Solder film, optical device components, and optical devices
The Au-Sn alloy solder film with a concentration gradient and multilayer structure addresses the issues of surface flatness and adhesion in optical devices, ensuring reliable bonding and reducing warpage, thereby improving device reliability.
Patent Information
- Application Number
- JP2020125105
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-22
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-07-22
AI Technical Summary
Existing solder films used in optical devices lack sufficient surface flatness and adhesion, leading to warpage and potential peeling or displacement of optical components, which compromises the reliability of the devices.
A solder film composed of an Au-Sn alloy with a concentration gradient in the thickness direction, combined with a multilayer structure and optional adhesive layers, enhances surface flatness and bonding strength, reducing warpage and improving adhesion.
The Au-Sn alloy film with a concentration gradient and multilayer structure provides excellent surface flatness, suppresses warpage, and ensures reliable bonding of optical components to mounting boards, enhancing the overall reliability of optical devices.
Smart Images

Figure 0007581684000002 
Figure 0007581684000003 
Figure 0007581684000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a solder film, and an optical device component and an optical device using the solder film. [Background technology]
[0002] In recent years, optical devices equipped with optical elements such as LDs (Laser Diodes) and LEDs (Light Emitting Diodes) have been used in applications such as displays, projectors, and automobile headlamps. In optical devices, components such as optical elements are fixed to a mounting substrate using a solder film. As the solder film, for example, a solder film containing Au and Sn is known.
[0003] For example, the following Patent Document 1 discloses a method for bonding an optical semiconductor element onto a mounting board using an AuSn multilayer solder in which Au layers and Sn layers are alternately laminated. In the AuSn multilayer solder of Patent Document 1, a total of seven Au layers and Sn layers are laminated.
[0004] Furthermore, the following Patent Document 2 discloses a method for forming a solder film containing Au and Sn, in which an evaporation source made of alloyed AuSn is heated at a first temperature to selectively evaporate Sn to form a Sn-rich first layer, and then the evaporation source is further heated at a second temperature higher than the first temperature to form a Au-rich second layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-006073 [Patent Document 2] JP 2008-263130 A Summary of the Invention [Problem to be solved by the invention]
[0006] In addition to optical elements, optical devices may also be equipped with submounts for mounting optical elements, components such as prisms, etc., and solder films are often used for bonding these components. However, the solder films of Patent Documents 1 and 2 do not have a sufficiently flat surface, and may not be able to sufficiently increase adhesion when fixing the above-mentioned components to a mounting substrate or the like. In addition, warping may occur due to the film stress of the solder film, and this may also prevent adhesion from being increased. In this case, the optical elements or prisms may peel off from the mounting substrate, or the optical elements or prisms may be displaced in the height direction. Therefore, there is a problem that the reliability of the optical device cannot be sufficiently increased.
[0007] An object of the present invention is to provide a solder film that has excellent surface flatness and is capable of suppressing warping, and an optical device component and an optical device that use the solder film. [Means for solving the problem]
[0008] The solder film of the present invention is a solder film used for fixing components in an optical device, and is characterized in that it comprises an Au-Sn alloy film, and the Au-Sn alloy film has a concentration gradient of Au and Sn in the thickness direction.
[0009] In the present invention, it is preferable that the Au-Sn alloy film has opposing first and second main surfaces, the first main surface being the main surface on the side on which the component is provided, the second main surface being the outer main surface opposite the side on which the component is provided, the direction connecting the first and second main surfaces being the thickness direction, and in the thickness direction, the concentration of Sn on the first main surface side is greater than the concentration of Au, and the concentration of Sn on the second main surface side is less than the concentration of Au.
[0010] In the present invention, the Au-Sn alloy film is preferably a vapor deposition film deposited using an Au-Sn alloy as a vapor deposition source.
[0011] In the present invention, the total mass of Au in the Au-Sn alloy film is M A The total mass of Sn is M S When the mass ratio of Au to the total mass of Au and Sn is M A / (M A +M S ) is preferably 0.60 or more and 0.90 or less.
[0012] In the present invention, it is preferable that the multilayer film is provided in which a plurality of the Au—Sn alloy films are laminated. It is more preferable that the number of the laminated Au—Sn alloy films in the multilayer film is 1 or more and 30 or less.
[0013] In the present invention, it is preferable to further include an adhesive film provided between the component and the Au-Sn alloy film. More preferably, the adhesive film has a first layer provided on the component side and containing at least one selected from the group consisting of Cr, Ti, and Ni, a second layer provided on the first layer and containing at least one selected from the group consisting of Ni, Pt, Pd, and Ni-Cr alloy, and a third layer provided on the second layer and containing Pt or Au.
[0014] In the present invention, it is preferable that the substrate further comprises an Au film provided on a main surface of the Au-Sn alloy film opposite to the component side, the Au film being the outermost layer.
[0015] In the present invention, the solder film preferably has an arithmetic mean surface roughness Ra of 0.05 μm or less.
[0016] In the present invention, it is preferable that the maximum surface height Rz of the solder film is 0.25 μm or less.
[0017] In the present invention, it is preferable that the entire solder film has a thickness of 1 μm or more and 10 μm or less.
[0018] An optical device component according to the present invention is characterized by comprising a component body having a main surface, and a solder film configured according to the present invention provided on the main surface of the component body.
[0019] In the present invention, the optical device part is preferably at least one selected from the group consisting of a prism, an optical element, a submount for mounting the optical element, and a packaging member for mounting the optical element.
[0020] The optical device of the present invention comprises a prism, an optical element that emits light to the prism or receives light from the prism, a package in which the prism and the optical element are mounted, and a submount provided between the optical element and the package, and is characterized in that the prism and the package are bonded together, the optical element and the submount are bonded together, the submount and the package are bonded together, or the components that make up the package are bonded together by a solder film configured according to the present invention. Effect of the Invention
[0021] According to the present invention, it is possible to provide a solder film having excellent surface flatness and capable of suppressing warping, and an optical device component and an optical device using the solder film. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic cross-sectional view showing a solder film and an optical device component according to a first embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view showing an enlarged view of a portion where a solder film is provided according to the first embodiment of the present invention. FIG. [Diagram 3] 1A to 1C are diagrams for explaining a method for producing an Au—Sn alloy film. [Figure 4] 6 is a schematic cross-sectional view showing an enlarged view of a portion where a solder film is provided according to a second embodiment of the present invention. FIG. [Diagram 5] FIG. 11 is a schematic cross-sectional view showing an enlarged view of a portion where a solder film is provided according to a third embodiment of the present invention. [Figure 6] 1 is a schematic cross-sectional view showing an optical device according to an embodiment of the present invention. [Figure 7] 1(a) to 1(c) are schematic diagrams illustrating a method for measuring warpage in a film-coated substrate. [Figure 8] 2 is a SEM photograph showing a cross section of the solder film obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Preferred embodiments will be described below. However, the following embodiments are merely examples, and the present invention is not limited to the following embodiments. In addition, in each drawing, components having substantially the same functions may be referred to by the same reference numerals.
[0024] [Solder film and optical device components] (First embodiment) Fig. 1 is a schematic cross-sectional view showing a solder film and an optical device component according to a first embodiment of the present invention, Fig. 2 is a schematic cross-sectional view showing an enlarged view of a portion where the solder film according to the first embodiment of the present invention is provided.
[0025] The prism 10 is an optical device component used in an optical device. The prism 10 includes a prism body 11, a solder film 1, and a reflective film 12.
[0026] Prism body 11 has a substantially trapezoidal cross-sectional shape. Prism body 11 has a bottom surface 11a, an inclined surface 11b connected to bottom surface 11a, and an upper surface 11c facing bottom surface 11a and connected to inclined surface 11b. The cross-sectional shape of prism body 11 is not particularly limited, and may be substantially triangular, etc. In this embodiment, prism body 11 is made of an appropriate glass material.
[0027] A reflective film 12 is provided on the inclined surface 11b of the prism body 11. The reflective film 12 is made of, for example, a dielectric multilayer film in which high refractive index films and low refractive index films are alternately laminated. Examples of materials for the high refractive index film include TiO 2 , Ta 2 O 5 , ZrO 2 , or HfO 2 Examples of the material for the low refractive index film include SiO 2 or MgF 2 Examples of the reflective film 12 include the following. The reflective film 12 may be a single-layer metal film, and is not particularly limited. The reflective film 12 may be provided on at least a part of the inclined surface 11b of the prism body 11, and may be provided on the entire surface of the inclined surface 11b, for example. By providing the reflective film 12 on the inclined surface 11b, the light emitted from the light source can be appropriately reflected. However, the reflective film 12 does not necessarily have to be provided. The reflective film 12 can be formed by stacking each layer by, for example, a sputtering method or a vacuum deposition method.
[0028] Furthermore, a solder film 1 is provided on the bottom surface 11a of the prism body 11. The prism 10, which is a component for an optical device, is fixed to a mounting board, a package, or the like by the solder film 1. Although the solder film 1 is preferably provided on the entire bottom surface 11a of the prism body 11, it is sufficient that the solder film 1 is provided on at least a part of the bottom surface 11a of the prism body 11. The solder film 1 may also wrap around to the side surface of the prism body 11. In that case, the bonding strength provided by the solder film 1 can be further increased.
[0029] 2, the solder film 1 is composed of a multilayer film 2 in which a plurality of Au—Sn alloy films 3 are laminated. The Au—Sn alloy film 3 is a film made of an alloy of Au and Sn.
[0030] The Au—Sn alloy film 3 has a first main surface 3a and a second main surface 3b facing each other. The first main surface 3a is the main surface on the prism body 11 side. The second main surface 3b is the outer main surface opposite the prism body 11. The direction connecting the first main surface 3a and the second main surface 3b is the thickness direction of the solder film 1.
[0031] In the Au-Sn alloy film 3, the Sn concentration is higher than the Au concentration on the first principal surface 3a side in the thickness direction. Also, the Sn concentration is lower than the Au concentration on the second principal surface 3b side. Therefore, the Au-Sn alloy film 3 has a concentration gradient of Au and Sn in the thickness direction.
[0032] In this specification, the Au or Sn concentration on the first main surface 3a side of the Au-Sn alloy film 3 refers to the Au or Sn concentration in a 50% thickness portion of the Au-Sn alloy film 3 from the first main surface 3a. Also, the Au or Sn concentration on the second main surface 3b side of the Au-Sn alloy film 3 refers to the Au or Sn concentration in a 50% thickness portion of the Au-Sn alloy film 3 from the second main surface 3b. Also, the Au or Sn concentration on each main surface side of the Au-Sn alloy film 3 can be measured by, for example, SEM-EDX.
[0033] In this specification, the Au-Sn alloy film 3 having a Au concentration gradient refers to a case where the Au concentration (mass ratio to the entire metal) on the first main surface 3a side of the Au-Sn alloy film 3 differs by 15% or more from the concentration (mass ratio to the entire metal) on the second main surface 3b side of the Au-Sn alloy film 3. However, it is preferable that the Au concentration increases from the first main surface 3a side toward the second main surface 3b side in the thickness direction of the Au-Sn alloy film 3.
[0034] The Au-Sn alloy film 3 having a Sn concentration gradient refers to a case in which the Sn concentration (mass ratio to the entire metal) on the first principal surface 3a side of the Au-Sn alloy film 3 differs by 10% or more from the Sn concentration (mass ratio to the entire metal) on the second principal surface 3b side of the Au-Sn alloy film 3. However, it is preferable that the Sn concentration in the Au-Sn alloy film 3 increases from the second principal surface 3b side toward the first principal surface 3a side in the thickness direction.
[0035] The solder film 1 of this embodiment includes an Au-Sn alloy film 3, which is an alloy of Au and Sn, and the Au-Sn alloy film 3 has a concentration gradient of Au and Sn in the thickness direction. Therefore, the solder film 1 has excellent surface flatness and can suppress warping. This can be explained as follows.
[0036] Conventionally, in solder films in which Au and Sn layers are alternately laminated, the Sn layers can undergo crystal growth when exposed to thermal energy, or can be affected by oxidation, causing the film surface to become rough.
[0037] In contrast, the solder film 1 of this embodiment includes the Au-Sn alloy film 3, so that the influence of crystal growth and oxidation caused by thermal energy can be reduced, and as a result, the film surface 1a can be made flatter. In addition, the concentration of Sn on the second main surface 3b side is reduced, so that the film surface 1a side can be made less susceptible to oxidation, and as a result, the film surface 1a can be made flat. Therefore, the solder film 1 can increase the bonding strength when mounting the prism 10, which is an optical device component, on a package or the like. In addition, since the concentration of Au on the film surface 1a side is increased, when an Au film is formed on the surface of a package or the like, as in the embodiment described later, the bonding strength of the solder film 1 can be further increased.
[0038] In addition, in the past, in a solder film in which Au layers and Sn layers are alternately laminated, warping may occur due to film stress caused by the difference in thermal expansion coefficient of each layer. In contrast, the solder film 1 of this embodiment is composed of an already alloyed Au-Sn alloy film 3, so film stress caused by the difference in thermal expansion coefficient of Au and Sn is unlikely to occur, and warping is unlikely to occur. In addition, when composed of a multilayer film 2 of Au-Sn alloy films 3 as in this embodiment, the thickness of each layer can be made thin, so that the film stress generated near the interface with the prism body 11 can also be reduced, and warping can be further suppressed.
[0039] Furthermore, since the solder film 1 of this embodiment is composed of the already alloyed Au-Sn alloy film 3, it can be bonded reliably in a short time when mounting the prism 10, which is an optical device component, in a package, etc. In addition, when it is composed of the multilayer film 2 of the Au-Sn alloy film 3 as in this embodiment, the thickness of each layer can be made thin, so that it can be bonded reliably in a shorter time.
[0040] In this embodiment, the Au-Sn alloy film 3 preferably contains 95 mass% or more of Au and Sn. Depending on the degree of refining Au and Sn, impurities such as Fe, Cr, Ni, etc. may be mixed into the alloy layer. In this case, it has been confirmed that the effect of the present invention is not impaired if the content of Au and Sn is 95 mass% or more.
[0041] In this embodiment, the mass ratio of Au to Sn (Au / Sn) on the first main surface 3a side of the Au-Sn alloy film 3 is preferably 60 / 40 or more, and preferably 70 / 30 or less. The mass ratio of Au to Sn (Au / Sn) on the second main surface 3b side of the Au-Sn alloy film 3 is preferably 75 / 25 or more, and preferably 95 / 5 or less. When the mass ratios (Au / Sn) on the first main surface 3a side and the second main surface 3b side of the Au-Sn alloy film 3 are within the above range, the film surface 1a can be made flatter, and the bonding strength of the solder film 1 can be further increased.
[0042] In this embodiment, the thickness of each layer in the Au-Sn alloy film 3 is preferably 1 μm or less, more preferably 500 nm or less. When the thickness of each layer in the Au-Sn alloy film 3 is equal to or less than the above upper limit, the film surface 1a of the solder film 1 can be made even flatter, and warping due to film stress can be further suppressed. In addition, when mounting, bonding can be performed more reliably in a shorter time. On the other hand, the lower limit of the thickness of each layer in the Au-Sn alloy film 3 is not particularly limited, but can be, for example, 30 nm. If the thickness of each layer in the Au-Sn alloy film 3 is smaller than the above lower limit, it may be difficult to form each layer.
[0043] In this embodiment, the thickness of the multilayer film 2 is preferably 10 μm or less, more preferably 6 μm or less. When the thickness of the multilayer film 2 is equal to or less than the above upper limit, the film surface 1a of the solder film 1 can be made even flatter, and warping due to film stress can be further suppressed. In addition, during mounting, bonding can be achieved more reliably in a shorter time. On the other hand, the lower limit of the thickness of the multilayer film 2 is not particularly limited, but can be set to, for example, 1 μm. When the thickness of the multilayer film 2 is smaller than the above lower limit, each layer becomes too thin, which may make it difficult to form each layer.
[0044] In this embodiment, the total number of layers of the Au-Sn alloy film 3 in the multilayer film 2 is preferably 1 or more, more preferably 5 or more, preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less. When the total number of layers of the Au-Sn alloy film 3 in the multilayer film 2 is equal to or greater than the above lower limit, warping due to membrane stress can be further suppressed. Also, bonding can be performed more quickly and reliably during mounting. When the total number of layers of the Au-Sn alloy film 3 in the multilayer film 2 is equal to or less than the above upper limit, each layer can be formed more easily, and productivity can be further improved.
[0045] In this embodiment, the total thickness of the solder film 1 is not particularly limited, but is preferably 1 μm or more, more preferably 3 μm or more, preferably 10 μm or less, and more preferably 6 μm or less. When the total thickness of the solder film 1 is equal to or greater than the above lower limit, the bonding strength of the solder film 1 can be further increased when mounting the solder film 1 on a package or the like. When the total thickness of the solder film 1 is equal to or less than the above upper limit, warping due to film stress can be further suppressed. Furthermore, when mounting the solder film 1, the solder film 1 can be reliably bonded in a shorter time. In this case, the positional deviation of the prism body 11 in the height direction is reduced, so that the positional accuracy of the prism 10, which is a component for an optical device, can be further effectively improved.
[0046] In this embodiment, the arithmetic mean roughness Ra of the film surface 1a of the solder film 1 is preferably 0.05 μm or less, more preferably 0.01 μm or less. When the arithmetic mean roughness Ra of the film surface 1a of the solder film 1 is equal to or less than the above upper limit, the adhesion between the solder film 1 and a package or the like can be further improved, and the joining strength of the solder film 1 can be further improved. The lower limit of the arithmetic mean roughness Ra of the film surface 1a of the solder film 1 is not particularly limited, but can be, for example, 0.005 μm. The arithmetic mean roughness Ra can be measured in accordance with JIS B 0601:2013.
[0047] In this embodiment, the maximum height Rz of the solder film 1 on the film surface 1a is preferably 0.25 μm or less, and more preferably 0.10 μm or less. When the maximum height Rz of the solder film 1 on the film surface 1a is equal to or less than the above upper limit, the adhesion between the solder film 1 and a package or the like can be further improved, and the joining strength of the solder film 1 can be further increased. The lower limit of the maximum height Rz of the solder film 1 on the film surface 1a is not particularly limited, but can be, for example, 0.005 μm. The maximum height Rz can be measured in accordance with JIS B 0601:2013.
[0048] In this embodiment, the total mass of Au in the Au—Sn alloy film 3 is M AThe total mass of Sn is M S When the mass ratio of Au to the total mass of Au and Sn is M A / (M A +M S ) is preferably 0.60 or more, more preferably 0.75 or more, and preferably 0.90 or less, more preferably 0.85 or less. In this case, the melting points (eutectic temperatures) of Au and Sn can be brought closer to the minimum value of 280°C, and bonding can be performed at a lower temperature during mounting.
[0049] In this embodiment, the solder film 1 can be formed by stacking each layer by a vapor deposition method using, for example, an Au-Sn alloy as a vapor deposition source. Specifically, this can be explained using a manufacturing method of the film-coated substrate 20 shown in FIG.
[0050] First, an Au-Sn alloy is placed in a container 21 shown in Fig. 3 to serve as a deposition source. Next, an electron gun is used to deposit all of the deposition source in the container 21 by a deposition method, forming one layer of an Au-Sn alloy film 3 on a glass substrate 22. The heating temperature can be set to 800°C or higher and 1000°C or lower, which is the temperature at which Au and Sn evaporate.
[0051] Next, the container 21 containing the Au-Sn alloy is replaced, and deposition is performed again to form a second layer of the Au-Sn alloy film 3. By repeating this operation, a multilayer film 2 can be formed. Thus, the number of Au-Sn alloy films 3 can be stacked equal to the number of containers 21. Note that it is preferable to set the heating temperature during the formation of each layer to the same temperature. The film thickness of each layer can be adjusted by the amount of Au-Sn alloy placed in the container 21.
[0052] The number of containers 21 is not particularly limited, but since it corresponds to the total number of layers of the Au-Sn alloy film 3 in the multilayer film 2, it is preferably 1 or more, more preferably 5 or more, preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.
[0053] As the deposition method, for example, a vacuum deposition method, an ion plating vacuum deposition method, an ion-assisted vacuum deposition method, or the like can be used.
[0054] In this manner, a multilayer film 2 can be formed in which Au--Sn alloy films 3 having a concentration gradient of Au and Sn in the thickness direction are laminated.
[0055] Second Embodiment FIG. 4 is a schematic cross-sectional view showing, in an enlarged manner, a portion where a solder film is provided according to a second embodiment of the present invention.
[0056] 4, the solder film 31 further has an adhesive film 33. The adhesive film 33 is provided between the prism body 11 and the multilayer film 2. Therefore, in the solder film 31, the multilayer film 2 is laminated on the adhesive film 33. By providing the adhesive film 33, the adhesion with the prism body 11 can be improved.
[0057] The adhesive film 33 has a first layer 33a, a second layer 33b, and a third layer 33c. The first layer 33a is a layer on the prism body 11 side. The second layer 33b is laminated on the first layer 33a. The third layer 33c is laminated on the second layer 33b. The third layer 33c is a layer on the multilayer film 2 side.
[0058] The material constituting the first layer 33a may be, for example, Ni, Cr, Ti, W, TiW, Mo, or a Ni-Cr alloy. Among these, Ni, Cr, or Ti is preferable. One of these materials may be used alone, or a combination of two or more of them may be used. Note that the material constituting the first layer 33a preferably contains 95% or more of the above-mentioned materials. However, the first layer 33a may contain impurities or additives as long as they do not impair the effects of the present invention.
[0059] The thickness of the first layer 33a is not particularly limited, but may be, for example, 0.5 μm or more and 5 μm or less. The first layer 33a may be formed by an appropriate method such as plating, vapor deposition, or sputtering.
[0060] The material constituting the second layer 33b may be, for example, Ni, Pt, Pd, or a Ni-Cr alloy. Among these, Ni, Pt, Pd, or a Ni-Cr alloy is preferable. One of these materials may be used alone, or a combination of two or more of these materials may be used. Note that the material constituting the second layer 33b preferably contains 95% or more of the above-mentioned materials. However, the second layer 33b may contain impurities or additives as long as they do not impair the effects of the present invention.
[0061] The thickness of the second layer 33b is not particularly limited, but may be, for example, 0.01 μm or more and 1 μm or less. The second layer 33b may be formed by an appropriate method such as plating, vapor deposition, sputtering, etc. In addition, the adhesion film 33 does not necessarily need to include the second layer 33b.
[0062] The third layer 33c preferably functions as a diffusion prevention layer, for example, to prevent the components of the multilayer film 2 from diffusing into the first layer 33a and the second layer 33b. This can further increase the bonding strength of the solder film 31 to a package or the like.
[0063] The third layer 33c is not particularly limited, but is Pt in this embodiment. In this case, it is possible to further suppress the components of the multilayer film 2 from diffusing into the first layer 33a and the second layer 33b. However, the material of the third layer 33c is not limited to Pt, and may be Au, Pd, or the like. These materials may be used alone or in combination. It is preferable that the third layer 33c contains 95% or more of the above-mentioned materials. However, the third layer 33c may contain impurities or additives within a range that does not impair adhesion.
[0064] The thickness of the third layer 33c is not particularly limited, but can be, for example, not less than 0.05 μm and not more than 1.0 μm.
[0065] The solder film 31 further includes an Au film 34. The Au film 34 is laminated on the second main surface 3b of the Au—Sn alloy film 3. The Au film 34 is provided on the solder film 31 as an outermost layer.
[0066] It is preferable that the Au film 34 contains 95% or more Au. However, the Au film 34 may contain impurities or additives as long as they do not impair adhesion. The other points are the same as those of the first embodiment.
[0067] Like the solder film 31 in the second embodiment, an adhesive film 33 may be further provided. Also, an Au film 34 may be provided as the outermost layer. When the outermost layer is the Au film 34, the outermost layer that contacts the package or the like can be made less susceptible to oxidation during mounting, and the bonding strength of the solder film 31 can be more reliably increased.
[0068] Also in the second embodiment, the solder film 31 includes the Au-Sn alloy film 3 and has a concentration gradient of Au and Sn in the thickness direction, so that the film surface 31a has excellent flatness and warpage can be suppressed. Furthermore, when the prism 30, which is an optical device component, is mounted on a package or the like, the solder film 31 can reliably bond the prism 30 in a short time.
[0069] (Third embodiment) FIG. 5 is a schematic cross-sectional view showing, in an enlarged manner, a portion where a solder film is provided according to a third embodiment of the present invention.
[0070] As shown in FIG. 5, in the solder film 41, an Au—Sn alloy single layer film 42, which is a single layer film of the Au—Sn alloy film 3, is provided.
[0071] In this embodiment, the thickness of the Au-Sn single layer film 42 is preferably 15 μm or less, more preferably 10 μm or less, and further preferably 2 μm or less. When the thickness of the Au-Sn alloy single layer film 42 is equal to or less than the above upper limit, the film surface 41a of the solder film 41 can be made even flatter, and warping due to film stress can be further suppressed. In addition, when mounting, bonding can be performed more reliably in a shorter time. On the other hand, the lower limit of the thickness of the Au-Sn alloy single layer film 42 is not particularly limited, but can be, for example, 30 nm. If the thickness of the Au-Sn alloy single layer film 42 is smaller than the above lower limit, it may be difficult to form the Au-Sn alloy single layer film 42.
[0072] In this way, the Au—Sn alloy single layer film 42 can be the same as the Au—Sn alloy film 3 in the first and second embodiments, except that the preferred thickness is different.
[0073] The other points are the same as those of the second embodiment.
[0074] Like the solder film 41 in the third embodiment, the multilayer film 2 may be replaced with an Au—Sn alloy single layer film 42, which is a single layer film of the Au—Sn alloy film 3. In this case, the productivity of the solder film 41 can be further improved.
[0075] Also in the third embodiment, the solder film 41 includes the Au-Sn alloy film 3 and has a concentration gradient of Au and Sn in the thickness direction, so that the film surface 41a has excellent flatness and warpage can be suppressed. Furthermore, when the prism 40, which is an optical device component, is mounted on a package or the like, the solder film 41 can reliably bond the prism 40 in a short time.
[0076] In the first to third embodiments, the prisms 10, 30, and 40 have been described as optical device components. However, in the present invention, the optical device component may be an optical element, a submount for mounting an optical element, or a packaging member for mounting an optical element.
[0077] [Optical devices] Fig. 6 is a schematic cross-sectional view showing an optical device according to one embodiment of the present invention. As shown in Fig. 6, an optical device 51 includes an optical element 52, a submount 53, a prism 10, and a package 54. The optical element 52, the submount 53, and the prism 10 are housed in the package 54.
[0078] More specifically, the package 54 is a container-like member having a bottom 55 and a sidewall 56 disposed on the bottom 55. The package 54 can be made of, for example, a ceramic material. Examples of the ceramic material that can be used include alumina and aluminum nitride. Among them, aluminum nitride is preferable from the viewpoint of further improving heat dissipation.
[0079] The bottom portion 55 has a mounting surface 55a. The sidewall portion 56 has an inner surface 56a. A metal film 58 is provided on the mounting surface 55a of the bottom portion 55 and the inner surface 56a of the sidewall portion 56.
[0080] In this embodiment, the optical element 52 and the prism 10 are disposed on the metal film 58 on the mounting surface 55a. More specifically, a submount 53 is provided on the metal film 58, and the optical element 52 is disposed thereon. At this time, one main surface 53a of the submount 53 is bonded to the optical element 52 by a solder film 1 (not shown). In addition, the other main surface 53b of the submount 53 is bonded to the metal film 58 by the solder film 1 (not shown). In addition, the prism 10 is also bonded to the metal film 58 by the solder film 1.
[0081] The package 54 does not necessarily have to have the metal film 58. However, it is preferable that the package 54 has the metal film 58 as in this embodiment. Such a configuration is particularly effective when the difference in thermal expansion coefficient between the submount 53 or prism 10 and the package 54 is relatively large.
[0082] The metal film 58 is preferably an Au film. In this case, since the metal film 58 is not easily oxidized, the bonding strength between the submount 53 or the prism 10 and the package 54 can be further increased during the manufacture of the optical device 51.
[0083] In this embodiment, a metal film 58 is provided on the entire mounting surface 55a of the bottom portion 55 and the entire inner surface 56a of the side wall portion 56. However, it is sufficient that the metal film 58 is provided at least on the portion where the submount 53 and the prism 10 are disposed.
[0084] A lid 57 is provided on a side wall 56 of the package 54 so as to seal the optical element 52 and the prism 10. The lid 57 is not particularly limited, but in this embodiment, it is a glass lid. The lid 57 and the side wall 56 are bonded together by a solder film 1 (not shown). In this case, since no gas is generated after bonding, impurities are unlikely to adhere to the reflective film 12 of the prism 10, and deterioration of the reflection characteristics is unlikely to occur.
[0085] In this embodiment, the optical element 52 is a light source that emits light to the prism 10. The light source is not particularly limited, and may be, for example, an LD or an LED. As shown in Fig. 6, light A emitted from the optical element 52 is reflected by the prism 10, passes through the cover 57, and is emitted to the outside of the optical device 51. The optical element 52 may be a light receiving element that receives the light from the prism 10.
[0086] The submount 53 is provided for mounting the optical element 52. The submount 53 also serves as a heat sink. Therefore, heat generated in the optical element 52 can be efficiently dissipated to the package 54 side through the submount 53.
[0087] In the optical device 51, the solder film 1 bonds the prism 10 and the package 54, bonds the optical element 52 and the submount 53, bonds the submount 53 and the package 54, and bonds the lid 57 and the sidewall 56 of the package 54. Therefore, in the optical device 51, warping of each member is suppressed and the bonding strength is increased. Therefore, the reliability of the optical device 51 is increased.
[0088] In addition, in the optical device 51, the lid 57 and the side wall 56 of the package 54 may be joined by a solder film having a low melting point, such as a Sn-Ag alloy. In this case, if the other components are joined by the solder film 1 having a higher melting point than the solder film having a low melting point, the optical element 52, the submount 53, and the prism 10 are less likely to be misaligned in the height direction due to heating when joining the lid 57 and the side wall 56 by the solder film after mounting the optical element 52, the submount 53, and the prism 10. Therefore, the reliability of the optical device 51 can be further improved.
[0089] The temperature for bonding the optical element 52, the submount 53, and the prism 10 may be, for example, 290° C. to 320° C. The temperature for bonding the lid 57 and the side wall 56 may be 220° C. to 270° C. Bonding within such a temperature range can further improve the positional accuracy of the optical element 52, the submount 53, and the prism 10 in the height direction.
[0090] In the present invention, at least one of the members constituting the optical element 52, the submount 53, the prism 10, and the package 54 may be bonded by the solder film 1, and is not particularly limited.
[0091] The present invention will be described in more detail below with reference to specific examples. The present invention is not limited to the following examples, and can be modified as appropriate within the scope of the present invention.
[0092] Example 1 First, a container containing an Au-Sn alloy was used as the deposition source, and an Au-Sn alloy film was formed on a glass substrate 62 (manufactured by Nippon Electric Glass Co., Ltd., OA-10G, thickness: 0.197 mm) shown in FIG. 7(a) by vacuum deposition. The heating temperature during deposition was set to approximately 100°C or less by radiant heat from the deposition source with the heater turned off. A total of 18 containers containing an Au-Sn alloy were used, and the same operation was performed under the same conditions to laminate a total of 18 layers of Au-Sn alloy films, thereby obtaining a film-coated substrate 60. At this time, the thickness of each Au-Sn alloy film was set to 270 nm. The overall thickness of the solder film 61 was set to 4.9 μm.
[0093] 8 is an SEM photograph showing a cross section of the solder film 61 obtained in Example 1. From FIG. 8, it can be confirmed that the solder film 61 obtained in Example 1 has a total of 18 laminated Au-Sn alloy films. In addition, in each Au-Sn alloy film, the concentration of Sn on the main surface side facing the glass substrate 62 was higher than the concentration of Au. On the other hand, the concentration of Sn on the main surface side opposite the glass substrate 62 was lower than the concentration of Au. Therefore, each Au-Sn alloy film had a concentration gradient of Au and Sn in the thickness direction.
[0094] Comparative Example 1 A total of 180 Au layers and Sn layers were alternately laminated by vapor deposition on a glass substrate 62 (manufactured by Nippon Electric Glass Co., Ltd., OA-10G, thickness: 0.197 mm), to obtain a film-coated substrate 60. In this case, the thickness of each Au layer was 28 nm. Also, the thickness of each Sn layer was 28 nm. The overall thickness of the solder film 61 was 5 μm.
[0095] [evaluation] (Warpage evaluation) In the evaluation of warpage, the dimensions of the film-coated substrate 60 were length a: 100 mm and width b: 10 mm, as shown in Figures 7(a) and 7(b). The Au layer and Sn layer were not formed on the portions of the film-coated substrate 60 from the first end 60b and the second end 60c in the longitudinal direction thereof, up to a length c: 3.5 mm.
[0096] In the evaluation of warpage, the film-coated substrate 60 was placed on the stage 70 shown in FIG. 7(c) and the warpage L was measured after leaving it at 25° C. for 1 hour. The film-coated substrate 60 was placed with the film surface 60a facing upward. The difference in height between the first end 60b and the second end 60c and the center of the length direction of the non-film surface 60d of the film-coated substrate 60 was taken as the warpage L. The warpage L was taken as the average of the warpage L of the two ends 60b, 60c. The non-film surface 60d is the surface facing the film surface 60a.
[0097] (Evaluation of surface flatness) The arithmetic mean roughness Ra and maximum height Rz of the film surface 60a of the film-coated substrate 60 were measured in accordance with JIS B 0601:2013.
[0098] (Adhesion evaluation) In the evaluation of adhesion, an aluminum nitride substrate having a gold-plated portion was prepared as a package. Next, the film-coated substrate 60 was attached to the gold-plated portion of the aluminum nitride substrate from the solder film 61 side, and the substrate was heated to 320° C. in a nitrogen atmosphere to bond the substrate.
[0099] Next, the adhesion was evaluated by pressing the film-coated substrate 60 from the side using a tension and compression tester (SV-201 manufactured by Imada Manufacturing Co., Ltd.) The adhesion was evaluated under both bonding times of 3 seconds and 10 seconds.
[0100] The results are shown in Table 1 below.
[0101] [Table 1]
[0102] As is clear from Table 1, it was confirmed that the solder film 61 of Example 1, which uses an Au-Sn alloy film having a concentration gradient of Au and Sn in the thickness direction, has excellent surface flatness and suppresses warping due to film stress. [Explanation of symbols]
[0103] 1,31,41,61...Solder film 1a,31a,41a...Membrane surface 2...Multilayer film 3...Au-Sn alloy film 3a…First main surface 3b…Second main surface 10,30,40...Prism 11…Prism body 11a…Bottom surface 11b...Slope 11c…Top surface 12...Reflection film 20,60...Film-coated substrate 21…Container 22,62…Glass substrate 33...Adhesive film 33a…First layer 33b…Second layer 33c…Third layer 34…Au film 42…Au-Sn alloy single layer film 51...Optical devices 52...Optical elements 53…Submount 53a...One side main surface 53b...other main surface 54…Package 55...Bottom 55a…Mounting surface 56…Side wall 56a…Inner surface 57…Cover body 58...Metal film 60a...Film surface 60b...first end 60c...Second end 60d…Non-membrane surface 70…Stage
Claims
1. A solder film used to fix components in an optical device, comprising: Au-Sn alloy film is provided; the Au—Sn alloy film has a concentration gradient of Au and Sn in a thickness direction; the Au—Sn alloy film has a first main surface and a second main surface opposed to each other; the first principal surface is a principal surface on which the component is provided, The second main surface is an outer main surface opposite to a side on which the component is provided, A direction connecting the first main surface and the second main surface is the thickness direction, A solder film, in which, in the thickness direction, a concentration of Sn on the first principal surface side is greater than a concentration of Au, and a concentration of Sn on the second principal surface side is smaller than a concentration of Au.
2. A solder film used to fix components in an optical device, comprising: Au-Sn alloy film is provided; the Au—Sn alloy film has a concentration gradient of Au and Sn in a thickness direction; A solder film having a surface with an arithmetic mean roughness Ra of 0.05 μm or less.
3. A solder film used to fasten components in an optical device, comprising: Au-Sn alloy film is provided; the Au—Sn alloy film has a concentration gradient of Au and Sn in a thickness direction; A solder film having a maximum surface height Rz of 0.25 μm or less.
4. A solder film used to fasten components in an optical device, comprising: Au-Sn alloy film is provided; the Au—Sn alloy film has a concentration gradient of Au and Sn in a thickness direction; The solder film has an overall thickness of 1 μm or more and 10 μm or less.
5. 5. The solder film according to claim 1, wherein the Au--Sn alloy film is a vapor deposition film deposited using an Au--Sn alloy as a vapor deposition source.
6. The total mass of Au in the Au—Sn alloy film is M A The total mass of Sn is M S When the ratio of the mass of Au to the total mass of Au and Sn is M A / (M A +M S 6. The solder film according to claim 1, wherein the ratio of the surface area of the solder paste to the surface area of the solder paste is 0.60 or more and 0.90 or less.
7. The solder film according to any one of claims 1 to 6, comprising a multi-layer film in which a plurality of the Au-Sn alloy films are laminated.
8. 8. The solder film according to claim 7, wherein the number of layers of the Au--Sn alloy film in the multilayer film is 1 to 30.
9. The solder film according to any one of claims 1 to 8, further comprising an adhesion film provided between said component and said Au-Sn alloy film.
10. The adhesive film is A first layer is provided on the component side and contains at least one selected from the group consisting of Cr, Ti, and Ni; a second layer provided on the first layer and including at least one selected from the group consisting of Ni, Pt, Pd, and a Ni-Cr alloy; a third layer disposed on the second layer, the third layer including Pt or Au; The solder film of claim 9 , comprising:
11. The solder film according to any one of claims 1 to 10, further comprising an Au film provided on a main surface of the Au-Sn alloy film opposite the component side, the Au film being an outermost layer.
12. A component body having a main surface; The solder film according to any one of claims 1 to 11, which is provided on the main surface of the component body; A component for an optical device comprising:
13. 13. The optical device part according to claim 12, which is at least one selected from the group consisting of a prism, an optical element, a submount for mounting the optical element, and a packaging member for mounting the optical element.
14. A prism and an optical element that emits light to the prism or receives light from the prism; a package in which the prism and the optical element are mounted; a submount provided between the optical element and the package; and Equipped with An optical device in which the prism and the package are bonded, the optical element and the submount are bonded, the submount and the package are bonded, or components constituting the package are bonded together by the solder film described in any one of claims 1 to 11.
Citation Information
Patent Citations
An-sn multi-layer solder
JP1998006073A
Au-Sn ALLOY LAMINATE SOLDER, AND ITS MANUFACTURING METHOD
JP2006110626A
FORMING METHOD OF AuSn LAYER AND MANUFACTURING METHOD OF SEMICONDUCTOR LIGHT-EMITTING DEVICE HAVING AuSn LAYER
JP2008263130A