Ink composition, cured product, light conversion layer, and color filter

By using an organic ligand with two or more carbon-carbon double bonds, the viscosity issues in ink compositions with luminescent nanocrystal particles are mitigated, facilitating efficient and cost-effective formation of light conversion layers through inkjet methods.

JP7581713B2Active Publication Date: 2024-11-13TOPPAN HOLDINGS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020150389
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-08
Publication Date
2024-11-13
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

The increase in viscosity of ink compositions containing luminescent nanocrystal particles due to organic ligands used for binding, particularly those with a (poly)alkyleneoxy group, poses challenges in forming light conversion layers using an inkjet method, leading to inefficiencies and waste of expensive materials.

Method used

Incorporating an organic ligand with two or more carbon-carbon double bonds, such as unsaturated fatty acids, helps suppress viscosity increases, allowing for effective dispersion of luminescent nanocrystal particles and formation of light conversion layers via inkjet methods.

Benefits of technology

The solution effectively maintains the ink composition's viscosity, enabling efficient and cost-effective formation of light conversion layers without wasting expensive luminescent nanocrystal particles, thereby improving the reliability and efficiency of the inkjet process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581713000002
    Figure 0007581713000002
  • Figure 0007581713000001
    Figure 0007581713000001
Patent Text Reader

Abstract

To suppress an increase in viscosity of an ink composition due to an organic ligand.SOLUTION: An ink composition includes: luminescent nanocrystal particles; organic ligands capable of being bonded to surfaces of the luminescent nanocrystal particles; and photopolymerizable compounds. The organic ligand has two or more carbon-carbon double bonds.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ink composition, a cured product, a light conversion layer, and a color filter. [Background technology]

[0002] Conventionally, pixel portions (color filter pixel portions) in displays such as liquid crystal display devices have been manufactured by photolithography using a curable resist material containing, for example, red organic pigment particles or green organic pigment particles, and an alkali-soluble resin and / or an acrylic monomer.

[0003] In recent years, there has been a strong demand for lower power consumption in displays, and methods for forming pixel portions such as red pixels and green pixels using luminescent nanocrystalline particles, such as quantum dots, quantum rods, and other inorganic phosphor particles, instead of the above-mentioned red organic pigment particles or green organic pigment particles, are being actively researched.

[0004] However, the above-mentioned photolithography-based color filter manufacturing method has a drawback in that the resist material, including the relatively expensive luminescent nanocrystal particles, is wasted in areas other than the pixel area due to the characteristics of the manufacturing method. Under these circumstances, in order to eliminate the waste of the resist material, a method of forming a light conversion layer using a curable ink composition by an inkjet method (inkjet method) has been considered (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-21033 A Summary of the Invention [Problem to be solved by the invention]

[0006] Incidentally, as a means for dispersing luminescent nanocrystalline particles well in an ink composition, it is known to use an organic ligand capable of binding (coordinating) to the surface of the luminescent nanocrystalline particles, as disclosed in Patent Document 1. However, according to the study by the present inventors, in order to suitably bind the organic ligand to the surface of the luminescent nanocrystalline particles, there is a restriction on the type of organic ligand, and under this restriction, the viscosity of the ink composition tends to increase due to the organic ligand. In particular, although the organic ligand containing a (poly)alkyleneoxy group described in Patent Document 1 is widely used, it is likely to cause an increase in the viscosity of the ink composition. The increase in the viscosity of the ink composition is undesirable, especially when forming a light conversion layer by an inkjet method.

[0007] Therefore, an object of one aspect of the present invention is to suppress an increase in viscosity of an ink composition caused by an organic ligand. [Means for solving the problem]

[0008] According to the investigations of the present inventors, it has been found that by using an organic ligand having two or more carbon-carbon double bonds, an increase in viscosity of the ink composition caused by the organic ligand can be suppressed.

[0009] One aspect of the present invention is an ink composition comprising luminescent nanocrystalline particles, an organic ligand capable of binding to the surface of the luminescent nanocrystalline particles, and a photopolymerizable compound, wherein the organic ligand comprises an organic ligand having two or more carbon-carbon double bonds.

[0010] The content of the organic ligand having two or more carbon-carbon double bonds may be 1 part by mass or more and 30 parts by mass or less based on 100 parts by mass of the luminescent nanocrystalline particles. The organic ligand having two or more carbon-carbon double bonds may further have a carboxyl group.

[0011] The ink composition may be used to form a light conversion layer by an inkjet method.

[0012] Another aspect of the present invention is a cured product of the above ink composition.

[0013] Another aspect of the present invention is a light conversion layer comprising a plurality of pixel portions and a light-shielding portion provided between the plurality of pixel portions, the plurality of pixel portions having light-emitting pixel portions including a cured product of the ink composition described above.

[0014] The light conversion layer may comprise, as light-emitting pixel units, a first light-emitting pixel unit containing light-emitting nanocrystal particles that absorb light with a wavelength in the range of 420 to 480 nm and emit light having a peak emission wavelength in the range of 605 to 665 nm, and a second light-emitting pixel unit containing light-emitting nanocrystal particles that absorb light with a wavelength in the range of 420 to 480 nm and emit light having a peak emission wavelength in the range of 500 to 560 nm.

[0015] Another aspect of the present invention is a color filter including the above-mentioned light conversion layer. Effect of the Invention

[0016] According to one aspect of the present invention, an increase in viscosity of the ink composition caused by the organic ligand can be suppressed. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of a color filter according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail. In this specification, the term "cured product of the ink composition" refers to a product obtained by curing a curable component in the ink composition (when the ink composition contains a solvent component, the ink composition after drying). Therefore, it is preferable that the cured product of the ink composition does not contain an organic solvent, but some organic solvent that has not been completely dried may remain. In addition, in this specification, the term "non-volatile content of the ink composition" refers to components other than the organic solvent contained in the ink composition. In other words, the term "non-volatile content of the ink composition" may be rephrased as the components before curing that should be contained in the cured product of the ink composition.

[0019] <Ink composition> The ink composition of one embodiment contains luminescent nanocrystalline particles, an organic ligand, and a photopolymerizable compound.

[0020] The ink composition is, for example, an ink composition for forming a light conversion layer (for example, for forming a pixel portion of a color filter) used to form a light conversion layer (pixel portion of a light conversion layer) of a color filter or the like. In one embodiment, this ink composition is a composition (inkjet ink) used in an inkjet method. The ink composition of one embodiment can contribute to making the inkjet method a low-cost process compared to photolithography methods in that it can form a pixel portion (light conversion layer) without wasting expensive luminescent nanocrystalline particles, inkjet heads, etc. Below, an embodiment of the ink composition will be described using an ink composition used to form a light conversion layer in an inkjet method as an example.

[0021] [Luminescent nanocrystal particles] Luminescent nanocrystalline particles are nano-sized crystals that absorb excitation light and emit fluorescence or phosphorescence, and are, for example, crystals whose maximum particle size measured by a transmission electron microscope or a scanning electron microscope is 100 nm or less.

[0022] The luminescent nanocrystal particles can, for example, absorb light of a predetermined wavelength and emit light (fluorescence or phosphorescence) of a wavelength different from the absorbed wavelength. The luminescent nanocrystal particles may be red-luminescent nanocrystal particles (red-luminescent nanocrystal particles) that emit light (red light) having an emission peak wavelength in the range of 605 to 665 nm, green-luminescent nanocrystal particles (green-luminescent nanocrystal particles) that emit light (green light) having an emission peak wavelength in the range of 500 to 560 nm, or blue-luminescent nanocrystal particles (blue-luminescent nanocrystal particles) that emit light (blue light) having an emission peak wavelength in the range of 420 to 480 nm. In this embodiment, it is preferable that the ink composition contains at least one of these luminescent nanocrystal particles. The light absorbed by the luminescent nanocrystalline particles may be, for example, light having a wavelength in the range of 400 nm or more and less than 500 nm (particularly, light having a wavelength in the range of 420 to 480 nm) (blue light) or light having a wavelength in the range of 200 nm to 400 nm (ultraviolet light). The emission peak wavelength of the luminescent nanocrystalline particles can be confirmed, for example, in a fluorescence spectrum or phosphorescence spectrum measured using a spectrofluorometer.

[0023] The red light-emitting nanocrystalline particles preferably have an emission peak wavelength of 665nm or less, 663nm or less, 660nm or less, 658nm or less, 655nm or less, 653nm or less, 651nm or less, 650nm or less, 647nm or less, 645nm or less, 643nm or less, 640nm or less, 637nm or less, 635nm or less, 632nm or less, or 630nm or less, and preferably have an emission peak wavelength of 628nm or more, 625nm or more, 623nm or more, 620nm or more, 615nm or more, 610nm or more, 607nm or more, or 605nm or more. These upper and lower limit values ​​can be arbitrarily combined. In the following similar descriptions, the upper and lower limit values ​​individually described can be arbitrarily combined.

[0024] The green light-emitting nanocrystalline particles preferably have an emission peak wavelength of 560 nm or less, 557 nm or less, 555 nm or less, 550 nm or less, 547 nm or less, 545 nm or less, 543 nm or less, 540 nm or less, 537 nm or less, 535 nm or less, 532 nm or less, or 530 nm or less, and preferably have an emission peak wavelength of 528 nm or more, 525 nm or more, 523 nm or more, 520 nm or more, 515 nm or more, 510 nm or more, 507 nm or more, 505 nm or more, 503 nm or more, or 500 nm or more.

[0025] The blue-light-emitting nanocrystalline particles preferably have an emission peak wavelength of 480 nm or less, 477 nm or less, 475 nm or less, 470 nm or less, 467 nm or less, 465 nm or less, 463 nm or less, 460 nm or less, 457 nm or less, 455 nm or less, 452 nm or less, or 450 nm or less, and preferably have an emission peak wavelength of 450 nm or more, 445 nm or more, 440 nm or more, 435 nm or more, 430 nm or more, 428 nm or more, 425 nm or more, 422 nm or more, or 420 nm or more.

[0026] According to the solution of the Schrodinger wave equation of the well-well potential model, the wavelength (emission color) of light emitted by a luminescent nanocrystal particle depends on the size (e.g., particle diameter) of the luminescent nanocrystal particle, but also on the energy gap of the luminescent nanocrystal particle. Therefore, the emission color can be selected by changing the constituent material and size of the luminescent nanocrystal particle used.

[0027] The luminescent nanocrystal particles may be luminescent nanocrystal particles (luminescent semiconductor nanocrystal particles) containing a semiconductor material. Examples of the luminescent semiconductor nanocrystal particles include quantum dots and quantum rods. Among these, quantum dots are preferred from the viewpoints of easy control of the emission spectrum, reduced production costs, and improved mass productivity while ensuring reliability.

[0028] The luminescent semiconductor nanocrystal particle may be composed of only a core containing a first semiconductor material, or may have a core containing the first semiconductor material and a shell containing a second semiconductor material different from the first semiconductor material and covering at least a part of the core. In other words, the structure of the luminescent semiconductor nanocrystal particle may be a structure consisting of only a core (core structure), or a structure consisting of a core and a shell (core / shell structure). The luminescent semiconductor nanocrystal particle may further have a shell (second shell) containing a third semiconductor material different from the first and second semiconductor materials and covering at least a part of the core, in addition to the shell (first shell) containing the second semiconductor material. In other words, the structure of the luminescent semiconductor nanocrystal particle may be a structure consisting of a core, a first shell, and a second shell (core / shell / shell structure). Each of the core and the shell may be a mixed crystal containing two or more kinds of semiconductor materials (for example, CdSe+CdS, CIS+ZnS, etc.).

[0029] The luminescent nanocrystalline particles preferably contain, as a semiconductor material, at least one semiconductor material selected from the group consisting of II-VI semiconductors, III-V semiconductors, I-III-VI semiconductors, Group IV semiconductors, and I-II-IV-VI semiconductors.

[0030] Specific semiconductor materials include CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, CdHgZnTe , CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe, HgZnSTe; GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, Al PAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb;SnS, SnSe, SnTe, PbS, PbSe , PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe; Si, Ge, SiC, SiGe, AgInSe2, CuGaSe2, CuInS2, CuGaS2, CuInSe2, AgInS2, AgGaSe2, AgGaS2, C, Si and Ge. From the viewpoints of easily controlling the emission spectrum and ensuring reliability, reducing production costs, and improving mass productivity, it is preferable that the luminescent semiconductor nanocrystal particles contain at least one selected from the group consisting of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, InP, InAs, InSb, GaP, GaAs, GaSb, AgInS2, AgInSe2, AgInTe2, AgGaS2, AgGaSe2, AgGaTe2, CuInS2, CuInSe2, CuInTe2, CuGaS2, CuGaSe2, CuGaTe2, Si, C, Ge, and Cu2ZnSnS4.

[0031] Examples of red-emitting semiconductor nanocrystal particles include CdSe nanocrystal particles, nanocrystal particles having a core / shell structure in which the shell portion is CdS and the inner core portion is CdSe, nanocrystal particles having a core / shell structure in which the shell portion is CdS and the inner core portion is ZnSe, nanocrystal particles of a mixed crystal of CdSe and ZnS, InP nanocrystal particles, nanocrystal particles having a core / shell structure in which the shell portion is ZnS and the inner core portion is InP, and nanocrystal particles having a core / shell structure. Examples of such nanocrystal particles include nanocrystal particles whose shell portion is a mixed crystal of ZnS and ZnSe and whose inner core portion is InP, nanocrystal particles of a mixed crystal of CdSe and CdS, nanocrystal particles of a mixed crystal of ZnSe and CdS, nanocrystal particles with a core / shell / shell structure in which the first shell portion is ZnSe, the second shell portion is ZnS, and the inner core portion is InP, and nanocrystal particles with a core / shell / shell structure in which the first shell portion is a mixed crystal of ZnS and ZnSe, the second shell portion is ZnS, and the inner core portion is InP.

[0032] Examples of green-emitting semiconductor nanocrystal particles include CdSe nanocrystal particles, nanocrystal particles of a mixed crystal of CdSe and ZnS, nanocrystal particles having a core / shell structure in which the shell portion is ZnS and the inner core portion is InP, nanocrystal particles having a core / shell structure in which the shell portion is a mixed crystal of ZnS and ZnSe and the inner core portion is InP, nanocrystal particles having a core / shell / shell structure in which the first shell portion is ZnSe, the second shell portion is ZnS, and the inner core portion is InP, and nanocrystal particles having a core / shell / shell structure in which the first shell portion is a mixed crystal of ZnS and ZnSe, the second shell portion is ZnS, and the inner core portion is InP.

[0033] Examples of blue-emitting semiconductor nanocrystal particles include ZnSe nanocrystal particles, ZnS nanocrystal particles, nanocrystal particles having a core / shell structure in which the shell part is ZnSe and the inner core part is ZnS, CdS nanocrystal particles, nanocrystal particles having a core / shell structure in which the shell part is ZnS and the inner core part is InP, nanocrystal particles having a core / shell structure in which the shell part is a mixed crystal of ZnS and ZnSe and the inner core part is InP, nanocrystal particles having a core / shell / shell structure in which a first shell part is ZnSe, a second shell part is ZnS, and an inner core part is InP, nanocrystal particles having a core / shell / shell structure in which a first shell part is a mixed crystal of ZnS and ZnSe, a second shell part is ZnS, and an inner core part is InP, and the like.

[0034] By changing the average particle diameter of semiconductor nanocrystal particles with the same chemical composition, the color to be emitted from the particles can be changed to red or green. In addition, it is preferable to use semiconductor nanocrystal particles that have as little adverse effect on the human body as possible. When using semiconductor nanocrystal particles containing cadmium, selenium, etc. as luminescent nanocrystal particles, it is preferable to select semiconductor nanocrystal particles that contain as little of the above elements (cadmium, selenium, etc.) as possible and use them alone, or to use them in combination with other luminescent nanocrystal particles so that the amount of the above elements is as small as possible.

[0035] The shape of the luminescent nanocrystal particles is not particularly limited, and may be any geometric shape or any irregular shape. The shape of the luminescent nanocrystal particles may be, for example, spherical, ellipsoidal, pyramidal, discoid, branched, net-like, rod-like, etc. However, it is preferable to use particles with little directional particle shape (for example, spherical, regular tetrahedral, etc.) as the luminescent nanocrystal particles, in order to further improve the uniformity and flowability of the ink composition.

[0036] The average particle size (volume average size) of the luminescent nanocrystal particles may be 1 nm or more, 1.5 nm or more, or 2 nm or more from the viewpoint of easily obtaining light emission of a desired wavelength and excellent dispersibility and storage stability. From the viewpoint of easily obtaining a desired emission wavelength, it may be 40 nm or less, 30 nm or less, or 20 nm or less. The average particle size (volume average size) of the luminescent nanocrystal particles is obtained by measuring with a transmission electron microscope or a scanning electron microscope and calculating the volume average size.

[0037] The luminescent nanocrystal particles may be dispersed in a colloidal form in an organic solvent, a photopolymerizable compound, or the like. The surfaces of the luminescent nanocrystal particles dispersed in the organic solvent are preferably passivated by the organic ligand described above. As the organic solvent, an organic solvent described below that is contained in the ink composition is used.

[0038] The luminescent nanocrystal particles may be commercially available products, such as indium phosphide / zinc sulfide, D-dot, and CuInS / ZnS from NN-Labs, and InP / ZnS from Aldrich.

[0039] The content of the luminescent nanocrystal particles is 20 parts by mass or more relative to 100 parts by mass of the non-volatile content of the ink composition from the viewpoint of improving the external quantum efficiency of the pixel portion, and is preferably 23 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more from the viewpoint of more easily obtaining the same effect. It is noteworthy that the present invention can exhibit excellent compatibility with the inkjet process while increasing the content of the luminescent nanocrystal particles. On the other hand, the content of the luminescent nanocrystal particles is preferably 50 parts by mass or less, 45 parts by mass or less, or 40 parts by mass or less relative to 100 parts by mass of the non-volatile content of the ink composition from the viewpoint of further improving the ejection stability and the external quantum efficiency of the pixel portion. In this specification, the content of the luminescent nanocrystal particles means the content of only the luminescent nanocrystal particles themselves, and does not include the content of the organic ligand even if the luminescent nanocrystal particles have an organic ligand.

[0040] The ink composition may contain two or more of red luminescent nanocrystal particles, green luminescent nanocrystal particles, and blue luminescent nanocrystal particles as the luminescent nanocrystal particles, but preferably contains only one of these particles. When the ink composition contains red luminescent nanocrystal particles, the content of the green luminescent nanocrystal particles and the content of the blue luminescent nanocrystal particles are preferably 10% by mass or less, more preferably 0% by mass, based on the total mass of the luminescent nanocrystal particles. When the ink composition contains green luminescent nanocrystal particles, the content of the red luminescent nanocrystal particles and the content of the blue luminescent nanocrystal particles are preferably 10% by mass or less, more preferably 0% by mass, based on the total mass of the luminescent nanocrystal particles.

[0041] [Organic Ligand] The organic ligand is an organic ligand capable of binding to the surface of the luminescent nanocrystalline particle. The organic ligand may, for example, be coordinated to the surface of the luminescent nanocrystalline particle. In other words, the surface of the luminescent nanocrystalline particle may be passivated by the organic ligand. The ink composition may, for example, include an organic ligand that is not coordinated to the surface of the luminescent nanocrystalline particle (e.g., free) in addition to the organic ligand that is coordinated to the surface of the luminescent nanocrystalline particle.

[0042] The organic ligand includes one or more organic ligands having two or more carbon-carbon double bonds (hereinafter also referred to as "organic ligand A"). The number of carbon-carbon double bonds in the organic ligand A is preferably three or more, and is preferably six or less, five or less, or four or less. In particular, three is preferable.

[0043] The organic ligand A preferably further has a carboxyl group. The number of carboxyl groups in the organic ligand A may be one or more, and is preferably one.

[0044] In one embodiment, the organic ligand A may be an unsaturated fatty acid having two or more carbon-carbon double bonds (unsaturated bonds) and one carboxyl group. Examples of unsaturated fatty acids (diunsaturated fatty acids) having two carbon-carbon double bonds (unsaturated bonds) include linoleic acid, eicosadienoic acid, docosadienoic acid, etc. Examples of unsaturated fatty acids (triunsaturated fatty acids) having three carbon-carbon double bonds (unsaturated bonds) include α-linolenic acid, γ-linolenic acid, pinolenic acid, α-eleostearic acid, β-eleostearic acid, mead acid, dihomo-γ-linolenic acid, eicosatrienoic acid, etc. Examples of unsaturated fatty acids (tetraunsaturated fatty acids) having four carbon-carbon double bonds (unsaturated bonds) include stearidonic acid, arachidonic acid, eicosatetraenoic acid, adrenic acid, etc. Examples of unsaturated fatty acids having five carbon-carbon double bonds (unsaturated bonds) (pentaunsaturated fatty acids) include bosseopentaenoic acid, eicosapentaenoic acid, osbondoic acid, sardine acid, tetracosapentaenoic acid, etc. Examples of unsaturated fatty acids having six carbon-carbon double bonds (unsaturated bonds) (hexaunsaturated fatty acids) include docosahexaenoic acid, herring acid, etc.

[0045] The content of organic ligand A is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, and particularly preferably 7 parts by mass or more, per 100 parts by mass of the luminescent nanocrystalline particles, from the viewpoint of improving compatibility with the polymerizable compound. The content of organic ligand A is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 15 parts by mass or less, per 100 parts by mass of the luminescent nanocrystalline particles, from the viewpoint of further suppressing an increase in viscosity of the ink composition.

[0046] The organic ligand may further include one or more other organic ligands (hereinafter also referred to as "organic ligand B") in addition to the organic ligand A. The organic ligand B has at least one functional group selected from the group consisting of, for example, an amino group, a carboxyl group, a thiol group, a phosphoric acid group, a phosphonic acid group, a phosphine group, a phosphine oxide group, and an alkoxysilyl group. The organic ligand B may further have one carbon-carbon double bond. In one embodiment, the organic ligand B may have a carboxyl group and one carbon-carbon double bond, or may have one carboxyl group and one carbon-carbon double bond.

[0047] Examples of the organic ligand B include hexanoic acid, lauric acid, oleic acid, oleylamine, dodecanethiol, n-trioctylphosphine, and n-trioctylphosphine oxide.

[0048] From the viewpoint of dispersion stability of the luminescent nanocrystal particles and maintenance of luminescent properties, the content of organic ligand B is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, even more preferably 7 parts by mass or more, and particularly preferably 10 parts by mass or more, per 100 parts by mass of the luminescent nanocrystal particles. From the viewpoint of further suppressing an increase in viscosity of the ink composition, the content of organic ligand B is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 25 parts by mass or less, per 100 parts by mass of the luminescent nanocrystal particles.

[0049] When the organic ligand includes organic ligand A and organic ligand B, the total content of the organic ligands may be 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more, relative to 100 parts by mass of the luminescent nanocrystal particles, from the viewpoint of dispersion stability of the luminescent nanocrystal particles and from the viewpoint of maintaining the luminescent properties, and may be 50 parts by mass or less, 45 parts by mass or less, 40 parts by mass or less, or 30 parts by mass or less, from the viewpoint of further suppressing an increase in the viscosity of the ink composition.

[0050] [Photopolymerizable compound] The photopolymerizable compound is a compound that polymerizes by irradiation with light, and may be, for example, a photoradical polymerizable compound. The photopolymerizable compound may be a photopolymerizable monomer or oligomer. The photopolymerizable compound is used together with a photopolymerization initiator. The photoradical polymerizable compound is used together with a photoradical polymerization initiator. In other words, the ink composition may contain a photopolymerizable component including a photopolymerizable compound and a photopolymerization initiator, or may contain a photoradical polymerizable component including a photoradical polymerizable compound and a photoradical polymerization initiator. The ink composition may contain one type of photopolymerizable compound, may contain two or more types, and preferably contains two or more types.

[0051] Examples of photoradical polymerizable compounds include monomers having an ethylenically unsaturated group (hereinafter also referred to as "ethylenically unsaturated monomers") and monomers having an isocyanate group. Here, the ethylenically unsaturated monomer means a monomer having an ethylenically unsaturated bond (carbon-carbon double bond). Examples of the ethylenically unsaturated monomer include monomers having an ethylenically unsaturated group such as a vinyl group, a vinylene group, or a vinylidene group. Monomers having these groups are sometimes referred to as "vinyl monomers".

[0052] The number of ethylenically unsaturated bonds in the ethylenically unsaturated monomer (for example, the number of ethylenically unsaturated groups) is, for example, 1 to 3. The ethylenically unsaturated monomer may be used alone or in combination of two or more. From the viewpoint of easily achieving both excellent discharge stability and excellent curability, and from the viewpoint of further improving external quantum efficiency, the photopolymerizable compound may contain a monomer having one ethylenically unsaturated group (monofunctional monomer) and a monomer having two or more ethylenically unsaturated groups (polyfunctional monomer), and may contain at least one selected from the group consisting of a monofunctional monomer, a monomer having two ethylenically unsaturated groups (bifunctional monomer), and a monomer having three ethylenically unsaturated groups (trifunctional monomer).

[0053] The ethylenically unsaturated group may be a vinyl group, a vinylene group, a vinylidene group, a (meth)acryloyl group, etc., and is preferably a (meth)acryloyl group. In this specification, the term "(meth)acryloyl group" means an "acryloyl group" and the corresponding "methacryloyl group". The same applies to the expressions "(meth)acrylate" and "(meth)acrylamide".

[0054] The photopolymerizable compound preferably contains at least one compound having a (meth)acryloyl group as an ethylenically unsaturated group, more preferably contains at least one selected from the group consisting of (meth)acrylates and (meth)acrylamides, even more preferably contains at least one (meth)acrylate, and particularly preferably contains at least one (meth)acrylate having a linear alkyl group having 8 or more carbon atoms. From the viewpoint of easily achieving both excellent discharge stability and excellent curing properties, and from the viewpoint of further improving external quantum efficiency, the photopolymerizable compound preferably contains two or more types of (meth)acrylates, more preferably contains a (meth)acrylate having one (meth)acryloyl group (monofunctional (meth)acrylate) and a (meth)acrylate having two or more (meth)acryloyl groups (polyfunctional (meth)acrylate), and even more preferably contains at least one selected from the group consisting of a monofunctional (meth)acrylate and a (meth)acrylate having two (meth)acryloyl groups (bifunctional (meth)acrylate) and a (meth)acrylate having three (meth)acryloyl groups (trifunctional (meth)acrylate).

[0055] Examples of the monofunctional monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, amyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Diethyl (meth)acrylate, nonylphenoxyethyl (meth)acrylate, glycidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (Meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, benzyl (meth)acrylate, phenylbenzyl (meth)acrylate, mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, N-[2-(acryloyloxy)ethyl]phthalimide, N-[2-(acryloyloxy)ethyl]tetrahydrophthalimide, 4-hydroxybutyl acrylate, 2 Examples of the acrylamide include 1-hydroxypropyl acrylate, 2-hydroxyethyl acrylate, acrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, diacetone acrylamide, 4-acryloylmorpholine, N-tert-butylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethylacrylamide, N-tert-octylacrylamide, N-butoxymethylacrylamide, N-phenylacrylamide, and N-dodecylacrylamide.

[0056] Specific examples of monomers having two ethylenically unsaturated groups (bifunctional monomers) include 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, Tricyclodecane dimethanol di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol hydroxypivalic acid ester diacrylate, tris(2-hydroxyethyl)isocyanurate, di(meth)acrylates in which two hydroxyl groups of a diol obtained by adding 4 moles or more of ethylene oxide or propylene oxide to 1 mole of neopentyl glycol are substituted with (meth)acryloyloxy groups; di(meth)acrylates in which two hydroxyl groups of a diol obtained by adding 2 moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A are substituted with (meth)acryloyloxy groups; Examples of such di(meth)acrylates include di(meth)acrylates in which two hydroxyl groups of a triol obtained by adding 3 moles or more of ethylene oxide or propylene oxide to 1 mole of phenol are substituted with (meth)acryloyloxy groups, di(meth)acrylates in which two hydroxyl groups of a diol obtained by adding 4 moles or more of ethylene oxide or propylene oxide to 1 mole of bisphenol A are substituted with (meth)acryloyloxy groups, N,N'-methylenebisacrylamide, and N,N'-ethylenebisacrylamide.

[0057] Specific examples of monomers having three ethylenically unsaturated groups (trifunctional monomers) include glycerin tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and EO-modified trimethylolpropane tri(meth)acrylate.

[0058] The photopolymerizable compound preferably contains a polymerizable compound having a LogP value of 3.3 or less. In this case, the volatilization of the ink composition can be suppressed due to the high polarity (the magnitude of the intermolecular force) of the photopolymerizable compound. On the other hand, when the polarity of the photopolymerizable compound is high, the viscosity of the ink composition tends to increase, but in the ink composition of this embodiment, the above-mentioned organic ligand A is used, so that the increase in viscosity caused by the polymerizable compound having high polarity is suppressed.

[0059] The LogP value of a photopolymerizable compound can be calculated using general-purpose chemical structure drawing software (e.g., ChemDraw). By drawing the chemical structure of the photopolymerizable compound for which you want to calculate the LogP value on the software and checking the Chemical Properties on the software, you can obtain the LogP value of the drawn photopolymerizable compound.

[0060] Preferred examples of the polymerizable compound having a LogP value of 3.3 or less include phenoxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxytriethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and EO-modified trimethylolpropane tri(meth)acrylate.

[0061] The polymerizable compound may further include a photopolymerizable compound having a LogP value of more than 3.3 in addition to the photopolymerizable compound having a LogP value of 3.3 or less. Preferred examples of the photopolymerizable compound having a LogP value of more than 3.3 include dodecyl (meth)acrylate, octadecyl (meth)acrylate, isobornyl (meth)acrylate, and 1,9-nonanediol di(meth)acrylate.

[0062] The photopolymerizable compound may be alkali-insoluble from the viewpoint of easily obtaining a pixel portion (cured product of the ink composition) having excellent reliability. In this specification, the photopolymerizable compound being alkali-insoluble means that the amount of the photopolymerizable compound dissolved in a 1% by mass aqueous potassium hydroxide solution at 25°C is 30% by mass or less based on the total mass of the photopolymerizable compound. The above-mentioned amount of the photopolymerizable compound dissolved is preferably 10% by mass or less, more preferably 3% by mass or less.

[0063] The content of the photopolymerizable compound may be 10 parts by mass or more, 15 parts by mass or more, or 20 parts by mass or more with respect to 100 parts by mass of the nonvolatile content of the ink composition from the viewpoint of easily obtaining a suitable viscosity as an inkjet ink, from the viewpoint of good curability of the ink composition, and from the viewpoint of improving the solvent resistance and abrasion resistance of the pixel portion (cured product of the ink composition). The content of the photopolymerizable compound may be 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, or 20 parts by mass or less with respect to 100 parts by mass of the nonvolatile content of the ink composition from the viewpoint of easily obtaining a suitable viscosity as an inkjet ink and from the viewpoint of obtaining better optical properties (for example, external quantum efficiency).

[0064] [Light scattering particles] The ink composition may further contain light-scattering particles. The light-scattering particles are, for example, optically inactive inorganic fine particles. When the ink composition contains light-scattering particles, the light from the light source irradiated to the pixel portion can be scattered, so that excellent optical properties (for example, external quantum efficiency) can be obtained.

[0065] Examples of materials constituting the light-scattering particles include simple metals such as tungsten, zirconium, titanium, platinum, bismuth, rhodium, palladium, silver, tin, platinum, and gold; metal oxides such as silica, barium sulfate, barium carbonate, calcium carbonate, talc, clay, kaolin, barium sulfate, barium carbonate, calcium carbonate, alumina white, titanium oxide, magnesium oxide, barium oxide, aluminum oxide, bismuth oxide, zirconium oxide, and zinc oxide; metal carbonates such as magnesium carbonate, barium carbonate, bismuth subcarbonate, and calcium carbonate; metal hydroxides such as aluminum hydroxide; complex oxides such as barium zirconate, calcium zirconate, calcium titanate, barium titanate, and strontium titanate; and metal salts such as bismuth subnitrate. From the viewpoint of excellent ejection stability and an excellent effect of improving external quantum efficiency, the light-scattering particles preferably contain at least one type selected from the group consisting of titanium oxide, alumina, zirconium oxide, zinc oxide, calcium carbonate, barium sulfate, barium titanate, and silica, and more preferably contain at least one type selected from the group consisting of titanium oxide, zirconium oxide, zinc oxide, and barium titanate.

[0066] The shape of the light-scattering particles may be spherical, filamentous, irregular, etc. However, it is preferable to use particles having a less directional particle shape (for example, spherical, regular tetrahedral, etc.) as the light-scattering particles, since this can further improve the uniformity, fluidity, and light scattering properties of the ink composition and can provide excellent ejection stability.

[0067] The average particle diameter (volume average diameter) of the light scattering particles in the ink composition may be 50 nm or more, 200 nm or more, or 300 nm or more from the viewpoint of excellent ejection stability and excellent effect of improving external quantum efficiency. The average particle diameter (volume average diameter) of the light scattering particles in the ink composition may be 1000 nm or less, 600 nm or less, or 400 nm or less from the viewpoint of excellent ejection stability. From the viewpoint of easy obtaining such an average particle diameter (volume average diameter), the average particle diameter (volume average diameter) of the light scattering particles used may be 50 nm or more, or 1000 nm or less. In this specification, the average particle diameter (volume average diameter) of the light scattering particles in the ink composition is measured by a dynamic light scattering nanotrack particle size distribution meter and obtained by calculating the volume average diameter. In addition, the average particle diameter (volume average diameter) of the light scattering particles used is obtained by, for example, measuring the particle diameter of each particle by a transmission electron microscope or a scanning electron microscope and calculating the volume average diameter.

[0068] The content of the light scattering particles may be 0.1 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more relative to 100 parts by mass of the nonvolatile content of the ink composition, from the viewpoint of a more excellent effect of improving external quantum efficiency. The content of the light scattering particles may be less than 10 parts by mass relative to 100 parts by mass of the nonvolatile content of the ink composition, from the viewpoint of excellent compatibility with the inkjet process and optical properties and their reproducibility, and may be 9 parts by mass or less, 7 parts by mass or less, or 5 parts by mass or less, from the viewpoint of more easily obtaining the effect.

[0069] The mass ratio of the content of the light-scattering particles to the content of the luminescent nanocrystal particles (light-scattering particles / luminescent nanocrystal particles) is preferably 0.05 or more, 0.07 or more, 0.1 or more, 0.13 or more, or 0.15 or more, from the viewpoint of excellent effect of improving external quantum efficiency. The mass ratio (light-scattering particles / luminescent nanocrystal particles) is preferably 0.2 or less, 0.19 or less, 0.18 or less, 0.17 or less, or 0.16 or less, from the viewpoint of further excellent compatibility with inkjet processes and optical properties and their reproducibility.

[0070] The total amount of the luminescent nanocrystal particles and the light scattering particles in the ink composition is preferably 20 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more, based on 100 parts by mass of the nonvolatile content of the ink composition, from the viewpoint of easily obtaining an appropriate viscosity for an inkjet ink. The total amount of the luminescent nanocrystal particles and the light scattering particles in the ink composition is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, based on 100 parts by mass of the nonvolatile content of the ink composition, from the viewpoint of easily obtaining an appropriate viscosity for an inkjet ink.

[0071] [Photopolymerization initiator] The ink composition may further contain a photopolymerization initiator. The photopolymerization initiator is, for example, a photoradical polymerization initiator or a photocationic polymerization initiator. As the photoradical polymerization initiator, a molecular cleavage type or a hydrogen abstraction type photoradical polymerization initiator is preferable.

[0072] As the molecular cleavage type photoradical polymerization initiator, benzoin isobutyl ether, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, etc. are preferably used. As other molecular cleavage type photoradical polymerization initiators, 1-hydroxycyclohexyl phenyl ketone, benzoin ethyl ether, benzyl dimethyl ketal, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one and 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one may be used in combination.

[0073] Examples of the hydrogen abstraction type photoradical polymerization initiator include benzophenone, 4-phenylbenzophenone, isophthalphenone, 4-benzoyl-4'-methyl-diphenyl sulfide, etc. A molecular cleavage type photoradical polymerization initiator and a hydrogen abstraction type photoradical polymerization initiator may be used in combination.

[0074] Commercially available products can also be used as the photocationic polymerization initiator. Examples of commercially available products include sulfonium salt-based photocationic polymerization initiators such as "CPI-100P" manufactured by San-Apro Co., Ltd., acylphosphine oxide compounds such as "Lucirin TPO" manufactured by BASF Co., Ltd., and "Irgacure 907", "Irgacure 819", "Irgacure 379EG", "Irgacure 184" and "Irgacure PAG290" manufactured by BASF Co., Ltd.

[0075] The content of the photopolymerization initiator may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 3 parts by mass or more, or 5 parts by mass or more relative to 100 parts by mass of the photopolymerizable compound from the viewpoint of the curability of the ink composition. The content of the photopolymerization initiator may be 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less relative to 100 parts by mass of the photopolymerizable compound from the viewpoint of the stability over time of the pixel portion (cured product of the ink composition).

[0076] [Polymer dispersant] The ink composition may further contain a polymer dispersant. The polymer dispersant is a polymer compound having a weight average molecular weight of 750 or more and a functional group having affinity for light scattering particles. The polymer dispersant has a function of dispersing light scattering particles. The polymer dispersant is adsorbed to the light scattering particles via a functional group having affinity for the light scattering particles, and disperses the light scattering particles in the ink composition by electrostatic repulsion and / or steric repulsion between the polymer dispersants. When the ink composition contains a polymer dispersant, the light scattering particles can be dispersed well even when the content of the light scattering particles is relatively high (for example, about 60% by mass). The polymer dispersant is preferably bound to the surface of the light scattering particles and adsorbed to the light scattering particles, but may be bound to the surface of the luminescent nanocrystal particles and adsorbed to the luminescent nanoparticles, or may be free in the ink composition.

[0077] Examples of functional groups having affinity for light-scattering particles include acidic functional groups, basic functional groups, and nonionic functional groups. The acidic functional groups have a dissociable proton and may be neutralized with a base such as an amine or hydroxide ion, while the basic functional groups may be neutralized with an acid such as an organic acid or an inorganic acid.

[0078] Examples of acidic functional groups include a carboxyl group (-COOH), a sulfo group (-SO3H), a sulfate group (-OSO3H), a phosphonic acid group (-PO(OH)3), a phosphoric acid group (-OPO(OH)3), a phosphinic acid group (-PO(OH)-), and a mercapto group (-SH).

[0079] Examples of basic functional groups include primary, secondary and tertiary amino groups, ammonium groups, imino groups, and nitrogen-containing heterocyclic groups such as pyridine, pyrimidine, pyrazine, imidazole and triazole.

[0080] Examples of the nonionic functional group include a hydroxy group, an ether group, a thioether group, a sulfinyl group (-SO-), a sulfonyl group (-SO2-), a carbonyl group, a formyl group, an ester group, a carbonate ester group, an amide group, a carbamoyl group, a ureido group, a thioamide group, a thioureido group, a sulfamoyl group, a cyano group, an alkenyl group, an alkynyl group, a phosphine oxide group, and a phosphine sulfide group.

[0081] The polymeric dispersant may be a polymer (homopolymer) of a single monomer, or a copolymer (copolymer) of multiple types of monomers. The polymeric dispersant may be any of a random copolymer, a block copolymer, or a graft copolymer. When the polymeric dispersant is a graft copolymer, it may be a comb-shaped graft copolymer or a star-shaped graft copolymer. The polymeric dispersant may be, for example, an acrylic resin, a polyester resin, a polyurethane resin, a polyamide resin, a polyether, a phenolic resin, a silicone resin, a polyurea resin, an amino resin, an epoxy resin, a polyamine such as polyethyleneimine and polyallylamine, or a polyimide.

[0082] As the polymer dispersant, commercially available products can be used. Examples of commercially available products that can be used include the Ajisper PB series manufactured by Ajinomoto Fine-Techno Co., Ltd., the DISPERBYK series and BYK series manufactured by BYK, and the Efka series manufactured by BASF.

[0083] [Organic solvents] The ink composition may further contain an organic solvent, such as ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol dibutyl ether, diethyl adipate, dibutyl oxalate, dimethyl malonate, diethyl malonate, dimethyl succinate, diethyl succinate, 1,4-butanediol diacetate, and glyceryl triacetate.

[0084] From the viewpoint of continuous ejection stability of the ink-jet ink, the boiling point of the organic solvent is preferably 150° C. or higher, and more preferably 180° C. or higher. In addition, since it is necessary to remove the solvent from the ink composition before curing the ink composition when forming a pixel portion, from the viewpoint of easy removal of the organic solvent, the boiling point of the organic solvent is preferably 300° C. or lower.

[0085] The organic solvent preferably contains an acetate compound having a boiling point of 150° C. or more. In this case, the affinity between the luminescent nanocrystal particles and the solvent is improved, and the luminescent nanocrystal particles can exhibit excellent luminescence properties. Specific examples of acetate compounds having a boiling point of 150° C. or more include monoacetate compounds such as diethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, and dipropylene glycol methyl ether acetate, diacetate compounds such as 1,4-butanediol diacetate and propylene glycol diacetate, and triacetate compounds such as glyceryl triacetate.

[0086] In the ink composition of this embodiment, the photopolymerizable compound also functions as a dispersion medium, so that it is possible to disperse the light-scattering particles and the luminescent nanocrystalline particles without using a solvent, which has the advantage that a step of removing the solvent by drying is not required when forming the pixel portion.

[0087] The ink composition may further contain components other than the above-mentioned components (for example, a thermosetting resin, a curing agent, a curing accelerator (curing catalyst), a polymerization inhibitor, a chain transfer agent, an antioxidant, etc.) within a range that does not impair the effects of the present invention.

[0088] The viscosity of the ink composition described above at the ink temperature during inkjet printing may be, for example, 2 mPa·s or more, 5 mPa·s or more, or 7 mPa·s or more, from the viewpoint of ejection stability during inkjet printing. The viscosity of the ink composition at the ink temperature during inkjet printing may be 20 mPa·s or less, 15 mPa·s or less, or 12 mPa·s or less. In this specification, the viscosity of the ink composition refers to the viscosity measured, for example, by an E-type viscometer, and is measured at 25°C.

[0089] When the viscosity of the ink composition at the ink temperature during inkjet printing is 2 mPa s or more, the meniscus shape of the inkjet ink at the tip of the ink ejection hole of the ejection head is stable, making it easy to control the ejection of the inkjet ink (for example, control of the ejection amount and ejection timing).On the other hand, when the viscosity of the ink composition at the ink temperature during inkjet printing is 20 mPa s or less, the inkjet ink can be smoothly ejected from the ink ejection hole.

[0090] The surface tension of the ink composition is preferably suitable for the inkjet method, specifically, preferably in the range of 20 to 40 mN / m, more preferably 25 to 35 mN / m. By setting the surface tension within this range, ejection control (e.g., control of the ejection amount and the ejection timing) can be facilitated, and the occurrence of flight curvature can be suppressed. Note that flight curvature refers to the occurrence of a deviation of 30 μm or more in the landing position of the ink composition from the target position when the ink composition is ejected from the ink ejection hole. When the surface tension is 40 mN / m or less, the meniscus shape at the tip of the ink ejection hole is stable, and therefore ejection control of the ink composition (e.g., control of the ejection amount and the ejection timing) can be facilitated. On the other hand, when the surface tension is 20 mN / m or more, the surrounding area of ​​the ink ejection hole can be prevented from being contaminated by the inkjet ink, and therefore the occurrence of flight curvature can be suppressed. That is, there is no risk of the ink composition not landing accurately on the pixel portion-forming region where it is intended to land, resulting in insufficient filling of the pixel portion, or of the ink composition landing on a pixel portion-forming region (or pixel portion) adjacent to the pixel portion-forming region where it is intended to land, resulting in reduced color reproducibility. Note that the surface tension described in this specification refers to the surface tension measured at 23°C, and is measured by the ring method (also called the ring method).

[0091] When the ink composition of the present embodiment is used as an ink composition for an inkjet system, it is preferable to apply it to an inkjet recording device of a piezo-jet system with a mechanical ejection mechanism using a piezoelectric element. In the piezo-jet system, the ink composition is not instantaneously exposed to high temperatures when ejected. Therefore, deterioration of the luminescent nanocrystal particles is unlikely to occur, and the expected luminescent characteristics can be more easily obtained in the pixel portion (light conversion layer).

[0092] Although one embodiment of the ink-jet ink composition has been described above, the ink-jet ink composition of the above-mentioned embodiment can be used in, for example, a photolithography method in addition to the ink-jet method. In this case, the ink composition contains an alkali-soluble resin as a binder polymer.

[0093] When the ink composition is used in a photolithography method, first, the ink composition is applied onto a substrate, and then the ink composition is dried to form a coating film. The coating film thus obtained is soluble in an alkaline developer, and is patterned by being treated with the alkaline developer. In this case, the alkaline developer is mostly an aqueous solution from the viewpoint of ease of waste liquid treatment of the developer, and therefore the coating film of the ink composition is treated with an aqueous solution. On the other hand, in the case of an ink composition using luminescent nanocrystalline particles (quantum dots, etc.), the luminescent nanocrystalline particles are unstable to water, and the luminescence (e.g., fluorescence) is impaired by moisture. For this reason, in this embodiment, an inkjet method that does not require treatment with an alkaline developer (aqueous solution) is preferred.

[0094] In addition, even if the coating film of the ink composition is not treated with an alkaline developer, if the ink composition is alkali-soluble, the coating film of the ink composition is likely to absorb moisture in the air, and the luminescence (e.g., fluorescence) of the luminescent nanocrystalline particles (quantum dots, etc.) is impaired over time. From this viewpoint, in this embodiment, the coating film of the ink composition is preferably alkali-insoluble. That is, the ink composition of this embodiment is preferably an ink composition capable of forming an alkali-insoluble coating film. Such an ink composition can be obtained by using an alkali-insoluble photopolymerizable compound as the photopolymerizable compound. The coating film of the ink composition being alkali-insoluble means that the amount of dissolution of the coating film of the ink composition in a 1% by mass aqueous potassium hydroxide solution at 25°C is 30% by mass or less based on the total mass of the coating film of the ink composition. The above-mentioned dissolution amount of the coating film of the ink composition is preferably 10% by mass or less, more preferably 3% by mass or less. Whether the ink composition is capable of forming an alkali-insoluble coating film can be confirmed by measuring the above-mentioned dissolution amount of a coating film having a thickness of 1 μm obtained by applying the ink composition onto a substrate and drying it under conditions of 80° C. and 3 minutes.

[0095] Another embodiment of the present invention is a cured product (cured film) of the ink composition, and it can be said that the cured product (cured film) of the ink composition is alkali-insoluble. This makes it easier to obtain pixel parts with excellent reliability. As described above, the cured product of the ink composition being alkali-insoluble means that the amount of the cured product of the ink composition dissolved in a 1% by mass aqueous potassium hydroxide solution at 25°C is 30% by mass or less based on the total mass of the cured product of the ink composition. The above-mentioned amount of dissolution of the cured product of the ink composition is preferably 10% by mass or less, more preferably 3% by mass or less.

[0096] <Method of manufacturing ink composition> The ink composition of the above-described embodiment is produced, for example, by a production method including a first step of preparing luminescent nanocrystalline particles and a second step of mixing the luminescent nanocrystalline particles, organic ligand A, and a photopolymerizable compound (and further other components as necessary).

[0097] In the first step, in one embodiment, luminescent nanocrystalline particles having an organic ligand bound to the surface are prepared. The organic ligand may be one or both of the above-mentioned organic ligand A and organic ligand B, and is preferably organic ligand B. The organic ligand can be bound to the surface of the luminescent nanocrystalline particles by a known method. Alternatively, the luminescent nanocrystalline particles having an organic ligand bound thereto can be purchased.

[0098] In the second step, all of the above components may be mixed at the same time. For example, the luminescent nanocrystal particles to which organic ligand B is bonded and the organic ligand A may be mixed first, and then the remaining components may be mixed. When replacing the dispersion medium from the solvent to the monomer, a method is preferred in which the solvent of the luminescent nanocrystal particle dispersion to which organic ligand B is bonded is removed by a method such as drying or decantation, and organic ligand A and necessary monomers are added thereto, and then the mixture is redispersed, or a method is preferred in which the organic ligand A and necessary monomers are added to the luminescent nanocrystal particle dispersion to which organic ligand B is bonded, and then the organic solvent is removed by an evaporator or thin-film distillation to obtain a monomer dispersion.

[0099] In the second step, for example, a dispersion treatment may be performed in addition to mixing. The dispersion treatment may be performed using a dispersion device such as a bead mill, a paint conditioner, a planetary agitator, or a jet mill. From the viewpoint of improving the dispersibility of the luminescent nanocrystalline particles and easily adjusting the average particle size of the luminescent nanocrystalline particles to a desired range, it is preferable to use a bead mill, a paint conditioner, or a jet mill. According to this method, the luminescent nanocrystalline particles can be sufficiently dispersed. Therefore, the optical characteristics (for example, external quantum efficiency) of the pixel portion can be improved, and an ink composition having excellent ejection stability can be easily obtained.

[0100] Luminescent nanoparticles are generally synthesized in a low polarity solvent for convenience of synthesis, and therefore the polarity of the organic ligand B bound to the luminescent nanoparticles immediately after synthesis in the first step is generally low. In this case, it was found that when the luminescent nanocrystal particles bound to the organic ligand B are mixed with a polymerizable compound (especially a highly polar polymerizable compound having a LogP value of 3.3 or less) in the second step, an increase in viscosity (and further aggregation of the luminescent nanocrystal particles) is likely to occur. In response to this, the present inventors have found that the increase in viscosity (and further aggregation of the luminescent nanocrystal particles) can be suppressed by using an organic ligand A.

[0101] <Ink composition set> An ink composition set of one embodiment includes the ink composition of the above-described embodiment. The ink composition set may include an ink composition (non-luminous ink composition) that does not contain luminous nanocrystalline particles, in addition to the ink composition (luminous ink composition) of the above-described embodiment. The non-luminous ink composition is, for example, a curable ink composition. The non-luminous ink composition may be a conventionally known ink composition, and may have the same composition as the ink composition (luminous ink composition) of the above-described embodiment, except that it does not contain luminous nanocrystalline particles.

[0102] Since the non-luminous ink composition does not contain luminous nanocrystalline particles, when light is incident on a pixel portion formed by the non-luminous ink composition (a pixel portion including a cured product of the non-luminous ink composition), the light emitted from the pixel portion has approximately the same wavelength as the incident light. Therefore, the non-luminous ink composition is suitably used for forming a pixel portion of the same color as the light from a light source. For example, when the light from the light source is light having a wavelength in the range of 420 to 480 nm (blue light), the pixel portion formed by the non-luminous ink composition can be a blue pixel portion.

[0103] The non-luminous ink composition preferably contains light-scattering particles. When the non-luminous ink composition contains light-scattering particles, the pixel portion formed by the non-luminous ink composition can scatter light incident on the pixel portion, thereby reducing the light intensity difference in the viewing angle of the light emitted from the pixel portion.

[0104] <Light conversion layer and color filter> Hereinafter, the details of the light conversion layer and the color filter obtained by using the ink composition set of the above-mentioned embodiment will be described with reference to the drawings. However, the following embodiment is an embodiment in which the ink composition contains light scattering particles. In the following description, the same or corresponding elements are designated by the same reference numerals, and duplicated descriptions will be omitted.

[0105] Fig. 1 is a schematic cross-sectional view of a color filter according to an embodiment. As shown in Fig. 1, the color filter 100 includes a base material 40 and a light conversion layer 30 provided on the base material 40. The light conversion layer 30 includes a plurality of pixel units 10 and a light shielding unit 20.

[0106] The light conversion layer 30 has a first pixel portion 10a, a second pixel portion 10b, and a third pixel portion 10c as the pixel portion 10. The first pixel portion 10a, the second pixel portion 10b, and the third pixel portion 10c are arranged in a lattice pattern so as to be repeated in this order. The light shielding portion 20 is provided between adjacent pixel portions, that is, between the first pixel portion 10a and the second pixel portion 10b, between the second pixel portion 10b and the third pixel portion 10c, and between the third pixel portion 10c and the first pixel portion 10a. In other words, these adjacent pixel portions are separated by the light shielding portion 20.

[0107] The first pixel portion 10a and the second pixel portion 10b are luminescent pixel portions (luminescent pixel portions) containing the cured product of the ink composition of the above-mentioned embodiment. The cured product shown in FIG. 1 contains luminescent nanocrystalline particles, an organic ligand, a curing component, and light-scattering particles. The first pixel portion 10a contains a first curing component 13a, and a first luminescent nanocrystalline particle 11a and a first light-scattering particle 12a, each dispersed in the first curing component 13a. Similarly, the second pixel portion 10b contains a second curing component 13b, and a second luminescent nanocrystalline particle 11b and a second light-scattering particle 12b, each dispersed in the second curing component 13b. The curing component is a component obtained by polymerization of a photopolymerizable compound, and contains a polymer of the photopolymerizable compound. In addition to the above polymer, the curing component may contain components other than the organic solvent contained in the ink composition (polymer dispersant, unreacted polymerizable compound, etc.). In the first pixel portion 10a and the second pixel portion 10b, the first curing component 13a and the second curing component 13b may be the same or different, and the first light-scattering particles 12a and the second light-scattering particles 12b may be the same or different.

[0108] First luminescent nanocrystalline particles 11a are red luminescent nanocrystalline particles that absorb light with wavelengths in the range of 420-480 nm and emit light with a peak emission wavelength in the range of 605-665 nm. That is, first pixel section 10a may be rephrased as a red pixel section for converting blue light into red light. Second luminescent nanocrystalline particles 11b are green luminescent nanocrystalline particles that absorb light with wavelengths in the range of 420-480 nm and emit light with a peak emission wavelength in the range of 500-560 nm. That is, second pixel section 10b may be rephrased as a green pixel section for converting blue light into green light.

[0109] The content of the luminescent nanocrystal particles in the luminescent pixel portion is preferably 5% by mass or more, and may be 10% by mass or more, 15% by mass or more, 20% by mass or more, or 30% by mass or more, based on the total mass of the cured product of the luminescent ink composition, from the viewpoint of achieving a superior effect of improving external quantum efficiency and obtaining superior luminescence intensity. The content of the luminescent nanocrystal particles is preferably 80% by mass or less, and may be 75% by mass or less, 70% by mass or less, or 60% by mass or less, based on the total mass of the cured product of the luminescent ink composition, from the viewpoint of achieving superior reliability of the pixel portion and obtaining superior luminescence intensity.

[0110] The content of the light-scattering particles in the luminous pixel portion may be 0.1 mass% or more, 1 mass% or more, or 3 mass% or more based on the total mass of the cured product of the luminous ink composition, from the viewpoint of a more excellent effect of improving external quantum efficiency. The content of the light-scattering particles may be 60 mass% or less, 50 mass% or less, 40 mass% or less, 30 mass% or less, 25 mass% or less, 20 mass% or less, or 15 mass% or less based on the total mass of the cured product of the luminous ink composition, from the viewpoint of a more excellent effect of improving external quantum efficiency and from the viewpoint of excellent reliability of the pixel portion.

[0111] The third pixel portion 10c is a non-luminous pixel portion (non-luminous pixel portion) containing the cured product of the non-luminous ink composition described above. The cured product does not contain luminous nanocrystalline particles, but contains light scattering particles and a curing component. That is, the third pixel portion 10c contains a third curing component 13c and a third light scattering particle 12c dispersed in the third curing component 13c. The third curing component 13c is, for example, a component obtained by polymerization of a polymerizable compound, and contains a polymer of the polymerizable compound. The third light scattering particle 12c may be the same as or different from the first light scattering particle 12a and the second light scattering particle 12b.

[0112] The third pixel unit 10c has a transmittance of 30% or more for light with a wavelength in the range of 420 to 480 nm, for example. Therefore, when a light source that emits light with a wavelength in the range of 420 to 480 nm is used, the third pixel unit 10c functions as a blue pixel unit. The transmittance of the third pixel unit 10c can be measured by a microspectrometer.

[0113] The content of the light scattering particles in the non-luminous pixel portion may be 1 mass % or more, 5 mass % or more, or 10 mass % or more based on the total mass of the cured product of the non-luminous ink composition, from the viewpoint of further reducing the light intensity difference at the viewing angle. The content of the light scattering particles may be 80 mass % or less, 75 mass % or less, or 70 mass % or less based on the total mass of the cured product of the non-luminous ink composition, from the viewpoint of further reducing light reflection.

[0114] The thickness of the pixel portion (the first pixel portion 10a, the second pixel portion 10b, and the third pixel portion 10c) may be, for example, 1 μm or more, 2 μm or more, or 3 μm or more. The thickness of the pixel portion (the first pixel portion 10a, the second pixel portion 10b, and the third pixel portion 10c) may be, for example, 30 μm or less, 20 μm or less, or 15 μm or less.

[0115] The light shielding portion 20 is a so-called black matrix that is provided to separate adjacent pixel portions to prevent color mixing and to prevent light leakage from a light source. The material constituting the light shielding portion 20 is not particularly limited, and in addition to metals such as chromium, cured products of resin compositions containing light shielding particles such as carbon fine particles, metal oxides, inorganic pigments, and organic pigments in a binder polymer, etc. can be used. As the binder polymer used here, one or more mixtures of resins such as polyimide resin, acrylic resin, epoxy resin, polyacrylamide, polyvinyl alcohol, gelatin, casein, and cellulose, photosensitive resin, and O / W emulsion type resin composition (for example, an emulsion of reactive silicone), etc. can be used. The thickness of the light shielding portion 20 may be, for example, 0.5 μm or more and 10 μm or less.

[0116] The substrate 40 is a transparent substrate having optical transparency, and can be, for example, a transparent glass substrate such as quartz glass, Pyrex (registered trademark) glass, or a synthetic quartz plate, or a transparent flexible substrate such as a transparent resin film or an optical resin film. Among these, it is preferable to use a glass substrate made of alkali-free glass that does not contain an alkali component in the glass. Specifically, Corning's "7059 Glass", "1737 Glass", "Eagle 200" and "Eagle XG", Asahi Glass's "AN100", and Nippon Electric Glass's "OA-10G" and "OA-11" are suitable. These materials have a small coefficient of thermal expansion and are excellent in dimensional stability and workability in high-temperature heat treatment.

[0117] The color filter 100 including the above-described light conversion layer 30 is suitably used when using a light source that emits light with a wavelength in the range of 420 to 480 nm.

[0118] The color filter 100 can be manufactured, for example, by forming the light-shielding portions 20 in a pattern on the substrate 40, and then forming the pixel portions 10 in the pixel portion-forming regions on the substrate 40 partitioned by the light-shielding portions 20. The pixel portions 10 can be formed by a method including a step of selectively attaching an ink composition (inkjet ink) to the pixel portion-forming regions on the substrate 40 by an inkjet method, a step of removing the organic solvent from the ink composition by drying, and a step of irradiating the dried ink composition with active energy rays (e.g., ultraviolet rays) to cure the ink composition and obtain a luminescent pixel portion. A luminescent pixel portion can be obtained by using the above-mentioned luminescent ink composition as the ink composition, and a non-luminescent pixel portion can be obtained by using a non-luminescent ink composition.

[0119] The light-shielding portion 20 can be formed by forming a thin metal film such as chromium or a thin film of a resin composition containing light-shielding particles in a region that is a boundary between a plurality of pixel portions on one surface of the substrate 40, and then patterning the thin film. The thin metal film can be formed by, for example, a sputtering method or a vacuum deposition method, and the thin film of a resin composition containing light-shielding particles can be formed by, for example, a coating method or a printing method. The patterning method can be, for example, a photolithography method.

[0120] Examples of the inkjet method include a bubble jet method using an electrothermal converter as an energy generating element, and a piezo jet method using a piezoelectric element.

[0121] In drying the ink composition, it is sufficient to remove at least a part of the organic solvent, and it is preferable to remove all of the organic solvent. The method for drying the ink composition is preferably drying under reduced pressure (reduced-pressure drying). From the viewpoint of controlling the composition of the ink composition, reduced-pressure drying is usually performed under a pressure of 1.0 to 500 Pa at 20 to 30° C. for 3 to 30 minutes.

[0122] The ink composition may be cured using, for example, a mercury lamp, a metal halide lamp, a xenon lamp, an LED, or the like. The wavelength of the irradiated light may be, for example, 200 nm or more and 440 nm or less. The exposure dose may be, for example, 10 mJ / cm. 2 or more, and 2 It may be the following:

[0123] Although an embodiment of the color filter and the light conversion layer, as well as the manufacturing method thereof, have been described above, the present invention is not limited to the above embodiment.

[0124] For example, the light conversion layer may have a pixel portion (blue pixel portion) containing a cured product of a luminescent ink composition containing blue luminescent nanocrystal particles instead of or in addition to the third pixel portion 10c. The light conversion layer may also have a pixel portion (e.g., a yellow pixel portion) containing a cured product of a luminescent ink composition containing nanocrystal particles that emit light of a color other than red, green, or blue. In these cases, it is preferable that each of the luminescent nanocrystal particles contained in each pixel portion of the light conversion layer has a maximum absorption wavelength in the same wavelength range.

[0125] At least a part of the pixel portion of the light conversion layer may contain a cured product of a composition containing a pigment other than the luminescent nanocrystalline particles.

[0126] The color filter may also have an ink-repellent layer made of a material having ink repellency narrower than the light-shielding portion on the pattern of the light-shielding portion. Instead of providing an ink-repellent layer, a photocatalyst-containing layer as a wettability-variable layer may be formed in a solid coating in a region including the pixel portion-forming region, and then the photocatalyst-containing layer may be exposed to light through a photomask to selectively increase the ink affinity of the pixel portion-forming region. Examples of photocatalysts include titanium oxide and zinc oxide.

[0127] The color filter may further include an ink receiving layer containing hydroxypropyl cellulose, polyvinyl alcohol, gelatin, or the like between the substrate and the pixel portion.

[0128] The color filter may also have a protective layer on the pixel portion. This protective layer is provided to flatten the color filter and prevent the components contained in the pixel portion, or the components contained in the pixel portion and the components contained in the photocatalyst-containing layer, from eluting into the liquid crystal layer. The material constituting the protective layer may be any material that is used as a known protective layer for color filters.

[0129] In addition, in the manufacture of the color filter and the light conversion layer, the pixel portion may be formed by a photolithography method instead of the inkjet method. In this case, first, the ink composition is applied in a layer shape to the substrate to form an ink composition layer. Next, the ink composition layer is exposed to light in a pattern shape and then developed using a developer. In this way, a pixel portion made of a cured product of the ink composition is formed. Since the developer is usually alkaline, an alkali-soluble material is used as the material of the ink composition. However, in terms of the efficiency of material use, the inkjet method is superior to the photolithography method. This is because, in principle, in the photolithography method, almost 2 / 3 or more of the material is removed, which wastes the material. For this reason, in this embodiment, it is preferable to form the pixel portion by the inkjet method using an inkjet ink.

[0130] In addition to the above-mentioned luminescent nanocrystal particles, the pixel portion of the light conversion layer of this embodiment may further contain a pigment having approximately the same color as the luminescent color of the luminescent nanocrystal particles. In order to contain the pigment in the pixel portion, the ink composition may contain the pigment.

[0131] Further, among the red pixel portion (R), green pixel portion (G), and blue pixel portion (B) in the light conversion layer of the present embodiment, one or two light-emitting pixel portions may be pixel portions containing a colorant without containing light-emitting nanocrystal particles. As the colorant that can be used here, known colorants can be used. For example, as the colorant used for the red pixel portion (R), diketopyrrolopyrrole pigments and / or anionic red organic dyes can be mentioned. As the colorant used for the green pixel portion (G), at least one selected from the group consisting of copper phthalocyanine halide pigments, phthalocyanine-based green dyes, and mixtures of phthalocyanine-based blue dyes and azo-based yellow organic dyes can be mentioned. As the colorant used for the blue pixel portion (B), ε-type copper phthalocyanine pigments and / or cationic blue organic dyes can be mentioned. When these colorants are contained in the light conversion layer, from the viewpoint of preventing a decrease in transmittance, the amount used is preferably 1 to 5% by mass based on the total mass of the pixel portion (cured product of the ink composition).

Example

[0132] Hereinafter, the present invention will be specifically described with reference to examples. However, the present invention is not limited only to the following examples. All the materials used in the examples were those in which argon gas was introduced to replace dissolved oxygen with argon gas. For titanium oxide, before mixing, it was heated at 175°C for 4 hours under a reduced pressure of 1 mmHg and then allowed to cool in an argon gas atmosphere. The liquid materials used in the examples were dehydrated with molecular sieves 3A for 48 hours or more before mixing.

[0133] [Example 1] <Preparation of QD Powder>[ An InP nanocrystal dispersion (InP QD in Heptane Red InP QD, QD particle (light-emitting nanocrystal particle) concentration 30%, organic ligand: oleic acid) manufactured by Nanosys was dried using an evaporator to obtain a QD powder (QD particle / organic ligand = 84% by mass / 16% by mass).

[0134] <Preparation of Light Scattering Particle Dispersion>[ In a container filled with argon gas, 4.0 g of titanium oxide (product name: CR-60-2, Ishihara Sangyo Kaisha, Ltd., average particle size (volume average diameter): 210 nm), 0.4 g of a polymer dispersant (product name: PB-821, Ajinomoto Fine-Techno Co., Ltd.), and 5.6 g of 1,6-hexanediol dimethacrylate (product name: Miramer M200, Miwon Co., Ltd.) were mixed. Zirconia beads (diameter: 1.25 mm) were then added to the resulting mixture, and the mixture was dispersed by shaking for 2 hours using a paint conditioner. The zirconia beads were then removed from the mixture using a polyester mesh filter to obtain a light-scattering particle dispersion.

[0135] <Preparation of Ink Composition> 3.1 g of the QD powder obtained above, 0.31 g of linolenic acid (organic ligand), and 3.82 g of dicyclopentanyl acrylate (LogP value: 2.93, product name: FA-513M, Hitachi Chemical Co., Ltd.) were mixed and stirred for 2 hours with a magnetic stirrer to obtain a QD monomer solution. 0.50 g of Omnirad TPO-H (manufactured by IGM Resin Co., Ltd.) and 0.01 g of Omnirad 819 (manufactured by IGM Resin Co., Ltd.) as photopolymerization initiators, and 0.10 g of Irganox1010 (manufactured by BASF Japan Co., Ltd.) as an antioxidant were added thereto and stirred. Furthermore, 1.0 g of the light-scattering particle dispersion obtained above was added. Finally, 0.53 g of 1,6-hexanediol dimethacrylate (LogP value: 3.13, product name: Viscoat #230, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and 0.55 g of dodecyl methacrylate (LogP value: 5.64, product name: Light Ester L, manufactured by Kyoeisha Chemical Co., Ltd.) were added, and the mixture was stirred continuously for 30 minutes to obtain an ink composition.

[0136] [Comparative Example 1] <Preparation of Ink Composition> 3.1 g of the QD powder obtained above was mixed with 4.02 g of dicyclopentanyl acrylate (LogP value: 2.93, product name: FA-513M, Hitachi Chemical Co., Ltd.) and stirred for 2 hours with a magnetic stirrer to obtain a QD monomer solution. 0.50 g of Omnirad TPO-H (manufactured by IGM Resin) and 0.01 g of Omnirad 819 (manufactured by IGM Resin) as photopolymerization initiators, and 0.10 g of Irganox1010 (manufactured by BASF Japan) as an antioxidant were added thereto and stirred. Furthermore, 1.0 g of the light-scattering particle dispersion obtained above was added. Finally, 0.59 g of 1,6-hexanediol dimethacrylate (LogP value: 3.13, product name: Viscoat #230, manufactured by Osaka Organic Chemical Industry Co., Ltd.) and 0.58 g of dodecyl methacrylate (LogP value: 5.64, product name: Light Ester L, manufactured by Kyoeisha Chemical Co., Ltd.) were added, and the mixture was stirred continuously for 30 minutes to obtain an ink composition.

[0137] [Comparative Example 2] <Synthesis of organic ligands for comparison> Polyethylene glycol (Mn350) (Sigma-Aldrich) was added to the flask, and then an equimolar amount of succinic anhydride (Sigma-Aldrich) was added to the polyethylene glycol (Mn350) while stirring in a nitrogen gas environment. The internal temperature of the flask was raised to 80°C, and the mixture was stirred for 8 hours to obtain a comparative organic ligand represented by the following formula (A) as a pale yellow viscous oil. [ka]

[0138] <Preparation of Ink Composition> An ink composition was obtained in the same manner as in Example 1, except that the comparative organic ligand synthesized above was used instead of linolenic acid (organic ligand).

[0139] [Measurement of Viscosity of Ink Composition] The viscosity of the ink compositions of the examples and comparative examples at 40° C. was measured using an E-type viscometer. The results are shown below. Example 1: 14.2 cP Comparative Example 1: Unmeasurable (due to aggregation of luminescent nanocrystalline particles in the ink composition) Comparative example 2: 19.7cP [Explanation of symbols]

[0140] 10...pixel portion, 10a...first pixel portion, 10b...second pixel portion, 10c...third pixel portion, 11a...first luminescent nanocrystal particle, 11b...second luminescent nanocrystal particle, 12a...first light-scattering particle, 12b...second light-scattering particle, 12c...third light-scattering particle, 20...light-shielding portion, 30...light conversion layer, 40...substrate, 100...color filter.

Claims

1. The composition comprises luminescent nanocrystalline particles, an organic ligand capable of binding to the surface of the luminescent nanocrystalline particles, and a photopolymerizable compound; The content of the luminescent nanocrystal particles is 20 parts by mass or more per 100 parts by mass of the non-volatile content of the ink composition. The ink composition, wherein the organic ligand comprises an organic ligand having two or more carbon-carbon double bonds.

2. 2. The ink composition according to claim 1, wherein the content of the organic ligand having two or more carbon-carbon double bonds is from 1 part by mass to 30 parts by mass with respect to 100 parts by mass of the luminescent nanocrystalline particles.

3. 3. The ink composition according to claim 1, wherein the organic ligand having two or more carbon-carbon double bonds further has a carboxyl group.

4. The ink composition according to any one of claims 1 to 3, which is used for forming a light conversion layer by an inkjet method.

5. A cured product of the ink composition according to any one of claims 1 to 4.

6. A light-shielding portion is provided between a plurality of pixel portions, The light conversion layer, wherein the plurality of pixel portions have luminescent pixel portions containing a cured product of the ink composition according to any one of claims 1 to 4.

7. As the light-emitting pixel portion, a first luminescent pixel portion containing luminescent nanocrystal particles that absorb light having a wavelength in the range of 420 to 480 nm and emit light having an emission peak wavelength in the range of 605 to 665 nm; a second luminescent pixel portion containing luminescent nanocrystal particles that absorb light having a wavelength in the range of 420 to 480 nm and emit light having an emission peak wavelength in the range of 500 to 560 nm; The light conversion layer of claim 6 .

8. A color filter comprising the light conversion layer according to claim 6 or 7.

Citation Information

Patent Citations

  • Ink composition, cured product thereof, light conversion layer, and color filter

    JP2020021033A

  • Inkjet ink for color filter, optical conversion layer, and color filter

    JP2020129034A

  • Acid stabilization of quantum dot-resin concentrates and premixes

    JP2020522591A