe 98 into the processing chamber 30. Also, by opening the valves 109 and 129, the inert gas supplied from the inert gas supply source 133 to the gas supply pipe 99 is controlled to a predetermined flow rate by the MFC 119, and then supplied from the nozzle 83 through the gas supply pipe 99 into the processing chamber 30. In this manner, the inert gas is supplied into the processing chamber 30, and the processing chamber 30 is purged. The supply of the inert gas into the processing chamber 30 continues until all the steps of the substrate processing process are completed.
[0070] (Film forming process) In the film forming process S220, the inside of the processing chamber is heated, and a processing gas is supplied into the processing chamber 30 to perform a film forming process to form a film on the wafer 200. Specifically, first, the processing chamber 30 is evacuated by the vacuum pump 144 so that the inside of the processing chamber 30 becomes a predetermined film forming pressure (vacuum degree). At this time, the pressure inside the processing chamber 30 is measured by the pressure sensor 142, and the APC valve 143 is feedback-controlled based on the measured pressure information. Also, the inside of the processing chamber 30 is heated by the heater 60 so that the inside of the processing chamber 30 becomes a predetermined temperature. At this time, the power supply to the heater parts 60A to 60C of the heater 60 is feedback-controlled based on the temperature information detected by the temperature sensors 62A to 62C, respectively, so that the temperature inside the processing chamber 30 becomes a predetermined temperature (film forming temperature) (S221). Next, the boat 148 and the wafer 200 start to rotate by a rotation mechanism (not shown).
[0071] In a state where the inside of the processing chamber 30 is maintained at a predetermined film formation temperature and a predetermined film formation pressure, the supply of the first processing gas and the second processing gas into the processing chamber 30 is started (S222). Specifically, the first processing gas supplied from the first processing gas supply source 130 into the gas supply pipe 90 by opening the valves 100 and 120 is controlled to a predetermined flow rate by the MFC 110, and then passes through the gas supply pipe 90 and is supplied from the nozzle 80 into the processing chamber 30. In addition, the first processing gas supplied from the first processing gas supply source 130 into the gas supply pipe 91 by opening the valves 101 and 121 is controlled to a predetermined flow rate by the MFC 111, and then passes through the gas supply pipe 91 and is supplied from the nozzle 81 into the processing chamber 30. In this manner, the first gas is supplied into the processing chamber 30. On the other hand, the second process gas supplied from the second process gas supply source 131 into the gas supply pipe 92 by opening the valves 102 and 122 is controlled to a predetermined flow rate by the MFC 112, and then passes through the gas supply pipe 92 and is supplied from the nozzle 82 into the process chamber 30. Also, the second process gas supplied from the second process gas supply source 131 into the gas supply pipe 93 by opening the valves 103 and 123 is controlled to a predetermined flow rate by the MFC 113, and then passes through the gas supply pipe 93 and is supplied from the nozzle 83 into the process chamber 30.
[0072] At this time, the inert gas supplied into the processing chamber 30 functions as a dilution gas that dilutes the film forming gas (first processing gas and second processing gas) or as a carrier gas that promotes diffusion into the processing chamber 30. By controlling the supply flow rate of the inert gas, the concentration and diffusion speed of the film forming gas (first processing gas and second processing gas) can be controlled.
[0073] The film forming gas (first processing gas and second processing gas) supplied into the processing chamber 30 rises in the inner pipe 34 (inside the processing chamber 30) and flows out from the upper end opening of the inner pipe 34 into the cylindrical space 37. Then, the film forming gas flows down the cylindrical space 37 and is exhausted from the exhaust pipe 141. The film forming gas comes into contact with the surface of the wafer 200 while passing through the processing chamber 30. At this time, a thin film is deposited on the surface of the wafer 200 by a thermal CVD reaction. After a preset processing time has elapsed and a thin film with a predetermined thickness has been formed on the wafer 200, the valves 100 to 103 and the valves 120 to 123 are closed, respectively, to stop the supply of the film forming gas into the processing chamber 30.
[0074] Then, valves 108, 128, 109, and 129 are left open, and the supply of the inert gas into the processing chamber 30 is continued while the processing chamber 30 is evacuated, thereby purging the processing chamber 30. Once the atmosphere in the processing chamber 30 has been replaced with the inert gas, the opening of the APC valve 143 is adjusted to return the pressure in the processing chamber 30 to normal pressure. Furthermore, the power supply to the heater 60 is stopped, and the temperature in the processing chamber 30 is lowered to a predetermined temperature (wafer unloading temperature) (S223).
[0075] The processing conditions for the film forming step (S220) according to this embodiment are as follows: Film formation temperature: 600°C to 850°C (preferably around 650°C to 800°C) Supply flow rate of first processing gas: 10 sccm to 2000 sccm (preferably 50 sccm to 200 sccm) Supply flow rate of second processing gas: 100 sccm to 10,000 sccm (preferably 500 sccm to 2,000 sccm) Film forming pressure: 1 Pa to 2666 Pa (preferably less than 133 Pa) By maintaining each of the process conditions constant at a certain value within each range, a film (silicon nitride film) having a thickness of, for example, 10 nm to 200 nm is formed on the wafer 200.
[0076] The first processing gas may be a silicon-containing gas. The silicon-containing gas may be, for example, dichlorosilane (SiH 2 Cl 2 DCS gas is one example.
[0077] The second process gas may be a nitrogen-containing gas. Examples of the nitrogen-containing gas include ammonia (NH 3 ) gas.
[0078] (Export process) In the unloading step S230, the processed wafers 200 are unloaded from the processing chamber 30. More specifically, after the wafers 200 are subjected to the film formation process, the rotation of the boat 148 and the wafers 200 by the rotation mechanism is stopped. Next, the seal cap 146 is lowered by the boat elevator to open the lower end of the manifold 38, and the boat 148 holding the processed wafers 200 is unloaded (boat unloading) to the outside of the reaction tube 32. Thereafter, the processed wafers 200 are removed from the boat 148 (wafer discharging).
[0079] In the film forming process (S220), a film (silicon nitride film) is formed on the wafer 200 by the film forming gas, but the film is also formed on the inner surface of the inner tube 34 (in other words, the inner surface of the processing chamber 30) by the film forming gas. That is, the film forming material adheres to the inner surface of the processing chamber 30. Therefore, when the film forming process is repeated, the thickness of the deposit (film forming material) adhered to the inner surface of the processing chamber 30 increases. Here, when the thickness of the deposit reaches a predetermined thickness, the cleaning process S260 described later is performed. Specifically, the film thickness that increases each time the film forming process is performed once is obtained in advance, and it is determined whether the film thickness (accumulated film thickness) after performing the film forming process multiple times has reached a predetermined thickness (S240). In S240, when it is determined that the film thickness after performing the film forming process multiple times has reached the predetermined thickness, the cleaning process S260 is performed.
[0080] (Empty boat loading process) In the empty boat loading step S250, an empty boat 148 not loaded with wafers 200, i.e., a boat 148 not loaded with wafers 200, is elevated by a boat elevator and loaded (boat loaded) into the processing chamber 30. In this state, the seal cap 146 seals the lower end of the manifold 38 via an O-ring. Note that the empty boat 148 may be loaded with dummy wafers (not shown) instead of product wafers.
[0081] (Cleaning process) In the cleaning step S260, the inside of the processing chamber 30 to which the cleaning gas is supplied is divided into three or more zones in the gas flow direction of the cleaning gas, the inside of the processing chamber 30 is heated so that the temperature difference T2 between the lower zone 30C located on the upstream side in the gas flow direction in the processing chamber 30 and the middle zone 30B adjacent to the lower zone 30C is larger than the temperature difference T1 between the upper zone 30A located on the downstream side in the gas flow direction and the middle zone 30B adjacent to the upper zone 30A, and while maintaining the temperature state in the heated processing chamber 30, a cleaning gas is supplied into the processing chamber 30 to remove deposits including a film forming material that are attached to the inner surface of the processing chamber 30. To be more specific, first, the inside of the processing chamber 30 is evacuated by the vacuum pump 144 to a predetermined cleaning pressure (vacuum degree) and the inside of the processing chamber 30 is heated by the heater 60 to a predetermined cleaning temperature (S261). Note that S261 is an example of a heating step in the present disclosure.
[0082] Here, a method for heating the inside of the processing chamber 30 by the heater 60 will be described in detail. First, the inside of the processing chamber 30 is divided into three zones in the gas flow direction of the cleaning gas, and the inside of the processing chamber 30 is heated so that the temperature difference T2 between the lower zone 30C and the middle zone 30B in the processing chamber 30 is larger than the temperature difference T1 between the upper zone 30A and the middle zone 30B. Specifically, the heating temperature of the heater part 60A of the heater 60 corresponding to the upper zone 30A, the heating temperature of the heater part 60B of the heater 60 corresponding to the middle zone 30B, and the heating temperature of the heater part 60C of the heater 60 corresponding to the lower zone 30C are adjusted to heat the processing chamber 30 so that the temperature difference T2 is larger than the temperature difference T1. Note that the temperature difference T2 is preferably set to 5 to 50 times the temperature difference T1. Furthermore, when the processing chamber 30 is heated, the inside of the processing chamber 30 may be heated so that the temperature of the lower zone 30C in the processing chamber 30 becomes lower than the temperature of the upper zone 30A. Furthermore, when heating the processing chamber 30, the processing chamber 30 may be heated so that the temperature of the lower zone 30C in the processing chamber 30 becomes lower than the temperature of the middle zone 30B. That is, the processing chamber 30 is heated so that the temperature of the zone located on the upstream side in the gas flow direction in the processing chamber 30 becomes lower than the temperature of the zone located on the downstream side in the gas flow direction in the processing chamber 30. Also, the processing chamber 30 may be heated so that the temperature of the zone located on the upstream side in the gas flow direction in the processing chamber 30 becomes lower than the temperature of the zone located on the midstream side in the gas flow direction in the processing chamber 30.
[0083] Next, the rotation mechanism starts to rotate the boat 148. In the present disclosure, the boat 148 does not necessarily have to be rotated.
[0084] Next, while maintaining the temperature state in the heated processing chamber 30 (a state in which the temperature difference T2 is larger than the temperature difference T1), a cleaning gas is supplied into the processing chamber 30 to remove deposits including a film forming material that are attached to the inner surface of the processing chamber 30. Specifically, while maintaining the inside of the processing chamber 30 at a predetermined cleaning temperature and a predetermined cleaning pressure, the supply of the cleaning gas into the processing chamber 30 is started. The cleaning gas supplied from the cleaning gas supply source 132 into the gas supply pipe 90 and the gas supply pipe 91 by opening the valves 104 and 124 and the valves 105 and 125 is controlled to a predetermined flow rate by the MFC 114 and the MFC 115, respectively, and then supplied from the nozzles 80 and 81 into the processing chamber 30 via the gas supply pipe 94 and the gas supply pipe 91, respectively. At the same time, the cleaning gas supplied from the cleaning gas supply source 132 into the gas supply pipes 96 and 97 by opening the valves 106 and 126 and the valves 107 and 127 is controlled to a predetermined flow rate by the MFCs 116 and 117, respectively, and then passed through the gas supply pipes 96 and 97 and is supplied into the processing chamber 30 from the nozzles 82 and 83, respectively (S262). Note that S262 is an example of a supply step of the present disclosure.
[0085] The supply amount of the cleaning gas may be controlled so that the etching rate (etching speed) of the deposits adhering to the inner surface of the processing chamber 30 is lower on the upstream side of the gas flow direction in the processing chamber 30 (in other words, the lower side (lower zone 30C) of the processing chamber 30) than on the downstream side of the gas flow direction in the processing chamber 30 (in other words, the upper side (upper zone 30A) of the processing chamber 30). Specifically, the supply ratio of the cleaning gas of the nozzles 81 and 83 that supply the cleaning gas to the processing chamber 30 from the midstream side of the gas flow direction in the processing chamber 30 (in other words, the middle side (middle zone 30B) of the processing chamber 30) or the upstream side, relative to the nozzles 80 and 82 that supply the cleaning gas to the processing chamber 30 from the upstream side of the gas flow direction, can be adjusted to make the etching rate of the deposits lower on the lower side of the processing chamber 30 than on the upper side of the processing chamber 30. Also, the supply amount of the cleaning gas may be such that the etching rate of the deposits is substantially the same on the upper side of the processing chamber 30 and the middle side of the processing chamber 30.
[0086] At this time, the inert gas supplied into the processing chamber 30 functions as a dilution gas that dilutes the cleaning gas, or as a carrier gas that promotes diffusion into the processing chamber 30. By controlling the supply flow rate of the inert gas, the concentration and diffusion rate of the cleaning gas can be controlled.
[0087] The cleaning gas supplied into the processing chamber 30 rises in the inner pipe 34 (inside the processing chamber 30), flows out from the upper end opening of the inner pipe 34 into the cylindrical space 37, flows down inside the cylindrical space 37, and is exhausted from the exhaust pipe 141. When the cleaning gas passes through the processing chamber 30, it comes into contact with deposits (in this embodiment, a nitride film, etc. Here, the nitride film is, for example, a silicon nitride film, etc.) accumulated in the processing chamber 30, and removes the deposits by a thermochemical reaction. That is, the cleaning gas that is heated and activated becomes an etching species, and etches and removes the silicon nitride film, etc., as deposits accumulated in the processing chamber 30. In this embodiment, the nozzles 80 to 84 that supply the film forming gas into the processing chamber 30 are used as nozzles that supply the cleaning gas into the processing chamber 30. With this configuration, the silicon nitride film that is attached to the nozzles 80 to 84 can also be efficiently removed. When a preset processing time has elapsed and removal of the silicon nitride film and the like is completed, the valves 104 to 107 and the valves 124 to 127 are closed, and the supply of the cleaning gas into the processing chamber 30 is stopped.
[0088] Then, the valves 108, 128, 109, and 129 are left open, and the supply of the inert gas into the processing chamber 30 is continued while the processing chamber 30 is evacuated, thereby purging the processing chamber 30 (S263).
[0089] The processing conditions for the cleaning step (S260) according to this embodiment are as follows: Cleaning temperature: 300°C to 500°C (preferably around 350°C to 450°C) Cleaning gas supply flow rate: 1sccm to 20000sccm (preferably 1sccm to 10000sccm Cleaning pressure: 1Pa~60000Pa (preferably 5000Pa~20000Pa) Examples are given below.
[0090] As the cleaning gas, it is preferable to use a gas containing a halogen element, specifically, a gas containing a fluorine element. 2, H.F., N.F. 3 , C.F. 4 The cleaning gas includes F 2 , H.F., N.F. 3 , C.F. 4 In the present disclosure, for example, NF 3 An example using gas will be described.
[0091] (Pre-coating process) In the pre-coating process S270, the inside of the processing chamber 30 is heated, and a processing gas is supplied into the processing chamber 30 to perform a pre-coating process for forming a film on the inner surface of the processing chamber 30. To be more specific, immediately after the cleaning process S260 is completed, while an empty boat 148 not loaded with wafers 200 is still loaded (boat loaded) into the processing chamber 30, the inside of the processing chamber 30 is evacuated by the vacuum pump 144 to a predetermined pre-coating pressure (vacuum level), and the inside of the processing chamber 30 is heated by the heater 60 to a predetermined cleaning temperature (S271). Then, the rotation mechanism starts to rotate the boat 148. The pre-coating temperature may be set lower than the film-forming temperature in the film-forming process S220.
[0092] Then, supply of the first process gas into the process chamber 30 is started (S272). The first process gas supplied from the first process gas supply source 130 into the gas supply pipes 90 and 91 by opening the valves 100 and 120 and the valves 101 and 121 is controlled to a predetermined flow rate by the MFCs 110 and 111, respectively, and then supplied from the nozzles 80 and 81 into the process chamber 30. At this time, the inert gas supplied into the process chamber 30 functions as a dilution gas that dilutes the first process gas, or as a carrier gas that promotes diffusion into the process chamber 30.
[0093] The first process gas supplied into the process chamber 30 rises in the inner pipe 34 (inside the process chamber 30), flows out from the upper end opening of the inner pipe 34 into the cylindrical space 37, flows down the cylindrical space 37, and is then exhausted from the exhaust pipe 141. The first process gas comes into contact with the inner wall of the process chamber 30 and the surface of the boat 148 while passing through the process chamber 30. At this time, when DCS gas is used as the first process gas, a silicon layer (Si layer) that is a silicon-containing layer having a thickness of less than one atomic layer to several atomic layers is formed on these surfaces. At this time, the maximum pressure in the process chamber 30 when the first process gas is supplied may be made higher than the maximum pressure in the process chamber 30 in the film forming step S220. After a preset process time has elapsed and the formation of the silicon layer is completed, the valves 100 and 120 as well as the valves 101 and 121 are closed to stop the supply of the first process gas into the process chamber 30.
[0094] Then, the valves 108, 128, 109, and 129 are left open, and the supply of the inert gas into the processing chamber 30 is continued while the processing chamber 30 is evacuated, thereby purging the processing chamber 30 (S273).
[0095] Then, the supply of the second process gas into the process chamber 30 is started (S274). The second process gas supplied from the second process gas supply source 131 into the gas supply pipes 92 and 93 by opening the valves 102 and 122 and the valves 103 and 123 is controlled to a predetermined flow rate by the MFCs 112 and 113, respectively, and then supplied from the nozzles 82 and 83 into the process chamber 30. At this time, the inert gas supplied into the process chamber 30 functions as a dilution gas that dilutes the second process gas, or as a carrier gas that promotes diffusion into the process chamber 30.
[0096] The second process gas supplied into the process chamber 30 rises in the inner pipe 34 (inside the process chamber 30), flows out from the upper end opening of the inner pipe 34 into the cylindrical space 37, flows down through the cylindrical space 37, and is then exhausted from the exhaust pipe 141. When passing through the process chamber 30, the second process gas comes into contact with the inner surface of the process chamber 30 and the silicon layer formed on the surface of the boat 148. NH 3When a gas is used, the silicon layer is nitrided to form a silicon nitride layer (SiN layer) of less than one atomic layer to several atomic layers. At this time, the maximum pressure in the processing chamber 30 when the second processing gas is supplied may be higher than the maximum pressure in the processing chamber 30 in the film forming step S220. When a preset processing time has elapsed and the nitridation of the silicon nitride layer is completed, the valves 102 and 122 as well as the valves 103 and 123 are closed to stop the supply of the second processing gas into the processing chamber 30.
[0097] Then, the valves 108, 128, 109, and 129 are left open, and the supply of the inert gas into the processing chamber 30 is continued while the processing chamber 30 is evacuated, thereby purging the processing chamber 30 (S275).
[0098] The above steps S272 to S275 constitute one cycle, and by performing this cycle one or more times, a silicon nitride film (pre-coat film) with a predetermined thickness is formed on the inner surface of the processing chamber 30 and the surface of the boat 148 (S276). It is preferable to repeat the above cycle multiple times. In addition, when a silicon-containing gas is used as the first process gas and a nitrogen-containing gas is used as the second process gas, the supply amounts of the first process gas and the second process gas may be adjusted so that the ratio of silicon (Si) contained in the pre-coat film is equal to or greater than the ratio of silicon (Si) contained in the silicon nitride film formed on the wafer 200 in the film formation process S220.
[0099] The processing conditions for the pre-coating step (S270) according to this embodiment are as follows: Precoat temperature: 600°C to 850°C (preferably around 650°C to 800°C) First process gas supply flow rate: 10 sccm to 2000 sccm (preferably 50 sccm to 200 sccm) Second process gas supply flow rate: 100 sccm to 10,000 sccm (preferably 500 sccm to 2,000 sccm) Film forming pressure: 1 Pa to 2666 Pa (preferably less than 133 Pa) By maintaining each processing condition constant at a certain value within each range, a silicon nitride film (pre-coat film) having a thickness of, for example, 10 to 100 nm is formed on the inner surface of the processing chamber 30 and the surface of the boat 148.
[0100] After the above cycle is repeated a predetermined number of times to deposit a silicon nitride film (pre-coat film) with a predetermined thickness, the valves 108 and 128, as well as the valves 109 and 129, are left open, and the supply of inert gas into the processing chamber 30 is continued while the processing chamber 30 is evacuated, thereby purging the processing chamber 30. After the gas inside the processing chamber 30 has been replaced with the inert gas, the opening of the APC valve 143 is adjusted to return the pressure inside the processing chamber 30 to normal pressure. In addition, the power supply to the heater 60 is stopped, and the temperature inside the processing chamber 30 is lowered to a predetermined temperature (boat removal temperature) (S277).
[0101] In addition, although an example of forming the pre-coat film by a cycle process is shown here, the present invention is not limited to this. The pre-coat film may be formed by a CVD film formation process having a timing in which the first process gas and the second process gas are simultaneously supplied.
[0102] (Empty boat removal process) In the empty boat unloading step S280, the empty boat is unloaded to the outside of the reaction tube 32. Specifically, after the pre-coating step S270 is completed, the rotation of the boat 148 by the rotation mechanism is stopped, the seal cap 146 is lowered by the boat elevator to open the lower end of the manifold 38, and the empty boat 148 is unloaded (boat unloaded) from the lower end of the manifold 38 to the outside of the reaction tube 32. Thereafter, the above-mentioned loading step S210 and film forming step S220 are sequentially performed.
[0103] <Program> The program according to an embodiment of the present disclosure is executed by the controller 70 as a computer. a heating step of dividing the inside of the processing chamber 30 into which the cleaning gas is supplied into three or more zones in the gas flow direction, and heating the inside of the processing chamber 30 so that a temperature difference (T2) between a zone (lower zone 30C) located on the upstream side in the gas flow direction in the processing chamber 30 and a zone (middle zone 30B) adjacent to the zone is greater than a temperature difference (T1) between a zone (upper zone 30A) located on the downstream side in the gas flow direction and a zone (middle zone 30B) adjacent to the zone; a supply step of supplying a cleaning gas into the processing chamber 30 while maintaining the temperature state in the processing chamber 30 heated in the heating step; This is a program that executes the above.
[0104] Next, the operation and effects of this embodiment will be described. In the film formation process immediately after cleaning, a phenomenon occurs in which the thickness (film thickness) of the film formed on the wafer 200 becomes thin (so-called film thickness drop phenomenon). This occurs because fluorine (F) of the fluorine-containing gas used in cleaning remains in the processing chamber 30. Specifically, the cleaning gas reacts with the deposits attached to the inner surface of the processing chamber 30, and the components of the cleaning gas are discharged to the outside of the reaction tube 32 together with the components of the deposits. In this reaction tube 32, there are places where the deposits are thick and places where they are thin, and the supply amount of the cleaning gas is adjusted according to the thick parts. For this reason, in the places where the deposits are thin, the deposits disappear during cleaning, and the components of the cleaning gas remain adsorbed without being discharged, or the components of the cleaning gas react with the surface of a member (e.g., boat 148) placed in the reaction tube 32, and the components of the cleaning gas remain on the surface of the member placed in the reaction tube 32. In this way, the fluorine, which is a component of the cleaning gas remaining in the reaction tube 32, is dissolved in the film-forming gas (e.g., DCS gas, NH 3The reaction gas reacts with the gas (at least one of the gases). This reduces the amount of deposition gas that reaches the wafer 200. As a result, the thickness of the film deposited on the wafer 200 becomes thinner. This phenomenon of the film thickness becoming thinner is noticeable when the deposition gas is supplied from the lower side to the upper side of the reaction tube 32. For this reason, there is a demand in the market for a production process that suppresses the film thickness drop phenomenon from occurring on the wafer 200 in the deposition process immediately after cleaning. In other words, there is a demand for uniform processing for each wafer 200. For this reason, in the cleaning process of this embodiment, the inside of the processing chamber 30 is divided into three or more zones in the gas flow direction, the inside of the processing chamber 30 is heated so that the temperature difference T2 between the lower zone 30C and the adjacent middle zone 30B in the processing chamber 30 is larger than the temperature difference T1 between the upper zone 30A and the adjacent middle zone 30B, and the cleaning gas is supplied into the processing chamber 30 while maintaining the temperature state. As a result, the cleaning speed (cleaning amount) in the lower zone 30C in the processing chamber 30 becomes slower than the cleaning speeds (cleaning amounts) in the upper zone 30A and the middle zone 30B. That is, by lowering the temperature of the lower zone 30C of the processing chamber 30, the consumption amount (reaction amount, decomposition amount, etc.) of the cleaning gas in the lower zone 30C can be reduced. As a result, the amount of fluorine element generated in the lower zone 30C of the processing chamber 30 can be reduced, and the remaining fluorine element after cleaning can be suppressed. Moreover, by setting the above temperature condition (T2>T1), it becomes possible to stably supply unreacted cleaning gas to the middle zone 30B and the upper zone 30A in the processing chamber 30. This improves the cleaning uniformity in the gas flow direction in the processing chamber 30. As a result, film formation inhibition factors in the next film formation process are reduced, and the film thickness drop phenomenon occurring on the wafer 200 can be suppressed even immediately after cleaning. In other words, the film thickness of the wafer 200 can be stabilized. Therefore, the processing for each wafer 200 can be made closer to uniformity.
[0105] By using a halogen-based gas as the cleaning gas, it is possible to shorten the time required to clean the deposits adhering to the inner surface of the processing chamber 30 .
[0106] In addition, the cleaning gas may be a fluorine-containing gas, specifically, F 2 , H.F., N.F. 3 , C.F. 4 By using a gas containing at least one of the above, it is possible to shorten the cleaning time for a film containing Si and N (silicon nitride film).
[0107] In this embodiment, the nozzle 80 and the nozzle 82 are capable of supplying the cleaning gas to the processing chamber 30 from the lower zone 30C toward the upper zone 30A of the processing chamber 30. This allows cleaning from the upstream to the downstream in the gas flow direction of the processing chamber 30. In other words, cleaning from the lower side to the upper side of the processing chamber 30 is possible.
[0108] In this embodiment, the nozzle 81 and the nozzle 83 are capable of supplying the cleaning gas to the processing chamber 30 in the middle zone 30B (midstream side) and the upper zone 30A (downstream side) of the processing chamber 30. Therefore, unreacted cleaning gas can be reliably supplied to the middle zone 30B and the upper zone 30A as well. This makes it possible to perform substantially uniform cleaning from the upstream side to the downstream side in the gas flow direction of the processing chamber 30. In addition, it is possible to improve the controllability of the cleaning atmosphere (conditions) from the upstream side to the downstream side in the gas flow direction in the processing chamber 30, and to suppress F residue from the upstream side to the downstream side in the gas flow direction.
[0109] In the precoating process of this embodiment, the precoating process is performed under conditions that form a silicon nitride film with a higher silicon content than the silicon content of the silicon nitride film formed in the film formation process. Specifically, the supply ratio of the first process gas in the precoating process is higher than the supply ratio of the first process gas during the film formation process. Here, the supply ratio is the supply ratio of the first process gas to the second process gas, and includes at least one of the supply flow rate and the supply time of the gas. For example, the supply flow rate of the first process gas in the precoating process is made higher than the supply flow rate of the first process gas during the film formation process. By supplying the first process gas and the second process gas in this manner, it is possible to remove fluorine remaining in the reaction tube 32, and the decrease in the film thickness during the film formation process can be suppressed. The first process gas used in the precoating process may be the same gas as the first process gas used in the film formation process, or a gas with a different molecular structure may be used.
[0110] In addition, in the pre-coating process of this embodiment, the pre-coating process is performed at a lower pressure than the film forming process, so that the exposure amount (contact time) of the first process gas to the residual F can be increased. As a result, the residual F reacts with DCS and is discharged. As a result, the amount of F remaining in the process chamber 30 can be reduced, and the film thickness drop rate can be improved. On the other hand, in the film formation process, the pressure is increased compared to the pre-coating process, so that the amount of exposure (contact time) between the first process gas and the residual F can be reduced. Even if F remains, the film thickness drop phenomenon during wafer processing can be suppressed.
[0111] FIG. 6 shows a graph showing the relationship between the cumulative film thickness (accumulated thickness of deposits) in the processing chamber 30 and the film thickness variation rate of each of the zones 30A-30C when the cleaning method of the comparative example is performed. In this comparative example cleaning method, the temperature of each of the zones 30A-30C is set to the same temperature. FIG. 7 shows a graph showing the relationship between the cumulative film thickness in the processing chamber 30 and the film thickness variation rate of each of the zones 30A-30C when the cleaning method of the embodiment is performed. In the cleaning method shown in FIG. 7, the temperature of each of the zones 30A-30C is controlled so that the temperature difference T2>the temperature difference T1, so that the film thickness variation rate of each of the zones 30A-30C relative to the cumulative film thickness in the processing chamber 30 is small. That is, it can be seen that in the cleaning method of the embodiment, the processing chamber 30 can be uniformly cleaned from the upstream to the downstream in the gas flow direction, and further, F residue on the upstream side of the gas flow direction is suppressed.
[0112] In the above embodiment, the DCS gas is used as the first process gas, but the present disclosure is not limited to this. For example, monochlorosilane (SiH 3 Cl, abbreviation: MCS) gas, trichlorosilane (SiHCl 3 (TCS) gas, tetrachlorosilane (SiCl 4 , abbreviation: STC) gas, hexachlorodisilane gas (Si 2 Cl 6 , abbreviation: HCDS) gas, octachlorotrisilane (Si 3 Cl 8 (abbreviation: OCTS) gas or other chlorosilane gases can be used. As the source gas, one or more of these can be used.
[0113] In addition to chlorosilane gas, other gases such as tetrafluorosilane (SiF 4 ) gas, difluorosilane (SiH 2 F 2 ) gas, tetrabromosilane (SiBr 4 ) gas, dibromosilane (SiH 2 Br 2) gas, tetraiodosilane (SiI 4 ) gas, diiodosilane (SiH 2 I 2 As the source gas, one or more of these can be used.
[0114] In addition to these, the source gas may be, for example, a gas containing Si and an amino group, i.e., an aminosilane gas. An amino group is a monovalent functional group obtained by removing hydrogen (H) from ammonia, a primary amine, or a secondary amine, and is represented by -NH 2 ,-NHR,-NR 2 Here, R represents an alkyl group, and -NR 2 The two R's may be the same or different.
[0115] The source gas is, for example, tetrakis(dimethylamino)silane (Si[N(CH 3 ) 2 ] 4 , abbreviation: 4DMAS) gas, tris(dimethylamino)silane (Si[N(CH 3 ) 2 ] 3 H, abbreviation: 3DMAS) gas, bis(diethylamino)silane (Si[N(C 2 H 5 ) 2 ] 2 H 2 , abbreviation: BDEAS) gas, bis(tertiary butyl amino)silane (SiH 2 [NH(C 4 H 9 )] 2 (BTBAS) gas, (diisopropylamino)silane (SiH 3 [N(C 3 H 7 ) 2 As the source gas, one or more of these can be used.
[0116] In the above embodiment, the second process gas is NH 3 Although an example using a gas has been described, the present disclosure is not limited to this. As the second process gas (reactive gas), for example, diazene (N 2 H 2 ) gas, hydrazine (N 2 H 4 ) Gas, N 3 H 8 As the reaction gas, one or more of these gases can be used.
[0117] In addition to these, the reactive gas may be, for example, a nitrogen (N), carbon (C) or hydrogen (H)-containing gas. The N, C and H-containing gas may be, for example, an amine-based gas or an organic hydrazine-based gas. The N, C and H-containing gas may be an N-containing gas, a C-containing gas, an H-containing gas or an N and C-containing gas.
[0118] The reactive gas may be, for example, monoethylamine (C 2 H 5 NH 2 , abbreviation: MEA) gas, diethylamine ((C 2 H 5 ) 2 NH, abbreviation: DEA) gas, triethylamine ((C 2 H 5 ) 3 N, abbreviated as TEA) gas and other ethylamine gases, and monomethylamine (CH 3 NH 2 , abbreviation: MMA) gas, dimethylamine ((CH 3 ) 2 NH (abbreviation: DMA) gas, trimethylamine ((CH 3 ) 3 Methylamine gases such as N, abbreviated as TMA, and monomethylhydrazine ((CH 3 )HN 2 H 2 , abbreviation: MMH) gas, dimethylhydrazine ((CH 3 ) 2 N 2 H 2, abbreviation: DMH) gas, trimethylhydrazine ((CH 3 ) 2 N 2 (CH 3 As the reactive gas, one or more of these can be used.
[0119] In the above-described embodiment, an example of film formation using a substrate processing apparatus that is a batch-type vertical apparatus that processes multiple substrates at a time has been described. However, the present disclosure is not limited to this and can also be suitably applied to film formation using a single-wafer type substrate processing apparatus that processes one or several substrates at a time.
[0120] In addition, in the above embodiment, an inert gas is supplied to the processing chamber 30 during the substrate processing step, but the present disclosure is not limited to this configuration. For example, the controller 70 may appropriately adjust the supply amount of the inert gas when purging the processing chamber 30 or to a degree to which the gas is diluted.
[0121] Furthermore, in the above embodiment, the inside of the processing chamber 30 is divided into three zones, but the present disclosure is not limited to this configuration. The inside of the processing chamber 30 may be divided into three or more zones. For example, FIG. 8 shows a substrate processing apparatus 150 in which the inside of the processing chamber 30 is divided into five zones. In this substrate processing apparatus 150, the heater 154 of the processing furnace 152 is composed of five heater parts 154A to 154E, and temperature sensors are arranged in parts corresponding to the heat generating areas of each heater part. These heater parts 154A to 154E and each temperature sensor are electrically connected to the controller 70. When such a substrate processing apparatus 150 is used, cleaning can be performed more uniformly from the upstream side to the downstream side in the gas flow direction of the processing chamber 30. In FIG. 8, the vicinity of the heater part 154E is located on the upstream side of the gas flow, the vicinity of the heater part 154A is located on the downstream side of the gas flow, and the vicinity of the heater part 154C is located on the midstream side of the gas flow. [Explanation of symbols]
[0122] 10 Substrate processing equipment 30 Processing Room 30A Upper Zone (Zone located downstream in the gas flow direction) 30B Middle zone (zone located on the midstream side of the gas flow direction) 30C Lower Zone (Zone located on the upstream side of the gas flow direction) 40 Processing gas supply system 50 Cleaning gas supply system 60 Heater 60A heater section 60B Heater part 60C heater section 70 Controller (control unit) 80 Nozzles 150 Substrate Processing Equipment 152 Processing furnace 154 Heater 200 wafers S210 Loading process S220 Film formation process S230 Unloading process S260 Cleaning process S270 Pre-coating process
Claims
1. A method for cleaning a processing chamber for performing a film formation process on a substrate, comprising the steps of: a heating step of dividing the inside of the processing chamber into which the cleaning gas is supplied into three or more zones in a gas flow direction, and heating the inside of the processing chamber so that a temperature difference between a zone located on the upstream side in the gas flow direction in the processing chamber and a zone adjacent to the zone is larger than a temperature difference between a zone located on the downstream side in the gas flow direction and a zone adjacent to the zone; a supply step of supplying the cleaning gas into the processing chamber after the heating step; having In the heating step, the processing chamber is heated so that an etching rate of deposits adhering to the inner surface of the processing chamber is lower on the upstream side of the gas flow direction in the processing chamber than on the downstream side of the gas flow direction in the processing chamber.
2. 2. The cleaning method according to claim 1, wherein in the heating step, the inside of the processing chamber is heated so that a temperature of a zone located upstream in the gas flow direction in the processing chamber becomes lower than a temperature of a zone located downstream in the gas flow direction.
3. 3. The cleaning method according to claim 1, wherein in the heating step, the inside of the processing chamber is heated so that a temperature of a zone located upstream in the gas flow direction within the processing chamber is lower than a temperature of a zone located midstream in the gas flow direction.
4. 4. The cleaning method according to claim 1, wherein in the heating step, the processing chamber is heated so that an etching rate of deposits adhering to an inner surface of the processing chamber is substantially the same on a downstream side in the gas flow direction within the processing chamber and a midstream side in the gas flow direction within the processing chamber.
5. The deposits adhering to the inner surface of the processing chamber include a nitride film; 5. The cleaning method according to claim 1, wherein the cleaning gas contains a halogen element.
6. The deposits adhering to the inner surface of the processing chamber include a film having Si and N, 6. The cleaning method according to claim 1, wherein the cleaning gas contains a fluorine element.
7. The cleaning gas contains F 2 , H.F., N.F. 3 and C.F. 4 The cleaning method according to claim 1 , further comprising at least one selected from the group consisting of:
8. 8. The cleaning method according to claim 1, wherein the cleaning gas is supplied from an upstream side to a downstream side of the processing chamber.
9. A gas supply nozzle capable of supplying a cleaning gas is connected to the upstream side of the processing chamber, 9. The cleaning method according to claim 1, wherein the cleaning gas is supplied to an upstream side of the processing chamber through the gas supply nozzle.
10. a second gas supply nozzle capable of supplying the cleaning gas to a downstream side of the processing chamber from a first gas supply nozzle serving as the gas supply nozzle is connected to the processing chamber; 10. The cleaning method according to claim 9, wherein the cleaning gas is supplied to an upstream side of the processing chamber through the first gas supply nozzle, and is also supplied to a downstream side of the processing chamber with respect to the first gas supply nozzle through the second gas supply nozzle.
11. the second gas supply nozzle has a portion extending from an upstream side to a downstream side of the processing chamber and a plurality of injection ports formed at intervals in a direction extending in the extending portion, 11. The cleaning method according to claim 10, wherein the cleaning gas is supplied to the processing chamber through a plurality of injection ports from an extending portion of a second gas supply nozzle.
12. 12. The cleaning method according to claim 1, further comprising a pre-coating process for performing a pre-coating process after the supplying process, in which a first gas containing a first element and a second gas containing a second element are supplied to form a film on an inner surface of the processing chamber in which a ratio of the first element is equal to or greater than a ratio of the first element in a film formed on a substrate in the film forming process.
13. 13. The cleaning method according to claim 12, wherein the pressure in the processing chamber when the pre-coating processing is performed is set to be lower than the pressure in the processing chamber when the film forming processing is performed.
14. a loading step of loading a substrate into a processing chamber; a film formation process for performing a film formation process by heating the inside of the processing chamber and supplying a processing gas into the processing chamber to form a film on the substrate; a carrying-out step of carrying out the processed substrate from the processing chamber; a removing step of dividing the inside of the processing chamber into which a cleaning gas is supplied into three or more zones in a gas flow direction of the cleaning gas, heating the inside of the processing chamber so that a temperature difference between a zone located on the upstream side in the gas flow direction in the processing chamber and a zone adjacent to the zone is larger than a temperature difference between a zone located on the downstream side in the gas flow direction and a zone adjacent to the zone, and supplying the cleaning gas into the heated processing chamber to remove deposits including a film-forming material that are deposited on an inner surface of the processing chamber; having A method for manufacturing a semiconductor device, in which the removal process heats the processing chamber so that an etching rate of the deposits adhering to the inner surface of the processing chamber is lower on the upstream side of the gas flow direction in the processing chamber than on the downstream side of the gas flow direction in the processing chamber.
15. a processing chamber for processing a substrate; a process gas supply system for supplying a process gas into the process chamber; a cleaning gas supply system for supplying a cleaning gas into the processing chamber; a heating unit capable of dividing the inside of the processing chamber into three or more zones in a gas flow direction of the cleaning gas and heating each zone individually; a control unit that controls the heating unit, the processing gas supply system, and the cleaning gas supply system; Equipped with the control unit is configured to be capable of controlling the heating unit to heat the inside of the processing chamber so that an etching rate of deposits adhering to an inner surface inside the processing chamber is lower on the upstream side in the gas flow direction inside the processing chamber than on the downstream side in the gas flow direction inside the processing chamber and a temperature difference between a zone located on the upstream side in the gas flow direction inside the processing chamber and a zone adjacent to the zone is larger than a temperature difference between a zone located on the downstream side in the gas flow direction and a zone adjacent to the zone, and is configured to be capable of controlling the cleaning gas supply system to supply the cleaning gas into the heated processing chamber. Substrate processing equipment.
16. On the computer, a heating step of dividing a processing chamber into which a cleaning gas is supplied into three or more zones in a gas flow direction, and heating the processing chamber so that a temperature difference between a zone located on the upstream side in the gas flow direction in the processing chamber and a zone adjacent to the zone is larger than a temperature difference between a zone located on the downstream side in the gas flow direction and a zone adjacent to the zone; a supply step of heating the processing chamber so that an etching rate of deposits adhering to an inner surface of the processing chamber is lower on an upstream side in the gas flow direction in the processing chamber than on a downstream side in the gas flow direction in the processing chamber, and supplying the cleaning gas into the heated processing chamber; A program that executes the following.
Citation Information
Patent Citations
Substrate processing apparatus and semiconductor device manufacturing method
JP2012216696A
Substrate processing device
JP2014209633A
Semiconductor device manufacturing method and substrate processing apparatus
WO2007116768A1
Substrate processing apparatus and semiconductor device manufacturing method
WO2008016143A1