Silicon wafer cleaning method and silicon wafer manufacturing method

The cleaning method using SC1, SC2, or ozone water cleaning with controlled ammonium hydroxide and hydrogen peroxide concentrations, followed by CMP polishing, addresses the issue of silicon wafer transport defects by achieving the desired roughness and maintaining quality, enhancing processing stability.

JP7582057B2Active Publication Date: 2024-11-13SHIN ETSU HANDOTAI CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021079337
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-09
Filing Date
2021-05-07
Publication Date
2024-11-13
Estimated Expiration
2041-05-07

AI Technical Summary

Technical Problem

Silicon wafers with smooth surfaces face challenges during processing steps due to increased contact area with chucks, leading to transportation failures, while excessively rough surfaces deteriorate quality with chuck marks. Existing cleaning methods like RCA cleaning worsen surface roughness, and there is a need for a method to selectively roughen one side of the wafer to improve transportability without compromising quality.

Method used

A cleaning method involving SC1, SC2, or ozone water cleaning followed by a diluted ammonium hydroxide or ammonium hydroxide and hydrogen peroxide solution with specific concentrations to form an oxide film, then etching the surfaces to achieve a roughness index of 0.3 nm to 5.5 nm and Haze value of 50 ppm to 1900 ppm, followed by CMP polishing to maintain the opposite side as a mirror finish.

Benefits of technology

The method effectively roughens the silicon wafer surfaces to enhance transportability by reducing chucking defects while maintaining excellent quality, ensuring stable processing and manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582057000008
    Figure 0007582057000008
  • Figure 0007582057000009
    Figure 0007582057000009
  • Figure 0007582057000010
    Figure 0007582057000010
Patent Text Reader

Abstract

To provide a cleaning method capable of roughening front and rear faces of a silicon wafer, to provide a method of manufacturing a silicon wafer capable of obtaining a silicon wafer only whose one side face is selectively roughened, and to provide a silicon wafer capable of reducing conveyance failures during a processing step.SOLUTION: Provided is a cleaning method of roughening a silicon wafer. An oxide film is formed on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning. Front and rear faces of the silicon wafer are roughened by cleaning the silicon wafer formed with the oxide film with any one of an ammonium hydroxide diluted water solution having an ammonium hydroxide concentration equal to or less than 0.051 mass% or a diluted water solution containing ammonium hydroxide and hydrogen peroxide water and having an ammonium hydroxide concentration equal to or less than 0.051 mass% and a hydrogen peroxide concentration equal to or less than 0.2 mass% and four times or less the ammonium hydroxide concentration.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a silicon wafer cleaning method capable of roughening the front and back surfaces of a semiconductor silicon wafer, a silicon wafer cleaning method capable of roughening the front and back surfaces or the back surface of a semiconductor silicon wafer, a silicon wafer manufacturing method, and a silicon wafer. [Background technology]

[0002] The manufacturing process for silicon wafers for semiconductor devices consists of a single crystal manufacturing process in which a single crystal ingot is grown using the Czochralski (CZ) method or other methods, and a wafer processing process in which this single crystal ingot is sliced ​​and processed to a mirror finish.To add further value, the process may also include an annealing process in which heat treatment is performed and an epitaxial growth process in which an epitaxial layer is formed.

[0003] The process of processing the wafer to a mirror finish consists of the DSP (double-sided polishing) process and the subsequent CMP (single-sided polishing) process. More specifically, from the perspective of particle quality and transportation, DSP processed wafers are not dried, but are cleaned as necessary and then stored underwater before being transported to the CMP process. Therefore, in the CMP process, wafers stored underwater must be chucked by a robot or similar device and transported to the CMP equipment. Similarly, after CMP polishing, wafers wet with abrasives or pure water must be chucked and transported to the cleaning process as necessary.

[0004] As described above, wafer processing requires wafer transport in a wet environment, not a dry one. However, especially in such a wet environment, when attempting to detach a wafer held by a chuck, the wafer may not detach even after the chuck is released, resulting in transport failure. This is thought to be due to the roughness of the wafer surface being chucked. If the chucked wafer surface is too rough, the contact area with the chuck increases, making it difficult for the wafer to detach even after the chuck is released. On the other hand, if the wafer surface is too rough, the contact area decreases, making the wafer more likely to detach. Generally, the chucked surface is prone to forming chuck marks, which reduces quality, and therefore the chucked surface is often the backside of the silicon wafer. Therefore, from the perspective of reducing transport failures, it is preferable for only the backside of the silicon wafer to be rough, and a wafer manufacturing method that achieves this is desired.

[0005] A common silicon wafer cleaning method is called RCA cleaning. This method combines SC1 (Standard Cleaning 1), SC2 (Standard Cleaning 2), and DHF (Diluted Hydrofluoric Acid) cleaning depending on the purpose. SC1 cleaning involves etching the silicon wafer surface with an alkaline cleaning solution containing ammonia water and hydrogen peroxide in a specified ratio, lifting off adhering particles. It then utilizes the electrostatic repulsion between the silicon wafer and the particles to remove particles while preventing them from reattaching to the silicon wafer. SC2 cleaning uses a cleaning solution containing hydrochloric acid and hydrogen peroxide in a specified ratio to dissolve and remove metal impurities from the silicon wafer surface. DHF cleaning uses dilute hydrofluoric acid to remove chemical oxide films from the silicon wafer surface. Ozone water, which has a strong oxidizing power, is sometimes used to remove organic matter adhering to the silicon wafer surface and to prevent chemical oxide films from forming on the silicon wafer surface after DHF cleaning. Silicon wafers are cleaned by combining these cleaning methods depending on the purpose. Of these, SC1 cleaning involves etching, and it is generally known that the surface roughness of the wafer deteriorates after SC1 cleaning.

[0006] Additionally, methods for evaluating wafer surface roughness include the Sa (three-dimensional calculated average height) value obtained using an atomic force microscope (AFM) and the Haze value obtained using a particle counter. Haze is expressed as cloudiness and is widely used as an index of the roughness of silicon surfaces, with a high haze level indicating a rough wafer surface.

[0007] Patent Document 1 describes a method of cleaning silicon wafers with a diluted aqueous solution of ammonium hydroxide, hydrogen peroxide, and water in a composition range of 1:1:5 to 1:1:2000, and forming native oxide films of different thicknesses. Patent Document 2 describes a method of cleaning silicon wafers with a diluted aqueous solution of ammonium hydroxide, hydrogen peroxide, and water in a composition range of 1:1:5 to 1:1:2000, and forming native oxide films of different thicknesses. - It is described that when the concentration is high, direct etching of Si occurs preferentially, and the wafer surface roughness deteriorates. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 7-66195 [Patent Document 2] Japanese Patent Application Laid-Open No. 2011-82372 [Patent Document 3] Japanese Patent Application Publication No. 7-240394 [Patent Document 4] Japanese Patent Application Publication No. 10-242107 [Patent Document 5] Japanese Patent Application Publication No. 11-121419 [Patent Document 6] Special Publication No. 2012-523706 Summary of the Invention [Problem to be solved by the invention]

[0009] As mentioned above, in order to reduce transport defects during processing, silicon wafers with a rough surface to be chucked are required.

[0010] The present invention has been made to solve the above problems, and aims to provide a cleaning method capable of roughening the front and back surfaces of a silicon wafer, a cleaning method capable of roughening either the front and back surfaces of a silicon wafer or the back surface, a method for manufacturing a silicon wafer capable of obtaining a silicon wafer having only one surface selectively roughened, and a silicon wafer capable of reducing transport defects during processing. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides a cleaning method for roughening a silicon wafer, comprising: An oxide film is formed on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is A diluted aqueous solution of ammonium hydroxide with an ammonium hydroxide concentration of 0.051% by mass or less, or A diluted aqueous solution containing ammonium hydroxide and hydrogen peroxide, in which the ammonium hydroxide concentration is 0.051% by mass or less and the hydrogen peroxide concentration is 0.2% by mass or less and is four times or less than the ammonium hydroxide concentration. and a method for cleaning a silicon wafer, the method comprising the steps of: roughening the front and back surfaces of the silicon wafer by cleaning the silicon wafer with an aqueous solution of any one of the above.

[0012] In such a method for cleaning a silicon wafer, roughening occurs during etching of the native oxide film, and it is possible to roughen the front and back surfaces of the silicon wafer.

[0013] determining in advance, for each of the oxide film forming methods, a relationship between the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, a cleaning temperature and a cleaning time, and a surface roughness after cleaning; It is preferable to carry out cleaning by selecting the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, cleaning temperature, and cleaning time based on the obtained relationship.

[0014] The degree of roughening formed by the cleaning method of the present invention varies depending on the oxide film formation method, the ammonium hydroxide concentration or the ammonium hydroxide concentration and hydrogen peroxide concentration, the cleaning temperature, and the cleaning time, so it is effective to determine in advance the relationship between these conditions and the degree of roughening.

[0015] The present invention also provides a method for producing a silicon wafer, which comprises performing CMP polishing on one surface of a silicon wafer cleaned by the silicon wafer cleaning method of the present invention, to obtain a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

[0016] After roughening by the cleaning method of the present invention, only one side of the silicon wafer is polished, thereby producing a wafer in which one side is in a good surface condition and only the side opposite to the one side is selectively roughened.

[0017] The present invention also provides a silicon wafer, characterized in that it has a roughened surface having a roughness index Sa value of 0.3 nm or more and 5.5 nm or less as measured with an atomic force microscope.

[0018] With such a silicon wafer, the roughened surface exhibits a roughness suitable for adsorption by a chuck, thereby reducing transport defects during the processing steps.

[0019] The present invention also provides a silicon wafer, characterized in that it has a roughened surface having a roughness index haze value of 50 ppm or more and 1900 ppm or less as measured with a particle counter.

[0020] With such a silicon wafer, the roughened surface exhibits a roughness suitable for adsorption by a chuck, thereby reducing transport defects during the processing steps.

[0021] The surface opposite to the roughened surface is preferably a mirror surface.

[0022] Such silicon wafers can exhibit excellent quality.

[0023] The present invention also provides a cleaning method for roughening a silicon wafer, comprising the steps of: a first cleaning step of forming an oxide film on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is an aqueous solution containing ammonium hydroxide, or Aqueous solution containing ammonium hydroxide and hydrogen peroxide a second cleaning step of roughening the front and rear surfaces or the rear surface of the silicon wafer by cleaning with an aqueous solution of any one of Including, The present invention provides a method for cleaning a silicon wafer, characterized in that the aqueous solution used in the second cleaning step has an etching selectivity of Si to SiO2 of 95 or more.

[0024] In this method of cleaning silicon wafers, the native oxide film formed in the first cleaning step is roughened when etched in the second cleaning step, making it possible to manufacture roughened wafers.

[0025] Further, the etching selectivity of Si to SiO2 of the aqueous solution used in the second cleaning step is calculated from (etching amount of Si / etching amount of SiO2), As the wafer for calculating the Si etching amount, a silicon wafer, an epitaxial wafer, or an SOI wafer having a bare surface exposed without a native oxide film is used, It is preferable to use a wafer with a silicon oxide film having a film thickness of 3 nm or more as the wafer for calculating the etching amount of SiO2.

[0026] This method allows for accurate evaluation of the etching behavior of SiO2 and Si.

[0027] In addition, the etching amount of SiO required for roughening to proceed in the second cleaning step is calculated in advance for each method of forming the oxide film in the first cleaning step as a roughening etching amount, Selecting a cleaning time for the second cleaning step so that the amount of SiO2 etched in the second cleaning step is equal to or greater than the amount of roughening etching, and / or It is preferable to add an additional cleaning step before the second cleaning step to thin the oxide film formed in the first cleaning step so that a portion of the oxide film remains, and to adjust the cleaning time so that the total amount of SiO2 etched in the additional cleaning step and the amount of SiO2 etched in the second cleaning step is equal to or greater than the roughening etching amount.

[0028] The roughening of the present invention is carried out by etching a predetermined amount of SiO2 during cleaning to expose Si on the surface. Therefore, by calculating the amount of SiO2 etching required for roughening in advance as the amount of roughening etching in this manner, the roughening can be progressed more reliably.

[0029] In addition, a relationship between the etching selectivity of Si to SiO2, the cleaning time, and the surface roughness is obtained in advance for each method of forming the oxide film in the first cleaning step, Based on the obtained relationship, it is preferable to select the etching selectivity ratio of Si to SiO2 and the cleaning time, and then perform the second cleaning step.

[0030] The degree of roughness formed by the cleaning method of the present invention varies depending on the method for forming the oxide film in the first cleaning step, the etching selectivity of Si to SiO2, and the cleaning time, so it is effective to determine in advance the relationship between these conditions and the degree of roughness.

[0031] The present invention also provides a method for producing a silicon wafer, characterized by performing CMP polishing on one surface of a silicon wafer that has been cleaned by the silicon wafer cleaning method of the present invention and has roughened front and back surfaces, to obtain a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

[0032] In this way, by polishing only the front surface after roughening the front and back surfaces, it is possible to produce a wafer in which only the back surface is roughened while the front surface is in a good condition.

[0033] Furthermore, the removal amount of the CMP polishing can be set to be equal to or greater than the amount of Si etched in the second cleaning step.

[0034] This prevents the LLS from remaining after CMP due to etching, and maintains good LLS quality.

[0035] The amount of Si etched in the second cleaning step can also be set to be equal to or less than the removal amount of the CMP polishing.

[0036] This prevents the LLS from remaining after CMP due to etching, and maintains good LLS quality. [Effects of the Invention]

[0037] As described above, one aspect of the method for cleaning a silicon wafer of the present invention can roughen the front and back surfaces of a silicon wafer.

[0038] Furthermore, the method for producing a silicon wafer of the present invention can produce a wafer in which one surface is in a good condition and only the surface opposite to the one surface is selectively roughened.

[0039] Furthermore, the silicon wafer of the present invention can reduce transport defects during processing steps.

[0040] In addition, in another aspect of the method for cleaning a silicon wafer of the present invention, the front and back surfaces or the back surface of the silicon wafer can be roughened. [Brief explanation of the drawings]

[0041] [Figure 1] 1 is a flowchart showing an example of a first embodiment of the method for cleaning a silicon wafer of the present invention. [Figure 2] This figure shows SEM images and haze values ​​after cleaning a bare surface and an O3 oxide film surface with three levels of liquid composition: NH4OH:H2O2:H2O = 1:1:10, 1:1:100, and 1:1:1000. [Figure 3] 1 is a graph showing three levels of Si etching amount with liquid compositions of NH 4 OH:H 2 O 2 :H 2 O=1:1:10, 1:1:100, and 1:1:1000. [Figure 4] 1 is a graph showing the difference in the amount of Si etching between a bare surface and an O3 oxide film surface in a liquid composition of NH4OH:H2O2:H2O=1:1:1000 (45° C.). [Figure 5] 10 is another graph showing the difference in the amount of Si etched from the O3 oxide film surface when the liquid composition is NH4OH:H2O2:H2O=1:1:1000 (80° C.). [Figure 6] FIG. 1 shows SEM images, Haze values, and AFM Sa values ​​after roughening using various oxide film forming methods, NH 4 OH concentrations, H 2 O 2 concentrations, cleaning temperatures, and cleaning times. [Figure 7] 10 is a graph showing the variation of haze with respect to cleaning time when cleaning is performed with different NH4OH concentrations, H2O2 concentrations, and cleaning times. [Figure 8] 1 is a flowchart showing an example of a second embodiment of the silicon wafer cleaning method of the present invention. [Figure 9] This figure shows SEM images and haze values ​​after cleaning a bare surface and an O3 oxide film surface with five levels of solution composition: NH4OH:H2O2:H2O = 1:1:10, 1:1:100, 1:1:1000, 1:0.01:10, and 1:0.05:100. [Figure 10] 1 is a graph showing the amount of Si etched at three levels of liquid composition: NH 4 OH:H 2 O 2 :H 2 O=1:1:10, 1:1:100, and 1:1:1000. [Figure 11] 1 is a graph showing the amount of SiO2 etched at three levels of liquid compositions NH4OH:H2O2:H2O=1:1:10, 1:1:100, and 1:1:1000. [Figure 12] 1 is a graph showing three levels of Si / SiO2 etching selectivity, with liquid compositions of NH4OH:H2O2:H2O=1:1:10, 1:1:100, and 1:1:1000. [Figure 13]FIG. 10 shows SEM images, Haze values, and AFM Sa values ​​after roughening with different oxide film species and Si / SiO 2 etching selectivity ratios. [Figure 14] 10 is a graph showing the variation of haze with respect to cleaning time when roughening is performed by changing the Si / SiO 2 etching selectivity and cleaning time. [Figure 15] 10 is a graph showing the Si etching amount and LLS quality after CMP polishing with a polishing stock removal of 500 nm. [Figure 16] 1 is a schematic side view showing a portion of an example of a silicon wafer of the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0042] As described above, in order to reduce transport defects during processing steps, silicon wafers with a rough surface to be chucked are required.

[0043] To achieve the above object, the present inventors conducted extensive research into the etching behavior of silicon wafers using a cleaning solution consisting of ammonium hydroxide, hydrogen peroxide, and water, from the perspectives of the presence or absence of an oxide film on the front and back surfaces of the silicon wafer, the type of oxide film (oxide film formation method), the solution composition (particularly the ammonium hydroxide and hydrogen peroxide concentrations), the cleaning temperature, and the cleaning time. As a result, they found that cleaning a silicon wafer having a native oxide film on its front and back surfaces with either a diluted ammonium hydroxide solution having an ammonium hydroxide concentration of 0.051% by mass or less, or a diluted solution containing ammonium hydroxide and hydrogen peroxide, in which the ammonium hydroxide concentration is 0.051% by mass or less and the hydrogen peroxide concentration is 0.2% by mass or less and is four times the ammonium hydroxide concentration, roughens the oxide film without uniformly etching it, and that the degree of roughening can be adjusted by controlling the type of native oxide film (oxide film formation method), the solution composition (particularly the ammonium hydroxide and hydrogen peroxide concentrations), the cleaning temperature, and the cleaning time, thereby completing the present invention.

[0044] Furthermore, in order to solve the above problems, the present inventors have conducted extensive research into the etching behavior using a cleaning solution consisting of ammonium hydroxide, hydrogen peroxide, and water, particularly into the difference in the etching behavior between SiO2 and Si. As a result, they have found that when a silicon wafer having a native oxide film on its surface is cleaned with a cleaning solution having a high etching selectivity ratio of Si to SiO2, rapid etching occurs at the exposed Si sites, resulting in roughening, and that this roughening behavior can be adjusted by controlling the selectivity ratio, thereby completing another aspect of the present invention.

[0045] That is, the present invention is a cleaning method for roughening a silicon wafer, comprising: An oxide film is formed on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is A diluted aqueous solution of ammonium hydroxide with an ammonium hydroxide concentration of 0.051% by mass or less, or A diluted aqueous solution containing ammonium hydroxide and hydrogen peroxide, in which the ammonium hydroxide concentration is 0.051% by mass or less and the hydrogen peroxide concentration is 0.2% by mass or less and is four times or less than the ammonium hydroxide concentration. The method for cleaning a silicon wafer is characterized in that the front and back surfaces of the silicon wafer are roughened by cleaning the silicon wafer with an aqueous solution of any one of the above.

[0046] The present invention also provides a method for producing a silicon wafer, comprising: performing CMP polishing on one surface of a silicon wafer cleaned by the silicon wafer cleaning method of the present invention, to obtain a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

[0047] The present invention also provides a silicon wafer having a roughened surface with a roughness index Sa value of 0.3 nm or more and 5.5 nm or less as measured with an atomic force microscope.

[0048] The present invention also provides a silicon wafer having a roughened surface with a roughness index haze value of 50 ppm or more and 1900 ppm or less as measured with a particle counter.

[0049] The present invention also provides a cleaning method for roughening a silicon wafer, comprising the steps of: a first cleaning step of forming an oxide film on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is an aqueous solution containing ammonium hydroxide, or Aqueous solution containing ammonium hydroxide and hydrogen peroxide a second cleaning step of roughening the front and rear surfaces or the rear surface of the silicon wafer by cleaning with an aqueous solution of any one of Including, The method for cleaning a silicon wafer is characterized in that the aqueous solution used in the second cleaning step has an etching selectivity of Si to SiO2 of 95 or more.

[0050] The present invention also provides a method for producing a silicon wafer, characterized by performing CMP polishing on one surface of a silicon wafer that has been cleaned by the silicon wafer cleaning method of the present invention and has roughened front and back surfaces, to obtain a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

[0051] It should be noted that Patent Documents 1 and 2 only mention the influence of surface roughness on the front and back surfaces of the wafer. Patent Documents 3 to 6 also disclose techniques related to cleaning semiconductor substrates such as silicon wafers, but do not provide detailed consideration of the influence of the presence or absence of a native oxide film on the silicon wafer before cleaning, the type of native oxide film, the liquid composition, temperature, or time.

[0052] The present invention will be described in detail below with reference to the drawings as examples of embodiments, but the present invention is not limited thereto.

[0053] (Silicon wafer cleaning method and silicon wafer manufacturing method) [First aspect] First, a first embodiment of the method for cleaning a silicon wafer according to the present invention will be described. FIG. 1 is a flowchart showing an example of the first embodiment of the method for cleaning a silicon wafer of the present invention. Prepare a silicon wafer to be roughened on both sides, as shown in S1 in Figure 1. There are no restrictions on the conductivity type or diameter of the wafer, and examples include wafers after DSP processing.

[0054] Next, as shown in S2, an oxide film is formed on the silicon wafer using SC1 cleaning, SC2 cleaning, or ozone cleaning. If a native oxide film is present on the wafer before cleaning, it is preferable to remove it with HF cleaning before performing the above-mentioned cleaning. This is because, in the present invention, the etching behavior and resulting roughness vary depending on the type of oxide film, i.e., the oxide film formation method. For example, for bare wafers such as those processed using DSP, oxide film formation can be performed directly without HF cleaning. Note that the cleaning conditions for SC1, SC2, and ozone water cleaning can be general conditions. For example, for SC1 cleaning, the mixture ratio of ammonium hydroxide, hydrogen peroxide, and water can be in the range of NH4OH:H2O2:H2O = 1:1:5 to 1:1:100, the cleaning temperature can be 60°C or higher, and the cleaning time can be 1 to 30 minutes. For example, in the case of SC2 cleaning, the mixing ratio of HCl, hydrogen peroxide, and water can be HCl:H2O2:H2O = 1:1:5 to 1:1:20, the cleaning temperature can be 60°C or higher, and the cleaning time can be 1 to 30 minutes. For example, in the case of ozone water cleaning, the ozone concentration can be 3 ppm to 25 ppm, the cleaning temperature can be room temperature, and the cleaning time can be 1 to 30 minutes. As will be described later, the roughness formed in the present invention varies depending on the type of oxide film formed in S2 (the method for forming the oxide film), so an appropriate cleaning solution can be selected depending on the desired roughness.

[0055] Next, as in step S3, cleaning is performed with a diluted aqueous solution of ammonium hydroxide having an ammonium hydroxide concentration of 0.051% by mass or less, or a diluted aqueous solution containing ammonium hydroxide and hydrogen peroxide, in which the ammonium hydroxide concentration is 0.051% by mass or less and the hydrogen peroxide concentration is 0.2% by mass or less and is four times or less than the ammonium hydroxide concentration. In this case, when cleaning is performed using, for example, a batch-type cleaning machine with continuous chemical tanks, cleaning in S3 can be performed after cleaning in S2, thereby allowing the cleaning of the present invention to be performed efficiently in one batch.

[0056] Here, the roughness formed by the present invention will be described in detail from the viewpoints of the presence or absence of an oxide film on the front and back surfaces of the silicon wafer, the type of oxide film (oxide film formation method), the liquid composition (ammonium hydroxide concentration and hydrogen peroxide concentration), the cleaning temperature, and the cleaning time.

[0057] Figure 2 shows the results of front and back surface observations using a scanning electron microscope (SEM) and haze values ​​obtained using a particle counter after cleaning the bare surface and O3 oxide film surface (formed by S2) of a DSP wafer using three SC1 solution compositions: NH4OH:H2O2:H2O = 1:1:10, 1:1:100, and 1:1:1000, at 80°C for 10 minutes. The chemical solutions used were 28% by mass ammonia water (NH4OH) and 30% by mass hydrogen peroxide water (H2O2), and are also expressed as weight (wt%) percentages. Note that mass% refers to the concentration expressed as a percentage of the mass ratio of the cleaning solution to the solutes (ammonium hydroxide and hydrogen peroxide) contained in it, and is also expressed as wt%. Only the surface cleaned with a liquid composition of 1:1:1000 compared to the O3 oxide film surface showed significant irregularities in the SEM image, and the haze value was 470 ppm, a much higher value than the other surfaces, indicating roughening. The bare surface cleaned with a liquid composition of 1:1:1000 also roughened slightly, but to a lesser extent than the O3 oxide film surface. These results show that the deposition of oxide films on both the front and back surfaces, and the low SC1 liquid composition, are the factors behind the roughening.

[0058] Figure 3 shows the silicon etching depth for SC1 solution compositions of NH4OH:H2O2:H2O = 1:1:10, 1:1:100, and 1:1:1000. The etching depth tends to increase with decreasing solution composition, indicating that etching is more dominant at lower solution compositions. Figures 4 and 5 show the results of an investigation of silicon etching depth for two surface conditions: bare and O3 oxide films, using a solution composition of 1:1:1000. At 45°C, etching progressed only on the bare surface, while it progressed only slightly on the O3 oxide film. At 80°C, etching progressed slowly on the O3 oxide film after 3 minutes at 80°C, but began to progress rapidly after 6 minutes. Although not shown in Figure 5, at 80°C, the bare surface etched more than 55 nm after 3 minutes, and the O3 oxide film etched more than 55 nm after 12 minutes. Therefore, it is clear that the etching behavior of Si and SiO2 differs significantly in a low-liquid-composition environment, with Si being easily etched and SiO2 being difficult to etch. Considering the results in Figure 2 together with the etching amounts in Figures 4 and 5, roughening occurs not on the bare surface, which has a large amount of Si etching, but on the O3 oxide film surface, which has a small amount of etching. This roughening is thought to be due to the etching behavior of the oxide film in a low-liquid-composition environment. Furthermore, since the same results were obtained with a liquid composition of NH4OH:H2O2:H2O = 1:0:1000 as with a liquid composition of 1:1:1000, roughening is also possible with a diluted ammonia solution that does not contain hydrogen peroxide.

[0059] Next, Figure 6 shows the results of an investigation into the effects of native oxide type (oxide formation method), solution composition (ammonium hydroxide and hydrogen peroxide concentrations), cleaning temperature, and cleaning time. SEM images reveal that, except for the wafer with an O3 oxide film cleaned at 80°C for 4 minutes with a solution composition of 1:2:1000, various roughness values ​​were formed depending on the oxide type, SC1 solution composition, cleaning temperature, and cleaning time. Furthermore, the Sa values ​​obtained by AFM varied widely from 0.31 to 5.5 nm, and the Haze values ​​also varied from 104 to 1871 ppm. In other words, by evaluating the post-cleaning roughness for various oxide formation methods, ammonium hydroxide concentrations (or ammonium hydroxide and hydrogen peroxide concentrations), cleaning temperature, and cleaning time, and determining the relationship between these conditions and post-cleaning roughness, cleaning conditions can be determined based on the desired roughness.

[0060] More detailed investigations of the solution composition, with the temperature fixed at 80°C, revealed that the haze values ​​increased with solution compositions of 1:1:500, 1:1:1000, and 1:3:1000, as shown in Figure 7. However, the haze value did not increase even after 15 minutes of cleaning with a cleaning solution of 1:5:1000, and the silicon wafers were not roughened. Therefore, hydrogen peroxide has the effect of inhibiting the progress of etching. Since the weight concentrations of NH4OH and HO2 in the solution composition of 1:3:1000 are 0.025 mass% and 0.099 mass%, respectively, the HO2 weight concentration must be four times or less than the NH4OH weight concentration. Because the cleaning method of the present invention relies on the etching action of ammonium hydroxide and the oxidizing action of hydrogen peroxide, the silicon wafer cleaning method of the present invention is effective in such cases. Furthermore, since the weight concentration of NH4OH in a liquid composition of 1:1:500 is 0.051 mass %, NH4OH must be 0.051 mass % or less, and the liquid composition can be changed within this range.

[0061] Next, the type of oxide film (oxide film formation method) was also investigated. A 5 nm thick thermal oxide film was created in a dry oxygen atmosphere using a resistance heating furnace, and then cleaned at 80°C for 10 minutes using a liquid composition of 1:1:1000. However, the haze value did not increase, and no roughening was observed in the SEM images. From these results, it is believed that oxide films formed using SC1, SC2, or ozone water cleaning are optimal for roughening within the time frame available for practical operation.

[0062] Considering that the oxide film formed by cleaning is generally about 1 nm thick, that there is an uneven and unstable layer called the structural transition layer at the interface between the silicon oxide film and silicon, and that roughening does not occur in a thermal oxide film with an oxide film thickness of 5 nm, it is thought that the roughening that occurs during etching of the oxide film occurs near the structural transition layer at the interface between the silicon oxide film and silicon. In the case of a 5 nm thick thermal oxide film, etching of the oxide film did not progress to near the structural transition layer with a cleaning time of 10 minutes, so roughening is thought not to have occurred. SC1 and ozone cleaning also slightly changed the thickness and film quality of the structural transition layer, and as a result, it is thought that the roughness changed depending on the type of native oxide film.

[0063] Therefore, as mentioned above, it is more preferable to determine in advance for each oxide film type (oxide film formation method) the relationship between the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, the cleaning temperature, the cleaning time, and the surface roughness after cleaning, and then select the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, the cleaning temperature, and the cleaning time based on the determined relationship, and then perform cleaning.The inventors' extensive research has shown that the roughness can be changed over a wide range, for example, the AFM roughness index Sa value from 0.3 to 5.5 nm, and the particle counter haze from 50 to 1871 ppm, as shown in Figures 6 and 7.

[0064] Finally, it is often desirable for the surface of a silicon wafer, which is the surface on which devices are fabricated, to have a good roughness. For example, if the cleaning method of the present invention is performed in a batch-type cleaning machine, both the front and back surfaces will be roughened. Therefore, a single-side polishing process such as CMP polishing can then be performed on one side of the wafer, resulting in a wafer with only the surface opposite the one side selectively roughened. Such wafers do not cause chucking problems even in wet environments, enabling stable production.

[0065] [Second aspect] Next, a second embodiment of the method for cleaning a silicon wafer according to the present invention will be described. FIG. 8 is a flowchart showing an example of the second embodiment of the method for cleaning a silicon wafer according to the present invention.

[0066] First, prepare a silicon wafer whose backside you want to roughen. There are no restrictions on the conductivity type or diameter of the wafer, and examples include wafers after DSP processing.

[0067] Next, as in SA1, an oxide film is formed on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone cleaning (first cleaning step). If a native oxide film is formed on the wafer before cleaning, it is preferable to remove it in advance by HF cleaning before performing the above-mentioned first cleaning step. This is because, in the present invention, the etching behavior and the roughness of the formed oxide film vary depending on the type of oxide film, i.e., the method of forming the oxide film in the first cleaning step. For example, for a bare wafer such as one after DSP processing, an oxide film can be formed directly without HF cleaning. Note that the cleaning conditions for SC1, SC2, and ozone water cleaning can be general conditions. These general conditions can be, for example, the conditions described in the first embodiment.

[0068] 8 is an optional step that can be performed after the first cleaning step SA1 and before the second cleaning step SA2 described below. Step SA3 will be described later.

[0069] Next, as in SA2, the silicon wafer on which the oxide film has been formed is cleaned with either an aqueous solution containing ammonium hydroxide or an aqueous solution containing ammonium hydroxide and hydrogen peroxide, both of which have an etching selectivity ratio of Si to SiO (Si / SiO etching selectivity) of 95 or more (second cleaning step).

[0070] Here, the roughening phenomenon of the present invention will be described in detail from the viewpoint of the etching behavior of Si and SiO2. The method for calculating the etching amount of Si and SiO2 will be described in detail later.

[0071] Figure 9 shows the results of surface observation with a scanning electron microscope (SEM) and the haze value obtained with a particle counter after cleaning the bare surface and O3 oxide film surface (formed in the first cleaning step SA1) of a DSP wafer with different SC1 compositions (liquid composition NH4OH:H2O2:H2O), cleaning temperatures, and cleaning times.

[0072] The chemical solutions used were 28% by mass ammonia water (NH4OH) and 30% by mass hydrogen peroxide water (H2O2), each expressed as a percentage by mass (wt). Note that mass% refers to the concentration expressed as a percentage of the mass ratio of the cleaning solution to the solutes (ammonium hydroxide, hydrogen peroxide) contained in it, and is also expressed as wt%. Figure 9 also shows the etching selectivity of Si to SiO2, calculated using a calculation method described below.

[0073] Only the samples cleaned with solutions with extremely high selectivity ratios to the O3 oxide film surface (1:1:1000, 1:0.01:10, and 1:0.05:100) showed significant irregularities in the SEM images, and the haze value was also significantly higher than the other samples (275-470 ppm), indicating roughening. Cleaning with solutions with extremely high selectivity ratios (1:1:1000, 1:0.01:10, and 1:0.05:100) also roughened the bare surface slightly, but to a lesser extent than the O3 oxide film surface. This indicates that the roughening was caused by the deposition of an oxide film on the surface and the high Si / SiO2 etching selectivity of the cleaning solution used in the second cleaning step SA2. This is because the oxide film formed in the first cleaning step SA1 is etched during the second cleaning step SA2, causing rapid etching of Si in areas where Si is locally exposed. Therefore, to promote roughening, cleaning must be performed with a cleaning solution that has a high Si / SiO2 etching selectivity, specifically, 95 or higher.

[0074] Next, a method for calculating the Si / SiO2 etching selectivity ratio, which serves as an index in the present invention, will be described in detail.

[0075] The etching selectivity of Si to SiO2 of the aqueous solution used in the second cleaning step SA2 can be calculated from (etching amount of Si / etching amount of SiO2).

[0076] The amount of silicon etched can be determined by preparing a silicon wafer, epitaxial wafer, or SOI (Silicon on Insulator) wafer that has no native oxide film, i.e., an exposed bare surface with no native oxide film, and then cleaning the prepared wafer with an aqueous solution of any liquid composition (the aqueous solution for which the Si / SiO2 etching selectivity is to be calculated), and measuring the difference in film thickness before and after cleaning, and this can be used as the amount of silicon etched.

[0077] For example, HF cleaning can be used to remove native oxide films. If a native oxide film exists on a wafer, Si etching does not occur until the native oxide film is etched away, making it impossible to accurately evaluate the amount of Si etching. Furthermore, the presence of a native oxide film accelerates the roughening phenomenon described above, which roughens the wafer surface and potentially affects the measured values. Therefore, wafers used to calculate the amount of Si etching must be wafers that do not have a native oxide film.

[0078] The wafer to be used can be selected appropriately based on the etching amount. Since the thickness of a silicon wafer is generally about 775 μm, if the etching amount is at least 1 μm or more, the amount of thickness change can be detected. For example, the wafer thickness measured with a general flatness measuring device can be used as an index, and the wafer thickness before and after cleaning can be used as the etching amount. Note that there are no particular restrictions on the measuring device as long as it can measure the wafer thickness. For example, if the etching amount is only a few tens of nm, the amount of thickness change is very small and it is difficult to detect that change, so it is not preferable to use the wafer thickness as an index.

[0079] For etching depths of tens to hundreds of nanometers, epitaxial wafers with epitaxial thicknesses of several micrometers or SOI wafers with a Si / SiO2 / Si structure with a top-side Si layer thickness of tens to hundreds of nanometers can be used. The appropriate etching depth can be selected based on the required etching depth. Regarding film thickness measurement, for example, in the case of epitaxial wafers, the difference in resistivity between the epitaxial layer and sublayer can be exploited to measure the epitaxial thickness after cleaning using spreading resistance measurements, thereby calculating the film thickness difference. For SOI wafer film thickness measurement, for example, spectroscopic ellipsometry can be used. For example, when etching depths of several nanometers are used, an SOI wafer with a Si layer of 100 nm or less can be used for accurate evaluation. Note that the evaluation method is not particularly limited as long as the epitaxial and Si layer thicknesses can be evaluated for both epitaxial and SOI wafers.

[0080] Next, it is desirable to prepare a wafer on which a silicon oxide film of 3 nm or more exists as a wafer for calculating the etching amount of SiO2.

[0081] Generally, when SC1 cleaning is performed on silicon wafers with a native oxide film, in which the etching of the oxide film and the oxidation reaction of silicon compete with each other, as the silicon oxide film is etched and thinned, oxidizing species are more likely to diffuse through the silicon oxide film, and the silicon oxidation reaction progresses, resulting in a constant native oxide film thickness regardless of cleaning time. In this case, even if the difference in film thickness before and after cleaning is calculated, the amount of SiO2 etching cannot be accurately determined due to the presence of the silicon oxide film formed by the silicon oxidation reaction. Furthermore, the thickness of a typical native oxide film is approximately 1 nm, making it difficult to accurately measure this 1 nm change.

[0082] Therefore, for example, by preparing a silicon oxide film of 3 nm or more by thermal oxidation and measuring the oxide film thickness before and after cleaning, the amount of SiO2 etched can be calculated with high accuracy. If the film thickness is 3 nm or more, oxidizing species cannot diffuse through the oxide film, and silicon oxidation does not occur. Therefore, since only SiO2 etching progresses, the amount of SiO2 etched can be calculated with high accuracy. Furthermore, the film thickness can also be measured with high accuracy.

[0083] The thickness of the silicon oxide film can be selected appropriately based on the etching amount. The prepared silicon oxide film-coated wafer can be washed with the aqueous solution for which the Si / SiO2 etching selectivity is to be calculated, and the difference in film thickness before and after washing can be calculated. For example, spectroscopic ellipsometry can be used as a measurement method.

[0084] In this way, after determining the etching amounts of Si and SiO2 with the same solution composition and cleaning temperature, the etching selectivity of Si to SiO2 can be calculated from (etching amount of Si / etching amount of SiO2). Note that it is also possible to calculate the etching rate per unit time and then calculate the etching selectivity of Si to SiO2 from (etching rate of Si / etching rate of SiO2).

[0085] If this index is above a certain value, the SiO2 is etched and only the Si is preferentially etched where the Si is exposed, resulting in roughening. Since the etching behavior of Si and SiO2 varies depending on the cleaning temperature, determining the Si / SiO2 selectivity for each composition and cleaning temperature allows for reliable roughening under a variety of conditions. Research conducted by the inventors has shown that roughening progresses in a cleaning solution with a selectivity of 95 (for example, a solution composition of 1:1:1000, cleaning conditions of 45°C). This indicates that the Si / SiO2 etching selectivity must be 95 or higher.

[0086] 10 to 12 show the etching amounts of Si and SiO2 and the calculated Si / SiO2 etching selectivity ratios when cleaning was performed for 3 minutes with three levels of solution composition and three levels of cleaning temperature. Figures 10 to 12 show that the solution with a solution composition of 1:1:1000 etched the most Si, while the solution with a solution composition of 1:1:1000 etched the least SiO2. Reflecting this result, the solution with a solution composition of 1:1:1000 etched the most Si.

[0087] Next, the amount of SiO2 etching required to promote roughening will be described in detail. As described above, the roughening of the present invention progresses when the native oxide film is etched during cleaning, resulting in rapid etching of Si where Si is exposed. In other words, roughening can be promoted by etching the amount of SiO2 required to expose Si when cleaning with a cleaning solution having a selectivity of 95 or higher. Therefore, for each of the oxide film formation methods in the first cleaning step SA1, the amount of SiO2 etching required for roughening in the second cleaning step SA2 is determined as the roughening etching amount, and the cleaning time for the second cleaning step SA2 is selected so that the amount of SiO2 etching in the second cleaning step SA2 is equal to or greater than the roughening etching amount. This ensures more reliable roughening and makes it easier to select the cleaning conditions for the second cleaning step SA2.

[0088] The etching behavior of oxide films depends on the quality of the oxide film, and it is known that the denser the film structure, the more difficult it is to etch. Table 1 below shows the results of cleaning oxide films formed by SC1 cleaning or ozone cleaning in the first cleaning step SA1 with cleaning solutions that have a high Si / SiO2 etching selectivity (95 or higher).

[0089] [Table 1]

[0090] When an oxide film was formed using SC1 cleaning in the first cleaning step SA1 in the first bath (Levels 1 and 2), the SiO2 etching amount in the second cleaning step SA2 in the second bath was 0.14 nm or more, resulting in roughening. However, when an oxide film was formed using ozone cleaning in the first cleaning step SA1 in the first bath (Levels 3 to 8), the SiO2 etching amount in the second cleaning step SA2 in the second bath was 0.2 nm or more, resulting in roughening. Thus, by calculating the SiO2 etching amount required for roughening for each oxide film formation method in the first cleaning step SA1 as the roughening etching amount, roughening can be reliably progressed. Note that the thickness of a native oxide film is typically known to be 1 nm. The reason the index etching amount is less than 1 nm in this invention is because the SiO2 etching amount is very dense and difficult to etch. By using the etching amount of the thermal oxide film as an index, even if the oxide film type differs depending on the oxide film formation method in the first cleaning step SA1, the etching amount required for roughening can be known in advance as the roughening etching amount, eliminating the need to calculate the etching amount for each oxide film type, and allowing the cleaning conditions to be quickly selected.

[0091] In addition, in the cleaning method of this embodiment, as shown in FIG. 8, an additional cleaning step SA3 may be added before the second cleaning step SA2 to thin the oxide film formed in the first cleaning step SA1 so that a portion of the oxide film remains, and the cleaning time may be adjusted so that the total amount of SiO2 etched in the additional cleaning step and the amount of SiO2 etched in the second cleaning step is equal to or greater than the roughening etching amount.

[0092] Table 2 below shows the results of judging the haze value and degree of roughening of wafers that underwent an oxide film formation in the first cleaning step SA1 in the first tank, an additional cleaning step SA3 to thin the oxide film in the second tank, and then cleaned in a cleaning solution with a Si / SiO2 etching selectivity of 95 in the second cleaning step SA2 in the third tank.

[0093] [Table 2]

[0094] In levels 2, 4, and 5, after the first cleaning step SA1 in the first tank, cleaning with SC1 was performed as an additional cleaning step SA3 in the second tank, followed by the second cleaning step SA2 in the third tank. On the other hand, in levels 1 and 3, the additional cleaning step SA3 was not performed.

[0095] For oxide films formed by SC1 cleaning in the first cleaning step SA1, cleaning with a cleaning solution with a Si / SiO2 etching selectivity ratio of 95 (liquid composition 1:1:1000, 45°C) for 3 minutes resulted in an etched SiO2 of 0.12 nm, below the 0.14 nm index of roughening progression, and therefore no roughening occurred (Level 1). On the other hand, when an additional cleaning step SA3 was performed before the second cleaning step SA2, with an aqueous solution containing ammonium hydroxide with a liquid composition of 1:0:100 for 1 minute, followed by the same cleaning as in Level 1, roughening progressed. Since the etched SiO2 in this additional cleaning step was 0.06 nm, the total etched SiO2 was 0.06 nm + 0.12 nm = 0.18 nm, exceeding the index of 0.14 nm, suggesting roughening had progressed. For ozone-oxidized films in Levels 3 to 5, roughening progressed only in Level 5, where the index was 0.2 nm or greater. Thus, an additional cleaning step SA3 can be added before the second cleaning step SA2 to facilitate roughening progression.

[0096] In this way, the etching amount of SiO2 may be adjusted by the cleaning temperature, cleaning time, and solution composition in the second cleaning step SA2, or the etching amount of SiO2 may be adjusted in the additional cleaning step SA3. Note that there are no particular limitations on the chemical solution used in the additional cleaning step SA3, as long as it is a cleaning solution that thins the silicon oxide film, and examples include an aqueous solution containing ammonium hydroxide and hydrofluoric acid.

[0097] Next, we investigated the effects of the native oxide film formation method (native oxide film type) and the Si / SiO2 etching selectivity ratio. Figure 13 shows the results. Comparing the SEM images reveals that various roughness values ​​are formed depending on the native oxide film type, Si / SiO2 etching selectivity ratio, and cleaning time. The haze values ​​measured using a KLA particle counter SP3 ranged from 88 to 1871 ppm, while the Sa values ​​measured using an AFM varied from 0.31 to 5.5 nm. In other words, by evaluating the surface roughness (surface roughness) after the second cleaning step in relation to the oxide film formation method (oxide film type) and Si / SiO2 etching selectivity ratio in the first cleaning step and determining the relationship between these conditions and the surface roughness after the second cleaning step, cleaning conditions can be determined based on the desired roughness. For example, it is preferable to determine the relationship between the Si / SiO2 etching selectivity ratio and cleaning time and surface roughness for each oxide film formation method in the first cleaning step (SA1), and then select the Si / SiO2 etching selectivity ratio and cleaning time based on the determined relationship before performing the second cleaning step. The discrepancy in the magnitude relationship between the Haze value and the Sa value is due to the difference in the detection methods used for both, and it is sufficient to use the appropriate indicator. Regarding the effect of cleaning time, as shown in Figure 14, the Haze value varies significantly depending on the cleaning time at two different levels of Si / SiO2 etching selectivity. This means that it is easy to achieve the desired roughness by adjusting the cleaning time. Thus, the roughening method of the present invention is useful because it allows for flexible control of the roughness formed by adjusting the type of oxide film formed in the first cleaning step (the method for forming the oxide film in the first cleaning step), the Si / SiO2 etching selectivity, and the cleaning time.

[0098] Next, we will discuss the cleaning method used in the cleaning of the present invention. Currently, most wafer cleaning methods use liquids such as chemicals or pure water, and are called wet cleaning. These methods are primarily divided into batch cleaning, in which many wafers are cleaned at once, and single-wafer cleaning, in which wafers are processed one at a time. In the batch cleaning method, both the front and back surfaces of the wafer are immersed in the chemical solution due to the equipment configuration, so the cleaning of the present invention roughens both surfaces. In contrast, the single-wafer cleaning method sprays the chemical solution onto the rotating wafer, allowing for cleaning of only one side of the wafer. The inventors' research has shown that roughening can be achieved with both batch and single-wafer cleaning methods, as long as the second cleaning step is performed using an aqueous solution with a SiO2 etching amount greater than or equal to a predetermined value and a Si / SiO2 etching selectivity of 95 or greater. It has been found that the appropriate method can be selected taking into account the wafer manufacturing process.

[0099] As described above, to produce wafers with only a rough back surface, in the case of the single wafer method, it is sufficient to clean only the back surface, but in the case of the batch method, both the front and back surfaces are roughened, so it is desirable to improve the quality of the front surface by a polishing process described below.

[0100] For example, by performing the silicon wafer cleaning method of the present invention in a batch-type cleaning machine to roughen both the front and back surfaces of a silicon wafer, and then performing single-side polishing such as CMP polishing on one surface (i.e., the front surface), it is possible to produce a wafer in which only the surface opposite to the one surface (i.e., the back surface) is selectively roughened.

[0101] Here, we will describe in detail the polishing process that can be performed after the silicon wafer cleaning method of the present invention. Wafers roughened with a cleaning solution with a Si / SiO2 etching selectivity of 95 or higher were subjected to CMP polishing with a target polishing depth of 500 nm. Using a KLA particle counter SP5, we evaluated the number of LLSs larger than 19 nm at 19 nm UP. As shown in Figure 15, the number of LLSs increased at levels with a large amount of Si etching. This is because the etching depth was too high and etching-induced defects could not be removed by polishing. In contrast, the number of LLSs was very low and good at levels with a small amount of Si etching. Therefore, the amount of Si etching can be used as an indicator to estimate the LLS quality after CMP. Furthermore, even at levels where the number of LLSs increased, increasing the CMP removal depth can improve LLS quality. Therefore, it is preferable to select the CMP removal depth based on the amount of Si etching. As mentioned above, roughening occurs after SiO2 is etched and Si is exposed. For example, if the cleaning time for the second cleaning step SA2 is set to 3 minutes and the roughening process begins after 2 minutes, the removal amount can be adjusted to be equal to or greater than the amount of Si etched during 1 minute of cleaning. This allows for the minimum necessary removal amount. Furthermore, if the polishing removal amount needs to be reduced from the perspective of production throughput, the second cleaning step SA2 can be performed under conditions that result in a small amount of Si etching. Controlling the etching amount or the polishing removal amount can be selected appropriately. By polishing under these conditions, wafers with good front surface LLS quality and selective back surface roughening can be produced, even when the front and back surfaces are roughened using a batch process. Such wafers can be manufactured without chucking failure, enabling stable production even in wet environments.

[0102] (silicon wafer) FIG. 16 is a schematic side view showing a part of an example of a silicon wafer of the present invention.

[0103] 16 has a roughened surface 2. The roughness index Sa value of the roughened surface 2 measured with an atomic force microscope is 0.3 nm or more and 5.5 nm or less. The roughness index Haze value of the roughened surface 2 measured with a particle counter is 50 ppm or more and 1900 ppm or less.

[0104] In such a silicon wafer 1, the roughened surface 2 exhibits a roughness suitable for adsorption by a chuck, and therefore, transportation defects during the processing step can be reduced.

[0105] A silicon wafer 1 having such a roughened surface 2 can be obtained by roughening the front and back surfaces of a silicon wafer using the silicon wafer cleaning method of the present invention.

[0106] 16 has a mirror surface 3 on the surface opposite to the roughened surface 2. Such a mirror surface 3 can be obtained by performing single-side polishing such as CMP polishing on one side of a silicon wafer that has been cleaned by the silicon wafer cleaning method of the present invention.

[0107] The silicon wafer 1 shown in FIG. 16 has a mirror surface 3 in addition to a roughened surface 2, and therefore can exhibit excellent quality. [Example]

[0108] EXAMPLES The present invention will be specifically explained below using examples and comparative examples, but the present invention is not limited to these.

[0109] (Examples 1 to 8) Bare silicon wafers after DSP processing were prepared and cleaned using a batch-type cleaning machine as follows. The chemicals used for SC1 cleaning were 28% by mass ammonia water (NH4OH) and 30% by mass hydrogen peroxide (H2O2). The first bath was either ozone water cleaning (25 ppm, 25°C / 3 min) or SC1 cleaning (NH4OH:H2O2:H2O = 1:1:10, 60°C / 3 min) for oxide film formation. The second bath was SC1 cleaning with varying solution composition, temperature, and time for roughening. More specific conditions are shown in Table 3. Haze evaluation was then performed using a KLA SP3 particle counter. Because the haze value of unroughened wafers was 20-30 ppm, wafers with a haze value of 50 ppm or higher were considered roughened. The results are shown in Table 3 below. As described in claim 1, the present invention roughens a silicon wafer, and therefore the actual examples are those in which roughening was ultimately achieved. However, for reference, levels in which roughening was not ultimately achieved are also shown in the Examples column of Table 3 below.

[0110] (Comparative Example 1) Wafer cleaning was performed in the same manner as in Example 2, except that SC1 cleaning was performed in the second tank with a liquid composition of NH4OH:H2O2:H2O = 1:5:1000. The results are shown in Table 3 below.

[0111] [Table 3]

[0112] When cleaning the ozone (O3) oxide film surface with a solution composition of NH4OH:H2O2:H2O = 1:1:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.033 mass%) or NH4OH:H2O2:H2O = 1:1:500 (NH4OH concentration: 0.051 mass%, H2O2 concentration: 0.066 mass%) (Examples 1 to 3), the haze value increased at 4 minutes when the solution composition was 1:1:1000 and the cleaning temperature was 70°C (Example 1), and at 3 minutes when the cleaning temperature was 80°C (Example 2), indicating that roughening had progressed. This is thought to be because etching of the oxide film progressed more rapidly at 80°C, making roughening more likely at 80°C. When the solution composition was 1:1:500 and the cleaning temperature was 80°C (Example 3), the haze value increased at 4 minutes and roughening had progressed.

[0113] Next, the ozone (O3) oxide film surface was cleaned at a cleaning temperature of 80°C with a liquid composition of NH4OH:H2O2:H2O = 1:2:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.066 mass%), a liquid composition of NH4OH:H2O2:H2O = 1:3:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.099 mass%), and a liquid composition of NH4OH:H2O2:H2O = 1:5:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.165 mass%) (Examples 4 and 5, and Comparative Example 1). When the liquid composition was 1:2:1000 (Example 4) and 1:3:1000 (Example 5), an increase in haze value was observed only after 10 minutes, but no roughening occurred after 3 or 5 minutes. In the liquid composition of 1:5:1000 (Comparative Example 1), no increase in haze value was observed even after 10 minutes, and no roughening occurred. This is thought to be because etching was suppressed by increasing only the amount of hydrogen peroxide.

[0114] Next, the SC1 oxide film surface formed by SC1 cleaning was cleaned with a liquid composition of NH4OH:H2O2:H2O = 1:2:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.066 mass%), a liquid composition of NH4OH:H2O2:H2O = 1:3:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.099 mass%), or a liquid composition of NH4OH:H2O2:H2O = 1:1:500 (NH4OH concentration: 0.051 mass%, H2O2 concentration: 0.066 mass%) (Examples 6 to 8). In these cases, roughening progressed within a cleaning time of 1.5 minutes with a liquid composition of 1:2:1000 (Example 6) and 1:1:500 (Example 8), and roughening progressed more easily than with an ozone (O3) oxide film surface. This is thought to be due to the difference in film thickness and film quality between the ozone (O3) oxide film and the SC1 oxide film. Thus, by determining the relationship between ammonium hydroxide concentration, hydrogen peroxide concentration, cleaning temperature, cleaning time, and surface roughness for each oxide film type (oxide film formation method), cleaning conditions can be selected based on this relationship, and wafers with the target roughness can be manufactured. In Example 7, it was also confirmed that the front and back surfaces of the wafers were roughened with a cleaning time of 6 minutes.

[0115] After CMP processing was performed on one side of a silicon wafer cleaned using the 1.5-minute second-tank cleaning time standard of Example 6, a chucking test was performed using a CMP polisher. The wafer was stored underwater and the roughened side (backside) opposite to the CMP-processed side was chucked, and the wafer was unchucked and transported to the polisher stage. This test was repeated 200 times, and the wafer was transported without any defects all 200 times.

[0116] (Comparative Examples 2 to 6) Bare silicon wafers after DSP processing equivalent to those in the examples were prepared and subjected to the following cleaning using a batch-type cleaning machine. In the first bath, an oxide film was formed by ozone water cleaning (Comparative Examples 2 and 3), or the bare surface was left uncleaned (Comparative Examples 4 to 6). In the second bath, a solution composition of NH4OH:H2O2:H2O = 1:1:10 (NH4OH concentration: 2.12 mass%, H2O2 concentration: 2.77 mass%) or NH4OH:H2O2:H2O = 1:1:100 (NH4OH concentration: 0.25 mass%, H2O2 concentration: 0.33 mass%) was used. Cleaning was also performed on the bare surface alone, using a solution composition of NH4OH:H2O2:H2O = 1:1:1000 (NH4OH concentration: 0.025 mass%, H2O2 concentration: 0.033 mass%). The cleaning conditions and results for Comparative Examples 2 to 6 are shown in Table 4 below.

[0117] [Table 4]

[0118] The haze value did not exceed 50 ppm in any of Comparative Examples 2 to 6. In Comparative Example 6, where the second-tank cleaning time was 10 minutes, a slight increase in the haze value was observed to 42 ppm, but since it did not exceed 50 ppm, it was determined that no roughening occurred.

[0119] One side of a silicon wafer cleaned for 10 minutes in the second bath as in Comparative Example 2 was subjected to CMP processing, and then a chuck test similar to that in the Example was carried out 200 times using a CMP polisher. As a result, a defect occurred in which the wafer did not detach from the chuck in 4 out of 200 times.

[0120] (Examples A1 to A12, A19 to A33) Bare wafers after DSP polishing were prepared and cleaned using a batch-type cleaning machine. The SC1 cleaning chemicals used were 28% by weight of aqueous ammonia (NH4OH) and 30% by weight of aqueous hydrogen peroxide (H2O2). The first bath was cleaned using either ozone water (25 ppm, 25°C / 3 min) or SC1 cleaning (NH4OH:H2O2:H2O = 1:1:10, 45°C / 3 min) for the first cleaning step to form an oxide film. The second bath was cleaned using SC1 cleaning with the composition, temperature, and time shown in Tables 5 and 6 for the second cleaning step to form a roughened surface. Haze evaluation was then performed using a KLA SP3 particle counter. The Si and SiO2 etching selectivity was calculated for each solution used in the second bath from the difference in film thickness before and after cleaning using the method described above. The amount of Si etching was calculated using silicon wafers with bare surfaces exposed after HF cleaning, with no native oxide film, and the amount of Si etching was determined using a flatness measuring device from the wafer thickness before and after wafer cleaning.The amount of SiO2 etching was calculated using wafers with a 5nm oxide film formed by thermal oxidation, and the amount of SiO2 etching was determined using a JA Woolam Spectroscopic Ellipsometry M-2000V from the oxide film thickness before and after cleaning.

[0121] Since the haze value of the wafer before roughening was about 20 ppm, it was determined that all of Examples A1 to A12 and A19 to A33 were roughened.

[0122] (Examples A13 to A18, and A34) Bare wafers after DSP polishing were prepared and cleaned using a batch-type cleaning machine as follows. The SC1 cleaning chemicals used were 28% by weight ammonia water (NH4OH) and 30% by weight hydrogen peroxide (H2O2). The first bath was used as the first cleaning step, either with ozone water (25 ppm, 25°C / 3 min) or SC1 cleaning (NH4OH:H2O2:H2O = 1:1:10, 45°C / 3 min) to form an oxide film. The second bath was used as an additional cleaning step to thin the oxide film, using ammonia water with a composition of 1:0:100 or 0.05 wt% HF to remove part of the oxide film formed in the first bath without exposing the bare surface. The third bath was used as the second cleaning step, using SC1 cleaning with varying compositions, temperatures, and times as shown in Tables 5 and 6. At the same time, for each solution used in the third bath, the amount of Si etched and the amount of SiO2 etched were calculated from the difference in film thickness before and after cleaning using the method described above, and the Si / SiO2 etching selectivity was calculated. For the additional cleaning process in the second bath, the amount of SiO2 etched was calculated in advance using a wafer with a 5 nm oxide film. The cleaning conditions were adjusted so that the total amount of SiO2 etched in the second and third baths was 0.2 nm or more when the oxide film type in the first bath was ozone oxide film, and 1.4 nm or more when the oxide film type in the first bath was SC1 oxide film. It was determined that all surfaces were roughened based on the SP3 haze value after cleaning.

[0123] [Table 5]

[0124] [Table 6]

[0125] Next, since the Si etching amount in Example A19 was 820 nm and the Si etching amount in Example A22 was 230 nm, the front surface of the silicon wafer in Example A19 was subjected to CMP polishing with a polishing allowance of 1000 nm, and the silicon wafer in Example A22 was subjected to CMP polishing with a polishing allowance of 500 nm. The LLS of each wafer after CMP processing was evaluated using a KLA SP5 / 19nmUp, and the results were 12 pcs and 19 pcs, respectively, demonstrating good LLS quality. Subsequently, a test was performed 200 times in which the backside of the wafer stored underwater was chucked and the wafer was unchucked and transported to the stage of a polishing machine. All 200 transports were successful without any defects.

[0126] (Comparative Examples A1 to A13) Bare wafers after DSP polishing were prepared and cleaned using a batch-type cleaning machine. The SC1 cleaning chemicals used were 28% by weight of aqueous ammonia (NH4OH) and 30% by weight of aqueous hydrogen peroxide (H2O2). The first bath was cleaned with ozone water (25 ppm, 25°C / 3 min) for the first cleaning step to form an oxide film. The second bath was cleaned with SC1 cleaning, with the composition, temperature, and duration varied as shown in Table 7 below, for the second cleaning step to form a roughened surface. Haze evaluation was then performed using a KLA SP3 particle counter. The Si etching volume and SiO2 etching volume were calculated for each aqueous solution used in the second bath from the difference in film thickness before and after cleaning, as described above, and the Si / SiO2 selectivity was calculated. The Si etching volume was calculated using silicon wafers with bare surfaces exposed after HF cleaning, with no native oxide film. The Si etching volume was determined from the wafer thickness before and after cleaning using a flatness measuring device. The amount of SiO2 etching was calculated using a wafer with a 5 nm oxide film formed by thermal oxidation, and the amount of SiO2 etching was determined using spectroscopic ellipsometry from the oxide film thickness before and after cleaning.

[0127] As shown in Table 7, in Comparative Examples A1 to A13, the haze values ​​of SP3 were all around 20 ppm, which was equivalent to that of a wafer that was not roughened, and it was determined that the wafer was not roughened.

[0128] [Table 7]

[0129] After performing CMP polishing with a removal amount of 500 nm compared to the level of Comparative Example A1, the same chuck test as in Example A19 was performed 200 times using a CMP polisher. In 4 out of 200 tests, a failure occurred in which the wafer did not detach from the chuck.

[0130] From the above results, it can be seen that in Examples A1 to A34 of the present invention, by using a silicon wafer having an etching selectivity ratio of Si to SiO of 95 or more in the second cleaning step, the front and back surfaces of the silicon wafer, especially the back surface, could be sufficiently roughened to exhibit a roughness suitable for adsorption by a chuck.

[0131] On the other hand, in Comparative Examples A1 to A13, the etching selectivity of Si to SiO2 was not 95 or more in the second cleaning step, and therefore the front and back surfaces of the silicon wafer, especially the back surface, could not be sufficiently roughened to exhibit a roughness suitable for adsorption by a chuck.

[0132] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention. [Explanation of symbols]

[0133] 1...silicon wafer, 2...roughened surface, 3...mirror surface.

Claims

1. A cleaning method for roughening a silicon wafer, comprising the steps of: An oxide film is formed on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is A dilute aqueous solution of ammonium hydroxide having an ammonium hydroxide concentration of 0.051% by mass or less, or A diluted aqueous solution containing ammonium hydroxide and hydrogen peroxide, the concentration of which is 0.051% by mass or less and the concentration of hydrogen peroxide is 0.2% by mass or less and 4 times or less than the concentration of the ammonium hydroxide. Roughening the front and back surfaces of the silicon wafer by washing with any one of the aqueous solutions of determining a relationship between the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, the cleaning temperature, the cleaning time, and the surface roughness after cleaning for each of the oxide film forming methods; A method for cleaning a silicon wafer, comprising: selecting the ammonium hydroxide concentration or the ammonium hydroxide concentration and the hydrogen peroxide concentration, a cleaning temperature, and a cleaning time based on the obtained relationship, and performing cleaning.

2. 2. A method for producing a silicon wafer, comprising the steps of: subjecting one surface of a silicon wafer cleaned by the method for cleaning a silicon wafer according to claim 1 to CMP polishing; and obtaining a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

3. A cleaning method for roughening a silicon wafer, comprising the steps of: A first cleaning step of forming an oxide film on the silicon wafer by SC1 cleaning, SC2 cleaning, or ozone water cleaning; The silicon wafer on which the oxide film is formed is an aqueous solution containing ammonium hydroxide, or Aqueous solution containing ammonium hydroxide and hydrogen peroxide a second cleaning step of roughening the front and back surfaces or the back surface of the silicon wafer by cleaning with an aqueous solution of any one of Including, The aqueous solution used in the second cleaning step is SiO 2 The etching selectivity of Si to Al is 95 or more; and a relationship between the etching selectivity of Si to SiO 2 and the cleaning time, and the surface roughness, is obtained in advance for each method of forming the oxide film in the first cleaning step; A method for cleaning a silicon wafer, comprising the steps of: selecting the etching selectivity of Si to SiO 2 and the cleaning time based on the obtained relationship, and carrying out a second cleaning step.

4. The SiO of the aqueous solution used in the second cleaning step 2 The etching selectivity of Si to SiO is expressed as (Si etching amount / SiO 2 The amount of etching is calculated from As the wafer for calculating the etching amount of Si, any one of a silicon wafer, an epitaxial wafer, and an SOI wafer having a bare surface without a native oxide film exposed is used, The SiO 2 4. The method for cleaning a silicon wafer according to claim 3, wherein a wafer with a silicon oxide film having a film thickness of 3 nm or more is used as a wafer for calculating the etching amount.

5. In advance, for each method of forming the oxide film in the first cleaning step, a SiO necessary for roughening to proceed in the second cleaning step is 2 The amount of etching is calculated as the amount of roughening etching. SiO in the second cleaning step 2 and / or selecting a cleaning time for the second cleaning step so that the etching amount of the roughening etching is equal to or greater than the roughening etching amount. Before the second cleaning step, an additional cleaning step is added to thin the oxide film formed in the first cleaning step so that a part of the oxide film remains, and the SiO 2 and the amount of SiO 2 5. The method for cleaning a silicon wafer according to claim 3, further comprising adjusting a cleaning time so that a total of an etching amount of the first etching step and an etching amount of the second etching step is equal to or greater than the roughening etching amount.

6. A method for producing a silicon wafer, comprising the steps of: performing CMP polishing on one surface of a silicon wafer that has been cleaned by the method for cleaning a silicon wafer according to any one of claims 3 to 5 and has a roughened front and back surfaces; and obtaining a silicon wafer in which only the surface opposite to the one surface is selectively roughened.

7. 7. The method for producing a silicon wafer according to claim 6, wherein a removal amount of the CMP polishing is set to be equal to or greater than an etching amount of Si in the second cleaning step.

8. 7. The method for producing a silicon wafer according to claim 6, wherein an etching amount of Si in the second cleaning step is set to be equal to or less than a removal amount of the CMP polishing.

Citation Information

Patent Citations

  • Deposition of oxide on surface of silicon wafer

    JP1995066195A

  • Surface cleaning method of semiconductor wafer

    JP1995240394A

  • Improved method of cleaning microelectronics circuit board

    JP1998242107A

  • Chemical for treating semiconductor substrate and treatment method thereof

    JP1999121419A

  • Laminated dielectric separating wafer and manufacture thereof

    JP2001044278A