Fine polytetrafluoroethylene fiber and its manufacturing method
The matrix spinning process with controlled conditions produces PTFE fibers with fine fineness and strength, addressing the limitations of existing methods for high-efficiency bag filters by ensuring uniformity and reducing yarn breakage.
Patent Information
- Application Number
- JP2020196583
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-27
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Existing methods for producing polytetrafluoroethylene (PTFE) fibers with fineness of 1.5 dtex or less are inadequate for high-efficiency bag filters due to uneven distribution, poor uniformity, and increased risk of yarn breakage during stretching, making them unsuitable for collecting smaller dust particles effectively.
A method involving a matrix spinning process with specific conditions: using a mixture of viscose and PTFE dispersion in a controlled coagulation bath with sulfuric acid and sodium sulfate, precise nozzle discharge, controlled firing and stretching, and alkaline washing to produce PTFE fibers with a fineness of 0.1 to 1.5 dtex, carbon content of 2.0% to 4.0%, and optimal tensile strength.
The method achieves PTFE fibers with fine fineness and high tensile strength, suitable for high-efficiency bag filters, maintaining excellent properties like heat resistance and chemical resistance while ensuring stable production and reduced yarn breakage.
Smart Images

Figure 0007581801000001
Abstract
Description
[Technical field]
[0001] The present invention relates to fine polytetrafluoroethylene fibers and a method for producing the same. [Background technology]
[0002] Fluororesin fibers, such as polytetrafluoroethylene (hereinafter sometimes referred to as PTFE) fibers, are widely used, primarily for industrial material applications, due to their excellent heat resistance, chemical resistance, electrical properties, and low friction coefficient and excellent sliding properties.
[0003] For example, PTFE fibers are widely used in bag filters for waste incinerators, taking advantage of their heat resistance and chemical resistance. Specifically, composites of PTFE fibers and glass fibers are used. In recent years, awareness of environmental issues has increased, and from the perspective of air pollution, one of these issues, there is a demand for highly efficient bag filters that can capture dust particles with smaller particle sizes. To solve this problem, finer PTFE fibers are required, and PTFE fibers with a fineness of 1.5 dtex or less are desired, but PTFE fibers with a fineness of 1.5 dtex or less have not been obtained.
[0004] Generally, as a method for producing PTFE fiber, in addition to the matrix spinning method in which a matrix substance is used for spinning and then a sintering process is performed, the split peeling method or paste extrusion method are known. Although the PTFE fiber obtained by the split peeling method or paste extrusion method has a low shrinkage rate against heat and excellent dimensional stability, since the fiber is produced by finely slicing, the cross section of the final fibrous material is flat and non-uniform, and the fineness is random and poor in uniformity. For this reason, fine fibers may be unevenly distributed locally, and when used as a bag filter, there is a disadvantage that breakage and leakage occur from the unevenly distributed fine fibers.
[0005] On the other hand, PTFE fibers obtained by the matrix spinning method have the advantages of uniform fiber cross section and small variation in fineness, and are known to be excellent for fineness (see Patent Document 1). Example 1 of Patent Document 1 describes that viscose is used as the matrix, 50% by weight of viscose is mixed with 50% of a 60% concentration of PTFE aqueous dispersion, and then the molding liquid is degassed under reduced pressure of 10 Torr and discharged into a coagulation bath through a hole diameter of 0.12 mm, semi-baked at a temperature of 280°C while providing 4% relaxation, then baked using a baking roller maintained at 350°C, taken up at a speed of 30 m / min, and hot-drawn at a temperature of 350°C to obtain fine PTFE fibers.
[0006] Moreover, Example 1 of Patent Document 2 describes that viscose is used as a matrix, and is mixed with an aqueous dispersion of high molecular weight PTFE having a number average molecular weight of 9,000,000, and spun using a spinneret. The matrix material is burned off in a baking process, and the undrawn yarn is temporarily wound up and then drawn at a draw ratio of 7 to obtain PTFE fiber. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2006-207097 A [Patent Document 2] JP 2017-82359 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the examples of Patent Document 1, the fineness is described as 2.2 dtex, which is not suitable for use as a high-capturing efficiency bag filter for capturing dust particles smaller than those of conventional products. In addition, in the examples of Patent Document 2, the fineness of 3.5 dtex is obtained by drawing an undrawn yarn at a draw ratio of 7 times, and no PTFE fiber with a fineness of 1.5 dtex or less has been obtained. Increasing the draw ratio of an undrawn yarn is not suitable from the viewpoint of industrial production, as it is prone to yarn breakage.
[0009] Therefore, an object of the present invention is to provide a fine polytetrafluoroethylene fiber with good productivity, which is suitable for use in high-capture efficiency bag filters and which can be produced by finely finening the fiber with a focus on the discharge from the spinning nozzle and the firing process while maintaining the material properties of fluorine-based fibers, such as heat resistance, chemical resistance, electrical properties, and a low friction coefficient and excellent sliding properties, and which is suitable for use in high-capture efficiency bag filters and which can be produced by a method for producing the fine polytetrafluoroethylene fiber. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention is configured as follows. [1] Single fiber fineness is 0.1 dtex or more 0.3dtex The following refers to polytetrafluoroethylene fibers, characterized in that the carbon content is 2.0% or more and 4.0% or less based on the fiber weight.
[0011] [2] A method for producing polytetrafluoroethylene fibers, comprising the steps of: extruding a mixture of viscose and an aqueous dispersion of polytetrafluoroethylene into a coagulation bath of an aqueous solution having a sulfuric acid concentration of 7% to 13% and a sodium sulfate concentration of 7% to 15% from a spinning nozzle having an extrusion hole of 40 μm to 80 μm and an orifice length of 40 μm or more at a take-up speed / extrusion linear speed of 1.5 to 4.0; having a total fineness / width of 100 ktex / m or less when passing through baking rollers; semi-baking at a temperature of 200° C. to 320° C. while providing 1% to 5% relaxation between baking rollers, followed by baking at a temperature of 320° C. to 350° C.; and either taking up the fiber once or stretching the fiber as it is. Effect of the Invention
[0012] The fine polytetrafluoroethylene fiber of the present invention can be made fine enough to be suitable for use in a high-capture efficiency bag filter. Furthermore, according to the method for producing the fine polytetrafluoroethylene fiber of the present invention, it is possible to obtain a fine polytetrafluoroethylene fiber suitable for use in a high-capture efficiency bag filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Polytetrafluoroethylene fiber> In general, fluororesins include PTFE copolymers such as tetrafluoroethylene-hexafluoropropylene polymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), and tetrafluoroethylene olefin copolymer (ETFE), which are produced by melt spinning. However, in the present invention, the PTFE resin is used, which is the most excellent in terms of heat resistance and chemical resistance. The PTFE of the present invention may be polytetrafluoroethylene, and is not particularly limited, but the number average molecular weight of PTFE is preferably 1 million or more, and more preferably 2 million or more and less than 12 million. By making the number average molecular weight of PTFE 2 million or more, it is possible to obtain woven fabrics, knitted fabrics, and webs with good tensile strength and good processability in the weaving process and carding process, and excellent quality. If the number average molecular weight of PTFE is 12 million or more, the spinnability is significantly deteriorated, making industrial production difficult.
[0014] The single fiber fineness of the polytetrafluoroethylene fiber of the present invention is preferably 0.1 dtex or more and 1.5 dtex or less. If the single fiber fineness is less than 0.1 dtex, the spinnability is significantly deteriorated, making industrial production difficult. On the other hand, if the single fiber fineness exceeds 1.5 dtex, the effect of fineness is reduced, making it unsuitable for use in high-capture efficiency bag filters.
[0015] The polytetrafluoroethylene fiber of the present invention preferably has a carbon content of 2.0% or more and 4.0% or less based on the fiber weight. If the carbon content is less than 2.0%, interfiber adhesion occurs, especially when the fiber is finely milled, and fabric defects in the weaving process and neps in the carding process are likely to occur, resulting in a significant decrease in productivity. If the carbon content exceeds 4.0%, the amount of foreign matter in the polytetrafluoroethylene fiber increases, the tensile strength decreases, and thread breakage is likely to occur in the drawing process and the weaving process and carding process, which are high-level processing, resulting in a significant decrease in productivity.
[0016] The tensile strength is preferably 0.8 cN / dtex or more and 3.0 cN / dtex or less. It is more preferably 1.0 cN / dtex or more and 2.8 cN / dtex or less. If it is less than 0.8 cN / dtex, the tensile strength becomes too weak, fiber breakage occurs frequently during high-order processing, and high-order processability is poor. Furthermore, the strength as a structure is also low, and the life of the structure is generally shortened. Also, those having a fiber tensile strength of more than 3.0 cN / dtex can be produced by increasing the baking temperature, but increasing the baking temperature causes fusion between single fibers, which makes it easier for fabric defects in the weaving process and neps in the carding process to occur, affecting productivity. Furthermore, the fiber tensile elongation is preferably 10% or more and 50% or less. It is more preferably 20% or more and 40% or less. If it is less than 10%, the stretch ratio needs to be increased, and process troubles due to stretch breakage occur frequently, resulting in poor productivity and a poor yield. If it exceeds 50%, the fiber becomes easily stretched and processability becomes poor. In addition, the product becomes easily stretched under load, tending to have poor dimensional stability.
[0017] <Method of manufacturing polytetrafluoroethylene fiber> The fine PTFE fiber of the present invention is made of PTFE resin, which is a type of fluororesin, and is preferably produced by a matrix spinning method in which a matrix substance is used for spinning, followed by a sintering step.
[0018] The matrix material is not particularly limited as long as it is a viscose that is commonly used in the production of rayon. A preferred example is viscose with a cellulose concentration of 5.0 to 11.0 wt%, an alkali concentration of 4.0 to 10.0 wt%, and carbon disulfide concentration of 27.0 to 32.0 wt% (relative to cellulose).
[0019] The PTFE resin dispersion used in the present invention for preparing the spinning dope preferably has a PTFE concentration of 50.0 to 70.0 wt% and contains a nonionic or anionic surfactant as a stabilizer in an amount of 3.0 to 10.0 wt% based on the PTFE polymer. The size of the dispersed particles in the PTFE resin dispersion is preferably 0.5 μm or less, more preferably 0.3 μm or less.
[0020] These spinning dope solutions are subjected to the spinning process after being degassed, but if the temperature during degassing is too high, there is a concern that the viscose will solidify, and there is also a concern that the water will evaporate and the PTFE will aggregate. Therefore, it is preferable to control the temperature during degassing to a low temperature of 15°C or less. The degree of vacuum during this process is preferably about 10 Torr or less.
[0021] Next, these spinning dope solutions are discharged from a die immersed in a coagulating bath and are coagulated in the coagulating bath.
[0022] As the coagulation bath, an aqueous solution of an inorganic mineral acid or an inorganic salt is used, but in the present invention, it is preferable to use a mixed aqueous solution containing sulfuric acid and sodium sulfate.
[0023] In this case, the sulfuric acid concentration is preferably 7.0 to 13.0 wt%. If the sulfuric acid concentration is less than 7.0 wt%, the speed at which the yarn coagulates in the coagulation bath becomes very slow, which is undesirable as it reduces production capacity or requires a longer immersion line. On the other hand, if the sulfuric acid concentration exceeds 13.0 wt%, the sulfuric acid attached to the fiber surface is difficult to deoxidize, and yarn breakage occurs frequently during the baking process.
[0024] The sodium sulfate concentration is preferably adjusted to 7.0 to 15.0 wt%. Sodium sulfate inhibits rapid coagulation of cellulose. If the sodium sulfate concentration is less than 7.0 wt%, the rate at which the threads coagulate in the coagulation bath becomes very fast, which is undesirable as it makes it difficult to control the fiber cross section. On the other hand, if the sodium sulfate concentration exceeds 15.0 wt%, the rate at which the threads coagulate in the coagulation bath becomes very slow, which is undesirable as it makes it difficult to control the fiber cross section. It is effective to use a mixed aqueous solution containing both the sulfuric acid concentration and the sodium sulfate concentration within the above-mentioned specific range as the coagulation bath in order to produce uniform PETF fibers.
[0025] The hole diameter of the nozzle hole to be used is preferably 40 μm or more and 80 μm or less, and the hole length is preferably 40 μm or more. When the hole diameter of the nozzle hole is in this range, an appropriate extrusion linear velocity is obtained, and good stretchability is imparted. In addition, when the hole length is in this range, the back pressure of the nozzle can be secured, and the spinning dope is evenly distributed to each hole of the nozzle, which leads to stable productivity of fine polytetrafluoroethylene fiber.
[0026] From the viewpoint of fineness, the take-up speed / discharge linear speed when discharging the spinning dope from the spinning nozzle is preferably 1.5 to 4.0. When this value is 1.5 or more, the spun yarn can maintain an appropriate tension and can be spun without adjacent single yarns adhering to each other, and when it is 4.0 or less, single yarn breakage due to excessive tension can be suppressed.
[0027] The solidified fibers are then washed in a refining process, and then semi-calcined and calcined.
[0028] For the scouring, it is preferable to wash with an alkaline aqueous solution containing an alkaline salt. In such an alkaline washing bath, an aqueous solution of a compound selected from hydroxides, carbonates, and bicarbonates of an alkaline metal or an alkaline earth metal is used, but generally, an aqueous solution of an alkaline metal salt, especially an aqueous solution of caustic soda, is preferably used. The concentration of these alkaline salts is preferably 0.08wt% or more and 0.18wt% or less. More preferably, it is 0.10wt% or more and 0.16wt% or less. If it is less than 0.08wt%, cellulose is difficult to decompose during burning, and as a result, a large amount of cellulose that cannot be completely decomposed remains in the fiber after burning, making subsequent drawing difficult, and thread breakage tends to occur frequently in the drawing process. On the other hand, if it exceeds 0.18wt%, cellulose begins to dissolve during alkaline washing, and residue tends to accumulate in the alkaline bath and guide. In addition, the strength of the undrawn yarn when entering the semi-burning and burning processes is low, and it is not preferable because it is easy to cause troubles through the process due to thread breakage.
[0029] Furthermore, the temperature of the alkaline bath is preferably 20° C. or less, and more preferably 15° C. or less. If the temperature of the alkaline bath exceeds 20° C., like the case where the alkali concentration is too high, cellulose dissolves in the alkaline washing, and residue tends to accumulate in the alkaline bath and on the guides, and the strength of the undrawn yarn decreases when it enters the semi-baking and baking processes, making it more likely to cause problems during the process, which is not preferable.
[0030] After scouring, semi-calcination is carried out. For semi-calcination, a contact type calcination roller or a non-contact type calcination heater can be used, but a contact type calcination roller is preferably used.
[0031] The undrawn yarn derived from the scouring bath or alkali bath may be passed through a contact-type semi-baking process maintained at a temperature of 200°C to 320°C while being relaxed by 1.0% to 5.0% between the baking rollers, to perform the semi-baking. In the contact-type semi-baking process maintained at a temperature of 200°C to 320°C, the undrawn yarn guided to the rollers rapidly shrinks on the rollers and increases in tension. If the relaxation rate is less than 1%, the tension becomes too high, making it difficult to maintain a uniform fiber cross section, and yarn breakage due to shrinkage is likely to occur frequently. If the relaxation rate exceeds 5%, the yarn is likely to slacken and problems with process passability are likely to occur. However, the relaxation may be given only once between the rollers immediately after entering the semi-baking, or may be given between the rollers in the semi-baking process and between the rollers in the baking process. The semi-baking process is performed before entering the subsequent baking process. If the roller temperature in the semi-baking step is lower than 200°C, the fibers are suddenly heated in the subsequent baking step, causing deformation of the fiber cross section or fusion between the single yarns. On the other hand, if the temperature is higher than 320°C, the fibers are suddenly heated in the semi-baking step, causing deformation of the fiber cross section or fusion between the single yarns. Therefore, the roller temperature in the semi-baking step is 200°C or higher and 320°C or lower, more preferably 250°C or higher and 320°C or lower. In this case, the temperature of each roller may be changed individually. The temperature of the baking rollers may be different from one another within the above range.
[0032] Next, the semi-baked yarn is baked at a temperature of 320°C or more and 350°C or less. At this stage, most of the cellulose is decomposed and vaporized, so the PTFE particles dispersed in the cellulose are thermally fused to form fibers, and a PTFE undrawn yarn is obtained. If the baking temperature is lower than 320°C, the PTFE particles in the fiber are not sufficiently fused to each other, and thread breakage occurs frequently during drawing after baking, and the fiber strength is also reduced, which is not preferable. On the other hand, if the baking temperature exceeds 380°C, the fiber cross-sectional shape is deformed, a uniform cross-sectional shape cannot be obtained, and inter-fiber adhesion occurs, which makes it easy for fabric defects in the weaving process and neps in the carding process to occur, and productivity is significantly reduced. Furthermore, PTFE is thermally decomposed, and thread breakage occurs frequently during drawing after baking, and the fiber strength is also reduced, which is not preferable. The temperature of each roller during baking may be changed independently. Also, it can be set without any particular limitation as long as it is within the above range.
[0033] From the viewpoint of producing fine PTFE fibers, when the undrawn yarns derived from the scouring bath or alkaline bath are passed through the calcination process, it is preferable that the total fineness / width of a single or multiple divided yarn bundles is 100 ktex / m or less. If it exceeds 100 ktex / m, the single yarns in the yarn bundle become dense and inter-fiber adhesion occurs, which tends to cause fabric defects in the weaving process and neps in the carding process, resulting in a significant decrease in productivity.
[0034] The undrawn PTFE yarn obtained by baking may be drawn after being wound up once, or may be drawn continuously without being wound up.
[0035] The stretching is preferably performed at a temperature of 300°C to 380°C. More preferably, the temperature is 310°C to 370°C. If the temperature is less than 300°C, stretching breakage occurs frequently, leading to a decrease in yield due to process troubles. If the temperature exceeds 380°C, the PTFE decomposes, leading to a decrease in fiber tensile strength.
[0036] The fibers obtained by the production method of the present invention can be crimped, if necessary, by a conventional crimping method, for example, by using a stuffing box, and then cut to a desired length to produce short PTFE fibers.
[0037] The polytetrafluoroethylene fiber of the present invention may be in the form of either filaments or staples, and may also be in the form of advanced processed products such as cloth, woven or knitted fabric, nonwoven fabric, felt, or mat. EXAMPLES
[0038] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. Various modifications and corrections are possible within the scope of the technical scope of the present invention. The methods for measuring various properties used in the examples are as follows.
[0039] [Measurement and evaluation method] (1) Single fiber size Apply an initial load (a load (g) of 6% of the fineness) to a multifilament sample exactly 1 m long, measure the mass of the sample to the nearest 1 / 10,000 g, and calculate the mass using the following formula: Single fiber fineness (dtex) = sample mass / (sample length x number of holes in spinning nozzle) x 10,000 The average value of three measurements was taken as the single fiber fineness (dtex).
[0040] (2) Coal content After 3 g of PTFE fiber was heat-treated at 300°C for 72 hours in an air atmosphere, the fiber mass change was measured and calculated using the following formula: Carbon content (%) = (fiber mass before heat treatment - fiber mass after heat treatment) / fiber mass before heat treatment × 100 The carbon content (%) was calculated.
[0041] (3) Production stability When the average number of times that yarn bundle breakage occurred in each spinning and drawing process per 100 kg of PTFE fiber produced was less than 10 times / 100 kg production, it was evaluated as "◎", when it was 10 to less than 30 times / 100 kg production, it was evaluated as "○", and when it was 30 times or more / 100 kg production, it was evaluated as "×". Production stability was evaluated as being excellent when it was ◎ or ○.
[0042] (4) Single yarn adhesion The PTFE fiber obtained after the thermal stretching was cut to 6 mm, and 200 mL of an aqueous dispersion of the fiber was prepared using Woopol (Matsumoto Yushi Seiyaku Co., Ltd.) as a dispersant at a dispersant concentration of 0.05% and a fiber amount of 1 g / L. The dispersion was then stirred at 500 rpm for 3 minutes. The aqueous dispersion of the fiber obtained was 118 g / m 2 The PTFE fiber was filtered by suction using a filter paper, and the number of pine needle-like or chip-like fiber bundles that were not separated into individual fibers in the morphology of the PTFE fiber after suction filtration was visually counted as "◎" when it was less than 5 / g, "○" when it was 5 or more but less than 15 / g, and "×" when it was 15 or more / g. A value of ◎ or ○ was judged to indicate excellent single yarn adhesiveness.
[0043] [Example 1] After mixing 46% by mass of viscose (cellulose concentration 9.0 wt%, alkali concentration 6.0 wt%) and 54% of PTFE aqueous dispersion with a concentration of 60%, the mixture was degassed under a reduced pressure of 10 Torr to obtain a spinning mixture with a cellulose / PTFE ratio of 12.8%. The spinning stock solution was wet-spun into a spinning bath solution with a sulfuric acid concentration of 9.0%, a sodium sulfate concentration of 10.0%, and a temperature of 15 ° C. using a round hole die with a hole diameter of 50 μm and a hole length of 50 μm, so that the spinning take-up speed / discharge linear speed was 3.8. The solidified unsintered yarn was then washed with warm water at a temperature of 70 ° C., and then refined by being introduced into an alkali bath containing a caustic soda solution with a concentration of 0.12%, and the acid components were completely removed. Thereafter, the unsintered yarns led out from the alkaline bath were squeezed with nip rollers, and then semi-sintered at a temperature of 320°C while being relaxed by 2% with a total fineness / width of 30 ktex / m for each yarn, and then sintered at a temperature of 345°C. After being wound up once, the yarns were hot-drawn at a ratio of 7.6 times at a temperature of 340°C to obtain PTFE fiber. The obtained PTFE fiber had a single fiber fineness of 0.29 dtex and a carbon content of 2.9%. The average number of times that yarn bundle breakage occurred in each process of spinning and drawing during the production of PTFE fiber was 6 times / 100 kg production, and the single yarn adhesiveness of this PTFE fiber was evaluated to be 3 pieces / g.
[0044] [Example 2] A PTFE fiber was obtained in the same manner as in Example 1, except that the draw ratio in the hot drawing was changed to 11.0 times. The obtained PTFE fiber had a single fiber fineness of 0.18 dtex and a carbon content of 2.9%. The average number of times that yarn bundle breakage occurred in each process of spinning and drawing during the production of the PTFE fiber was 9 times / 100 kg production, and the single yarn adhesiveness of this PTFE fiber was evaluated to be 4 pieces / g.
[0045] [ Reference Example 1 ] PTFE fiber was obtained in the same manner as in Example 1, except that the hole diameter of the discharge hole of the spinneret was changed to 70 μm, the hole length was changed to 70 μm, the spinning take-up speed / discharge linear speed was changed to 1.3, the total fineness / width of each filament in the baking process was changed to 90 ktex / m, and the stretch ratio of the hot drawing was changed to 8.0 times. The obtained PTFE fiber had a single fiber fineness of 1.5 dtex and a carbon content of 3.5%. The average number of times that the filament bundle broke in each process of spinning and drawing during the production of the PTFE fiber was 3 times / 100 kg production, and the single filament adhesiveness of this PTFE fiber was evaluated to be 4 pieces / g.
[0046] [Comparative Example 1] PTFE fiber was obtained in the same manner as in Example 1, except that the calcination temperature was changed to 375°C. The obtained PTFE fiber had a single fiber fineness of 0.29 dtex and a carbon content of 1.8%. The average number of times that yarn bundle breakage occurred in each process of spinning and drawing during the production of the PTFE fiber was 3 times / 100 kg production, and the single fiber adhesiveness of this PTFE fiber was evaluated to be 28 pieces / g.
[0047] [Comparative Example 2] PTFE fiber was obtained in the same manner as in Example 1, except that the semi-calcination temperature was changed to 280°C and the calcination temperature was changed to 310°C. The obtained PTFE fiber had a single fiber fineness of 0.30 dtex and a carbon content of 6.2%. The average number of times that yarn bundle breakage occurred in each process of spinning and drawing during the production of the PTFE fiber was 36 times / 100 kg production, and the single yarn adhesiveness of this PTFE fiber was evaluated to be 2 pieces / g.
[0048] [Comparative Example 3] PTFE fiber was obtained in the same manner as in Example 1, except that the hole diameter of the spinneret discharge hole was changed to 100 μm, the hole length was changed to 100 μm, the spinning take-up speed / discharge linear speed was changed to 2.1, and the total fineness / width of each yarn in the baking process was changed to 100 ktex / m. The obtained PTFE fiber had a single fiber fineness of 2.11 dtex and a carbon content of 3.2%, and is not suitable for use as a high-capture efficiency bag filter. In addition, the average number of times that the yarn bundle broke in each process of spinning and drawing during the production of the PTFE fiber was 21 times / 100 kg production, and the single yarn adhesiveness of this PTFE fiber was evaluated and found to be 3 pieces / g.
[0049] [Comparative Example 4] PTFE fiber was obtained in the same manner as in Example 1, except that the hole length of the discharge hole of the spinneret was changed to 30 μm, the spinning take-up speed / discharge linear speed was changed to 1.3, and the total fineness / width of each yarn in the baking process was changed to 100 ktex / m. The obtained PTFE fiber had a single fiber fineness of 3.29 dtex and a carbon content of 3.4%, and is not suitable for use as a high-capture efficiency bag filter. In addition, the average number of times that the yarn bundle broke in each spinning and drawing process during the production of the PTFE fiber was 11 times / 100 kg production, and the single yarn adhesiveness of this PTFE fiber was evaluated and found to be 2 pieces / g.
[0050] [Table 1]
[0051] The PTFE fibers produced in Examples 1 to 3 and Comparative Examples 1 to 6 were evaluated for the above-mentioned (1) single fiber fineness, (2) carbon content, (3) production stability, and (4) single fiber adhesiveness, and the results are shown in Table 1. As a result, it was clear that the PTFE fibers of the present invention can be made fine while maintaining the properties of fluorine-based fiber materials, such as heat resistance, chemical resistance, electrical properties, and low friction coefficient and excellent sliding properties, and are suitable for use in high-collection-efficiency bag filters, and a method for producing fine PTFE fibers with good productivity can be provided.
Claims
1. A polytetrafluoroethylene fiber characterized in that the single fiber fineness is 0.1 dtex or more and 0.3 dtex or less, and the carbon content is 2.0% or more and 4.0% or less based on the fiber weight.
2. A method for producing the polytetrafluoroethylene fiber described in claim 1, comprising discharging a mixed solution of viscose and an aqueous dispersion of polytetrafluoroethylene from a spinning nozzle having an outlet hole of 40 μm or more and an outlet length of 40 μm or more into a coagulation bath of an aqueous solution having a sulfuric acid concentration of 7% to 13% and a sodium sulfate concentration of 7% to 15% at a take-up speed / exhaust linear speed of 1.5 to 4.0, the total fineness / width when passing through baking rollers being 100 ktex / m or less, and the fiber being semi-baked at a temperature of 200°C to 320°C while providing 1% to 5% relaxation between baking rollers, and then baking at a temperature of 320°C to 350°C, and the fiber being either wound up once or stretched as is.
Citation Information
Patent Citations
Method for producing polytetrafluoroethylene fiber having small fineness and fabric using the same
JP2006207097A
Mixed polytetrafluoroethylene fiber with different fineness fiber, method for producing the same and cloth by using the same
JP2006241606A
Method for producing fluorine-based hollow fiber
JP2010047859A
Fluororesin based fiber and method for producing the same, and textile employing fluororesin based fiber
JP2014080714A
Polytetrafluoroethylene fiber for bag filter, method of manufacturing the same
JP2017082359A