Gas barrier film manufacturing method and gas barrier film
By forming an aluminum oxide vapor-deposited film and adjusting secondary ion intensity ratios through time-of-flight secondary ion mass spectrometry, the method enhances gas barrier film properties, addressing the issue of insufficient barriers in conventional methods.
Patent Information
- Application Number
- JP2020158631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-23
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-09-23
AI Technical Summary
Conventional gas barrier film manufacturing methods result in films with insufficient gas barrier properties, and there is a need for improved methods to enhance these properties.
A method involving the formation of an aluminum oxide vapor-deposited film on a resin base material, followed by time-of-flight secondary ion mass spectrometry to adjust the intensity ratios of secondary ions AlO/Al, AlOH/Al, and C/CH within specific ranges to optimize gas barrier properties.
The method enables the production of a gas barrier film with enhanced oxygen and water vapor barrier properties, ensuring transparency and reducing impurities, thereby improving overall gas barrier performance.
Smart Images

Figure 0007581727000002 
Figure 0007581727000003 
Figure 0007581727000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a gas barrier film and a gas barrier film. [Background technology]
[0002] 2. Description of the Related Art In order to improve the gas barrier properties against oxygen gas and water vapor, a vapor-deposited film of an inorganic oxide such as alumina has been formed on a substrate made of a plastic film (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-001457 A Summary of the Invention [Problem to be solved by the invention]
[0004] In conventional gas barrier film manufacturing methods, there is a risk that the film may be subjected to subsequent processes with insufficient gas barrier properties. Furthermore, gas barrier films obtained by conventional gas barrier film manufacturing methods have room for improvement in terms of gas barrier properties.
[0005] The present disclosure has been made in view of the above circumstances, and has an object to provide a method for producing a gas barrier film having excellent gas barrier properties. Another object of the present disclosure is to provide a gas barrier film. [Means for solving the problem]
[0006] The present disclosure relates to a method for producing a gas barrier film, the method including the steps of forming an aluminum oxide vapor-deposited film on a resin substrate, and subjecting the aluminum oxide vapor-deposited film to time-of-flight secondary ion mass spectrometry to detect secondary ions, Al + Secondary ions for AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO+ and a step of confirming that the count number of secondary ions is 2.5 to 3.6 at the maximum. + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + and confirming that the maximum count is 4.0 to 7.0.
[0007] In one embodiment, the manufacturing method according to the present disclosure includes subjecting the aluminum oxide vapor deposition film to time-of-flight secondary ion mass spectrometry to obtain secondary ions Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) × 100 is the secondary ion CH + Secondary ion C + The method may further comprise a step of confirming that the intensity ratio C / CH is 1.0 to 3.0 when the intensity ratio C / CH is 1.7 to 3.0.
[0008] In one embodiment, the manufacturing method according to the present disclosure may further include a step of adjusting conditions for forming the aluminum oxide vapor deposition film.
[0009] The present disclosure provides a method for producing a semiconductor device comprising the steps of: (a) forming a semiconductor substrate having an aluminum oxide vapor deposition film on the resin substrate; and (b) detecting a secondary ion Al when the aluminum oxide vapor deposition film is subjected to time-of-flight secondary ion mass spectrometry. + Secondary ions for AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO + The maximum count is 2.5 to 3.6, and the secondary ion Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + The gas barrier film has a maximum count of 4.0 to 7.0.
[0010] In one embodiment, when a time-of-flight secondary ion mass spectrometry is performed on the aluminum oxide vapor deposition film of the gas barrier film according to the present disclosure, secondary ions Al +Secondary ion AlOH + The intensity ratio (AlOH / Al) × 100 is the secondary ion CH + Secondary ion C + When the intensity ratio C / CH is 1.7 to 3.0, it may be 1.0 to 3.0. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a method for producing a gas barrier film having excellent gas barrier properties. Also, according to the present disclosure, it is possible to provide a gas barrier film having excellent gas barrier properties. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram of a gas barrier film according to one embodiment. [Diagram 2] FIG. 2 is a graph showing the measurement results of the intensity ratio (AlO / Al)×100 in each example. [Diagram 3] FIG. 3 is a graph showing the measurement results of the intensity ratio (AlOH / Al)×100 in each example. [Figure 4] FIG. 4 is a graph showing the measurement results of the intensity ratio C / CH and the intensity ratio (AlOH / Al)×100 in each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Method of manufacturing gas barrier film> The method for producing a gas barrier film generally comprises a film forming step, an oxidation degree checking step, and a first hydroxide degree checking step, and may further comprise a second hydroxide degree checking step and an adjustment step.
[0014] [Film formation process] The film forming step is a step of forming an aluminum oxide vapor deposition film on a resin substrate.
[0015] (Resin substrate) The resin substrate is not particularly limited, and a known resin film (or sheet) can be used. Examples of the material of the resin substrate include polyester resins such as polyethylene terephthalate, polyamide resins such as polyamide resin 6, polyamide resin 66, polyamide resin 610, polyamide resin 612, polyamide resin 11, and polyamide resin 12, and polyolefin resins such as α-olefin polymers and copolymers such as polyethylene and polypropylene.
[0016] The resin substrate may be a single layer or a multi-layer. When the resin substrate is a multi-layer, the materials of each layer may be the same or different. The resin substrate can be obtained, for example, by using the above-mentioned resin to form a film using a film-forming method such as an extrusion method or an inflation method, or by using two or more resins to form a film by combining the resins using a multi-layer co-extrusion film-forming method.
[0017] The resin film constituting the resin substrate may be stretched uniaxially or biaxially, if desired, using a tenter system, a tubular system or the like.
[0018] The surface of the resin substrate may be subjected to plasma treatment to improve adhesion to the aluminum oxide vapor deposition film. The plasma treatment can be carried out, for example, using a hollow anode plasma treatment device (see Japanese Patent No. 4433794).
[0019] Taking into consideration gas barrier properties, processability, and the like, the thickness of the resin substrate can be practically set to 3 to 200 μm, and may be 6 to 30 μm.
[0020] (evaporated aluminum oxide film) The aluminum oxide vapor deposition film (hereinafter sometimes referred to as an alumina vapor deposition film) can be formed by using a physical vapor deposition (PVD) method such as vacuum deposition, sputtering, ion plating, ion cluster beam, etc. In the PVD method, an aluminum raw material is heated under reduced pressure, and oxygen is introduced thereto to oxidize the aluminum, thereby vapor-depositing alumina onto the resin substrate.
[0021] The thickness of the alumina vapor deposition film can be from 5 to 300 nm, and may be from 10 to 150 nm, from the viewpoints of film uniformity, flexibility, and the like.
[0022] The conditions for forming the alumina vapor deposition film are appropriately adjusted from the viewpoint of obtaining excellent gas barrier properties. The conditions for obtaining the desired oxidation and hydroxylation degrees of the alumina vapor deposition film are as follows. The alumina vapor deposition film is formed by arbitrarily changing either the amount of oxygen introduced or the amount of aluminum evaporated, or both, and using a film forming device capable of adjusting the ratio of oxygen to aluminum. Since the light transmittance of the film changes depending on the ratio of oxygen to aluminum, it is desirable for the film forming device to have a mechanism for measuring the light transmittance of the film. From the viewpoint of the uniformity of the film and the reduction of impurities, the degree of vacuum during film formation can be 0.1 Pa or less, and is desirably 0.01 Pa or less. By making the atmosphere during film formation an inert gas such as argon or dry air, it is possible to prevent gases other than oxygen from reacting with aluminum. In particular, since water vapor reacts with aluminum to increase the degree of hydroxylation, it is desirable for the water vapor partial pressure to be 0.001 Pa or less.
[0023] [Oxidation degree confirmation process] The oxidation degree confirmation process involves performing time-of-flight secondary ion mass spectrometry on the aluminum oxide deposition film, and detecting secondary ions Al + Secondary ions for AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO +It is a step of confirming that the count is 2.5 to 3.6 when it is at its maximum. When the strength ratio (AlO / Al)×100 is 2.5 or more, excellent water vapor barrier properties and transparency can be obtained, and when it is 3.6 or less, excellent oxygen barrier properties can be obtained. From this viewpoint, the strength ratio (AlO / Al)×100 may be 2.9 to 3.6.
[0024] In addition, the secondary ion AlO + The maximum count is after etching, when hydrocarbon ions originating from the atmosphere have been removed by time-of-flight secondary ion mass spectrometry. Therefore, the components of a clean aluminum oxide film are detected, and AlO + This defines the intensity ratio when the number of counts is maximum.
[0025] [First hydroxylation degree confirmation step] The first hydroxylation degree confirmation step is to perform time-of-flight secondary ion mass spectrometry on the aluminum oxide vapor deposition film, and detect the secondary ions Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + It is a step of confirming that the maximum count number is 4.0 to 7.0. When the strength ratio (AlOH / Al)×100 is in this range, excellent oxygen barrier properties can be obtained. From this viewpoint, the strength ratio (AlOH / Al)×100 in the first hydroxylation degree confirmation step may be 4.0 to 6.5, or may be 4.0 to 6.0.
[0026] [Second Hydroxidation Degree Confirmation Step] The second hydroxylation confirmation step is to perform time-of-flight secondary ion mass spectrometry on the aluminum oxide deposition film, and detect the secondary ions Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) × 100 is the secondary ion CH + Secondary ion C +When the intensity ratio C / CH is 1.7 to 3.0, it is confirmed that the intensity ratio is 1.0 to 3.0. When the intensity ratio (AlOH / Al)×100 is 1.0 or more, excellent water vapor barrier properties and transparency are easily obtained, and when it is 3.0 or less, excellent oxygen barrier properties are easily obtained. From this viewpoint, when the intensity ratio C / CH is 1.7 to 3.0, the intensity ratio (AlOH / Al)×100 may be 1.1 to 2.5.
[0027] When the intensity ratio C / CH is 1.7 to 3.0 after etching of the aluminum oxide deposition film, it is considered that the native oxide film formed by exposure to the atmosphere and AlO + The intensity ratio was obtained at a depth closer to the substrate than when it is at its maximum, where the barrier performance is easily reflected. By keeping the intensity ratio C / CH at 3.0 or less, damage caused by etching and contamination with substrate components can be suppressed, and the proportion of components not derived from the aluminum oxide vapor deposition film can be kept low.
[0028] A time-of-flight secondary ion mass spectrometer (TOF-SIMS) is a surface analysis device that performs qualitative analysis of the very surface layer (approximately 1 nm deep) of a sample. When a sample is irradiated with primary ions (pulses), the energy of the ions slightly destroys the sample surface, causing secondary ions to form. These secondary ions are then separated into positive and negative ions and detected. Taking advantage of the fact that molecular weight is proportional to flight time, the exact mass is determined by measuring the flight time until detection, and the structure of the ion is assigned from the exact mass, and the components are characterized from the multiple ion groups detected. The TOF-SIMS measurement conditions are as follows: Primary ion: Bi3 ++ Acceleration voltage: 30 kV Current: 1.6nA (DC) Neutralization gun: electrons (positive and negative), Ar ions (positive only) Etching gun: Bi Device name: nanoTOF (ULVAC-PHI, Inc.) Measurement area: 100~600μm□ Etching area: 400 to 2400 μm (The etching area should be set to be larger than the measurement area.)
[0029] [Adjustment process] The adjustment step is a step of adjusting the conditions for forming the aluminum oxide vapor deposition film. Specifically, the adjustment step is a step of feeding back to the film formation step when the alumina vapor deposition film does not have the expected strength ratio in the oxidation degree confirmation step or the first and second hydroxide degree confirmation steps. The adjustment step makes it possible to more efficiently manufacture a gas barrier film having excellent gas barrier properties.
[0030] [Other processes] The method for producing a gas barrier film may further include an anchor coat layer forming step of forming an anchor coat layer and a barrier coat layer forming step of forming a barrier coat layer. The anchor coat layer forming step can be performed prior to the film forming step, and the barrier coat layer forming step can be performed after the film forming step.
[0031] (Anchor coat layer) An anchor coat layer may be provided on the resin substrate to improve adhesion with the aluminum oxide vapor deposition film. Examples of materials for the anchor coat layer include polyester resin, polyamide resin, polyurethane resin, epoxy resin, phenol resin, (meth)acrylic resin, polyvinyl acetate resin, polyolefin resin such as polyethylene or polypropylene, or copolymers or modified resins thereof, and cellulose resin. The anchor coat layer can be formed using a resin composition containing these resins as the main component of the vehicle. For example, the primer layer described in Japanese Patent No. 4205806 may be used as the anchor coat layer.
[0032] The thickness of the anchor coat layer can be set to 0.01 to 2 μm, and may be 0.05 to 0.5 μm, from the viewpoints of the uniformity and flexibility of the layer.
[0033] (Barrier coat layer) A barrier coat layer may be provided on the alumina vapor deposition film to further improve the gas barrier property. For example, a gas barrier coating layer containing any one compound selected from metal alkoxides, their hydrolysates, and their polymers, and a hydroxyl group-containing polymer compound can be used as the barrier coat layer (see Japanese Patent No. 2790054, Japanese Patent No. 4200972, etc.).
[0034] The thickness of the barrier coat layer may be set to 0.01 to 50 μm from the viewpoints of gas barrier properties, flexibility, and the like.
[0035] <Gas barrier film> 1 is a schematic diagram of a gas barrier film according to an embodiment of the present disclosure. As shown in the figure, a gas barrier film 10 includes at least a resin substrate 1 and an aluminum oxide vapor-deposited film 2 on the resin substrate 1.
[0036] When the aluminum oxide vapor deposition layer of the gas barrier film was subjected to time-of-flight secondary ion mass spectrometry, the secondary ion Al + Secondary ions for AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO + The maximum count is 2.5 to 3.6. In addition, when the aluminum oxide vapor deposition film of the gas barrier film is subjected to time-of-flight secondary ion mass spectrometry, the secondary ion Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + The maximum count is 4.0 to 7.0. In addition, when the aluminum oxide vapor deposition film of the gas barrier film is subjected to time-of-flight secondary ion mass spectrometry, the secondary ion Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) × 100 is the secondary ion CH + Secondary ion C + When the intensity ratio C / CH is 1.7 to 3.0, it may be 1.0 to 3.0.
[0037] The gas barrier film can be formed with a printing layer or a coating layer (for example, the above-mentioned anchor coat layer or barrier coat layer) as necessary, laminated with other resin films, and then used as a packaging material, optical material, sealing material, etc. EXAMPLES
[0038] The present disclosure will be described in detail below using examples, but the present disclosure is not limited to only the following examples.
[0039] <Preparation of Barrier Film> Barrier films were produced according to the following Experimental Examples 1 to 4.
[0040] Experimental Example 1: A 12 μm-thick polyethylene terephthalate film was prepared as a transparent resin substrate, and one side of the film was subjected to hollow anode plasma treatment with an applied power of 8 kW, a treatment time of 0.05 sec, a treatment gas of a mixture of argon and oxygen, and a treatment unit pressure of 0.5 Pa. Next, an alumina vapor deposition film was formed on the plasma-treated surface of the resin substrate using an electron beam heating method. At this time, oxygen was not introduced, and the thickness of the alumina vapor deposition film was set to 10 nm. By the above method, a gas barrier film of Experimental Example 1 was obtained.
[0041] Experimental Example 2: The resin substrate was subjected to plasma treatment in the same manner as in Experimental Example 1, and an alumina vapor deposition film was provided on the plasma-treated surface of the resin substrate using an electron beam heating method. The amount of oxygen introduced during film formation was 20,000 sccm. The amount of evaporated aluminum was adjusted so that the light transmittance after film formation was 75% when the light transmittance of the resin substrate before film formation was 100%. The wavelength at which the light transmittance was measured was 366 nm. A gas barrier film of Experimental Example 2 was obtained by the above method.
[0042] Experimental Example 3: A gas barrier film of Experimental Example 3 was obtained in the same manner as in Experimental Example 2, except that the amount of oxygen introduced during film formation was set to 22,500 sccm and the amount of evaporated aluminum was adjusted so that the light transmittance was 88%.
[0043] Experimental Example 4: A gas barrier film of Experimental Example 4 was obtained in the same manner as in Experimental Example 3, except that the amount of oxygen introduced during film formation was set to 50,000 sccm and the amount of evaporated aluminum was adjusted so that the light transmittance was 98%.
[0044] The aluminum oxide vapor deposition layer of the gas barrier film obtained in each example was subjected to time-of-flight secondary ion mass spectrometry under the following conditions. Secondary ion AlO + The secondary ion Al when the count number is maximum + Secondary ions for AlO + The strength ratio (AlO / Al)×100 was calculated. The results are shown in Table 1 (degree of oxidation). It was then confirmed whether the strength ratio (AlO / Al)×100 was 2.5 to 3.6. Secondary ion AlO + The secondary ion Al when the count number is maximum + Secondary ion AlOH + The strength ratio (AlOH / Al)×100 was calculated. The results are shown in Table 1 (hydroxylation degree 1). It was then confirmed whether the strength ratio (AlOH / Al)×100 was within a range of 4.0 to 7.0. Fig. 2 is a graph showing the measurement results of the intensity ratio (AlO / Al)×100 for each example, and Fig. 3 is a graph showing the measurement results of the intensity ratio (AlOH / Al)×100 for each example. Primary ion: Bi3 ++ Acceleration voltage: 30 kV Current: 1.6nA (DC) Neutralization gun: electrons (positive and negative), Ar ions (positive only) Measurement area: 150μm□ (before etching), 100μm□ (after etching) Etching gun: Bi Etching area: 400μm Device name: nanoTOF (ULVAC-PHI, Inc.)
[0045] Time-of-flight secondary ion mass spectrometry was performed in the same manner as in the oxidation degree confirmation process. Secondary ion CH + Secondary ion C + When the intensity ratio C / CH is 1.7 to 3.0, the secondary ion Al + Secondary ion AlOH + The strength ratio (AlOH / Al)×100 was calculated. The results are shown in Table 1 (hydroxylation degree 2). It was then confirmed whether the strength ratio was 1.0 to 3.0. FIG. 4 is a graph showing the measurement results of the intensity ratio C / CH and the intensity ratio (AlOH / Al)×100 in each example.
[0046] <Various evaluations> The barrier films obtained in each example were subjected to various evaluations, and the results are shown in Table 1.
[0047] (Oxygen barrier evaluation) For the gas barrier films produced in each example, the oxygen transmission rate was measured using an oxygen transmission rate measuring device (OXTRAN 2 / 22 manufactured by MOCON) under conditions of a temperature of 30° C. and a humidity of 70%.
[0048] (Water vapor barrier evaluation) For the gas barrier films produced in each example, the water vapor transmission rate was measured using a water vapor transmission rate measuring device (PERMATRAN-W 3 / 34 manufactured by MOCON) under conditions of a temperature of 40° C. and a humidity of 90%.
[0049] (Transparency Assessment) The light transmittance of the gas barrier film produced in each example was measured using a spectrophotometer (UV-visible spectrophotometer V-650 manufactured by JASCO Corporation) at a measurement wavelength of 366 nm.
[0050] [Table 1]
[0051] The above experiments demonstrated that, by confirming that the strength ratios (AlO / Al)×100 and (AlOH / Al)×100 are within the desired ranges after the formation of the alumina vapor deposition film, it is possible to obtain excellent gas barrier films as shown in Experimental Examples 2 and 3. [Explanation of symbols]
[0052] 1...resin substrate, 2...aluminum oxide vapor deposition film, 10...gas barrier film.
Claims
1. A process for forming an aluminum oxide vapor deposition film on a resin substrate, comprising the steps of: The aluminum oxide deposition film was subjected to time-of-flight secondary ion mass spectrometry to obtain secondary ions Al + Secondary ions AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO + The count is 3.307 to 3.564 when the count is at its maximum. Secondary ion Al + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + and forming an aluminum oxide vapor deposition film that satisfies the above condition: the count number is 4.482 to 5.123 at the maximum.
2. The method according to claim 1 , further comprising the step of adjusting conditions for forming the aluminum oxide vapor deposition film.
3. A resin substrate and an aluminum oxide vapor-deposited film on the resin substrate, When the aluminum oxide deposition film was subjected to time-of-flight secondary ion mass spectrometry, secondary ions Al + Secondary ions AlO + The intensity ratio (AlO / Al) x 100 is the secondary ion AlO + The count number of the secondary ion Al is 3.307 to 3.564 at the maximum. + Secondary ion AlOH + The intensity ratio (AlOH / Al) x 100 is the secondary ion AlO + The gas barrier film has a maximum count of 4.482 to 5.123.
Citation Information
Patent Citations
Manufacture of transparent film of interrupting gas
JP1987103359A
Vapor-deposited composite film of aluminum oxide and its preparation
JP1999080934A
High gas barrier film and method for manufacturing the same
JP2003291245A
Gas barrier vapor deposition film
JP2014001457A
Barrier resin film, barrier laminate and packaging material using the barrier laminate
JP2019155646A