Resin sheet, laminated sheet, semiconductor device and method for manufacturing same

A resin sheet with tailored properties addresses productivity and reliability issues in semiconductor sealing by forming a uniform sealing layer over multiple elements, enhancing mechanical strength and dielectric performance.

JP7582545B1Active Publication Date: 2024-11-13TOYO INK MFG CO LTD +1

Patent Information

Application Number
JP2024085872
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-11-13
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

Existing methods for sealing semiconductor elements face challenges in productivity and reliability, particularly when forming via holes and ensuring uniform coverage over multiple elements, leading to issues like gaps and low storage stability.

Method used

A resin sheet composed of a thermosetting composition containing a resin and a crosslinking agent, with specific properties such as elongation at break, dielectric constant, and dielectric loss tangent, is used to form a sealing layer that can be thermocompression bonded and cured, allowing for simultaneous coverage of multiple semiconductor elements.

Benefits of technology

The solution provides high productivity, excellent coverage, and improved reliability by reducing cracks and gaps, enhancing mechanical strength and dielectric properties, suitable for applications in 5G communication systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582545000001_ABST
    Figure 0007582545000001_ABST
Patent Text Reader

Abstract

Provided are a resin sheet, a laminated sheet, a semiconductor device, and a manufacturing method thereof, which are excellent in productivity, excellent in coverage even when a plurality of semiconductor elements are collectively covered, and are highly reliable. [Solution] In a laminate 1 in which a resin sheet 12 is sandwiched between a first release liner 11 and a second release liner 13, the resin sheet 12 for semiconductor encapsulation is a thermosetting composition containing a resin (A) and a crosslinking agent (B), and the resin sheet 12 has an elongation at break of 10 to 400% at 23°C after heating at 150°C for 1 hour, and a relative dielectric constant of 3 or less at a frequency of 10 GHz and 23°C after heating at 150°C for 1 hour, and a dielectric tangent of 0.01 or less at a frequency of 10 GHz and 23°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resin sheet, a laminate sheet, a semiconductor device, and a method for manufacturing the same. [Background technology]

[0002] The sealing layer protects electronic components from physical impacts, temperature changes, etc. The formation of the sealing layer is gradually being replaced by a heat-meltable resin sheet instead of the conventional conformal coating. For example, Patent Document 1 discloses a method for sealing electronic components by covering electronic components mounted on a substrate with a sheet made of a thermosetting composition and heat-curing the composition. Patent Document 2 discloses a method for producing a sealing film having an insulating layer and an electromagnetic wave shielding layer. The sealing film has an elongation percentage of 150 to 3500% at the softening point and is provided with unevenness corresponding to the unevenness formed on the electronic component mounting substrate. Patent Document 3 discloses a method for producing a semiconductor device including a step of temporarily attaching a sealing film to a semiconductor chip formed on a mounting substrate, heating and pressurizing the semiconductor chip in a reduced pressure environment to embed the semiconductor chip in a resin composition layer, and a step of curing the resin composition layer to seal the semiconductor chip and obtain a cured body. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-054363 A [Patent Document 2] JP 2019-021757 A [Patent Document 3] JP 2014-29958 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the method of Patent Document 3, since the sealing film can be used for one-time coating, versatility and productivity can be improved. However, there is a problem in productivity in that after forming a cured body of the sealing film, it is necessary to form a via hole that penetrates from the top surface of the cured body to the connection wiring by a laser (see Figures 8 to 10 of the same document).

[0005] The present disclosure has been made in consideration of the above-mentioned problems, and its purpose is to provide a resin sheet, a laminated sheet, a semiconductor device, and a manufacturing method thereof that are capable of forming a sealing layer that is highly productive, has excellent covering properties even when multiple semiconductor elements are collectively covered, and is highly reliable. [Means for solving the problem]

[0006] As a result of extensive investigations, the present inventors have found that the problems of the present disclosure can be solved in the following aspect, and have thus completed the present disclosure. [1]: A resin sheet for semiconductor encapsulation for forming an encapsulation layer for a semiconductor element, The resin sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B), The resin sheet has an elongation at break of 10 to 400% at 23°C after being heated at 150°C for 1 hour; The resin sheet for semiconductor encapsulation has a relative dielectric constant of 3 or less at a frequency of 10 GHz and 23°C after heating the resin sheet at 150°C for 1 hour, and a dielectric loss tangent of 0.01 or less at a frequency of 10 GHz and 23°C. [2]: The resin sheet for semiconductor encapsulation according to [1], wherein the resin sheet is sandwiched between two 50 μm PPS (polyphenylene sulfide) substrates, thermocompressed at 5 MPa and 80° C., then heat-treated at 150° C. for one hour, and then subjected to a two-week wet heat test under conditions of 121° C. and 100% humidity. When a peel test is performed between one of the PPS substrates and the resin sheet under conditions of a peel angle of 90° and a peel speed of 300 mm / min, at least a portion of the material breaks. [3]: Resin (A) is, The resin sheet for semiconductor encapsulation according to [1], comprising a urethane-based resin (A1) containing a structural unit derived from at least any one of polyols selected from dimerdiols and trimertriols, and / or a structural unit derived from at least any one of polyamines selected from dimerdiamines and trimertriamines, and having a urethane bond and optionally having a urea bond. [4]: The resin sheet for encapsulating semiconductors according to [3], wherein the acid value of the urethane resin (A1) is 1 to 20 mgKOH / g. [5]: The resin sheet for encapsulating a semiconductor according to [3] or [4], wherein the urethane resin (A1) has a weight-average molecular weight of 50,000 to 200,000. [6]: The resin sheet for encapsulating a semiconductor according to any one of [1] to [5], wherein the crosslinking agent (B) contains an epoxy compound. [7]: A laminate sheet obtained by laminating the resin sheet according to any one of [1] to [6] and one or more functional sheets. [8]: A semiconductor device comprising: a substrate; a semiconductor element mounted on the substrate; and an encapsulating layer encapsulating the semiconductor element, the encapsulating layer being formed from a cured product of the resin sheet according to any one of [1] to [6]. [9]: The semiconductor device according to [8], wherein the average thickness of the cured product is 10 to 300 μm.

[10] : A method for manufacturing a semiconductor device for collectively covering a plurality of semiconductor elements mounted on a substrate, comprising the steps of: A step of temporarily attaching the resin sheet according to any one of [1] to [6] to the plurality of semiconductor elements; a step of softening the resin sheet by heating and / or pressing the resin sheet to cover and bond the upper surface of the substrate and the upper and side surfaces of the plurality of semiconductor elements; and curing the resin sheet to encapsulate the semiconductor element. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a resin sheet, a laminated sheet, a semiconductor device, and a manufacturing method thereof that are highly productive, have excellent coverage even when covering multiple semiconductor elements collectively, and are highly reliable. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a laminate according to the present embodiment. [Diagram 2] FIG. 4 is a schematic cross-sectional view showing an example of a laminate according to Modification 1. [Diagram 3] FIG. 11 is a schematic cross-sectional view showing an example of a laminate according to Modification 2. [Figure 4] FIG. 11 is a schematic cross-sectional view showing an example of a laminate according to Modification 3. [Diagram 5] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 6] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 7] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 8] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 9] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 10] 1A to 1C are cross-sectional views each showing a schematic example of a manufacturing process of the semiconductor device according to the embodiment. [Figure 11] 1 is a schematic cross-sectional view showing an example of a semiconductor device according to an embodiment of the present invention. [Figure 12] FIG. 2 is a schematic cross-sectional view of a test substrate of the present embodiment. [Figure 13] FIG. 4 is a schematic cross-sectional view for explaining a method for evaluating coverage in the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present disclosure will be described in detail below. Other embodiments are also included in the scope of the present disclosure as long as they are consistent with the gist of the present disclosure. In this specification, a numerical range specified using "~" includes the numerical values ​​written before and after "~" as the lower and upper limits. Unless otherwise noted, each component in this specification may be used independently, either alone or in combination of two or more types. The numerical values ​​described in this specification refer to values ​​obtained by the methods described in the Examples below.

[0010] 1. Resin sheet The resin sheet of the present disclosure (hereinafter also referred to as the present resin sheet) is a sheet suitable for forming an encapsulating layer for encapsulating a semiconductor element (for semiconductor encapsulation). The present resin sheet has an advantage that it can encapsulate a plurality of semiconductor elements formed on a substrate or the like at once. Of course, the present resin sheet may be used for encapsulating a single semiconductor element. The present resin sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B), and is converted into an encapsulating layer, which is a cured product, through an encapsulation process. The present resin sheet may be a single layer or multiple layers. In the case of multiple layers, it is formed by laminating layers of the same and / or different resin compositions.

[0011] Since the resin sheet has excellent flexibility, it is suitable for use in forming an encapsulating layer for an unencapsulated semiconductor element. In addition, since the resin sheet is lightweight, has a high degree of design freedom, and can be integrated into a complex shape, it is suitable for use in mounting multiple encapsulated semiconductor chips on a substrate and encapsulating them all at once. Furthermore, taking advantage of the low dielectric properties of the resin sheet, the resin sheet may be used, in addition to encapsulation purposes, for example, for the purpose of insulating protection, in the application of forming a coating layer for electronic components including semiconductor chips encapsulated with semiconductor elements (packaged ICs, etc.).

[0012] In this specification, the semiconductor element includes power semiconductor elements such as IGBT (insulated gate bipolar transistor), MOSFET (metal oxide semiconductor field effect transistor), bipolar transistor, and diode; light emitting elements such as LED, optical semiconductor elements such as light receiving elements; semiconductor integrated circuits formed on semiconductor substrates such as silicon substrates, and semiconductor chips obtained by dividing semiconductor integrated circuits formed on semiconductor substrates. As described above, the resin sheet has excellent dielectric properties, is lightweight and can be integrated into complex shapes, and has a high degree of design freedom, making it particularly suitable for use in the information and communications field. Semiconductor elements are usually formed or mounted on the upper surface of a base substrate.

[0013] In the present disclosure, encapsulation refers to forming an encapsulating layer by using the present resin sheet to cover an object such as a semiconductor element (hereinafter, the semiconductor element will be described) and curing the sheet. The encapsulating layer of the present disclosure includes the general mode of covering a semiconductor element with an encapsulating layer, and includes the mode of directly encapsulating a semiconductor element as well as the mode of further encapsulating a semiconductor module in which a semiconductor element is encapsulated. Among these, the present resin sheet has low elasticity and is excellent in adhesion and stress relaxation, and is therefore particularly suitable for application to the mode of encapsulating all substrates while preventing warping.

[0014] It is important that the resin sheet has an elongation at break of 10 to 400% at 23° C. after heating for 1 hour at 150° C. Furthermore, it is important that the resin sheet has a relative dielectric constant of 3 or less at a frequency of 10 GHz and 23° C. after heating for 1 hour at 150° C., and a dielectric loss tangent of 0.01 or less at a frequency of 10 GHz and 23° C.

[0015] The elongation at break and dielectric properties of the present disclosure were evaluated under the condition of a sufficiently cured stage, that is, the condition of heating the resin sheet at 150°C for 1 hour. The "sufficiently cured stage" may include not only the cured product, but also the product in the middle of curing. In this specification, the cured product refers to a state in which the curing reaction does not substantially proceed even if further heating is performed, and the sealing layer is a cured product. The cured product does not include a state in which a part of the resin sheet may undergo a curing reaction when formed, but which may be cured by further heating. At the stage of the thermosetting composition, a part of the components may be in a semi-cured B-stage state. The cured product of the thermosetting composition is generally obtained by heating it at 100 to 180°C for about 20 minutes to 2 hours.

[0016] The resin sheet has an elongation at break of 10 to 400% at 23°C after heating at 150°C for 1 hour, so that the resin sheet has excellent coverage for recesses formed by mounting semiconductor elements. More specifically, the resin sheet has an elongation at break of 10% or more at 23°C after heating at 150°C for 1 hour, so that the resin sheet can maintain an appropriate breaking strength while maintaining an appropriate deformation force, and can significantly improve the occurrence of defects such as cracks and breaks in the sealing layer. The resin sheet has an elongation at break of 400% or less at 23°C after heating at 150°C for 1 hour, so that the sealing layer has excellent mechanical strength. As a result, the sealing layer can be significantly improved from cracks and breaks that cause a decrease in reliability.

[0017] The lower limit of the elongation at break is more preferably 100%, more preferably 120%, and even more preferably 200%. The upper limit of the elongation at break is more preferably 390%, more preferably 380%, and even more preferably 360%. In addition, in the case where the resin sheet is anisotropic in elongation after heating at 150°C for 1 hour, the direction with the lowest elongation is 10% or more, and the direction with the highest elongation is 400% or less. In addition, the elongation at break refers to the value of the permanent elongation after the sheet breaks when the resin sheet is subjected to a tensile test at 23°C after heating at 150°C for 1 hour, and was performed by the method described in the examples below, i.e., the method specified by JISK7161:1994.

[0018] The breaking strength of the resin sheet at 23°C after heating at 150°C for 1 hour is preferably 10 to 60 MPa, more preferably 15 to 50 MPa, and even more preferably 20 to 45 MPa, from the viewpoints of increasing flexibility and improving coverage over uneven surfaces such as semiconductor elements.

[0019] The elongation at break after heating the resin sheet at 150°C for 1 hour can be adjusted by the thickness of the resin sheet. The elongation at break tends to decrease as the thickness increases. The elongation at break can be adjusted by the type of resin (A) of the resin sheet and the weight average molecular weight (Mw) of the resin (A). The elongation at break at 23°C after heating the resin sheet at 150°C for 1 hour can be adjusted by the crosslink density of the sealing layer. As a method for adjusting the elongation at break at 23°C after heating the resin sheet at 150°C for 1 hour, a method of adjusting the number of functional groups and equivalent weight of the crosslinking agent (B) in the thermosetting composition for forming the resin sheet is also suitable. The crosslinking agent (B) is preferably bifunctional or higher, and more preferably contains a trifunctional to tetrafunctional crosslinking agent (B). The content of the crosslinking agent (B) in the composition can also be adjusted. Furthermore, the content of the crosslinking agent (B) in the composition can also be adjusted by the type, amount, and particle size of the filler. The flexibility can also be adjusted by the type of flexibility adjuster that does not contribute to crosslinking, such as a plasticizer, an inert resin that is unreactive by itself, or an oligomer.

[0020] In the case of high-frequency circuits, the transmission loss of electric signals is greatly affected by dielectric loss. The dielectric loss increases in proportion to the product of the square root of the dielectric constant of the material and the dielectric loss tangent of the material. For this reason, the insulating layer in contact with the conductor is required to be made of a material with both a low dielectric constant and a low dielectric loss tangent. Although the sealing material that seals the semiconductor element is not located in close proximity to the conductor, the transmission loss can be effectively suppressed by using a material with excellent dielectric properties. Therefore, the resin sheet of the present disclosure is suitable for use in the fifth generation communication system (5G) and the next generation communication system (beyond 5G), etc.

[0021] The upper limit of the dielectric constant is more preferably 2.8, more preferably 2.6, and even more preferably 2.5. The lower limit of the dielectric constant is not particularly limited, but is preferably 1.5 from the viewpoint of productivity. The upper limit of the dielectric tangent is more preferably 0.008, more preferably 0.005, and even more preferably 0.004. The lower limit of the dielectric tangent is not particularly limited, but is preferably 0.0001 from the viewpoint of productivity.

[0022] The above-mentioned relative dielectric constant and dielectric loss tangent after heating the resin sheet at 150° C. for 1 hour can be adjusted by the type of resin (A), the number of polar groups of resin (A), the acid value, the acid value of the thermosetting composition, etc. The type and acid value of resin (A) will be described later.

[0023] The total content of the resin (A) and the crosslinking agent (B) in the present resin sheet (total mass) is preferably from 70 to 100 mass %, more preferably from 80 to 95 mass %.

[0024] The resin sheet preferably has a peel strength of 2 N / cm or more under the following measurement conditions. That is, the resin sheet is sandwiched between two 50 μm PPS substrates and thermocompressed at 5 MPa and 80° C. Then, heat treatment is performed at 150° C. for 1 hour. Then, a wet heat test is performed for 2 weeks under conditions of 121° C. and 100% humidity. After these steps, a peel test is performed between one PPS substrate and the resin sheet for this test piece at a peel angle of 90° and a peel speed of 300 mm / min. The lower limit of the peel strength is more preferably 2.5 N / cm, even more preferably 3 N / cm, and even more preferably at least a part of the material is broken. By setting the peel strength to 2 N / cm or more, a resin sheet that can provide a sealing layer with excellent mechanical properties can be provided.

[0025] The thickness of the resin sheet can be appropriately designed. For example, the thickness of the resin sheet can be set to 1 to 1000 μm. From the viewpoint of coverage and handling, 1 to 500 μm is preferable, 3 to 300 μm is more preferable, and 10 to 150 μm is even more preferable. By setting the thickness Ta of the resin sheet to 1 μm or more, the pressure in the pressing process is diffused within the resin sheet, and sufficient coverage is exhibited. By setting the thickness of the resin sheet to 1000 μm or less, the degree of design freedom can be increased. In addition, the pressure loss absorbed by the resin sheet against the pressure applied in the pressing process is small, and the resin (A) etc. flows sufficiently, so that excellent coverage is exhibited.

[0026] From the viewpoint of coating strength, the Tg of the resin sheet after heating at 150° C. for 1 hour is preferably 0 to 100° C. The lower limit of the Tg is more preferably 10° C., and further preferably 15° C. The upper limit of the Tg is more preferably 80° C., and further preferably 45° C.

[0027] From the viewpoint of coating properties, the tensile storage modulus of this resin sheet at 10 Hz and 25°C after heating at 150°C for 1 hour is 5×10 6 ~5×10 9 Preferably, the concentration is 1×10 7 ~3×10 9 More preferably, it is 2×10 7 ~1×10 9Furthermore, the resin sheet has a tensile storage modulus of 10 Hz and 150°C after being heated at 150°C for 1 hour of 1×10 5 ~1×10 7 Preferably, 5×10 5 ~5×10 6 More preferably, it is 7×10 5 ~2×10 6 It is even more preferable that:

[0028] From the viewpoint of achieving a balance between handling ease and heat resistance of the coating film, the Tan δ peak value at 23° C. after heating the resin sheet at 150° C. for 1 hour is preferably 0.3 to 1.2, more preferably 0.5 to 1.1, and even more preferably 0.6 to 1.0. The tensile storage modulus and Tan δ peak value can be adjusted by the type of resin (A) and the type and amount of crosslinking agent (B).

[0029] Conventionally, liquid inks and the like have been used as sealing layers, but there are problems with productivity. The sealing film of Patent Document 3 can increase productivity in that the sealing layer can be filled in the recesses between semiconductor chips all at once, but has a problem that it is difficult to handle due to its high fluidity. When changing from the filling type to the covering type as in Patent Document 3, that is, when the sealing layer is covered along the shape of the semiconductor element, gaps are likely to occur between the adherend and the covering layer at the corners of the unevenness formed by mounting the semiconductor element, especially at right angles, and further, gaps are likely to occur over time, resulting in low storage stability.

[0030] According to the present resin sheet, the sealing layer can be formed in a lump along the shape of the semiconductor element, so that the material loss of the resin sheet can be suppressed. In addition, since the resin sheet can be coated in a lump, the productivity and the degree of freedom in design can be significantly improved. Furthermore, since the breaking elongation rate at 23°C after heating the resin sheet at 150°C for 1 hour is within the above range, the gaps that occur at the corners (especially parts with right angles, etc.) between the adherend (semiconductor element, etc.) and the coating layer, which was previously difficult to achieve, can be significantly improved, and excellent coating properties can be achieved. After the sealing layer is formed, other functional layers such as a conductive layer may be further coated. According to this method, the functional layers can be stacked in the same equipment, so that productivity is excellent.

[0031] 1-1.Thermosetting composition The resin sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B). The crosslinking agent (B) preferably has two or more functional groups. At least one of the resin (A) and the crosslinking agent (B) contains a thermosetting component. It is preferable that the resin (A) and the crosslinking agent (B) are mutually cured by heat treatment. Note that a part of the thermosetting component may be cured at the stage of the resin sheet.

[0032] 1-1a.Resin (A) Resin (A) functions as a binder to adhere to and fix the adherend. Resin (A) is preferably a thermosetting resin, but thermoplastic resins, photocurable resins, and mixtures thereof may also be used as resin (A). Thermosetting resins are resins that have multiple functional groups that can be used in crosslinking reactions by heating, and may have functional groups that can self-crosslink.

[0033] The functional group of the thermosetting resin may be appropriately selected depending on the combination with the crosslinking agent (B) described later, and examples thereof include a hydroxyl group, a carboxyl group, an amino group, an epoxy group, an oxetanyl group, an oxazoline group, an oxazine group, an aziridine group, a thiol group, an isocyanate group, a blocked isocyanate group, and a silanol group. From the viewpoint of reactivity, the functional group is preferably a carboxyl group, a hydroxyl group, or an epoxy group.

[0034] The acid value of the thermosetting resin is preferably 1 to 30 mgKOH / g, more preferably 2 to 20 mgKOH / g, and even more preferably 3 to 15 mgKOH / g. By setting the acid value of the resin (A) to 1 mgKOH / g or more, the crosslinking density with the crosslinking agent (B) can be optimized while maintaining good intermolecular forces with the adherend such as a semiconductor element, and the sealing property can be improved. In addition, by setting the acid value of the resin (A) to 30 mgKOH / g or less, the adhesion can be improved while maintaining good intermolecular forces with the adherend such as a semiconductor element.

[0035] The content of resin (A) in the present resin sheet (total mass) is preferably 50 to 99.5 mass%. Examples of resin (A) include amide resins, imide resins, (meth)acrylic resins, maleic acid resins, butadiene resins, urethane resins such as urethane resins and urethane urea resins, oxetane resins, phenoxy resins, polyamide-imide resins, alkyd resins, amino resins, polylactic acid resins, oxazoline resins, benzoxazine resins, silicone resins, and fluororesins. Among these, resin (A) preferably contains a urethane resin including a urethane resin and / or a urethane urea resin.

[0036] The weight average molecular weight (Mw) of the resin (A) can be appropriately designed, but is preferably 10,000 to 1,000,000 from the viewpoint of increasing the mechanical strength of the sealing layer and enhancing the storage stability of the resin sheet. From the viewpoint of durability and adhesion, it is more preferably 25,000 to 300,000, and even more preferably 50,000 to 200,000. The ratio (Mw / Mn) of the number average molecular weight (Mn) and Mw, which indicates the degree of dispersion of the resin (A), is preferably 1 to 17, more preferably 5 to 14, and even more preferably 6.5 to 10. By setting the Mw / Mn to 1 to 17, it becomes easier to control the fluidity of the resin, and the covering property is improved. In addition, the speed at which the resin wets the adherend is made uniform, thereby improving the adhesion.

[0037] The urethane resin can be appropriately designed and is not limited, but a urethane resin (A1) containing a structural unit derived from at least one polyol of dimer diol and trimer triol, and / or a structural unit derived from at least one polyamine of dimer diamine and trimer triamine, and having a urethane bond and optionally having a urea bond is preferred. Hereinafter, the structures derived from the structural units are also collectively referred to as "dimer structures". The urethane bond is formed by the reaction of a hydroxyl group with an isocyanate group, and the urea bond is formed by the reaction of an amino group with an isocyanate group. The urethane resin is obtained by urethane bonding of reactive components including two or more polyol components in one molecule and a polyisocyanate component having two or more isocyanate groups in one molecule. The urethane urea resin is obtained, for example, by reacting a urethane prepolymer of terminal isocyanate obtained by reacting a polyol with a polyisocyanate with a chain extender such as a polyamine component having two or more amino groups in one molecule.

[0038] By using a urethane resin (A1) that combines a dimer structure with a urethane bond or a urethane bond and a urea bond, excellent flexibility and an appropriate elongation at break at 23°C after heat treatment of the resin sheet at 150°C for 1 hour are obtained, resulting in excellent sealing properties. In addition, it is believed that the unshared electron pair of the nitrogen atom contained in the urethane bond, etc., prevents the sealing layer from breaking or rupturing, thereby realizing not only excellent covering properties but also strong adhesive strength with the adherend.

[0039] Suitable examples of the urethane resin (A1) include a urethane resin (A1-1) having a dimer structure, a urethane bond, and no urea bond, and a urethane urea resin (A1-2) having a dimer structure and a urethane bond and a urea bond. The urethane resin (A1) is used alone or in combination of two or more. By using the urethane resin (A1), it is possible to achieve both excellent sealing properties for semiconductor elements, adhesion to various adherends, and adhesiveness. In addition, there is an advantage in that the biomass degree can be increased.

[0040] Dimer diol is obtained by reducing the carboxy group of dimer acid, and trimer triol is obtained by reducing the carboxy group of trimer acid to alcohol. Dimer diamine and trimer triamine can be obtained by, for example, amidating the carboxy group of dimer acid and trimer acid, respectively, and converting them to amines by Hofmann rearrangement. The carboxy group of dimer acid may be converted to an isocyanate group by Curtius rearrangement, and the dimer polyisocyanate having at least dimer diisocyanate and trimer triisocyanate may be used for the synthesis of urethane resin (A1).

[0041] An example of a commercially available dimer diol product is "Pripol 2033" manufactured by Croda Japan.

[0042] Commercially available dimer diamine products include, for example, "Priamine 1071", "Priamine 1073", "Priamine 1074", and "Priamine 1075" manufactured by Croda Japan, and "Versamine 551" and "Versamine 552" manufactured by BASF Japan.

[0043] The ratio of the monomer having a dimer structure used in polymerization of the urethane resin (A1) is preferably 25 to 100% by mass per 100% by mass of all monomers used in the synthesis. By making it 25% by mass or more, the covering property that follows the unevenness between a plurality of semiconductor elements can be improved. The lower limit is more preferably 40% by mass, and even more preferably 50% by mass. The upper limit is more preferably 90% by mass, and even more preferably 70% by mass. The ratio of the constitutional unit having a dimer structure can be calculated from the content (% by mass) of the monomer having a dimer structure in 100% by mass of all monomers among the raw material monomers used in synthesizing the urethane resin (A1). Usually, the ratio of the monomers used in the synthesis is equivalent to the constitutional ratio in the resin.

[0044] Dimer acids are produced from unsaturated fatty acids (e.g., oleic acid and linolenic acid are examples of unsaturated fatty acids with 18 carbon atoms) derived from natural products such as vegetable oils. For example, they are liquid dibasic acids that are produced by dimerization by reacting double bonds with each other by adding a catalyst at 200°C or higher. Dimer acids do not have a single skeleton, but have multiple structures, and there are several types of isomers. Dimer acids obtained from unsaturated fatty acids with 18 carbon atoms include, for example, monocyclic, aromatic, polycyclic, and linear types as shown in (1) below. [ka]

[0045] Trimer acid is usually a by-product of dimer acid production. Like dimer acid, trimer acid has isomers. Dimer acid is usually a mixture of dimer acid and trimer acid, and commercially available dimer polyol is usually a mixture containing dimer diol and trimer triol. Similarly, commercially available dimer diamine is usually a mixture containing dimer diamine and trimer triamine.

[0046] The unsaturated fatty acid is preferably a raw material having 10 to 30 carbon atoms, more preferably an unsaturated fatty acid having 12 to 24 carbon atoms. Specific examples of unsaturated fatty acids include natural fatty acids such as soybean oil fatty acid, tall oil fatty acid, rapeseed oil fatty acid, and the like, and oleic acid, linoleic acid, linolenic acid, and erucic acid, which are obtained by refining these fatty acids. The unsaturated bonds may be hydrogenated as necessary to reduce the degree of unsaturation. Dimer polyamines and dimer polyols with reduced degrees of unsaturation are suitable in terms of oxidation resistance (particularly coloring in high temperature ranges) and suppression of gelation during synthesis. The urethane resin (A1) has a dimer structure derived from one or more types of monomers.

[0047] The urethane resin (A1) preferably has, in addition to a dimer structure, a structural unit derived from a monomer containing an alicyclic structure (excluding structural units derived from a monomer having a dimer structure. Hereinafter, also referred to as an alicyclic structure). By using the urethane resin (A1) in which a dimer structure and an alicyclic structure are combined, the adhesion in the sealing layer can be more effectively improved.

[0048] From the viewpoint of achieving better water resistance, it is preferable to contain 0 to 200 parts by mass of a monomer (m2) having an alicyclic structure (hereinafter also referred to as monomer (m2). Monomers corresponding to monomer (m1) are not included in (m2)) relative to 100 parts by mass of a monomer (m1) having a dimer structure used in the synthesis of the urethane resin (A1) (hereinafter also referred to as monomer (m1)). The lower limit of the content is more preferably 25 parts by mass, and even more preferably 40 parts by mass. The upper limit of the content is more preferably 130 parts by mass, and even more preferably 80 parts by mass. The monomer (m2) is preferably a low molecular weight compound. The molecular weight is preferably 50 to 800, and more preferably 100 to 250.

[0049] The type of monomer (m2) is not limited. When the monomer (m2) is a polyol, suitable examples include 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol and mixtures thereof, 1,3-cyclohexanediol, 1,4-cyclohexanediol and mixtures thereof, and hydrogenated bisphenol A. Among these, there is 1,4-cyclohexanedimethanol. In 100% by mass of polyol used in the synthesis of the urethane resin (A1), the content of dimer polyol is preferably 50 to 100% by mass, more preferably 60 to 99% by mass, and further preferably 70 to 97% by mass.

[0050] When the monomer (m2) is a polyisocyanate, suitable examples include hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, etc. These may be polymeric compounds such as trimers. Preferred examples of the monomer (m2) as a polyamine include isophorone diamine (IPDA), menthene diamine, norbornane diamine, tricyclodecane diamine, adamantane diamine, diaminocyclohexane, 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-3,6-diethylcyclohexane, diaminodiethylmethylcyclohexane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (bis(4-amino-3-methylcyclohexyl)methane), 3,3',5,5'-tetramethyl-4,4'-diaminodicyclohexylmethane, and 4,4'-diaminodicyclohexylmethane. Among these, isophorone diamine is preferred.

[0051] The urethane resin (A1) preferably has a structural unit derived from a monomer containing a polyolefin structure (excluding structural units derived from a monomer having a dimer structure) in addition to the dimer structure. Hereinafter, this is also referred to as a polyolefin structure. By using the urethane resin (A1) in which a dimer structure and a polyolefin structure are combined, the dielectric properties of the sealing layer can be more effectively improved. From the viewpoint of the balance between the flexibility and heat resistance of the coating film, the number average molecular weight of the monomer having a polyolefin structure is preferably 500 to 5,000, more preferably 1,000 to 3,000.

[0052] From the viewpoint of improving the dielectric properties, it is preferable to contain 0 to 100 parts by mass of a monomer (m3) having a polyolefin structure (hereinafter also referred to as monomer (m3). Monomers corresponding to monomers (m1) or (m2) are not included in (m3)) relative to 100 parts by mass of a monomer (m1) having a dimer structure used in the synthesis of the urethane resin (A1). The lower limit of the content is more preferably 1 part by mass, and even more preferably 2 parts by mass. Moreover, the upper limit of the content is more preferably 70 parts by mass, and even more preferably 45 parts by mass.

[0053] The type of monomer (m3) is not limited. A suitable example of the monomer (m3) is a polyol, and it is a hydrogenated polyolefin. A suitable example of the hydrogenated polyolefin is polybutadiene polyol. A commercially available product can be used as it is. Examples of commercially available hydrogenated polybutadiene polyols include GI-1000, GI-2000, and GI-3000 (trade names of Nippon Soda Co., Ltd.), "R-45EPI" (trade name of Idemitsu Petrochemical Co., Ltd.), "Polytail H" (trade name of Mitsubishi Chemical Corporation), "KRASOL HLBH-P2000" and "KRASOL HLBH-P3000" (trade name of Cray Valley Corporation). The number average molecular weight (Mn) of the hydrogenated polybutadiene polyol is 500 to 10,000 from the viewpoint of lamination suitability and tack reduction. The lower limit of the Mn is more preferably 800, and even more preferably 1,000. The upper limit of the Mn is more preferably 5000, further preferably 3000, and further preferably 2500. The larger the molecular weight of the polyolefin structure, the greater the effect of lowering the dielectric constant.

[0054] Furthermore, in order to adjust the acid value, it is preferable to use a diol having a carboxy group in the molecule as a monomer. Suitable examples include dimethylolpropionic acid (DMPA), dimethylolbutanoic acid (DMBA), N,N-bishydroxyethylglycine, and methyl 3-[bis(2-hydroxyethyl)amino]propionate. Among these, dimethylolpropionic acid and dimethylolbutanoic acid are preferable from the viewpoint of solubility in a solvent. By using a diol having a carboxy group in the molecule, a carboxy group can be introduced into the urethane resin (A1-1) and the urethane urea resin (A1-2), and crosslinking with a crosslinking agent (B) having, for example, an epoxy group or a carbodiimide group can be imparted.

[0055] Monomer components other than those mentioned above may be used within the scope of the present disclosure. For example, polyol components such as aromatic polyol, polyether polyol, polyester polyol, polycarbonate polyol, polycaprolactone diol, polycarbonate polyol, polyacrylate polyol, polysiloxane polyol, polyisoprene polyol, and polybutadiene polyol can be exemplified. In addition, polyamine components such as aromatic-containing aliphatic polyamine, aromatic polyamine, and polyamine having a heterocyclic structure can be exemplified. Further, aromatic polyisocyanate, aliphatic polyisocyanate, trimer or polymeric compound thereof, allophanate type polyisocyanate, and biuret type polyisocyanate can be exemplified. In the above monomers, a monomer having an alicyclic structure is referred to as a monomer (m2). Similarly, in the above monomers, a monomer having a polyolefin structure is referred to as a monomer (m3). The same applies below.

[0056] From the viewpoint of achieving excellent resistance to moist heat, it is preferable that the composition does not contain a "polyester structure" such as polyester polyol, or a "polycarbonate structure" such as polycarbonate polyol.

[0057] Specific examples of other monomers in the polyol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, and 2-monoglycerin ether. Specific examples of other monomers in polyisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl diisocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, butane-1,4- Examples of the polyisocyanates include diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, xylylene diisocyanate, dimeryl diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, bis-chloromethyl-diphenylmethane-diisocyanate, and 2,6-diisocyanate-benzyl chloride. These may be trimers to form an isocyanurate ring structure. These polyisocyanates may be used alone or in combination of two or more. Among these, tolylene diisocyanate xylylene diisocyanate, hexamethylene diisocyanate, and isocyanurate of hexamethylene diisocyanate are preferred. Specific examples of other monomers of polyamines are not particularly limited, but diamines are preferred because of the ease of adjusting Mw.Specific examples include diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, pentamethylenediamine, and p-phenylenediamine, as well as diamines having hydroxyl groups such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropyldiamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, di-2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine.These polyamines can be used alone or in combination of two or more.

[0058] From the viewpoint of imparting coating hardness, it is preferable to include a structural unit derived from a polyfunctional polyamine having three or more functional groups. Specific examples of polyamines having three or more functional groups include diethylenetriamine, iminobispropylamine (IBPA, 3,3'-diaminodipropylamine), triethylenetetramine, N-(3-aminopropyl)butane-1,4-diamine (spermidine), 6,6-iminodihexylamine, 3,7-diazanonane-1,9-diamine, and N,N'-bis(3-aminopropyl)ethylenediamine. It is preferable that the polyfunctional polyamine has three amino groups. It is further preferable to use it in combination with a diamine. As other polyamines, hexamethylenediamine, iminobispropylamine, and bisanilinefluorene are suitable.

[0059] Monoamines may also be added during the synthesis of the urethane urea resin (A1-2). The monoamines act as reaction terminators when producing the urethane urea resin (A1-2), binding to the molecular end of the urethane urea resin (A1-2) and inhibiting further reaction. As the amount of monoamine used increases, the molecular weight of the urethane urea resin decreases, so the final molecular weight of the urethane urea resin (A1-2) can be adjusted by changing the combined ratio of the amount of polyamine and the amount of monoamine. Examples of monoamines include n-butylamine, di-n-butylamine (DnBA), n-propylamine, n-pentylamine, n-hexylamine, n-octylamine, benzylamine (BA), and dibenzylamine. Furthermore, by using a monoamine having a reactive functional group other than an amino group, a new reactive functional group can be introduced to the end of the urethane urea resin (A1-2). Examples of the monoamine having a reactive functional group other than an amino group include monoamines having a phenolic hydroxyl group, monoamines having a non-phenolic hydroxyl group, and monoamines having a sulfanyl group (also called a mercapto group or a thiol group). Examples of the monoamine having a phenolic hydroxyl group include 2-aminophenol (2-AM), 3-aminophenol (3-AM), 4-aminophenol (4-AM), 2-(aminomethyl)phenol, acetaminophen, and 2-(butylamino)phenol. Examples of the monoamine having a non-phenolic hydroxyl group include monoethanolamine, diethanolamine, aminopropanol, and aminobutanol. Examples of the monoamine having a sulfanyl group include 4-aminothiol.

[0060] From the viewpoints of improving conformability to semiconductor elements having uneven shapes and preventing cracks and breakage, the content of the urethane resin (A1) is preferably 50 to 100 parts by mass, more preferably 70 to 99.9 parts by mass, and even more preferably 80 to 99 parts by mass, per 100 parts by mass of the resin (A).

[0061] The acid value of the urethane resin (A1) is preferably 1 to 30 mg / KOH, more preferably 3 to 20 mg / KOH, and even more preferably 5 to 15 mg / KOH, from the viewpoint of adjusting the relative dielectric constant and the dielectric loss tangent of the resin sheet under the above conditions. The acid value of the urethane resin (A1) can be adjusted, for example, by the amount of a diol component having a carboxyl group added as a chain extender.

[0062] Any reactive functional group can be introduced into the urethane resin (A1). Specific examples include a carboxy group, a phenolic hydroxyl group, a hydroxyl group (a hydroxyl group other than a phenolic hydroxyl group), and a sulfanyl group (also called a mercapto group or a thiol group). From the viewpoint of achieving a balance between adhesion and storage stability, a phenolic hydroxyl group and a hydroxyl group (a hydroxyl group other than a phenolic hydroxyl group) are preferred, and a phenolic hydroxyl group is more preferred.

[0063] The Mw of the urethane resin (A1), like that of the resin (A), is preferably from 10,000 to 1,000,000, more preferably from 25,000 to 300,000, and even more preferably from 50,000 to 200,000. By setting the Mw of the urethane resin (A1) within the above range, the breaking elongation can be made appropriate, and cracks and breakage can be effectively prevented.

[0064] The Tg of the urethane resin (A1) is preferably −10 to 100° C., more preferably 0 to 70° C., and even more preferably 5 to 40° C. By setting the Tg of the urethane resin (A1) within the above range, the present resin sheet has excellent flexibility and coverage.

[0065] The amine value of the urethane resin (A1) is preferably from 0.1 to 15 mgKOH / g, more preferably from 0.5 to 10 mgKOH / g. By setting the amine value of the urethane resin (A1) within the above range, excellent dielectric properties are obtained.

[0066] The hydroxyl value of the urethane resin (A1) is preferably from 1 to 50 mgKOH / g, more preferably from 3 to 30 mgKOH / g. By setting the hydroxyl value of the urethane resin (A1) within the above range, the dielectric properties are excellent.

[0067] The method for producing the urethane resin (A1) is not particularly limited, and it can be produced by a known method. The urethane resin (A1-1) can be obtained, for example, by reacting a polyol and a polyisocyanate. The urethane urea resin (A1-2) can be obtained, for example, by reacting a urethane prepolymer having an isocyanate terminal, which is made of a polyol and a polyisocyanate, with a polyamine and, if necessary, a polymerization terminator. For example, there is a prepolymer method in which a polyol and a polyisocyanate are reacted at a temperature of 50°C to 150°C (urethane reaction) using a solvent inactive to an isocyanate group as necessary, and further using a urethane catalyst as necessary, to produce a prepolymer having an isocyanate group at the end, and then the prepolymer is reacted with a polyamine at 10°C to 60°C to obtain a urethane urea resin. In the synthesis of the urethane urea resin (A1-2), the ratio of the total molar number of the amino groups of the polyamine to the molar number of the isocyanate groups in the prepolymer is preferably 0.9 to 2.00, more preferably 0.95 to 1.1. As another method, a one-shot method is also suitable in which a high molecular weight polyol, a polyisocyanate, and a polyamine (and a polymerization terminator as necessary) are reacted in one step to obtain the urethane resin (A1). The polyamine may be used in the urethane reaction of the polyol and the polyisocyanate.

[0068] In order to introduce a dimer structure into the urethane resin (A1-1), a dimer polyol and / or a dimer diisocyanate, etc. are used. In order to introduce a dimer structure into the urethane urea resin (A1-2), a dimer polyol, a dimer diisocyanate, and / or a dimer polyamine, etc. are used.

[0069] From the viewpoint of imparting coating hardness, it is preferable to include a structural unit derived from a polyfunctional polyamine having three or more functional groups. A polymerization terminator may be used for the purpose of adjusting Mw, etc. The polymerization terminator is not limited, but examples thereof include monovalent active hydrogen compounds such as monoamine compounds having primary or secondary amino groups.

[0070] In producing the prepolymer of the urethane resin (A1-1) or the urethane urea resin (A1-2), the amount of the polyol and the polyisocyanate is preferably in the range of an NCO / OH ratio, which is the ratio of the number of moles of the isocyanate group of the polyisocyanate to the number of moles of the total hydroxyl group of the polymer polyol, of 1.0 to 3.0, more preferably 1.1 to 1.5.

[0071] In terms of reaction control, it is preferable to use an organic solvent in the synthesis of the prepolymer of the urethane resin (A1-1) or the urethane urea resin (A1-2). The organic solvent is preferably an organic solvent inactive to an isocyanate group, such as ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethers such as dioxane and tetrahydrofuran; and esters such as ethyl acetate, butyl acetate, and propyl acetate. These are used alone or in combination of two or more.

[0072] Furthermore, a catalyst may be used in the synthesis of the prepolymer of the urethane resin (A1-1) or the urethane urea resin (A1-2). Examples of the catalyst include tertiary amine catalysts such as triethylamine and dimethylaniline, and metal catalysts such as tin and zinc. These catalysts are usually used in the range of 0.001 to 1 mol % based on the polyol compound.

[0073] 1-1b. Crosslinking agent (B) The crosslinking agent (B) is a component that can be crosslinked by a curing treatment, and is preferably a component that can be cured by forming a three-dimensional crosslinked structure with the resin (A). By using the crosslinking agent (B), the crosslinking reaction with the reactive functional group of the resin (A) occurs during the heat pressing or heat aging in the pressing process, thereby making the adhesion to the adherend such as a semiconductor element stronger. The crosslinking agent (B) preferably has a plurality of functional groups capable of reacting with the functional groups of the resin (A). Examples of the crosslinking agent (B) include known compounds such as silane coupling agents, epoxy compounds, acid anhydride group-containing compounds, imidazole compounds, isocyanate compounds, aziridine compounds, and amine compounds. From the viewpoint of adjusting the elongation at break at 23°C after the heat treatment of the resin sheet, silane coupling agents, epoxy compounds, aziridine compounds, imidazole compounds, and isocyanate compounds are preferred, and epoxy compounds are more preferred.

[0074] The epoxy compound is not particularly limited as long as it has an epoxy group in the molecule. For example, epoxy resins such as glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, or cyclic aliphatic (alicyclic) epoxy resins can be used. In order to improve the heat resistance and adhesion of the coating film, multifunctional epoxy resins having three or more functionalities are useful, and when flexibility of the coating film is required, bifunctional epoxy resins such as bisphenol A type and bisphenol F type are useful. Examples of glycidyl ether type epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AD ​​type epoxy resins, cresol novolac type epoxy resins, phenol novolac type epoxy resins, α-naphthol novolac type epoxy resins, bisphenol A type novolac type epoxy resins, dicyclopentadiene type epoxy resins, tetrabromobisphenol A type epoxy resins, brominated phenol novolac type epoxy resins, tris(glycidyloxyphenyl)methane, and tetrakis(glycidyloxyphenyl)ethane. Examples of the glycidylamine type epoxy resin include tetraglycidyldiaminodiphenylmethane, triglycidylparaaminophenol, triglycidylmetaaminophenol, and tetraglycidylmetaxylylenediamine. Examples of glycidyl ester type epoxy resins include diglycidyl phthalate, diglycidyl hexahydrophthalate, and diglycidyl tetrahydrophthalate. Examples of cyclic aliphatic (alicyclic) epoxy resins include epoxycyclohexylmethyl-epoxycyclohexanecarboxylate, or bis(epoxycyclohexyl)adipate. As the epoxy compound, one of the above compounds may be used alone, or two or more of them may be used in combination. As the epoxy compound, from the viewpoints of high adhesiveness and heat resistance, bisphenol A type epoxy resin, cresol novolac type epoxy resin, phenol novolac type epoxy resin, tris(glycidyloxyphenyl)methane, or tetrakis(glycidyloxyphenyl)ethane are preferred. Examples of commercially available products include bisphenol A type epoxy resins such as jER828, 1002, and 1004, both available from Mitsubishi Chemical Corporation; novolac type epoxy resins such as jER152 and 154, both available from Mitsubishi Chemical Corporation, and YDPN-638 and YDCN-700, both available from Nippon Steel Chemical & Material Co., Ltd.; bisphenol F type epoxy resins such as YDF-170 and YDF2001, both available from Nippon Steel Chemical & Material Co., Ltd.; and multifunctional epoxy resins having three or more functional groups, such as JER1031S and 1032H60, both available from Mitsubishi Chemical Corporation, TETRAD-X, both available from Mitsubishi Gas Chemical Company, Inc., and TECHMORE VG3101L, both available from Printec Co., Ltd.

[0075] The aziridine compound is not particularly limited as long as it contains an aziridine group in the molecule. For example, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxite), N,N'-toluene-2,4-bis(1-aziridinecarboxite), bisisophthaloyl-1-(2-methylaziridine), tri-1-aziridinylphosphine oxide, N,N'-hexamethylene-1,6-bis(1-aziridinecarboxite), trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, tris-2,4,6-(1-aziridinyl)-1,3,5-triazine, trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-( 1-aziridinyl)butyrate], trimethylolpropane tris[3-(1-(2-methyl)aziridinyl)propionate], trimethylolpropane tris[3-(1-aziridinyl)-2-methylpropionate], 2,2'-bishydroxymethylbutanol tris[3-(1-aziridinyl)propionate], pentaerythritol tetra[3-(1-aziridinyl)propionate], diphenylmethane-4,4-bis-N,N'-ethyleneurea, 1,6-hexamethylene bis-N,N'-ethyleneurea, 2,4,6-(triethyleneimino)-Syn-triazine, bis[1-(2-ethyl)aziridinyl]benzene-1,3-carboxylic acid amide. Among these, 2,2'-bishydroxymethylbutanol tris[3-(1-aziridinyl)propionate] is preferred from the viewpoint of heat resistance.

[0076] The imidazole compounds are 2-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-dimethylimidazole, 2-phenylimidazole, imidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[ Examples of imidazole compounds include 2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole, and further include compounds with improved storage stability such as imidazole compounds encapsulated in microcapsules. Among these, 2-phenylimidazole is preferred from the viewpoint of storage stability.

[0077] The isocyanate compound is not particularly limited as long as it has an isocyanate group in the molecule. In particular, hexamethylene diisocyanate trimer having an isocyanurate ring and blocked with MEK oxime or pyrazole is preferred from the viewpoint of heat resistance.

[0078] In the present disclosure, it is preferable to contain two or more crosslinking agents from the viewpoint of improving water-resistant insulation and covering properties. A suitable example includes a suitable example including two or more selected from a silane coupling agent, an epoxy compound, an aziridine compound, an imidazole compound, and an isocyanate compound. An example in which any one or more of a silane coupling agent, an epoxy compound, an aziridine compound, an imidazole compound, and an isocyanate compound is used in combination with an epoxy compound of a different type from the epoxy compound is even more suitable. Among these, a combination including two or more selected from an epoxy compound, an aziridine compound, and an imidazole compound is more suitable.

[0079] The content of the crosslinking agent (B) (total content when two or more types are used in combination) is preferably 0.01 to 30 mass%, more preferably 0.05 to 20 mass%, and even more preferably 0.1 to 10 mass%, based on the total mass of the resin sheet. By setting the content to the above content (0.01 to 30 mass%), it is possible to suitably adjust the water-resistant insulation property and the covering property while improving the compatibility with the resin (A). Furthermore, the content of the crosslinking agent (B) relative to the resin (A) is preferably 0.1 to 20 mass parts of the crosslinking agent (B) relative to 100 mass parts of the resin (A) from the viewpoint of the coating film strength, more preferably 1 to 10 mass parts, and even more preferably 3 to 6.5 mass parts.

[0080] 1-1c.Other ingredients Organic fillers such as resin beads and inorganic fillers such as metal oxides can be used as additives for adjusting the elongation at break at 23° C. after heating the resin sheet for 1 hour at 150° C. The amount of organic filler and / or inorganic filler added (total content when both are used) is preferably 0.1 to 30% by mass, more preferably 0.3 to 15% by mass, and even more preferably 0.5 to 5% by mass, relative to 100% by mass of the total amount of the resin sheet.

[0081] Examples of additives for adjusting the breaking elongation include organic fillers such as poly(meth)acrylate beads, acrylic-styrene copolymer beads, polycarbonate beads, polyvinyl chloride beads, polytetrafluoroethylene powder, polyethylene powder, epoxy resin powder, polyamide powder, polyurethane powder, polysiloxane powder, and polymer fillers such as silicone, acrylic, styrene-butadiene rubber, and butadiene rubber having a multilayered core-shell structure. Examples of inorganic fillers include inorganic compounds such as silica, alumina, magnesium hydroxide, barium sulfate, calcium carbonate, titanium oxide, zinc oxide, antimony trioxide, magnesium oxide, talc, kaolinite, mica, basic magnesium carbonate, sericite, montmorolinite, kaolinite, bentonite, boron nitride, aluminum nitride, titanium nitride, and carbon black. Among these, from the viewpoint of coating film resistance against scratches, titanium oxide, titanium nitride, silica, talc, mica, kaolinite, or montmorillonite is preferred, and titanium oxide, titanium nitride, and silica are more preferred. In the present disclosure, from the viewpoint of coating film resistance, two or more types of inorganic fillers may be contained. Specifically, an example containing a combination of silica and one or more types selected from titanium oxide, titanium nitride, silica, talc, mica, kaolinite, or montmorillonite is preferred.

[0082] The average primary particle size (hereinafter referred to as particle size) of the inorganic filler is preferably 1 to 100 nm. By making the particle size 1 nm or more, it is easy to maintain the viscosity of the resin composition at a level suitable for coating. Furthermore, by making the particle size 100 nm or less, the coating film resistance is improved. The particle size of the inorganic filler can be determined from the average value of about 20 primary particles observed from an image magnified about 50,000 to 1,000,000 times by a transmission electron microscope (TEM).

[0083] The inorganic filler may be mixed with the resin (A) after mechanical crushing, and the mixture may be further dispersed. A dispersant is preferably used for the dispersion treatment. The dispersant can impart repulsive forces between the inorganic fillers so that the inorganic fillers dispersed through the above-mentioned dispersion treatment do not aggregate again. As the dispersant, a conventionally known compound can be used. For example, a polymer dispersant, a pigment derivative dispersant, or a surfactant selected from cationic, anionic, or nonionic surfactants can be used. The Mw of these dispersants is, for example, about 1,000 to 30,000.

[0084] The resin sheet may contain a curing accelerator to adjust the crosslinking rate during the curing process or the physical properties of the resin sheet. The curing accelerator is not particularly limited and can be selected appropriately. Specific examples of the curing accelerator include amine-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. These are used alone or in combination of two or more. From the viewpoint of coating suitability, the content of the curing accelerator is preferably from 0.01 to 10 mass %, and more preferably from 0.1 to 5 mass %, based on the total amount (100 mass %) of the resin sheet.

[0085] The thermosetting composition of the present disclosure may further contain various additives within the scope of the present disclosure. For example, a thermally conductive filler, a conductive filler, etc. may be exemplified. Furthermore, additives such as an antistatic agent, a flame retardant, an antioxidant, an ultraviolet light inhibitor, a colorant, a dispersant, a surface conditioning additive, a curing retarder, a softener, an antiblocking agent, an adhesion improver, and an embedding improver may be appropriately added.

[0086] 2.Laminated sheet The laminate sheet of the present disclosure (also referred to as the present laminate sheet) is a sheet in which the present resin sheet and one or more functional sheets are laminated. The functional sheet is not particularly limited. Specifically, examples of the functional sheet include an electromagnetic wave shielding sheet, a heat conductive sheet that dissipates heat from a semiconductor element, a shielding sheet that prevents the semiconductor element from being seen or blocks light, a moisture-proof sheet that protects the semiconductor element from moisture, a decorative sheet, a flame-retardant sheet that has been given flame retardancy, a protective sheet that has been given hard coat properties, a bonding sheet that improves bonding with a semiconductor element, etc., and any combination of these functional sheets. A functional layer can be formed by covering the functional sheet of the present laminate sheet.

[0087] By using this laminate sheet, it is possible to form an encapsulating layer and a functional layer in a semiconductor element at the same time. The properties of the functional sheet in this laminate sheet can be designed as appropriate. It is preferable that the functional sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B), and the functional sheet has an elongation at break of 10 to 400% at 23°C after heating at 150°C for 1 hour. It is more preferable that the laminate sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B), and the functional sheet has an elongation at break of 10 to 400% at 23°C after heating at 150°C for 1 hour.

[0088] It is more preferable that the laminate sheet has a dielectric constant of 3 or less at a frequency of 10 GHz and 23° C. and a dielectric loss tangent of 0.01 or less at a frequency of 10 GHz and 23° C. after heating the functional sheet at 150° C. for 1 hour. It is even more preferable that the laminate sheet has a dielectric constant of 3 or less at a frequency of 10 GHz and 23° C. and a dielectric loss tangent of 0.01 or less at a frequency of 10 GHz and 23° C. after heating the functional sheet at 150° C. for 1 hour.

[0089] When a thermally conductive sheet is used as the functional sheet, it is preferable to add a thermally conductive filler to the thermosetting composition of the present resin sheet. When an electromagnetic wave shielding sheet is used as the functional sheet, a conductive filler may be added to the thermosetting composition of the present resin sheet.

[0090] The thermally conductive filler may be a metal oxide, a metal nitride, a metal hydroxide, a metal carbonate, a metal silicate, a hydrated metal compound, a crystalline silica, a non-crystalline silica, a silicon carbide, or a composite thereof. The conductive filler may be a metal filler, a conductive ceramic filler, or a mixture thereof. The metal filler may be a metal powder such as gold, silver, copper, or nickel, an alloy powder such as solder, or a core-shell type filler such as silver-coated copper powder, gold-coated copper powder, silver-coated nickel powder, or gold-coated nickel powder. However, from the viewpoint of controlling the relative dielectric constant and the dielectric loss tangent, the resin sheet is preferably as low in metal content as possible.

[0091] The content of the inorganic filler (total content when two or more kinds are included) is preferably 0.01 to 20 mass% based on the total amount (100 mass%) of the functional sheet from the viewpoint of coverage, and the lower limit is more preferably 0.1 mass%, and the upper limit is more preferably 15 mass%, more preferably 10 mass%, and even more preferably 5 mass%. By including 0.01 to 20 mass% of the inorganic filler, the effect of increasing the fluidity of the functional sheet in the pressing process is easily exhibited, and coverage is improved. In addition, from the viewpoint of controlling the dielectric properties, the lower the metal content of the functional sheet, the more preferable. In 100 mass% of the inorganic filler, the total amount of the conductive filler and the thermally conductive filler is preferably 0 to 20 mass%, and more preferably 0 to 15 mass%. Examples of the metal oxide include a metal-containing compound having electrical conductivity and an insulating metal oxide, and an insulating metal oxide is preferable.

[0092] 3.Laminate The laminate of the present disclosure is a laminate in which the resin sheet of the present disclosure and a material used in the manufacturing process or until the time of manufacturing are integrated, or a laminate in which the laminate sheet of the present disclosure and a material used in the manufacturing process are integrated. Examples of the material include a cushioning material and a protective sheet. By using the laminate of the present disclosure in the manufacturing method of the semiconductor device of the present disclosure, the manufacturing process can be simplified.

[0093] In the manufacture of the semiconductor device of the present disclosure, as described later, it is not essential to use the present laminate, and the present resin sheet or the present laminate sheet may be used alone. In addition, the present resin sheet and the above-mentioned cushioning material that is not integrated with the present resin sheet may be superimposed in the manufacturing process to cover them together. In addition, after the sealing layer is formed by covering the present resin sheet, a functional sheet may be covered to form a functional layer. Furthermore, a manufacturing process sheet such as a cushioning material or a protective sheet may be superimposed on the present resin sheet or the present laminate sheet to form a sealing layer.

[0094] The deeper the unevenness of the semiconductor element to be encapsulated is, and the shorter the distance between the semiconductor elements is, the lower the encapsulation performance tends to be. However, by using a cushioning material, it is expected that the covering property and flexibility of the resin sheet and the laminated sheet can be more effectively brought out. Furthermore, by protecting the resin sheet and the laminated sheet with a protective sheet, it is possible to effectively prevent the intrusion of dust and the like into the encapsulation layer, etc. From the viewpoint of workability, a release liner is preferable as the protective sheet. In addition, a protective sheet may be provided on the cushioning material so that the cushioning material does not adhere to parts of the manufacturing equipment when the cushioning material is softened.

[0095] Examples of the release liner include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; plastic films such as polyolefin films such as polypropylene and polyethylene; or plastic sheets coated with a release agent such as silicone resin to provide a release layer, etc. The thickness of the release liner is not particularly limited, but is usually about 10 to 200 μm.

[0096] A schematic cross-sectional view showing an example of the present laminate is shown in Figure 1. As shown in the figure, laminate 1 is a laminate in which resin sheet 12 is sandwiched between first release liner 11 and second release liner 13.

[0097] FIG. 2 is a schematic cross-sectional view showing an example of a laminate according to the first modification of the present disclosure. The laminate 2 is a laminate in which a first release liner 11, a resin sheet 12, and a cushioning material 14 are laminated in this order. The cushioning material 14 is a material that softens or melts when heated and / or pressed, and has a function of promoting the conformity of the resin sheet 12 to the semiconductor element. The cushioning material 14 is not particularly limited as long as it is a material having thermoplasticity, but it is preferable that it has a melting temperature and / or Tg lower than the temperature at the time of heating and / or pressing. Suitable examples include a polyolefin sheet, a vinyl chloride sheet, and a PVA sheet. Depending on the depth of the recess formed between the semiconductor elements, the thickness of the cushioning material is usually about 100 μm to 1 mm. When a plurality of cushioning materials 14 are laminated, it is preferable that the total thickness is within this range.

[0098] 3 is a schematic cross-sectional view showing an example of a laminate according to the second modification of the present disclosure. This laminate 3 is composed of four layers: a first release liner 11 / a first resin sheet 12a / a second resin sheet 12b / a second release liner 13. The first resin sheet 12a is temporarily attached onto a semiconductor element. Like the laminate 3, the resin sheet may be composed of multiple layers.

[0099] 4 shows a schematic top view illustrating an example of a laminate according to the third modification of the present disclosure. This laminate 4 is composed of a first release liner 11 / a resin sheet 12 / a conductive pattern 15 / a second release liner 13. The resin sheet 12 is an insulating sheet and mainly performs a sealing function. The conductive pattern 15 is formed in a desired position on the resin sheet 12. The conductive pattern 15 is used for purposes such as electrically connecting the encapsulated semiconductor element and / or the mounting board to the outside.

[0100] 4. Method for producing resin sheet, laminated sheet, and laminate The method for producing the resin sheet is not particularly limited, but a suitable example is a method in which a resin composition obtained by adding an arbitrary solvent to the components constituting the resin sheet is applied to a substrate, etc. The purpose of adding the solvent is to adjust the viscosity to a level suitable for coating. The manufacturing method of this laminated sheet is not particularly limited, but includes a method of forming a functional sheet by a method similar to that of the resin sheet described above and then laminating it with a resin sheet, a method of coating a functional sheet on a resin sheet, or a method of coating a resin sheet on a functional sheet. For coating, a comma coater, a die coater, a roll coater, a lip coater, a reverse coater, a gravure coater, a bar coater, a curtain coater, dip coating, spin coating, silk screen, casting, etc. After coating, the solvent contained in the resin composition can be removed by heating and drying the coating film using a hot air oven, an infrared heater, etc.

[0101] The laminate can be manufactured by a known method. For example, the laminate can be manufactured by laminating each sheet after manufacturing. The laminate 1 in FIG. 1 can be obtained, for example, by coating a resin composition on a first release liner 11, drying the coating film to laminate a resin sheet 12, and laminating a second release liner 13 and the resin sheet 12. The laminate 2 in FIG. 2 can be obtained, for example, by coating a resin composition on a first release liner 11, drying the coating film to laminate a resin sheet 12, and laminating an exposed surface of the resin sheet 12 and a cushioning material 14. The laminate 3 in FIG. 3 can be obtained, for example, by manufacturing a laminate of the first release liner 11 and the first resin sheet 12a constituting the resin sheet, and a laminate of the second release liner 13 and the second resin sheet 12b constituting the resin sheet, respectively, by the same method as the laminate 1, and laminating them. The laminate in Figure 4 can be obtained, for example, by obtaining a laminate of a first release liner 11 / resin sheet 12, forming a conductive pattern 15 on the resin sheet 12 using a photoresist or the like, and laminating a second release liner 13 onto the conductive pattern 15.

[0102] 5. Semiconductor device and manufacturing method thereof The manufacturing method of the semiconductor device of this embodiment is a manufacturing method of a semiconductor device that collectively covers multiple semiconductor elements mounted on a substrate, and includes a step of temporarily attaching the resin sheet to the side of the multiple semiconductor elements, a step of softening the resin sheet by heating and / or pressurizing the resin sheet to cover and bond the upper surface of the substrate and the upper and side surfaces of the multiple semiconductor elements, and a step of hardening the resin sheet to seal the semiconductor elements.

[0103] The resin sheet may be a single layer or a multi-layer resin sheet of the present disclosure. It may also be a laminated resin sheet in which a single layer or a multi-layer resin sheet and one or more functional sheets are laminated. Furthermore, the resin sheet alone or the laminated sheet may be a laminated resin sheet in which materials used in the manufacturing process or until the manufacturing process are integrated.

[0104] An example of a schematic cross-sectional view of the semiconductor device of this embodiment is shown in Fig. 11. An example of a method for manufacturing the semiconductor device 100 will be described with reference to cross-sectional views of the manufacturing steps in Figs. 5 to 10. However, the method for manufacturing the semiconductor device of this embodiment is not limited to the following method. 5, a mounting substrate 21 on which a conductor pattern 22 such as electrode pads and connection wiring is formed is prepared, and a semiconductor element 24 is mounted via bumps 23. The gap between the semiconductor element 24 and the mounting substrate 21 is filled with an underfill material 25. The size of the semiconductor element is, for example, 1000 μm or less in thickness and 1,000,000 μm in plan view area. 2 The thickness is preferably 800 μm or less, and the area in plan view is preferably 640,000 μm or less. 2 More preferably, the thickness is 500 μm or less and the area in plan view is 250,000 μm or less. 2 The following is more preferable: The interval between the semiconductor elements mounted on the substrate is, for example, 10 to 5000 μm.

[0105] Next, the first release liner 11 is peeled off from the laminate 1, and the exposed resin sheet 12 is placed on the semiconductor element 24 for temporary attachment. The temporary attachment can be performed, for example, by heat pressing. Thereafter, the second release liner 13 is peeled off, and a cushioning material 16 is further placed on the resin sheet 12 (see FIG. 6). A protective sheet such as a release sheet (not shown) may be further placed on the cushioning material 16.

[0106] Next, under reduced pressure conditions, heating and / or pressure is applied from the cushion material 16 side, and the resin sheet 12 is softened and deformed by the pressing force of the cushion material 16 to cover the semiconductor element 24 (see FIG. 7). Note that reduced pressure conditions are not essential, and the process may be performed under normal pressure or in a vacuum. Thereafter, the cushion material 16 is peeled off, and the covered resin sheet is thermally cured to form the sealing layer 17 as a cured product (see FIG. 8). Note that, although the method of further performing a thermal curing process after peeling off the cushion material has been described, the thermal curing process may be performed before peeling off the cushion material. The curing reaction progresses during the aforementioned heating and / or pressure application, and by using a resin sheet that has a moderate elongation even in the sealing layer after curing, it is believed that peeling, cracks, and gaps at corners can be suppressed even under room temperature conditions.

[0107] According to the present resin sheet, as shown in Fig. 8, it is possible to cover the recesses formed between semiconductor elements according to their shapes. Therefore, the thickness of the present resin sheet can be determined from the thickness required for the sealing layer. This makes it possible to prevent loss of the present resin sheet compared to the mode in which the recesses are filled as in Patent Document 3. However, in cases where the size of the recesses is small compared to the desired thickness of the sealing layer, there is also a mode in which the present resin sheet is filled into the recesses instead of covering them, and this does not exclude the mode of filling.

[0108] The pressing method is not particularly limited, but a heat press and / or a vacuum press are preferable. From the viewpoint of the filling property of the resin sheet, the temperature during pressing is preferably 20 to 200°C, more preferably 30 to 150°C, further preferably 40 to 130°C, and particularly preferably 60 to 110°C. The curing conditions after peeling off the cushioning material 16 can be appropriately designed as long as the thermosetting resin is cured. For example, the heating temperature is preferably 40 to 250°C, more preferably 80 to 220°C, and further preferably 100 to 190°C. The heating time is preferably 30 to 300 minutes, more preferably 60 to 240 minutes, and further preferably 90 to 180 minutes. By setting the heating temperature and heating time as described above, the curing of the resin composition constituting the resin sheet can be promoted, the residual stress of the sealing layer can be removed, and the quality of the sealing layer can be improved. Through these steps, the sealing layer is formed from the resin sheet. The average thickness of the sealing layer (cured product) can be appropriately designed, but is preferably 10 to 300 μm.

[0109] Next, a half-cut groove 26 is formed in the mounting substrate 21 (see FIG. 9). The half-cut groove can be manufactured by a known method. For example, the half-cut groove can be formed by dicing. Instead of the half-cut groove, a contact hole may be formed by laser processing.

[0110] Thereafter, conductive sheet 18 is placed on sealing layer 17 and temporarily attached to sealing layer 17, and cushioning material 16 is further placed on conductive sheet 18 (see FIG. 10). A release sheet (not shown) or the like may further be placed on cushioning material 16.

[0111] Next, under reduced pressure, heating and / or pressure is applied from the cushion material 16 side, whereby the conductive sheet 18 is deformed by the pressing force of the cushion material 16 to cover the sealing layer 17. Then, the cushion material 16 is peeled off, whereby the conductive layer 19 covers the sealing layer 17 in one go. Through these steps, the semiconductor device 100 is formed (see FIG. 11).

[0112] The resin sheet of the present invention has high conformability to uneven surfaces and is therefore suitable for use in collectively sealing a plurality of semiconductor elements. In the above embodiment, a manufacturing example has been described in which the sealing layer 17 is formed using the resin sheet 12, and the conductive layer 19 is formed thereon. In the present semiconductor device, the sealing layer and the like may be formed using, for example, the laminate shown in Figs. 2 to 4. Also, a laminate sheet may be used instead of the resin sheet. Note that, although the method for manufacturing the semiconductor device using the present resin sheet has been described above, the semiconductor device can also be manufactured using the same method when the present laminate sheet is used. EXAMPLES

[0113] Hereinafter, the present disclosure will be specifically described with reference to examples and comparative examples, but the present disclosure is not limited to the examples. In the following description, "parts" and "%" represent "parts by mass" and "% by mass", respectively, unless otherwise specified.

[0114] The values ​​obtained in this example were obtained by the following method. [Weight average molecular weight (Mw)] Mw is a polystyrene-equivalent value determined by GPC (gel permeation chromatography) measurement under the following measurement conditions: Equipment: Shodex GPC System-21 (Showa Denko K.K.) Column: A column consisting of one Shodex KF-802 (Showa Denko K.K.), one Shodex KF-803L (Showa Denko K.K.), and one Shodex KF-805L (Showa Denko K.K.) connected in series. Solvent: Tetrahydrofuran Flow rate: 1.0mL / min Temperature: 40℃ Sample concentration: 0.2% Sample injection volume: 100 μL

[0115] [Acid value] The acid value was measured using an automatic titrator GT-200 manufactured by Mitsubishi Chemical Analyc Corporation in accordance with the potentiometric titration method of JIS K0070, and the acid value was calculated by converting the measured acid value (mgKOH / g) into solid content.

[0116] [Tg of resin (A)] The coating solution of resin (A) was applied onto the release layer of a 75 μm-thick second release liner (Mitsui Chemicals Tohcello, SP-PET-O3) so that the thickness after drying was 25 μm, and dried in a hot air oven at 100 ° C for 3 minutes. Then, the release layer side of a 50 μm-thick first release liner (Mitsui Chemicals Tohcello, SP-PET-O1) was attached to the resin (A) side. Next, the first release liner and the second release liner were peeled off, and the Tg of the obtained resin (A) was measured by a differential scanning calorimeter (TA Instruments, "Discovery DSC 2500"). About 2 mg of the sample was placed in an aluminum pan, weighed, and set in the differential scanning calorimeter. The same type of aluminum pan without the sample was used as a reference, and the sample was held at 100 ° C for 5 minutes, and then quenched to -50 ° C using liquid nitrogen. Thereafter, the temperature was increased at a rate of 5° C. / min, and the Tg of the resin (A) was determined from the obtained DSC chart.

[0117] [Production example of resin (A)] [Production Example of Urethane Resin (A1-1) R1] A reaction vessel (hereinafter simply referred to as "reaction vessel") equipped with a stirrer, a thermometer, a reflux condenser, a dropping device, and a nitrogen inlet tube was charged with 130 parts of Pripol 2033 as a dimer diol, 8 parts of dimethylol butanoic acid (DMBA) as a polyol other than dimer, 85 parts of isophorone diisocyanate (IPDI) as a polyisocyanate, and 100 parts of toluene, and reacted for 8 hours at 80°C under a nitrogen atmosphere. An appropriate amount of toluene was added to this to obtain a 30% solids solution of urethane resin R1 with an acid value of 10 mgKOH / g, Mw 60,000, and Tg 0°C.

[0118] [Production example of urethane urea resin (A1-2) R2] In a reaction vessel, 130 parts of Pripol 2033 as a dimer diol, 8 parts of dimethylol butanoic acid as a polyol other than the dimer, 85 parts of isophorone diisocyanate as a polyisocyanate, and 100 parts of toluene were charged and reacted for 8 hours at 80 ° C. under a nitrogen atmosphere. 122 parts of toluene were added to this to obtain a solution of a urethane prepolymer having an isocyanate group at the end. The obtained prepolymer solution was heated to 70 ° C. and while maintaining the temperature, a solution of 67 parts of Priamine 1075 as a dimer diamine, 140 parts of isopropyl alcohol, and 331 parts of methyl ethyl ketone was dropped over 1 hour. After the dropwise addition, the reaction was continued for another 8 hours at 70 ° C. By adding an appropriate amount of toluene to this, a 30% solids solution of urethane urea resin R2 with an acid value of 10 mg KOH / g, Mw 190,000, and Tg 23 ° C. was obtained.

[0119] [Production examples of urethane urea resins (A1-2, etc. R3 to R9)] Urethane urea resins R3 to R9 were produced in the same manner as for urethane urea resin R2, except that the compositions and blending amounts (parts by mass) were changed to those shown in Table 1. Note that blanks indicate that no blending was performed. The acid value, Mw, and Tg are shown in Table 1.

[0120] [Production example of (meth)acrylic resin R10] In a reaction vessel, 80 parts of ethyl acetate, 20 parts of methyl methacrylate, 79 parts of n-butyl methacrylate, 1 part of methacrylic acid, and 0.1 parts of 2,2'-azobisisobutyronitrile as an initiator were charged, and the atmosphere in the reaction vessel was replaced with nitrogen gas. Then, the mixture was heated to 65°C while stirring under a nitrogen atmosphere to start the reaction. The reaction solution was then reacted at 65°C for 4 hours. After the reaction was completed, the mixture was cooled and diluted with ethyl acetate to obtain a 25% solids solution of (meth)acrylic resin R10 with Mw 35,000, Tg 35°C, and acid value 7 mgKOH / g.

[0121] The abbreviations in the table are as follows. (Dimer diol) Pripol 2033: Croda Japan Co., Ltd. (carbon number: 36, hydroxyl value: 209 mg KOH / g) (Other polyols) CHDM: Cyclohexanedimethanol GI-1000: G-1000 manufactured by Nippon Soda Co., Ltd. (hydroxyl value: 75.5 mg KOH / g, number average molecular weight: 1486) HDO: 1,6-Hexanediol DMBA: Dimethylolbutanoic acid (Polyisocyanate component) IPDI: Isophorone diisocyanate HDI: Hexamethylene diisocyanate (Dimer diamine) Priamine 1075: Croda Japan Co., Ltd. (amine value: 208 mg KOH / g, diamine content 98% or more) (Other polyamines) IPDA: Isophoronediamine (Other Ingredients) DnBA: Di-n-butylamine Silica: SiO2 (AEROSIL50, manufactured by Nippon Aerosil Co., Ltd., number average primary particle size 50 nm, specific surface area by BET method 35 to 65 m 2 / g)

[0122] [Production Example of Resin Composition] [Example 1] As the resin (A1-1), 333 parts of a solution of urethane resin R1 (100 parts of resin (A), 233 parts of solvent) was mixed with 5 parts (solid content equivalent) of an epoxy compound (JER1031S, manufactured by Mitsubishi Chemical Corporation) and 1 part (solid content equivalent) of an imidazole compound (Curesol 2PZ, manufactured by Shikoku Chemical Industry Co., Ltd.) as the crosslinking agent (B). Then, an appropriate amount of toluene was added, and the mixture was filtered with a membrane filter having a pore size of 10 μm to remove coarse foreign matter that may cause coating unevenness, thereby obtaining a resin composition with a solid content of 25%.

[0123] [Examples 2 to 11, Comparative Examples 1 and 2] A resin composition was prepared in the same manner as in Example 1, except that the components, blend amounts (blended amounts converted into solid content), etc. were changed as shown in Table 2.

[0124] [Examples of manufacturing resin sheets and laminates] Each resin composition of the Examples and Comparative Examples was applied onto the release layer of a 75 μm-thick second release liner (Mitsui Chemicals Tohcello, SP-PET-O3) so that the thickness after drying was 50 μm (for the resin sheet for measuring dielectric properties, the coating was applied so that the film thickness after drying was 200 μm), and a resin sheet was formed on the release liner by drying for 3 minutes in a hot air oven at 100° C. Next, the release layer side of a 50 μm-thick first release liner (Mitsui Chemicals Tohcello, SP-PET-O1) was attached to the exposed resin sheet, and laminates of Examples 2 to 11 and Comparative Examples 1 and 2 were obtained, in which the first release liner / resin sheet / second release liner were laminated in this order.

[0125] [Elongation at break] The laminate of each example was cut into a size of 15 mm wide x 20 mm long. Next, the first release liner and the second release liner were peeled off to obtain a measurement sample made of a resin sheet. After heating the resin sheet of each example at 150°C for 1 hour, the elongation of each measurement sample was measured at room temperature (23°C), a pulling speed of 50 mm / min, and a relative humidity of 50% using a tensile tester at the time when the coating film broke (measured according to the method specified in JISK7161:1994). Note that the elongation was defined as 0% when there was no deformation, 100% when the length after pulling was twice the original length, and 200% when the length was three times the original length.

[0126] [Breaking strength] The strength of each sample at the time of break was determined under the same conditions as those for measuring the breaking elongation.

[0127] [Peel strength after wet heat test] The resin sheet from which the first and second release liners of the laminate of each example had been peeled off was sandwiched between two 50 μm PPS (polyphenylene sulfide) substrates (Toray Industries, Torelina #50 3030) and thermocompressed at 5 MPa and 80° C. Then, it was heated at 150° C. for 1 hour. Then, a two-week wet heat test was performed under conditions of 121° C. and 100% humidity. After these steps, a peel test was performed between one PPS substrate and the resin sheet for this test piece at a peel angle of 90° and a peel speed of 300 mm / min. When the peel strength could be measured, the numerical value was recorded, and when at least a part of the resin sheet was broken and the peel strength could not be measured, it was indicated as ◯.

[0128] [Dielectric properties of resin sheet after heat treatment] The resin sheet of each example (film thickness after drying: 200 μm) was heated at 150° C. for 1 hour, and then the relative dielectric constant and dielectric loss tangent were determined for the sheet at a measurement temperature of 23° C. and a measurement frequency of 10 GHz by the cavity resonator method using a dielectric constant measuring device manufactured by AET Corporation.

[0129] [Tg of resin sheet after heat treatment] The resin sheet of each example (film thickness after drying: 50 μm) was heated at 150° C. for 1 hour, and then Tg was measured in the same manner as for the Tg of resin (A).

[0130] [Tensile storage modulus and Tan δ peak value after heat treatment of resin sheet] The resin sheet (film thickness 50 μm after drying) of each example was heated at 150 ° C for 1 hour, and measured using a dynamic elastic modulus measuring device (model number: DVA-200, manufactured by IT Measurement and Control) under the conditions of deformation mode "tensile", frequency 10 Hz, heating rate 10 ° C / min, and measurement temperature range -30 to 200 ° C, and the measured values ​​of tensile storage elastic modulus at 25 ° C and 150 ° C were read. In addition, the loss tangent was calculated by dividing the loss elastic modulus value measured at the same time by the storage elastic modulus value, and the Tan δ peak value at -30 to 200 ° C was read.

[0131] [Preparation of test board] A substrate was prepared in which a 5×5 array of non-molded semiconductor elements (1×1 cm) 24a was mounted on a substrate 21a made of glass epoxy. The thickness of the substrate 21a was 0.3 mm, and the thickness of the semiconductor elements 24a, i.e., the height from the upper surface of the substrate 21a to the top surface of the semiconductor elements 24a, was 0.7 mm (see FIG. 12). In order to evaluate under harsh conditions where gaps are likely to occur in the coating, the angle between the substrate 21a and the semiconductor elements 24a was set to 90° (the corners (see FIG. 13) were 90°).

[0132] [Evaluation method and criteria] [Water-resistant insulation] The first and second release liners of each example laminate, 50 mm wide and 100 mm long, were peeled off, and the exposed resin sheet (film thickness after drying: 50 μm) was pressed against a 70 mm wide, 120 mm long Kapton 300H sheet at 170°C, 2.0 MPa, and 30 minutes, and then thermally cured to obtain a test piece. The surface resistance of the resin sheet of the test piece was measured under conditions of 23°C and 50% RH using a ring probe URS of Mitsubishi Chemical Analytech's "Hiresta UP MCP-HT800," and this was taken as the initial surface resistance. The test piece was then left to stand for one week under conditions of 121°C and 100% RH, and then left to stand for one hour under conditions of 23°C and 50% RH, and the surface resistance was measured in the same manner as in the initial state, and the surface resistance after the water resistance test was determined. The difference was calculated by subtracting the surface resistance after the water resistance test from the initial surface resistance, and was evaluated according to the following criteria. A: The difference is 1.0 x 10 2 Ω / □ or less. B: The difference is 1.0 x 10 2 / □ Over 1.0×10 3 Ω / □ or less. C: The difference is 1.0 x 10 3 Ω / □ over 1.0×10 4 Ω / □ or less. D: The difference is 1.0 x 10 4 Ω / □ over 1.0×10 5 Ω / □ or less. E: The difference is 1.0 x 10 5 Over Ω / □.

[0133] [Coating] Each laminate was cut to 10 cm x 10 cm, and the first release liner was peeled off to expose the resin sheet. The resin sheet side was then placed on the semiconductor element of the test substrate. After that, the second release liner on the opposite side was peeled off to expose the surface, and a 50 μm thick TPX (Opulant X-44B, manufactured by Mitsui Chemicals Tocello Co., Ltd.) and a 2.0 mm thick PVC film (Celeb T, manufactured by Okamoto Co., Ltd.) were laminated in order as a cushioning material, and cardboard was further laminated to prevent sticking. Next, the test piece was pressed from above against the substrate surface under conditions of 5 MPa and 160°C for 30 minutes, and the resin sheet was covered along the shape of the semiconductor element to form a sealing layer. Then, the cushioning material and the cardboard were peeled off. The sealing layer protruding from the test substrate of the obtained test piece was roughly removed using a cutter, and a cross section of the test substrate was formed by polishing, so that the gap between the semiconductor elements could be observed. The gap between the semiconductor elements was observed with an electron microscope (magnification 500 times) to evaluate the coverage. Between the semiconductor elements, the sealing layer and the test substrate were deemed to be covered when the maximum diameter of the gap 51 at the corner portion (encircled line in FIG. 13) was 10 μm or less. The pass rate of the coverage test in the observed cross section was determined and evaluated according to the following criteria. A: 100%. B: Does not meet criterion A and is 90% or more. C: Does not meet criteria A or B, and is 80% or more. D: Does not meet criteria A to C and is 70% or more. E: Does not meet any of the criteria A to D.

[0134] [Storage stability] Four samples of each laminate were prepared and stored at -10°C, 0°C, 15°C, and 25°C for 48 hours at 50% humidity. Test pieces were then prepared in the same manner as in the evaluation of coverage, and evaluated in the same manner as in [coverage] above. That is, the clear rate of the coverage test on the observed cross section was determined, and evaluated according to the following criteria. A: For test pieces prepared after storing the laminate at 25℃, the clear rate of the coating test is 70% or more. B: Not applicable to criterion A. For test pieces prepared after storing the laminate at 15°C, the pass rate of the coating test was 70% or more. C: Not corresponding to criteria A or B, for the test piece prepared after storing the laminate at 0℃, the pass rate of the coating test is 70% or more. D: Not corresponding to criteria A to C, in the test piece prepared after storing the laminate at -10°C, the pass rate of the coating test is 70% or more. E: Does not meet criteria A to D.

[0135] [tear] As in the evaluation of coverage, a test substrate of a test piece on which a sealing layer was formed was used, and the number of tears (maximum length 1 μm or more) in the sealing layer was counted under a microscope (magnification 50x) and evaluated according to the following criteria. A: The number of tears is 0 to 1. B: The number of tears is 2 to 5. C: The number of tears is 6 to 10. D: The number of tears is between 11 and 15. E: The number of tears is 16 or more.

[0136] All of the above evaluations were made on a five-point scale, with A being outstanding, B being next best, C being next best, D being practical, and E being below target performance.

[0137] [Table 1]

[0138] [Table 2]

[0139] When a resin sheet having an elongation rate at break at 23°C after heat treatment at 150°C for 1 hour of less than 100% is used, it has been confirmed that there are problems with coverage, storage stability, and breakage, as shown in Comparative Example 1. Furthermore, when a resin sheet having a dielectric constant that does not satisfy 3 or less and 0.01 or less after heat treatment at 150°C for 1 hour is used, it has been confirmed that there are problems with water-resistant insulation, as shown in Comparative Example 2. On the other hand, it has been confirmed that a resin sheet according to the present disclosure having an elongation rate at break at 23°C after heat treatment at 150°C for 1 hour of 10 to 400%, a dielectric constant after heat treatment at 150°C for 1 hour of 3 or less, and a dielectric loss tangent of 0.01 or less can be obtained, as shown in Examples 1 to 11.

[0140] The storage stability of the resin sheet is greatly affected by the reactivity of the crosslinking agent used. That is, when a highly reactive crosslinking agent is used as a component of the resin sheet, refrigerated or frozen storage may be required to maintain the quality. In this example, the evaluation was performed using a highly reactive crosslinking agent, and it was confirmed that the storage stability was excellent as shown in Examples 1 to 11 by setting the elongation at break after the above-mentioned heat treatment of the resin sheet to a specific range and the dielectric properties to a specific range. Furthermore, it was confirmed that even better storage stability could be obtained by using a urethane-based resin (A1) having a dimer structure as the resin (A) or by adjusting the amount of the crosslinking agent (B) appropriately. [Explanation of symbols]

[0141] 1 to 4: Laminate 11: First release liner 12: Resin sheet 13: Second release liner 14, 16: Cushioning material 15: Conductive pattern 17: Sealing layer 18: Conductive sheet 19: Conductive layer 21: Mounting board 22: Conductive pattern 23: Bump 24: Semiconductor elements 25: Underfill material 26: Half cut groove 51: Gap 100: Semiconductor device

Claims

1. A resin sheet for semiconductor encapsulation for forming an encapsulation layer for a semiconductor element, The resin sheet is a thermosetting composition containing a resin (A) and a crosslinking agent (B), The resin (A) includes a urethane-based resin (A1) which contains a structural unit derived from at least any one of polyols, i.e., a dimer triol and a trimer triol, and / or a structural unit derived from at least any one of polyamines, i.e., a dimer triamine and a trimer triamine, and which has a urethane bond and may have a urea bond; The resin sheet has an elongation at break of 10 to 400% at 23°C after being heated at 150°C for 1 hour, The resin sheet for semiconductor encapsulation has a relative dielectric constant of 3 or less at a frequency of 10 GHz and 23°C after heating the resin sheet at 150°C for 1 hour, and a dielectric dissipation factor of 0.01 or less at a frequency of 10 GHz and 23°C.

2. 2. The resin sheet for semiconductor encapsulation according to claim 1, wherein a test piece is sandwiched between two 50 μm PPS (polyphenylene sulfide) substrates, thermocompressed at 5 MPa and 80° C., heat-treated at 150° C. for one hour, and then subjected to a wet heat test for two weeks under conditions of 121° C. and 100% humidity, and at least a portion of the material is broken when a peel test is performed between one of the PPS substrates and the resin sheet under conditions of a peel angle of 90° and a peel speed of 300 mm / min.

3. 2. The resin sheet for semiconductor encapsulation according to claim 1, wherein the acid value of the urethane resin (A1) is 1 to 20 mgKOH / g.

4. 2. The resin sheet for semiconductor encapsulation according to claim 1, wherein the weight average molecular weight of the urethane resin (A1) is 50,000 to 200,000.

5. 2. The resin sheet for semiconductor encapsulation according to claim 1, wherein the crosslinking agent (B) contains an epoxy compound.

6. A laminated sheet comprising the resin sheet according to any one of claims 1 to 5 and one or more functional sheets laminated together.

7. A semiconductor device comprising a substrate, a semiconductor element mounted on the substrate, and an encapsulating layer that encapsulates the semiconductor element, the encapsulating layer being formed from a cured product of the resin sheet according to any one of claims 1 to 5.

8. 8. The semiconductor device according to claim 7, wherein the average thickness of the cured product is 10 to 300 μm.

9. A method for manufacturing a semiconductor device for collectively covering a plurality of semiconductor elements mounted on a substrate, comprising the steps of: A step of temporarily attaching the resin sheet according to any one of claims 1 to 5 to the side of the plurality of semiconductor elements; a step of softening the resin sheet by heating and / or pressing the resin sheet to cover and bond the upper surface of the substrate and the upper and side surfaces of the plurality of semiconductor elements; and curing the resin sheet to encapsulate the semiconductor element.

Citation Information

Patent Citations

  • Sealing method of electronic component

    JP2012054363A

  • Semiconductor device manufacturing method

    JP2014029958A

  • Sealing film and film-covered electronic component-mounted substrate

    JP2018019054A

  • Sealing film and method for sealing electronic component-mounted substrate

    JP2019021757A

  • Sealing film, and sealing film-covered electronic component-mounted substrate

    JP2019106492A

Cited By

  • Encapsulating laminated sheet, resin-encapsulated semiconductor element substrate, and resin-encapsulated semiconductor device

    JP7810306B1