Multilayer film and manufacturing method thereof, and optical film and manufacturing method thereof
A multilayer film structure with specific crystalline polymer layers addresses curling issues in optical film production, enabling thin films with a nonzero and less than one NZ coefficient, enhancing handling and optical properties.
Patent Information
- Application Number
- JP2020218266
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing methods for producing optical films with a nonzero and less than one NZ coefficient often result in films that are thick due to curling issues when contacted with solvents, leading to poor handling properties and inadequate retardation.
A multilayer film structure comprising layers (A) and (B) made of crystalline polymers with specific intrinsic birefringence properties and thickness relationships, allowing for the production of thin optical films with an NZ coefficient greater than 0 and less than 1 through controlled solvent application and drying.
The multilayer film approach enables the production of thin optical films with desired optical properties, improving handling and reducing curling, while maintaining a desired NZ coefficient.
Smart Images

Figure 0007581872000003 
Figure 0007581872000001 
Figure 0007581872000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer film and a method for producing the same, and an optical film and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art A method for producing a resin film is known, which includes a step of stretching a film containing a crystalline resin as a main component, and contacting the resulting stretched film with a hydrocarbon solvent (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-026909 A Summary of the Invention [Problem to be solved by the invention]
[0004] By contacting a film made of a resin containing a crystalline polymer with a solvent, the retardation Rth in the thickness direction of the film can be changed. After changing the retardation Rth in the thickness direction of the film, the film can be stretched to obtain an optical film having an NZ coefficient greater than 0 and less than 1.
[0005] On the other hand, depending on the conditions under which the film is brought into contact with the solvent, the film may curl, etc., and the handling properties of the film may be reduced. For example, when the film is brought into contact with the solvent by immersing the film in the solvent, if the film is thin, curling is likely to occur. Therefore, a film having a certain degree of thickness is usually used. In addition, for example, when the film is brought into contact with the solvent by coating the film with the solvent, a thin film is likely to curl, so a film having a certain thickness is usually used. Therefore, the optical film obtained by stretching the film usually has a large thickness.
[0006] If the amount of the solvent applied is reduced to reduce the amount of the solvent in contact with the film in order to suppress curling, the desired retardation may not be imparted to the resulting film.
[0007] Therefore, there is a need for a multilayer film that can be stretched to obtain an optical film having a thin thickness and an NZ coefficient greater than 0 and less than 1; a method for producing the multilayer film; an optical film having a thin thickness and an NZ coefficient greater than 0 and less than 1; and a method for producing the optical film. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by making the film a multilayer film containing a predetermined layer (A) and layer (B), thereby completing the present invention. That is, the present invention provides the following.
[0009] [1] A layer (A) made of a resin (a) having a positive intrinsic birefringence containing a crystalline polymer (Pa); and a layer (B) made of a resin (b) having a positive intrinsic birefringence and containing a polymer (Pb) having crystallinity, The NZ coefficient Nza of the layer (A) satisfies the following formula (1), The NZ coefficient Nzb of the layer (B) satisfies the following formula (2), A multilayer film, wherein the birefringence Δna of the layer (A) in the thickness direction and the birefringence Δnb of the layer (B) in the thickness direction satisfy the following formula (3): Nza<0 (1) Nzb<0 (2) 1<Δnb / Δna<10 (3) [2] The multilayer film according to [1], wherein the crystalline polymer (Pb) is a polymer containing an alicyclic structure. [3] The multilayer film according to [1] or [2], wherein the layer (A) and the layer (B) are directly connected to each other. [4] The multilayer film according to any one of [1] to [3], wherein the retardation Rtha of the layer (A) in the thickness direction and the retardation Rthb of the layer (B) in the thickness direction satisfy the following formula (4): 1 <Rthb / Rtha≦3···(4) [5] A method for producing the multilayer film according to any one of [1] to [4], A step (1) of preparing a substrate film made of the resin (a); (2) a step of forming a coating layer on at least one of the two surfaces of the base film by coating a resin solution containing the resin (b) and a solvent; (3) drying the coating layer to form a layer (B) and obtain the multilayer film; A method for producing a multilayer film comprising the steps of: [6] A method for producing an optical film, comprising a step of stretching the multilayer film according to any one of [1] to [4] to obtain an optical film. [7] An optical film which is a stretched product of the multilayer film according to any one of [1] to [4]. Effect of the Invention
[0010] According to the present invention, it is possible to provide a multilayer film that can be stretched to obtain an optical film having a small thickness and an NZ coefficient greater than 0 and less than 1; a method for producing the multilayer film; an optical film having a small thickness and an NZ coefficient greater than 0 and less than 1; and a method for producing the optical film. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a multilayer film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0013] In the following description, a "long" film refers to a film having a length of 5 times or more its width, preferably 10 times or more its width, specifically a film having a length sufficient to be wound into a roll for storage or transportation. There is no particular upper limit to the length of the film, and it may be, for example, 100,000 times or less its width.
[0014] In the following description, unless otherwise specified, the oblique direction of a long film refers to an in-plane direction of the film that is neither parallel nor perpendicular to the longitudinal direction of the film.
[0015] In the following description, unless otherwise specified, a material with positive intrinsic birefringence means a material whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Also, a material with negative intrinsic birefringence means a material whose refractive index in the stretching direction is smaller than that in the direction perpendicular thereto. The value of intrinsic birefringence can be calculated from the dielectric constant distribution.
[0016] In the following description, the in-plane retardation Re of a layer is a value expressed by Re=(nx-ny)×d unless otherwise specified. Furthermore, the retardation Rth in the thickness direction of a layer is a value expressed by Rth=[{(nx+ny) / 2}-nz]×d unless otherwise specified. Furthermore, the NZ coefficient of a layer is a value expressed by (nx-nz) / (nx-ny) unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the layer and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the layer. d represents the thickness of the layer. The measurement wavelength is 590 nm unless otherwise specified. The NZ coefficient can be calculated from the formula NZ coefficient=Rth / Re+0.5.
[0017] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effect of the present invention, for example, within a range of ±3°, ±2°, or ±1°.
[0018] In the following description, the longitudinal direction of a long film is usually parallel to the film transport direction in the production line. The MD direction (machine direction) is the film transport direction in the production line, and is usually parallel to the longitudinal direction of the long film. The TD direction (transverse direction) is a direction parallel to the film surface, perpendicular to the MD direction, and usually parallel to the width direction of the long film.
[0019] In the following description, a "polymer having crystallinity" refers to a polymer having a melting point Tm. In other words, a "polymer having crystallinity" refers to a polymer whose melting point can be observed by a differential scanning calorimeter (DSC). In the following description, a polymer having crystallinity may be referred to as a "crystalline polymer". Furthermore, a resin containing a crystalline polymer may be referred to as a "crystalline resin". This crystalline resin is preferably a thermoplastic resin.
[0020] [1. Overview of multilayer film] A multilayer film according to one embodiment of the present invention comprises a layer (A) made of a resin (a) containing a crystalline polymer (Pa) and having a positive intrinsic birefringence, and a layer (B) made of a resin (b) containing a crystalline polymer (Pb) and having a positive intrinsic birefringence, wherein the NZ coefficient Nza of the layer (A) satisfies the following formula (1), the NZ coefficient Nzb of the layer (B) satisfies the following formula (2), and the birefringence Δna in the thickness direction of the layer (A) and the birefringence Δnb in the thickness direction of the layer (B) satisfy the following formula (3). Nza<0 (1) Nzb<0 (2) 1<Δnb / Δna<10 (3)
[0021] When the multilayer film contains layer (A) and layer (B) and satisfies the above formulas (1) to (3), an optical film that is thin when stretched and has an NZ coefficient greater than 0 and less than 1 can be produced from the multilayer film.
[0022] In one embodiment, the multilayer film is a multilayer film that can be obtained by a production method including steps (1) to (3) described below.
[0023] [1.1. Multilayer film structure] The structure of the multilayer film according to this embodiment will be described below with reference to the drawings. FIG. 1 is a cross-sectional view that illustrates a multilayer film according to one embodiment of the present invention. The multilayer film 100 includes a layer 110 as layer (A) and a layer 120 as layer (B). The layer 110 has a first surface 110U and a second surface 110D as major surfaces. The layer 120 is provided directly on the first surface 110U of the layer 110. In other words, there is no other layer between the layer 110 and the layer 120, and the first surface 110U of the layer 110 is in contact with the major surface of the layer 120 without any other layer therebetween.
[0024] In another embodiment, the multilayer film may include a second layer (B) in addition to the layer (A) and the first layer (B). In this embodiment, the first layer (B) is provided directly on the first surface, which is the main surface, of the layer (A), and the second layer (B) is provided directly on the second surface, which is the main surface, of the layer (A). Both the first layer (B) and the second layer (B) satisfy the above formulas (1) to (3).
[0025] [1.2. Multilayer film materials] The materials of the layer (A) and the layer (B) included in the multilayer film of the present embodiment will be described below. The description of the layer (B) can be applied to both the first layer (B) and the second layer (B).
[0026] (Layer(A)) The layer (A) is made of a resin (a) containing a crystalline polymer (Pa) and having a positive intrinsic birefringence, and contains and is formed from the resin (a).
[0027] The polymer (Pa) having crystallinity (hereinafter also referred to as crystalline polymer (Pa)) may be, for example, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN); polyolefin such as polyethylene (PE) or polypropylene (PP); and the like, but is not particularly limited, and preferably contains an alicyclic structure. By using a crystalline polymer (Pa) containing an alicyclic structure, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability and light weight of the multilayer film can be improved. The polymer containing an alicyclic structure refers to a polymer having an alicyclic structure in the molecule. Such a polymer containing an alicyclic structure may be, for example, a polymer obtainable by a polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof.
[0028] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, a cycloalkane structure is preferred because it is easy to obtain a multilayer film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.
[0029] In the crystalline polymer (Pa) containing an alicyclic structure, the ratio of the structural unit having an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. By increasing the ratio of the structural unit having an alicyclic structure as described above, heat resistance can be improved. The ratio of the structural unit having an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the crystalline polymer (Pa) containing an alicyclic structure, the remainder other than the structural unit having an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.
[0030] Examples of the crystalline polymer (Pa) containing an alicyclic structure include the following polymers (α) to (δ). Among these, polymer (β) is preferred because it is easy to obtain an optical film having excellent heat resistance. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.
[0031] Specifically, the crystalline polymer (Pa) containing an alicyclic structure is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenated product having crystallinity. Among them, a dicyclopentadiene ring-opening polymer hydrogenated product having crystallinity is particularly preferred. Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.
[0032] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.
[0033] As the polymer (α) to polymer (δ), polymers obtained by the production method disclosed in WO 2018 / 062067 can be used.
[0034] The melting point Tm of the crystalline polymer (Pa) is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. By using a crystalline polymer (Pa) having such a melting point Tm, a multilayer film having an even better balance between formability and heat resistance can be obtained.
[0035] Usually, the crystalline polymer (Pa) has a glass transition temperature Tg. The specific glass transition temperature Tg of the crystalline polymer (Pa) is not particularly limited, but is usually 85°C or higher and usually 170°C or lower.
[0036] The glass transition temperature Tg and melting point Tm of a polymer can be measured by the following method. First, the polymer is melted by heating, and the melted polymer is quenched with dry ice. Then, using this polymer as a test specimen, the glass transition temperature Tg and melting point Tm of the polymer can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min (heating mode).
[0037] The weight average molecular weight (Mw) of the crystalline polymer (Pa) is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. The crystalline polymer (Pa) having such a weight average molecular weight has an excellent balance between moldability and heat resistance.
[0038] The molecular weight distribution (Mw / Mn) of the crystalline polymer (Pa) is preferably 1.0 or more, more preferably 1.5 or more, and preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. The crystalline polymer (Pa) having such a molecular weight distribution has excellent moldability.
[0039] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.
[0040] The crystalline polymer (Pa) may be used alone or in combination of two or more kinds in any ratio.
[0041] The proportion of the crystalline polymer (Pa) in the crystalline resin (a) is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the crystalline polymer (Pa) is equal to or more than the lower limit of the above range, the heat resistance of the multilayer film can be improved. The upper limit of the proportion of the crystalline polymer (Pa) can be 100% by weight or less.
[0042] The crystalline resin (a) may contain optional components in addition to the crystalline polymer (Pa). Examples of the optional components include antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, and benzimidazoline derivatives). Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than the crystalline polymer (Pa), such as soft polymers. One type of optional component may be used alone, or two or more types may be used in any ratio.
[0043] (Layer (B)) The layer (B) is made of a resin (b) containing a crystalline polymer (Pb) and having a positive intrinsic birefringence, and contains and is formed from the resin (b). The polymer (Pb) having crystallinity (hereinafter also referred to as crystalline polymer (Pb)) may be, for example, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN); polyolefin such as polyethylene (PE) or polypropylene (PP); and is not particularly limited, but preferably contains an alicyclic structure. By using a crystalline polymer (Pb) containing an alicyclic structure, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability, and light weight of the multilayer film can be improved.
[0044] The crystalline polymer (Pb) containing an alicyclic structure may be the same as the crystalline polymers listed as the examples and preferred examples of the crystalline polymer (Pa) having an alicyclic structure. This allows the crystalline polymer (Pb) to have the same advantages as the crystalline polymer (Pa).
[0045] The melting point Tm and glass transition temperature Tg of the crystalline polymer (Pb) may be in the same range as the preferred melting point range and preferred glass transition temperature range of the crystalline polymer (Pa), respectively, so that the crystalline polymer (Pb) can obtain the same advantages as the crystalline polymer (Pa).
[0046] The weight average molecular weight (Mw) of the crystalline polymer (Pb) may be in the same range as the preferred weight average molecular weight (Mw) range of the crystalline polymer (Pa). This allows the crystalline polymer (Pb) to obtain the same advantages as the crystalline polymer (Pa).
[0047] The molecular weight distribution (Mw / Mn) of the crystalline polymer (Pb) can be in the same range as the preferred molecular weight distribution (Mw / Mn) range of the crystalline polymer (Pa). This allows the crystalline polymer (Pb) to obtain the same advantages as the crystalline polymer (Pa).
[0048] The crystalline polymer (Pb) may be used alone or in combination of two or more kinds in any ratio.
[0049] The ratio of the crystalline polymer (Pb) in the crystalline resin (b) may be in the same range as the preferred ratio range of the crystalline polymer (Pa) in the crystalline resin (a), thereby allowing the crystalline resin (b) to obtain the same advantages as the crystalline resin (a).
[0050] The crystalline resin (b) may contain optional components in addition to the crystalline polymer (Pb). Examples of the optional components include the same examples as the optional components that may be contained in the crystalline resin (a). The optional components may be used alone or in combination of two or more kinds in any ratio.
[0051] The crystalline resin (a) and the crystalline resin (b) may be the same resin or different resins.
[0052] [1.3. Optical properties of multilayer films] As described above, the multilayer film of the present embodiment satisfies the above formulas (1) to (3). The NZ coefficient Nza of the layer (A) is usually less than 0, preferably −5 or less, more preferably −10 or less, and is preferably −200 or more, more preferably −100 or more.
[0053] The NZ coefficient Nza can be adjusted by adjusting the manufacturing conditions of the multilayer film, such as adjusting the in-plane retardation of the base film used in the manufacture of the multilayer film, adjusting the thickness of the layer (coating layer) of the resin solution containing resin (b) formed on the base film, etc. Usually, NZa can be made smaller by increasing the thickness of the coating layer formed on the base film.
[0054] The NZ coefficient Nzb of the layer (B) is usually less than 0, preferably −10 or less, more preferably −20 or less, and preferably −200 or more, more preferably −100 or more.
[0055] The NZ coefficient Nzb can be adjusted by adjusting the manufacturing conditions of the multilayer film, for example, by adjusting the thickness of the coating layer. Usually, NZb can be made smaller by increasing the thickness of the coating layer.
[0056] The ratio (Δnb / Δna) of the birefringence Δnb in the thickness direction of layer (B) to the birefringence Δna in the thickness direction of layer (A) satisfies the above formula (3) and is usually greater than 1, preferably greater than 2, more preferably greater than 3, and is usually less than 10, preferably less than 9.5, more preferably less than 9.
[0057] By setting the NZ coefficient Nza of layer (A), the NZ coefficient Nzb of layer (B), and the ratio (Δnb / Δna) within the above ranges, the optical film obtained by stretching the multilayer film can have an NZ coefficient greater than 0 and less than 1.
[0058] The value of Δnb / Δna can be adjusted, for example, by adjusting the value of Δna. Usually, the value of Δna can be made smaller by increasing the thickness of the coating layer.
[0059] The in-plane retardation Re, retardation in the thickness direction Rth, and birefringence Δn in the thickness direction of each of the layer (A) and layer (B) according to this embodiment can be determined, for example, as follows. For the entire multilayer film, the in-plane retardation Re0, the retardation in the thickness direction Rth0, and the thickness d are measured. Layer (B) is scraped off from the surface of the multilayer film, leaving only layer (A). The thickness of the portion to be scraped off from the multilayer film can be determined by roughly estimating the thickness db of layer (B) from the concentration of resin (b) in the resin solution used to form layer (B) and the thickness of the layer of the resin solution (coating layer). Next, the in-plane retardation Rea, the retardation in the thickness direction Rtha, and the thickness da of the layer (A) are measured. The in-plane retardation Reb and the retardation in the thickness direction Rthb of the layer (B) are calculated according to the following formula. Reb=Re0-Rea Rthb = Rth0 - Rtha
[0060] The NZ coefficient of each layer can be calculated from the in-plane retardation Re and the retardation in the thickness direction Rth of each layer according to the formula: NZ=Rth / Re+0.5.
[0061] From the retardation Rth of each layer in the thickness direction thus obtained, the birefringence Δn of each layer in the thickness direction is calculated according to the following formula. Δna=Rtha / da Δnb=Rthb / db
[0062] The birefringence Δna in the thickness direction of the layer (A) is preferably −0.01 or more, more preferably −0.005 or more, and preferably 0 or less, more preferably −0.0001 or less, and further preferably −0.001 or less. By having the birefringence Δna within the above range, the value of Δnb / Δna can be more easily adjusted to a desired range, and the layer (A) can be made thinner.
[0063] The retardation Rtha in the thickness direction of the layer (A) is preferably −100 nm or more, more preferably −90 nm or more, even more preferably −80 nm or more, and preferably −10 nm or less, more preferably −15 nm or less, even more preferably −20 nm or less.
[0064] It is preferable that the retardation Rtha in the thickness direction of the layer (A) and the retardation Rthb in the thickness direction of the layer (B) satisfy the following formula (4). 1 <Rthb / Rtha≦3···(4) This allows the thickness of the optical film obtained by stretching the multilayer film to be thinner.
[0065] The value of Rthb / Rtha is more preferably 1.3 or more, further preferably 1.5 or more, and more preferably 2.8 or less, further preferably 2.5 or less.
[0066] [1.4. Thickness of multi-layer film] The thickness of the multilayer film is preferably 25 μm or less, more preferably 23 μm or less, even more preferably 20 μm or less, and is preferably 10 μm or more. This makes it possible to easily produce a thin optical film from the multilayer film.
[0067] [2. Multilayer film manufacturing method] The multilayer film of the present embodiment can be produced by any method, for example, the multilayer film of the present embodiment can be produced by a production method including the following steps (1) to (3). Step (1): A step of preparing a substrate film made of the resin (a). Step (2): A step of forming a coating layer on at least one of the two surfaces of the base film by applying a resin solution containing the resin (b) and a solvent. Step (3): A step of drying the coating layer to form layer (B) and obtaining the multilayer film. Steps (1), (2), and (3) are usually carried out in this order. The manufacturing method of this embodiment may include any optional steps in addition to steps (1) to (3).
[0068] [2.1. Process (1)] In step (1), a substrate film made of resin (a) is prepared. The substrate film prepared is made of the same resin as the resin (a) contained in layer (A), contains the resin, and is formed from the resin.
[0069] However, the crystallinity of the crystalline polymer (Pa) contained in the substrate film is preferably small. The specific crystallinity is preferably less than 10%, more preferably less than 5%, and particularly preferably less than 3%. Since the crystallinity of the crystalline polymer (Pa) contained in the substrate film is small, many molecules of the crystalline polymer (Pa) contained in the substrate film can be oriented in the thickness direction in step (2), and therefore the retardation Rth in the thickness direction of the multilayer film can be adjusted in a wide range.
[0070] The substrate film preferably has a small content of organic solvent, and more preferably does not contain organic solvent. The ratio of the organic solvent contained in the substrate film (solvent content) to 100% by weight of the substrate film is preferably 1% or less, more preferably 0.5% or less, particularly preferably 0.1% or less, and ideally 0.0%. Since the amount of organic solvent contained in the substrate film is small, many molecules of the crystalline polymer (Pa) can be oriented in the thickness direction in step (2), and therefore the retardation Rth in the thickness direction of the multilayer film can be adjusted in a wide range.
[0071] The solvent content of the substrate film can be measured by density.
[0072] The base film may be a sheet-like film, but is preferably a long film. By using a long base film, the multilayer film can be continuously produced, and the productivity of the multilayer film can be effectively improved.
[0073] The substrate film is preferably a film having optical isotropy. That is, the substrate film is preferably a film having a small birefringence (Re / d) in the in-plane direction and a small absolute value of birefringence |Rth / d| in the thickness direction. Having optical isotropy means that the orientation of the molecules of the crystalline polymer (Pa) contained in the substrate film is low and is substantially in a non-oriented state. When such an optically isotropic substrate film is used, precise control of the optical properties of the substrate film is not required, and therefore precise control of the orientation of the molecules of the crystalline polymer (Pa) is not required, so that the manufacturing method of the multilayer film can be simplified.
[0074] The substrate film can be a film produced by any production method. As the production method of the substrate film, a resin molding method such as injection molding, extrusion molding, press molding, inflation molding, blow molding, calendar molding, cast molding, compression molding, etc. is preferable because it can obtain a substrate film that does not contain an organic solvent. Among these, extrusion molding is preferable because it is easy to control the thickness.
[0075] The manufacturing conditions in the extrusion molding method are preferably as follows. The cylinder temperature (molten resin temperature) is preferably Tm or higher, more preferably "Tm+20°C" or higher, and preferably "Tm+100°C" or lower, more preferably "Tm+50°C" or lower. The cooling body that the molten resin extruded into a film first comes into contact with is not particularly limited, but a cast roll is usually used. The cast roll temperature is preferably "Tg-50°C" or higher, preferably "Tg+70°C" or lower, more preferably "Tg+40°C" or lower. Furthermore, the cooling roll temperature is preferably "Tg-70°C" or higher, more preferably "Tg-50°C" or higher, and preferably "Tg+60°C" or lower, more preferably "Tg+30°C" or lower. When the substrate film is manufactured under such conditions, a substrate film having a thickness of 1 μm to 1 mm can be easily manufactured. Here, "Tm" represents the melting point of the crystalline polymer (Pa), and "Tg" represents the glass transition temperature of the crystalline polymer (Pa).
[0076] The in-plane retardation Re1 of the base film is preferably 10 nm or less, more preferably 8 nm or less, and further preferably 5 nm or less, and is usually 0 nm or more, and may be 0 nm or 1 nm or more.
[0077] The absolute value |Rth1| of the retardation Rth1 in the thickness direction of the base film is preferably 15 nm or less, more preferably 10 nm or less, and even more preferably 8 nm or less, and is usually 0 nm or more, and may be 0 nm or 1 nm or more.
[0078] The thickness of the base film is preferably 8 μm or more, more preferably 10 μm or more, and even more preferably 13 μm or more, and is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less. By having the thickness of the base film within the above range, the obtained multilayer film can be made thin, and curling of the multilayer film can be reduced, thereby improving the handleability of the multilayer film.
[0079] [2.2. Process (2)] In step (2), a resin solution containing the resin (b) and a solvent is applied to at least one of the two surfaces of a substrate film to form a coating layer. Step (2) generally changes the birefringence in the thickness direction of the substrate film to obtain layer (A) from the substrate film, and step (2) also reduces the thickness of the resulting multilayer film and provides the multilayer film with desired optical properties. Furthermore, by applying a resin solution onto the surface of a substrate film to form a coating layer, a multilayer film in which Layer (A) and Layer (B) are in direct contact with each other can be produced.
[0080] The solvent contained in the resin solution is usually an organic solvent. Examples of the organic solvent include solvents that are difficult to dissolve the crystalline polymer (Pa) contained in the base film, but can penetrate into the base film, such as hydrocarbon solvents such as toluene, limonene, and decalin; and carbon disulfide. The type of organic solvent may be one type or two or more types.
[0081] By applying a resin solution containing an organic solvent onto the surface of the base film, the organic solvent comes into contact with the surface of the base film. This changes the birefringence in the thickness direction of the base film, and the layer (A) is formed from the base film. The reason why the birefringence in the thickness direction of the base film is changed by bringing the organic solvent into contact with the surface of the base film, and the layer (A) is formed, is presumed to be as follows, but is not intended to limit the present invention.
[0082] When the substrate film made of the crystalline resin (a) is brought into contact with an organic solvent in step (2), the organic solvent penetrates into the substrate film. The action of the penetrated organic solvent causes micro-Brownian motion in the molecules of the crystalline polymer (Pa) in the film, and the molecular chains of the film are oriented.
[0083] The surface area of the base film is large on the main surfaces, the front surface and the back surface. Therefore, the penetration speed of the organic solvent is high in the thickness direction through the front surface or the back surface. Then, the orientation of the molecules of the crystalline polymer (Pa) can proceed so that the molecules of the polymer are oriented in the thickness direction.
[0084] In this way, the molecules of the crystalline polymer (Pa) are oriented in the thickness direction, and thus the birefringence in the thickness direction of the base film changes. Thus, through step (2), a layer (A) can be obtained from the base film.
[0085] In addition, in step (2), when a resin solution is applied onto the surface of the substrate film to form a coating layer, it is believed that a flow of the solvent occurs from the coating layer toward the main surface of the substrate film. As a result, it is believed that the molecules of the crystalline polymer (Pb) contained in the crystalline resin (b) in the coating layer are oriented in the thickness direction in the coating layer, and as a result, it is believed that the layer (B) can be obtained from the coating layer. However, the above speculation does not limit the present invention.
[0086] In step (2), the resin solution may be applied to only one of the two surfaces of the base film to form a coating layer, or the resin solution may be applied to both surfaces to form coating layers on both sides of the base film.
[0087] The coating method used in step (2) is preferably a method capable of controlling the thickness of the coating layer formed on the surface of the substrate film by coating. Examples of the coating method include wire bar coating, spraying, roll coating, gravure coating, die coating, curtain coating, slide coating, and extrusion coating, with wire bar coating and die coating being preferred.
[0088] The thickness of the coating layer formed in step (2) is the thickness immediately after coating. The thickness of the coating layer can be adjusted, for example, by adjusting the settings of the coating device (e.g., the type of wire bar, the flow rate of the resin solution from the coating device, and the conveying speed of the base film).
[0089] The thickness of the coating layer is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 8 μm or more, and is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less. By keeping the thickness of the coating layer within the above range, the handleability of the multilayer film can be improved. Here, the thickness of the coating layer means the total thickness of the two coating layers formed when coating layers are formed on both sides of the substrate film.
[0090] The concentration of resin (b) in the resin solution is preferably a concentration at which resin (b) does not precipitate, and is preferably 5% by weight or more, more preferably 10% by weight or more, and preferably 40% by weight or less, more preferably 35% by weight or less, based on 100% by weight of the resin solution.
[0091] The temperature of the resin solution to be applied may be any temperature within the range of the boiling point of the solvent contained in the resin solution or less, and is preferably a temperature at which the resin (b) can be dissolved in the organic solvent. The temperature of the resin solution may be, for example, 130°C to 150°C.
[0092] [2.3. Process (3)] In step (3), the coating layer is dried to form a layer (B) to obtain a multilayer film including the layers (A) and (B). The solvent can be removed from the coating layer by step (3).
[0093] As the drying method, any method can be adopted depending on the boiling point of the solvent used, and examples of the drying method include natural drying, heat drying, reduced pressure drying, reduced pressure heat drying, etc.
[0094] [2.4. Optional Process] According to the above-mentioned manufacturing method, a long multilayer film can be manufactured using a long base film. In addition to steps (1) to (3), the manufacturing method of the multilayer film may include a step of winding the long multilayer film thus manufactured into a roll. Furthermore, the manufacturing method of the multilayer film may include a step of cutting the long multilayer film into a desired shape.
[0095] [3. Uses of multi-layer films] By stretching the multilayer film of this embodiment, an optical film having a small thickness and an NZ coefficient greater than 0 and less than 1 can be obtained. The optical film can be provided, for example, in a display device. In this case, the optical film can improve the display quality, such as the viewing angle, contrast, and image quality, of an image displayed on the display device. Therefore, the multilayer film of this embodiment can be preferably used to produce an optical film.
[0096] [4. Optical films] As described above, by stretching the multilayer film, an optical film can be obtained as a stretched product of the multilayer film. By stretching the multilayer film, an optical film having a small thickness and an NZ coefficient greater than 0 and less than 1 can be obtained.
[0097] The thickness dc of the optical film is preferably 10 μm or more, more preferably 13 μm or more, and is preferably 25 μm or less, more preferably 20 μm or less.
[0098] In one embodiment, the optical film has an in-plane retardation that can function as a half wave plate. The in-plane retardation Rec of the optical film is preferably 240 nm or more, more preferably 250 nm or more, and preferably 300 nm or less, more preferably 290 nm or less.
[0099] The NZ coefficient Nzc of the optical film is preferably greater than 0, more preferably 0.2 or more, even more preferably 0.3 or more, and is preferably less than 1, more preferably 0.8 or less, even more preferably 0.7 or less.
[0100] The optical film preferably has high transparency. The specific total light transmittance of the optical film is preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more. The total light transmittance of the optical film can be measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrometer.
[0101] [5. Manufacturing method of optical film] The method for producing an optical film according to one embodiment of the present invention includes a step of stretching the multilayer film to obtain an optical film. Hereinafter, the step of stretching the multilayer film to obtain an optical film is also referred to as step (4). The multilayer film may be produced by any method, but is preferably a multilayer film produced by a production method including the steps (1) to (3) described above. Therefore, the method for producing an optical film preferably includes the steps (1) to (3) and step (4). Steps (1), (2), (3), and (4) are usually performed in this order. The method for producing a multilayer film may include any step in addition to the step (4), or may include any step in addition to the steps (1) to (4).
[0102] [5.1. Process (4)] In step (4), the multilayer film is stretched to obtain an optical film. By stretching the multilayer film, the molecules of the crystalline polymer contained in layers (A) and (B) of the multilayer film can be oriented in a direction corresponding to the stretching direction.
[0103] There is no limitation on the stretching direction, and examples thereof include the longitudinal direction, the width direction, and the oblique direction. Here, the oblique direction refers to a direction perpendicular to the thickness direction, and is neither parallel nor perpendicular to the width direction. The stretching direction may be one direction or two or more directions. Thus, examples of the stretching method include uniaxial stretching methods such as a method of uniaxially stretching a resin film in the longitudinal direction (longitudinal uniaxial stretching method) and a method of uniaxially stretching a resin film in the width direction (transverse uniaxial stretching method); biaxial stretching methods such as a simultaneous biaxial stretching method in which a resin film is stretched in the longitudinal direction and simultaneously stretched in the width direction, and a sequential biaxial stretching method in which a resin film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction; and a method of stretching a resin film in an oblique direction (oblique stretching method). Other examples of the uniaxial stretching method include a fixed uniaxial stretching method in which the film is stretched with both ends fixed, and a free uniaxial stretching method in which the film is stretched without both ends fixed.
[0104] From the viewpoint of easily imparting a desired NZ coefficient to the optical film by stretching, the stretching in step (4) is preferably a uniaxial stretching method, more preferably a free uniaxial stretching method.
[0105] The stretching ratio is preferably 1 or more, more preferably 1.01 or more, and is preferably 1.5 or less, more preferably 1.4 or less. It is desirable to appropriately set the specific stretching ratio depending on factors such as the optical properties, thickness, and strength of the multilayer film to be stretched. When the stretching ratio is equal to or greater than the lower limit of the above range, the birefringence can be significantly changed by stretching, whereas when the stretching ratio is equal to or less than the upper limit of the above range, the direction of the slow axis can be easily controlled and breakage of the film can be effectively suppressed.
[0106] The stretching temperature is preferably "Tg+5°C" or higher, more preferably "Tg+10°C" or higher, and preferably "Tg+100°C" or lower, more preferably "Tg+90°C" or lower. Here, "Tg" represents the glass transition temperature of the crystalline polymer (Pa). When the stretching temperature is equal to or higher than the lower limit of the above range, the multilayer film can be sufficiently softened to perform uniform stretching. When the stretching temperature is equal to or lower than the upper limit of the above range, the hardening of the multilayer film due to the progress of crystallization of the crystalline polymer can be suppressed, so that the stretching can be performed smoothly. In addition, the birefringence can be significantly changed by stretching. Furthermore, usually, the haze of the optical film obtained after stretching can be reduced to increase the transparency. Step (4) may further include any one of the following steps in addition to the step of stretching the multilayer film (referred to as step (4b)). Step (4a): Preheating the multilayer film. Step (4c): Heat treating the multilayer film. Step (4d): Cooling the stretched multilayer film.
[0107] When step (4) includes step (4a), step (4a) is usually carried out before step (4b). When step (4) includes step (4c), step (4c) is usually carried out after step (4b). When the step (4) includes the step (4d), the step (4d) is usually carried out after the steps (4a) to (4c).
[0108] The heat treatment can promote crystallization of the crystalline polymer contained in the stretched multilayer film, and thus the heat resistance of the optical film can be improved by the step (4c).
[0109] The heat treatment temperature is usually equal to or higher than the glass transition temperature Tg of the crystalline polymer (Pa) and equal to or lower than the melting point Tm of the crystalline polymer (Pa). More specifically, the heat treatment temperature is preferably equal to or higher than Tg°C, more preferably equal to or higher than Tg+10°C, and is preferably equal to or lower than Tm-20°C, more preferably equal to or lower than Tm-40°C. Within the above temperature range, the crystallization of the crystalline polymer can be rapidly promoted while suppressing cloudiness due to the progress of crystallization.
[0110] The treatment time of the heat treatment is preferably 1 second or more, more preferably 5 seconds or more, and is preferably 30 minutes or less, more preferably 15 minutes or less.
[0111] The preheating temperature in step (4a) is usually the same as the stretching temperature in step (4b), but may be different. The preheating temperature is preferably T1-10°C or higher, more preferably T1-5°C or higher, and preferably T1+5°C or lower, more preferably T1+2°C or lower, relative to the stretching temperature T1. The preheating time is optional, and may be preferably 1 second or more, more preferably 5 seconds or more, and may be preferably 60 seconds or less, more preferably 30 seconds or less.
[0112] The cooling temperature in step (4d) is set to be lower than the heating temperature in the step performed before step (4d). The cooling time is optional, and may be preferably 1 second or more, more preferably 5 seconds or more, and may be preferably 30 seconds or less, more preferably 20 seconds or less. The optical film after step (4) may contain residual stress. Therefore, the method for producing an optical film may include, for example, a step of performing a relaxation treatment in which the stretched film is thermally shrunk to remove the residual stress. In the relaxation treatment, the residual stress can usually be removed by causing the stretched film to thermally shrink in an appropriate temperature range while maintaining the film flat.
[0113] By using a long multilayer film, a long optical film can be produced. The method for producing an optical film may include a step of winding the long optical film thus produced into a roll, and may further include a step of cutting the long optical film into a desired shape. EXAMPLES
[0114] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.
[0115] In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature and pressure unless otherwise specified.
[0116] (Method of measuring weight average molecular weight Mw and number average molecular weight Mn of polymer) The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.
[0117] (Method for measuring hydrogenation rate of polymer) The hydrogenation rate of the polymer was measured using orthodichlorobenzene-d4 as a solvent at 145°C. 1 Measurements were performed by H-NMR.
[0118] (Method of measuring glass transition temperature Tg and melting point Tm) The glass transition temperature Tg and melting point Tm of the polymer were measured as follows. First, the polymer was melted by heating, and the melted polymer was quenched with dry ice. Then, the glass transition temperature Tg and melting point Tm of the polymer were measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode) using the polymer as a test specimen.
[0119] (Check the sign of the intrinsic birefringence) The sign of the intrinsic birefringence of the resin to be measured (crystalline resin A or crystalline resin B) was confirmed according to the following procedure. The resin to be confirmed was molded using a hot melt extrusion film molding machine equipped with a T-die to obtain a long resin film (thickness 39 μm) with a width of approximately 400 mm. The operating conditions of the film forming machine were as follows: Barrel temperature setting: 280℃~300℃ Die temperature = 270℃ Cast roll temperature = 80℃
[0120] The obtained resin film was cut into a size of 50 mm x 150 mm to obtain a film piece. The film piece was freely uniaxially stretched using a tensile tester equipped with a thermo-hygrostat (Instron "5564" model) as a measuring device. The stretching temperature was (Tg+15°C of the resin forming the film) and the stretching speed was 1.5 times / min. The slow axis direction of the stretched film piece was then determined using an "AxoScan OPMF-1" manufactured by AXOMETRICS. When the stretching direction and the slow axis direction were parallel, the inherent birefringence of the resin constituting the film piece was deemed to be positive, and when the stretching direction and the slow axis direction were perpendicular, the inherent birefringence of the resin constituting the film piece was deemed to be negative.
[0121] (Method for measuring the ratio of racemo-dyads in polymers) The ratio of racemo-dyads in the polymer was measured as follows. The ratio of the racemo-dyads in the polymer was measured by applying the inverse-gated decoupling method at 200°C using orthodichlorobenzene-D4 as a solvent. 13 C-NMR measurements were performed. 13In the C-NMR measurement, a signal at 43.35 ppm from the meso dyad and a signal at 43.43 ppm from the racemo dyad were identified, with the peak at 127.5 ppm from orthodichlorobenzene-d4 as the reference shift. The ratio of the racemo dyads in the polymer was calculated based on the intensity ratio of these signals.
[0122] (Method of measuring film thickness) The thickness of the film or layer was measured using a contact thickness gauge (Mitsutoyo Co., Ltd., Code No. 543-390).
[0123] (Methods for measuring Re, Rth, NZ coefficient, and thickness direction birefringence Δn) The in-plane retardation Re and the retardation Rth in the thickness direction of the film or layer were measured with an "AxoScan OPMF-1" manufactured by AXOMETRICS, Inc. The measurement was performed at a wavelength of 590 nm. Furthermore, the NZ coefficient of the film or layer was calculated according to the following formula. NZ=Rth / Re+0.5 The birefringence Δn of the film or layer in the thickness direction was calculated by the following formula. Δn=Rth(nm) / d(nm)
[0124] Samples of layer (A) in the multilayer film for measuring these optical properties were prepared as follows. While the surface of the multilayer film was wetted with water, layer (B) on the surface was scraped off using sandpaper (No. 4000, No. 8000, and No. 15000) to leave only layer (A). The thickness of the portion to be scraped off from the multilayer film (i.e., the thickness of the portion of layer (B)) was estimated based on the concentration Cb (33%) of resin (b) in the coating liquid used to form layer (B) and the thickness of the coating layer (12 μm), assuming that the thickness of layer (B) obtained after drying the coating layer would be Cb% (33%) of the thickness of the coating layer. For the layer (A) thus obtained, the in-plane retardation Rea, the retardation in the thickness direction Rtha, the NZ coefficient Nza, and the birefringence Δna in the thickness direction were measured.
[0125] The in-plane retardation Reb, retardation in the thickness direction Rthb, and NZ coefficient Nz of layer (B) in the multilayer film were calculated according to the following formulas. Reb=Re0-Rea Rthb = Rth0 - Rtha NZb=Rthb / Reb+0.5
[0126] [Production Example 1. Production of Crystalline Resin A] A metallic pressure-resistant reactor was thoroughly dried and then purged with nitrogen. 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene were added to the metallic pressure-resistant reactor and heated to 53°C.
[0127] 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex was dissolved in 0.70 parts of toluene to prepare a solution. 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution was added to this solution and stirred for 10 minutes to prepare a catalyst solution. This catalyst solution was added to a pressure-resistant reactor to start a ring-opening polymerization reaction. The reaction was then continued for 4 hours while maintaining the temperature at 53°C to obtain a solution of a ring-opened polymer of dicyclopentadiene. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.
[0128] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").
[0129] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.
[0130] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated product of a crystalline ring-opening polymer of dicyclopentadiene. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 93°C, the melting point (Tm) was 267°C, and the ratio of racemo-dyads was 89%.
[0131] 100 parts of the obtained hydrogenated ring-opening polymer of dicyclopentadiene was mixed with 1.1 parts of an antioxidant (tetrakis [methylene-3- (3', 5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.), and then the mixture was put into a twin-screw extruder (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.) equipped with four die holes having an inner diameter of 3 mm. The mixture of the hydrogenated ring-opening polymer of dicyclopentadiene and the antioxidant was molded into a strand shape by hot melt extrusion molding, and then chopped with a strand cutter to obtain a pellet-shaped crystalline resin A. The operating conditions of the twin-screw extruder were as follows. Barrel temperature setting: 270~280℃ Die temperature setting = 250℃ Screw speed: 145 rpm Furthermore, when the sign of the intrinsic birefringence of the crystalline resin A was confirmed by the above-mentioned method, the sign was "positive."
[0132] [Production Example 2. Production of Crystalline Resin B] A metallic pressure reactor was thoroughly dried and then purged with nitrogen. 152.7 parts of cyclohexane, 42.9 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.53 parts of 1-hexene were added to the metallic pressure reactor and heated to 53°C.
[0133] 0.028 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex was dissolved in 2.772 parts of toluene to prepare a solution. 0.156 parts of a 19% diethylaluminum ethoxide / n-hexane solution was added to this solution and stirred for 10 minutes to prepare a catalyst solution. This catalyst solution was added to a pressure-resistant reactor to start a ring-opening polymerization reaction. After that, the reaction was continued for 4 hours while maintaining the temperature at 53°C to obtain a solution of a ring-opened polymer of dicyclopentadiene. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,680 and 27,000, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.11.
[0134] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.37 parts of methanol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").
[0135] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.
[0136] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated product of a crystalline ring-opening polymer of dicyclopentadiene. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 95°C, the melting point (Tm) was 266°C, and the ratio of racemo-dyads was 89%.
[0137] 100 parts of the obtained hydrogenated ring-opening polymer of dicyclopentadiene was mixed with 1.1 parts of an antioxidant (tetrakis [methylene-3- (3', 5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.), and then the mixture was put into a twin-screw extruder (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.) equipped with four die holes having an inner diameter of 3 mm. The mixture of the hydrogenated ring-opening polymer of dicyclopentadiene and the antioxidant was molded into a strand shape by hot melt extrusion molding, and then chopped with a strand cutter to obtain a pellet-shaped crystalline resin B. The operating conditions of the twin-screw extruder were as follows. Barrel temperature setting: 270~280℃ Die temperature setting = 250℃ Screw speed: 145 rpm Furthermore, when the sign of the intrinsic birefringence of the crystalline resin B was confirmed by the above-mentioned method, the sign was "positive."
[0138] [Production Example 3. Production of coating resin solution using crystalline resin B] Decalin solvent was placed in a pressure-resistant container, and crystalline resin B as resin (b) produced in Production Example 2 was added thereto so as to have a concentration of 33%. Then, the mixture was heated at 200°C for 1 hour under a nitrogen gas atmosphere. After confirming that crystalline resin B had dissolved, the temperature was slowly lowered to 130°C and maintained at that temperature, to prepare a resin solution for coating at a temperature of 130°C. In order to prevent crystalline resin B from precipitating due to a temperature drop, the solution was left to stand while maintaining the liquid temperature at 130°C until it was used in the coating process.
[0139] [Example 1] (1-1. Step (1): Production of film made of crystalline resin A) The crystalline resin A as the resin (a) produced in Production Example 1 was molded using a hot melt extrusion film molding machine equipped with a T-die to obtain an extruded film (film (1), thickness 15 μm) as a long substrate film with a width of approximately 400 mm. The obtained extruded film was wound up into a roll shape. The operating conditions of the film forming machine were as follows: Barrel temperature setting: 280℃~300℃ Die temperature = 270℃ Cast roll temperature = 80℃
[0140] The properties of the extruded film (Film (1)) are shown in the table below. In the table, the abbreviations have the following meanings. "Re1": In-plane retardation "Rth1": Retardation in the thickness direction "d1": Thickness "Δn1": Birefringence in the thickness direction (Rth1 / d1) "Nz1": NZ coefficient
[0141] [Table 1]
[0142] (1-2. Process (2): Coating process) From the roll of extruded film as the base film produced in (1-1), an extruded film was cut into an A4 size (210 mm x 297 mm) with the long side being the conveying direction (MD direction) during the production of the extruded film. The resin solution obtained in Production Example 3 was coated on one side of the cut-out extruded film using a bar coater so that the coating layer had a thickness of 12 μm. The thickness of the coating layer was adjusted by selecting the bar of the bar coater.
[0143] As a result, a coating layer having a thickness of 12 μm was formed on the surface of the base film, and film (2) was obtained. From the concentration of resin (b) in the resin solution and the thickness of the coating layer, the thickness of layer (B) obtained by drying the coating layer was calculated to be about 4 μm.
[0144] (1-3. Process (3): Drying process) Thereafter, the film (2) was dried in a vacuum oven at 170° C. to dry the coating layer, thereby obtaining a multilayer film. The multilayer film and the layers (A) and (B) constituting the multilayer film were evaluated by the above-mentioned methods.
[0145] (1-4. Process (4): Stretching and heating process) The obtained multilayer film was cut to a size of 100 mm x 100 mm. The cut multilayer film was fed to a stretching machine (manufactured by Etoh Corporation), and both ends of the film were held by five clips, and the film was freely uniaxially stretched 1.2 times in the longitudinal direction in the extrusion film formation process to produce film (c) as an optical film. The stretching was carried out by: (4a): preheating the multilayer film to 160°C, then; (4b): stretching the preheated multilayer film at 160°C, then; (4c): holding the stretched multilayer film in a tensed state at a temperature of 160°C to promote crystallization, then; (4d): cooling the multilayer film (optical film) with promoted crystallization at a temperature of 100°C. The optical film was evaluated by the above-mentioned methods.
[0146] [Comparative Example 1] A film (3) and an optical film were obtained in the same manner as in Example 1, except for the following changes. The extruded film (film (1)) was not subjected to (1-2. step (2)) and (1-3. step (3)), but instead was subjected to the following solvent immersion step to obtain film (3). The film (1) was immersed in toluene by passing the film (1) through a bath filled with toluene. The time during which the film (1) passed through the bath (i.e., the time during which the film (1) was in contact with toluene) was 5 seconds. The film (2) obtained by passing the film (1) through the bath was passed through an oven at 80°C to dry the film (2), thereby obtaining a film (3). In (1-4. Step (4)), film (3) was used instead of the multilayer film, and instead of freely uniaxially stretching film (3), it was fixedly uniaxially stretched by the following method to obtain an optical film. The film (3) was fed to a transverse stretching machine using a tenter method, and while adjusting the take-up tension and the tenter chain tension, it was fixedly uniaxially stretched 1.5 times in the transverse direction to produce a film (c) as an optical film. The stretching was carried out by (4a): preheating the film (3) to 110°C, then; (4b): stretching the preheated film (3) at 110°C, then; (4c): holding the stretched film (3) under tension at a temperature of 170°C to promote crystallization, then; (4d): cooling the crystallization-promoted film (3) (optical film) at a temperature of 100°C.
[0147] The layer (A) and the optical film included in the film (3) were evaluated by the above-mentioned methods.
[0148] The results are shown in the table below. In the table below, the abbreviations have the following meanings. "Crystalline COP-A": Crystalline resin A containing the hydrogenated product of the ring-opening polymer of dicyclopentadiene obtained in Production Example 1 "Crystalline COP-B": Crystalline resin B containing the hydrogenated product of the ring-opening polymer of dicyclopentadiene obtained in Production Example 2 "Layer structure": Layer structure of the multilayer film or film (3) "B / A": Two-layer structure of layer (B) / layer (A) "A": Single layer structure of layer (A) only "Rea": In-plane retardation of layer (A) "Rtha": Retardation in the thickness direction of layer (A) "Δna": Birefringence in the thickness direction of layer (A) (Rtha / da) "da": thickness of layer (A) "Nza": NZ coefficient of layer (A) "Reb": In-plane retardation of layer (B) "Rthb": Retardation in the thickness direction of layer (B) "Δnb": Birefringence in the thickness direction of layer (B) (Rthb / db) "db": thickness of layer (B) "Nzb": NZ coefficient of layer (B) "Rec": In-plane retardation of optical film "Rthc": Retardation in the thickness direction of the optical film "Nzc": NZ coefficient of optical film "dc": Optical film thickness Regarding the steps (2) and (3), the items of the coating target, coating layer thickness, and coating conditions are shown for the immersion step in Comparative Example 1.
[0149] [Table 2]
[0150] From the above results, the following can be seen: It can be seen that by stretching the multilayer film according to Example 1, a thin optical film having an NZ coefficient greater than 0 and less than 1 and a thickness of 20 μm or less can be obtained. On the other hand, it is found that the optical film obtained by stretching the film (3) according to the comparative example has an NZ coefficient greater than 0 and less than 1, but a thickness greater than 20 μm. The above results show that the multilayer film of the present invention makes it possible to produce a thin optical film having an NZ coefficient greater than 0 and less than 1. [Explanation of symbols]
[0151] 100 Multilayer Film 110 layers (layer (A)) 110U First Surface 110D Second Surface 120 layers (layer (B))
Claims
1. A layer (A) made of a resin (a) containing a crystalline polymer (Pa) and having a positive intrinsic birefringence; and a layer (B) made of a resin (b) having a positive intrinsic birefringence and containing a polymer (Pb) having crystallinity, The NZ coefficient Nza of the layer (A) satisfies the following formula (1), The NZ coefficient Nzb of the layer (B) satisfies the following formula (2), A multilayer film, wherein the birefringence Δna in the thickness direction of the layer (A) and the birefringence Δnb in the thickness direction of the layer (B) satisfy the following formula (3): Nza<0...(1) Nzb<0...(2) 1<Δnb / Δna<10 (3)
2. The multilayer film according to claim 1 , wherein the crystalline polymer (Pb) is a polymer containing an alicyclic structure.
3. The multilayer film according to claim 1 or 2, wherein the layer (A) and the layer (B) are directly connected to each other.
4. The multilayer film according to any one of claims 1 to 3, wherein a retardation Rtha in the thickness direction of the layer (A) and a retardation Rthb in the thickness direction of the layer (B) satisfy the following formula (4): 1<Rthb / Rtha≦3...(4)
5. A method for producing the multilayer film according to any one of claims 1 to 4, comprising the steps of: A step (1) of preparing a substrate film made of the resin (a); (2) a step of coating a resin solution containing the resin (b) and a solvent on at least one of the two surfaces of the base film to form a coating layer; (3) drying the coating layer to form a layer (B) and obtain the multilayer film; A method for producing a multilayer film comprising the steps of:
6. A method for producing an optical film, comprising a step of stretching the multilayer film according to any one of claims 1 to 4 to obtain an optical film.
7. An optical film which is a stretched product of the multilayer film according to any one of claims 1 to 4.
Citation Information
Patent Citations
Method for producing birefringent film and liquid crystal display device using the same
JP1993346507A
Retardation film laminate and method for manufacturing the same, polarizing plate and liquid crystal display device
JP2014106338A
Optical laminate and liquid crystal display device
JP2015031753A
Method for producing resin film, resin film, and optical film
JP2016026909A
Method for producing film with thickness retardation (RTH) having negative value
JP2018036535A