Glass with film and film with hard coat layer

A laminated film with reflective properties and a hard coat layer on glass effectively balances heat shielding and visible light transmission, addressing interference and thermal issues in existing materials.

JP7582555B1Active Publication Date: 2024-11-13OJI HLDG CORP
View PDF 12 Cites -1 Cited by

Patent Information

Application Number
JP2024518242
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-02-27
Filing Date
2024-02-21
Publication Date
2024-11-13
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

Existing transparent materials struggle to balance heat shielding performance with visible light transmission, often causing interference colors and radio wave interference, and may lead to thermal damage due to temperature differences.

Method used

A laminated film with reflective properties in the near-infrared region, composed of at least 50 layers of polyester films with differing refractive indices, combined with a hard coat layer, is applied to glass to enhance heat shielding while maintaining visible light transmission.

Benefits of technology

The solution provides excellent heat shielding performance with minimal reduction in visible light transmittance, reducing thermal cracking risks and maintaining high transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582555000001
    Figure 0007582555000001
  • Figure 0007582555000002
    Figure 0007582555000002
Patent Text Reader

Abstract

Disclosed are: film-attached glass having a laminated film on glass, the laminated film being a polyester laminated film consisting of at least 50 layers with reflective properties in the near-infrared region, the laminated film having a hard coat layer, and the film-attached glass having a solar reflectance of 20% or more and a reduction in visible light transmittance of less than 8% compared to glass alone; and a hard coat layer-attached film used in combination with glass, having a hard coat layer on a laminated film, the laminated film being a polyester laminated film consisting of at least 50 layers with reflective properties in the near-infrared region, and having a solar reflectance of 20% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film-coated glass and a film with a hard coat layer. [Background technology]

[0002] Transparent materials with heat ray shielding properties have been developed as one of the energy saving measures for buildings such as buildings and houses, and for transportation such as trains and automobiles. For example, transparent materials for window panels have been developed that transmit visible light from the sunlight pouring through windows, but block heat rays and have a heat insulating function to prevent indoor heat from escaping to the outside.

[0003] A widely used method for imparting a heat ray shielding function to a transparent material for window panes is to form a uniform layer of a metal such as aluminum on a film or the like.

[0004] However, such a uniform metal layer generally reflects electromagnetic waves, which can cause problems such as making it difficult to use mobile phones, portable televisions, etc. indoors or in cars. Therefore, glass sheets and films that have the function of blocking heat rays but transmitting electromagnetic waves have been developed.

[0005] Examples of such transparent materials for window panels include those in which a heat ray absorbing material is contained in the glass or in the interlayer film used in laminated glass to block heat rays with the heat ray absorbing material, and those in which a polymer multilayer laminate film in which polymers with different refractive indexes are alternately laminated is inserted between the glass to reflect and block heat rays. Methods that use heat ray absorbing materials have problems in that sunlight incident from the outside is converted into thermal energy, and the heat is radiated into the room, reducing the heat ray blocking efficiency, and the glass temperature rises as a result of absorbing heat rays, which can cause the glass body to break due to the difference with the outside air temperature.

[0006] On the other hand, a polymer multilayer laminate film can selectively reflect light in the near-infrared region by controlling the layer thickness and selecting the wavelength to be reflected, thereby improving heat-shielding performance while maintaining visible light transmittance, and also maintaining excellent radio wave transmittance.

[0007] However, when a stretched film is used as a polymer multilayer laminate film, the refractive index of the film may differ in three orthogonal directions, i.e., the width direction, length direction, and thickness direction of the film, resulting in large retardation. If this retardation is within a certain range, there is a problem that interference colors are visible when viewed through a polarizer such as polarized sunglasses.

[0008] Therefore, Patent Document 1 reports a laminate film that suppresses interference colors and provides good visibility even when viewed through a polarizer, and a glass window member that uses the laminate film. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 6225495 Summary of the Invention [Problem to be solved by the invention]

[0010] However, it is desired to further improve the heat insulating performance of transparent materials while maintaining the visible light transmitting performance.

[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a film-coated glass and a film with a hard coat layer that are excellent in both heat shielding performance and visible light transmission performance. [Means for solving the problem]

[0012] The present inventors have found that the heat shielding performance can be efficiently improved by combining glass with a specific laminate film having reflective properties in the near-infrared region.

[0013] The present invention has been completed based on the above-mentioned investigations. That is, the present invention has the following configuration.

[0014] (1) The film-coated glass of the present invention is a film-coated glass having a laminated film on a glass, The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, The laminated film has a hard coat layer, The film-coated glass is characterized in that it has a solar reflectance of 20% or more and a reduction in visible light transmittance of less than 8% compared to the glass alone. (2) The glass is preferably clear glass, green glass, double glazing, low-emissivity double glazing, laminated glass, or low-emissivity laminated glass. (3) The glass is a low-emissivity insulating glass, The low-emissivity insulating glass is a double-glazed glass having a hollow layer between a plurality of glass panes, with a low-emissivity film provided on the surface of at least one of the glass panes facing the hollow layer, and preferably has reflective properties at specific wavelengths. (4) The glass is the low-emissivity laminated glass, The low-emissivity laminated glass is a laminated glass having a configuration in which a low-emissivity film is sandwiched between a plurality of glass plates, and preferably has reflection characteristics at a specific wavelength. (5) The glass is green glass, The green glass preferably has absorption properties in the infrared region. (6) In the film-coated glass of the present invention, the laminated film is preferably disposed on the indoor side. (7) The solar reflectance of the film-coated glass of the present invention is preferably 28% or more. (8) The hard-coat film of the present invention is a hard-coat film having a hard-coat layer on a laminate film, which is used in combination with glass, The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, The laminated film is characterized in that it has a solar reflectance of 20% or more. (9) The hard-coat-layer-attached film of the present invention preferably has a hard-coat layer on at least one side of the laminate film, and has an adhesive layer on the hard-coat layer or on the side opposite to the side on which the hard-coat layer is arranged. (10) The hard-coat-layer-attached film of the present invention preferably has the hard-coat layer and the pressure-sensitive adhesive layer on different surfaces. (11) In the hard coat layer-attached film of the present invention, the glass is preferably clear glass, green glass, insulating glass, low-emissivity insulating glass, laminated glass, or low-emissivity laminated glass. (12) The laminate film in the hard coat layer-attached film of the present invention preferably has an average reflectance of 70% or more in the wavelength band of 900 to 1200 nm. (13) The laminate film in the hard coat layer-attached film of the present invention preferably has a thickness of 30 μm to 500 μm. Effect of the Invention

[0015] The film-attached glass and the film with a hard coat layer of the present invention are excellent in heat shielding performance and in visible light transmission performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described, however, the embodiment of the present invention is not limited to the following embodiment.

[0017] The film-coated glass of the present embodiment is a film-coated glass having a laminated film on a glass, The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, The laminated film has a hard coat layer, The film-coated glass is characterized in that it has a solar reflectance of 20% or more and a reduction in visible light transmittance of less than 8% compared to the glass alone.

[0018] The hard coat layer-attached film of the present embodiment is a hard coat layer-attached film having a hard coat layer on a laminate film, which is used in combination with glass, and The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, It is characterized by having a solar reflectance of 20% or more.

[0019] The hard coat layer-attached film of the present embodiment may have a hard coat layer on at least one side of the laminated film, and may have an adhesive layer on the hard coat layer or on the side opposite to the side on which the hard coat layer is arranged. The hard coat layer-attached film of the present embodiment may have the hard coat layer and the adhesive layer on different sides.

[0020] The film-attached glass of the present embodiment may have a hard coat layer on at least one side of the laminated film, and an adhesive layer on the hard coat layer or on the side opposite to the side on which the hard coat layer is arranged. The film-attached glass of the present embodiment may have the hard coat layer and the adhesive layer on different sides of the laminated film. In this case, the film-attached glass of the present embodiment may have a hard coat layer on the side opposite to the side on which the glass is arranged of the laminated film, and an adhesive layer between the glass and the laminated film.

[0021] In this specification, heat shielding means heat ray shielding properties.

[0022] (visible light, near infrared rays, far infrared rays, ultraviolet rays) In this specification, visible light refers to electromagnetic waves that can be recognized by the naked eye, and generally refers to electromagnetic waves with a wavelength of 380 to 780 nm. Near-infrared rays are electromagnetic waves with a wavelength of approximately 800 to 2500 nm, and have a wavelength close to red visible light. Near-infrared rays are contained in sunlight and have the effect of heating objects. In contrast, far-infrared rays are electromagnetic waves with a wavelength of approximately 5 to 20 μm (5000 to 20000 nm), which are not contained in sunlight and are close to the wavelength emitted from objects at around room temperature. Moreover, ultraviolet rays are electromagnetic waves with a wavelength of approximately 10 to 380 nm.

[0023] In this specification, heat rays refer to the range from ultraviolet rays to near infrared rays.

[0024] Hereinafter, each member constituting the film-attached glass and the hard coat layer-attached film will be described. Members common to both will be described together.

[0025] (Glass) The glass in the film-attached glass and the film with a hard coat layer is a transparent plate for taking in sunlight from the outside into buildings, vehicles, ships, etc. Generally, so-called inorganic glass plates are used. Soda-lime glass is a representative example of inorganic glass. Examples of the shape of window glass include curved and plate-like. Examples of glass that can be used include clear glass, green glass, double-glazed glass, low-emissivity double-glazed glass, laminated glass, and low-emissivity laminated glass. Among them, the use of low-emissivity double-glazed glass, low-emissivity laminated glass, and green glass is preferred because high heat-shielding performance can be obtained while maintaining a high visible light transmittance, and the use of low-emissivity double-glazed glass is particularly preferred.

[0026] Low-emissivity insulating glass is a type of insulating glass having a hollow layer between multiple (e.g., two) glass sheets, with a low-emissivity film provided on the surface of at least one of the glass sheets facing the hollow layer, and preferably has a reflection characteristic in a specific wavelength (preferably in the infrared region). Low-emissivity insulating glass may be either an insulating type or a heat-shielding type. Low-emissivity laminated glass is a type of laminated glass having a low-emissivity film sandwiched between multiple (e.g., two) glass sheets, and preferably has a reflection characteristic in a specific wavelength (preferably in the infrared region). Green glass is manufactured by adding metal to glass raw materials, and preferably has an absorption characteristic in the infrared region.

[0027] The low-emissivity film has a function of reducing the emissivity of thermal energy (such as infrared rays), and is preferably a film containing at least one selected from the group consisting of metals, metal oxides, and metal nitrides. Examples of such low-emissivity films include single films and multiple types of laminated films formed by sputtering, CVD, powder deposition, spraying, deposition, etc. Constituent components of the film include metals such as Ag and Al, metal oxides including Zn, Ga, Ti, Sn, Si, Ta, Al, In, Ni, Cr, and Zr, metal nitrides, alloys, alloy oxides, and alloy nitrides of the above metals, etc.

[0028] (Laminated film) The laminated film is a laminate of 50 or more layers of two or more polyester films having different optical properties. The different optical properties here mean that the refractive index differs by 0.01 or more in any of two orthogonal directions arbitrarily selected in the plane and a direction perpendicular to the plane. The alternately laminated film means that polyester films made of different resins are laminated in a regular arrangement in the thickness direction. By alternately laminating polyester films having different optical properties in this way, it becomes possible to reflect light of a specific wavelength specified by the relationship between the difference in refractive index of each layer and the layer thickness. The number of layers to be laminated is preferably 400 or more, more preferably 800 or more. The upper limit of the number of layers is, for example, about 1000 layers. The more the number of layers increases, the higher the reflectance can be achieved for light in a wider wavelength band, and therefore a laminated film with high heat shielding performance can be obtained.

[0029] The laminated film desirably has an average reflectance of 70% or more at wavelengths of 900 to 1200 nm. For use in applications requiring high transparency, high heat shielding performance can be obtained while maintaining transparency by efficiently reflecting light at wavelengths of 900 to 1200 nm, which is slightly longer than the visible light region. The average reflectance at wavelengths of 900 to 1200 nm is preferably 80% or more, more preferably 90% or more.

[0030] Similarly, the average reflectance of the film-coated glass in the wavelength band of 900 to 1200 nm is preferably 60% or more on at least one side. More preferably, the average reflectance of the film-coated glass in the wavelength band of 900 to 1200 nm is 60% or more on both sides. In addition, the average reflectance of the film-coated glass in the wavelength band of 900 to 1200 nm is preferably 70% or more on at least one side. By improving the heat shielding property by increasing the reflectance, it is preferable because heat cracking caused by the glass absorbing heat is less likely to occur. The shielding coefficient generally used as a heat shielding performance shows the effects of both an increase in absorptance and an increase in reflectance, but for the above reasons, an increase in reflectance is preferable to an increase in absorptance, especially for window glass for buildings.

[0031] The polyester resin used in the laminated film may be a copolymer or a mixture. The polyester is preferably a polyester obtained by polymerization of a monomer mainly composed of an aromatic dicarboxylic acid or an aliphatic dicarboxylic acid and a diol or an ester-forming derivative thereof. Examples of the aromatic dicarboxylic acid include terephthalic acid, phthalic acid, isophthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid. Examples of the aliphatic dicarboxylic acid include adipic acid, suberic acid, sebacic acid, dimer acid, dodecanedioic acid, cyclohexanedicarboxylic acid, and ester derivatives thereof. Among them, terephthalic acid and 2,6-naphthalenedicarboxylic acid are preferable. These components may be used alone or in combination of two or more. Furthermore, oxyacids such as hydroxybenzoic acid may be partially copolymerized.

[0032] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2-bis(4-hydroxyethoxyphenyl)propane, diethylene glycol, triethylene glycol, polyalkylene glycol, isosorbate, and spiroglycol. Among these, ethylene glycol is preferred. These diol components may be used alone or in combination of two or more.

[0033] Preferred polyester resins used in the laminated film include polyethylene terephthalate and copolymers thereof, polyethylene naphthalate and copolymers thereof, polybutylene terephthalate and copolymers thereof, polybutylene naphthalate and copolymers thereof, polyhexamethylene terephthalate and copolymers thereof, and polyhexamethylene naphthalate and copolymers thereof.

[0034] In the laminate film, the difference in the average in-plane refractive index between adjacent layers made of polyester resins having different optical properties is preferably 0.03 or more, more preferably 0.05 or more, and even more preferably 0.1 to 0.15.

[0035] Specific examples of laminated films include those in which at least one polyester resin comprises polyethylene terephthalate or polyethylene naphthalate, and at least one polyester resin comprises a spiroglycol carboxylate unit. More preferably, at least one polyester resin comprises polyethylene terephthalate or polyethylene naphthalate, and at least one polyester resin is a polyester obtained using spiroglycol and cyclohexanedicarboxylic acid.

[0036] Other specific examples of laminate films include those in which at least one polyester resin contains polyethylene terephthalate or polyethylene naphthalate, and may be a single composition or may be copolymerized with a small amount of other repeating units, or may be blended with a small amount of other polyester resin, and at least one polyester resin contains cyclohexanedimethanol carboxylate units.

[0037] The laminated film may be biaxially stretched. The stretching may be performed in two directions successively or simultaneously. The stretching ratio varies depending on the type of resin, and is usually preferably 2 to 15 times, more preferably 2 to 7 times. The laminated film may be subjected to a surface treatment such as corona treatment, flame treatment, or plasma treatment as necessary, and then provided with functions such as easy slip, easy adhesion, and antistatic properties by in-line coating.

[0038] As the laminated film, for example, the one described in Japanese Patent No. 6225495 can be used.

[0039] The thickness of the laminated film is not particularly limited and is, for example, 30 to 500 μm, preferably 35 to 400 μm, and more preferably 40 to 300 μm.

[0040] (Hard coat layer) The hard coat layer is a layer provided on at least one surface of the laminate film. The hard coat layer can be provided on either the side of the laminate film opposite to the side on which the glass is placed, or between the glass and the laminate film, but is preferably provided on the side of the laminate film opposite to the side on which the glass is placed.

[0041] The thickness of the hard coat layer is from 0.1 to 20 μm, preferably from 0.5 to 10 μm, and more preferably from 0.9 to 6 μm.

[0042] For the hard coat layer, an ultraviolet-curable resin is used because it is relatively easy to form a coating film with high hardness. Examples of ultraviolet-curable resins include acrylic resins, silicone resins, urethane resins, olefin resins, and ester resins, among which acrylic resins are preferred because of their ease of handling and processing.

[0043] The ultraviolet-curable acrylic resin is a polymer of a curable composition made of a monomer or oligomer having an acrylic polymerizable unsaturated group. The monomer or oligomer having an acrylic polymerizable unsaturated group may be monofunctional or polyfunctional.

[0044] Specific examples of monofunctional monomers having an acrylic polymerizable unsaturated group include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, stearyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate. These may be used alone or in combination of two or more.

[0045] Specific examples of monofunctional oligomers having an acrylic polymerizable unsaturated group include ethoxylated o-phenylphenol acrylate, methoxypolyethylene glycol acrylate, and phenoxypolyethylene glycol acrylate.

[0046] In order for a composition comprising a monomer or oligomer having an acrylic polymerizable unsaturated group to be curable, it is preferable that the monomer or oligomer having an acrylic polymerizable unsaturated group contains a polyfunctional (meth)acrylic acid ester. Specific examples of the polyfunctional (meth)acrylic acid ester include bifunctional (meth)acrylates such as dipropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene oxide modified neopentyl glycol di(meth)acrylate, modified bisphenol A di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, and polyethylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Examples of the acrylate include trifunctional (meth)acrylates such as trimethylolpropane ethoxy tri(meth)acrylate, polyether tri(meth)acrylate, and glycerin propoxy tri(meth)acrylate, and tetrafunctional or higher (meth)acrylates such as pentaerythritol tetra(meth)acrylate, pentaerythritol ethoxy tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, propionic acid modified dipentaerythritol penta(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. These polyfunctional acrylates may be used alone or in combination of two or more. In addition, in order to ensure the hardness of the hard coat layer, it is preferable to use a tetrafunctional or higher (meth)acrylic acid ester.

[0047] In addition, it is preferable to use a fluorine-containing acrylic resin in which part of hydrogen is replaced with fluorine as the monomer or oligomer having an acrylic polymerizable unsaturated group, since this further improves the scratch resistance and stain resistance.

[0048] The ultraviolet-curable urethane-based curable resin is a polymer of a urethane acrylate monomer or oligomer. The urethane acrylate oligomer is a polymer in which polyoxyalkylene segments or saturated polyester segments or both are linked via urethane bonds and has acryloyl groups at both ends.

[0049] In order to obtain an ultraviolet-curable resin, it is necessary to add a polymerization initiator, if necessary, to the above-mentioned monomer or oligomer having a polymerizable unsaturated group to obtain an ultraviolet-curable composition.

[0050] As the ultraviolet polymerization initiator, various known polymerization initiators can be used. Specific examples include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, α-hydroxyacetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl, 1-hydroxycyclohexyl phenyl ketone ... Examples of the ultraviolet polymerization initiator include (2-hydroxy-2-propyl)phenyl-2-(2-methoxy)phenyl-ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, propiophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, and p-dimethylamine benzoic acid ester. These ultraviolet polymerization initiators may be used alone or in combination of two or more. The amount of the ultraviolet polymerization initiator added is preferably 1 to 10% by mass relative to the monomer or oligomer having a polymerizable unsaturated group.

[0051] In addition, the hard coat layer may contain components other than those described above as necessary, as long as the effects of the present embodiment are not impaired. Examples of components that can be added to the hard coat layer include ultraviolet absorbers, light stabilizers (hindered amine light stabilizers (HALS), etc.), and fluorine-based antifouling agents.

[0052] (Adhesive layer) The adhesive layer is a layer that bonds the laminated film and glass. The adhesive layer may be made of adhesives and pressure sensitive adhesives that are generally used for bonding glass. The adhesive layer may be made of various resins such as acrylic, rubber (natural rubber, polybutadiene, etc.), silicone, urethane, polyvinyl butyral, polyvinyl acetal, and ethylene-vinyl acetate. Among these, it is preferable to use at least one of acrylic resin, rubber resin, and silicone resin from the viewpoint of durability.

[0053] (Method of manufacturing film with hard coat layer) Next, a method for producing the hard coat layer-attached film of the present embodiment will be described.

[0054] The film with a hard coat layer of the present embodiment can be produced by forming a hard coat layer on a laminate film.

[0055] The method for forming the hard coat layer will be described. An appropriate amount of ultraviolet curable resin is mixed with a solvent to prepare a solution with an appropriate viscosity. The solution is coated onto a laminated film. After drying, a hard coat layer can be formed by a curing reaction using ultraviolet light.

[0056] A method for forming an adhesive layer will be described. First, an appropriate amount of a solvent is mixed with an adhesive or pressure-sensitive adhesive to prepare a solution of a coating composition with an appropriate viscosity. Next, the obtained solution is coated on a laminated film. The solution is then dried to form an adhesive layer. Alternatively, the obtained solution may be coated on another sheet to form an adhesive layer, and then the adhesive layer may be attached to the laminated film.

[0057] Moreover, the film-attached glass of the present embodiment can be produced by using a hard coat layer-attached film having an adhesive layer, and attaching the hard coat layer-attached film to glass via the adhesive layer.

[0058] In the film-coated glass of the present embodiment, the laminate film may be attached to either the indoor side or the outdoor side, and it is preferable that the laminate film is disposed on the indoor side.

[0059] [Performance of film-coated glass and film with hard coat layer] Various properties of the film-attached glass and the film with a hard coat layer will be described below.

[0060] (Visible light transmittance) The glass with a film and the film with a hard coat layer transmit visible light with a wavelength of 380 to 780 nm. The visible light transmittance of the glass with a film and the film with a hard coat layer is preferably 60% or more. If the visible light transmittance is 60% or more, the field of view is excellent. More preferably, it is 70% or more. Furthermore, the reduction in visible light transmittance of the glass with a film is preferably less than 8% compared to that of the glass alone, and more preferably less than 5%. The visible light transmittance can be measured using a spectrophotometer in accordance with JIS S3107:2013.

[0061] (Solar reflectance) The film-attached glass and the film with a hard coat layer preferably have a solar reflectance of 20% or more. If the solar reflectance is 20% or more, the film has excellent heat shielding properties. The solar reflectance is more preferably 28% or more, and even more preferably 30% or more. The solar reflectance can be measured using a spectrophotometer in accordance with JIS S3107:2013.

[0062] The film with a hard coat layer of the present embodiment has excellent visible light transmission performance and excellent heat shielding performance, and therefore can be attached to glass in windows of buildings, windows of transportation vehicles such as automobiles, etc. The film-coated glass of the present embodiment can also be used as window glass. EXAMPLES

[0063] The present embodiment will be described more specifically with reference to the following examples.

[0064] Example 1 (Preparation of Thermoplastic Resin) Thermoplastic resin A was prepared as [Toray F20S] (polyethylene terephthalate, intrinsic viscosity 0.65, melting point 255°C, in-plane refractive index of the film obtained by stretching and heat-treating this resin: 1.66), and thermoplastic resin B was prepared as a copolymer of 80 mol % of amorphous polyethylene terephthalate with an intrinsic viscosity of 0.72 and 20 mol % of spiroglycol (in-plane refractive index of the film obtained by stretching and heat-treating this resin: 1.55).

[0065] (Preparation of Laminate) The thermoplastic resin A and the thermoplastic resin B were each melted at 280°C in a vented twin-screw extruder, and then the thermoplastic resin A and the thermoplastic resin B were joined in a feed block so as to be alternately laminated to obtain a laminate. The thickness of each layer was adjusted to be the same. The outermost layers on both the front and back of the laminate were both made of thermoplastic resin A. The laminate was extruded from a T-die and molded into a sheet, and then cooled against a casting drum to obtain a laminate.

[0066] (Stretching process) The laminate was heated with a roll set to a surface temperature of 80°C, and then further heated with a radiation heater so that the laminate film temperature reached 90°C. The laminate was then stretched 4 times in the longitudinal direction while being cooled to obtain a uniaxially stretched film.

[0067] (Surface treatment) After subjecting both sides of the uniaxially stretched film to a corona discharge treatment in air, a composition dispersion containing 2% by mass of silica particles (product name: Sea Hoster KE, manufactured by Nippon Shokubai Co., Ltd.) and 98% by mass of polyester resin (product name: TP294, manufactured by Mitsubishi Chemical Corporation) was applied to form an easy-adhesion layer having a thickness of 200 nm.

[0068] The uniaxially stretched film was heated to 100° C. with a heater, stretched 4 times in the transverse direction with a tenter, gradually cooled to room temperature, and then wound up.

[0069] The thickness of the obtained laminated film was 75 μm. In addition, it retained high transparency while reflecting light of 900 to 1200 nm, and had a nearly flat reflectance distribution in the visible light region of wavelengths of 400 to 700 nm. The average reflectance of the laminated film alone in the range of 900 to 1200 nm was 90% or more. The laminated film had 50 or more layers.

[0070] (Formation of hard coat layer) A coating composition consisting of 100 parts by mass of ARONIX (trademark) M-940 (hexafunctional acrylate, solid content 100% by mass) manufactured by Toagosei Co., Ltd., 4 parts by mass of Irgacure 184 (photoinitiator, solid content 100% by mass) manufactured by BASF, 0.5 parts by mass of OPTOOL DAC-HP (fluorine-based antifouling material, solid content 20% by mass) manufactured by Daikin Industries, Ltd., and 1,300 parts by mass of PGM (solvent, solid content 0% by mass) was applied to one side of the obtained laminated film with a Mayer bar to a thickness of 2.0 μm after drying, dried at 80° C. for 1 minute, and then illuminated with a high-pressure mercury lamp (illuminance 400 mW / cm 2 ) with a light output of 150 mJ / cm 2 The coating was cured by irradiating it with ultraviolet light so as to form a hard coat layer.

[0071] (Formation of adhesive layer) A coating composition consisting of 100 parts by mass of SK1429DT (acrylic adhesive, solids content 30% by mass) manufactured by Soken Chemical Industries, Ltd., 3 parts by mass of AD-5A (aluminum complex curing agent, solids content 5% by mass) manufactured by Soken Chemical Industries, Ltd., and 3 parts by mass of Tinuvin (trademark) 928 (benzotriazole ultraviolet absorber, solids content 100% by mass) manufactured by BASF was applied onto the silicone-treated surface of a separator sheet (manufactured by Mitsubishi Chemical Corporation, MRQ#38, 38 μm thick) that had been treated with silicone, and the coating was dried for 2 minutes in a hot air oven at 100° C. to form an adhesive layer approximately 12 μm thick.

[0072] The PET surface of the film and the adhesive layer surface of a separator sheet were laminated together and aged for 7 days to produce a film with an adhesive layer.

[0073] (Preparation of glass with film) The separator sheet of the adhesive layer-attached film was peeled off, and the adhesive side was laminated to neutral Low-E insulating glass (insulation type) manufactured by YKK AP, to prepare glass with film of Example 1.

[0074] Example 2 A film-coated glass was produced in the same manner as in Example 1, except that a float glass having a nominal thickness of 3 mm was used as the glass to be laminated.

[0075] Example 3 A glass with a film was produced in the same manner as in Example 1, except that green glass (manufactured by AGC, product name: Sungreen, nominal thickness 5 mm) was used as the glass to be laminated.

[0076] Example 4 A film-coated glass was produced in the same manner as in Example 1, except that thermoplastic resin A and thermoplastic resin B were laminated so that the average reflectance of the laminate film alone from 900 to 1200 nm was 80% or more and the thickness was 108 μm.

[0077] Example 5 A film-coated glass was produced in the same manner as in Example 4, except that a float glass having a nominal thickness of 3 mm was used as the glass to be laminated.

[0078] Example 6 A glass with a film was produced in the same manner as in Example 4, except that green glass (manufactured by AGC, product name: Sungreen, nominal thickness 5 mm) was used as the glass to be laminated.

[0079] Comparative Example 1 Instead of the laminated film, a polyethylene terephthalate film (highly adhesive biaxially stretched PET film, Toyobo Co., Ltd. Cosmoshine (trademark) A4360, thickness 38 μm) was used, and the hard coat layer was made of a paint consisting of 100 parts by mass of Aronix M-940 (hexafunctional acrylate, solid content 100% by mass) manufactured by Toa Gosei Co., Ltd., 4 parts by mass of Irgacure 184 (photoinitiator, solid content 100% by mass) manufactured by BASF, 0.5 parts by mass of Optool DAC-HP (fluorine-based antifouling material, solid content 20% by mass) manufactured by Daikin Industries, Ltd., 1300 parts by mass of PGM (solvent, solid content 0% by mass), and 90 parts by mass of YMF-02A (near-infrared absorbing material, solid content 18.5% by mass) manufactured by Sumitomo Metal Mining Co., Ltd. A glass with a film was produced in the same manner as in Example 1.

[0080] Comparative Example 2 A film-coated glass was produced in the same manner as in Comparative Example 1, except that a float glass having a nominal thickness of 3 mm was used as the glass to be laminated.

[0081] Comparative Example 3 A glass with a film was produced in the same manner as in Comparative Example 1, except that green glass (manufactured by AGC, product name: Sungreen, nominal thickness 5 mm) was used as the glass to be laminated.

[0082] Comparative Example 4 Instead of the laminated film, a polyethylene terephthalate film (highly adhesive biaxially stretched PET film, Toyobo Co., Ltd. Cosmoshine (trademark) A4360, thickness 38 μm) was used on one entire surface thereof, and the following first metal oxide layer 1, first silver alloy layer 2, second metal oxide layer 3, second silver alloy layer 4, and third metal oxide layer 5 were laminated in sequence by sputtering to form a three-layer metal oxide layer. Except for this, a film was used in the same manner as in Example 1. The sputtering method was performed under a vacuum of 0.4 Pa. The composition and thickness of each layer are as follows. An adhesive layer was formed on the surface of the metal oxide layer of the obtained film, and a hard coat layer was formed on the PET surface.

[0083] First metal oxide layer 1: ITO, 27 nm First silver alloy layer 2: AgPd (silver alloy containing 1 atomic % palladium), 10 nm Second metal oxide layer 3: ITO, 55 nm Second silver alloy layer 4: AgPd (silver alloy containing 1 atomic % palladium), 10 nm Third metal oxide layer 5: ITO, 27 nm

[0084] Comparative Example 5 A film-coated glass was produced in the same manner as in Comparative Example 4, except that a float glass having a nominal thickness of 3 mm was used as the glass to be laminated.

[0085] Comparative Example 6 A glass with a film was produced in the same manner as in Comparative Example 4, except that green glass (manufactured by AGC, product name: Sungreen, nominal thickness 5 mm) was used as the glass to be laminated.

[0086] <Evaluation items> (Visible light transmittance, visible light reflectance, solar transmittance, solar reflectance, solar absorptance) Measurements were performed using a spectrophotometer (Shimadzu Corporation, SolidSpec-3700i DUV) in the wavelength range of 300 to 2500 nm, based on JIS S3107: 2013. The solar absorptance was calculated using the following formula. (Solar absorptance) = 100% - (Solar transmittance) - (Solar reflectance) Evaluation criteria for visible light transmittance: If the reduction in visible light transmittance was less than 5% compared to the glass alone, it was given an "A", if it was between 5% and less than 7%, it was given a "B", if it was between 7% and less than 8%, it was given a "C", and if it was 8% or more, it was given a "D". Evaluation criteria for solar reflectance: If the solar reflectance is 30% or more, it is rated as "A", if it is 28% or more but less than 30%, it is rated as "B", if it is 20% or more but less than 28%, it is rated as "C", and if it is less than 20%, it is rated as "D". Evaluation criteria for overall evaluation: The lower of the visible light transmittance and solar reflectance was used.

[0087] (Shielding coefficient) Spectral reflectance was measured in the wavelength range of 5.5μm to 25μm using a Fourier transform infrared spectrophotometer (Shimadzu Corporation, IRTracer-100). Normal emissivity was calculated according to JIS R 3106 (Test methods for transmittance, reflectance, and emissivity of flat glass and calculation methods for solar heat gain coefficient of architectural flat glass), Appendix JB, JB.2 Calculation method for normal emissivity. In calculating normal emissivity, the value at wavelength 23.3μm was used for the spectral reflectance in the wavelength range of 25.2μm to 50.0μm. The obtained normal emissivity was used to calculate the shading coefficient based on JIS S 3107:2013.

[0088] The evaluation results of the laminate films with the hard coat layer and the pressure-sensitive adhesive layer and the glass with the film in Examples 1 to 6 and Comparative Examples 1 to 6 are shown in Table 1. [Table 1]

[0089] The shading coefficients of the films used in Examples 1 to 3 and Comparative Examples 1 to 6 were comparable, ranging from 0.73 to 0.76. In Examples 1 to 6, the reduction in visible light transmittance was within 4% compared to glass alone. In all of Comparative Examples 1 to 6, the reduction in visible light transmittance was 8% or more compared to glass alone.

[0090] The solar reflectance was increased in Examples 1 to 6 and Comparative Examples 4 to 6 compared to the solar reflectance of the glass alone. For each glass, the Examples had a higher solar reflectance than the Comparative Examples. Specifically, Examples 1, 3, and 4 and Comparative Example 4 had a solar reflectance of 30% or more, Example 6 and Comparative Example 1 had a solar reflectance of 28% or more, Examples 2, 5, Comparative Examples 5 and 6 had a solar reflectance of 20% or more, and Comparative Examples 2 and 3 had a solar reflectance of less than 20%.

[0091] In Examples 3 and 6 and Comparative Example 6, the solar absorptance was significantly reduced compared to Sungreen alone.

[0092] From the results of visible light transmittance and solar reflectance, Examples 1 to 6 had excellent heat shielding performance while maintaining transparency.

[0093] Furthermore, the improvement rate of solar reflectance compared to that of glass alone is shown in Table 2. The ratio of the improvement rate of films a and b to that of film d was 1.8 and 2.4 only when Low-E double glazing was used, which was higher than the values ​​of 1.0 to 1.3 for the other two glasses. [Table 2]

[0094] From the above results, the present invention provides a film-attached glass and a film with a hard coat layer that are excellent in both heat shielding performance and visible light transmission performance.

Claims

1. A film-coated glass having a laminated film on the glass, The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, The laminated film has a hard coat layer, The film-coated glass has a solar reflectance of 20% or more and a visible light transmittance reduction of less than 8% compared to the glass alone, The glass is a low-emissivity insulating glass.

2. The low-emissivity double-glazed glass is a double-glazed glass having a hollow layer between multiple glass panes and a low-emissivity film provided on the surface of at least one of the glass panes facing the hollow layer, and has reflective characteristics at specific wavelengths, as described in claim 1.

3. The film-coated glass according to claim 1 or 2, wherein the laminated film is disposed on the interior side.

4. The film-coated glass according to claim 1 , wherein the film-coated glass has a solar reflectance of 28% or more.

5. A hard coat layer-attached film having a hard coat layer on a laminated film, which is used in combination with glass, The laminated film is a polyester laminated film having a reflectance characteristic in the near infrared region and consisting of at least 50 layers, The solar reflectance is 20% or more, The glass is a low-emissivity insulating glass.

6. 6. The film with a hard coat layer according to claim 5, which has a hard coat layer on at least one surface of the laminated film, and has an adhesive layer on the hard coat layer or on the surface opposite to the surface on which the hard coat layer is disposed.

7. The film with a hard coat layer according to claim 6 , wherein the hard coat layer and the adhesive layer are provided on different surfaces.

8. The film with a hard coat layer according to any one of claims 5 to 7, wherein the laminated film has an average reflectance of 70% or more in a wavelength band of 900 to 1200 nm.

9. The film with a hard coat layer according to any one of claims 5 to 7, wherein the laminate film has a thickness of 30 µm to 500 µm.

Citation Information

Patent Citations

  • Building wall structure

    JP2005016168A

  • Low emissive multilayered glass

    JP2007070146A

  • Heat insulating laminated glass

    JP2010222233A

  • Method for producing laminated glass

    JP2011195417A

  • Structure for laminated glass, layered laminated glass comprising the same, and method for manufacturing the same

    JP2013209246A