Coated negative electrode active material and all-solid-state battery

The coated negative electrode material with a silicon oxide layer and lithium titanate coating stabilizes the Si-based active material, addressing path breakage and resistance issues, enhancing the durability and capacity retention of all-solid-state batteries.

JP7582135B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021148503
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-13
Publication Date
2024-11-13
Estimated Expiration
2041-09-13

AI Technical Summary

Technical Problem

Si-based active materials in negative electrode layers of all-solid-state batteries experience significant volume change during charging and discharging, leading to path breakage and increased reaction resistance, which decreases capacity over cycles.

Method used

A coated negative electrode active material is developed with a silicon oxide layer between the Si-based active material and a coating layer containing lithium oxide, such as lithium titanate, to improve adhesion and stabilize the structure, thereby reducing path disconnection and resistance.

Benefits of technology

The coated negative electrode material effectively suppresses the increase in reaction resistance during high cycles, maintaining capacity retention and improving the durability of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582135000002
    Figure 0007582135000002
  • Figure 0007582135000003
    Figure 0007582135000003
  • Figure 0007582135000004
    Figure 0007582135000004
Patent Text Reader

Abstract

To provide a coated negative electrode active material capable of suppressing an increase in reaction resistance during high cycles.SOLUTION: The above problem is solved by providing a coated negative electrode active material that includes a Si-based active material, and a coating layer that covers at least a part of the surface of the Si-based active material and contains lithium oxide, where a silicon oxide layer is formed between the Si-based active material and the coating layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a coated negative electrode active material and an all-solid-state battery. [Background technology]

[0002] As an anode active material used in the anode layer of a battery, a Si-based active material is known. Patent Document 1 discloses an anode active material for a lithium secondary battery, which includes active particles capable of absorbing / releasing lithium ions and a coating layer coated on the surface of the active particles, the coating layer including a first material being a nano hollow fiber and a second material being a carbon precursor or LTO, and describes the use of Si as the active particles.

[0003] In addition, an all-solid-state battery is a battery having a solid electrolyte layer between a positive electrode active material layer and a negative electrode active material layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries having an electrolyte solution containing a flammable organic solvent. Patent Document 2 describes a negative electrode mixture for an all-solid-state battery, which contains at least one selected from the group consisting of carbon, Si, and Sn as a negative electrode active material, and Li 4 Ti 5 O 12 It is described that by using this in combination, the value of the discharge capacity relative to the charge capacity is high in a charge / discharge test of up to 30 cycles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-528907 A [Patent Document 2] JP 2020-53154 A Summary of the Invention [Problem to be solved by the invention]

[0005] Since Si-based active materials have a large theoretical capacity, it is easy to achieve high energy density in all-solid-state batteries using Si-based active materials. On the other hand, Si-based active materials undergo large volume changes during charging and discharging. Therefore, when Si-based active materials are used as negative electrode active materials, path breaks (disconnection of ionic conduction paths and electronic conduction paths) occur in the negative electrode active material layer with charge and discharge cycles, which tends to increase resistance and reduce capacity. Therefore, when Si-based active materials are used as negative electrode active materials, it is necessary to suppress the increase in reaction resistance during high cycles.

[0006] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a coated negative electrode active material capable of suppressing an increase in reaction resistance during high cycle times. [Means for solving the problem]

[0007] The present disclosure provides a coated negative electrode active material having a Si-based active material and a coating layer containing lithium oxide, the coating layer covering at least a portion of the surface of the Si-based active material, wherein a silicon oxide layer is formed between the Si-based active material and the coating layer.

[0008] According to the present disclosure, by providing a silicon oxide layer between a Si-based active material and a coating layer, the adhesion between the Si-based active material and the coating layer is improved, and a coated negative electrode active material can be obtained that can suppress an increase in reaction resistance during high cycles.

[0009] In the above disclosure, the silicon oxide layer may be amorphous.

[0010] In the above disclosure, the lithium oxide may be lithium titanate.

[0011] In the above disclosure, the lithium titanate is Li 4 Ti 5 O 12 may be also possible.

[0012] In the above disclosure, the silicon oxide layer may contain Ti element.

[0013] In the above disclosure, the coating layer may contain Si elements.

[0014] The present disclosure also provides an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein the negative electrode active material layer contains the above-mentioned coated negative electrode active material.

[0015] According to the present disclosure, since the negative electrode active material layer contains the above-mentioned coated negative electrode active material, an all-solid-state battery can be obtained in which an increase in reaction resistance during high cycles is suppressed. Effect of the Invention

[0016] Advantageous Effects of Invention The present disclosure has an effect of providing a coated negative electrode active material capable of suppressing an increase in reaction resistance during high cycles. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a coated negative electrode active material according to the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. [Diagram 3] 1 is a SEM image of Si particles in Comparative Example 1. [Figure 4] 1 is a SEM image of the coated negative electrode active material of Example 1. [Diagram 5] 1 is an EDX mapping image of the coated negative electrode active material of Example 1. [Figure 6] 1 is a HAADF-STEM image of the coated negative electrode active material of Example 1. [Figure 7] 1 shows the results of STEM-EDX analysis of the coated negative electrode active material of Example 1. [Figure 8] 1 shows the results of calculating the capacity retention rates for each cycle of the batteries of Comparative Example 1 and Example 1. [Figure 9]1 shows the results of impedance measurements performed on the batteries of Comparative Example 1 and Example 1 after the initial charge / discharge and after endurance testing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A.Coated negative electrode active material The coated negative electrode active material in the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view showing an example of the coated negative electrode active material in the present disclosure. The coated negative electrode active material 1 shown in Fig. 1 has a Si-based active material 2 and a coating layer 3 containing lithium oxide that coats at least a part of the surface of the Si-based active material 2, and a silicon oxide layer 4 is formed between the Si-based active material 2 and the coating layer 3.

[0019] According to the present disclosure, at least a part of the surface of the Si-based active material is covered with a coating layer containing lithium oxide, so that the volume change of the coated negative electrode active material can be suppressed. This is because the lithium oxide has a smaller volume change during charging and discharging than the Si-based active material. Furthermore, since a silicon oxide layer is formed between the Si-based active material and the coating layer, the adhesion between the Si-based active material and the coating layer is good. As a result, the coating layer having lithium ion conductivity follows the expansion and contraction of the Si-based active material, so that the disconnection of the ion conduction path and the electron conduction path due to the isolation of the Si-based active material can be suppressed. Therefore, the increase in reaction resistance during high cycles can be suppressed.

[0020] 1.Coating layer The coating layer in the present disclosure is a layer that covers at least a part of the surface of the Si-based active material and contains lithium oxide. The lithium oxide usually has a smaller volume change due to charging and discharging than the Si-based active material. The lithium oxide may contain lithium element, metal element Me, and oxygen element. The metal element Me may be Ti or Nb.

[0021] The lithium oxide is preferably lithium titanate. Lithium titanate is a compound containing Li, Ti, and O, for example, Li 4 Ti 5 O12 , Li 4 TiO 4 , Li 2 TiO 3 , Li 2 Ti 3 O 7 The lithium titanate preferably has at least one of a layered structure and a spinel structure.

[0022] Lithium titanate usually has electronic conductivity in the state where Li is inserted. The electronic conductivity in the state where Li is inserted (25°C) is, for example, 8.0 × 10 -1 S / cm or more. Therefore, in the present disclosure, the coating layer containing lithium titanate is in close contact with the Si-based active material, which can further suppress the disconnection of the electronic conduction path due to the expansion and contraction of the Si-based active material. On the other hand, when a short circuit occurs, for example, Li is released from the lithium titanate, and the amount of heat generated can be reduced by cutting off the electronic conduction path using this insulation (shutdown function). The electronic conductivity (25°C) of lithium titanate in a state in which the inserted Li is released is, for example, 2.1 x 10 -6 S / cm or less.

[0023] An example of a lithium oxide is lithium niobate (e.g., LiNbO 3 ), lithium niobium titanium oxides (e.g., LiNbTiO 3 ), LiCoVO 4 , LiMgSnO 4 , LiVMoO 6 etc.

[0024] The coating layer may contain only one type of lithium oxide, or may contain two or more types of lithium oxide.

[0025] The coating layer preferably contains lithium oxide as a main component. The proportion of lithium oxide in the coating layer is, for example, 70% by weight or more, or may be 80% by weight or more, or may be 90% by weight or more.

[0026] The coating layer preferably contains Si element derived from the Si-based active material, because this further improves the adhesion between the Si-based active material and the coating layer. The ratio of the Si element to the metal element Me in the coating layer (the molar ratio of (Si / Me)) may be 0.1 or more and 0.4 or less, or may be 0.2 or more and 0.3 or less. The above ratio can be calculated from point analysis of TEM-EDX. If the ratio of Si element in the coating layer is too low, the adhesion between the Si-based active material and the coating layer may decrease. If the ratio of Si element is too high, the ratio of Si-based active material in the coated negative electrode active material may decrease, and the energy density may decrease. In addition, if the coating layer contains lithium titanate, the electronic conductivity of the coating layer may decrease.

[0027] The average thickness of the coating layer is, for example, 5 nm or more, may be 30 nm or more, or may be 50 nm or more. If the coating layer is too thin, the effect of the present disclosure may not be obtained. On the other hand, the average thickness of the coating layer is, for example, 100 nm or less, may be 80 nm or less, or may be 60 nm or less. The average thickness of the coating layer can be measured, for example, using a transmission electron microscope (TEM) or the like.

[0028] The coating layer is preferably an aggregate of particles, as shown in FIG. 5. In this case, the average particle size (D 50 ) is, for example, 5 nm or more, may be 30 nm or more, or may be 50 nm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 100 nm or less, may be 80 nm or less, or may be 60 nm or less. 50 ) can be calculated, for example, from measurements using a scanning electron microscope (SEM). When the coating layer is an aggregate of particles, the average particle size of the particles is usually smaller than the average particle size of the Si-based active material.

[0029] The coating layer covers at least a part of the surface of the Si-based active material via a silicon oxide layer. The coating layer may be formed on a part of the surface of the Si-based active material or may be formed on the entire surface. The coverage rate of the Si-based active material by the coating layer is, for example, 70% or more, may be 80% or more, and may be 90% or more. On the other hand, the coverage rate may be 100% or may be less than 100%. The coverage rate can be confirmed, for example, by HAADF-STEM analysis (high-angle annular dark-field scanning transmission electron microscopy analysis) and EDX analysis (energy-dispersive X-ray fluorescence spectroscopy analysis).

[0030] The method for forming the coating layer will be described in detail in "5. Method for manufacturing a coated negative electrode active material" described later, so the description here is omitted.

[0031] 2. Silicon oxide layer The silicon oxide layer is formed between the Si-based active material and the coating layer and is a layer containing silicon oxide. The fact that the silicon oxide layer is formed between the Si-based active material and the coating layer can be confirmed, for example, by performing HAADF-STEM analysis (high-angle annular dark-field scanning transmission electron microscopy analysis) and EDX analysis (energy-dispersive X-ray fluorescence spectroscopy analysis) on the cross-section of the coated negative electrode active material.

[0032] The silicon oxide layer contains silicon element and oxygen element and is mainly composed of silicon oxide represented by the general formula: SiOx. The above x represents the ratio of silicon to oxygen and is, for example, a real number satisfying 0 < x < 2, and may be a real number satisfying 0.5 ≤ x ≤ 1.5. The proportion of the silicon oxide represented by the general formula: SiOx in the silicon oxide layer is, for example, 70% by weight or more, may be 80% by weight or more, and may be 90% by weight or more.

[0033] The silicon oxide layer preferably contains the metal element Me derived from the coating layer in addition to the silicon element and the oxygen element. This is because the adhesion between the Si-based active material and the coating layer is further improved. The ratio of the metal element Me to the Si element contained in the silicon oxide layer (Me / Si molar ratio) is, for example, a value greater than 0, and may be 0.05 or more, or may be 0.1 or more. If the ratio of the Me element is too small, the adhesion may decrease. On the other hand, it may be, for example, 0.5 or less. The ratio can be calculated from a point analysis of TEM-EDX. It can also be calculated by XPS analysis. The silicon oxide layer may contain lithium element.

[0034] The silicon oxide layer is preferably amorphous. If the silicon oxide layer is amorphous, the metal element Me is more likely to diffuse into the silicon oxide layer when a coating layer is formed on the silicon oxide, and the adhesion between the coating layer and the Si-based active material is improved. The fact that the silicon oxide layer is amorphous can be confirmed by image analysis using a transmission electron microscope (TEM) or the like.

[0035] The average thickness of the silicon oxide layer is, for example, 2 nm or more, may be 5 nm or more, or may be 10 nm or more. On the other hand, the average thickness of the silicon oxide layer is, for example, 20 nm or less, may be 15 nm or less. If the silicon oxide layer is too thin, the adhesion between the Si-based active material and the coating layer cannot be ensured. Also, if the silicon oxide layer is too thick, the proportion of the Si-based active material in the coated negative electrode active material is reduced, and the energy density may be reduced.

[0036] The silicon oxide layer may be formed on a part of the surface of the Si-based active material, or may be formed on the entire surface. The coverage of the Si-based active material with the silicon oxide layer is, for example, 70% or more, 80% or more, or 90% or more. On the other hand, the coverage may be 100% or less than 100%. The coverage can be confirmed, for example, by HAADF-STEM analysis (high angle dark field scanning transmission electron microscope analysis) and EDX analysis (energy dispersive X-ray fluorescence spectrometry).

[0037] The method for forming the silicon oxide layer will be described in detail in "5. Manufacturing method of coated negative electrode active material" below, and therefore the description thereof will be omitted here.

[0038] 3.Si-based active material The Si-based active material is an active material containing the Si element. Examples of the Si-based active material include simple Si and Si alloys. The Si alloy preferably contains the Si element as a main component. The ratio of the Si element in the Si alloy may be, for example, 50 mol% or more, 70 mol% or more, or 90 mol% or more. Examples of the Si alloy include Si-Al alloys, Si-Sn alloys, Si-In alloys, Si-Ag alloys, Si-Pb alloys, Si-Sb alloys, Si-Bi alloys, Si-Mg alloys, Si-Ca alloys, Si-Ge alloys, and Si-Pb alloys. The Si alloy may be a two-component alloy or a multi-component alloy of three or more components.

[0039] It is preferable that the Si-based active material does not contain the metal element Me (for example, Ti element) derived from the coating layer, since this may result in a low energy density.

[0040] The shape of the Si-based active material may be, for example, particulate. 50 ) is, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 50 μm or less, and may be 20 μm or less. In the present disclosure, it is preferable that the average particle size (D 50 ) can be calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0041] 4.Coated negative electrode active material The coated negative electrode active material in the present disclosure is generally used in an all-solid-state battery. The all-solid-state battery will be described in detail in "B. All-solid-state battery" below, and therefore will not be described here. In the coated negative electrode active material of the present disclosure, a silicon oxide layer and a coating layer are formed continuously in this order on the surface of a Si-based active material. In the present disclosure, the metal element Me originating from the coating layer is preferably diffused into the silicon oxide film. On the other hand, the metal element Me originating from the coating layer is preferably not diffused into the Si-based active material. Also, it is preferable that Si originating from the Si-based active material is diffused into the coating layer. In the present disclosure, it is preferable that the metal element Me originating from the coating layer is diffused into the silicon oxide film, and that Si originating from the Si-based active material is diffused into the coating layer. This is because the adhesion between the coating layer and the Si-based active material is further improved.

[0042] The ratio of the metal element Me to the element Si in the coated negative electrode active material (the molar ratio of (Me / Si)) may be 0.01 to 0.2. The ratio can be calculated by point analysis using TEM-EDX. It can also be calculated by XPS analysis. When the ratio is 0.05 or more, a coverage rate of 80% or more can be obtained.

[0043] 5. Manufacturing method of coated negative electrode active material The coated negative electrode active material in the present disclosure can be produced, for example, by a production method including a step of preparing a Si-based active material, a step of applying a lithium oxide precursor solution to the surface of the Si-based active material to form a precursor layer, and a heat treatment step of heat-treating the precursor layer.

[0044] (1) Si-based active material preparation process The Si-based active material may be prepared by self-synthesis or by purchasing a commercially available product. The Si-based active material is the same as that described in "A. Coated negative electrode active material," so the description is omitted here.

[0045] In the present disclosure, before the step of forming the precursor layer, a step of forming a silicon oxide layer on the surface of the Si-based active material may be performed in advance. The method of forming the silicon oxide layer is not particularly limited, but may include, for example, oxygen plasma treatment, treatment under an oxidizing atmosphere, and silane coupling agent treatment. In addition, the silicon oxide layer may be formed simultaneously with the coating layer in the heat treatment step described later.

[0046] (2) Precursor layer formation process This step is a step of applying a lithium oxide precursor solution to the surface of the Si-based active material to form a precursor layer. The precursor solution in the present disclosure usually contains a raw material of the lithium oxide and a solvent.

[0047] The precursor solution usually contains a Li source of lithium oxide. Examples of the Li source include Li inorganic salts, Li alkoxides, and Li hydroxides. Examples of the Li inorganic salts include lithium nitrate, lithium sulfate, and lithium acetate. Examples of the Li alkoxides include ethoxylithium and methoxylithium. Examples of the Li hydroxides include lithium hydroxide.

[0048] Examples of the raw material for lithium oxide include metal complexes, metal alkoxides, metal inorganic salts, and metal hydroxides. Examples of the metal complexes include metal acid complexes, specifically metal peroxo complexes and metal oxalato complexes. Examples of the metal peroxo complexes include peroxotitanate complexes. Examples of the metal inorganic salts include metal nitrates, metal sulfates, and metal acetates.

[0049] A method for preparing a precursor solution containing a metal peroxo complex may include, for example, adding hydrogen peroxide and ammonia water to a metal oxide. The amount of hydrogen peroxide and ammonia water added may be appropriately adjusted so as to obtain a transparent solution (homogeneous solution). When the precursor solution contains hydrogen peroxide in this way, the surface of the Si-based active material is oxidized by the oxidizing action of hydrogen peroxide, so that a silicon oxide layer is formed simultaneously with the coating layer after the heat treatment process.

[0050] When the precursor solution contains a metal alkoxide, the precursor layer is usually formed by a sol-gel method, in which the metal alkoxide is converted into a sol state by hydrolysis and polycondensation, and then converted into a gel state by polycondensation and aggregation.

[0051] The type of the solvent of the precursor solution is not particularly limited, and examples thereof include alcohol, water, and the like. Examples of alcohol include methanol, ethanol, propanol, butanol, and the like. The solvent of the precursor solution may be mainly composed of alcohol. The ratio of alcohol in the solvent is preferably 50 mol % or more, may be 70 mol % or more, or may be 90 mol % or more. The solvent of the precursor solution may be mainly composed of water. The ratio of water in the solvent is preferably 50 mol % or more, may be 70 mol % or more, or may be 90 mol % or more.

[0052] For example, if the precursor solution contains a metal alkoxide, the solvent is preferably anhydrous or dehydrated alcohol, whereas, for example, if the precursor solution contains a metal peroxo complex, the solvent is preferably water.

[0053] The method for applying the precursor solution is not particularly limited, but includes a method in which the Si-based active material is immersed in the precursor solution and stirred and dispersed. The solvent is then dried to obtain a powder.

[0054] (3) Heat treatment process The heat treatment step in the present disclosure is a step of heat treating the precursor layer.

[0055] The heat treatment temperature is not particularly limited as long as it is a temperature at which the desired coating layer can be formed, but is, for example, 100°C or higher, preferably 150°C or higher, and more preferably 200°C or higher. On the other hand, the heat treatment temperature is, for example, 600°C or lower, preferably 500°C or lower. If the heat treatment temperature is too high, the silicon oxide layer may crystallize, making it difficult for the metal element Me to diffuse into the silicon oxide layer, and the adhesion between the Si-based active material and the coating layer may decrease. In addition, the silicon oxide layer may become thicker, the proportion of the Si-based active material may decrease, and the energy density may decrease.

[0056] The heat treatment time is appropriately set so as to form a desired coating layer. The heat treatment time is, for example, within a range of 30 minutes to 48 hours, and preferably within a range of 1 hour to 20 hours. The heat treatment atmosphere is, for example, an argon atmosphere.

[0057] B. All-solid-state battery Fig. 2 is a schematic cross-sectional view of an all-solid-state battery according to the present disclosure. The all-solid-state battery 10 shown in Fig. 2 has a positive electrode active material layer 11, a negative electrode active material layer 12 containing the above-mentioned coated negative electrode active material, a solid electrolyte layer 13 formed between the positive electrode active material layer 11 and the negative electrode active material layer 12, a positive electrode current collector 14 that collects current from the positive electrode active material layer 11, and a negative electrode current collector 15 that collects current from the negative electrode active material layer 12.

[0058] According to the present disclosure, since the negative electrode active material layer contains the above-mentioned coated negative electrode active material, an all-solid-state battery can be obtained in which an increase in reaction resistance during high cycles is suppressed.

[0059] 1.Negative electrode active material layer The negative electrode active material layer in the present disclosure contains the above-mentioned coated negative electrode active material. The negative electrode active material layer may contain only the coated negative electrode active material as the negative electrode active material, or may contain other negative electrode active materials. The total ratio of the coated negative electrode active materials to all the negative electrode active materials contained in the negative electrode active material layer is, for example, 50% by volume or more, may be 70% by volume or more, or may be 90% by volume or more.

[0060] The ratio of the negative electrode active material in the negative electrode active material layer is, for example, 30% by volume or more, and may be 50% by volume or more. If the ratio of the negative electrode active material is too small, the volume energy density may not be improved. On the other hand, the ratio of the negative electrode active material in the negative electrode active material layer is, for example, 80% by volume or less. If the ratio of the negative electrode active material is too large, good electron conduction paths and ion conduction paths may not be formed.

[0061] The negative electrode active material layer preferably contains a solid electrolyte. As the solid electrolyte, for example, a sulfide solid electrolyte, an oxide solid electrolyte, Examples of the solid electrolyte include inorganic solid electrolytes such as nitride solid electrolytes and halide solid electrolytes.

[0062] Examples of the sulfide solid electrolyte include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and halogen. Examples of halogen include F, Cl, Br, and I. The sulfide solid electrolyte may be glass (amorphous) or glass ceramics. Examples of the sulfide solid electrolyte include Li. 2 SP 2 S 5 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li2 S-SiS 2 , Li 2 S-GeS 2 , Li 2 SP 2 S 5 -GeS 2 Examples include:

[0063] The negative electrode active material layer may contain a conductive material. Examples of the conductive material include carbon materials, metal particles, and conductive polymers. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF).

[0064] The negative electrode active material layer may contain a binder. Examples of the binder include a fluoride-based binder, a polyimide-based binder, and a rubber-based binder. The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0065] 2. Positive electrode active material layer The positive electrode active material layer in the present disclosure is a layer containing at least a positive electrode active material. The positive electrode active material layer may contain at least one of a conductive material, a solid electrolyte, and a binder, as necessary.

[0066] The positive electrode active material may be, for example, an oxide active material. For example, LiCoO 2 , LiMnO 2 , LiNiO 2 , LiVO 2 , LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 Rock salt layered active materials such as LiMn 2 O 4 , Li 4 Ti 5 O 12 , Li(Ni 0.5 Mn 1.5 )O 4Spinel-type active materials such as LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 Examples of the olivine type active material include those mentioned above.

[0067] A protective layer containing a Li-ion conductive oxide may be formed on the surface of the oxide active material. This is because it is possible to suppress the reaction between the oxide active material and the solid electrolyte. Examples of the Li-ion conductive oxide include LiNbO 3 The thickness of the protective layer is, for example, 1 nm or more and 30 nm or less. In addition, the positive electrode active material is, for example, Li 2 S can also be used.

[0068] The shape of the positive electrode active material may be, for example, particulate. 50 ) is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 50 μm or less, and may be 20 μm or less.

[0069] The conductive material, solid electrolyte, and binder used in the positive electrode active material layer are the same as those described in "1. Negative electrode active material layer" above, and therefore will not be described here. The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0070] 3.Solid electrolyte layer The solid electrolyte layer in the present disclosure is a layer disposed between the positive electrode active material layer and the negative electrode active material layer and containing at least a solid electrolyte. The solid electrolyte layer preferably contains a sulfide solid electrolyte as the solid electrolyte. The solid electrolyte layer may also contain a binder. The solid electrolyte and binder used in the solid electrolyte layer are the same as those described in "1. Negative electrode active material layer" above, and therefore will not be described here. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.

[0071] 4.All-solid-state battery The all-solid-state battery in the present disclosure usually has a positive electrode current collector that collects the positive electrode active material layer and a negative electrode current collector that collects the negative electrode active material layer. The positive electrode current collector and the negative electrode current collector may be, for example, in the form of a foil. The material of the positive electrode current collector may be, for example, SUS, aluminum, nickel, or carbon. The material of the negative electrode current collector may be, for example, SUS, copper, nickel, or carbon.

[0072] The all-solid-state battery in the present disclosure has at least one power generation unit having a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer, and may have two or more. When the all-solid-state battery has a plurality of power generation units, they may be connected in parallel or in series. The all-solid-state battery in the present disclosure includes an exterior body that houses a positive electrode current collector, a positive electrode material layer, a solid electrolyte layer, a negative electrode active material layer, and a negative electrode current collector. The type of the exterior body is not particularly limited, and may be, for example, a laminate exterior body.

[0073] The all-solid-state battery in the present disclosure may have a restraining tool that applies a restraining pressure to the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer along the thickness direction. By applying the restraining pressure, a good ion conduction path and an electron conduction path are formed. The restraining pressure is, for example, 0.1 MPa or more, may be 1 MPa or more, or may be 5 MPa or more. On the other hand, the restraining pressure is, for example, 100 MPa or less, may be 50 MPa or less, or may be 20 MPa or less.

[0074] The all-solid-state battery in the present disclosure is typically an all-solid-state lithium-ion secondary battery. The use of the all-solid-state battery is not particularly limited, but examples thereof include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, it is preferable to use the all-solid-state battery as a driving power source for hybrid electric vehicles or electric vehicles. In addition, the all-solid-state battery in the present disclosure may be used as a power source for moving objects other than vehicles (for example, railways, ships, and aircraft), and may be used as a power source for electrical products such as information processing devices.

[0075] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0076] The all-solid-state battery of the present disclosure will be described more specifically below using examples and comparative examples.

[0077] [Comparative Example 1] (Preparation of negative electrode) Negative electrode active material (Si particles, average particle size 2.5μm) and sulfide solid electrolyte (10LiI-15LiBr-75(0.75Li 2 S-0.25P 2 S 5 ), average particle size 0.5 μm), conductive material (VGCF), and binder (SBR) were prepared. These were weighed out so that the weight ratio of negative electrode active material:sulfide solid electrolyte:binder was 66.7:31.9:1.3, and mixed with a dispersion medium (diisobutyl ketone). VGCF was weighed out so that its ratio in the negative electrode active material layer was 2.5 volume % and added. The obtained mixture was dispersed with an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a negative electrode slurry. The obtained negative electrode slurry was applied onto a negative electrode current collector (Ni foil) and dried under conditions of 100°C for 30 minutes. After that, a 1 cm 2 The negative electrode active material layer was 80 μm thick, and the negative electrode current collector was formed by punching out the negative electrode active material layer.

[0078] (Preparation of positive electrode) Cathode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ) and sulfide solid electrolyte (10LiI-15LiBr-75(0.75Li 2 S-0.25P 2 S 5), conductive material (VGCF), and binder (PVdF) were prepared. These were weighed out so that the weight ratio of positive electrode active material:sulfide solid electrolyte:conductive material:binder was 84.7:13.4:1.3:0.6, and mixed with a dispersion medium (heptane). The resulting mixture was dispersed with an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a positive electrode slurry. The resulting positive electrode slurry was applied onto a positive electrode current collector (aluminum foil) and dried at 100°C for 30 minutes. After that, a 1 cm 2 A positive electrode having a positive electrode active material layer and a positive electrode current collector was obtained by punching out the positive electrode active material layer to a size of 80 μm. The thickness of the positive electrode active material layer was 80 μm.

[0079] (Preparation of solid electrolyte layer) Inner diameter cross-sectional area 1cm 2 A sulfide solid electrolyte (10LiI-15LiBr-75(0.75Li 2 S-0.25P 2 S 5 )) and 4 ton / cm 2 A solid electrolyte layer (thickness: 15 μm) was obtained by pressing with a pressing machine.

[0080] (Preparation of evaluation cells) A positive electrode is placed on one side of the solid electrolyte layer, and 1 ton / cm 2 (≒98MPa). Next, a negative electrode was placed on the other side of the solid electrolyte layer and pressed with a pressure of 4 ton / cm 2 (≒392 MPa). This resulted in an evaluation cell.

[0081] [Comparative Example 2 and Comparative Example 3] In addition to VGCF, LTO (Li 4 Ti 5 O 12 , average particle size 0.5 μm) was used in the negative electrode active material layer. 4 Ti 5 O 12A negative electrode slurry was prepared in the same manner as in Comparative Example 1, except that the ratio (volume %) of was changed to the value shown in Table 1. A negative electrode active material layer was produced in the same manner as in Comparative Example 1, except that the obtained negative electrode slurry was used, and an evaluation cell was obtained.

[0082] [Example 1] (Synthesis of coated negative electrode active material) Using Si particles (average particle size 5 μm), a coated negative electrode active material with a ratio of (Si-SiOx) / LTO ≈ 0.5 g / 0.35 g was synthesized.

[0083] First, CH 3 COOLi·2H 2 1.24 g of O powder was placed in a recovery flask. 20 ml of hydrogen peroxide solution (concentration: 30% by weight) and 20 ml of ammonia water (concentration: 28% by weight) were added to the recovery flask and dispersed by stirring. 2 TiO 3 1.47 g of the powder was added and dissolved by stirring for 40 minutes. This resulted in a pale yellow transparent solution containing a peroxotitanate complex. This reaction is represented by the following formulas (1) and (2). H 2 TiO 3 +H 2 O 2 +OH - ⇔[TiO(O 2 )(OH)] - +2H 2 O (1) H 2 TiO 3 +H 2 O 2 +2OH - ⇔[TiO(O 2 )(OH) 2 ] 2- +2H 2 O (2)

[0084] Next, the eggplant flask containing the pale yellow transparent solution was immersed in a water bath at 60°C, and 2 g of Si particles were added to the pale yellow transparent solution and stirred for about 35 minutes to disperse it. Next, the above solution was heated to 60°C in a rotary evaporator at reduced pressure (60 hPa (0.06 atm)) to evaporate the solvent. Next, the powder was collected by drying at 100°C. Next, the temperature was increased at a rate of 10°C / min, and main sintering was performed at 600°C for 5 hours in an Ar gas atmosphere to perform crystallization (heat treatment process). Next, the mixture was allowed to cool (natural cooling). As a result, a silicon oxide layer and Li were formed on the surface of the Si particles. 4 Ti 5 O 12 A powdered coated negative electrode active material having a coating layer containing (LTO) was obtained.

[0085] Except for using the negative electrode slurry prepared using the obtained coated negative electrode active material, a negative electrode active material layer was produced in the same manner as in Comparative Example 1, and an evaluation cell was obtained. The proportion (volume %) of LTO in the negative electrode active material layer is shown in Table 1.

[0086] [Example 2] A coated negative electrode active material was synthesized in the same manner as in Example 1, except that the blending amounts were adjusted so that the ratio of (Si-SiOx) / LTO was ≈0.5 g / 0.15 g. A negative electrode active material layer was produced in the same manner as in Comparative Example 1, except that a negative electrode slurry prepared using the obtained coated negative electrode active material was used, and an evaluation cell was obtained. The proportion (volume %) of LTO in the negative electrode active material layer is shown in Table 1.

[0087] [SEM observation] The Si particles used in Comparative Example 1 and the coated negative electrode active material synthesized in Example 1 were observed by a scanning electron microscope (SEM). Respective SEM images are shown in Fig. 3 and Fig. 4. In addition, EDX mapping images of O atoms, Si atoms, and Ti atoms were obtained for the coated negative electrode active material synthesized in Example 1. The results are shown in Fig. 5. From Fig. 4 and Fig. 5, it was confirmed that a coating layer containing lithium titanate (LTO layer) was formed on the surface of the Si particles.

[0088] [HAADF-STEM observation] A cross-sectional sample of the negative electrode layer was prepared from the evaluation cell obtained in Example 1, and HAADF-STEM analysis (high angle dark field scanning transmission electron microscopy) and EDX analysis (energy dispersive X-ray fluorescence spectrometry) were performed on the cross-section of the coated negative electrode active material. The HAADF-STEM image is shown in FIG. 6. The STEM-EDX analysis result is shown in FIG. 7. From FIG. 6 and FIG. 7, it was confirmed that an amorphous silicon oxide layer was formed between the Si particles and the coating layer containing lithium titanate. It was also confirmed that the amorphous silicon oxide layer contained Ti elements, and the LTO layer contained Si elements.

[0089] [Evaluation method] (Capacity maintenance rate) A charge / discharge test was performed on each of the batteries of Comparative Examples 1 to 3 and Examples 1 to 2 to evaluate them. The batteries were restrained to a fixed size at a restraining pressure of 5 MPa, and constant current-constant voltage (CC-CV) charging was performed at 0.461 mA to 4.35 V. Then, CC-CV discharging was performed at 0.461 mA to 3.0 V. Then, the all-solid-state battery was charged again. This charging was regarded as the initial charging. Evaluation was performed up to 600 cycles at 2C. The discharge capacity at the first cycle and the discharge capacity at the 100th cycle of the cycle test were determined, and the capacity retention rate was calculated by the following formula. Capacity retention rate (%) = (100th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100 Similarly, the capacity retention rate at the 600th cycle was calculated for the batteries of Comparative Example 1 and Example 1. The results are summarized in Table 1. Furthermore, the capacity retention rate from the 1st cycle to the 600th cycle was calculated for the batteries of Comparative Example 1 and Example 1 and is shown in FIG.

[0090] (Reaction resistance increase rate) The reaction resistance was evaluated by the impedance method. Specifically, for the batteries of Comparative Example 1 and Example 1, after the initial charge and discharge, the OCV of the all-solid-state battery was adjusted to 3.9 V, AC impedance measurement was performed, and a Nyquist plot shown in FIG. 9 (initial in FIG. 9) was obtained. The arc component obtained by the Nyquist plot was defined as the reaction resistance. Similarly, the reaction resistance after the above 600 cycles was evaluated (after durability in FIG. 9). The reaction resistance increase rate (times) was calculated by the following formula. The results are shown in Table 1. Reaction resistance increase rate (times) = reaction resistance after 600 cycles ÷ reaction resistance after 1 cycle

[0091] [Table 1]

[0092] From the results in Table 1, it was confirmed that the batteries of Example 1 and Example 2 could suppress the increase in reaction resistance at high cycles, and a high capacity retention rate was obtained even at high cycles. On the other hand, the batteries of Comparative Example 1 to Comparative Example 3 had a low capacity retention rate of about 70% at 100 cycles, regardless of the presence or absence of LTO addition and the amount of LTO. This is presumed to be because the Si particles and LTO particles that were once physically separated could not return to contact with each other due to the expansion and contraction of Si when LTO was simply added, and the Si particles became isolated. On the other hand, in Example 1 and Example 2, it is presumed that the adhesion between the Si particles and the coating layer was good due to the formation of a silicon oxide layer between the Si particles and the coating layer, and the increase in reaction resistance at high cycles could be suppressed. [Explanation of symbols]

[0093] 1 … Coated negative electrode active material 2...Si-based active material 3 … Covering layer 4 … Silicon oxide layer 10… All-solid-state battery 11... Positive electrode active material layer 12... Negative electrode active material layer 13…Solid electrolyte layer 14... Positive electrode current collector 15… Negative current collector

Claims

1. A coated negative electrode active material for use in an all-solid-state battery, comprising: a Si-based active material; and a coating layer containing lithium oxide, the coating layer coating at least a portion of a surface of the Si-based active material, A coated negative electrode active material, comprising a silicon oxide layer formed between the Si-based active material and the coating layer.

2. The coated negative electrode active material of claim 1, wherein the silicon oxide layer is amorphous.

3. 3. The coated negative electrode active material according to claim 1, wherein the lithium oxide is lithium titanate.

4. The lithium titanate is Li 4 Ti 5 O 12 The coated negative electrode active material according to claim 3 .

5. The coated negative electrode active material described in claim 3 or claim 4, wherein the silicon oxide layer contains Ti element.

6. A coated negative electrode active material described in any one of claims 1 to 5, wherein the coating layer contains Si element.

7. a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, An all-solid-state battery, wherein the negative electrode active material layer contains the coated negative electrode active material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for preparing silicon@lithium titanate core-shell structure composite material

    CN109935805A

  • Anode active material for lithium secondary cell, method for manufacturing the same, and lithium secondary cell equipped with anode active material

    JP2010140901A

  • Negative electrode active material for lithium secondary batteries, method for manufacturing the same, and lithium secondary battery containing the same

    JP2013528907A

  • Negative electrode material for lithium ion secondary batteries, method for manufacturing negative electrode material for lithium ion secondary batteries, resin composition for lithium ion secondary battery negative electrodes, negative electrode for lithium ion secondary batteries, and lithium ion secondary battery

    JP2015079727A

  • Method for producing sulfide solid-state battery

    JP2019106352A