Blocked polyisocyanate composition, resin composition, resin film and laminate

The block polyisocyanate composition addresses the challenges of polyurethane resin paints by providing low-temperature curability and water-based dispersibility, enhancing storage stability and water resistance in resin films.

JP7581517B2Active Publication Date: 2024-11-12ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023532030
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-19
Filing Date
2022-06-29
Publication Date
2024-11-12
Estimated Expiration
2042-06-29

AI Technical Summary

Technical Problem

Conventional polyurethane resin paints using polyisocyanates face challenges such as inconvenience due to two-component mixing, rapid gelling, difficulty in automatic painting, incompatibility with water-based paints, and the need for high-temperature baking, which limits their application and reduces work efficiency.

Method used

A block polyisocyanate composition comprising components (A) and (B) with specific nonionic hydrophilic group contents and differing blocked isocyanate structures, allowing for good dispersibility in water-based compositions and curability at low temperatures, suppressing gas generation and maintaining water resistance.

Benefits of technology

The composition achieves excellent dispersibility and curability in water-based paints at low temperatures, reducing gas generation during storage, and ensuring high water resistance when formed into a resin film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581517000001
    Figure 0007581517000001
  • Figure 0007581517000002
    Figure 0007581517000002
  • Figure 0007581517000003
    Figure 0007581517000003
Patent Text Reader

Abstract

The present invention provides a block polyisocyanate composition or the like that contains a block polyisocyanate component (A) and a block polyisocyanate component (B). When the contained amount of nonionic hydrophilic groups in the block polyisocyanate component (A) is represented as (a) mass% and the contained amount of nonionic hydrophilic groups in the block polyisocyanate component (B) is represented as (b) mass%, the relation of 0≤(b)<(a) is satisfied.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a blocked polyisocyanate composition, a resin composition, a resin film, and a laminate. [Background technology]

[0002] Conventionally, polyurethane resin paints have very good abrasion resistance, chemical resistance, and stain resistance. In particular, polyurethane resin paints using polyisocyanates obtained from aliphatic diisocyanates or alicyclic diisocyanates have even better weather resistance, and the demand for them is increasing. However, polyurethane resin paints are generally two-liquid, which makes their use extremely inconvenient. That is, ordinary polyurethane resin paints are composed of two components, polyol and polyisocyanate, and it is necessary to store the polyol and polyisocyanate separately and mix them when painting. In addition, once the two are mixed, the paint gels in a short time and becomes unusable. Because polyurethane resin paints have such problems, it is extremely difficult to use them for automatic painting in fields where line painting is performed, such as automobile painting or weak electric painting. In addition, isocyanates easily react with water, so they cannot be used with water-based paints such as electrodeposition paints. Furthermore, when paints containing isocyanates are used, it is necessary to thoroughly clean the painter and paint tank at the end of work, which significantly reduces work efficiency.

[0003] In order to improve the above-mentioned problems, it has been proposed to use a blocked polyisocyanate in which all active isocyanate groups are blocked with a blocking agent. This blocked polyisocyanate does not react with polyol at room temperature. However, by heating, the blocking agent dissociates, and the active isocyanate groups are regenerated and react with polyol to cause a crosslinking reaction, thereby improving the above-mentioned problems. Therefore, many blocking agents have been studied, and representative examples include phenol, methyl ethyl ketoxime, etc.

[0004] However, when using blocked polyisocyanates using these blocking agents, a high baking temperature of 140° C. or more is generally required. The need for baking at a high temperature is not only disadvantageous in terms of energy, but also requires the substrate to have heat resistance, which is a factor limiting its applications.

[0005] On the other hand, research has been conducted on low-temperature bake-type blocked polyisocyanates using active methylene compounds such as acetoacetate esters and malonic acid diesters. For example, Patent Documents 1 and 2 propose blocked polyisocyanate compositions that cure at 90°C.

[0006] In addition, from the viewpoint of protecting the global environment, there is an increasing need for aqueous resin compositions. In order to ensure dispersibility in aqueous resin compositions, for example, Patent Document 3 discloses a technique for improving dispersibility in aqueous resin compositions by modifying blocked polyisocyanate with a hydrophilic group. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2002-322238 A [Patent Document 2] JP 2006-335954 A [Patent Document 3] Patent No. 3947260 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the physical properties required for a blocked polyisocyanate include curability when baked at a low temperature of 90° C. or less, dispersibility in an aqueous resin composition, and storage stability as an aqueous resin composition, and it is very difficult to satisfy all of these requirements.

[0009] The present invention has been made in view of the above circumstances, and provides a blocked polyisocyanate composition which has good dispersibility in an aqueous resin composition, excellent curability and maintenance of curability (gel fraction retention) when baked at a low temperature of 90°C or less immediately after preparation of the aqueous resin composition and after storage, suppresses the amount of gas generated when stored as an aqueous resin composition, and has excellent water resistance when formed into a resin film, as well as a resin composition, a resin film, and a laminate which use the blocked polyisocyanate composition. [Means for solving the problem]

[0010] That is, the present invention includes the following aspects. (1) A blocked polyisocyanate composition comprising a blocked polyisocyanate component (A) and a blocked polyisocyanate component (B), When the nonionic hydrophilic group content of the blocked polyisocyanate component (A) is (a) mass %, and the nonionic hydrophilic group content of the blocked polyisocyanate component (B) is (b) mass %, the relationship of 0≦(b)<(a) is satisfied. death, The structure (Y) of the blocked isocyanate group of the blocked polyisocyanate component (B) is a structure represented by the following general formula (II), and contains 1 mol % or more of the structure represented by the following general formula (II-1) relative to 100 mol % of the structure represented by the following general formula (II): , blocked polyisocyanate composition 。

[0011] [ka]

[0012] (In general formula (II), R 21 、R 22 、R 23 、R 24 、R 25 and R 26 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bond.

[0013] [ka]

[0014] (In general formula (II-1), R 211 、R 212 , and R 213 Each of R is independently an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxy group and an amino group. 211 , R 212 and the R 213 The total number of carbon atoms in R is 3 to 20. 214 、R 215 and R 216 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bond.

[0015] (2) the nonionic hydrophilic group content (a) of the blocked polyisocyanate component (A) is 1.0 to 55.0 mass%, The blocked polyisocyanate component (B) has a nonionic hydrophilic group content (b) of 0 to 20.0 mass %, (a) / (b) is 100 / 0~60 / 40, and 2. The blocked polyisocyanate composition according to claim 1, wherein a mass ratio (A) / (B) of the component (A) to the component (B) is 1 / 99 to 99 / 1. (3) The blocked polyisocyanate composition according to (1) or (2), wherein the nonionic hydrophilic group content of the blocked polyisocyanate composition is 0.1 mass% or more and 25.0 mass% or less, based on the total mass of the solid content of the blocked polyisocyanate composition. (4) The blocked polyisocyanate composition according to any one of (1) to (3), wherein the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) and the structure (Y) of the blocked isocyanate group of the blocked polyisocyanate component (B) are different from each other. (5) The blocked polyisocyanate composition according to any one of (1) to (3), which satisfies 0<(b)<(a). (6) The curing temperatures at which the gel fraction in the resin film using each of the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) reaches 80 mass% or more are defined as (A T1 ) and (B T1 ), then (A T1 )>(B T1 ) relationship, The blocked polyisocyanate composition according to any one of (1) to (4), wherein the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are each mixed with an acrylic polyol having a hydroxyl group content of 4.5% by mass so that the ratio NCO / OH of the molar amount of isocyanate groups in the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) to the molar amount of hydroxyl groups in the acrylic polyol is 1.0, and the solid content is adjusted with butyl acetate to 50% by mass, and each of the adjusted solutions obtained is applied to a polypropylene plate so as to have a dry film thickness of 40 μm, and the resulting resin film is dried by heating at a temperature of 80° C. or higher in 5° C. increments for 30 minutes, and then the resulting resin film is immersed in acetone at 23° C. for 24 hours, and the gel fraction is expressed as a percentage obtained by dividing the mass of the undissolved portion by the mass before immersion. (7) The curing temperatures at which the gel fraction in the resin film using each of the blocked polyisocyanate components (A) and (B) reaches 80 mass% or more are defined as (A T2 ) and (B T2 ), then (A T2 )>(B T2 ) relationship, The blocked polyisocyanate composition according to any one of (1) to (4), wherein the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are each mixed with a polycaprolactone triol having a number average molecular weight of 850 so that a ratio NCO / OH of the molar amount of isocyanate groups in the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) to the molar amount of hydroxyl groups in the polycaprolactone triol is 1.0, and the solid content is adjusted with butyl acetate to 50 mass %, and each of the adjusted solutions obtained is applied to a polypropylene plate so as to have a dry film thickness of 40 μm, and the resulting resin film is dried by heating at a temperature of 80° C. or higher in 5° C. increments for 30 minutes. The gel fraction is expressed as a percentage obtained by dividing the mass of the undissolved portion by the mass before immersion when the resin film is immersed in acetone at 23° C. for 24 hours.

[0016] ( 8 In the general formula (II), 24 , R 25 and the above R 26 of which one is a hydrogen atom, Any of (1) through (7) 2. The blocked polyisocyanate composition according to claim 1 . ( 9 In the general formula (II-1),211 , R 212 and the R 213 The total number of carbon atoms is 4 to 20. Any of (1) through (8) 2. The blocked polyisocyanate composition according to claim 1 . ( 10 (1) to (5), wherein the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) is one or more structures selected from the group consisting of a structure represented by the following general formula (III) and a structure represented by the following general formula (IV), 9 ) The blocked polyisocyanate composition according to any one of the preceding claims.

[0017] [ka]

[0018] (In general formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. 31 , R 32 and the R 33 At least one of the R 34 , R 35 and the above R 36 At least one of the isocyanate groups is a hydrogen atom. The wavy lines represent the bond sites with the residues of polyisocyanate excluding the isocyanate groups.)

[0019] [ka]

[0020] (In general formula (IV), R 41 , R 42 and R 43are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bonding site with a residue of a polyisocyanate excluding an isocyanate group. ( 11 ) the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are derived from a polyisocyanate and a blocking agent, respectively; The polyisocyanate is a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates. 10 ) The blocked polyisocyanate composition according to any one of the preceding claims. ( 12 ) the average number of isocyanate groups of the polyisocyanate is 3.5 or more; ( 11 ) The blocked polyisocyanate composition according to claim 1. ( 13 ) the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) is the same as that of the blocked isocyanate group of the blocked polyisocyanate component (B). The above The blocked polyisocyanate composition according to any one of (1) to (3), which has the same structure as the structure (Y). ( 14 )(1)~( 13 2. A resin composition comprising the blocked polyisocyanate composition according to claim 1 and a polyvalent hydroxy compound. ( 15 )( 14 2. A resin film obtained by curing the resin composition described in claim 1. ( 16 ) on the substrate, ( 15 A laminate comprising one or more layers of the resin film according to The thickness of each of the resin films is from 1 μm to 50 μm. Effect of the Invention

[0021] According to the above aspect, it is possible to provide a blocked polyisocyanate composition that has good dispersibility in an aqueous resin composition, has excellent curability and maintenance of curability (gel fraction retention) when baked at a low temperature of 90°C or less immediately after preparation and after storage, has a suppressed amount of gas generation when stored as an aqueous resin composition, and has excellent water resistance when formed into a resin film. The resin composition of the above aspect contains the blocked polyisocyanate composition, has excellent curability when baked at a low temperature of 90°C or less immediately after preparation and after storage, has a suppressed amount of gas generation when stored, and has excellent water resistance when formed into a resin film. The resin film and laminate of the above aspect are obtained by curing the resin composition and have excellent water resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment. The present invention can be carried out with appropriate modifications within the scope of the gist of the present invention.

[0023] In this specification, the term "polyol" refers to a compound having two or more hydroxyl groups (-OH). As used herein, the term "polyisocyanate" refers to a reaction product in which multiple monomeric compounds having one or more isocyanate groups (-NCO) are bonded together.

[0024] In this specification, the term "structural unit" refers to a structure resulting from one molecule of a monomer in a structure constituting a polyisocyanate or a blocked polyisocyanate. For example, a structural unit derived from a malonic acid ester refers to a structure resulting from one molecule of a malonic acid ester in a blocked polyisocyanate. The structural unit may be a unit formed directly by a (co)polymerization reaction of a monomer, or may be a unit in which a part of the unit is converted into a different structure by treating the (co)polymer.

[0025] <Blocked polyisocyanate composition> The blocked polyisocyanate composition of the present embodiment contains a blocked polyisocyanate component (A) (hereinafter, may be simply referred to as “component (A)”) and a blocked polyisocyanate component (B) (hereinafter, may be simply referred to as “component (B)”).

[0026] The nonionic hydrophilic group content of the blocked polyisocyanate composition of this embodiment is 0.1% by mass or more and 25.0% by mass or less, preferably 1.0% by mass or more and 20.0% by mass or less, more preferably 3.0% by mass or more and 15.0% by mass or less, and even more preferably 5.0% by mass or more and 12.0% by mass or less, based on the total mass of the solid content of the blocked polyisocyanate composition. When the nonionic hydrophilic group content of the blocked polyisocyanate composition is within the above numerical range, the dispersibility of the blocked polyisocyanate composition, the amount of gas generated when stored as an aqueous coating composition, and the low-temperature curing property after storage tend to be good. The nonionic hydrophilic group content of the blocked polyisocyanate composition of the present embodiment can be calculated, for example, from the nonionic hydrophilic group contents in component (A) and component (B) and the mixing ratio of component (A) and component (B).

[0027] When the nonionic hydrophilic group content of component (A) is (a) mass %, and the nonionic hydrophilic group content of component (B) is (b) mass %, the relationship 0≦(b)<(a) is satisfied. In other words, it can also be said that the nonionic hydrophilic group content of component (A) is greater than the nonionic hydrophilic group content of component (B) and is a value exceeding 0.

[0028] The lower limit of the nonionic hydrophilic group content of component (A) is preferably 1.0 mass%, more preferably 4.0 mass%, further preferably 8.0 mass%, and particularly preferably 12.0 mass%, relative to the mass of the solid content of component (A), from the viewpoint of the aqueous dispersion stability of the blocked polyisocyanate composition. On the other hand, the upper limit of the nonionic hydrophilic group content of component (A) is preferably 55.0 mass%, more preferably 50.0 mass%, even more preferably 48.0 mass%, and particularly preferably 44.0 mass%, relative to the mass of the solid content of component (A), from the viewpoint of the water resistance of the resulting resin film. That is, the nonionic hydrophilic group content of component (A) is preferably 1.0 mass% or more and 55.0 mass% or less, more preferably 4.0 mass% or more and 50.0 mass% or less, even more preferably 8.0 mass% or more and 48.0 mass% or less, and particularly preferably 12.0 mass% or more and 44.0 mass% or less, based on the mass of the solid content of component (A). When the nonionic hydrophilic group content of component (A) is within the above numerical range, the water dispersibility of the resulting blocked polyisocyanate composition becomes better, and a homogeneous film tends to be obtained. Alternatively, from the viewpoint of suppressing a decrease in water resistance, the nonionic hydrophilic group content of component (A) is preferably from 1.0 to 10.0 mass%, more preferably from 1.0 to 9.0 mass%.

[0029] From the viewpoint of suppressing a decrease in the hardness and strength of the obtained resin film, the content of nonionic hydrophilic groups added to the blocked polyisocyanate contained in component (A), expressed as a molar ratio, relative to 100 mol% of the isocyanate groups in the raw material polyisocyanate, is preferably 2 mol% or more and 50 mol% or less, more preferably 4 mol% or more and 45 mol% or less, even more preferably 6 mol% or more and 40 mol% or less, even more preferably 8 mol% or more and 35 mol% or less, and most preferably 10 mol% or more and 30 mol% or less. Alternatively, from the viewpoint of suppressing a decrease in water resistance, the content of nonionic hydrophilic groups added to the blocked polyisocyanate contained in component (A), expressed as a molar ratio, is preferably from 2 mol % to 10 mol %, and more preferably from 4 mol % to 8 mol %, relative to 100 mol % of the isocyanate groups in the raw material polyisocyanate.

[0030] The lower limit of the nonionic hydrophilic group content of component (B) is not particularly limited, but from the viewpoint of the aqueous dispersion stability of the blocked polyisocyanate composition, the lower limit is preferably 0.0 mass%, more preferably 0.1 mass%, even more preferably 1.0 mass%, and particularly preferably 2.0 mass%, relative to the mass of the solid content of component (B). On the other hand, the upper limit of the nonionic hydrophilic group content of component (B) is preferably 20.0 mass%, more preferably 15.0 mass%, even more preferably 10.0 mass%, and particularly preferably 5.0 mass%, relative to the mass of the solid content of component (B), from the viewpoint of the water resistance of the resulting resin film. That is, the nonionic hydrophilic group content of component (B) is preferably from 0.0 mass% to 20.0 mass% relative to the mass of the solid content of component (B), more preferably from 0.1 mass% to 15.0 mass%, even more preferably from 1.0 mass% to 10.0 mass%, and particularly preferably from 2.0 mass% to 5.0 mass%. When the nonionic hydrophilic group content of component (B) is within the above range, the water dispersibility of the resulting blocked polyisocyanate composition tends to be better and the storage stability tends to be better.

[0031] From the viewpoint of suppressing a decrease in the hardness and strength of the obtained resin film, the content of the nonionic hydrophilic groups added to the blocked polyisocyanate, expressed as a molar ratio, relative to 100 mol% of the isocyanate groups in the raw material polyisocyanate, is preferably 0.00 mol% or more and 20.00 mol% or less, more preferably 0.25 mol% or more and 15.00 mol% or less, even more preferably 0.50 mol% or more and 10.00 mol% or less, even more preferably 0.75 mol% or more and 5.00 mol% or less, and most preferably 1.00 mol% or more and 3.00 mol% or less.

[0032] The nonionic hydrophilic group content of component (A) and component (B) can be obtained, for example, by calculating the ratio of the mass of the nonionic hydrophilic compound to the total mass of the solid content of each component as a percentage (mass %), assuming that all of the nonionic hydrophilic compound used has reacted with the isocyanate group of the polyisocyanate. The nonionic hydrophilic group contents of component (A) and component (B) can also be quantified by, for example, extracting and separating component (A) and component (B) in the blocked polyisocyanate composition with a polar solvent or the like, and subjecting the separated components to NMR measurement.

[0033] The structure (X) of the blocked isocyanate group of component (A) (hereinafter may be simply referred to as the "blocked isocyanate structure (X)") may be the same as or different from the structure (Y) of the blocked isocyanate group of component (B) (hereinafter may be simply referred to as the "blocked isocyanate structure (Y)").

[0034] Each of the components (A) and (B) was mixed with an acrylic polyol having a hydroxyl group content of 4.5% by mass so that the ratio NCO / OH of the molar amount of the isocyanate group of each of the components (A) and (B) to the molar amount of the hydroxyl group of the acrylic polyol was 1.0, and the solid content was adjusted with butyl acetate so that the solid content was 50% by mass. Each of the adjusted solutions obtained was applied to a polypropylene plate so that the dry film thickness was 40 μm, and the resin film obtained was dried by heating at a temperature of 80° C. or higher in 5° C. increments. The gel fraction was expressed as a percentage of the value obtained by dividing the mass of the undissolved portion by the mass before immersion when the resin film was immersed in acetone at 23° C. for 24 hours. The curing temperatures at which the gel fraction in the resin film using the components (A) and (B) reached 80% by mass or more were determined as (A T1 ) and (B T1 ), then (A T1 )>(B T1 That is, the curing temperature (A) at which the gel fraction of the resin film using component (A) is 80 mass % or more is satisfied. T1 ) is the curing temperature at which the gel fraction of the resin film using component (B) reaches 80 mass % or more (B T1) This is presumably because the blocked isocyanate structure (X) of component (A) and the blocked isocyanate structure (Y) of component (B) are different from each other, and the portion derived from the blocking agent in the blocked isocyanate structure (Y) of component (B) is more likely to dissociate at low temperatures than the blocked isocyanate structure (X) of component (A).

[0035] Curing temperature (A T1 ) is the curing temperature (B T1 ), but is not particularly limited as long as it is higher than the curing temperature (A T1 ) is not particularly limited, but from the viewpoint of the low-temperature curing properties of the resulting blocked polyisocyanate composition, it can be, for example, 150°C or less, 140°C or less, or 130°C or less.

[0036] Curing temperature (B T1 ) is the curing temperature (A T1 ), but is not particularly limited as long as it is lower than the curing temperature (B T1 The lower limit of the temperature is not particularly limited, but from the viewpoint of the storage stability of the resulting blocked polyisocyanate composition, it can be, for example, 70°C or more, 75°C or more, or 80°C. Each of the components (A) and (B) is mixed with a polycaprolactone triol having a number average molecular weight of 850 (e.g., Plaxel 308 (manufactured by Daicel Corporation)) so that the ratio NCO / OH of the molar amount of the isocyanate groups of each of the components (A) and (B) to the molar amount of the hydroxyl groups of the polycaprolactone triol is 1.0, and the total of the polycaprolactone triol and the blocked polyisocyanate component is adjusted to 50 mass% of the entire adjusted liquid. Approximately 2 ml of each of the adjusted liquids obtained is placed on an aluminum cup, and heated and dried for 30 minutes at temperatures of 80°C or higher in 5°C increments. The resulting resin film is then immersed in acetone at 23°C for 24 hours. The gel fraction is expressed as a percentage of the mass of the undissolved portion divided by the mass before immersion. The curing temperatures at which the gel fraction in the resin film using the components (A) and (B) reaches 80 mass% or more are respectively defined as (A T2 ) and (B T2 ), then (A T2 )>(B T2 That is, the curing temperature (A) at which the gel fraction of the resin film using component (A) is 80 mass % or more is satisfied. T2 ) is the curing temperature at which the gel fraction of the resin film using component (B) reaches 80 mass % or more (B T2 ) This is presumably because the blocked isocyanate structure (X) of component (A) and the blocked isocyanate structure (Y) of component (B) are different from each other, and the portion derived from the blocking agent in the blocked isocyanate structure (Y) of component (B) is more likely to dissociate at low temperatures than the blocked isocyanate structure (X) of component (A). Curing temperature (A T2 ) is the curing temperature (B T2 ), but is not particularly limited as long as it is higher than the curing temperature (A T2 ) is not particularly limited, but from the viewpoint of the low-temperature curing properties of the resulting blocked polyisocyanate composition, it can be, for example, 150°C or less, 140°C or less, or 130°C or less. Curing temperature (B T2 ) is the curing temperature (AT2 ), but is not particularly limited as long as it is lower than the curing temperature (B T2 The lower limit of the temperature is not particularly limited, but from the viewpoint of the storage stability of the resulting blocked polyisocyanate composition, it can be, for example, 70°C or more, 75°C or more, or 80°C.

[0037] When the structure (X) of the blocked isocyanate group of component (A) is the same as the structure (Y) of the blocked isocyanate group of component (B), T1 )=(B T1 ) or (A T2 )=(B T2 ) may also be used.

[0038] The mixing ratio of component (A) and component (B) can be expressed as the mass ratio (A) / (B) of component (A) to component (B), and is preferably 1 / 99 to 99 / 1, more preferably 5 / 95 to 95 / 5, even more preferably 10 / 90 to 90 / 10, and particularly preferably 20 / 80 to 80 / 20. When the mass ratio (A) / (B) is within the above range, it is possible to achieve both low-temperature curing properties immediately after production and after storage when made into a water-based coating composition, and the amount of gas generated during storage. The mixing ratio of component (A) and component (B) in the blocked polyisocyanate composition can be calculated, for example, by extracting and separating component (A) and component (B) in the blocked polyisocyanate composition with a polar solvent or the like, and subjecting the separated components to NMR measurement.

[0039] Hereinafter, each of the constituent components contained in the blocked polyisocyanate composition of the present embodiment will be described in detail.

[0040] <Blocked polyisocyanate component> The blocked polyisocyanate composition of the present embodiment preferably contains, as blocked polyisocyanate components, components (A) and (B) which are different from each other.

[0041] Component (A) is derived from a polyisocyanate, a nonionic hydrophilic compound, and one or more blocking agents, i.e., a reaction product of a polyisocyanate, a nonionic hydrophilic compound, and one or more blocking agents. Component (A) contains a blocked isocyanate having a blocked isocyanate structure (X). The blocked isocyanate structure (X) is a structure formed by blocking an isocyanate group of a polyisocyanate with a blocking agent.

[0042] Component (B) is derived from a polyisocyanate and one or more blocking agents, i.e., it is a reaction product of a polyisocyanate and one or more blocking agents. Component (B) contains a blocked isocyanate having a blocked isocyanate structure (Y). The blocked isocyanate structure (Y) is a structure formed by blocking an isocyanate group of a polyisocyanate with a blocking agent. The blocked polyisocyanate structure (X) of component (A) and the blocked polyisocyanate structure (Y) of component (B) can be identified by, for example, extracting and separating components (A) and (B) in the blocked polyisocyanate composition with a polar solvent or the like, and subjecting the separated components to NMR measurement or the like.

[0043] The blocked polyisocyanate contained in component (B) may have a nonionic hydrophilic group. In this case, component (B) is derived from a polyisocyanate, a nonionic hydrophilic compound, and one or more blocking agents.

[0044] The nonionic hydrophilic compounds used in components (A) and (B) may be the same or different, as long as the condition that the content of nonionic hydrophilic groups in component (A) is higher than that in component (B) is satisfied. Similarly, the polyisocyanates used in components (A) and (B) may be the same or different.

[0045] [Blocked isocyanate structure (X)] The blocked isocyanate structure (X) is a structural unit formed by reacting an isocyanate group of a polyisocyanate with a blocking agent.

[0046] Among these, as the blocked isocyanate structure (X), from the viewpoints of storage stability and low-temperature curing property, a structural unit obtained by reacting an isocyanate group of a polyisocyanate with a pyrazole-based compound or a malonic acid ester-based compound is preferred, and a structural unit obtained by reacting an isocyanate group of a polyisocyanate with a malonic acid ester-based compound is more preferred.

[0047] [Structure (III)] Examples of structural units formed by reaction of an isocyanate group of a polyisocyanate with a malonic acid ester compound include a structure represented by the following general formula (III) (hereinafter, sometimes referred to as "structure (III)").

[0048] [ka]

[0049] (In general formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. 31 , R 32and the R 33 At least one of the R 34 , R 35 and the above R 36 At least one of the isocyanate groups is a hydrogen atom. The wavy lines represent the bond sites with the residues of polyisocyanate excluding the isocyanate groups.)

[0050] R 31 , R 32 , R 33 , R 34 , R 35 and R 36 The alkyl group in the formula (I) preferably has 1 or more and 20 or less carbon atoms, more preferably has 1 or more and 8 or less carbon atoms, further preferably has 1 or more and 6 or less carbon atoms, and particularly preferably has 1 or more and 4 or less carbon atoms.

[0051] Specific examples of the alkyl group having no substituent include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a sec-butyl group, an isobutyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, an n-hexyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 2,2-dimethylbutyl group, a 2,3-dimethylbutyl group, an n-heptyl group, a 2-methylhexyl group, a 3-methylhexyl group, a 2,2-dimethylpentyl group, a 2,3-dimethylpentyl group, a 2,4-dimethylpentyl group, a 3,3-dimethylpentyl group, a 3-ethylpentyl group, a 2,2,3-trimethylbutyl group, an n-octyl group, an isooctyl group, a 2-ethylhexyl group, a nonyl group, and a decyl group.

[0052] R 31 , R 32 , R 33 , R 34 , R 35 and R 36 When is an alkyl group having a substituent, the substituent is a hydroxy group or an amino group.

[0053] Examples of the alkyl group containing a hydroxy group as a substituent include a hydroxymethyl group, a hydroxyethyl group, and a hydroxypropyl group.

[0054] Examples of the alkyl group containing an amino group as a substituent include an aminomethyl group, an aminoethyl group, an aminopropyl group, and an aminobutyl group.

[0055] Examples of the alkyl group containing a hydroxy group and an amino group as a substituent include a hydroxyaminomethyl group, a hydroxyaminoethyl group, and a hydroxyaminopropyl group.

[0056] Among these, R 33 and R 36 is a hydrogen atom, and R 31 , R 32 , R 34 , and R 35 are each independently an unsubstituted alkyl group having 1 to 4 carbon atoms, and R 33 and R 36 is a hydrogen atom, and R 31 , R 32 , R 34 , and R 35 are each independently a methyl group or an ethyl group.

[0057] [Structure (IV)] Examples of structural units formed by reaction of an isocyanate group of a polyisocyanate with a pyrazole-based compound include a structure represented by the following general formula (IV) (hereinafter, sometimes referred to as "structure (IV)").

[0058] [ka]

[0059] (In general formula (IV), R 41 , R 42 and R 43are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bonding site with a residue of a polyisocyanate excluding an isocyanate group.

[0060] R 41 , R 42 and R 43 From the viewpoint of compatibility, the alkyl group in preferably has 1 or more and 20 or less carbon atoms, more preferably 1 or more and 8 or less, even more preferably 1 or more and 6 or less, and particularly preferably 1 or more and 4 or less carbon atoms.

[0061] R 41 , R 42 and R 43 Specific examples of the alkyl group having no substituent and the alkyl group having a substituent in the above formula (III) include the same as those exemplified in the above formula (III).

[0062] Among them, from the viewpoint of compatibility of the blocked polyisocyanate composition, R 41 , R 42 and R 43 Among these, it is preferable that at least one of them is an alkyl group. From the viewpoint of industrial availability, R 42 is a hydrogen atom, and R 41 and R 43 More preferably, is a methyl group.

[0063] [Blocked isocyanate structure (Y)] The blocked isocyanate structure (Y) is a structural unit formed by reacting an isocyanate group of a polyisocyanate with a blocking agent.

[0064] Among these, as the blocked isocyanate structure (Y), from the viewpoints of storage stability and low-temperature curing property, a structural unit obtained by reacting an isocyanate group of a polyisocyanate with an imidazole-based compound or a malonic acid ester-based compound is preferred, and a structural unit obtained by reacting an isocyanate group of a polyisocyanate with a malonic acid ester-based compound is more preferred.

[0065] [Structure (I)] Examples of structural units formed by reaction of an isocyanate group of a polyisocyanate with an imidazole-based compound include a structure represented by the following general formula (I) (hereinafter, sometimes referred to as "structure (I)").

[0066] [ka]

[0067] (In general formula (I), R 11 , R 12 and R 13 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. 11 , R 12 and the above R 13 The total number of carbon atoms is 1 to 20. The wavy lines represent the bonding sites with the residues of polyisocyanate excluding the isocyanate groups.

[0068] R 11 , R 12 and R 13 From the viewpoint of compatibility, the alkyl group in preferably has 1 or more and 20 or less carbon atoms, more preferably 1 or more and 8 or less, even more preferably 1 or more and 6 or less, and particularly preferably 1 or more and 4 or less carbon atoms.

[0069] R 11 , R 12 and R 13 Specific examples of the alkyl group having no substituent and the alkyl group having a substituent in the above formula (III) include the same as those exemplified in the above formula (III).

[0070] Among them, from the viewpoint of compatibility of the blocked polyisocyanate composition, R 11 , R 12 and R 13Among these, it is preferable that at least one of them is an alkyl group. From the viewpoint of low-temperature curing properties, R 11 It is more preferable that only R is an alkyl group. 12 and R 13 is a hydrogen atom, and R 11 is more preferably a methyl group or an ethyl group.

[0071] [Structure (II)] Examples of structural units formed by reaction of an isocyanate group of a polyisocyanate with a malonic acid ester compound include a structure represented by the following general formula (II) (hereinafter, sometimes referred to as "structure (II)").

[0072] [ka]

[0073] (In general formula (II), R 21 , R 22 , R 23 , R 24 , R 25 and R 26 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bond.

[0074] R 21 , R 22 , R 23 , R 24 , R 25 and R 26 Specific examples of the alkyl group having no substituent and the alkyl group having a substituent in the above formula (III) include the same as those exemplified in the above formula (III). Among them, R 21 , R 22 , R 23 , R 24 , R 25 and R 26 The alkyl group in R is preferably an unsubstituted alkyl group having 1 to 4 carbon atoms.24 , R 25 and R 26 Of these, it is preferable that at least one is a hydrogen atom, and it is more preferable that only one is a hydrogen atom.

[0075] When the structure (Y) is the structure (II), it is preferable to contain 1 mol% or more of the structure represented by the following general formula (II-1) (hereinafter, sometimes referred to as "structure (II-1)") relative to 100 mol% of the structure (II), more preferably 5 mol% or more, even more preferably 20 mol% or more, even more preferably 40 mol% or more, particularly preferably 50 mol% or more, and most preferably 80 mol% or more. When the content of the structure (II-1) is the above lower limit or more, the low temperature curing property when made into an aqueous resin composition is better. On the other hand, the upper limit of the content of the structure (II-1) is, for example, 100 mol% relative to 100 mol% of the structure (II), that is, all of the structure (II) can be structure (II-1), 90 mol% relative to 100 mol% of the structure (II), and 80 mol% relative to 100 mol% of the structure (II).

[0076] [ka]

[0077] (In general formula (II-1), R 211 , R 212 , and R 213 Each of R is independently an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxy group and an amino group. 211 , R 212 and the R 213 The total number of carbon atoms in R is 3 to 20. 214 , R 215 and R 216 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy line represents a bond.

[0078] R 211 , R 212 and R 213 The total number of carbon atoms is 3 or more and 20 or less, preferably 4 or more and 20 or less, more preferably 4 or more and 12 or less, further preferably 4 or more and 9 or less, and particularly preferably 4 or more and 6 or less. R 211 , R 212 and R 213 By making the total carbon number of the above-mentioned lower limit or more, storage stability can be exhibited when the aqueous resin composition is prepared. On the other hand, by making the total carbon number of the above-mentioned upper limit or less, low temperature curing property can be exhibited.

[0079] R 211 , R 212 , R1 23 , R 214 , R 215 and R 216 Specific examples of the alkyl group having no substituent and the alkyl group having a substituent in the above formula (III) include the same as those exemplified in the above formula (III).

[0080] Among these, R 211 , R 212 and R 213 are each independently preferably an unsubstituted alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group.

[0081] Among others, R 214 , R 215 and R 216 The alkyl group in R is preferably an unsubstituted alkyl group having 1 to 4 carbon atoms. 214 , R 215 and R 216 Of these, it is preferable that at least one is a hydrogen atom, and it is more preferable that only one is a hydrogen atom.

[0082] [Polyisocyanate] Polyisocyanates are reaction products obtained by reacting multiple monomer compounds having one or more isocyanate groups (-NCO) (hereinafter, sometimes referred to as "isocyanate monomers").

[0083] The isocyanate monomer is preferably one having a carbon number of 4 to 30. Specific examples of the isocyanate monomer include the following. These isocyanate monomers may be used alone or in combination of two or more. (1) Aromatic diisocyanates such as diphenylmethane-4,4'-diisocyanate (MDI), 1,5-naphthalene diisocyanate, tolylene diisocyanate (TDI), xylylene diisocyanate, and m-tetramethylxylylene diisocyanate (TMXDI). (2) Aliphatic diisocyanates such as 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate (hereinafter sometimes referred to as "HDI"), 2,2,4-trimethyl-1,6-diisocyanatohexane, 2,4,4-trimethyl-1,6-hexamethylene diisocyanate, 2-methylpentane-1,5-diisocyanate (MPDI), and lysine diisocyanate (hereinafter sometimes referred to as "LDI"). (3) Alicyclic diisocyanates such as isophorone diisocyanate (hereinafter sometimes referred to as "IPDI"), 1,3-bis(diisocyanatemethyl)cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, diisocyanatenorbornane, and di(isocyanatemethyl)norbornane. (4) Triisocyanates such as 4-isocyanatomethyl-1,8-octamethylene diisocyanate (hereinafter sometimes referred to as "NTI"), 1,3,6-hexamethylene triisocyanate (hereinafter sometimes referred to as "HTI"), bis(2-isocyanatoethyl) 2-isocyanatoglutarate (hereinafter sometimes referred to as "GTI"), and lysine triisocyanate (hereinafter sometimes referred to as "LTI").

[0084] Among them, the isocyanate monomer is preferably one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates, because of their excellent weather resistance. In addition, the isocyanate monomer is more preferably HDI or IPDI, because of its industrial availability. In addition, the isocyanate monomer is even more preferably HDI, because of its low viscosity of the blocked polyisocyanate component.

[0085] As the isocyanate monomer used in the production of the polyisocyanate, either an aliphatic diisocyanate or an alicyclic diisocyanate may be used alone or in combination, but it is preferable to use an aliphatic diisocyanate and an alicyclic diisocyanate in combination, and it is particularly preferable to use HDI and IPDI. By using an aliphatic diisocyanate and an alicyclic diisocyanate, the toughness and hardness of the coating film can be further improved.

[0086] In the polyisocyanate, from the viewpoint of improving the coating hardness and strength, the mass ratio of the constituent units derived from an aliphatic diisocyanate to the constituent units derived from an alicyclic diisocyanate (constituent units derived from an aliphatic diisocyanate / constituent units derived from an alicyclic diisocyanate) is preferably from 50 / 50 to 95 / 5, more preferably from 55 / 45 to 93 / 7, even more preferably from 60 / 40 to 91 / 9, and even more preferably from 65 / 35 to 90 / 10. By setting the mass ratio of the constituent units derived from an aliphatic diisocyanate to the constituent units derived from an alicyclic diisocyanate to be equal to or greater than the above lower limit, it is possible to more effectively prevent a decrease in flexibility when the coating film is formed, whereas by setting the mass ratio to be equal to or less than the above upper limit, it is possible to more effectively improve the hardness when the coating film is formed.

[0087] The mass ratio of the constituent units derived from the aliphatic diisocyanate to the constituent units derived from the alicyclic diisocyanate can be calculated, for example, by the following method. First, the mass of the unreacted aliphatic diisocyanate and the mass of the unreacted alicyclic diisocyanate are calculated from the mass of the unreacted diisocyanate after the reaction and the aliphatic diisocyanate concentration and the alicyclic diisocyanate concentration in the unreacted diisocyanate obtained by gas chromatography measurement. Next, the mass of the unreacted aliphatic diisocyanate and the mass of the unreacted alicyclic diisocyanate calculated above are subtracted from the mass of the charged aliphatic diisocyanate and the mass of the alicyclic diisocyanate, respectively, and the obtained difference is the mass of the constituent units derived from the aliphatic diisocyanate and the mass of the constituent units derived from the alicyclic diisocyanate, respectively. Next, the mass of the constituent units derived from the aliphatic diisocyanate is divided by the mass of the constituent units derived from the alicyclic diisocyanate to obtain the mass ratio of the constituent units derived from the aliphatic diisocyanate to the constituent units derived from the alicyclic diisocyanate.

[0088] (Polyol) The polyisocyanate is preferably derived from the above-mentioned diisocyanate monomer and a polyol having an average hydroxyl functional group number of 3.0 to 8.0. This allows the average number of isocyanate groups in the obtained polyisocyanate to be larger. In the polyisocyanate, urethane groups are formed by the reaction between the hydroxyl groups of polyol B and the isocyanate groups of the diisocyanate monomer.

[0089] The average number of hydroxyl functional groups in the polyol is preferably 3.0 or more and 8.0 or less, more preferably 3 or more and 6 or less, even more preferably 3 or more and 5 or less, and particularly preferably 3 or 4. The average number of hydroxyl functional groups in the polyol referred to here is the number of hydroxyl groups present in one molecule of the polyol.

[0090] From the viewpoint of improving the coating hardness and strength, the number average molecular weight of the polyol is preferably 100 or more and 1,000 or less, preferably 100 or more and 900 or less, more preferably 100 or more and 600 or less, more preferably 100 or more and 570 or less, even more preferably 100 or more and 500 or less, even more preferably 100 or more and 400 or less, particularly preferably 100 or more and 350 or less, and most preferably 100 or more and 250 or less. When the number average molecular weight of the polyol is within the above range, the blocked polyisocyanate composition has excellent low-temperature curing properties when formed into a coating film, and is particularly excellent in hardness and strength. The number average molecular weight Mn of the polyol is, for example, the number average molecular weight based on polystyrene standard measured by GPC.

[0091] Examples of such polyols include trimethylolpropane, glycerol, and polycaprolactone polyols derived from trihydric or higher polyhydric alcohols and ε-caprolactone.

[0092] Commercially available polycaprolactone polyols include, for example, Daicel Corporation's "PLACCEL 303" (number average molecular weight 300), "PLACCEL 305" (number average molecular weight 550), "PLACCEL 308" (number average molecular weight 850), and "PLACCEL 309" (number average molecular weight 900).

[0093] (Production method of polyisocyanate) The method for producing polyisocyanate will be described in detail below. The polyisocyanate can be obtained by, for example, carrying out an allophanate reaction to form an allophanate group, a uretdione reaction to form a uretdione group, an iminooxadiazinedione reaction to form an iminooxadiazinedione group, an isocyanurate reaction to form an isocyanurate group, a urethanization reaction to form a urethane group, and a biuret reaction to form a biuret group all at once in the presence of an excess of isocyanate monomer, and removing the unreacted isocyanate monomer after the reaction is completed. That is, the polyisocyanate obtained by the above reaction is a reaction product in which a plurality of the above-mentioned isocyanate monomers are bonded together, and which has one or more groups selected from the group consisting of an allophanate group, a uretdione group, an iminooxadiazinedione group, an isocyanurate group, a urethane group, and a biuret group. Alternatively, the above reactions may be carried out separately and the resulting polyisocyanates may be mixed in a specific ratio. From the viewpoint of ease of production, it is preferable to carry out the above reaction at one time to obtain a polyisocyanate, and from the viewpoint of freely adjusting the molar ratio of each functional group, it is preferable to produce them separately and then mix them.

[0094] (1) Method for producing allophanate group-containing polyisocyanate The allophanate group-containing polyisocyanate can be obtained by adding an alcohol to an isocyanate monomer and using an allophanate reaction catalyst. The alcohol used to form the allophanate group is preferably an alcohol formed only from carbon, hydrogen and oxygen. Specific examples of the alcohol include, but are not limited to, monoalcohols, dialcohols, etc. These alcohols may be used alone or in combination of two or more. Examples of monoalcohols include methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, and nonanol. Examples of the dialcohol include ethylene glycol, 1,3-butanediol, neopentyl glycol, and 2-ethylhexanediol. Among them, as the alcohol, a monoalcohol is preferable, and a monoalcohol having a molecular weight of 200 or less is more preferable.

[0095] Examples of the allophanate reaction catalyst include, but are not limited to, alkyl carboxylates of tin, lead, zinc, bismuth, zirconium, zirconyl, and the like. Examples of tin alkylcarboxylates (organotin compounds) include tin 2-ethylhexanoate and dibutyltin dilaurate. An example of the alkylcarboxylate of lead (organic lead compound) is lead 2-ethylhexanoate. Examples of zinc alkylcarboxylates (organic zinc compounds) include zinc 2-ethylhexanoate. An example of the alkyl carboxylate of bismuth is bismuth 2-ethylhexanoate. An example of the zirconium alkylcarboxylate is zirconium 2-ethylhexanoate. An example of the zirconyl alkylcarboxylate is zirconyl 2-ethylhexanoate, etc. These catalysts can be used alone or in combination of two or more. In addition, an isocyanurate reaction catalyst described later can also serve as an allophanate reaction catalyst. When an allophanate reaction is carried out using an isocyanurate reaction catalyst described later, an isocyanurate group-containing polyisocyanate (hereinafter, sometimes referred to as an "isocyanurate-type polyisocyanate") is naturally produced. Among these, it is preferable from the viewpoint of economical production to carry out the allophanate formation reaction and the isocyanurate formation reaction using an isocyanurate formation catalyst described below as the allophanate formation reaction catalyst.

[0096] The lower limit of the amount of the allophanate reaction catalyst used is preferably 10 ppm by mass, more preferably 20 ppm by mass, further preferably 40 ppm by mass, and particularly preferably 80 ppm by mass, relative to the mass of the charged isocyanate monomer. The upper limit of the amount of the allophanate reaction catalyst used is preferably 1000 ppm by mass, more preferably 800 ppm by mass, further preferably 600 ppm by mass, and particularly preferably 500 ppm by mass, relative to the mass of the charged isocyanate monomer. That is, the amount of the allophanate reaction catalyst used is preferably 10 ppm by mass or more and 1,000 ppm by mass or less, more preferably 20 ppm by mass or more and 800 ppm by mass or less, even more preferably 40 ppm by mass or more and 600 ppm by mass or less, and particularly preferably 80 ppm by mass or more and 500 ppm by mass or less, relative to the mass of the charged isocyanate monomer.

[0097] The lower limit of the allophanate reaction temperature is preferably 40°C, more preferably 60°C, further preferably 80°C, and particularly preferably 100°C. The upper limit of the allophanate reaction temperature is preferably 180°C, more preferably 160°C, and even more preferably 140°C. That is, the allophanate reaction temperature is preferably 40°C or higher and 180°C or lower, more preferably 60°C or higher and 160°C or lower, even more preferably 80°C or higher and 140°C or lower, and particularly preferably 100°C or higher and 140°C or lower. By setting the allophanate formation reaction temperature to the above lower limit or higher, it is possible to further increase the reaction rate. By setting the allophanate formation reaction temperature to the above upper limit or lower, it is possible to more effectively suppress coloration of the polyisocyanate.

[0098] (2) Method for producing uretdione group-containing polyisocyanate When a polyisocyanate having a uretdione group is derived from an isocyanate monomer, it can be produced, for example, by polymerizing the isocyanate monomer using a uretdione reaction catalyst or by heat. The uretdione reaction catalyst is not particularly limited, but examples thereof include tertiary phosphines such as trialkylphosphine, tris(dialkylamino)phosphine and cycloalkylphosphine, Lewis acids, and the like. Examples of the trialkylphosphine include tri-n-butylphosphine and tri-n-octylphosphine. Examples of tris(dialkylamino)phosphines include tris-(dimethylamino)phosphine and the like. Examples of cycloalkylphosphines include cyclohexyl-di-n-hexylphosphine. Examples of Lewis acids include boron trifluoride and zinc oxychloride.

[0099] Many of the uretdione reaction catalysts can also simultaneously promote the isocyanurate reaction. When a uretdione-forming reaction catalyst is used, it is preferable to add a deactivator for the uretdione-forming reaction catalyst such as phosphoric acid or methyl paratoluenesulfonate to terminate the uretdione-forming reaction when a desired yield is achieved. When one or more diisocyanates selected from the group consisting of the aliphatic diisocyanates and the alicyclic diisocyanates are heated to obtain a polyisocyanate having a uretdione group without using a uretdione reaction catalyst, the heating temperature is preferably 120° C. or higher, and more preferably 150° C. or higher and 170° C. or lower. The heating time is preferably 1 hour or longer and 4 hours or shorter.

[0100] (3) Method for producing iminooxadiazinedione group-containing polyisocyanate When an iminooxadiazinedione group-containing polyisocyanate is derived from an isocyanate monomer, an iminooxadiazinedione reaction catalyst is usually used. Examples of the iminooxadiazinedione catalyst include the following 1) or 2). 1) (Poly)hydrogen fluoride represented by the general formula M[Fn] or the general formula M[Fn(HF)m] (wherein m and n are integers satisfying the relationship m / n>0. M is an n-charged cation (mixture) or one or more radicals with a total valence of n.) 2) A compound comprising a compound represented by the general formula R1-CR'2-C(O)O- or R2=CR'-C(O)O- and a quaternary ammonium cation or a quaternary phosphonium cation. (In the formula, R1 and R2 are each independently a linear, branched, or cyclic, saturated or unsaturated perfluoroalkyl group having from 1 to 30 carbon atoms. Each of the multiple R's is independently a hydrogen atom, or an alkyl or aryl group having from 1 to 20 carbon atoms which may contain a heteroatom.)

[0101] Specific examples of the compound 1) ((poly)hydrogen fluoride) include tetramethylammonium fluoride hydrate, tetraethylammonium fluoride, and the like. Specific examples of the compound 2) include 3,3,3-trifluorocarboxylic acid, 4,4,4,3,3-pentafluorobutanoic acid, 5,5,5,4,4,3,3-heptafluoropentanoic acid, and 3,3-difluoroprop-2-enoic acid. Among them, as the iminooxadiazinedione reaction catalyst, 1) is preferred from the viewpoint of availability, and 2) is preferred from the viewpoint of safety.

[0102] The lower limit of the amount of the iminooxadiazinedione catalyst used is not particularly limited, but from the viewpoint of reactivity, it is preferably 5 ppm, more preferably 10 ppm, and even more preferably 20 ppm by mass relative to the raw material isocyanate monomer such as HDI. The upper limit of the amount of the iminooxadiazinedione catalyst used is preferably 5000 ppm, more preferably 2000 ppm, and even more preferably 500 ppm, in terms of mass ratio relative to the raw material isocyanate monomer such as HDI, from the viewpoints of suppressing coloration and discoloration of the product and controlling the reaction. That is, the amount of the iminooxadiazinedione catalyst used is preferably 5 ppm or more and 5000 ppm or less, more preferably 10 ppm or more and 2000 ppm or less, and even more preferably 20 ppm or more and 500 ppm or less, by mass ratio relative to the raw material isocyanate monomer such as HDI.

[0103] The lower limit of the reaction temperature for the iminooxadiazinedione formation is not particularly limited, but from the viewpoint of the reaction rate, it is preferably 40°C, more preferably 50°C, and even more preferably 60°C. The upper limit of the reaction temperature for the iminooxadiazinedione formation is preferably 150°C, more preferably 120°C, and even more preferably 110°C, from the viewpoint of suppressing coloration and discoloration of the product. That is, the reaction temperature for the iminooxadiazinedione formation is preferably 40°C or higher and 150°C or lower, more preferably 50°C or higher and 120°C or lower, and even more preferably 60°C or higher and 110°C or lower.

[0104] When the iminooxadiazine dionation reaction reaches a desired iminooxadiazine dione group content, the iminooxadiazine dionation reaction can be stopped. The iminooxadiazine dionation reaction can be stopped, for example, by adding an acidic compound to the reaction solution. Examples of the acidic compound include phosphoric acid, acidic phosphate ester, sulfuric acid, hydrochloric acid, and sulfonic acid compounds. This neutralizes the iminooxadiazine dionation reaction catalyst, or inactivates it by thermal decomposition or chemical decomposition. After the reaction is stopped, filtration is performed if necessary.

[0105] (4) Method for producing isocyanurate group-containing polyisocyanate Examples of catalysts for deriving a polyisocyanate containing an isocyanurate group from an isocyanate monomer include commonly used isocyanuration reaction catalysts.

[0106] The isocyanurate reaction catalyst is not particularly limited, but is preferably a catalyst having basicity in general. Specific examples of the isocyanurate reaction catalyst include the following. 1) Hydroxides of tetraalkylammonium such as tetramethylammonium, tetraethylammonium, and tetrabutylammonium, and organic weak acid salts such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above tetraalkylammonium. 2) Hydroxides of aryltrialkylammonium such as benzyltrimethylammonium and trimethylphenylammonium, and organic weak acid salts such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above aryltrialkylammonium. 3) Hydroxyalkylammonium hydroxides, such as trimethylhydroxyethylammonium, trimethylhydroxypropylammonium, triethylhydroxyethylammonium, and triethylhydroxypropylammonium, and organic weak acid salts, such as acetates, propionates, octylates, caprates, myristates, and benzoates of the above hydroxyalkylammoniums. 4) Metal salts, such as tin, zinc, lead, etc., of alkyl carboxylic acids, such as acetic acid, propionic acid, caproic acid, octylic acid, capric acid, and myristic acid. 5) Metal alcoholates such as sodium and potassium. 6) Aminosilyl group-containing compounds such as hexamethylenedisilazane. 7) Mannich bases. 8) Mixtures of tertiary amines and epoxy compounds. 9) Phosphorus compounds such as tributylphosphine.

[0107] Among these, from the viewpoint of preventing the production of unnecessary by-products, the isocyanurate reaction catalyst is preferably a quaternary ammonium hydroxide or a weak organic acid salt of a quaternary ammonium, and more preferably a tetraalkylammonium hydroxide, a weak organic acid salt of a tetraalkylammonium, an aryltrialkylammonium hydroxide, or a weak organic acid salt of an aryltrialkylammonium.

[0108] The upper limit of the amount of the isocyanurate reaction catalyst used is preferably 1000 ppm by mass, more preferably 500 ppm by mass, and even more preferably 100 ppm by mass, based on the mass of the charged isocyanate monomer. On the other hand, the lower limit of the amount of the isocyanurate reaction catalyst used is not particularly limited, and may be, for example, 10 ppm by mass.

[0109] The isocyanurate reaction temperature is preferably from 50° C. to 120° C., and more preferably from 60° C. to 90° C. By keeping the isocyanurate reaction temperature at or below the upper limit, coloration of the polyisocyanate tends to be more effectively suppressed.

[0110] When a desired conversion rate (the ratio of the mass of polyisocyanate produced in the isocyanuration reaction to the mass of the charged isocyanate monomer) is reached, the isocyanuration reaction is stopped by adding an acidic compound (e.g., phosphoric acid, an acidic phosphoric acid ester, etc.). In order to obtain polyisocyanate, it is necessary to stop the reaction at an early stage. However, since the reaction rate of the isocyanurate reaction is very fast at the early stage, it is difficult to stop the reaction at an early stage, and therefore the reaction conditions, particularly the amount and method of adding the catalyst, must be carefully selected. For example, a method of adding the catalyst in portions at regular intervals is recommended as a suitable method.

[0111] Therefore, the conversion rate of the isocyanurate reaction to obtain a polyisocyanate is preferably 10% or more and 60% or less, more preferably 15% or more and 55% or less, and even more preferably 20% or more and 50% or less. By setting the conversion rate of the isocyanurate reaction to the upper limit or less, the viscosity of the blocked polyisocyanate component can be made lower. By setting the conversion rate of the isocyanurate reaction to the lower limit or more, the reaction terminating operation can be more easily carried out.

[0112] When deriving a polyisocyanate containing an isocyanurate group, a monohydric to hexahydric alcohol can be used in addition to the above isocyanate monomers. Examples of the alcohol having a valence of 1 to 6 that can be used include non-polymerizable alcohol and polymerizable alcohol. The term "non-polymerizable alcohol" used herein means an alcohol that does not have a polymerizable group. On the other hand, the term "polymerizable alcohol" means an alcohol obtained by polymerizing a monomer having a polymerizable group and a hydroxyl group. Examples of the non-polymerizable alcohol include polyhydric alcohols such as monoalcohols, diols, triols, and tetraols. Examples of monoalcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, n-pentanol, n-hexanol, n-octanol, n-nonanol, 2-ethylbutanol, 2,2-dimethylhexanol, 2-ethylhexanol, cyclohexanol, methylcyclohexanol, and ethylcyclohexanol. Examples of diols include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-methyl-1,2-propanediol, 1,5-pentanediol, 2-methyl-2,3-butanediol, and Examples of the hexanediol include hexanediol, 1,6-hexanediol, 1,2-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 2,3-dimethyl-2,3-butanediol, 2-ethyl-hexanediol, 1,2-octanediol, 1,2-decanediol, 2,2,4-trimethylpentanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-diethyl-1,3-propanediol. Examples of triols include glycerin and trimethylolpropane. An example of the tetraols is pentaerythritol.

[0113] The polymerizable alcohol is not particularly limited, but examples thereof include polyester polyols, polyether polyols, acrylic polyols, polyolefin polyols, and the like.

[0114] The polyester polyols are not particularly limited, but examples thereof include products obtained by a condensation reaction between a dibasic acid alone or a mixture of dibasic acids and a polyhydric alcohol alone or a mixture of polyhydric alcohols. The dibasic acid is not particularly limited, but examples thereof include at least one dibasic acid selected from the group consisting of carboxylic acids such as succinic acid, adipic acid, sebacic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, and terephthalic acid. The polyhydric alcohol is not particularly limited, but examples thereof include at least one polyhydric alcohol selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, neopentyl glycol, trimethylolpropane, and glycerin. Examples of polyester polyols include polycaprolactones obtained by ring-opening polymerization of ε-caprolactone using the above polyhydric alcohols.

[0115] The polyether polyols are not particularly limited, but examples thereof include polyether polyols obtained by adding an alkylene oxide or a mixture of an alkylene oxide to a polyhydric alcohol or a mixture of an alkylene oxide using an alkali metal hydroxide or a strong basic catalyst, polyether polyols obtained by reacting an alkylene oxide with a polyamine compound, and so-called polymer polyols obtained by polymerizing acrylamide or the like using the above-mentioned polyethers as a medium.

[0116] Examples of the alkali metal include lithium, sodium, and potassium.

[0117] Examples of the strong basic catalyst include alcoholates and alkylamines.

[0118] Examples of the polyhydric alcohol include those exemplified for the polyester polyols above.

[0119] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.

[0120] Examples of the polyamine compound include ethylenediamines.

[0121] The acrylic polyols are not particularly limited, but examples thereof include copolymers of a single or mixture of ethylenically unsaturated bond-containing monomers having a hydroxyl group and a single or mixture of other ethylenically unsaturated bond-containing monomers copolymerizable therewith.

[0122] The ethylenically unsaturated bond-containing monomer having a hydroxyl group is not particularly limited, but examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.

[0123] The other ethylenically unsaturated bond-containing monomer copolymerizable with the ethylenically unsaturated bond-containing monomer having a hydroxyl group is not particularly limited, and examples thereof include acrylic acid esters, methacrylic acid esters, unsaturated carboxylic acids, unsaturated amides, vinyl-based monomers, and vinyl-based monomers having a hydrolyzable silyl group.

[0124] Examples of acrylic esters include methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, benzyl acrylate, and phenyl acrylate.

[0125] Examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate, and phenyl methacrylate.

[0126] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, and itaconic acid.

[0127] Examples of the unsaturated amide include acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleic acid amide, and maleimide.

[0128] Examples of the vinyl monomer include glycidyl methacrylate, styrene, vinyl toluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.

[0129] Examples of vinyl monomers having a hydrolyzable silyl group include vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.

[0130] Examples of polyolefin polyols include hydroxyl-terminated polybutadiene and hydrogenated products thereof.

[0131] (5) Method for producing urethane group-containing polyisocyanate When a polyisocyanate containing a urethane group is derived from an isocyanate monomer, it can be produced, for example, by mixing an excess of the isocyanate monomer, the polyol, and, if necessary, an alcohol other than the polyol, and adding a urethane reaction catalyst as necessary.

[0132] Examples of the polyol include those exemplified in the above "polyol".

[0133] Examples of the alcohol other than the polyol include those exemplified in the above "Method for producing an isocyanurate group-containing polyisocyanate" except for those exemplified in the above "Polyol".

[0134] The urethanization reaction catalyst is not particularly limited, but examples thereof include tin-based compounds, zinc-based compounds, and amine-based compounds.

[0135] The urethanization reaction temperature is preferably 50°C or higher and 160°C or lower, and more preferably 60°C or higher and 120°C or lower.

[0136] By controlling the urethanization reaction temperature to be equal to or lower than the above upper limit, coloration of the polyisocyanate tends to be more effectively suppressed.

[0137] The urethane reaction time is preferably from 30 minutes to 4 hours, more preferably from 1 hour to 3 hours, and even more preferably from 1 hour to 2 hours.

[0138] The molar ratio of the isocyanate group of the isocyanate monomer to the molar amount of the hydroxyl group of the polyol (and, if necessary, the alcohol other than the polyol) is preferably 2 / 1 or more and 50 / 1 or less. When the molar ratio is equal to or more than the lower limit, the viscosity of the polyisocyanate can be made lower. When the molar ratio is equal to or less than the upper limit, the yield of the urethane group-containing polyisocyanate can be increased.

[0139] (6) Method for producing biuret group-containing polyisocyanate The biuretizing agent for deriving a polyisocyanate containing a biuret group from an isocyanate monomer is not particularly limited, and examples thereof include water, a monohydric tertiary alcohol, formic acid, an organic primary monoamine, and an organic primary diamine. The amount of isocyanate groups per mole of the biuretizing agent is preferably 6 moles or more, more preferably 10 moles or more, and even more preferably 10 moles or more and 80 moles or less. When the amount of molar isocyanate groups per mole of the biuretizing agent is equal to or more than the lower limit, the viscosity of the polyisocyanate becomes sufficiently low, and when it is equal to or less than the upper limit, the low-temperature curing property of the resin film is further improved.

[0140] A solvent may be used in the biuretization reaction. The solvent may be any solvent that dissolves the isocyanate monomer and the biuretization agent such as water and forms a homogeneous phase under the reaction conditions.

[0141] Specific examples of the solvent include ethylene glycol-based solvents and phosphoric acid-based solvents.

[0142] Examples of ethylene glycol solvents include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-propyl ether acetate, ethylene glycol monoisopropyl ether acetate, ethylene glycol mono-n-butyl ether acetate, ethylene glycol diacetate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol di-n-propyl ether, ethylene glycol diisopropyl ether, ethylene glycol di-n-butyl ether, ethylene glycol methyl ethyl ether, ethylene glycol methyl isopropyl ether, ethylene glycol methyl-n-butyl ether, ethylene glycol ethyl-n-propyl ether, ethylene glycol ethyl isopropyl ether, ethylene glycol ethyl-n-butyl ether, ethylene glycol-n-propyl-n-butyl ether, ethylene glycol isopropyl-n-butyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol mono-n-propyl ether acetate, diethylene glycol monoisopropyl ether acetate, diethylene glycol mono-n-butyl ether acetate, diethylene glycol diacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol di-n-propyl ether, diethylene glycol diisopropyl ether, diethylene glycol di-n-butyl ether, diethylene glycol methyl ethyl ether, diethylene glycol methyl isopropyl ether, diethylene glycol methyl-n-propyl ether, diethylene glycol methyl-n-butyl ether, diethylene glycol ethyl isopropyl ether, diethylene glycol ethyl-n-propyl ether, diethylene glycol ethyl-n-butyl ether, diethylene glycol-n-propyl-n-butyl ether, diethylene glycol isopropyl-n-butyl ether, and the like.

[0143] Examples of the phosphoric acid-based solvent include trimethyl phosphate, triethyl phosphate, tripropyl phosphate, and tributyl phosphate.

[0144] These solvents may be used alone or in combination of two or more.

[0145] Among these, the ethylene glycol solvent is preferably ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol diacetate or diethylene glycol dimethyl ether.

[0146] As the phosphoric acid-based solvent, trimethyl phosphate or triethyl phosphate is preferred.

[0147] The biuretization reaction temperature is preferably from 70° C. to 200° C., and more preferably from 90° C. to 180° C. By keeping it below the upper limit, coloration of the polyisocyanate tends to be more effectively prevented.

[0148] The above-mentioned allophanate formation reaction, uretdione formation reaction, iminooxadiazinedione formation reaction, isocyanurate formation reaction, urethanization reaction, and biuret formation reaction may be carried out successively, or some of them may be carried out in parallel. After the reaction is completed, unreacted isocyanate monomer is removed from the reaction solution by thin-film distillation, extraction, or the like to obtain a polyisocyanate.

[0149] Furthermore, an antioxidant or an ultraviolet absorber may be added to the obtained polyisocyanate, for example, for the purpose of suppressing coloration during storage. Examples of the antioxidant include hindered phenols such as 2,6-di-tert-butyl-p-cresol. Examples of the ultraviolet absorber include benzotriazole and benzophenone. These antioxidants and ultraviolet absorbers may be used alone or in combination of two or more. The amount of these to be added is preferably 10 ppm by mass or more and 500 ppm by mass or less based on the mass of the polyisocyanate.

[0150] (Average number of isocyanate groups in polyisocyanate) The average number of isocyanate groups in the polyisocyanate is preferably 2 or more from the viewpoint of improving the low-temperature curing property when formed into a resin film, and from the viewpoint of achieving both the low-temperature curing property when formed into a resin film and compatibility with the polyvalent hydroxy compound, it is more preferably 3.0 to 20.0, even more preferably 3.2 to 10.0, particularly preferably 3.4 to 8.0, and most preferably 3.5 to 6.0. The average number of isocyanate functional groups of the polyisocyanate can be measured by the method described in the Examples below.

[0151] [Blocking agent] Examples of blocking agents include 1) alcohol compounds, 2) alkylphenol compounds, 3) phenol compounds, 4) active methylene compounds, 5) mercaptan compounds, 6) acid amide compounds, 7) acid imide compounds, 8) imidazole compounds, 9) urea compounds, 10) oxime compounds, 11) amine compounds, 12) imide compounds, 13) bisulfites, 14) pyrazole compounds, 15) triazole compounds, etc. More specifically, examples of blocking agents include the following:

[0152] 1) Alcohol compounds: Alcohols such as methanol, ethanol, 2-propanol, n-butanol, sec-butanol, 2-ethyl-1-hexanol, 2-methoxyethanol, 2-ethoxyethanol, and 2-butoxyethanol. 2) Alkylphenol compounds: mono- and di-alkylphenols having an alkyl group having 4 or more carbon atoms as a substituent. Specific examples of the alkylphenol compounds include monoalkylphenols such as n-propylphenol, iso-propylphenol, n-butylphenol, sec-butylphenol, tert-butylphenol, n-hexylphenol, 2-ethylhexylphenol, n-octylphenol, and n-nonylphenol; and dialkylphenols such as di-n-propylphenol, diisopropylphenol, isopropyl cresol, di-n-butylphenol, di-tert-butylphenol, di-sec-butylphenol, di-n-octylphenol, di-2-ethylhexylphenol, and di-n-nonylphenol. 3) Phenolic compounds: phenol, cresol, ethylphenol, styrenated phenol, hydroxybenzoic acid esters, etc. 4) Active methylene compounds: acetoacetate esters (methyl acetoacetate, ethyl acetoacetate, methyl isobutanoylacetate, ethyl isobutanoylacetate), acetylacetone, malonate esters (dimethyl malonate, diethyl malonate, dipropyl malonate, dibutyl malonate, dicyclohexyl malonate, diphenyl malonate, di-sec-butyl malonate, diisopropyl malonate, isopropylethyl malonate, di-tert-butyl malonate, di(2-methyl-2-butyl) malonate, di(2-methyl-2-pentyl) malonate, (tert-butyl)ethyl malonate, (2-methyl-2-butyl)ethyl malonate, (2-methyl-2-butyl)isopropyl malonate, (2-methyl-2-pentyl)ethyl malonate, (2-methyl-2-pentyl)isopropyl malonate, (2-methyl-2-pentyl)hexylisopropyl malonate), etc. 5) Mercaptan compounds: butyl mercaptan, dodecyl mercaptan, etc. 6) Acid amide compounds: acetanilide, acetic acid amide, ε-caprolactam, δ-valerolactam, γ-butyrolactam, etc. 7) Acid imide compounds: succinimide, maleimide, etc. 8) Imidazole compounds: imidazole, 2-methylimidazole, 4-methylimidazole, 2-ethylimidazole, 2-isopropylimidazole, 2,4-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-methyl-2-phenylimidazole, etc. 9) Urea compounds: urea, thiourea, ethyleneurea, etc. 10) Oxime compounds: formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, cyclohexanone oxime, etc. 11) Amine compounds: diphenylamine, aniline, carbazole, di-n-propylamine, diisopropylamine, isopropylethylamine, etc. 12) Imine compounds: ethyleneimine, polyethyleneimine, etc. 13) Bisulfite compounds: sodium bisulfite, etc. 14) Pyrazole compounds: pyrazole, 3-methylpyrazole, 3,5-dimethylpyrazole, etc. 15) Triazole compounds: 3,5-dimethyl-1,2,4-triazole, etc.

[0153] [Nonionic hydrophilic compounds] Specific examples of the nonionic hydrophilic compound include monoalcohols and compounds in which ethylene oxide is added to the hydroxyl group of alcohol. Examples of the monoalcohol include methanol, ethanol, butanol, etc. The nonionic hydrophilic compound may be used alone or in combination of two or more. In addition to ethylene oxide, an alkylene oxide having 3 or more carbon atoms may be added to the hydroxyl group of the alcohol. Among them, an addition of ethylene oxide and propylene oxide is preferable, and an addition of only ethylene oxide is more preferable. Examples of compounds in which ethylene oxide is added to the hydroxyl group of an alcohol include ethylene glycol, diethylene glycol, polyethylene glycol, etc. These nonionic hydrophilic compounds also have an active hydrogen group that reacts with an isocyanate group.

[0154] Among these, as the nonionic hydrophilic compound, polyethylene glycol monoalkyl ether in which ethylene oxide is added to the hydroxyl group of a monoalcohol is preferred, since it can improve the water dispersibility of the blocked polyisocyanate composition with a small amount used.

[0155] The number of ethylene oxide additions in the ethylene oxide-added compound is preferably from 4 to 30, and more preferably from 4 to 25. When the number of ethylene oxide additions is equal to or more than the above lower limit, water dispersibility tends to be more effectively imparted to the blocked polyisocyanate composition, and when the number of ethylene oxide additions is equal to or less than the above upper limit, the blocked polyisocyanate composition tends to be less susceptible to precipitation during low-temperature storage.

[0156] [Other hydrophilic compounds] At least a portion of the blocked polyisocyanate may further have a structural unit derived from a hydrophilic compound other than the nonionic hydrophilic compound, that is, a hydrophilic group other than the nonionic hydrophilic group.

[0157] The other hydrophilic compound is a compound having a hydrophilic group other than the nonionic hydrophilic group. In addition to the hydrophilic group other than the nonionic hydrophilic group, the other hydrophilic compound preferably has one or more active hydrogen groups for reacting with at least one of the isocyanate groups of the polyisocyanate per molecule of the other hydrophilic compound. Specific examples of the active hydrogen group include hydroxyl group, mercapto group, carboxylic acid group, amino group, and thiol group.

[0158] Examples of other hydrophilic compounds include cationic hydrophilic compounds and anionic hydrophilic compounds. These hydrophilic compounds may be used alone or in combination of two or more. Among them, the other hydrophilic compounds are preferably anionic hydrophilic compounds from the viewpoint of suppressing the decrease in hardness and strength of the obtained resin film and from the viewpoint of improving emulsifiability.

[0159] (cationic hydrophilic compounds) As the cationic hydrophilic compound, specifically, a compound having both cationic hydrophilic group and active hydrogen group can be mentioned.In addition, a compound having active hydrogen group such as glycidyl group and a compound having cationic hydrophilic group such as sulfide, phosphine can be combined to form a hydrophilic compound.In this case, a compound having isocyanate group and a compound having active hydrogen group are reacted in advance, functional group such as glycidyl group is added, and then a compound such as sulfide, phosphine is reacted.From the viewpoint of ease of production, a compound having both cationic hydrophilic group and active hydrogen group is preferred.

[0160] Specific examples of compounds having both a cationic hydrophilic group and an active hydrogen group include dimethylethanolamine, diethylethanolamine, diethanolamine, methyldiethanolamine, etc. Furthermore, the tertiary amino groups added using these compounds can also be quaternized with, for example, dimethyl sulfate or diethyl sulfate.

[0161] The reaction between the cationic hydrophilic compound and the alicyclic polyisocyanate can be carried out in the presence of a solvent. In this case, the solvent is preferably one that does not contain an active hydrogen group, and specific examples thereof include ethyl acetate, propylene glycol monomethyl ether acetate, and dipropylene glycol dimethyl ether.

[0162] The cationic hydrophilic groups added to the blocked polyisocyanate are preferably neutralized with a compound having an anionic group, such as a carboxy group, a sulfonic acid group, a phosphoric acid group, a halogen group, or a sulfate group.

[0163] Specific examples of compounds having a carboxy group include formic acid, acetic acid, propionic acid, butyric acid, and lactic acid.

[0164] A specific example of the compound having a sulfonic acid group is ethanesulfonic acid.

[0165] Specific examples of compounds having a phosphoric acid group include phosphoric acid and acidic phosphate esters.

[0166] A specific example of the compound having a halogen group is hydrochloric acid.

[0167] Specific examples of compounds having a sulfate group include sulfuric acid.

[0168] Among them, as the compound having an anionic group, a compound having a carboxy group is preferable, and acetic acid, propionic acid or butyric acid is more preferable.

[0169] (anionic hydrophilic compounds) Specific examples of the anionic hydrophilic group include a carboxy group, a sulfonic acid group, a phosphoric acid group, a halogen group, and a sulfate group.

[0170] Specific examples of the anionic hydrophilic compound include compounds having both an anionic group and an active hydrogen group, and more specific examples include compounds having a carboxy group of a monohydroxycarboxylic acid or polyhydroxycarboxylic acid as the anionic group.

[0171] Examples of monohydroxycarboxylic acids include 1-hydroxyacetic acid, 3-hydroxypropanoic acid, 12-hydroxy-9-octadecanoic acid, hydroxypivalic acid, and lactic acid.

[0172] Examples of compounds having a carboxy group of a polyhydroxycarboxylic acid as an anionic group include dimethylol acetic acid, 2,2-dimethylol butyric acid, 2,2-dimethylol pentanoic acid, dihydroxysuccinic acid, and dimethylol propionic acid.

[0173] Further, compounds having both a sulfonic acid group and an active hydrogen group are also included, and more specifically, for example, isethionic acid is included.

[0174] Among these, hydroxypivalic acid or dimethylolpropionic acid is preferred as a compound having both an anionic group and an active hydrogen group.

[0175] The anionic hydrophilic group added to the blocked polyisocyanate is preferably neutralized with an amine compound, which is a basic substance.

[0176] Specific examples of the amine compound include ammonia and water-soluble amino compounds.

[0177] Specific examples of water-soluble amino compounds include monoethanolamine, ethylamine, dimethylamine, diethylamine, triethylamine, propylamine, dipropylamine, isopropylamine, diisopropylamine, triethanolamine, butylamine, dibutylamine, 2-ethylhexylamine, ethylenediamine, propylenediamine, methylethanolamine, dimethylethanolamine, diethylethanolamine, and morpholine. In addition, tertiary amines such as triethylamine and dimethylethanolamine can also be used. These amine compounds may be used alone or in combination of two or more.

[0178] [Production method of component (A)] Component (A) is not particularly limited, but can be obtained, for example, by reacting the above polyisocyanate, the above blocking agent, and the above nonionic hydrophilic compound.

[0179] The reaction of the polyisocyanate with the nonionic hydrophilic compound and the reaction of the polyisocyanate with the blocking agent can be carried out simultaneously, or one of the reactions can be carried out in advance before the second or subsequent reaction is carried out. Among these, it is preferable to carry out the reaction of the polyisocyanate with the nonionic hydrophilic compound first, obtain a hydrophilic compound-modified polyisocyanate modified with the nonionic hydrophilic compound, and then react the obtained hydrophilic compound-modified polyisocyanate with the blocking agent.

[0180] The reaction between polyisocyanate and nonionic hydrophilic compound may be carried out using an organic metal salt, a tertiary amine compound, or an alcoholate of an alkali metal as a catalyst. Examples of the metal constituting the organic metal salt include tin, zinc, and lead. Examples of the alkali metal include sodium.

[0181] The reaction temperature between the polyisocyanate and the nonionic hydrophilic compound is preferably from -20°C to 150°C, more preferably from 30°C to 130°C. The reaction temperature being equal to or higher than the lower limit tends to increase the reactivity. The reaction temperature being equal to or lower than the upper limit tends to suppress side reactions more effectively.

[0182] It is preferable to completely react the nonionic hydrophilic compound with the polyisocyanate so that no unreacted nonionic hydrophilic compound remains. By not leaving any unreacted nonionic hydrophilic compound, there is a tendency to more effectively suppress the deterioration of the aqueous dispersion stability of the blocked polyisocyanate composition and the low-temperature curing property when the blocked polyisocyanate composition is made into a resin film.

[0183] The reaction between the nonionic hydrophilic compound-modified polyisocyanate and the blocking agent can be carried out regardless of the presence or absence of a solvent, to give a blocked polyisocyanate.

[0184] The blocking agents may be used alone or in combination of two or more.

[0185] The amount of the blocking agent added may usually be 80 mol % or more and 200 mol % or less, and preferably 90 mol % or more and 150 mol % or less, based on the total molar amount of isocyanate groups. In addition, when a solvent is used, it is sufficient to use a solvent that is inactive to an isocyanate group.

[0186] When a solvent is used, the content of non-volatile matters derived from the polyisocyanate and the blocking agent per 100 parts by mass of the blocked polyisocyanate composition may usually be from 10 parts by mass to 95 parts by mass, preferably from 20 parts by mass to 80 parts by mass, and more preferably from 30 parts by mass to 75 parts by mass.

[0187] In the blocking reaction, an organic metal salt of tin, zinc, lead or the like, a tertiary amine compound, an alcoholate of an alkali metal such as sodium, or the like may be used as a catalyst.

[0188] The amount of catalyst added varies depending on the temperature of the blocking reaction, etc., but may usually be from 0.05 to 1.5 parts by mass, and preferably from 0.1 to 1.0 part by mass, per 100 parts by mass of polyisocyanate.

[0189] The blocking reaction can generally be carried out at a temperature of from −20° C. to 150° C., preferably from 0° C. to 100° C., and more preferably from 10° C. to 80° C. When the temperature of the blocking reaction is equal to or higher than the lower limit, the reaction rate can be increased, and when the temperature is equal to or lower than the upper limit, side reactions can be suppressed.

[0190] After the blocking reaction, a neutralization treatment may be carried out by adding an acidic compound or the like.

[0191] The acidic compound may be an inorganic acid or an organic acid. Examples of the inorganic acid include hydrochloric acid, phosphorous acid, and phosphoric acid. Examples of the organic acid include methanesulfonic acid, p-toluenesulfonic acid, dioctyl phthalate, and dibutyl phthalate.

[0192] [Production method of component (B)] The method for producing component (B) is not particularly limited, but it can be produced, for example, by a method similar to the method for producing component (A) described above.

[0193] For example, when the blocked polyisocyanate structure (Y) of the blocked polyisocyanate contained in the component (B) is the structure (II), the following two methods can be mentioned. 1) A method of reacting the above polyisocyanate with the above malonic acid ester having a tertiary alkyl group, and the above malonic acid ester having a secondary alkyl group or the above malonic acid ester having a primary alkyl group. 2) A method in which the polyisocyanate is reacted with at least one blocking agent selected from the group consisting of the malonic acid ester having a tertiary alkyl group, the malonic acid ester having a secondary alkyl group, and the malonic acid ester having a primary alkyl group, and an alcohol having a chain alkyl group is added to the obtained reaction product to introduce an alkyl group derived from the alcohol by transesterification of the terminal ester site of the reaction product.

[0194] Of the above two methods, method 2) is preferred from the viewpoint of reaction control.

[0195] The blocking reaction between the polyisocyanate and the blocking agent can be carried out regardless of the presence or absence of a solvent, to give a blocked polyisocyanate.

[0196] As the blocking agent, among malonic acid ester compounds, diisopropyl malonate, di-tert-butyl malonate, or di(2-methyl-2-butyl) malonate is preferable. Each of these blocking agents may be used alone or in combination of two or more.

[0197] The amount of the blocking agent added may usually be 80 mol % or more and 200 mol % or less, and preferably 90 mol % or more and 150 mol % or less, based on the total molar amount of isocyanate groups.

[0198] When a solvent is used, it is sufficient to use a solvent that is inactive to an isocyanate group.

[0199] When a solvent is used, the content of non-volatile matters derived from the polyisocyanate and the blocking agent per 100 parts by mass of the blocked polyisocyanate composition is as described for component (A).

[0200] In the blocking reaction, an organic metal salt of tin, zinc, lead or the like, a tertiary amine compound, an alcoholate of an alkali metal such as sodium, or the like may be used as a catalyst. The amount of catalyst added and the blocking reaction temperature are as described above for the blocked polyisocyanate composition (A).

[0201] After the blocking reaction, neutralization treatment may be carried out by adding an acidic compound, etc. As the acidic compound, the same compounds as those used as component (A) can be used.

[0202] When a hydrophilic compound including a nonionic hydrophilic compound is used, the reaction can be carried out in the same manner as for component (A).

[0203] In the case of producing the polyvinyl alcohol by the above method 2), the above blocking reaction is followed by an ester exchange reaction.

[0204] The alcohol having a chain alkyl group used in the transesterification reaction of method 2) may be any alcohol having a chain alkyl group, and examples thereof include tertiary alcohols such as tert-butanol and tert-amyl alcohol (2-methyl-2-butanol).

[0205] In addition, the chain alkyl group of the alcohol may be the same as that of the blocking agent, or may be a different chain alkyl group. When the chain alkyl group is different from that of the blocking agent, it is preferable to use a monoalcohol having a chain alkyl group with a different number of alkyl substitutions from that of the blocking agent. Specifically, for example, when a single malonic acid ester having a secondary alkyl group is used as the blocking agent, a monoalcohol having a tertiary alkyl group can be used.

[0206] In the case of producing by the method 2), it is preferable to remove the generated alcohol or the residual added alcohol during or after the transesterification reaction by distillation under normal or reduced pressure.

[0207] Among them, in order to efficiently proceed with the transesterification reaction, it is preferable to remove the generated alcohol during the transesterification reaction by performing an operation such as distillation. In this case, in order to efficiently remove the alcohol component generated by the transesterification reaction, it is more preferable that the alcohol component to be added has a boiling point higher than that of the generated alcohol component.

[0208] The transesterification reaction can generally be carried out at 0° C. or higher and 150° C. or lower, preferably 30° C. or higher and 120° C. or lower, and more preferably 50° C. or higher and 100° C. or lower. When the temperature of the transesterification reaction is equal to or higher than the lower limit, the reaction rate can be increased, and when the temperature is equal to or lower than the upper limit, side reactions can be suppressed.

[0209] The amount of the alcohol component in component (B) (i.e., the content of the blocked isocyanate structure substituted with the linear alkyl group of the alcohol by transesterification) is preferably 0.05 parts by mass or more and 41 parts by mass or less, more preferably 0.1 parts by mass or more and 30 parts by mass or less, and even more preferably 0.5 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the solid content of component (B). When the amount of the alcohol component is equal to or more than the above lower limit, the storage stability of the aqueous resin composition becomes better, and when the amount is equal to or less than the above upper limit, thickening during blending of the aqueous paint can be further suppressed.

[0210] <Other components> The blocked polyisocyanate composition of the present embodiment may further contain additives such as a solvent in addition to the blocked polyisocyanate component.

[0211] Examples of the solvent include 1-methylpyrrolidone, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether, 3-methoxy-3-methyl-1-butanol, ethylene glycol diethyl ether, diethylene glycol diethyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether (DPDM), propylene glycol dimethyl ether, methyl ethyl ketone, and acetonitrile. Examples of the solvent include ethanol, methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethanol, methanol, iso-propanol, 1-propanol, iso-butanol, 1-butanol, tert-butanol, 2-ethylhexanol, cyclohexanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, ethyl acetate, isopropyl acetate, butyl acetate, toluene, xylene, pentane, iso-pentane, hexane, iso-hexane, cyclohexane, solvent naphtha, and mineral spirits. These solvents may be used alone or in combination of two or more. From the viewpoint of dispersibility in water, the solvent is preferably one having a solubility in water of 5% by mass or more, and specifically, DPDM is preferred.

[0212] The blocked polyisocyanate composition of the present embodiment may further contain a surfactant in addition to the above-mentioned blocked polyisocyanate component. By containing a surfactant, the blocked polyisocyanate composition of the present embodiment can have better dispersibility.

[0213] Examples of the surfactant include anionic surfactants such as aliphatic soaps, rosin acid soaps, alkyl sulfonates, dialkylaryl sulfonates, alkyl sulfosuccinates, polyoxyethylene alkyl ether sulfates, and polyoxyethylene alkylaryl ether sulfates; and nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, and polyoxyethylene oxypropylene block copolymers.

[0214] As the anionic surfactant, the surface tension at 25°C of an aqueous solution consisting of 0.1 mass% of the anionic dispersant relative to the total mass of the aqueous solution and water, as measured by the Wilhelmy method, is preferably 32 mN / m or more and 51 mN / m or less, more preferably 34 mN / m or more and 50 mN / m or less, even more preferably 36 mN / m or more and 48 mN / m or less, and particularly preferably 37 mN / m or more and 47 mN / m or less.

[0215] The nonionic surfactant preferably has an HLB (Hydrophile Lipophile Balance) value of 10 or more and 20 or less, and more preferably has an HLB value of 14 or more and 17 or less.

[0216] <Method for producing blocked polyisocyanate composition> The blocked polyisocyanate composition of the present embodiment can be obtained by mixing the components (A) and (B), and, if necessary, other components such as a solvent. Alternatively, the blocked polyisocyanate composition may be produced by mixing the components (A) and (B) and, if necessary, other components such as a solvent when formulating the coating material. Among these, it is preferable to previously mix the components (A) and (B) with other components such as a solvent, as necessary, to produce a blocked polyisocyanate composition.

[0217] ≪Resin composition≫ The resin composition of the present embodiment includes a blocked polyisocyanate composition and a polyvalent hydroxy compound. The resin composition of the present embodiment can also be called a one-liquid type resin composition including a curing agent component and a base component.

[0218] The resin composition of the present embodiment, by containing the blocked polyisocyanate composition, has excellent curing properties when baked at a low temperature of 90°C or less immediately after production and after storage, the amount of gas generated during storage is suppressed, and when formed into a resin film, it has excellent water resistance.

[0219] Furthermore, the resin composition of the present embodiment has excellent storage stability when made into an aqueous resin composition, and is therefore particularly suitable for use as an aqueous resin composition.

[0220] The components of the resin composition of the present embodiment will be described in detail below.

[0221] <Polyhydroxy compounds> In this specification, the term "polyhydric hydroxy compound" refers to a compound having at least two hydroxy groups (hydroxyl groups) in one molecule, and is also called a "polyol." Specific examples of the polyhydric hydroxy compound include aliphatic hydrocarbon polyols, polyether polyols, polyester polyols, epoxy resins, fluorine-containing polyols, and acrylic polyols. Among these, the polyhydric hydroxy compound is preferably a polyester polyol, a fluorine-containing polyol or an acrylic polyol.

[0222] [Aliphatic hydrocarbon polyols] Examples of the aliphatic hydrocarbon polyols include hydroxyl-terminated polybutadiene and hydrogenated products thereof.

[0223] [Polyether polyols] The polyether polyols include, for example, those obtained by any one of the following methods (1) to (3). (1) Polyether polyols or polytetramethylene glycols obtained by adding an alkylene oxide, either alone or in a mixture, to a polyhydric alcohol, either alone or in a mixture. (2) Polyether polyols obtained by reacting alkylene oxide with a polyfunctional compound. (3) Polymer polyols obtained by polymerizing acrylamide or the like using the polyether polyols obtained in (1) or (2) as a medium. Examples of the polyhydric alcohol include glycerol and propylene glycol. Examples of the alkylene oxide include ethylene oxide and propylene oxide. Examples of the polyfunctional compound include ethylenediamine and ethanolamines.

[0224] [Polyester polyols] Examples of the polyester polyols include the following polyester polyols (1) and (2). (1) Polyester polyol resins obtained by a condensation reaction between a dibasic acid, either alone or in a mixture of two or more kinds, and a polyhydric alcohol, either alone or in a mixture of two or more kinds. (2) Polycaprolactones obtained by ring-opening polymerization of ε-caprolactone with polyhydric alcohols. Examples of the dibasic acid include carboxylic acids such as succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, and 1,4-cyclohexanedicarboxylic acid. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerol, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.

[0225] [Epoxy resins] Examples of the epoxy resins include novolac type epoxy resins, β-methylepicrotype epoxy resins, cyclic oxirane type epoxy resins, glycidyl ether type epoxy resins, glycol ether type epoxy resins, epoxy type aliphatic unsaturated compounds, epoxidized fatty acid esters, ester type polycarboxylic acids, aminoglycidyl type epoxy resins, halogenated type epoxy resins, and resorcinol type epoxy resins, as well as resins obtained by modifying these epoxy resins with amino compounds, polyamide compounds, or the like.

[0226] [Fluorine-containing polyols] Examples of the fluorine-containing polyols include copolymers of fluoroolefins, cyclohexyl vinyl ethers, hydroxyalkyl vinyl ethers, and monocarboxylic acid vinyl esters, as disclosed in Reference Document 1 (JP-A-57-34107) and Reference Document 2 (JP-A-61-275311).

[0227] [Acrylic polyols] The acrylic polyols can be obtained, for example, by polymerizing a polymerizable monomer having one or more active hydrogens in one molecule, or by copolymerizing a polymerizable monomer having one or more active hydrogens in one molecule with another monomer copolymerizable with the polymerizable monomer, as necessary.

[0228] Examples of the polymerizable monomer having one or more active hydrogens in one molecule include the following (i) to (iii). These may be used alone or in combination of two or more. (i) Acrylic esters having active hydrogen, such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-hydroxybutyl acrylate. (ii) Methacrylic acid esters having active hydrogen, such as 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, and 2-hydroxybutyl methacrylate. (iii) (meth)acrylic acid esters having polyvalent active hydrogen, such as acrylic acid monoester or methacrylic acid monoester of glycerol, and acrylic acid monoester or methacrylic acid monoester of trimethylolpropane.

[0229] Examples of other monomers copolymerizable with the polymerizable monomer include the following (i) to (v). These may be used alone or in combination of two or more. (i) Acrylic esters such as methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, and 2-ethylhexyl acrylate. (ii) Methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate, and glycidyl methacrylate. (iii) Unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid. (iv) Unsaturated amides such as acrylamide, N-methylol acrylamide, and diacetone acrylamide. (v) Styrene, vinyl toluene, vinyl acetate, acrylonitrile, etc.

[0230] Further examples include acrylic polyols obtained by copolymerizing polymerizable ultraviolet-stable monomers disclosed in Reference Document 3 (JP-A-1-261409) and Reference Document 4 (JP-A-3-006273), etc.

[0231] Specific examples of the polymerizable ultraviolet-stable monomer include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, and 2-hydroxy-4-(3-methacryloxy-2-hydroxypropoxy)benzophenone.

[0232] For example, the above-mentioned monomer components are solution-polymerized in the presence of a known radical polymerization initiator such as a peroxide or an azo compound, and the resulting solution is diluted with an organic solvent, etc., as necessary, to obtain an acrylic polyol.

[0233] When obtaining a water-based acrylic polyol, it can be produced by a known method such as a method of solution polymerization of an olefinic unsaturated compound and converting it into an aqueous phase, or emulsion polymerization, etc. In this case, water solubility or water dispersibility can be imparted by neutralizing the acidic moiety of a carboxylic acid-containing monomer such as acrylic acid or methacrylic acid, or a sulfonic acid-containing monomer, etc., with an amine or ammonia.

[0234] [Hydroxyl value and acid value of polyhydric hydroxy compounds] The hydroxyl value of the polyvalent hydroxy compound contained in the resin composition of this embodiment is preferably 5 mgKOH / g or more and 300 mgKOH / g or less, more preferably 10 mgKOH / g or more and 280 mgKOH / g or less, and even more preferably 30 mgKOH / g or more and 250 mgKOH / g or less. When the hydroxyl value of the polyvalent hydroxy compound is within the above range, a resin film having various excellent physical properties such as tensile strength can be obtained. Specifically, when the hydroxyl group of the polyvalent hydroxy compound is equal to or more than the above lower limit, the crosslink density of the urethane due to the reaction with the polyisocyanate is further increased, and the function of the urethane bond is more easily exhibited. On the other hand, when the hydroxyl group of the polyvalent hydroxy compound is equal to or less than the above upper limit, the crosslink density does not increase too much, and the mechanical properties of the resin film are better. The hydroxyl value of the polyvalent hydroxy compound is measured, for example, by potentiometric titration and calculated as a value relative to the solid content in the polyvalent hydroxy compound.

[0235] [Glass transition temperature Tg of polyhydroxy compounds] The glass transition temperature Tg of the polyhydric hydroxy compound contained in the resin composition of this embodiment is preferably 0°C or more and 100°C or less, more preferably 0°C or more and 90°C or less, even more preferably 0°C or more and 80°C or less, and particularly preferably 5°C or more and 70°C or less. When the glass transition temperature of the polyhydric hydroxy compound is within the above range, a resin film having superior tensile strength can be obtained. The glass transition temperature of the polyhydric hydroxy compound can be measured, for example, using a differential scanning calorimeter (DSC) measuring device.

[0236] [Weight average molecular weight Mw of polyhydroxy compound] The weight average molecular weight Mw of the polyhydric hydroxy compound is 5.0×10 3 Above 2.0×10 5 It is preferable that the value is less than 5.0×10 3 More than 1.5 x 10 5 More preferably, it is 5.0×10 or less. 3 Above 1.0×10 5 It is more preferable that the weight average molecular weight Mw of the polyhydric hydroxy compound is within the above range, so that a resin film having excellent physical properties such as tensile strength can be obtained. The weight average molecular weight Mw of the polyhydric hydroxy compound is a weight average molecular weight based on polystyrene standard measured by gel permeation chromatography (GPC).

[0237] [NCO / OH] The molar equivalent ratio (NCO / OH) of the isocyanate groups of the blocked polyisocyanate composition to the hydroxyl groups of the polyvalent hydroxy compound contained in the resin composition of the present embodiment is determined depending on the physical properties of the resin film required, and is usually 0.01 or more and 10.00 or less, preferably 0.10 or more and 5.00 or less, more preferably 0.20 or more and 3.00 or less, and even more preferably 0.25 or more and 2.00 or less.

[0238] [Blocked polyisocyanate composition content] In the resin composition of the present embodiment, the content of the blocked polyisocyanate may be an amount such that the molar equivalent ratio of the isocyanate group of the blocked polyisocyanate to the hydroxyl group of the polyvalent hydroxy compound is within the above range, and for example, it is preferably 1 part by mass or more and 200 parts by mass or less, more preferably 5 parts by mass or more and 180 parts by mass or less, and even more preferably 10 parts by mass or more and 150 parts by mass or less, relative to 100 parts by mass of the polyvalent hydroxy compound. When the content of the blocked polyisocyanate is within the above range, a resin film having excellent various physical properties such as tensile strength can be obtained. The content of the blocked polyisocyanate can be calculated, for example, from the blending amount, or can be calculated by identifying and quantifying using a nuclear magnetic resonance (NMR) method and a gas chromatography / mass spectrometry (GC / MS method).

[0239] <Other additives> The resin composition of the present embodiment may further contain other additives. Other additives include, for example, curing agents capable of reacting with crosslinkable functional groups in the polyhydric hydroxy compound, curing catalysts, solvents, pigments (extender pigments, colored pigments, metallic pigments, etc.), ultraviolet absorbers, light stabilizers, radical stabilizers, yellowing inhibitors that suppress coloring during the baking process, coating surface conditioners, flow conditioners, pigment dispersants, defoamers, thickeners, film-forming assistants, and the like.

[0240] Examples of the curing agent include melamine resins, urea resins, epoxy group-containing compounds or resins, carboxyl group-containing compounds or resins, acid anhydrides, alkoxysilane group-containing compounds or resins, and hydrazide compounds.

[0241] The curing catalyst may be a basic compound or a Lewis acid compound. Examples of the basic compound include metal hydroxides, metal alkoxides, metal carboxylates, metal acetylacetinates, hydroxides of onium salts, onium carboxylates, halides of onium salts, metal salts of active methylene compounds, onium salts of active methylene compounds, aminosilanes, amines, phosphines, etc. As the onium salts, ammonium salts, phosphonium salts, or sulfonium salts are preferable. Examples of the Lewis acid compound include an organotin compound, an organozinc compound, an organotitanium compound, and an organozirconium compound.

[0242] Examples of the solvent include the same solvents as those exemplified in the blocked polyisocyanate composition.

[0243] In addition, known pigments (extender pigments, colored pigments, metallic pigments, etc.), ultraviolet absorbers, light stabilizers, radical stabilizers, yellowing inhibitors that suppress coloring during the baking process, coating surface conditioners, flow conditioners, pigment dispersants, defoamers, thickeners, and film-forming aids can be appropriately selected and used.

[0244] <Method of producing resin composition> The resin composition of the present embodiment can be used as either a solvent-based or aqueous-based resin composition, but is preferably used as an aqueous-based resin composition. In this case, the blocked polyisocyanate composition may be prepared by previously mixing components (A) and (B) and, if necessary, other components such as a solvent, and then adding the mixture to the polyhydric hydroxy compound that is the main component, or components (A) and (B) and, if necessary, other components such as a solvent, may each be added to the polyhydric hydroxy compound that is the main component. Among these, it is preferable to add a mixture of components (A) and (B) and, if necessary, other components such as a solvent, which is previously mixed, to the polyhydric hydroxy compound that is the main component.

[0245] When producing a water-based resin composition (water-based resin composition), first, additives such as a curing agent capable of reacting with a crosslinkable functional group in the polyhydroxy compound, a curing catalyst, a solvent, pigments (body pigments, coloring pigments, metallic pigments, etc.), an ultraviolet absorber, a light stabilizer, a radical stabilizer, an anti-yellowing agent for suppressing coloring during the baking process, a coating surface conditioner, a flow conditioner, a pigment dispersant, an antifoaming agent, a thickener, and a film-forming assistant are added to the polyhydroxy compound or its water dispersion or water solution as necessary. Next, the above-mentioned blocked polyisocyanate composition or its water dispersion is added as a curing agent, and water or a solvent is further added as necessary to adjust the viscosity. Next, the mixture is forcibly stirred with a stirring device to obtain a water-based resin composition (water-based resin composition).

[0246] When producing a solvent-based resin composition, first, additives such as a curing agent capable of reacting with a crosslinkable functional group in the polyhydroxy compound, a curing catalyst, a solvent, pigments (body pigments, coloring pigments, metallic pigments, etc.), ultraviolet absorbers, light stabilizers, radical stabilizers, yellowing inhibitors for suppressing coloring during the baking process, coating surface conditioners, flow conditioners, pigment dispersants, defoamers, thickeners, and film-forming assistants are added to the polyhydroxy compound or its solvent dilution as necessary. Then, the above-mentioned blocked polyisocyanate composition is added as a curing agent, and a solvent is further added as necessary to adjust the viscosity. Then, the solvent-based resin composition can be obtained by stirring by hand or using a stirring device such as a mixer.

[0247] <Resin film> The resin film of the present embodiment is formed by curing the above-mentioned resin composition. The resin film of the present embodiment has excellent water resistance.

[0248] The resin film of the present embodiment is obtained by applying the above-mentioned resin composition to a substrate using a known method such as roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, etc., and then curing the composition by heating.

[0249] From the viewpoints of energy saving and heat resistance of the substrate, the heating temperature is preferably from about 70°C to about 120°C, more preferably from about 70°C to about 110°C, and even more preferably from about 75°C to about 100°C. From the viewpoints of energy saving and heat resistance of the base material, the heating time is preferably from about 1 minute to about 60 minutes, and more preferably from about 2 minutes to about 40 minutes.

[0250] The substrate is not particularly limited, and examples thereof include outer panels of automobile bodies such as passenger cars, trucks, motorcycles, and buses; automobile parts such as bumpers; outer panels of household electrical appliances such as mobile phones and audio equipment; and various films. Among these, outer panels of automobile bodies or automobile parts are preferred.

[0251] The material of the substrate is not particularly limited, and examples thereof include metal materials such as iron, aluminum, brass, copper, tinplate, stainless steel, zinc-plated steel, and zinc alloy (Zn-Al, Zn-Ni, Zn-Fe, etc.)-plated steel; resins such as polyethylene resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, and epoxy resin, and plastic materials such as various FRPs; inorganic materials such as glass, cement, and concrete; wood; and fibrous materials such as paper and cloth. Among these, metal materials and plastic materials are preferred.

[0252] The substrate may be a surface treatment such as phosphate treatment, chromate treatment, complex oxide treatment, etc., performed on the surface of the above-mentioned metal material, or a metal surface such as a car body formed from the above-mentioned metal material, and further, a coating film may be formed thereon. The substrate on which a coating film is formed may be a substrate that has been subjected to a surface treatment as necessary and has a primer coating film formed thereon, for example, a car body on which a primer coating film is formed by electrochemical paint. The substrate may be a surface treatment performed as desired on the surface of the above-mentioned plastic material, or a plastic surface such as an automobile part formed from the above-mentioned metal material. The substrate may also be a combination of a plastic material and a metal material.

[0253] Since the resin film of the present embodiment has excellent low-temperature curing properties, it is suitable for use as a coating film for products in various fields where energy saving is required, or for materials with low heat resistance.

[0254] <Laminate> The laminate of the present embodiment is formed by laminating one or more layers of the above-mentioned resin film on a substrate. The thickness of each resin film layer is 1 μm or more and 50 μm or less. The laminate of the present embodiment has excellent water resistance due to the inclusion of the resin film.

[0255] The laminate of the present embodiment may include two or more layers of the above resin films having the same composition, or may include two or more layers of the above resin films having different compositions.

[0256] Examples of the substrate include the same ones exemplified in the above "resin film".

[0257] The laminate of the present embodiment can be obtained by coating the above-mentioned resin composition on a substrate using a known method such as roll coating, curtain flow coating, spray coating, bell coating, electrostatic coating, etc., and then heating and curing the composition, or by coating all layers and then heating and curing the entire layer at once.

[0258] The laminate of the present embodiment may include, in addition to the substrate and the resin film, layers made of other known components, such as a primer layer, an adhesive layer, and a decorative layer. EXAMPLES

[0259] Hereinafter, the present embodiment will be described in more detail based on examples and comparative examples, but the present embodiment is not limited to the following examples in any way. In the following, Example 11 is considered as a reference example.

[0260] <Test items> The polyisocyanates and blocked polyisocyanate components obtained in the Synthesis Examples, and the blocked polyisocyanate compositions obtained in the Examples and Comparative Examples were subjected to measurement of various physical properties and evaluations according to the methods described below.

[0261] [Physical Properties 1] (Isocyanate group (NCO) content) In order to measure the NCO content of the polyisocyanate, the polyisocyanate before being blocked with a blocking agent was used as a measurement sample. First, 2 g to 3 g of the measurement sample was weighed out (Wg) in a flask. Then, 20 mL of toluene was added to dissolve the measurement sample. Then, 20 mL of a 2N toluene solution of di-n-butylamine was added, mixed, and left at room temperature for 15 minutes. Then, 70 mL of isopropyl alcohol was added and mixed. Then, this liquid was titrated with a 1N hydrochloric acid solution (factor F) as an indicator. The titration value obtained was V2 mL. Then, the titration value obtained without the polyisocyanate sample was V1 ml. Then, the isocyanate group (NCO) content (mass%) of the polyisocyanate was calculated from the following formula.

[0262] Isocyanate group (NCO) content (mass%) = (V1-V2) x F x 42 / (W x 1000) x 100

[0263] The available NCO content of the blocked isocyanate composition was calculated by the following formula.

[0264] Effective NCO content [mass%] = {100 × (mass of isocyanate groups in the solid content of the polyisocyanate used in the blocking reaction)} / (mass of the blocked polyisocyanate composition after the blocking reaction)

[0265] [Physical Properties 2] (Number average molecular weight and weight average molecular weight) The number average molecular weight and weight average molecular weight are those measured by gel permeation chromatography (GPC) using the following apparatus, using polystyrene as a standard. In order to measure the number average molecular weight of the polyisocyanate, the polyisocyanate before being blocked with a blocking agent was used as a measurement sample. The weight average molecular weight was measured by directly using the blocked polyisocyanate composition or the polyvalent hydroxy compound as a sample under the following measurement conditions.

[0266] (Measurement conditions) Equipment: Tosoh Corporation, HLC-802A Column: Tosoh Corporation, G1000HXL x 1 G2000HXL x 1 G3000HXL x 1 Carrier: Tetrahydrofuran Detection method: Differential refractometer

[0267] [Physical Properties 3] (Average number of isocyanate groups) The average number of isocyanate groups (average NCO number) of the polyisocyanate was calculated by the following formula. In the formula, "Mn" is the number average molecular weight of the polyisocyanate, and the value measured in the above "Physical Properties 2" was used. "NCO content" is the isocyanate group content of the polyisocyanate measured before blocking with a blocking agent, and the value calculated in the above "Physical Properties 1" was used.

[0268] Average number of isocyanate groups = (Mn x NCO content x 0.01) / 42

[0269] [Physical Properties 4] (Solid content of blocked polyisocyanate composition) The solids content of the blocked polyisocyanate composition was determined as follows. First, an aluminum dish with a bottom diameter of 38 mm was precisely weighed. Next, about 1 g of the blocked polyisocyanate composition produced in the Examples and Comparative Examples was precisely weighed on the aluminum dish (W1). Next, the blocked polyisocyanate composition was adjusted to a uniform thickness. Next, the blocked polyisocyanate composition placed on the aluminum dish was kept in an oven at 105°C for 1 hour. Next, after the aluminum dish reached room temperature, the blocked polyisocyanate composition remaining on the aluminum dish was precisely weighed (W2). Next, the solid content (mass%) of the blocked polyisocyanate composition was calculated from the following formula.

[0270] Solid content of blocked polyisocyanate composition (mass%)=W2 / W1×100

[0271] [Physical Properties 5] (Modification amount and composition ratio of nonionic hydrophilic groups) The modification amount and constituent ratio of the nonionic hydrophilic group in each blocked polyisocyanate component and each blocked polyisocyanate composition were calculated by the following method, assuming that all of the nonionic hydrophilic compounds used had reacted with the isocyanate groups of the polyisocyanate. That is, the modification amount of the nonionic hydrophilic group was calculated as a percentage (mol %) from the ratio of the molar amount of the nonionic hydrophilic compound to the molar amount of the isocyanate group of the raw material polyisocyanate. The constituent ratio of the nonionic hydrophilic group was calculated as a percentage (mass %) from the ratio of the mass of the nonionic hydrophilic compound to the total mass of the solid content of the obtained blocked polyisocyanate component or blocked polyisocyanate composition.

[0272] [Physical Properties 6] (Amount of modification of blocked isocyanate structure) The degree of modification of the blocked isocyanate structure in each blocked polyisocyanate component and blocked polyisocyanate composition was calculated by the following method, assuming that all of the blocking agent used had reacted. That is, the degree of modification with the blocked isocyanate structure was calculated as a percentage (mol %) from the ratio of the molar amount of the blocking agent to the molar amount of the isocyanate groups in the raw material polyisocyanate.

[0273] [Physical Properties 7-1] (Curing temperature of blocked polyisocyanate component) Acrylic polyol Nuplex, "Setalux (registered trademark) 1767" (trade name), OH (mass %) (on solids) = 4.5, solid content 65 mass %, and each blocked polyisocyanate component were mixed so that the ratio of the molar amount of isocyanate groups to the molar amount of hydroxyl groups (isocyanate groups / hydroxyl groups) was 1.0, and the paint solid content was adjusted to 50 mass % with butyl acetate. The obtained adjusted liquid was applied to a polypropylene (PP) plate so that the dry film thickness was 40 μm, and then heated and dried for 30 minutes at temperatures of 80 ° C or higher in 5 ° C increments to obtain a resin film. The gel fraction was calculated as the percentage (mass %) of the value obtained by dividing the undissolved part mass when the obtained resin film was immersed in acetone at 23 ° C for 24 hours by the mass before immersion. The temperature at which the gel fraction reached 80 mass % or more was determined as the curing temperature of the blocked polyisocyanate component. [Physical Properties 7-2] (Curing temperature of blocked polyisocyanate component) Polycaprolactone triol (manufactured by Daicel Corporation), "Placcel 308" (trade name, number average molecular weight 850), and each blocked polyisocyanate component were mixed so that the ratio of the molar amount of isocyanate groups to the molar amount of hydroxyl groups (isocyanate groups / hydroxyl groups) was 1.0, and the total of polycaprolactone triol and the blocked polyisocyanate component was adjusted with butyl acetate so that it was 50% by mass of the entire adjusted liquid. About 2 ml of the adjusted liquid was added to an aluminum cup, and heated and dried for 30 minutes at temperatures of 80°C or higher in 5°C increments to obtain a resin film. The gel fraction was calculated as the percentage (mass%) of the value obtained by dividing the undissolved mass of the obtained resin film by the mass before immersion when the resin film was immersed in acetone at 23°C for 24 hours. The temperature at which the gel fraction reached 80% by mass or more was determined as the curing temperature of the blocked polyisocyanate component.

[0274] [Physical Properties 8] (Quantitative determination of the ratio of structure (II-1)) Each blocked polyisocyanate component (B) is evaporated at 50°C or less to remove the solvent and other components, and then dried under reduced pressure. 13 The ratio (mol %) of Structure (II-1) relative to 100 mol % of Structure (II) was quantified by C-NMR.

[0275] (Measurement conditions) Device: JEOL “JEOL-ECZ500(SC)” (product name) Solvent: deuterated chloroform Accumulation count: 5120 times Sample concentration: 50wt / vol% Chemical shift standard: deuterated chloroform was set at 77.0 ppm by mass.

[0276] [Preparation of Waterborne Resin Composition] Water-based base acrylic polyol (Nuplex Corporation, "Setaqua (registered trademark) 6515" (trade name), OH (mass%) (on solids) = 3.3, Acid value (mgKOH / g) = 9.9, solid content 45 mass%) and each blocked polyisocyanate composition were mixed so that the ratio of the molar amount of isocyanate groups to the molar amount of hydroxyl groups (isocyanate groups / hydroxyl groups) was 0.80. Further, ion-exchanged water was mixed, and a small amount of dimethylaminoethanol was added to adjust the pH to about 8.0 to 8.5 and the solid content to 40 mass%. Next, the solution was stirred at 1000 rpm for 15 minutes using a homodisper, and after defoaming, a water-based resin composition was obtained.

[0277] [Rating 1] (dispersibility) The aqueous resin composition obtained in the above "Preparation of aqueous resin composition" was allowed to stand at room temperature, and the appearance of the aqueous resin composition was evaluated according to the following evaluation criteria.

[0278] (Evaluation Criteria) ◎: No change even after 72 hours ○: Sediment present after 24 hours or more but less than 72 hours △: Settling occurs after 8 hours or more but less than 24 hours ×: Settling occurs after 8 hours or less

[0279] [Rating 2] (Low temperature curing) The resin composition obtained in the above "Preparation of Waterborne Resin Composition" was applied to a polypropylene (PP) plate so that the dry film thickness was 40 μm, and then heated and dried at 85°C and 90°C for 30 minutes to obtain a resin film. The obtained resin film was immersed in acetone at 23°C for 24 hours, and the percentage (mass%) of the undissolved part mass divided by the mass before immersion was calculated as the gel fraction. Using the calculated gel fraction, the low-temperature curing property was evaluated according to the following evaluation criteria.

[0280] (Evaluation Criteria) ○: Gel fraction was 80% by mass or more at 85°C △: Gel fraction was 80% by mass or more at 90°C ×: Gel fraction was less than 80% by mass at 90°C

[0281] [Rating 3] (Gas generation during storage) Water was further added to the aqueous resin composition obtained in the above "Preparation of aqueous resin composition" to adjust the solid content to 15% by mass. Next, 200 g of the adjusted solution was charged into an Erlenmeyer flask, and a burette was set. The Erlenmeyer flask containing the solution was placed in a water bath at 40°C for 10 days, and the change in the liquid level of the burette was recorded to calculate the amount of gas generated. Using the calculated amount of gas generated, the amount of gas generated during storage was evaluated according to the following evaluation criteria.

[0282] (Evaluation Criteria) ○: Less than 20mL △: 20mL or more but less than 25mL ×: 25mL or more

[0283] [Rating 4] (Low temperature hardening after storage) The resin composition obtained in the above "Preparation of Waterborne Resin Composition" was stored at 40°C for 10 days. The resin composition after storage was applied to a polypropylene (PP) plate so that the dry film thickness was 40 μm, and then heated and dried at 85°C for 30 minutes to obtain a resin film. The obtained resin film was immersed in acetone at 23°C for 24 hours, and the percentage (mass%) of the undissolved part mass divided by the mass before immersion was calculated as the gel fraction. Using the calculated gel fraction, the low-temperature curing property after storage was evaluated according to the following evaluation criteria.

[0284] (Evaluation Criteria) ○: Gel fraction was 80% by mass or more △: Gel fraction was 70% by mass or more and less than 80% by mass ×: Gel fraction was less than 70% by mass

[0285] [Rating 5] (water resistance) The resin composition obtained in the above "Preparation of Waterborne Resin Composition" was applied to a glass plate so that the dry film thickness was 40 μm, and then the applied film was dried by heating at 85° C. for 30 minutes to obtain a resin film. 2 mL of ion-exchanged water was dropped onto the obtained resin film, and the film was left at 23° C. for 8 hours. The ion-exchanged water was then wiped off, and the appearance was evaluated according to the following evaluation criteria.

[0286] [Rating 6] (Gel fraction retention rate) The resin composition obtained in the above "Preparation of Waterborne Resin Composition" was stored at 40°C for 5 days. The resin composition after storage was applied to a polypropylene (PP) plate so that the dry film thickness was 40 μm, and then heated and dried at 85°C for 30 minutes to obtain a resin film. The obtained resin film was immersed in acetone at 23°C for 24 hours, and the percentage (mass%) of the value obtained by dividing the undissolved part mass by the mass before immersion was calculated as the gel fraction. The value obtained by dividing the gel fraction obtained by the gel fraction calculated in Evaluation 2 "Low temperature curing property" when heated at 85°C for 30 minutes was calculated as the gel fraction retention. (Evaluation Criteria) ○: Gel fraction retention rate was 85% by mass or more △: Gel fraction retention rate was 80% by mass or more and less than 85% by mass ×: Gel fraction retention rate was less than 80% by mass

[0287] (Evaluation Criteria) ○: No change △: Only blisters occurred ×: Whitening and blistering

[0288] <Synthesis of polyisocyanate> [Synthesis Example 1-1] (Synthesis of Polyisocyanate P-1) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of HDI and 5.3 parts by mass of polyester polyol (polycaprolactone triol) derived from a trihydric alcohol and ε-caprolactone (manufactured by Daicel Chemical Industries, Ltd., "Placcel 303" (trade name), average number of functional groups: 3, number average molecular weight: 300) were charged under a nitrogen gas flow, and the temperature inside the reactor was kept at 89°C for 1 hour under stirring to carry out a urethane reaction. Thereafter, the temperature inside the reactor was kept at 63°C, and an isocyanurate catalyst tetramethylammonium caprylate was added, and when the yield reached 52% by mass, phosphoric acid was added to stop the reaction. After filtering the reaction liquid, unreacted HDI was removed using a thin-film evaporator to obtain an isocyanurate-type polyisocyanate (hereinafter, sometimes referred to as "polyisocyanate P1-1"). The NCO content of the obtained polyisocyanate P-1 was 18.6% by mass, the number average molecular weight was 1220, and the average number of isocyanate groups was 5.4. 1 H-NMR analysis confirmed the presence of isocyanurate groups.

[0289] [Synthesis Example 1-2] (Synthesis of Polyisocyanate P-2) In a four-neck flask equipped with a thermometer, stirring blade, and reflux condenser, 100 parts by mass of HDI was charged under a nitrogen stream, and the temperature inside the reactor was maintained at 60°C while stirring. 0.095 parts by mass of trimethylbenzylammonium hydroxide was added, and after 4.5 hours, when the conversion rate reached 40% by mass, 0.02 parts by mass of phosphoric acid was added to stop the reaction. After filtering the reaction liquid, unreacted HDI was removed using a thin-film evaporator to obtain an isocyanurate-type polyisocyanate (hereinafter, sometimes referred to as "polyisocyanate P-2"). The NCO content of the obtained polyisocyanate P-2 was 22.0% by mass, the number average molecular weight was 655, and the average number of isocyanate groups was 3.4. The obtained polyisocyanate P-2 had the following characteristics: 1 H-NMR analysis confirmed the presence of isocyanurate groups.

[0290] <Production of Blocked Polyisocyanate Component (A)> [Synthesis Example 2-1] (Production of Blocked Polyisocyanate Component A-1) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 87.1 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 30 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 33.0 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, diisopropyl malonate was added to the solution so that it was 70 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1, and dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%. Next, 1.5 parts by mass of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and then the external bath was adjusted so that the solution temperature was 55°C, and the blocking reaction was carried out at 55°C for 6 hours or more. After confirming the disappearance of the peak of the isocyanate group by infrared spectroscopy (IR), a blocked polyisocyanate component A-1 was obtained.

[0291] [Synthesis Example 2-2] (Production of Blocked Polyisocyanate Component A-2) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 29.0 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 10 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 22.8 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, diisopropyl malonate was added to the solution so that the amount was 90 mol% relative to 100 mol% of the isocyanate group of the polyisocyanate P-1, and dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%. Next, 1.3 mass parts of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and the external bath was adjusted so that the solution temperature was 55°C, and the blocking reaction was carried out at 55°C for 6 hours or more. After confirming the disappearance of the peak of the isocyanate group by infrared spectroscopy (IR), a blocked polyisocyanate component A-2 was obtained.

[0292] [Synthesis Example 2-3] (Production of Blocked Polyisocyanate Component A-3) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (trade name)), and 87.1 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 30 mol% relative to 100 mol% of the isocyanate groups of polyisocyanate P-1) were mixed under a nitrogen gas flow, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 80°C, and 3,5-dimethylpyrazole (DPM) was charged so that it was 70 mol% relative to 100 mol% of the isocyanate groups of polyisocyanate P-1, and the external bath was adjusted so that the solution temperature was 80°C, and the blocking reaction was carried out at 80°C for 30 minutes or more. After confirming the disappearance of the isocyanate group peak by infrared spectroscopy (IR), dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass %, thereby obtaining a blocked polyisocyanate component A-3.

[0293] [Synthesis Example 2-4] (Production of Blocked Polyisocyanate Component A-4) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 17.4 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 6 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 20.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the solution so that the content was 94 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was further added to adjust the solid content to 60 mass%. Next, 1.2 mass parts of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and then the external bath was adjusted so that the solution temperature was 55°C, and the blocking reaction was carried out at 55°C for 6 hours or more. After confirming the disappearance of the peak of the isocyanate group by infrared spectroscopy (IR), a blocked polyisocyanate component A-4 was obtained.

[0294] [Synthesis Example 2-5] (Production of Blocked Polyisocyanate Component A-5) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (trade name)), 23.2 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating units: 15, manufactured by Nippon Nyukazai Co., Ltd.): 3.8 parts by mass (2 mol% relative to 100 mol% of the isocyanate groups of Polyisocyanate P-1) and 22.4 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen gas flow, and the mixture was reacted at 120°C for 3 hours. The reaction solution was cooled to 40°C, diisopropyl malonate was added to the mixture so that the amount was 90 mol% relative to 100 mol% of the isocyanate group of the polyisocyanate P-1, and dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%. Next, 1.3 parts by mass of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and the external bath was adjusted so that the solution temperature was 55°C, and the blocking reaction was carried out at 55°C for 6 hours or more. After confirming the disappearance of the peak of the isocyanate group by infrared spectroscopy (IR), a blocked polyisocyanate component A-5 was obtained.

[0295] <Production of Blocked Polyisocyanate Component (B)> [Synthesis Example 3-1] (Production of Blocked Polyisocyanate Component B-1) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1 and diisopropyl malonate were charged under a nitrogen gas flow so that the amount was 100 mol% relative to 100 mol% of the isocyanate groups of the polyisocyanate P-1, and dipropylene glycol dimethyl ether (DPDM) was further added to adjust the solid content to 70 mol%. Next, while stirring, 1.1 parts by mass of a methanol solution containing sodium methylate (28 mol% relative to the total mass of the solution) was dropped, and the external bath was adjusted so that the solution temperature was 55°C, and a blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70 mol%. Then, 168 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate groups) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-1. Regarding the obtained blocked polyisocyanate component B-1, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0296] [Synthesis Example 3-2] (Production of Blocked Polyisocyanate Component B-2) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 0.7 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating units: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 0.25 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 17.8 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the solution so that the amount was 99.75 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was further added to adjust the solid content to 70 mass%. Next, 1.1 parts by mass of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and the external bath was adjusted so that the solution temperature was 55°C, and a blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70 mass%. Then, 168 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-2. Regarding the obtained blocked polyisocyanate component B-2, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0297] [Synthesis Example 3-3] (Production of Blocked Polyisocyanate Component B-3) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 5.8 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 18.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 98 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 165 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-3. Regarding the obtained blocked polyisocyanate component B-3, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0298] [Synthesis Example 3-4] (Production of Blocked Polyisocyanate Component B-4) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 11.6 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 4 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 19.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 96 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 161 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-4. Regarding the obtained blocked polyisocyanate component B-4, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0299] [Synthesis Example 3-5] (Production of Blocked Polyisocyanate Component B-5) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-2 obtained in Synthesis Example 1-2, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 13.9 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 4 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 20.1 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the solution so that the amount was 96 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-2. Dipropylene glycol dimethyl ether (DPDM) was further added to adjust the solid content to 70 mass%. Next, 1.3 parts by mass of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was dropped while stirring, and the external bath was adjusted so that the solution temperature was 55°C, and a blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70 mass%. Then, 192 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-5. Regarding the obtained blocked polyisocyanate component B-5, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0300] [Synthesis Example 3-6] (Production of Blocked Polyisocyanate Component B-6) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 17.4 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating units: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 6 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 54.2 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount of diisopropyl malonate was 94 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70 mass%. Next, 1.2 mass parts of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70 mass%. Then, 158 mass parts of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) were added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-6. The ratio of structure (II-1) to 100 mol% of structure (II) of the obtained blocked polyisocyanate component B-6 was measured and found to be 54 mol%.

[0301] [Synthesis Example 3-7] (Production of Blocked Polyisocyanate Component B-7) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (trade name)), and 6.3 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol% relative to 100 mol% of the isocyanate groups of polyisocyanate P-1) were mixed under a nitrogen gas flow, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 60°C, and 2-ethylimidazole was charged so that the amount was 98 mol% relative to 100 mol% of the isocyanate groups of polyisocyanate P-1, and the external bath was adjusted so that the solution temperature was 60°C, and the blocking reaction was carried out at 60°C for 90 minutes or more. After confirming the disappearance of the isocyanate group peak by infrared spectroscopy (IR), dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass %, thereby obtaining blocked polyisocyanate component B-7.

[0302] [Synthesis Example 3-8] (Production of Blocked Polyisocyanate Component B-8) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (trade name)), 14.5 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating units: 15, manufactured by Nippon Nyukazai Co., Ltd.): 1.9 parts by mass (1 mol% amount relative to 100 mol% of the isocyanate groups of Polyisocyanate P-1) and 20.5 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen gas flow, and the mixture was reacted at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 94 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 160 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-8. Regarding the obtained blocked polyisocyanate component B-8, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%.

[0303] [Synthesis Example 3-9] (Production of Blocked Polyisocyanate Component B-9) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 27.1 parts by mass of poly(oxyethylene, oxypropylene) glycol monobutyl ether (average molecular weight: 970) (hereinafter, sometimes abbreviated as "EO-PO") (an amount equivalent to 6 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 22.4 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 94 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 158 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-9. Regarding the obtained blocked polyisocyanate component B-9, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%. [Synthesis Example 3-10] (Production of Blocked Polyisocyanate Component B-10) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.02 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 87.1 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating units: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 30 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 33.0 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 70 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70 mass%. Next, 1.5 parts by mass of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70 mass%. Then, 118 parts by mass of 2-methyl-2-butanol (400 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-10. Regarding the obtained blocked polyisocyanate component B-10, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 54 mol%. [Synthesis Example 3-11] (Production of Blocked Polyisocyanate Component B-11) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 5.8 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 18.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 98 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 82.4 parts by mass of 2-methyl-2-butanol (200 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 1 hour while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-11. Regarding the obtained blocked polyisocyanate component B-11, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 5 mol%. [Synthesis Example 3-12] (Production of Blocked Polyisocyanate Component B-12) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 5.8 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 18.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 98 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 82.4 parts by mass of 2-methyl-2-butanol (200 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 80°C for 3 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-12. Regarding the obtained blocked polyisocyanate component B-12, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 25 mol%. [Synthesis Example 3-13] (Production of blocked polyisocyanate component B-13) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 5.8 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 18.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and diisopropyl malonate was added to the mixture so that the amount was 98 mol% relative to 100 mol% of the isocyanate group of polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 70% by mass. Next, 1.2 parts by mass of a methanol solution containing sodium methylate (28% by mass relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. Blocking reaction was carried out at 55°C for 5 hours to obtain a blocked polyisocyanate component intermediate with a solid content of 70% by mass. Then, 82.4 parts by mass of 2-methyl-2-butanol (200 mol% relative to the blocked isocyanate group) was added, and the reaction was carried out at 100°C for 8 hours while removing the generated isopropyl alcohol by distillation under normal pressure. Thereafter, isopropanol and 2-methyl-2-butanol were further distilled off under reduced pressure (50 kPa) at 60°C, and finally, dipropylene glycol dimethyl ether (DPDM) was added to adjust the solid content to 60 mass%, thereby obtaining blocked polyisocyanate component B-13. Regarding the obtained blocked polyisocyanate component B-13, the ratio of structure (II-1) to 100 mol% of structure (II) was measured and found to be 74 mol%. [Synthesis Example 3-14] (Production of Blocked Polyisocyanate Component B-14) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 100 parts by mass of the polyisocyanate P-1 obtained in Synthesis Example 1-1, 0.01 parts by mass of 2-ethylhexyl acid phosphate (manufactured by Johoku Chemical Industry Co., Ltd., "JP-508T" (product name)), 5.8 parts by mass of methoxypolyethylene glycol (MPG-081, ethylene oxide repeating unit: 15, manufactured by Nippon Nyukazai Co., Ltd.) (amount equivalent to 2 mol % relative to 100 mol % of the isocyanate groups of Polyisocyanate P-1), and 18.7 parts by mass of dipropylene glycol dimethyl ether (DPDM) were mixed under a nitrogen stream, and the reaction was carried out at 120°C for 3 hours. The reaction solution was cooled to 40°C, and di-tert-butyl malonate was added to the mixture so that the content was 98 mol% relative to 100 mol% of the isocyanate group of the polyisocyanate P-1. Dipropylene glycol dimethyl ether (DPDM) was then added to adjust the solid content to 60 mass%. Next, 1.2 mass parts of a methanol solution containing sodium methylate (28 mass% relative to the total mass of the solution) was added dropwise while stirring, and the external bath was adjusted so that the solution temperature was 55°C. The solution was then subjected to a blocking reaction at 55°C for 6 hours or more. After confirming the disappearance of the peak of the isocyanate group by infrared spectroscopy (IR), a blocked polyisocyanate component B-14 was obtained.

[0304] [Example 1] (Production of Blocked Polyisocyanate Composition BL-a1) A four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser was charged with 25 parts by mass of the blocked polyisocyanate component A-1 obtained in Synthesis Example 2-1 and 75 parts by mass of the blocked polyisocyanate component B-1 obtained in Synthesis Example 3-1 under a nitrogen gas flow, the external bath was adjusted so that the solution temperature was 40°C, and the mixture was mixed at 40°C for 1 hour or more to obtain a blocked polyisocyanate composition BL-a1.

[0305] [Examples 2 to 15, 18 to 23 and Comparative Example 3] (Production of Blocked Polyisocyanate Compositions BL-a2 to BL-a15, BL-a18 to BL-a23, and BL-b3) Each blocked polyisocyanate composition was produced in the same manner as in Example 1, except that the combinations and mixing ratios of the blocked polyisocyanate components (A) and (B) to be blended were as shown in Tables 1 to 4.

[0306] [Example 16] (Production of blocked polyisocyanate composition BL-a16) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 25 parts by mass of the blocked polyisocyanate component A-1 obtained in Synthesis Example 2-1 and 75 parts by mass of the blocked polyisocyanate component B-1 obtained in Synthesis Example 3-1 were charged under a nitrogen gas flow, the external bath was adjusted so that the solution temperature was 40° C., and the mixture was mixed at 40° C. for 1 hour or more. Then, 2.0 parts by mass of an anionic surfactant (polyoxyethylene polycyclic phenyl ether sulfate ammonium salt (polyoxyethylene (oxyethylene repeat number n=10-15) alkyl (alkyl carbon number C=1,8,9) (mono- to penta) styryl-phenyl ether sulfate ammonium salt) (surface tension at 25° C. 40.3 mN / m)) was added, and the mixture was mixed for 15 minutes to obtain a blocked polyisocyanate composition BL-a16.

[0307] [Example 17] (Production of blocked polyisocyanate composition BL-a17) In a four-neck flask equipped with a thermometer, a stirring blade, and a reflux condenser, 25 parts by mass of the blocked polyisocyanate component A-1 obtained in Synthesis Example 2-1 and 75 parts by mass of the blocked polyisocyanate component B-1 obtained in Synthesis Example 3-1 were charged under a nitrogen gas flow, the external bath was adjusted so that the solution temperature was 40° C., and the mixture was mixed for 1 hour or more at 40° C. Then, 2.0 parts by mass of a nonionic surfactant (manufactured by Nippon Nyukazai Co., Ltd., "Newcol 714" (trade name), polyoxyethylene polycyclic phenyl ether, HLB=15.0) was added, and the mixture was mixed for 15 minutes to obtain a blocked polyisocyanate composition BL-a17.

[0308] [Comparative Example 1] (Production of Blocked Polyisocyanate Composition BL-b1) The blocked polyisocyanate component A-4 obtained in Synthesis Example 2-4 was used as it was as blocked polyisocyanate composition BL-b1.

[0309] [Comparative Example 2] (Production of blocked polyisocyanate composition BL-b2) The blocked polyisocyanate component B-6 obtained in Synthesis Example 3-6 was used as it was as blocked polyisocyanate composition BL-b2.

[0310] [Comparative Example 4] (Production of blocked polyisocyanate composition BL-b4) The blocked polyisocyanate component B-8 obtained in Synthesis Example 3-8 was used as it was as blocked polyisocyanate composition BL-b4.

[0311] [Comparative Example 5] (Production of blocked polyisocyanate composition BL-b5) The blocked polyisocyanate component B-9 obtained in Synthesis Example 3-9 was used as it was as blocked polyisocyanate composition BL-b5.

[0312] The results of various evaluations of the blocked polyisocyanate compositions obtained in the Examples and Comparative Examples are shown in Tables 1 to 4 below.

[0313] [Table 1]

[0314] [Table 2]

[0315] [Table 3]

[0316] [Table 4]

[0317] As shown in Tables 1 to 4, in the blocked polyisocyanate compositions BL-a1 to BL-a23 (Examples 1 to 23) containing components (A) and (B), the content of the nonionic hydrophilic group of the blocked polyisocyanate composition is within a specific numerical range, the content of the nonionic hydrophilic group of component (A) is greater than the content of the nonionic hydrophilic group of component (B), the blocked isocyanate structure of component (A) and the blocked isocyanate structure of component (B) are different from each other, and the curing temperature at which the gel fraction reaches 80 mass% or more is higher for component (A) than for component (B), the compositions had good dispersibility in the aqueous resin composition, a small amount of gas generated during storage when made into an aqueous resin composition, excellent low-temperature curing properties and low-temperature curing properties after storage, excellent maintenance of curing properties (gel fraction retention), and excellent water resistance when made into a resin film. Furthermore, in a comparison of blocked polyisocyanate compositions BL-a1, BL-a2, and BL-a5 (Examples 1, 2, and 5) in which the mixing ratios of components (A) and (B) were similar, ranging from 24 / 76 to 27 / 73, and components (B) having different contents of nonionic hydrophilic groups were blended, it was found that the greater the content of nonionic hydrophilic groups in component (B), the better the dispersibility in the aqueous resin composition and the low-temperature curing property after storage, the better the maintenance of curing properties (gel fraction retention), and the smaller the amount of gas generated during storage when made into an aqueous resin composition, which tended to be better. In a comparison of blocked polyisocyanate compositions BL-a4 and BL-a8 (Examples 4 and 8), which had similar mixing ratios of components (A) and (B) of 18 / 82 to 19 / 81 and contained components (B) with different contents of nonionic hydrophilic groups, there was a tendency that the dispersibility in the aqueous resin composition became better as the content of nonionic hydrophilic groups in component (B) increased, whereas there was a tendency that the curability when formed into a resin film became better as the content of nonionic hydrophilic groups in component (B) decreased. In comparing blocked polyisocyanate compositions BL-a4 to BL-a7 (Examples 4 to 7) with different mixing ratios of component (A) and component (B), it was found that the dispersibility in the aqueous resin composition, the amount of gas generated during storage when made into an aqueous resin composition, and the low-temperature curing property after storage tended to be better as the mixing ratio of component (A) increased, while the curing property when made into a resin film tended to be better as the mixing ratio of component (B) increased. In a comparison of blocked polyisocyanate compositions BL-a8 and BL-a9 (Examples 8 and 9) which contain component (B) having a different type of raw material polyisocyanate, the blocked polyisocyanate composition BL-a8 which contains component (B) using a raw material polyisocyanate having a larger average number of isocyanate groups tended to be more excellent in dispersibility in an aqueous resin composition and low-temperature curing properties. In a comparison of blocked polyisocyanate compositions BL-a12, BL-a16, and BL-a17 (Examples 12, 16, and 17) which differ in the presence or absence of added anionic surfactant or nonionic surfactant, it was observed that the addition of an anionic surfactant or a nonionic surfactant tended to result in better dispersibility.

[0318] On the other hand, the blocked polyisocyanate composition BL-b1 (Comparative Example 1) containing only the component (A) had good dispersibility in the aqueous resin composition, generated a small amount of gas during storage when made into an aqueous resin composition, and had excellent low-temperature curing properties after storage, but had poor low-temperature curing properties and water resistance when made into a resin film. Blocked polyisocyanate compositions BL-b2, BL-b4, and BL-b5 containing only component (B) (Comparative Examples 2, 4, and 5) had good dispersibility in an aqueous resin composition and were excellent in low-temperature curing properties when made into an aqueous resin composition and in water resistance when made into a resin film. However, they generated a large amount of gas during storage and were poor in low-temperature curing properties after storage and in maintenance of curing properties (gel fraction retention). Blocked polyisocyanate composition BL-b3 (Comparative Example 3), which contains components (A) and (B) but in which the content of nonionic hydrophilic groups in component (A) is the same as the content of nonionic hydrophilic groups in component (B), had good dispersibility in an aqueous resin composition, generated a small amount of gas during storage when made into an aqueous resin composition, and had excellent low-temperature curing properties and water resistance when made into a resin film; however, the low-temperature curing properties and maintenance of curing properties (gel fraction retention) after storage were poor. [Industrial Applicability]

[0319] According to the blocked polyisocyanate composition of the present embodiment, it is possible to provide a blocked polyisocyanate composition that has good dispersibility in an aqueous resin composition, has excellent curability and curability maintenance (gel fraction retention) when baked at a low temperature of 90°C or less immediately after preparation and after storage, has a suppressed amount of gas generation when stored as an aqueous resin composition, and has excellent water resistance when formed into a resin film. The resin composition of the present embodiment contains the blocked polyisocyanate composition, has excellent curability and curability maintenance (gel fraction retention) when baked at a low temperature of 90°C or less immediately after preparation and after storage, has a suppressed amount of gas generation when stored, and has excellent water resistance when formed into a resin film. In addition, the resin composition of the present embodiment has excellent low-temperature curability and curability maintenance (gel fraction retention), and can provide a resin film with excellent water resistance, and is therefore suitable for use in coating materials with low heat resistance.

Claims

1. A blocked polyisocyanate composition comprising a blocked polyisocyanate component (A) and a blocked polyisocyanate component (B), When the nonionic hydrophilic group content of the blocked polyisocyanate component (A) is (a) mass %, and the nonionic hydrophilic group content of the blocked polyisocyanate component (B) is (b) mass %, the relationship of 0≦(b)<(a) is satisfied, The structure (Y) of the blocked isocyanate group of the blocked polyisocyanate component (B) is a structure represented by the following general formula (II), and the blocked polyisocyanate composition contains 1 mol % or more of the structure represented by the following general formula (II-1) relative to 100 mol % of the structure represented by the following general formula (II): 【Chemistry 1】 (In general formula (II), R 21 , R 22 , R 23 , R 24 , R 25 and R 26 each independently represent a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. The wavy lines represent bonds.) 【Chemistry 2】 (In general formula (II-1), R 211 , R 212 , and R 213 each independently represent an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxy group and an amino group. The total number of carbon atoms in R 211 , R 212 , and R 213 is 3 to 20. R 214 , R 215 , and R 216 each independently represent a hydrogen atom, or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxy group and an amino group. The wavy lines represent bonds.)

2. The nonionic hydrophilic group content (a) of the blocked polyisocyanate component (A) is 1.0 to 55.0 mass %, The nonionic hydrophilic group content (b) of the blocked polyisocyanate component (B) is 0 to 20.0 mass %, (a) / (b) is 100 / 0 to 60 / 40; and The blocked polyisocyanate composition according to claim 1, wherein the mass ratio (A) / (B) of component (A) to component (B) is 1 / 99 to 99 / 1.

3. 3. The blocked polyisocyanate composition according to claim 1, wherein the nonionic hydrophilic group content of the blocked polyisocyanate composition is 0.1% by mass or more and 25.0% by mass or less, based on the total mass of the solid content of the blocked polyisocyanate composition.

4. The blocked polyisocyanate composition according to claim 1 or 2, wherein the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) and the structure (Y) of the blocked isocyanate group of the blocked polyisocyanate component (B) are different from each other.

5. The blocked polyisocyanate composition according to claim 1 or 2, which satisfies 0<(b)<(a).

6. The curing temperatures at which the gel fraction in the resin film using each of the blocked polyisocyanate components (A) and (B) reaches 80 mass % or more are respectively defined as (A T1 ) and (B T1 ), then (A T1 )>(B T1 ) relationship, 5. The blocked polyisocyanate composition according to claim 4, wherein the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are each mixed with an acrylic polyol having a hydroxyl group content of 4.5% by mass so that a ratio NCO / OH of the molar amount of isocyanate groups in the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) to the molar amount of hydroxyl groups in the acrylic polyol is 1.0, and the solid content is adjusted with butyl acetate to 50% by mass. Each of the adjusted solutions obtained is applied to a polypropylene plate so as to have a dry film thickness of 40 μm, and the resulting resin film is dried by heating at a temperature of 80° C. or higher in 5° C. increments for 30 minutes. The gel fraction is expressed as a percentage obtained by dividing a mass of an undissolved portion by a mass before immersion in acetone at 23° C. for 24 hours.

7. The curing temperatures at which the gel fraction in the resin film using each of the blocked polyisocyanate components (A) and (B) reaches 80 mass % or more are respectively defined as (A T2 ) and (B T2 ), then (A T2 )>(B T2 ) relationship, 5. The blocked polyisocyanate composition according to claim 4, wherein the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are each mixed with a polycaprolactone triol having a number average molecular weight of 850 so that a ratio NCO / OH of the molar amount of isocyanate groups in the blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) to the molar amount of hydroxyl groups in the polycaprolactone triol is 1.0, and the solid content is adjusted with butyl acetate to 50 mass %, and each of the adjusted solutions obtained is applied to a polypropylene plate so as to have a dry film thickness of 40 μm, and the resulting resin film is heated and dried for 30 minutes at a temperature of 80° C. or higher in 5° C. increments, and then the resulting resin film is immersed in acetone at 23° C. for 24 hours, and the gel fraction is expressed as a percentage obtained by dividing the mass of the undissolved portion by the mass before immersion.

8. In the general formula (II), the R 24 , the R 25 and the R 26 The blocked polyisocyanate composition according to claim 1 or 2, wherein one of the above is a hydrogen atom.

9. In the general formula (II-1), the R 211 , the R 212 and the R 213 The blocked polyisocyanate composition according to claim 1 or 2, wherein the total carbon number of the above is 4 or more and 20 or less.

10. The blocked polyisocyanate composition according to claim 4, wherein the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) is one or more structures selected from the group consisting of a structure represented by the following general formula (III) and a structure represented by the following general formula (IV): 【Chemistry 3】 (In general formula (III), R 31 , R 32 , R 33 , R 34 , R 35 and R 36 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxyl group and an amino group. 31 , the R 32 and the R 33 At least one of the R 34 , the R 35 and the R 36 At least one of these is a hydrogen atom. The wavy lines represent the bonding sites with the residues of polyisocyanate excluding the isocyanate groups.) 【Chemistry 4】 (In general formula (IV), R 41 , R 42 and R 43 are each independently a hydrogen atom or an alkyl group which may contain one or more substituents selected from the group consisting of a hydroxy group and an amino group. The wavy lines represent the bonding sites with the residues of polyisocyanate excluding the isocyanate groups.)

11. The blocked polyisocyanate component (A) and the blocked polyisocyanate component (B) are derived from a polyisocyanate and a blocking agent, respectively; 5. The blocked polyisocyanate composition according to claim 4, wherein the polyisocyanate is a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates.

12. The blocked polyisocyanate composition according to claim 11, wherein the polyisocyanate has an average number of isocyanate groups of 3.5 or more.

13. The blocked polyisocyanate composition according to claim 1 or 2, wherein the structure (X) of the blocked isocyanate group of the blocked polyisocyanate component (A) is the same as the structure (Y) of the blocked isocyanate group of the blocked polyisocyanate component (B).

14. A resin composition comprising the blocked polyisocyanate composition according to claim 4 and a polyhydric hydroxy compound.

15. A resin film obtained by curing the resin composition according to claim 14.

16. A laminate comprising one or more layers of the resin film according to claim 15 laminated on a substrate, The thickness of each of the resin films is 1 μm or more and 50 μm or less.

Citation Information

Patent Citations

  • Blocked polyisocyanate composition and one-package thermosetting composition containing the same

    JP1997278865A

  • Block isocyanate group-containing resin composition and thermosetting composition containing the same

    JP2002322238A

  • Blocked polyisocyanate composition and one-component coating composition

    JP2006335954A

  • Aqueous blocked polyisocyanate, fiber treatment agent composition, and fiber

    JP2014065833A

  • Polarizer protective film, polarizing plate, and image display device

    JP2015106067A