Resistivity measuring device and resistivity measuring method

The resistivity measuring device suppresses mercury oxidation by directing inert gas to the electrode area, ensuring stable and cost-effective resistivity measurements for semiconductor wafers.

JP7582252B2Active Publication Date: 2024-11-13SHIN ETSU HANDOTAI CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2022082586
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-19
Publication Date
2024-11-13
Estimated Expiration
2042-05-19

AI Technical Summary

Technical Problem

Existing resistivity measuring devices using mercury electrodes suffer from mercury oxidation due to atmospheric oxygen, leading to increased measurement variability and decreased efficiency, with existing mitigation methods being costly and time-consuming.

Method used

A resistivity measuring device that supplies inert gas, such as nitrogen, from multiple directions to the mercury electrode area, reducing oxygen concentration locally and preventing mercury oxidation.

Benefits of technology

Stabilizes mercury electrode performance over time, allowing accurate resistivity measurements at a lower cost without replacing the entire device with nitrogen, thereby extending measurement longevity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582252000004
    Figure 0007582252000004
  • Figure 0007582252000005
    Figure 0007582252000005
  • Figure 0007582252000006
    Figure 0007582252000006
Patent Text Reader

Abstract

To provide a resistivity measurement device and a resistivity measurement method, capable of measuring the resistivity of a semiconductor wafer stably for a long time while suppressing, at low cost, deterioration of a mercury electrode due to oxidation of mercury.SOLUTION: A resistivity measurement device for a semiconductor wafer includes a mercury electrode part including a mercury electrode as a measurement probe, and inert gas supplying means configured to supply inert gas from at least three directions to the mercury electrode part.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resistivity measuring device and a resistivity measuring method, and more specifically, to resistivity measurement of semiconductors (including compound semiconductors) in general by a CV method using mercury. [Background technology]

[0002] One of the characteristics of a semiconductor wafer is resistivity, which can be evaluated, for example, by measuring the dopant concentration using a capacitance-voltage (CV) method.

[0003] For example, Patent Document 1 describes a method for evaluating the insulating properties of a buried oxide film by contacting a Hg probe with a Si active layer of an SOI wafer using the Hg-CV method.

[0004] Patent Document 2 describes a resistivity measuring device and a measuring method using the Hg-CV method, in which the measuring probe is freely movable in the vertical direction.

[0005] Patent Document 3 describes a method in which a forward bias voltage and a reverse bias voltage are applied to a resistivity measuring device using the Hg-CV method to determine the capacitance, and the resistivity is determined from the relationship between the reverse bias voltage and the capacitance.

[0006] FIG. 9 shows an example of a conventional semiconductor wafer resistivity measuring device.

[0007] The resistivity measuring device 10' shown in FIG. 9 includes a mercury electrode unit 1. The mercury electrode unit 1 includes, for example, an Hg Schottky electrode 11 and an Hg ohmic electrode 12. The Hg Schottky electrode 11 and the Hg ohmic electrode 12 are mercury electrodes serving as measurement probes. The resistivity measuring device 10' further includes a wafer chuck 2. The wafer chuck 2 is configured to hold a wafer 100 that is to be measured. The Hg Schottky electrode 11 and the Hg ohmic electrode 12 are connected to a voltage application device and a calculation device, not shown.

[0008] When performing measurements using resistivity measurement apparatus 10', mercury from Hg Schottky electrode 11 is brought into contact with resistivity measurement surface 101 of wafer 100 as shown in Fig. 9. The Hg ohmic electrode may be formed by bringing mercury into contact with the same surface as resistivity measurement surface 101 as shown in Fig. 9, or a wafer chuck 2 on the back side of measurement surface 101 may be used. With Hg Schottky electrode 11 and Hg ohmic electrode 12 formed in this manner, CV measurement is performed. At this time, the inside of apparatus 10', including the periphery of mercury electrode portion 1, is in an air atmosphere.

[0009] In such a device 10', the mercury used as an electrode during measurement is gradually oxidized when it comes into contact with the air (especially oxygen). As a result, the daily measurement value gradually changes and tends to increase. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2004-235463 A [Patent Document 2] JP 2010-153611 A [Patent Document 3] JP 2018-098271 A Summary of the Invention [Problem to be solved by the invention]

[0011] As a countermeasure against oxidation, it is necessary to lower the oxygen concentration by replacing the inside of the equipment with nitrogen, etc. Possible methods for this include 1) placing the wafer on the measurement stage, then circulating the inside of the equipment by exhausting the atmosphere and supplying nitrogen, and 2) placing the wafer on the measurement stage, then flushing with nitrogen and waiting until the oxygen concentration falls below a specified level, etc. However, these methods have significant disadvantages, such as increased equipment costs and longer measurement times that reduce measurement efficiency, and are therefore not practical.

[0012] The present invention has been made to solve the above problems, and has an object to provide a resistivity measuring device and a resistivity measuring method that can suppress deterioration of a mercury electrode due to oxidation of mercury at low cost and measure the resistivity of a semiconductor wafer stably for a long period of time. [Means for solving the problem]

[0013] In order to solve the above problems, the present invention provides a semiconductor wafer resistivity measuring device, comprising: a mercury electrode portion having a mercury electrode as a measurement probe; an inert gas supply means configured to flow an inert gas to the mercury electrode portion from at least three directions; The present invention provides a resistivity measuring device comprising:

[0014] The resistivity measuring device of the present invention can locally reduce the oxygen concentration in the mercury electrode portion, thereby suppressing the deterioration of the mercury electrode and enabling the resistivity of the wafer to be measured stably for a long period of time.

[0015] In addition, by using this device, the oxygen concentration near the mercury electrode, which causes the oxidation of mercury, can be reduced without replacing the entire atmosphere inside the device with nitrogen, making it possible to suppress deterioration of the mercury electrode due to the oxidation of mercury at low cost.

[0016] That is, the resistivity measuring device of the present invention can suppress deterioration of the mercury electrode due to oxidation of mercury at low cost and can measure the resistivity of a semiconductor wafer stably for a long period of time.

[0017] For example, the inert gas supplying means may be configured to supply nitrogen gas as the inert gas.

[0018] The inert gas is not particularly limited, but for example, nitrogen gas, which is versatile and relatively inexpensive, can be used.

[0019] The inert gas supplying means is preferably configured to supply the inert gas from three to six directions.

[0020] Although the oxidation of mercury can be suppressed if the inert gas is flowed from three or more directions, from the viewpoint of simplifying the structure, it is preferable that the inert gas is flowed from three to six directions.

[0021] The inert gas supplying means is preferably configured to supply the inert gas at a flow rate of 0.3 to 0.9 L / min.

[0022] If an inert gas supplying means capable of keeping the flow rate of the inert gas within this range is provided, the oxidation of mercury can be more reliably suppressed.

[0023] It is more preferable that the inert gas supplying means is configured to supply the inert gas at a flow rate of 0.4 to 0.8 L / min.

[0024] If an inert gas supply means capable of keeping the flow rate of the inert gas within this range is provided, the oxidation of mercury can be suppressed more reliably.

[0025] The present invention also provides a method for measuring resistivity of a semiconductor wafer, comprising the steps of: An inert gas is passed through the mercury electrode part, which is equipped with a mercury electrode as a measurement probe, from at least three directions. The present invention provides a resistivity measuring method, characterized in that the resistivity of a semiconductor wafer is measured using the mercury electrode.

[0026] The resistivity measurement method of the present invention can locally reduce the oxygen concentration in the mercury electrode portion, thereby suppressing the deterioration of the mercury electrode and enabling the resistivity of the wafer to be measured stably for a long period of time.

[0027] Furthermore, this method can reduce the oxygen concentration near the mercury electrode, which causes the oxidation of mercury, without the need to replace the atmosphere inside the device with nitrogen, making it possible to suppress deterioration of the mercury electrode due to the oxidation of mercury at low cost.

[0028] That is, according to the resistivity measuring method of the present invention, it is possible to suppress the deterioration of the mercury electrode due to the oxidation of mercury at low cost and to measure the resistivity of a semiconductor wafer stably for a long period of time.

[0029] For example, nitrogen gas can be flowed as the inert gas.

[0030] The inert gas is not particularly limited, but for example, nitrogen gas, which is versatile and relatively inexpensive, can be used.

[0031] It is preferable that the semiconductor wafer is disposed on the mercury electrode portion so as to cover the mercury electrode portion from above.

[0032] By performing measurements in this manner with the semiconductor wafer positioned so as to cover the mercury electrode section from above, it is possible to prevent air from entering the mercury electrode section from above and maintain a reduced oxygen concentration in the vicinity of the mercury electrode section, thereby more reliably suppressing deterioration of the mercury electrode due to oxidation.

[0033] It is preferable that the inert gas is caused to flow toward the mercury electrode from three to six directions.

[0034] Although the oxidation of mercury can be suppressed if the inert gas is flowed from three or more directions, from the viewpoint of simplifying the structure, it is preferable to flow the inert gas from three to six directions.

[0035] The inert gas is preferably flowed at a flow rate of 0.3 to 0.9 L / min.

[0036] By setting the flow rate of the inert gas within this range, oxidation of mercury can be more reliably suppressed. Effect of the Invention

[0037] As described above, the resistivity measuring device of the present invention can suppress deterioration of the mercury electrode due to oxidation of mercury at low cost and can stably measure the resistivity of a semiconductor wafer for a long period of time.

[0038] Furthermore, the resistivity measuring method of the present invention can suppress deterioration of the mercury electrode due to oxidation of mercury at low cost, and can measure the resistivity of a semiconductor wafer stably for a long period of time. [Brief description of the drawings]

[0039] [Figure 1] FIG. 1 is a schematic side view showing an example of a resistivity measuring device of the present invention. [Diagram 2] FIG. 2 is a diagram showing the arrangement of a mercury electrode section and an inert gas supply means in an example of a resistivity measuring device of the present invention. [Diagram 3] FIG. 11 is a diagram showing the arrangement of a mercury electrode section and an inert gas supply means in another example of the resistivity measuring device of the present invention. [Figure 4] 1 is a graph showing the relationship between the flow rate of N 2 gas flowed through the mercury electrode portion and the O 2 concentration in the vicinity of the mercury electrode portion in Example 1 and Comparative Example 1. [Diagram 5] 5 is a graph showing an enlarged portion of the graph shown in FIG. 4. [Figure 6] 1 is a graph showing the change over time in resistivity measured using a resistivity measuring device of Comparative Example 1. [Figure 7]2 is a graph showing the change over time in resistivity measured by the resistivity measuring device of Example 1. [Figure 8] 1 is a graph showing the relationship between the flow rate of N2 supplied to the mercury electrode part and the O2 concentration in the vicinity of the mercury electrode part in Example 1 and Comparative Examples 1 to 3. [Figure 9] FIG. 1 is a schematic side view showing an example of a conventional resistivity measuring device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] As described above, there has been a need for the development of a resistivity measuring device and a resistivity measuring method that can suppress deterioration of a mercury electrode due to oxidation of mercury at low cost and can stably measure the resistivity of a semiconductor wafer for a long period of time.

[0041] As a result of extensive research into the above-mentioned problems, the inventors discovered that by flowing an inert gas from at least three directions into a mercury electrode section equipped with a mercury electrode as a measurement probe, it is possible to locally reduce the oxygen concentration with a simpler configuration than the method of replacing the entire inside of the casing with nitrogen that is considered based on conventional technology, and thereby to suppress deterioration of the mercury electrode, thereby completing the present invention.

[0042] That is, the present invention is a semiconductor wafer resistivity measuring device, a mercury electrode portion having a mercury electrode as a measurement probe; an inert gas supply means configured to flow an inert gas to the mercury electrode portion from at least three directions; The resistivity measuring device is characterized by comprising:

[0043] The present invention also provides a method for measuring resistivity of a semiconductor wafer, comprising the steps of: An inert gas is passed through the mercury electrode part, which is equipped with a mercury electrode as a measurement probe, from at least three directions. The resistivity measuring method is characterized in that the resistivity of a semiconductor wafer is measured using the mercury electrode.

[0044] The present invention will be described in detail below with reference to the drawings, but the present invention is not limited thereto.

[0045] In addition, the semiconductor wafer to be measured for resistivity in the present invention is not particularly limited as long as it is a wafer containing a semiconductor. For example, the measurement target may be a silicon wafer, a Si layer of an SOI substrate, a compound semiconductor layer of a compound semiconductor substrate, etc.

[0046] [Resistivity measuring device] FIG. 1 is a schematic side view of an example of a resistivity measuring device of the present invention.

[0047] 1 includes a mercury electrode section 1. The mercury electrode section 1 includes, for example, an Hg Schottky electrode 11 and an Hg ohmic electrode 12. The Hg Schottky electrode 11 and the Hg ohmic electrode 12 are mercury electrodes serving as measurement probes.

[0048] The resistivity measuring device 10 further includes pipes 3. Each of the pipes 3 is fluidly connected to an inert gas storage tank (not shown). Each of the pipes 3 is provided with a valve 31 configured to adjust the flow rate of the inert gas from the inert gas storage tank. The pipes 3, the inert gas storage tank, and the valve 31 constitute an inert gas supplying means configured to flow the inert gas to the mercury electrode unit 1 from at least three directions.

[0049] Fig. 2 shows the positional relationship between the mercury electrode 1 and a pipe 3 serving as an inert gas supply means in the resistivity measuring device 10 shown in Fig. 1. The arrows shown in Fig. 2 indicate the direction of flow of the inert gas supplied from the pipe 3.

[0050] In the example shown in Fig. 2, the resistivity measuring device 10 includes three pipes 3. Thus, the resistivity measuring device 10 of the example shown in Fig. 1 and Fig. 2 includes an inert gas supplying means configured to flow an inert gas to the mercury electrode portion 1 from three directions.

[0051] The resistivity measurement apparatus 10 further includes an optional wafer chuck 2. The wafer chuck 2 is configured to hold a wafer 100 to be measured. The Hg Schottky electrode 11 and the Hg ohmic electrode 12 are connected to a voltage application device and an optional computing device (both not shown).

[0052] In Fig. 1, mercury of a Hg Schottky electrode 11 is brought into contact with a resistivity measurement surface 101 of a wafer 100. The Hg ohmic electrode may be a mercury electrode 12 that is brought into contact with mercury on the same surface as the resistivity measurement surface 101 as shown in Fig. 1, or a wafer chuck 2 on the back side of the measurement surface 101 may be used.

[0053] With such a resistivity measuring device 10 of the present invention, it is possible to flow an inert gas in a pinpoint manner near the mercury electrode section 1 having the mercury electrodes 11 and 12. Furthermore, by flowing the inert gas to the mercury electrode section 1 from at least three directions, the vectors of the inert gas flows cancel each other near the mercury electrode section 1, and the inert gas can be retained near the mercury electrode section 1. As a result, it is possible to locally reduce the oxygen concentration near the mercury electrode section 1 with a simple configuration. This makes it possible to suppress deterioration of the mercury electrodes 11 and 12 due to oxidation of mercury, and to stably measure the resistivity of the wafer 100 for a long period of time.

[0054] Furthermore, by using this device 10, the oxygen concentration near the mercury electrode 1, which causes the oxidation of mercury, can be reduced without replacing the entire inside of the device (for example, the casing 4 shown in Figure 2) with nitrogen, so that the deterioration of the mercury electrodes 11 and 12 over time due to the oxidation of mercury can be suppressed at low cost.

[0055] That is, according to the resistivity measuring device 10 of the present invention, the deterioration of the mercury electrodes 11 and 12 due to the oxidation of mercury can be suppressed at low cost, and the resistivity of a semiconductor wafer can be measured stably for a long period of time.

[0056] On the other hand, if the inert gas supply means is configured to flow the inert gas to the mercury electrode part 1 from one or two directions, the flowing inert gas cannot be retained near the mercury electrode part 1, and the oxygen concentration near the mercury electrode part 1 cannot be reduced.

[0057] Flowing inert gas from three or more directions can suppress the oxidation of mercury, but increasing the number of directions beyond six does not change the effect of reducing the oxygen concentration. Considering the disadvantage of increased complexity due to the increased number of pipes installed, it is preferable that the inert gas supply means 3 is configured to flow inert gas from three to six directions.

[0058] FIG. 3 shows an example in which the inert gas supplying means is configured to flow the inert gas to the mercury electrode portion 1 from six directions, that is, an example in which six pipes 3 are installed.

[0059] As in the example shown in Figures 2 and 3, if two adjacent pipes are arranged so that the angles they form with the mercury electrode 1 at the center are approximately equal (within an error of 15°), the flow vectors of the inert gas flowing through pipe 3 cancel each other out near the mercury electrode 1, making it possible to more reliably retain the supplied inert gas near the mercury electrode 1.

[0060] The inert gas is not particularly limited, but for example, nitrogen gas, which is versatile and relatively inexpensive, can be used.

[0061] The inert gas supplying means is preferably configured to supply the inert gas at a flow rate of 0.3 to 0.9 L / min.

[0062] If the device includes an inert gas supply means configured to flow the inert gas at a flow rate of 0.3 to 0.9 L / min, it is possible to completely eliminate the atmosphere, particularly oxygen, near the mercury electrode portion 1 while suppressing turbulence in the flow of the inert gas and preventing the inclusion of the surrounding air.

[0063] More preferably, the inert gas supplying means is configured to supply the inert gas at a flow rate of 0.4 to 0.8 L / min.

[0064] [Resistivity measurement method] Next, an example of the resistivity measurement method of the present invention will be described with reference to Figures 1 and 2 again. However, the resistivity measurement method of the present invention is not limited to the one using the resistivity measurement device 10 of the present invention shown in Figures 1 and 2.

[0065] In this example, using a resistivity measuring device 10 shown in FIG. 1, an inert gas is flowed from at least three directions into a mercury electrode unit 1 having mercury electrodes 11 and 12 as measuring probes as shown in FIG. 3, and the resistivity of a semiconductor wafer 100 is measured using the mercury electrodes 11 and 12.

[0066] Although the specific measurement procedure is not particularly limited, for example, a reverse bias is applied to the semiconductor wafer 100 by a voltage application device (not shown) connected to each of the Hg Schottky electrode 11 and the Hg ohmic electrode 12 to obtain the capacitance, and the dopant concentration at a desired depth can be measured by a calculation device (not shown) from the relationship between the reverse bias voltage and the capacitance. In addition, the measured dopant concentration can be converted into resistivity by using a predetermined conversion formula.

[0067] Such a resistivity measurement method of the present invention allows the inert gas to flow pinpoint near the mercury electrode section 1 including the mercury electrodes 11 and 12. Furthermore, by flowing the inert gas to the mercury electrode section 1 from at least three directions, the vectors of the inert gas flows cancel each other near the mercury electrode section 1, allowing the inert gas to remain near the mercury electrode section 1. As a result, the oxygen concentration near the mercury electrode section 1 can be locally reduced with a simple configuration. This makes it possible to suppress deterioration over time of the mercury electrodes 11 and 12 due to oxidation of mercury, and allows the resistivity of the wafer 100 to be measured stably for a long period of time.

[0068] Furthermore, according to the method of the present invention, the oxygen concentration near the mercury electrode 1, which causes the oxidation of mercury, can be reduced without replacing the entire atmosphere inside the device (for example, the casing 4 shown in FIG. 2) with nitrogen, so that the deterioration of the mercury electrodes 11 and 12 due to the oxidation of mercury can be suppressed at low cost.

[0069] That is, according to the resistivity measuring method of the present invention, the deterioration of the mercury electrodes 11 and 12 due to the oxidation of mercury can be suppressed at low cost, and the resistivity of a semiconductor wafer can be measured stably for a long period of time.

[0070] On the other hand, when an inert gas is flowed from one or two directions to the mercury electrode part 1, the flowing inert gas cannot be retained near the mercury electrode part 1, and the oxygen concentration near the mercury electrode part 1 cannot be reduced.

[0071] Flowing inert gas from three or more directions can suppress the oxidation of mercury, but increasing the number of directions beyond six does not change the effect of reducing the oxygen concentration. Considering the disadvantage of increased complexity due to the increased number of pipes installed, it is preferable for pipe 3 to flow inert gas from three to six directions.

[0072] Furthermore, as shown in FIG. 1, by performing measurements with a semiconductor wafer 100 placed on the mercury electrode part 1 so as to cover the upper part of the mercury electrode part 1, it is possible to prevent air from entering the mercury electrode part 1 from above, reliably maintain a low oxygen concentration in the mercury electrode part 1, and more reliably suppress deterioration of the mercury electrodes 11 and 12 due to oxidation.

[0073] The inert gas is not particularly limited, but for example, nitrogen gas can be used.

[0074] It is preferable to flow the inert gas at a flow rate of 0.3 to 0.9 L / min.

[0075] By flowing the inert gas at a flow rate of 0.3 to 0.9 L / min, it is possible to completely remove the air, particularly oxygen, near the mercury electrode 1 while suppressing turbulence in the inert gas flow and preventing the inclusion of the surrounding air.

[0076] It is more preferable to flow the inert gas at a flow rate of 0.4 to 0.8 L / min.

[0077] By flowing the inert gas during measurement, it is possible to suppress deterioration of the mercury electrodes 11 and 12 during measurement. Furthermore, by flowing the inert gas not only during measurement but also while measurement is not being performed, it is possible to more reliably suppress deterioration of the mercury electrodes 11 and 12. EXAMPLES

[0078] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0079] Example 1 In Example 1, the resistivity measuring device 10 shown in FIGS. 1 and 2 was used, pipes 3 were installed in three directions relative to the mercury electrode part 1 as shown in FIG. 2, nitrogen gas was caused to flow into the mercury electrode part 1 from three directions, the dopant concentration of the semiconductor wafer 100 was measured, and the resistivity was calculated from the measured dopant concentration using a conversion formula.

[0080] In Example 1, a silicon wafer as the semiconductor wafer 100 was disposed so as to cover the mercury electrode 1 as shown in FIG.

[0081] In Example 1, the flow rate of the nitrogen gas was changed between 0.075 L / min and 4.0 L / min, and the resistivity of the semiconductor wafer 100 was measured.

[0082] Comparative Example 1 In Comparative Example 1, the resistivity of a semiconductor wafer 100 was measured in the same manner as in Example 1, except that a resistivity measuring apparatus 10' shown in FIG. 9 was used.

[0083] In each of Example 1 and Comparative Example 1, the oxygen concentration near the mercury electrode 1 of the resistivity measuring device 10 or 10' was measured with an oxygen concentration meter. The oxygen concentration for each flow rate of nitrogen gas in each example is shown in Tables 1 and 2 below, and in Figs. 4 and 5. Fig. 5 is an enlarged view of a portion of Fig. 4. In Table 1, Figs. 4 and 5, Comparative Example 1, which does not have the piping 3, is shown as having a flow rate of "0".

[0084] [Table 1]

[0085] [Table 2]

[0086] As is clear from Tables 1 and 2 above and Figures 4 and 5, in Example 1 in which nitrogen was flowed from three directions to the mercury electrode part 1, the oxygen concentration near the mercury electrode part 1 was significantly reduced compared to Comparative Example 1 in which nitrogen was not flowed.

[0087] In particular, when nitrogen gas was flowed at a relatively low flow rate of 0.30 L / min to 0.90 L / min, the oxygen concentration could be reduced to 0% (below the detection limit), as shown in Table 2 and FIGS.

[0088] FIG. 6 shows the change over time of the measured resistivity in Comparative Example 1. FIG. 7 shows the change over time of the measured resistivity in Example 1 when nitrogen gas was continuously flowed at a flow rate of 0.5 L / min. Note that, as the semiconductor wafer 100, a wafer for daily management was used, and measurements were repeatedly performed on the same sample. FIG. 6 and FIG. 7 show the relative values ​​of the measured resistivity when the resistivity of the silicon wafer measured on the first day of measurement (first day) is taken as 1.

[0089] 6, the measured resistivity increased as the number of measurement days passed in Comparative Example 1. Specifically, this result suggests that Comparative Example 1 was unable to suppress deterioration over time due to oxidation of the mercury electrodes 11 and 12.

[0090] 7, in Example 1, the increase in the measured resistivity even after the passage of measurement days was significantly suppressed compared to Comparative Example 1. This result suggests that in Example 1, the oxygen concentration in the vicinity of the mercury electrode part 1 was reduced, thereby suppressing the deterioration over time due to oxidation of the mercury electrodes 11 and 12.

[0091] (Comparative Examples 2 and 3) Comparative Examples 2 and 3 were the same as Example 1, except that the number of pipes for flowing nitrogen gas was one and two, respectively.

[0092] In each of Comparative Example 2 and Comparative Example 3, the oxygen concentration in the vicinity of the mercury electrode 1 of the resistivity measuring device was measured in the same manner as in Example 1.

[0093] FIG. 8 shows the oxygen concentration for each flow rate of nitrogen gas in Example 1, Comparative Example 2, and Comparative Example 3.

[0094] As is clear from FIG. 8, in Comparative Example 2 in which one pipe 3 was used, the oxygen concentration in the vicinity of the mercury electrode 1 could not be sufficiently reduced even when nitrogen gas was flowed.

[0095] In Comparative Example 3, in which two pipes 3 were used, the oxygen concentration near the mercury electrode 1 could be reduced more than in Comparative Example 2, but could not be reduced to the same level as in Example 1.

[0096] From these results, it is evident that it is essential to flow the inert gas to the mercury electrode portion 1 from at least three directions.

[0097] (Examples 2 to 4) Examples 2 to 4 were the same as Example 1, except that the number of pipes for flowing nitrogen gas was four, five, and six, respectively.

[0098] As a result, in Examples 2 to 4, similarly to Example 1, the oxygen concentration in the vicinity of the mercury electrode portion 1 could be reduced to 0%.

[0099] Furthermore, the minimum and maximum flow rates per pipe at which the oxygen concentration reached 0% in Example 2 (four pipes), Example 3 (five pipes), and Example 4 (six pipes) are shown in Table 3 below, along with the results for Example 1 (three pipes).

[0100] [Table 3]

[0101] As is clear from the results shown in Table 3, the flow rate range in which the oxygen concentration can be maintained at 0% tends to gradually narrow as the number of pipes increases.

[0102] From the above-described examples, it is understood that the resistivity measuring device and resistivity measuring method of the present invention can suppress the oxidation of the mercury electrode, and can perform CV measurement for measuring the resistivity of a semiconductor wafer stably for a long period of time. Furthermore, according to the present invention, the oxygen concentration that causes the oxidation of mercury can be reduced without replacing the inside of the device with nitrogen, so that the deterioration of the mercury electrode due to the oxidation of mercury can be suppressed at low cost.

[0103] The present specification includes the following aspects. [1] A resistivity measuring device for a semiconductor wafer, comprising: a mercury electrode unit having a mercury electrode as a measurement probe; and an inert gas supplying means configured to flow an inert gas into the mercury electrode unit from at least three directions. [2] The resistivity measuring device according to [1], wherein the inert gas supplying means is configured to supply nitrogen gas as the inert gas. [3] The resistivity measuring device according to [1] or [2], characterized in that the inert gas supplying means is configured to flow the inert gas from three to six directions. [4] The resistivity measuring device according to any one of [1] to [3], characterized in that the inert gas supply means is configured to flow the inert gas at a flow rate of 0.3 to 0.9 L / min. [5] The resistivity measuring device according to any one of [1] to [3], characterized in that the inert gas supply means is configured to flow the inert gas at a flow rate of 0.4 to 0.8 L / min. [6] A method for measuring the resistivity of a semiconductor wafer, comprising the steps of: flowing an inert gas from at least three directions into a mercury electrode portion having a mercury electrode as a measurement probe; and measuring the resistivity of the semiconductor wafer using the mercury electrode. [7] The resistivity measurement method according to [6], characterized in that nitrogen gas is flowed as the inert gas. [8] The resistivity measuring method according to [6] or [7], characterized in that the semiconductor wafer is placed on the mercury electrode portion so as to cover the mercury electrode portion from above. [9] The resistivity measuring method according to any one of [6] to [8], wherein the inert gas is caused to flow around the mercury electrode from three to six directions.

[10] The resistivity measurement method according to any one of [6] to [9], wherein the inert gas is caused to flow at a flow rate of 0.3 to 0.9 L / min.

[0104] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0105] 1...mercury electrode part, 2...wafer chuck, 3...piping, 4...housing, 10 and 10'...resistivity measuring device, 11...Hg Schottky electrode (mercury electrode), 12...Hg ohmic electrode (mercury electrode), 31...valve, 100...semiconductor wafer, 101...resistivity measuring surface.

Claims

1. An apparatus for measuring resistivity of a semiconductor wafer, comprising: a mercury electrode portion having a mercury electrode as a measurement probe; an inert gas supply means configured to flow an inert gas from three to six directions to the mercury electrode portion; A resistivity measuring device comprising:

2. 2. The resistivity measuring device according to claim 1, wherein the inert gas supplying means is configured to supply nitrogen gas as the inert gas.

3. 3. The resistivity measuring device according to claim 1, wherein the inert gas supplying means is configured to supply the inert gas at a flow rate of 0.3 to 0.9 L / min.

4. 3. The resistivity measuring device according to claim 1, wherein the inert gas supplying means is configured to supply the inert gas at a flow rate of 0.4 to 0.8 L / min.

5. A method for measuring resistivity of a semiconductor wafer, comprising the steps of: An inert gas is passed through a mercury electrode part equipped with a mercury electrode as a measurement probe from three to six directions. A resistivity measuring method, comprising measuring the resistivity of a semiconductor wafer by using the mercury electrode.

6. 6. The resistivity measuring method according to claim 5, wherein nitrogen gas is supplied as the inert gas.

7. 6. The resistivity measuring method according to claim 5, wherein the semiconductor wafer is disposed on the mercury electrode portion so as to cover the mercury electrode portion from above.

8. 7. The resistivity measuring method according to claim 6, wherein the semiconductor wafer is disposed on the mercury electrode portion so as to cover the mercury electrode portion from above.

9. 9. The resistivity measuring method according to claim 5, wherein the inert gas is caused to flow at a flow rate of 0.3 to 0.9 L / min.

Citation Information

Patent Citations

  • Oxidation preventive device for leading edge of probe card

    JP1991257841A

  • Probe scanning mechanism and memory device applying scanning type tunnel microscope

    JP1995130013A

  • Method of evaluating SOI wafer

    JP2004235463A

  • Preprocessing method of epitaxial layer, and resistivity measuring method and apparatus of epitaxial layer

    JP2006203026A

  • Quality evaluation method and manufacturing method of silicon wafer

    JP2007042942A