Nonwoven fabric manufacturing method
A controlled stretching process with specific airflow parameters and waste heat utilization addresses thread breakage issues, achieving finer and more uniform nonwoven fabric filaments.
Patent Information
- Application Number
- JP2020173254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-10-14
AI Technical Summary
Existing methods for producing finer nonwoven fabric filaments face challenges as increasing jet airflow volume or temperature leads to thread breakage and uneven filament quality due to thermal deformation and turbulence.
A method involving a controlled stretching process with a specific slit interval, temperature, and moisture removal of high-pressure air, utilizing waste heat from the manufacturing process to adjust airflow parameters, ensuring uniform filament production without excessive energy consumption.
The method produces finer filaments with improved uniformity and reduced thread breakage, utilizing waste heat to optimize airflow conditions and reduce environmental impact.
Smart Images

Figure 0007581761000002 
Figure 0007581761000003 
Figure 0007581761000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for producing a nonwoven fabric comprising a stretching process. [Background technology]
[0002] In the nonwoven fabric manufacturing apparatus, a molten thermoplastic resin is discharged from a spinneret as a filament aggregate in a spinning process, and this filament aggregate is cooled in a cooling process, and a traction force is generated on the filament aggregate by an air jet generated in a drawing process, so that the filament aggregate is sucked and drawn in a vertical direction. By controlling the air jet in this drawing process, the fiber diameter of the filaments can be adjusted.
[0003] Nonwoven fabrics are also used in the fields of sanitary products such as diapers, sanitary products, and underarm sweat pads, as well as in the field of disposable clothing, and are often used as top sheet layers that come into contact with the skin of users, etc. There has been a demand for nonwoven fabrics to have improved texture uniformity and hydrophobicity in order to improve the feel on the skin and to prevent the penetration of body fluids such as urine and blood, that is, to have finer filament fiber diameters, for example, of 9 to 13 (μm).
[0004] Here, in order to make the filaments thinner, it is necessary to increase the traction force on the filament aggregate, and to achieve this, the air volume of the injected air stream is increased or the frictional stress of the injected air stream is increased.
[0005] First, in order to further fine the filaments of the nonwoven fabric, the volume of the jet airflow is increased, specifically by increasing the pressure of the high-pressure air supplied to the drawing process. However, as described in Patent Document 1, for example, a huge amount of energy is required to generate high-pressure air. In addition, this jet airflow pulls the filament aggregate while maintaining a strong turbulent state, causing the filament aggregate to sway, which causes thread breakage. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2010 / 110293 Summary of the Invention [Problem to be solved by the invention]
[0007] On the other hand, in order to further fine the filaments of the nonwoven fabric, the frictional stress of the jet air stream is increased, specifically by increasing the temperature of the high-pressure air supplied to the drawing process. However, when the temperature of the high-pressure air is relatively high, the extremely narrow slit interval becomes non-uniform in the longitudinal direction due to thermal deformation, etc., and the jet air stream pulling the filament aggregate also becomes non-uniform, causing yarn breakage.
[0008] Therefore, it has been difficult to thin the filaments simply by increasing the volume of the jet of air or the temperature of the high-pressure air.
[0009] Therefore, an object of the present invention is to provide a method for producing a nonwoven fabric that can further finely disperse the filaments constituting the nonwoven fabric without excessively increasing the volume of the jet airflow or the temperature of the high-pressure air, and without causing thread breakage. [Means for solving the problem]
[0010] In order to solve the above problems, a method for producing a nonwoven fabric includes a spinning step in which a molten thermoplastic resin is extruded as a filament assembly composed of filaments, a cooling step in which cooling air is supplied to the filament assembly to cool it, and a stretching step in which the filament assembly is stretched by high-pressure air injected from a slit inside an ejector, and in the stretching step, the interval between the slits is set to 0.3 to 0.6 (mm), and the discharge air volume per slit length is set to 1000 to 3000 (m 3 / h / m) and the temperature of the high-pressure air is set to 30 to 60 (°C).
[0011] In addition, the manufacturing method of the nonwoven fabric may be characterized in that the stretching process includes a step of generating high-pressure air, a step of removing moisture from the generated high-pressure air, and a step of heating the high-pressure air from which the moisture has been removed.
[0012] The method for producing a nonwoven fabric may be characterized in that in the step of heating the high-pressure air, waste heat from at least one of the spinning step, the cooling step, the conveying step of conveying the filament aggregate, the entanglement step of entangling the filament aggregate to form a nonwoven fabric, the drying step of drying the nonwoven fabric, and the winding step of winding up the nonwoven fabric is utilized as a heat source for heating the high-pressure air.
[0013] The method for producing a nonwoven fabric may be characterized in that the thermoplastic resin is a polyolefin resin.
[0014] The method for producing a nonwoven fabric may be characterized in that the thermoplastic resin contains a polypropylene resin or a polypropylene-ethylene copolymer. Effect of the Invention
[0015] According to the present invention, it is possible to provide a method for producing a nonwoven fabric that can further finely disperse the filaments constituting the nonwoven fabric without excessively increasing the volume of the jetted airflow or the temperature of the high-pressure air, and without causing yarn breakage. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic diagram showing an example of a nonwoven fabric manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] 2A and 2B are diagrams illustrating the stretching means shown in FIG. 1, and show (a) a schematic diagram of the stretching means and (b) a cross-sectional perspective view of an ejector in the XZ plane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of the present invention will be described in detail with reference to Figures 1 and 2. However, the present invention is not limited to this embodiment.
[0018] <Nonwoven fabric manufacturing equipment> The bundle of filaments (hereinafter referred to as "filament aggregate") 3 according to this embodiment and the nonwoven fabric 5 including the same can be obtained by a nonwoven fabric manufacturing apparatus using a normal composite melt spinning method without using any special equipment. Among them, a nonwoven fabric manufacturing apparatus using a spunbond method, which has excellent productivity, is preferably used.
[0019] 1 shows a schematic diagram of a spunbond nonwoven fabric manufacturing apparatus (hereinafter referred to as "nonwoven fabric manufacturing apparatus") 100 as an example of a nonwoven fabric manufacturing apparatus according to one embodiment of the present invention, for illustrative purposes and not for limitation purposes. The open arrows A, B, and C in the figure respectively represent the spinning direction of the filament aggregate 3, the conveying direction (MD direction) of the filament aggregate 3, and the rotation direction of the collection belt 51. The open arrows D, E, and F in the figure respectively represent cooling air, separation gas, and high-pressure air. Furthermore, the X-axis direction in the figure indicates the conveying direction B, and the Z-axis direction indicates a direction perpendicular to the X-axis direction and parallel to the spinning direction A.
[0020] The nonwoven fabric manufacturing apparatus 100 is composed of a first extruder 11 and a second extruder 12 (spinning means, spinning process), a spinneret 20 (spinning means, spinning process), a cooling means 30 (cooling process), a stretching means (stretching process) 40, a collection conveyor (transporting means, transporting process) 50, a hot embossing roll (entangling means, entangling process) 60, and a winder (winding means, winding process) 70. The outlines of these components will be explained in order below.
[0021] The first extruder 11 melts the first raw material resin 1 and sends a predetermined flow rate of the melt to the spinneret 20 by the rotation of the spiral first rotor 13. Similarly, the second extruder 12 melts the second raw material resin 2 and sends a predetermined flow rate of the melt to the spinneret 20 by the rotation of the spiral second rotor 14.
[0022] (First raw material resin) The first raw material resin 1 is mainly composed of a thermoplastic resin. That is, the first raw material resin 1 can contain the thermoplastic resin in an amount of 90% by mass or more and 100% by mass or less based on the total solid content of the first raw material resin 1. Examples of thermoplastic resins that can be used for the first raw material resin 1 include polyolefin resins such as polypropylene (PP) and polyethylene (PE). From the viewpoint of the spinnability of filaments made of composite fibers, polypropylene (PP) is preferably used as the thermoplastic resin.
[0023] (Second raw material resin) The second raw material resin 2 is mainly composed of a thermoplastic resin. In detail, the second raw material resin 2 contains the thermoplastic resin in an amount of 90% by mass or more and 100% by mass or less based on the total solid content of the second raw material resin 2.
[0024] Thermoplastic resins applicable to the main component of the second raw material resin 2 include polyolefin resins such as polypropylene (PP) and polyethylene (PE). One type of thermoplastic resin may be used, or two or more types may be used in combination. From the viewpoint of the feel of the filament made of the composite fiber, polyethylene (PE) is preferably used as the thermoplastic resin.
[0025] (Additives) The filament made of composite fiber may contain additives, as necessary, in addition to the thermoplastic resin in each of the first raw material resin 1 and the second raw material resin 2, within the range that does not impair the object of the present invention.
[0026] Examples of raw materials for additives include various stabilizers such as known heat stabilizers and weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, and the like.
[0027] Examples of the stabilizer include anti-aging agents such as 2,6-di-t-butyl-4-methylphenol (BHT); phenolic antioxidants such as tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, β-(3,5-di-t-butyl-4-hydroxyphenyl)propionic acid alkyl ester, and 2,2'-oxamidobis[ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; fatty acid metal salts such as zinc stearate, calcium stearate, and calcium 1,2-hydroxystearate; and polyhydric alcohol fatty acid esters such as glycerin monostearate, glycerin distearate, pentaerythritol monostearate, pentaerythritol distearate, and pentaerythritol tristearate. These may also be used in combination.
[0028] Examples of the lubricant include oleamide, erucamide, and stearamide.
[0029] Furthermore, the composition may contain fillers such as silica, diatomaceous earth, alumina, titanium oxide, magnesium oxide, pumice powder, pumice balloons, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium sulfate, potassium titanate, barium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, graphite, aluminum powder, and molybdenum sulfide.
[0030] The spinneret 20 has a plurality of conjugate spinning nozzles (not shown) configured to form and discharge a desired fiber structure. From these nozzles, a filament aggregate 3 consisting of conjugate fibers formed by conjugating the melts from the first extruder 11 and the second extruder 12 is spun in the direction of gravity.
[0031] The cooling means 30 is an open type including a pair of cooling fans 30L, 30R, and blows cooling air D, which is a laminar and uniform flow, from the X-axis direction, which is a direction perpendicular to the spinning direction A, to the spun filament aggregate 3 to cool the filament aggregate 3. In addition, the high-temperature separation gas E exhausted from the filament aggregate 3 is exhausted above the pair of cooling fans 30L, 30R, not along the spinning direction A, so that the filament aggregate 3 can be efficiently cooled.
[0032] The stretching means 40 includes an ejector 41. The ejector 41 is an open type, and ejects high-pressure air F as a driving fluid with a component in the spinning direction A inside to generate a low-pressure portion. The filament assembly 3 is sucked into the ejector 41 by the generated low-pressure portion, and is stretched in the spinning direction A together with the high-pressure air F.
[0033] The collecting conveyor 50 includes a collecting belt 51, first to fourth rolls 55 to 58 wound around the apex of the inverted trapezoidal orbit of the collecting belt 51, and a suction box 59 disposed below the collecting belt 51 on the upper orbit to face it. The collecting belt 51 moves clockwise on the orbit in a circulating direction C with the driving rotation of at least one of the first to fourth rolls 55 to 58. The filament aggregate 3 drawn from the ejector 41 is directly deposited to a predetermined thickness on the collecting belt 51 of the collecting conveyor 50 and is transported to a heat embossing roll 60 in a transporting direction B.
[0034] The thermal embossing roll 60 comprises a pair of cylindrical rolls having an uneven cylindrical surface heated to a predetermined temperature and a flat cylindrical surface. The pair of cylindrical rolls squeezes the deposited filament aggregate 3, and entangles a part of the filament aggregate 3 by pressure and heat to form a nonwoven fabric 5. This entanglement process is also called a thermal embossing method, and the nonwoven fabric 5 obtained by this method has an embossed pattern on the surface.
[0035] In addition to the thermal embossing method, the nonwoven fabric 5 according to this embodiment can employ methods for entangling fibers, such as needle punching, water jetting, ultrasonic waves, or hot air through thermal fusion. The needle punching method is a method in which a needle is inserted into the filament assembly 3 to entangle the filaments. The water jet method is a method in which high-pressure water is sprayed onto the filament assembly 3 to entangle the filaments. The ultrasonic method is a method in which ultrasonic waves are used to melt and entangle some of the filaments. The hot air through method is a method in which hot air is blown onto the filament assembly 3 to melt and entangle some of the filaments.
[0036] (Nonwoven fabric) The nonwoven fabric 5 according to this embodiment is made of filament aggregates 3 and may have a single-layer structure made of one layer, or may have a multi-layer structure made of multiple layers.
[0037] The winder 70 winds the continuous nonwoven fabric 5 with a predetermined winding tightness without causing wrinkles in the fabric.
[0038] <About extension methods> FIG. 2 is a diagram for explaining the stretching means 40 shown in FIG. 1, and (a) shows a schematic diagram of the stretching means 40, and (b) shows a cross-sectional perspective view of the ejector 41 in the XZ plane. The Y-axis direction in the diagram indicates the CD direction perpendicular to the X-axis direction and the Z-axis direction, respectively. The open arrow F in the diagram indicates high-pressure air, and the black arrows H and L indicate a heat medium in a high-temperature state and a heat medium in a low-temperature state. Here, FIG. 2(b) is a diagram that is exaggerated in schematic form to explain the ejector 41, and differs from the actual positional relationship between the ejector 41 and the filament assembly 3 and the slit interval S between the pair of slits 42c. Here, the slit interval S of the ejector 41 in this embodiment is assumed to be extremely narrow (for example, 0.3 to 0.6 (mm)).
[0039] In the conventional stretching means, as described in, for example, JP-B-48-28386 (see, in particular, FIG. 1), high-pressure air F from a compressor or the like is directly introduced into the injector 41, and then the high-pressure air F is ejected from the slit as an airflow, which directly contacts the filament assembly 3 while pulling the filament assembly 3. When such a stretching means is used that directly introduces high-pressure air F from a compressor or the like into the injector 41, the temperature of the high-pressure air F becomes relatively high, and the extremely narrow slit interval S becomes non-uniform in the longitudinal direction due to thermal deformation or the like, which causes a problem of variation in the quality of the nonwoven fabric 5. In contrast, in the present embodiment, the temperature of the high-pressure air F is appropriately controlled to suppress thermal deformation of the slit 42c and improve the quality of the nonwoven fabric 5.
[0040] Furthermore, the inventors have found that moisture contained in the high pressure air F adheres to the filament aggregates 3, which may cause variations in the quality of the nonwoven fabric 5. Therefore, in this embodiment, in addition to appropriately controlling the temperature of the high pressure air F, the quality of the nonwoven fabric 5 can be further improved by removing the moisture contained in the high pressure air F as necessary.
[0041] In the stretching means 40 in this embodiment, as shown in Fig. 2(a), in order to make it possible to remove moisture contained in the high-pressure air F as necessary, a cooling type air dryer capable of processing high-pressure air F at a high pressure and a large flow rate is adopted as the dryer 48 downstream of the compressor 47, as will be described in detail later. Here, by adopting the cooling type air dryer, the high-pressure air F that has passed through the dryer 48 is cooled from a high-temperature, high-pressure state to a low-temperature, high-pressure state. At this time, the viscosity coefficient of the high-pressure air F decreases, so the frictional stress of the injected air flow in the ejector 41 decreases, and there was a risk that the traction force on the filament assembly 3 could not be increased.
[0042] Therefore, in the stretching means 40 of this embodiment, a heat exchanger 49 that is fluidly connected between the dryer 48 and the ejector 41 is used to increase the frictional stress of the high-pressure air F, as will be described in detail later, and the high-pressure air F is heated to a desired temperature as necessary.
[0043] 2(a), the stretching means 40 in this embodiment is composed of a compressor 47 that ejects high-pressure air F, a dryer 48 that removes moisture from the high-pressure air F, a heat exchanger 49 that heats the high-pressure air F to a desired temperature, and an ejector 41 that ejects the high-pressure air F to stretch the filament assembly 3, which are fluidly connected in this order. Below, an overview of each of these components will be explained in order.
[0044] The compressor 47 sucks in and compresses the surrounding air, and controls the pressure so that the pressure of the high-pressure air F supplied to the ejector 41 is high (for example, 0.1 to 0.7 (MPa)). Here, in the compressor 47, a huge amount of energy is required to generate high-pressure air F, so it is extremely difficult to further increase the pressure of the high-pressure air F.
[0045] The dryer 48 is a cooling type air dryer capable of processing high pressure and large flow rate high pressure air F. In the dryer 48, a refrigerator (not shown) or the like is used to cool the high pressure air F, whereby moisture is separated and removed due to the difference in the amount of saturated water vapor, generating dry high pressure air F with an atmospheric pressure dew point temperature of approximately -17 (°C). At this time, the separated and removed drain is discharged to the outside through a drain pipe 48a.
[0046] The heat exchanger 49 is a fin tube type heat exchanger that is excellent in heat exchange between the heat medium H, L (for example, liquid) and air. The heat exchanger 49 includes a heat exchange container 49a, a plurality of fin tubes 49b provided in the heat exchange container 49a, and a U-shaped tube 49c that fluidly connects the plurality of fin tubes 49b to each other. One end and the other end of the plurality of fin tubes 49b that are fluidly connected to each other are fluidly connected to external pipes 49d, 49e, which are closed circuits that communicate with a pump (not shown), and the heat medium H, L that recovers waste heat from the nonwoven fabric manufacturing apparatus 100 flows through the plurality of fin tubes 49b via the external pipes 49d, 49e. In addition, one end and the other end of the heat exchange container 49a include an inlet port 49f that is fluidly connected to the dryer 48 and an outlet port 49g that is fluidly connected to the ejector 41, respectively.
[0047] Therefore, in the heat exchanger 49, the high pressure air F introduced from the inlet port 49f flows around the fin tubes 49b whose surface area is increased by the fins, and is heated by efficiently exchanging heat with the high temperature heat medium H flowing inside the fin tubes 49b, and is sent to the ejector 41. Here, in order to heat the high pressure air F to a desired temperature in the heat exchanger 49, the flow rate of the high temperature heat medium H supplied to the heat exchanger 49 is adjusted by controlling the rotation speed of the pump, a flow rate adjustment valve (not shown) provided in the closed circuit, or the like.
[0048] The heat exchanger 49 in this embodiment utilizes waste heat from the nonwoven fabric manufacturing apparatus 100, and the external pipes 49d, 49e, which are closed circuits, are provided near a heat source that generates waste heat in the nonwoven fabric manufacturing apparatus 100. In addition, at least one of the spinning means (spinning process) 11, 12, 20, the cooling means (cooling process) 30, the conveying means (conveying process) 50 that conveys the filament aggregates 3, the entangling means (entangling process) 60 that entangles the filament aggregates 3 to form the nonwoven fabric 5, the drying means (drying process) (not shown) that dries the nonwoven fabric 5, and the winding means (winding process) 70 that winds up the nonwoven fabric 5 is utilized as a heat source that generates waste heat in the nonwoven fabric manufacturing apparatus 100 in this embodiment. Furthermore, the heat exchanger 49 in this embodiment is a fin-tube type heat exchanger that is excellent at exchanging heat between the heat medium H, L (e.g., liquid) and air, but is not limited to this. For example, when using a heat source that generates waste heat as waste gas in the nonwoven fabric manufacturing apparatus 100, a plate type heat exchanger that is excellent at exchanging heat between air and air may be used.
[0049] As shown in FIG. 2(b), the ejector 41 is composed of an upper body 42 and a lower body 43 connected to the upper body 42. First, the upper body 42 is a horizontally elongated, approximately rectangular parallelepiped, and has an intake port 42a at the center in the X-axis direction, penetrating in the Z-axis direction and extending in the Y-axis direction. The upper body 42 also has a pair of chambers 42b inside, which face each other in the X-axis direction and extend in the Y-axis direction so as to sandwich the intake port 42a. The upper body 42 has a pair of slits 42c extending in the Y-axis direction with an extremely narrow slit interval S (e.g., 0.3 to 0.6 (mm)) in the Z-axis direction, so as to fluidically communicate the intake port 42a and the pair of chambers 42b. The pair of slits 42c are made of metal, and each has a predetermined inclination angle (e.g., 0 to 10 (°)) that is symmetrical with respect to the YZ plane. Furthermore, the upper body 42 has a plurality of inlets 42d for introducing the high-pressure air F into the pair of chambers 42b. Next, the lower body 43 is a vertically elongated, generally rectangular parallelepiped, and has an outlet port 43a at the center in the X-axis direction, which penetrates in the Z-axis direction, extends in the Y-axis direction, and is in fluid communication with the intake port 42a.
[0050] Thus, in the ejector 41, high-pressure air F is introduced into the pair of chambers 42b through a diffuser 42e fluidly connected to the inlet 42d. The high-pressure air F that has passed through the diffuser 42e is pressure-recovered and is held at high pressure in the pair of chambers 42b. The high-pressure air F held in the pair of chambers 42b is then ejected through a pair of slits 42c to the outlet 43a, generating a low-pressure portion in the intake port 42a. The filament assembly 3 is sucked into the low-pressure portion in the intake port 42a, and is stretched in the spinning direction A from the intake port 42a to the outlet 43a by the traction force generated by the ejected airflow.
[0051] Therefore, in this embodiment, on the premise that the ejector 41 has an extremely narrow slit interval S, the amount of airflow of the injected air by the compressor 47 and the temperature of the high-pressure air F by the heat exchanger 49 are appropriately adjusted, so that the filaments constituting the nonwoven fabric 5 can be further thinned without causing thread breakage, and thermal deformation of the slits 42c can be suppressed. In addition, in this embodiment, the dryer 48 is a cooling type air dryer capable of processing the high-pressure air F from the compressor 47 at a high pressure and a large flow rate, so that the moisture contained in the high-pressure air F can be separated and removed as necessary. Therefore, it is possible to suppress variations in the quality of the nonwoven fabric 5 caused by the moisture contained in the high-pressure air F adhering to the filament aggregate 3. At this time, the high-pressure air F is cooled to a low-temperature, high-pressure state by the cooling type air dryer, but since the heat exchanger 49 is fluidly connected to the downstream side of the cooling type air dryer, the temperature of the high-pressure air F can be appropriately adjusted. In addition, in the embodiment, the heat exchanger 49 actively utilizes waste heat from the nonwoven fabric manufacturing apparatus 100, and therefore, the cost of the equipment can be reduced and the environmental load can be reduced.
[0052] <Comparative evaluation of high pressure air, ejector and filament> In comparative evaluations of the high-pressure air, ejector 41, and filament according to each of Examples 1 to 10 of the present invention, eight parameters related to physical properties were compared with Comparative Examples 1 to 3. The comparative evaluations are shown in Table 1 below. Here, as a common condition in the comparative evaluations, the material of the filament was polypropylene resin. Also, in the ejector 41, the slit length in the Y-axis direction was set to 4 (m).
[0053] [Table 1]
[0054] <Evaluation of thread breakage resistance> When a filament breaks, it appears as a lump of filament in the nonwoven fabric 5. Therefore, the resistance to breakage was evaluated by measuring the number of filaments per unit area of the nonwoven fabric 5 (120,000 m2) using a defect detector (SmartView automatic defect inspection system manufactured by COGNEX). 2 ) was measured, and the number of clumped (convex) filaments per spool was measured, i.e., the number of defects. If the number of defects was 10 or more, it was rated as "X" because there was a lot of yarn breakage; if the number was 6 to 10, it was rated as "△" because there was little yarn breakage; if the number was 3 to 6, it was rated as "O" because there was almost no yarn breakage; and if the number was less than 3, it was rated as "◎" because there was no yarn breakage.
[0055] <Evaluation of uniformity of texture> Nonwoven fabrics have unevenness due to variations in filament thickness, etc. Therefore, the uniformity of the formation was evaluated by acquiring a light transmission image of the nonwoven fabric 5 using a formation totalizer (FMT-MIII formation evaluation system manufactured by Nomura Shoji Co., Ltd.) and measuring the formation index (variable coefficient of absorbance, the smaller the value, the better the formation). If the average value was 400 or more, it was marked as "x", if the average value was 350 or more and less than 400, it was marked as "△", if the average value was 300 or more and less than 350, it was marked as "○", and if the average value was less than 300, it was marked as "◎".
[0056] In this embodiment, when the "air volume per unit length of the slit" is large or the "temperature of the high-pressure air F" is high, the traction force of the jet airflow on the filament aggregate 3 increases, and the "fiber diameter of the filament" becomes smaller, so that the "evaluation of resistance to thread breakage" decreases, while the "uniformity of the formation" tends to improve. On the other hand, when the "air volume per unit length of the slit" is small or the "temperature of the high-pressure air F" is low, the traction force of the jet airflow on the filament aggregate 3 decreases, and the "fiber diameter of the filament" becomes thicker, so that the "evaluation of resistance to thread breakage" increases, while the "uniformity of the formation" tends to decrease. In addition, when the "presence or absence of moisture removal" is "○", the moisture contained in the high-pressure air F is prevented from adhering to the filament aggregate 3, so that the "uniformity of the formation" tends to improve.
[0057] <About high pressure air pressure> In this embodiment, the "pressure of the high pressure air F" refers to the pressure of the high pressure air F supplied to the ejector 41. This "pressure of the high pressure air F" is a parameter that affects the "air volume per unit length of the slit".
[0058] In this embodiment, when a very narrow slit interval S (for example, 0.3 to 0.6 (mm)) is used, the "pressure of the high pressure air F" (see Table 1) is preferably 0.1 to 0.7 (MPa). Here, if the "pressure of the high pressure air F" is 0.1 (MPa) or more, the "air volume per unit length of the slit" is set to the desired 1000 (m), which will be described later in detail. 3 On the other hand, if the "pressure of the high pressure air F" is 0.7 (MPa) or less, the "air volume per unit length of the slit" can be set to the desired 3000 (m 3 / h / m). However, a "pressure of high pressure air" exceeding 0.7 (MPa) is not practical because it limits the compression capacity of the compressor 47 and requires a huge amount of energy consumption, so this comparative evaluation was not performed.
[0059] <About the temperature of high pressure air> In the present embodiment, the "temperature of the high-pressure air F" refers to the temperature of the high-pressure air F supplied to the ejector 41. This "temperature of the high-pressure air F" is a parameter that influences the "air volume per unit length of the slit," the "filament fiber diameter," the "evaluation of uniformity of formation," and the "evaluation of resistance to yarn breakage."
[0060] In this embodiment, the "temperature of the high pressure air F" (see Table 1) is preferably 30 to 60°C. Here, if the "temperature of the high pressure air F" is 30°C or higher, the frictional stress of the jet airflow jetted by the ejector 41 can be increased, and the "air volume per unit length of the slit" can be increased, so that the "fiber diameter of the filaments" is narrowed and the "evaluation of uniformity of the formation" can be improved. On the other hand, if the "temperature of the high pressure air F" is 60°C or lower, thermal deformation of the extremely narrow slit 42c through which the jet airflow is jetted can be suppressed and the slit interval S can be made uniform, that is, the jet airflow pulling the filament aggregate 3 can be made uniform, so that the "evaluation of resistance to yarn breakage" can be improved.
[0061] <Whether or not moisture is removed from high-pressure air> In this embodiment, "whether or not moisture is removed from the high-pressure air F" refers to whether or not the high-pressure air F is cooled in the dryer 48 to generate dry high-pressure air F with an atmospheric dew point temperature of approximately -17 (°C) due to the difference in the amount of saturated water vapor. This "whether or not moisture is removed from the high-pressure air F" is a parameter that affects the "evaluation of the uniformity of the formation".
[0062] <About slit spacing> In this embodiment, the "slit interval S" refers to the slit interval S in the Z-axis direction between the pair of slits 42c of the ejector 41. This "slit interval S" is a parameter that affects the "air volume per unit length of the slit".
[0063] The "slit interval S" in this embodiment (see Table 1) is assumed to be extremely narrow, and is preferably 0.3 to 0.6 (mm). Here, if the "slit interval S" is 0.3 (mm) or more, the "air volume per unit length of the slit" is set to the desired 1000 (m), as will be described later in detail. 3 On the other hand, if the "slit interval S" is 0.6 (mm) or less, the "air volume per unit length of the slit" can be set to the desired 3000 (m 3 / h / m) or less. It is to be noted that making the "slit interval S" less than 0.2 (mm) is not practical because it becomes very difficult to control the gap dimension, and therefore this comparative evaluation is not performed. Also, making the "slit interval S" more than 0.6 (mm) results in a very large "air volume per unit length of the slit" and causes large vibrations in the filament assembly 3, so this comparative evaluation is not performed.
[0064] <Air volume per unit length of slit> In this embodiment, the "air volume per unit length of the slit" refers to the air volume per unit length of the slit 42c in the Y-axis direction in the airflow injected from the ejector 41. This "air volume per unit length of the slit" is a parameter that influences the "filament fiber diameter," the "evaluation of uniformity of formation," and the "evaluation of resistance to yarn breakage."
[0065] In this embodiment, the "air volume per unit length of the slit" (see Table 1) is 1000 to 3000 (m 3 / h / m) is preferable. Here, the "air volume per unit length of the slit" is 1000 (m 3 If the "fiber diameter of the filament" is 3000 (m / h / m) or more, the "fiber diameter of the filament" will be as small as desired, and the "evaluation of uniformity of the formation" can be improved. On the other hand, if the "air volume per unit length of the slit" is 3000 (m 3 / h / m) or less, the vibration occurring in the filament assembly 3 can be suppressed, and the "evaluation of resistance to yarn breakage" can be improved.
[0066] <About filament fiber diameter> As for the fiber diameter of the filaments, in the same manner as the average single fiber fineness (dtex), a photograph of the filaments was taken at a magnification of 1000 times using an electron microscope (Hitachi S-3500N), and 100 of the filaments were randomly selected, the fiber diameter (denier) of the selected filaments was measured, and the average value of the 100 filaments was calculated. This fiber diameter of the filaments is a parameter that affects the "evaluation of the uniformity of the formation."
[0067] <Comparative evaluation results for high pressure air, ejector and filament> As is clear from the comparison of the evaluations of Examples 1 to 10, the "slit interval S" is extremely narrow, 0.3 to 0.6 (mm), and the "air volume per unit length of the slit" is 1000 to 3000 (m 3 / h / m) and the "temperature of the high-pressure air F" of 30 to 60 (℃), it is possible to increase the traction force exerted by the injected air current on the filament aggregate 3, make the "filament fiber diameter" relatively thin (9 to 13 (μm)), and also achieve a "resistance to yarn breakage" and "uniformity of texture" of "△" or higher, thereby achieving a well-balanced improvement.
[0068] Here, by bringing the "pressure of the high-pressure air F" and the "temperature of the high-pressure air F" closer to the upper limit (0.7 (MPa) and 60 (℃)) (see Examples 3 and 5), or bringing the "slit interval S" closer to the upper limit (0.6 (mm)) (see Example 6), the "air volume per unit length of the slit" increases, and the "filament fiber diameter" can be made even thinner. As a result, although the "evaluation of resistance to yarn breakage" is "△", the "evaluation of uniformity of texture" can be improved to "○" or "◎".
[0069] Furthermore, by changing the "whether or not moisture is removed by high-pressure air F" from "×" (see Examples 1 to 3) to "○" (see Examples 8 to 10), the "evaluation of uniformity of texture" can be further improved.
[0070] In contrast to the above, in Comparative Example 1, the "pressure of the high-pressure air F" and the "slit interval S" are less than the preferred lower limit, so the "air volume per unit length of the slit" is small and the "fiber diameter of the filament" is thick. As a result, the "evaluation of the uniformity of the formation" is "x", which is lowered. In Comparative Example 2, the "temperature of the high-pressure air F" is less than the preferred lower limit, so the traction force of the jet airflow on the filament aggregate 3 is small and the "fiber diameter of the filament" is thick, so the "uniformity of the formation" is "x", which is lowered. Furthermore, in Comparative Example 3, the "temperature of the high-pressure air F" is greater than the preferred upper limit, so the slit 42c is thermally deformed, so the slit interval S becomes non-uniform, that is, the jet airflow pulling the filament aggregate 3 becomes non-uniform, which causes variations in the degree of cooling of the filament and the fiber diameter of the filament. As a result, the "evaluation of the resistance to thread breakage" and the "evaluation of the uniformity of the formation" are "x", which are lowered.
[0071] <Other> The present invention is not limited to the above-described embodiments, examples, and modified examples, and can be modified or changed as appropriate without departing from the technical concept of the present invention. [Explanation of symbols]
[0072] 1. First raw resin 2. Second raw material resin 3 Filament assembly 5. Nonwoven fabric 11 First extruder (spinning process) 12 Second extruder (spinning process) 20 Spinneret (spinning process) 30 Cooling means (cooling process) 30L,30R cooling blower 40 Stretching means (stretching process) 41 Ejector 42 Upper body 42a Air intake 42b Twin chambers 42c Pair of slits 42d Introduction 42e Diffuser 43 Lower Body 43a Discharge port 47 Compressor 48 Hairdryer 48a Drain pipe 49 Heat exchanger 49a Heat exchange vessel 49b Fin Tube 49c U-tube 49d, 49e External piping 49f Inlet port 49g Exit Port 50 Collection conveyor 51 Collection Belt 59 Suction Box 60 Heat embossing roll 70 Winder 100 Spunbond nonwoven fabric manufacturing equipment D Cooling Air E Separation gas F High pressure air H High temperature heat transfer medium L Low temperature heat transfer medium S slit spacing V spinning speed
Claims
1. A method for producing a nonwoven fabric, comprising the steps of: A spinning process in which the molten thermoplastic resin is extruded as a filament aggregate composed of filaments; a cooling step of supplying cooling air to the filament assembly to cool it; a stretching step of stretching the filament assembly by high-pressure air injected from a slit inside an ejector; Equipped with In the stretching step, The interval between the slits is set to 0.3 to 0.6 (mm), and the air volume per unit length of the slit is set to 1000 to 3000 (m 3 / h / m) and the temperature of the high pressure air is 30 to 60 (°C).
2. The stretching step comprises: generating high pressure air; removing moisture from the generated high-pressure air by cooling it; heating the high-pressure air from which moisture has been removed; The method for producing a nonwoven fabric according to claim 1, further comprising:
3. In the step of heating the high pressure air, 3. The method for producing a nonwoven fabric according to claim 1, characterized in that waste heat from at least one of the spinning process, the cooling process, the conveying process for conveying the filament aggregate, the entangling process for entangling the filament aggregate to form a nonwoven fabric, the drying process for drying the nonwoven fabric, and the winding process for winding up the nonwoven fabric is utilized as a heat source for heating the high-pressure air.
4. The method for producing a nonwoven fabric according to any one of claims 1 to 3, wherein the thermoplastic resin is a polyolefin resin.
5. The method for producing a nonwoven fabric according to any one of claims 1 to 4, wherein the thermoplastic resin comprises a polypropylene resin or a polypropylene-ethylene copolymer.
Citation Information
Patent Citations
High speed air current drawing apparatus
JP1977008178A
Nonwoven fabric made of polypropylene and its production
JP2001146670A
Method for producing nonwoven fabric from continuous filament
JP2001181957A
Method and machine for producing web with unidirectionally arranged filaments
JP2003278070A
Production method for filament non-woven fabric
WO2010110293A1