Binder composition for all-solid-state secondary battery, slurry composition for all-solid-state secondary battery, solid electrolyte-containing layer and all-solid-state secondary battery
The use of a binder composition with an acrylic polymer and coagulant in specific concentrations, along with a slurry composition, addresses the high-temperature storage challenges of all-solid-state secondary batteries by enhancing their capacity retention under elevated temperatures.
Patent Information
- Application Number
- JP2020549169
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-28
- Filing Date
- 2019-09-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2039-09-20
AI Technical Summary
All-solid-state secondary batteries face challenges in maintaining high-temperature storage characteristics, particularly when exposed to high temperatures, due to the use of conventional acrylic polymers as binders, which do not adequately address capacity reduction under such conditions.
A binder composition for all-solid-state secondary batteries containing an acrylic polymer and a coagulant in specific mass ppm ranges, along with a slurry composition that includes a solid electrolyte and an organic solvent, forms a solid electrolyte-containing layer that enhances high-temperature storage characteristics.
The proposed binder and slurry compositions enable the formation of a solid electrolyte-containing layer that significantly improves the high-temperature storage performance of all-solid-state secondary batteries, ensuring better capacity retention under elevated temperatures.
Smart Images

Figure 0007581877000001 
Figure 0007581877000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder composition for an all-solid-state secondary battery, a slurry composition for an all-solid-state secondary battery, a solid electrolyte-containing layer, and an all-solid-state secondary battery. [Background technology]
[0002] In recent years, the demand for secondary batteries such as lithium-ion secondary batteries has been increasing for various applications, including portable terminals such as portable information terminals and portable electronic devices, as well as small home power storage devices, motorcycles, electric vehicles, hybrid electric vehicles, etc. As the applications expand, further improvements in the safety of secondary batteries are required.
[0003] In view of this, as a secondary battery with high safety, attention has been focused on all-solid-state secondary batteries that use solid electrolytes instead of organic solvent electrolytes, which are highly flammable and have a high risk of ignition in the event of leakage.
[0004] Here, the all-solid-state secondary battery has a positive electrode, a negative electrode, and a solid electrolyte layer located between the positive electrode and the negative electrode. The electrodes (positive electrode, negative electrode) of the all-solid-state secondary battery are formed, for example, by applying a slurry composition containing an electrode active material (positive electrode active material, negative electrode active material), a binder, and a solid electrolyte onto a current collector, and then drying the applied slurry composition to provide an electrode mixture layer (positive electrode mixture layer, negative electrode mixture layer) on the current collector. The solid electrolyte layer of the all-solid-state secondary battery is formed, for example, by applying a slurry composition containing a binder and a solid electrolyte onto an electrode or a release substrate, and then drying the applied slurry composition.
[0005] Acrylic polymers have been used as binders for forming solid electrolyte layers. For example, in Patent Document 1, a binder composition containing an acrylic polymer and an organic solvent is prepared by emulsion-polymerizing a monomer in water in the presence of sodium dodecylbenzenesulfonate as an emulsifier to obtain an aqueous dispersion of an acrylic polymer, and then replacing the aqueous dispersion with an organic solvent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 152262 Summary of the Invention [Problem to be solved by the invention]
[0007] Here, particularly in recent years, in the field of electric vehicles and the like, all-solid-state secondary batteries are often exposed to high-temperature conditions (e.g., 80°C or higher), and there has been a problem of suppressing the capacity decrease under high-temperature conditions (i.e., improving high-temperature storage characteristics). That is, there has been a demand for forming a layer containing a solid electrolyte, such as a solid electrolyte layer or an electrode mixture layer (hereinafter referred to as a "solid electrolyte-containing layer"), using a binder composition containing an acrylic polymer, and for adequately ensuring the high-temperature storage characteristics of the all-solid-state secondary battery.
[0008] Therefore, an object of the present invention is to provide a binder composition for an all-solid-state secondary battery and a slurry composition for an all-solid-state secondary battery, which are capable of forming a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics. Another object of the present invention is to provide a solid electrolyte-containing layer capable of imparting excellent high-temperature storage characteristics to an all-solid-state secondary battery, and to provide an all-solid-state secondary battery having excellent high-temperature storage characteristics. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that a slurry composition prepared using a binder composition containing an acrylic polymer and a predetermined amount of a coagulant can form a solid electrolyte-containing layer capable of imparting excellent high-temperature storage properties to an all-solid-state secondary battery, thereby completing the present invention.
[0010] That is, the present invention aims to advantageously solve the above problems, and the binder composition for all-solid-state secondary batteries of the present invention is characterized in that it contains an acrylic polymer and a coagulant in an amount of 500 ppm by mass to 5000 ppm by mass relative to the acrylic polymer. In this way, if a solid electrolyte-containing layer is formed using a slurry composition containing a binder composition that contains an acrylic polymer and a coagulant, and the amount of the coagulant relative to the acrylic polymer is within the above-mentioned range, it is possible to make the all-solid-state secondary battery exhibit excellent high-temperature storage characteristics.
[0011] In the present invention, the term "acrylic polymer" refers to a polymer containing 50% by mass or more of (meth)acrylic acid ester monomer units. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic. In the present invention, "containing a monomer unit" means that "a polymer obtained by using the monomer contains a repeating unit derived from the monomer". In addition, in the present invention, the ratio of each repeating unit (monomer unit) constituting the polymer is 1 H-NMR and 13 It can be measured using nuclear magnetic resonance (NMR) techniques such as C-NMR. In the present invention, the term "coagulant" refers to a substance that is added to aggregate and coagulate the acrylic polymer dispersed in water, and that instantly and irreversibly coagulates the acrylic polymer particles dispersed in water in the room temperature range (e.g., 15°C to 30°C). In the present invention, the content of the "coagulant" relative to the "acrylic polymer" can be determined by elemental analysis.
[0012] Here, in the binder composition for an all-solid-state secondary battery of the present invention, the coagulant is preferably a metal sulfate having a valence of 1 to 3. By using a metal sulfate having a valence of 1 to 3 as the coagulant, it is possible to sufficiently improve the high-temperature storage characteristics of the all-solid-state secondary battery while ensuring the production efficiency of the binder composition.
[0013] In the binder composition for an all-solid-state secondary battery of the present invention, an emulsion polymer can be used as the acrylic polymer. The binder composition for an all-solid-state secondary battery of the present invention may further contain an organic solvent.
[0014] The present invention also aims to advantageously solve the above problems, and the slurry composition for an all-solid-state secondary battery of the present invention is characterized in that it contains a solid electrolyte and a binder composition for an all-solid-state secondary battery containing the above-mentioned organic solvent. In this way, by forming a solid electrolyte-containing layer using a slurry composition containing a solid electrolyte and a binder composition containing an organic solvent, it is possible to make the all-solid-state secondary battery exhibit excellent high-temperature storage characteristics.
[0015] Here, the slurry composition for an all-solid-state secondary battery of the present invention can contain an inorganic solid electrolyte as the solid electrolyte.
[0016] The slurry composition for an all-solid-state secondary battery of the present invention may further include an electrode active material. By using the slurry composition for an all-solid-state secondary battery containing the electrode active material, it is possible to satisfactorily form an electrode mixture layer that can provide the all-solid-state secondary battery with excellent high-temperature storage properties.
[0017] The present invention also aims to advantageously solve the above problems, and the solid electrolyte-containing layer of the present invention is characterized in that it is formed using any one of the above-mentioned slurry compositions for all-solid-state secondary batteries. The solid electrolyte-containing layer formed using the above-mentioned slurry composition for all-solid-state secondary batteries can provide the all-solid-state secondary battery with excellent high-temperature storage characteristics.
[0018] Furthermore, the present invention aims to advantageously solve the above problems, and the all-solid-state secondary battery of the present invention is characterized by comprising the above-mentioned solid electrolyte-containing layer. By using the above-mentioned solid electrolyte layer, an all-solid-state secondary battery capable of exhibiting excellent high-temperature storage characteristics can be obtained. Effect of the Invention
[0019] According to the present invention, it is possible to provide a binder composition for an all-solid-state secondary battery and a slurry composition for an all-solid-state secondary battery, which are capable of forming a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics. Moreover, according to the present invention, it is possible to provide a solid electrolyte-containing layer that can enable an all-solid-state secondary battery to exhibit excellent high-temperature storage characteristics, and an all-solid-state secondary battery having excellent high-temperature storage characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment of the present invention will be described in detail. Here, the binder composition for an all-solid-state secondary battery of the present invention is used when preparing the slurry composition for an all-solid-state secondary battery of the present invention. The slurry composition for an all-solid-state secondary battery of the present invention is used when forming a solid electrolyte-containing layer such as an electrode mixture layer or a solid electrolyte layer used in an all-solid-state secondary battery such as an all-solid-state lithium ion secondary battery. In addition, the all-solid-state secondary battery of the present invention is composed of at least one layer selected from the group consisting of a positive electrode mixture layer of a positive electrode, a negative electrode mixture layer of a negative electrode, and a solid electrolyte layer, which is a solid electrolyte-containing layer of the present invention formed using the slurry composition for an all-solid-state secondary battery of the present invention.
[0021] (Binder composition for all-solid-state secondary batteries) The binder composition of the present invention contains an acrylic polymer and a coagulant, and may further contain other components such as an organic solvent, etc. The binder composition of the present invention requires that the content of the coagulant is 500 ppm by mass or more and 5000 ppm by mass or less based on the acrylic polymer.
[0022] Furthermore, a slurry composition prepared using the binder composition of the present invention can form a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics.
[0023] <Acrylic polymer> The acrylic polymer is a component that functions as a binder in the solid electrolyte-containing layer formed from the slurry composition containing the binder composition. The binder composition of the present invention may contain one type of acrylic polymer or may contain two or more types of acrylic polymers.
[0024] <<Composition>> Here, as described above, the acrylic polymer is a polymer containing 50% by mass or more of (meth)acrylic acid ester monomer units as repeating units. The acrylic polymer may contain repeating units other than the (meth)acrylic acid ester monomer units (hereinafter referred to as "other repeating units").
[0025] [(Meth)acrylic acid ester monomer unit] The (meth)acrylic acid ester monomer capable of forming the (meth)acrylic acid ester monomer unit is not particularly limited, but may be, for example, a (meth)acrylic acid alkyl ester monomer and a (meth)acrylic acid alkoxyalkyl ester monomer. The (meth)acrylic acid ester monomer may be used alone or in combination of two or more kinds.
[0026] The (meth)acrylic acid alkyl ester monomer is not particularly limited, but is preferably an ester of an alkanol having 1 to 8 carbon atoms and (meth)acrylic acid. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. These can be used alone or in combination of two or more. Among these, from the viewpoint of sufficiently improving the high-temperature storage characteristics of the all-solid-state secondary battery, ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred.
[0027] The (meth)acrylic acid alkoxyalkyl ester monomer is not particularly limited, but is preferably an ester of an alkoxyalkyl alcohol having 2 to 8 carbon atoms and (meth)acrylic acid. Specifically, methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, and 4-methoxybutyl (meth)acrylate can be mentioned. These can be used alone or in combination of two or more. Among these, from the viewpoint of sufficiently improving the high-temperature storage characteristics of the all-solid-state secondary battery, 2-ethoxyethyl (meth)acrylate and 2-methoxyethyl (meth)acrylate are preferred, and 2-ethoxyethyl acrylate and 2-methoxyethyl acrylate are particularly preferred.
[0028] In order to ensure the binding property of the acrylic polymer, the content of the (meth)acrylic acid ester monomer unit in the acrylic polymer must be 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more. On the other hand, the upper limit of the content of the (meth)acrylic acid ester monomer unit in the acrylic polymer is not particularly limited, and can be 100% by mass or less. From the viewpoint of sufficiently improving the high-temperature storage characteristics of the all-solid-state secondary battery, it is preferable to use, as the acrylic polymer, a polymer containing 30% by mass or more and 100% by mass or less of (meth)acrylic acid alkyl ester monomer units as (meth)acrylic acid ester monomer units. Furthermore, from the viewpoint of sufficiently improving the high-temperature storage characteristics of the all-solid-state secondary battery, the acrylic polymer preferably contains both an ethyl acrylate unit and an n-butyl acrylate unit.
[0029] [Other repeating units] The other repeating units are not particularly limited as long as they are derived from a monomer copolymerizable with the above-mentioned (meth)acrylic acid ester monomer, and examples thereof include aromatic vinyl monomer units, α,β-ethylenically unsaturated nitrile monomer units, acrylamide monomer units, etc. The monomers capable of forming the other repeating units may be used alone or in combination of two or more.
[0030] Examples of aromatic vinyl monomers capable of forming aromatic vinyl monomer units include styrene, α-methylstyrene, and divinylbenzene. These may be used alone or in combination of two or more.
[0031] Examples of α,β-ethylenically unsaturated nitrile monomers capable of forming α,β-ethylenically unsaturated nitrile monomer units include acrylonitrile and methacrylonitrile. These can be used alone or in combination of two or more.
[0032] Examples of the acrylamide monomer capable of forming the acrylamide monomer unit include acrylamide and methacrylamide. These can be used alone or in combination of two or more.
[0033] In addition to the above-mentioned aromatic vinyl monomers, α,β-ethylenically unsaturated nitrile monomers, and acrylamide monomers, olefin monomers such as ethylene, vinyl acetate, propylene, butadiene, and isoprene can also be used to form other repeating units.
[0034] Among these, as the monomer capable of forming the other repeating unit, styrene, acrylonitrile, methacrylonitrile, ethylene and vinyl acetate are preferred, and acrylonitrile, methacrylonitrile and ethylene are more preferred.
[0035] The content of other repeating units in the acrylic polymer is 50% by mass or less, preferably 40% by mass or less, and more preferably 30% by mass or less.
[0036] <<Preparation method>> The method for preparing the acrylic polymer by polymerizing the above-mentioned monomers is not particularly limited, but it is preferable to prepare it by emulsion polymerization, which will be described later in the section "Production method of binder composition". That is, the acrylic polymer is preferably a polymer prepared by emulsion polymerization (emulsion polymer).
[0037] <Coagulant> As described above, the coagulant is a substance capable of coagulating the acrylic polymer dispersed in water by agglomeration and coagulation. Although not particularly limited in the present invention, the coagulant is usually added to coagulate the acrylic polymer in the aqueous dispersion (e.g., emulsion polymerization liquid) obtained by polymerization reaction in water, and remains in the binder composition.
[0038] <<Type>> Here, the coagulant is not particularly limited, but examples thereof include monovalent to trivalent metal salts. Here, the monovalent to trivalent metal salts are salts containing metals that become monovalent to trivalent metal ions when dissolved in water, and are not particularly limited, but examples thereof include salts of inorganic acids selected from hydrochloric acid, nitric acid, and sulfuric acid, and organic acids such as acetic acid, and metals selected from sodium, potassium, lithium, magnesium, calcium, zinc, titanium, manganese, iron, cobalt, nickel, aluminum, and tin. Hydroxides of these metals can also be used.
[0039] Specific examples of the monovalent or more and trivalent or less metal salts include metal chlorides such as sodium chloride, potassium chloride, lithium chloride, magnesium chloride, calcium chloride, zinc chloride, titanium chloride, manganese chloride, iron chloride, cobalt chloride, nickel chloride, aluminum chloride, and tin chloride; metal nitrates such as sodium nitrate, potassium nitrate, lithium nitrate, magnesium nitrate, calcium nitrate, zinc nitrate, titanium nitrate, manganese nitrate, iron nitrate, cobalt nitrate, nickel nitrate, aluminum nitrate, and tin nitrate; metal sulfates such as sodium sulfate, potassium sulfate, lithium sulfate, magnesium sulfate, calcium sulfate, zinc sulfate, titanium sulfate, manganese sulfate, iron sulfate, cobalt sulfate, nickel sulfate, aluminum sulfate, and tin sulfate; and the like. Among these, calcium chloride, sodium chloride, magnesium chloride, zinc chloride, and metal sulfates are preferred, metal sulfates are more preferred, and sodium sulfate and magnesium sulfate are even more preferred, from the viewpoint of sufficiently improving the high-temperature storage characteristics of the all-solid-state secondary battery while ensuring the production efficiency of the binder composition. These can be used alone or in combination.
[0040] <<Content>> The content of the coagulant in the binder composition of the present invention must be 500 ppm by mass or more and 5000 ppm by mass or less, preferably 800 ppm by mass or more, and preferably 4500 ppm by mass or less, more preferably 4000 ppm by mass or less, and even more preferably 3500 ppm by mass or less, relative to the acrylic polymer.
[0041] Here, as described above, the coagulant is usually added to coagulate the acrylic polymer in the aqueous dispersion obtained by the polymerization reaction in water, and in such a case, it inevitably remains in the obtained binder composition (especially the acrylic polymer). According to the present inventor, it has become clear that if the amount of this coagulant is excessive, the high-temperature storage characteristics of the all-solid-state secondary battery cannot be sufficiently ensured. That is, if the content of the coagulant contained in the binder composition exceeds 5000 mass ppm with respect to the acrylic polymer, the all-solid-state secondary battery cannot exhibit excellent high-temperature storage characteristics. On the other hand, if the amount of the coagulant added to coagulate the acrylic polymer in the aqueous dispersion is reduced or the acrylic polymer after coagulation is washed excessively in order to reduce the amount of the coagulant, the recovery rate of the acrylic polymer is excessively reduced, the manufacturing process becomes complicated, and the manufacturing efficiency of the binder composition is impaired. From this viewpoint, the content of the coagulant contained in the binder composition needs to be 500 mass ppm or more. The content (residual amount) of the coagulant in the binder composition can be adjusted by changing the type of emulsifier used in preparing the acrylic polymer, the amount of the coagulant added to the aqueous dispersion of the acrylic polymer, and the washing conditions for the acrylic polymer (binder composition) after coagulation.
[0042] <<Other ingredients>> There are no particular limitations on the components that the binder composition may optionally contain other than the acrylic polymer and the coagulant described above.
[0043] For example, the binder composition may contain an organic solvent as another component. Examples of the organic solvent include chain aliphatic hydrocarbons such as hexane, cyclic aliphatic hydrocarbons such as cyclopentane and cyclohexane, aromatic hydrocarbons such as toluene and xylene, ketones such as ethyl methyl ketone, cyclohexanone and diisobutyl ketone, esters such as ethyl acetate, butyl acetate, γ-butyrolactone and ε-caprolactone, acylonitriles such as acetonitrile and propionitrile, ethers such as tetrahydrofuran, ethylene glycol diethyl ether and n-butyl ether, alcohols such as methanol, ethanol, isopropanol, ethylene glycol and ethylene glycol monomethyl ether, and amides such as N-methylpyrrolidone and N,N-dimethylformamide. Among them, from the viewpoint of suppressing deterioration of the solid electrolyte and obtaining a solid electrolyte-containing layer having excellent ion conductivity, it is preferable to use a non-polar organic solvent as the organic solvent, and it is more preferable to use hexane or xylene. Furthermore, from the viewpoint of further improving the high-temperature storage characteristics of the all-solid-state secondary battery, xylene is particularly preferable. The above organic solvents can be used alone or in combination of two or more kinds.
[0044] In addition, the binder composition may contain, as other components, a component used in preparing the acrylic polymer described later in the section "Production method of binder composition", or may contain any component described later in the section "Slurry composition for all-solid-state secondary battery".
[0045] <Method for producing binder composition> The method for producing the binder composition of the present invention described above is not particularly limited, but may include, for example, the following steps: A step of emulsion-polymerizing a monomer containing a (meth)acrylic acid ester monomer in the presence of an emulsifier to obtain an emulsion polymerization liquid containing an acrylic polymer (emulsion polymerization step); A step of adding a coagulant to the emulsion polymerization liquid to coagulate the acrylic polymer to obtain a water-containing crumb (coagulation step); A step of washing the hydrous crumbs (washing step); and A step of drying the washed wet crumbs (drying step); It is preferable to produce the binder composition through the above-mentioned emulsion polymerization step, coagulation step, washing step, and drying step. The method for producing the binder composition through the above-mentioned emulsion polymerization step, coagulation step, washing step, and drying step may include steps other than the emulsion polymerization step, coagulation step, washing step, and drying step (hereinafter, referred to as "other steps").
[0046] <<Emulsion polymerization process>> In the emulsion polymerization step, a monomer such as the above-mentioned (meth)acrylic acid ester monomer is emulsion-polymerized in water in the presence of an emulsifier to obtain an emulsion polymerization liquid (aqueous dispersion of an acrylic polymer) containing an acrylic polymer. Here, the emulsion polymerization method in the emulsion polymerization step is not particularly limited as long as the monomer such as the (meth)acrylic acid ester monomer can be polymerized, and for example, any method using an emulsifier, a polymerization initiator, a polymerization terminator, etc. can be used.
[0047] The emulsifier is not particularly limited, and any of a nonionic emulsifier, an anionic emulsifier, and a cationic emulsifier can be used. Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers such as polyoxyethylene dodecyl ether, polyoxyethylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether, polyoxyethylene alkyl esters, polyoxyethylene sorbitan alkyl esters, polyoxyethylene polyoxypropylene glycol, and polyethylene glycol monostearate. Examples of the anionic emulsifier include salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid, alkylbenzenesulfonates such as sodium dodecylbenzenesulfonate, higher alcohol sulfates such as sodium lauryl sulfate, higher phosphates such as sodium alkyl phosphates, and alkyl sulfosuccinates. Examples of the cationic emulsifier include alkyltrimethylammonium chloride, dialkylammonium chloride, and benzylammonium chloride.
[0048] These emulsifiers can be used alone or in combination of two or more. Among these emulsifiers, nonionic emulsifiers and anionic emulsifiers are preferred, and it is more preferred to use a combination of a nonionic emulsifier and an anionic emulsifier. By using a combination of a nonionic emulsifier and an anionic emulsifier, it is possible to effectively suppress the generation of dirt caused by the adhesion of an acrylic polymer to a polymerization apparatus (e.g., a polymerization tank) used in emulsion polymerization, while reducing the amount of coagulant used in the coagulation step described below, and as a result, the amount of coagulant in the finally obtained binder composition (acrylic polymer) can be reduced. Furthermore, by using a combination of a nonionic emulsifier and an anionic emulsifier, the emulsifying action can be enhanced, and the amount of emulsifier used can be reduced. As a result, the amount of emulsifier remaining in the finally obtained binder composition (acrylic polymer) can be reduced, and the water resistance of the obtained acrylic polymer can be further improved.
[0049] Here, the amount of emulsifier used is preferably 0.1 parts by mass or more and 5 parts by mass or less, more preferably 0.5 parts by mass or more and 4 parts by mass or less, and even more preferably 1 part by mass or more and 3 parts by mass or less, in terms of the total amount of emulsifier used relative to 100 parts by mass of all monomers used in the polymerization. In addition, when a nonionic emulsifier and an anionic emulsifier are used in combination, the amount of the nonionic emulsifier used is preferably 0.1 to 4 parts by mass, more preferably 0.2 to 3 parts by mass, and even more preferably 0.5 to 2 parts by mass, relative to 100 parts by mass of the total monomers used in the polymerization, and the amount of the anionic emulsifier used is preferably 0.1 to 4 parts by mass, more preferably 0.2 to 3 parts by mass, and even more preferably 0.5 to 2 parts by mass, relative to 100 parts by mass of the total monomers used in the polymerization. In addition, the usage ratio is preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 80 / 20, and even more preferably 25 / 75 to 75 / 25, in terms of the mass ratio of the nonionic emulsifier / anionic emulsifier.
[0050] As the polymerization initiator, an azo compound such as azobisisobutyronitrile; an organic peroxide such as diisopropylbenzene hydroperoxide, cumene hydroperoxide, paramenthane hydroperoxide, benzoyl peroxide; an inorganic peroxide such as potassium persulfate, sodium persulfate, ammonium persulfate; and the like can be used. These polymerization initiators can be used alone or in combination of two or more kinds. The amount of the polymerization initiator used is preferably 0.001 part by mass or more and 1.0 part by mass or less with respect to 100 parts by mass of the total monomers used in the polymerization.
[0051] In addition, the organic peroxide and inorganic peroxide as the polymerization initiator are preferably used as a redox polymerization initiator in combination with a reducing agent. The reducing agent to be used in combination is not particularly limited, but includes compounds containing reduced metal ions such as ferrous sulfate, sodium ferric hexamethylenediaminetetraacetate, and cuprous naphthenate; ascorbic acid (salts) such as ascorbic acid, sodium ascorbate, and potassium ascorbate; erythorbic acid (salts) such as erythorbic acid, sodium erythorbate, and potassium erythorbate; sugars; sulfinates such as sodium hydroxymethanesulfinate; sodium sulfite, potassium sulfite, sodium hydrogen sulfite, and aldehyde sulfite. Sulfites such as sodium hydrogen sulfite and potassium hydrogen sulfite; pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium hydrogen pyrosulfite, and potassium hydrogen pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid (salts) such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite, and potassium hydrogen phosphite; pyrophosphorous acid (salts) such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite, and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, etc. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 0.0003 parts by mass or more and 0.4 parts by mass or less relative to 100 parts by mass of the polymerization initiator. In the present invention, the term "acid (salt)" means an acid and / or a salt of the acid.
[0052] Examples of the polymerization terminator include hydroxylamine, hydroxylamine sulfate, diethylhydroxyamine, hydroxylamine sulfonic acid and its alkali metal salts, sodium dimethyldithiocarbamate, hydroquinone, etc. The amount of the polymerization terminator used is not particularly limited, but is preferably 0.1 parts by mass or more and 2 parts by mass or less based on 100 parts by mass of the total monomers used in the polymerization.
[0053] The amount of water used is not particularly limited, but is preferably 80 parts by mass or more and 500 parts by mass or less, more preferably 100 parts by mass or more and 300 parts by mass or less, based on 100 parts by mass of all monomers used in the polymerization.
[0054] In the emulsion polymerization, if necessary, polymerization auxiliary materials such as a molecular weight regulator, a particle size regulator, a chelating agent, an oxygen scavenger, etc. Any of these polymerization auxiliary materials can be used.
[0055] Here, the emulsion polymerization may be carried out by any method, including batch, semi-batch, and continuous, but semi-batch is preferred. Specifically, the polymerization reaction is carried out while continuously dropping the monomer used for polymerization into a reaction system containing a polymerization initiator and a reducing agent from the start of the polymerization reaction until an arbitrary time has elapsed. For example, it is preferable to carry out the polymerization reaction while continuously dropping at least one of the monomers, polymerization initiator, and reducing agent used for polymerization into the polymerization reaction system from the start of the polymerization reaction until an arbitrary time has elapsed. It is more preferable to carry out the polymerization reaction while continuously dropping all of the monomers, polymerization initiator, and reducing agent used for polymerization into the polymerization reaction system from the start of the polymerization reaction until an arbitrary time has elapsed. By carrying out the polymerization reaction while continuously dropping these, the emulsion polymerization can be carried out stably, and the polymerization reaction rate can be improved. The polymerization is usually carried out at a temperature range of 0°C to 70°C, preferably 5°C to 50°C.
[0056] In addition, when the polymerization reaction is carried out while continuously dropping the monomers used for polymerization, it is preferable to mix the monomers used for polymerization with an emulsifier and water to form a monomer emulsion, and to continuously drop the monomer emulsion. The method for preparing the monomer emulsion is not particularly limited, and examples thereof include a method of stirring the total amount of the monomers used for polymerization, the total amount of the emulsifier, and water using a stirrer such as a homomixer or a disk turbine. The amount of water used in the monomer emulsion is preferably 10 parts by mass or more and 70 parts by mass or less, more preferably 20 parts by mass or more and 50 parts by mass or less, based on 100 parts by mass of the total monomers used for polymerization.
[0057] In addition, when the polymerization reaction is carried out while continuously dropping all of the monomers, polymerization initiator, and reducing agent used in the polymerization into the polymerization reaction system from the start of the polymerization reaction until a desired time has elapsed, these may be dropped into the polymerization system using separate dropping devices, or at least the polymerization initiator and the reducing agent may be mixed in advance and, if necessary, dropped into the polymerization system in the form of an aqueous solution from the same dropping device. After the dropping is completed, the reaction may be continued for a desired time in order to further improve the polymerization reaction rate.
[0058] <<Coagulation process>> In the coagulation step, a coagulant is added to the emulsion polymerization liquid obtained in the above-mentioned emulsion polymerization step to coagulate the acrylic polymer, thereby obtaining water-containing crumbs (coagulated material containing the acrylic polymer, the coagulant, and water).
[0059] As the coagulant, the above-mentioned monovalent to trivalent metal salt can be suitably used. The amount of the coagulant used is preferably 1 part by mass to 20 parts by mass, more preferably 2 parts by mass to 15 parts by mass, based on 100 parts by mass of the acrylic polymer in the emulsion polymerization liquid, from the viewpoint of making the content (residual amount) of the coagulant in the finally obtained acrylic polymer fall within the above range.
[0060] The solidification temperature is not particularly limited, but is preferably 50°C or higher and 90°C or lower, and more preferably 60°C or higher and 80°C or lower.
[0061] <<Cleaning process>> In the washing step, the water-containing crumbs obtained in the coagulation step are washed. By washing the water-containing crumbs, the amount of remaining components (coagulant, etc.) other than the acrylic polymer can be reduced.
[0062] The washing method is not particularly limited, but includes a method in which water is used as a washing liquid and the water-containing crumb is mixed with the added water to wash the crumb. The temperature during washing is not particularly limited, but is preferably 5°C to 60°C, more preferably 10°C to 50°C. The mixing time is not particularly limited, but is preferably 1 minute to 60 minutes, more preferably 2 minutes to 30 minutes.
[0063] The amount of water added to the hydrous crumbs during washing is not particularly limited, but from the viewpoint of effectively reducing the content (residual amount) of coagulant in the final binder composition, the amount of water added is preferably 150 parts by mass or more and 9,800 parts by mass or less, more preferably 150 parts by mass or more and 1,800 parts by mass or less, relative to 100 parts by mass of the acrylic polymer contained in the hydrous crumbs.
[0064] The number of times of washing with water is not particularly limited, and may be one time, but from the viewpoint of reducing the content (residual amount) of the coagulant in the binder composition finally obtained, it is preferably 2 to 10 times, more preferably 3 to 8 times. From the viewpoint of reducing the content (residual amount) of the coagulant in the binder composition finally obtained, it is preferable to wash with water many times, but even if washing is performed beyond the above range, the effect of removing the coagulant is small, while the number of steps increases, which increases the influence of the decrease in production efficiency. Furthermore, in order to further reduce the content (residual amount) of the coagulant, a completely different process is required, such as dissolving it in an organic solvent such as toluene once and then coagulating it by a method such as putting it into methanol. Therefore, it is preferable to perform the coagulation washing method, which has good industrial production efficiency, and it is preferable to set the number of times of washing with water to the above range. In the washing step, after washing with water, acid washing may be further performed using an acid as a washing liquid.
[0065] <<Drying process>> In the drying step, the water-containing crumbs that have been subjected to the above-mentioned washing step are dried to obtain a solidified and dried product containing the acrylic polymer and the coagulant. The drying method usable in the drying step is not particularly limited, but for example, a dryer such as a screw-type extruder, a kneader-type dryer, an expander dryer, a hot air dryer, or a reduced pressure dryer can be used for drying. A drying method combining these may also be used. Furthermore, before drying in the drying step, the water-containing crumb may be filtered using a sieve such as a rotary screen or a vibration screen; a centrifugal dehydrator; or the like, as necessary. Here, the drying temperature in the drying step is not particularly limited and varies depending on the dryer used for drying. For example, when a hot air dryer is used, the drying temperature is preferably 80°C or higher and 200°C or lower, and more preferably 100°C or higher and 170°C or lower.
[0066] <<Other processes>> Other steps that may be included in the method for producing the binder composition described above are not particularly limited. For example, the solidified and dried product obtained in the drying step described above may be used as the binder composition as it is, or after the drying step, a step of adding an organic solvent to the solidified and dried product (organic solvent adding step) may be carried out, and a liquid composition containing an acrylic polymer, a coagulant, and an organic solvent may be used as the binder composition.
[0067] (Slurry composition for all-solid-state secondary battery) The slurry composition of the present invention includes a binder composition containing a solid electrolyte and the above-mentioned organic solvent. In other words, the slurry composition of the present invention is a composition in which at least a solid electrolyte, the above-mentioned acrylic polymer, and the above-mentioned coagulant are dispersed and / or dissolved in an organic solvent. Since the slurry composition of the present invention is prepared using the above-mentioned binder composition of the present invention, the slurry composition can form a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics.
[0068] Incidentally, when the slurry composition for an all-solid-state secondary battery of the present invention is used for forming an electrode mixture layer (i.e., when it is a slurry composition for an all-solid-state secondary battery electrode), it usually contains at least a solid electrolyte, an acrylic polymer, a coagulant, and an organic solvent. Furthermore, when the slurry composition for an all-solid-state secondary battery of the present invention is used for forming a solid electrolyte layer (i.e., when it is a slurry composition for a solid electrolyte layer of an all-solid-state secondary battery), it usually does not contain an electrode active material, and contains at least a solid electrolyte, an acrylic polymer, a coagulant, and an organic solvent.
[0069] <Solid electrolyte> As the solid electrolyte, either an inorganic solid electrolyte or an organic solid electrolyte can be used, but the inorganic solid electrolyte is preferably used.
[0070] The inorganic solid electrolyte is not particularly limited, and a crystalline inorganic ion conductor, an amorphous inorganic ion conductor, or a mixture thereof can be used. For example, when the all-solid-state secondary battery is an all-solid-state lithium ion secondary battery, the inorganic solid electrolyte can usually be a crystalline inorganic lithium ion conductor, an amorphous inorganic lithium ion conductor, or a mixture thereof. Among them, from the viewpoint of improving battery performance such as high-temperature storage characteristics, it is preferable that the inorganic solid electrolyte contains a sulfide-based inorganic solid electrolyte. In the following, a case where the slurry composition for an all-solid-state secondary battery is a slurry composition for an all-solid-state lithium-ion secondary battery will be described as an example, but the present invention is not limited to the following example.
[0071] As crystalline inorganic lithium ion conductors, Li3N, LISICON (Li 14 Zn(GeO4)4), perovskite-type Li 0.5 La 0.5 TiO3, garnet type Li7La3Zr2O 10 , LIPON (Li 3+y PO 4-x N x ), Thio-LISICON (Li 3.25 Ge0.25 P 0.75 S4) etc. The above-mentioned crystalline inorganic lithium ion conductors can be used alone or in combination of two or more kinds.
[0072] The amorphous inorganic lithium ion conductor is not particularly limited as long as it contains sulfur atoms and has ion conductivity, and examples thereof include glass Li-Si-SO, Li-PS, and those made using a raw material composition containing Li2S and a sulfide of an element of Groups 13 to 15 of the periodic table. Here, examples of the elements of Groups 13 to 15 include Al, Si, Ge, P, As, and Sb. Examples of sulfides of elements of Groups 13 to 15 include Al2S3, SiS2, GeS2, P2S3, P2S5, As2S3, and Sb2S3. Examples of methods for synthesizing amorphous inorganic lithium ion conductors using raw material compositions include amorphization methods such as mechanical milling and melt quenching. Examples of amorphous inorganic lithium ion conductors obtained using raw material compositions containing Li2S and sulfides of elements of Groups 13 to 15 of the periodic table include Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-Al2S3, and Li2S-P2S5 is more preferred. The amorphous inorganic lithium ion conductors described above can be used alone or in combination of two or more kinds.
[0073] Among the above, from the viewpoint of improving battery performance such as high-temperature storage characteristics, an amorphous inorganic lithium ion conductor is preferable as the inorganic solid electrolyte for an all-solid-state lithium ion secondary battery, and an amorphous sulfide containing Li and P is more preferable. Since an amorphous sulfide containing Li and P has high lithium ion conductivity, using it as an inorganic solid electrolyte can reduce the internal resistance of the battery and improve the output characteristics.
[0074] In addition, from the viewpoint of reducing the internal resistance of the battery and improving the output characteristics, the amorphous sulfide containing Li and P is more preferably a sulfide glass made of Li2S and P2S5, and is particularly preferably a sulfide glass manufactured from a mixed raw material of Li2S and P2S5 having a molar ratio of Li2S:P2S5 of 65:35 to 85:15. In addition, the amorphous sulfide containing Li and P is preferably a sulfide glass ceramic obtained by reacting a mixed raw material of Li2S and P2S5 having a molar ratio of Li2S:P2S5 of 65:35 to 85:15 by a mechanochemical method. In addition, from the viewpoint of maintaining a high lithium ion conductivity, the mixed raw material preferably has a molar ratio of Li2S:P2S5 of 68:32 to 80:20.
[0075] In addition to the Li2S and P2S5, the inorganic solid electrolyte may contain at least one sulfide selected from the group consisting of Al2S3, B2S3 and SiS2 as a starting material to the extent that the ion conductivity is not reduced. The addition of such a sulfide can stabilize the glass component in the inorganic solid electrolyte. Similarly, the inorganic solid electrolyte may contain at least one lithium ortho-oxo acid selected from the group consisting of Li3PO4, Li4SiO4, Li4GeO4, Li3BO3 and Li3AlO3, in addition to Li2S and P2S5. When such a lithium ortho-oxo acid is contained, the glass component in the inorganic solid electrolyte can be stabilized.
[0076] <Acrylic polymer> The acrylic polymer is one contained in the binder composition, and specifically, the one exemplified in the above section "Binder composition for all-solid-state secondary battery" can be used. In the slurry composition, the binder may be dissolved in the organic solvent, or may be dispersed in the form of particles, for example, without being dissolved in the organic solvent.
[0077] Here, the amount of the acrylic polymer contained in the slurry composition for all-solid-state secondary batteries is not particularly limited, and is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.2 parts by mass or more, and preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less per 100 parts by mass of the solid electrolyte. If the amount of the acrylic polymer is equal to or more than the lower limit, the solid electrolyte-containing layer can be formed well. Also, if the amount of the acrylic polymer is equal to or less than the upper limit, the ion conductivity of the solid electrolyte-containing layer can be suppressed from decreasing.
[0078] <Coagulant> The coagulant is one contained in the binder composition, and specifically, the ones exemplified in the above section "Binder composition for all-solid-state secondary battery" can be used. As described above, the coagulant is derived from the binder composition, and therefore the content of the coagulant relative to the acrylic polymer in the slurry composition of the present invention is the same as the content of the coagulant relative to the acrylic polymer in the binder composition of the present invention described above.
[0079] <Organic solvent> As the organic solvent, those exemplified in the above section "Binder composition for all-solid-state secondary battery" can be used. The organic solvent contained in the slurry composition may be only that contained in the binder composition, or may be added separately during preparation of the slurry composition.
[0080] <Electrode active material> Here, the electrode active material is a material that transfers electrons at the electrode of the all-solid-state secondary battery. For example, when the all-solid-state secondary battery is an all-solid-state lithium ion secondary battery, the electrode active material is usually a material that can absorb and release lithium. In the following, a case where the slurry composition for an all-solid-state secondary battery is a slurry composition for an all-solid-state lithium-ion secondary battery will be described as an example, but the present invention is not limited to the following example.
[0081] The positive electrode active material for the all-solid-state lithium ion secondary battery is not particularly limited, and examples thereof include a positive electrode active material made of an inorganic compound and a positive electrode active material made of an organic compound. The positive electrode active material may be a mixture of an inorganic compound and an organic compound.
[0082] Examples of the positive electrode active material made of an inorganic compound include transition metal oxides, composite oxides of lithium and transition metals (lithium-containing composite metal oxides), and transition metal sulfides. Examples of the transition metals include Fe, Co, Ni, and Mn. Specific examples of inorganic compounds used in the positive electrode active material include lithium-containing composite metal oxides such as LiCoO2 (lithium cobalt oxide), LiNiO2, LiMnO2, LiMn2O4, LiFePO4, and LiFeVO4; transition metal sulfides such as TiS2, TiS3, and amorphous MoS2; Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, and V6O 13 and the like. These compounds may be partially element-substituted. The positive electrode active materials made of the inorganic compounds described above can be used alone or in combination of two or more kinds.
[0083] Examples of the positive electrode active material made of an organic compound include polyaniline, polypyrrole, polyacene, disulfide-based compounds, polysulfide-based compounds, and N-fluoropyridinium salts. The positive electrode active materials made of the above-mentioned organic compounds can be used alone or in combination of two or more kinds.
[0084] In addition, examples of the negative electrode active material for the all-solid-state lithium-ion secondary battery include carbon allotropes such as graphite and coke. The negative electrode active material made of carbon allotropes can also be used in the form of a mixture or coating with metals, metal salts, oxides, etc. In addition, examples of the negative electrode active material that can be used include oxides or sulfates of silicon, tin, zinc, manganese, iron, nickel, etc.; metallic lithium; lithium alloys such as Li-Al, Li-Bi-Cd, and Li-Sn-Cd; lithium transition metal nitrides; and silicone. The above-mentioned negative electrode active materials can be used alone or in combination of two or more kinds.
[0085] <Optional ingredients> The slurry composition of the present invention may contain components other than the above-mentioned solid electrolyte, acrylic polymer, coagulant, organic solvent, and electrode active material. Examples of such optional components include known binders other than acrylic polymers, conductive materials, dispersants, leveling agents, antifoaming agents, and reinforcing materials. Furthermore, for example, when the all-solid-state secondary battery is an all-solid-state lithium ion secondary battery, examples of other components include lithium salts. These other components are not particularly limited as long as they do not affect the battery reaction.
[0086] As known binders other than acrylic polymers, polymer compounds such as fluorine-based polymers, diene-based polymers, and nitrile-based polymers can be used. These polymer compounds can be used alone or in combination. Here, as the fluorine-based polymers, diene-based polymers, and nitrile-based polymers, for example, the fluorine-based polymers, diene-based polymers, and nitrile-based polymers described in JP-A-2012-243476 can be used.
[0087] The conductive material is for ensuring electrical contact between electrode active materials in the electrode mixture layer formed using the slurry composition for all-solid-state secondary batteries (slurry composition for all-solid-state secondary battery electrodes). Examples of the conductive material include carbon black (e.g., acetylene black, Ketjen Black (registered trademark), furnace black, etc.), single-layer or multi-layer carbon nanotubes (multi-layer carbon nanotubes include cup-stack type), carbon nanohorns, vapor-grown carbon fibers, milled carbon fibers obtained by crushing polymer fibers after firing, single-layer or multi-layer graphene, conductive carbon materials such as carbon nonwoven fabric sheets obtained by firing nonwoven fabrics made of polymer fibers, and fibers or foils of various metals. These may be used alone or in combination of two or more.
[0088] The lithium salt, dispersant, leveling agent, defoamer, and reinforcing material are not particularly limited, and for example, those described in JP-A-2012-243476 can be used.
[0089] <Method for producing slurry composition> The method for preparing the above-mentioned slurry composition of the present invention is not particularly limited, but the slurry composition can be obtained by mixing the binder composition prepared by the procedure described above in the section "Method for Producing Binder Composition", the solid electrolyte, and the electrode active material and any optional components added as necessary in the presence of an organic solvent.
[0090] (Solid electrolyte containing layer) The solid electrolyte-containing layer of the present invention is a layer that contains a solid electrolyte. Examples of the solid electrolyte-containing layer include an electrode mixture layer (positive electrode mixture layer, negative electrode mixture layer) that transfers electrons via an electrochemical reaction, and a solid electrolyte layer provided between a positive electrode mixture layer and a negative electrode mixture layer that face each other. The solid electrolyte-containing layer of the present invention is formed using the above-mentioned slurry composition for all-solid-state secondary batteries, and can be formed, for example, by applying the above-mentioned slurry composition to the surface of a suitable substrate to form a coating film, and then drying the formed coating film. That is, the solid electrolyte-containing layer of the present invention is made of the dried product of the above-mentioned slurry composition, and usually contains at least a solid electrolyte, an acrylic polymer, and a coagulant. Note that each component contained in the solid electrolyte-containing layer is contained in the above-mentioned slurry composition, and the content ratio of those components is usually equal to the content ratio in the above-mentioned slurry composition.
[0091] Furthermore, since the solid electrolyte-containing layer of the present invention is formed from the slurry composition for an all-solid-state secondary battery of the present invention, it is possible to make the all-solid-state secondary battery exhibit excellent high-temperature storage characteristics.
[0092] <Base material> Here, there is no limitation on the substrate to which the slurry composition is applied, and for example, a coating film of the slurry composition may be formed on the surface of a release substrate, the coating film may be dried to form a solid electrolyte-containing layer, and the release substrate may be peeled off from the solid electrolyte-containing layer. In this way, the solid electrolyte-containing layer peeled off from the release substrate may be used as a free-standing film to form battery components (e.g., electrodes, solid electrolyte layers, etc.) of an all-solid-state secondary battery. However, from the viewpoint of omitting the step of peeling off the solid electrolyte-containing layer and increasing the manufacturing efficiency of the battery component, it is preferable to use a current collector or an electrode as the substrate. Specifically, when preparing the electrode mixture layer, it is preferable to apply the slurry composition onto a current collector as the substrate. Also, when preparing the solid electrolyte layer, it is preferable to apply the slurry composition onto an electrode (positive electrode or negative electrode).
[0093] <<Current collector>> As the current collector, a material having electrical conductivity and electrochemical durability is used. Specifically, as the current collector, for example, a current collector made of iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. Among them, as the current collector used for the negative electrode, copper foil is particularly preferable. Also, as the current collector used for the positive electrode, aluminum foil is particularly preferable. Note that, the above-mentioned materials may be used alone or in combination of two or more kinds in any ratio.
[0094] <<Electrode>> The electrodes (positive and negative electrodes) are not particularly limited, but may be an electrode in which an electrode mixture layer containing an electrode active material, a solid electrolyte, and a binder is formed on the above-mentioned current collector. The electrode active material, solid electrolyte, and binder contained in the electrode mixture layer in the electrode are not particularly limited, and known materials can be used. The electrode mixture layer in the electrode may correspond to the solid electrolyte-containing layer of the present invention.
[0095] <Method of forming solid electrolyte-containing layer> The following methods can be used to form a solid electrolyte-containing layer on a substrate such as the current collector or electrode. 1) A method in which the slurry composition of the present invention is applied to the surface of a substrate (in the case of an electrode, the surface on the electrode mixture layer side; the same applies below) and then dried; 2) a method of immersing a substrate in the slurry composition of the present invention and then drying the substrate; and 3) A method in which the slurry composition of the present invention is applied onto a release substrate, followed by drying to produce a solid electrolyte-containing layer, and the resulting solid electrolyte-containing layer is transferred onto the surface of an electrode or the like. Among these, the method 1) is particularly preferred because it is easy to control the thickness of the solid electrolyte-containing layer. The method 1) specifically includes a step of applying a slurry composition onto a substrate (application step) and a step of drying the slurry composition applied onto the substrate to form a solid electrolyte-containing layer (solid electrolyte-containing layer formation step).
[0096] <<Coating process>> In the coating step, the method for coating the slurry composition on the substrate is not particularly limited, and examples thereof include a doctor blade method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method.
[0097] <<Solid electrolyte-containing layer formation process>> In the solid electrolyte-containing layer forming step, the method for drying the slurry composition on the substrate is not particularly limited and may be any known method. Examples of the drying method include drying with warm air, hot air, or low-humidity air, vacuum drying, and drying with infrared rays or electron beams. In addition, when the solid electrolyte-containing layer is an electrode mixture layer, it is preferable to perform a pressing treatment using a roll press or the like after drying. By performing the pressing treatment, the obtained electrode mixture layer can be further densified.
[0098] (electrode) An electrode obtained by forming an electrode mixture layer on a current collector using the slurry composition for an all-solid-state secondary battery of the present invention has an electrode mixture layer containing at least a solid electrolyte, an acrylic polymer, a coagulant, and an electrode active material, and can provide the all-solid-state secondary battery with excellent high-temperature storage characteristics.
[0099] (solid electrolyte layer) In addition, the solid electrolyte layer formed using the slurry composition for an all-solid-state secondary battery of the present invention contains at least a solid electrolyte, an acrylic polymer, and a coagulant, and can provide the all-solid-state secondary battery with excellent high-temperature storage characteristics.
[0100] (All-solid-state secondary battery) The all-solid-state secondary battery of the present invention usually has a positive electrode, a solid electrolyte layer, and a negative electrode, and is characterized in that at least one of the positive electrode composite layer of the positive electrode, the negative electrode composite layer of the negative electrode, and the solid electrolyte layer is the solid electrolyte-containing layer of the present invention. That is, the all-solid-state secondary battery of the present invention has at least one of a positive electrode having a positive electrode composite layer formed using the slurry composition for the positive electrode of the all-solid-state secondary battery as the slurry composition for the all-solid-state secondary battery of the present invention, a negative electrode having a negative electrode composite layer formed using the slurry composition for the negative electrode of the all-solid-state secondary battery as the slurry composition for the all-solid-state secondary battery of the present invention, and a solid electrolyte layer formed using the slurry composition for the solid electrolyte layer of the all-solid-state secondary battery as the slurry composition for the all-solid-state secondary battery of the present invention. The all-solid-state secondary battery of the present invention is provided with the solid electrolyte-containing layer of the present invention, and therefore has excellent battery performance such as high-temperature storage characteristics.
[0101] Here, the all-solid-state secondary battery electrode having an electrode mixture layer that does not correspond to the solid electrolyte-containing layer of the present invention and that can be used in the all-solid-state secondary battery of the present invention is not particularly limited as long as it has an electrode mixture layer that does not correspond to the solid electrolyte-containing layer of the present invention, and any all-solid-state secondary battery electrode can be used.
[0102] In addition, the solid electrolyte layer that does not correspond to the solid electrolyte-containing layer of the present invention and that can be used in the all-solid-state secondary battery of the present invention is not particularly limited, and any solid electrolyte layer such as the solid electrolyte layers described in, for example, JP-A-2012-243476, JP-A-2013-143299, and JP-A-2016-143614 can be used.
[0103] The all-solid-state secondary battery of the present invention can be obtained by laminating a positive electrode and a negative electrode so that the positive electrode composite layer of the positive electrode and the negative electrode composite layer of the negative electrode face each other through a solid electrolyte layer, optionally applying pressure to obtain a laminate, and then placing the laminate in a battery container as is or after rolling or folding, depending on the shape of the battery, and sealing the battery. If necessary, an expand metal, a fuse, an overcurrent prevention element such as a PTC element, a lead plate, etc. can be placed in the battery container to prevent pressure rise inside the battery and overcharging and discharging. The shape of the battery may be any of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc. EXAMPLES
[0104] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In the examples and comparative examples, the content of the coagulant in the binder composition, the recovery rate of the acrylic polymer, and the high-temperature storage characteristics of the all-solid-state secondary battery were measured and evaluated by the following methods.
[0105] <Coagulant content> The binder composition (solidified and dried product) was subjected to elemental analysis by inductively coupled plasma atomic emission spectroscopy (ICP-AES) to measure the content of the coagulant in the solidified and dried product. Specifically, the content ratio of the elements constituting the used coagulant in the binder composition was obtained by elemental analysis, and the content of the coagulant was calculated from the obtained content ratio. <Acrylic polymer recovery rate> The ratio of the amount of the acrylic polymer that could be recovered as the binder composition to the theoretical yield estimated from the total amount of charged monomers and the polymerization conversion rate was calculated as the recovery rate (%). <High temperature storage characteristics> The capacity of the fabricated all-solid-state secondary battery was measured and designated as the initial capacity C0. Then, the all-solid-state secondary battery after the initial capacity measurement was stored in a thermostatic chamber at 80° C. for 100 hours, 500 hours, and 1000 hours, and the capacity C after 100 hours of storage was measured. 100, Capacity after 500 hours storage C 500 , Capacity after 1000 hours storage C 1000 The capacity retention rate (C 100 / C0×100%, C 500 / C0×100%, C 1000 The higher the capacity retention rate, the better the high-temperature storage characteristics of the all-solid-state secondary battery. The capacity of the all-solid-state secondary battery was measured as follows. The all-solid-state secondary battery was subjected to a charge-discharge cycle in which it was charged at a constant current of 0.1 C at 25° C. until the battery reached 4.2 V, then charged at a constant voltage, and discharged again at a constant current of 0.1 C until the battery reached 3.0 V. Five charge-discharge cycles were performed, and the discharge capacity at the fifth cycle was recorded as the capacity.
[0106] Example 1 <Preparation of Binder Composition> <<Emulsion polymerization process>> A mixing vessel equipped with a homomixer was charged with 47.701 parts of pure water, 49.3 parts of ethyl acrylate and 49.3 parts of n-butyl acrylate as (meth)acrylic acid ester monomers (the ratio of ethyl acrylate to the total monomers was 50% and 50%, respectively), 0.709 parts of sodium lauryl sulfate (trade name "EMAL 2FG", manufactured by Kao Corporation) as an anionic surfactant, and 1.82 parts of polyoxyethylene dodecyl ether (trade name "EMULGEN 105", manufactured by Kao Corporation) as a nonionic surfactant, and the mixture was stirred to obtain a monomer emulsion. Next, 170.853 parts of pure water and 2.98 parts of the monomer emulsion obtained above were added to a polymerization reaction tank equipped with a thermometer and a stirrer, and cooled to a temperature of 12 ° C. under a nitrogen stream. Next, 145.85 parts of the monomer emulsion obtained above, 0.00033 parts of ferrous sulfate and 0.264 parts of sodium ascorbate as reducing agents, and 7.72 parts of a 2.85% aqueous potassium persulfate solution (0.22 parts as the amount of potassium persulfate) as a polymerization initiator were continuously dropped into the polymerization reaction tank over 3 hours. Thereafter, the reaction was continued for 1 hour while maintaining the temperature in the polymerization reaction tank at 23 ° C., and it was confirmed that the polymerization conversion rate reached 95%, and hydroquinone was added as a polymerization terminator to terminate the polymerization reaction, thereby obtaining an emulsion polymerization liquid. <<Coagulation process>> The emulsion polymerization liquid obtained in the emulsion polymerization step was transferred to a coagulation tank, and 60 parts of industrial water was added to 100 parts of this emulsion polymerization liquid to obtain a mixed liquid. After the mixed liquid was heated to 85°C, 3.3 parts of sodium sulfate (11 parts to 100 parts of the acrylic polymer contained in the mixed liquid) was continuously added as a coagulant while stirring at a temperature of 85°C, thereby coagulating the acrylic polymer and obtaining water-containing crumbs of the acrylic polymer. <<Cleaning process>> The hydrous crumbs were washed with water by adding 160 parts of industrial water to 100 parts of solids of the hydrous crumbs obtained in the washing step, stirring the mixture at 15°C for 5 minutes in a coagulation tank, and then draining the water from the coagulation tank. This washing was repeated a total of four times. <<Drying process>> The water-containing crumbs washed in the washing step were dried in a hot air dryer at 110°C for 1 hour to obtain a solidified and dried product. The solidified and dried product (binder composition) was used to measure the content of the coagulant and the recovery rate of the acrylic polymer. The results are shown in Table 1. Furthermore, it was confirmed by NMR measurement that the acrylic polymer contained 50% ethyl acrylate units and 50% n-butyl acrylate units. It was also confirmed that in other examples and comparative examples, the proportion of each monomer in the total monomers used to prepare the acrylic polymer was consistent with the proportion of the monomer units derived from that monomer in the acrylic polymer. <<Organic solvent addition process>> The solidified and dried product obtained in the drying step was dissolved in xylene, and then subjected to a heating and decompression treatment using an evaporator to prepare a liquid composition (water content: 82 ppm by mass, solid content concentration: 7%) as a binder composition. <Preparation of Slurry Composition for Solid Electrolyte Layer> In a glove box under an argon gas atmosphere (water concentration 0.6 mass ppm, oxygen concentration 1.8 mass ppm), 100 parts of sulfide glass (Li2S / P2S5=70mol% / 30mol%, number average particle size: 1.2μm, cumulative 90% particle size: 2.1μm) consisting of Li2S and P2S5 as a solid electrolyte was mixed with 2 parts (solid content equivalent) of the binder composition obtained as described above, and further, xylene was added as an organic solvent to adjust the solid content concentration to 65 mass%. Then, the mixture was mixed with a planetary mixer to prepare a slurry composition for a solid electrolyte layer. <Preparation of Positive Electrode Slurry Composition> 100 parts of lithium cobalt oxide (average particle size: 11.5 μm) as a positive electrode active material, 150 parts of sulfide glass (Li2S / P2S5=70mol% / 30mol%, number average particle size: 0.4 μm) consisting of Li2S and P2S5 as a solid electrolyte, 13 parts of acetylene black as a conductive agent, and 2 parts (solid content equivalent) of the binder composition obtained as described above were mixed, and then xylene was added as an organic solvent to adjust the solid content concentration to 78%, and then mixed with a planetary mixer for 60 minutes. After that, the solid content concentration was further adjusted to 74% with xylene and then mixed for 10 minutes to prepare a positive electrode slurry composition. <Preparation of Slurry Composition for Negative Electrode> A negative electrode slurry composition was prepared by mixing 100 parts of graphite (average particle size: 20 μm) as a negative electrode active material, 50 parts of sulfide glass consisting of Li2S and P2S5 (Li2S / P2S5=70 mol% / 30 mol%, number average particle size: 0.4 μm) as a solid electrolyte, and 2 parts (equivalent to the solid content) of the binder composition obtained as described above. Xylene was further added as an organic solvent to adjust the solid content to 60%, and then mixing with a planetary mixer. <Manufacturing of all-solid-state secondary batteries> The positive electrode slurry composition was applied to the surface of a current collector (aluminum foil, thickness: 20 μm) and dried (110° C., 20 minutes) to form a positive electrode composite layer with a thickness of 50 μm, thereby obtaining a positive electrode. The negative electrode slurry composition was applied to the surface of another current collector (copper foil, thickness: 18 μm) and dried (110° C., 20 minutes) to form a negative electrode composite layer with a thickness of 30 μm, thereby obtaining a negative electrode. Next, the above-mentioned slurry composition for solid electrolyte layer was applied to the surface of the positive electrode mixture layer of the above-mentioned positive electrode and dried (110°C, 10 minutes) to form a solid electrolyte layer with a thickness of 18 µm, thereby obtaining a positive electrode with a solid electrolyte layer. The above-mentioned positive electrode with solid electrolyte layer and the negative electrode were bonded together so that the solid electrolyte layer of the positive electrode with solid electrolyte layer and the negative electrode composite layer of the negative electrode were in contact with each other, and pressed to obtain an all-solid-state secondary battery. The thickness of the solid electrolyte layer of the all-solid-state secondary battery after pressing was 11 μm. The high-temperature storage characteristics of this all-solid-state secondary battery were evaluated. The results are shown in Table 1.
[0107] Example 2 In preparing the binder composition, 2-ethylhexyl acrylate was further used as a monomer in the emulsion polymerization process (the ratio of ethyl acrylate to the total monomers was 48%, n-butyl acrylate to the total monomers was 45%, and 2-ethylhexyl acrylate to the total monomers was 7%), magnesium sulfate was used as a coagulant instead of sodium sulfate in the coagulation process, and the amount of industrial water added in the washing process was changed to 150 parts. In the same manner as in Example 1, except for this, binder compositions (water content: 75 mass ppm, solid content concentration: 7.5%), various slurry compositions, and all-solid-state secondary batteries were manufactured, and measurements and evaluations were performed. The results are shown in Table 1.
[0108] Example 3 Except for changing the number of water washes in the washing step to one time during the preparation of the binder composition, the binder composition (water content: 58 mass ppm, solid content concentration: 7.5%), various slurry compositions, and all-solid secondary batteries were produced, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0109] Example 4 In preparing the binder composition, the amount of ethyl acrylate and n-butyl acrylate used as monomers in the emulsion polymerization process was changed so that the ratio of the total monomers was 55% and 45%, respectively, the amount of sodium sulfate used as a coagulant in the coagulation process was changed to 1.2 parts, and the amount of industrial water added in the washing process was changed to 200 parts. Except for this, the binder composition (water content: 88 mass ppm, solid content concentration: 7.2%), various slurry compositions, and all-solid secondary batteries were manufactured, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0110] Example 5 Except for using diisobutyl ketone instead of xylene when preparing the binder composition, the slurry composition for the solid electrolyte layer, the slurry composition for the positive electrode, and the slurry composition for the negative electrode, the binder composition (water content: 95 mass ppm, solid content concentration: 8.2%), various slurry compositions, and all-solid secondary batteries were manufactured, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0111] Example 6 Except for using n-butyl ether instead of xylene when preparing the binder composition, the slurry composition for the solid electrolyte layer, the slurry composition for the positive electrode, and the slurry composition for the negative electrode, the binder composition (water content: 48 mass ppm, solid content concentration: 7.5%), various slurry compositions, and all-solid secondary batteries were manufactured, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0112] Comparative Example 1 Except for changing the amount of sodium sulfate as a coagulant to 15 parts in the coagulation step during the preparation of the binder composition, the binder composition (water content: 68 mass ppm, solid content concentration: 7.4%), various slurry compositions, and all-solid secondary batteries were manufactured, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0113] Comparative Example 2 Except for not carrying out the washing step during the preparation of the binder composition and subjecting the water-containing crumbs obtained in the solidification step directly to the drying step, the binder composition (water content: 58 mass ppm, solid content concentration: 7.5%), various slurry compositions, and all-solid secondary batteries were manufactured, measured, and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0114] Comparative Example 3 A binder composition (water content: 86 ppm by mass, solid content: 7.6%) was prepared in the same manner as in Example 1, except that the amount of sodium sulfate used as a coagulant in the coagulation step was changed to 0.1 parts during the preparation of the binder composition. However, since the amount of the coagulant was insufficient and coagulation was insufficient, the recovery rate of the acrylic polymer was extremely low (45%), and no slurry compositions or all-solid-state secondary batteries were produced.
[0115] In addition, in Tables 1 and 2 shown below, "XY" indicates xylene, "DIK" stands for diisobutyl ketone, "BE" refers to n-butyl ether.
[0116] [Table 1]
[0117] [Table 2]
[0118] From Tables 1 and 2, it can be seen that in Examples 1 to 6, in which a binder composition containing an acrylic polymer and a coagulant and in which the content of the coagulant is within a predetermined range is used for preparing the solid electrolyte-containing layer, all-solid-state secondary batteries having excellent high-temperature storage characteristics are obtained. On the other hand, from Table 2, it can be seen that in Comparative Examples 1 and 2 in which the binder composition having a coagulant content exceeding a predetermined upper limit was used for preparing the solid electrolyte-containing layer, the high-temperature storage characteristics of the all-solid-state secondary battery were impaired. Furthermore, from Table 2, it can be seen that in Comparative Example 3, in which the amount of coagulant used in preparing the binder composition was reduced to make the content of the coagulant contained in the binder composition less than the predetermined lower limit, the recovery rate of the acrylic polymer was significantly reduced as described above. [Industrial Applicability]
[0119] According to the present invention, it is possible to provide a binder composition for an all-solid-state secondary battery and a slurry composition for an all-solid-state secondary battery, which are capable of forming a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics. Moreover, according to the present invention, it is possible to provide a solid electrolyte-containing layer that can provide an all-solid-state secondary battery with excellent high-temperature storage characteristics, and an all-solid-state secondary battery having excellent high-temperature storage characteristics.
Claims
1. A binder composition for an all-solid-state secondary battery (excluding binder compositions containing an antioxidant and a lubricant), comprising an acrylic polymer, a coagulant in an amount of 500 ppm by mass or more and 5,000 ppm by mass or less relative to the acrylic polymer, and an organic solvent.
2. The binder composition for an all-solid-state secondary battery according to claim 1 , wherein the coagulant is a monovalent or more and trivalent or less metal sulfate.
3. The binder composition for an all-solid-state secondary battery according to claim 1 or 2, wherein the acrylic polymer is an emulsion polymer.
4. A slurry composition for an all-solid-state secondary battery, comprising a solid electrolyte and the binder composition for an all-solid-state secondary battery according to claim 3.
5. The slurry composition for an all-solid-state secondary battery according to claim 4 , wherein the solid electrolyte is an inorganic solid electrolyte.
6. The slurry composition for an all-solid-state secondary battery according to claim 4 or 5, further comprising an electrode active material.
7. A solid electrolyte-containing layer comprising a dried slurry composition for an all-solid secondary battery according to any one of claims 4 to 6.
8. An all-solid-state secondary battery comprising the solid electrolyte-containing layer according to claim 7.
Citation Information
Patent Citations
Method for manufacturing polymer
JP2003342321A
Composition for electrochemical element electrode
JP2006269827A
Slurry for secondary battery
JP2014056813A
Positive electrode for lithium ion secondary battery and lithium ion secondary battery
JP2014203804A
Composite particle for electrochemical element electrode, electrochemical element electrode, electrochemical element, and method for manufacturing composite particle for electrochemical element electrode and electrochemical element electrode
JP2016046226A