LAMINATE, MANUFACTURING METHOD FOR LAMINATE, AND BATTERY CASE
A laminate structure with a compressed foam core, fiber-reinforced plastic outer layer, and metal layer addresses the need for lightweight, thin, and flame-resistant battery case materials by enhancing strength and resistance, ensuring safety against heat abnormalities.
Patent Information
- Application Number
- JP2024538960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-04
- Filing Date
- 2023-07-13
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2043-07-13
AI Technical Summary
Existing battery case materials face challenges in achieving a balance between being lightweight, thin, and providing high flame resistance and strength, especially for applications like electric vehicle batteries, as conventional resin foam cores are easily flammable and require thickness for adequate flame resistance.
A laminate structure comprising a core layer of foam, an outer layer of fiber-reinforced plastic, and a metal layer, with the foam core compressed to enhance flame resistance and strength, utilizing specific resin compositions and manufacturing methods to ensure lightweight and thin profiles.
The laminate achieves excellent flame resistance and strength, suitable for battery cases, preventing excessive temperature rise during abnormal heat generation, thus ensuring safety.
Smart Images

Figure 0007582565000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate that is lightweight and thin while also having excellent flame resistance and strength, and can be suitably used for various molded product applications, and a battery case using the same. [Background technology]
[0002] Lithium-ion batteries, which are used in many electric vehicles, have the risk of catching fire, so their battery cases must be strong and highly flame-resistant and fire-resistant. At the same time, to realize cars with better fuel economy and a lower environmental impact, molding materials that can further reduce the weight and space of the battery case itself while fully maintaining the above-mentioned performance are required.
[0003] As a lightweight and high-strength molding material, a so-called FRP sandwich molded body is known, in which a resin foam is used as a core material and is sandwiched between fiber-reinforced plastics (see, for example, Patent Document 1). However, the resin foam used as the core material of the sandwich molded body is generally flammable, and in order to impart a certain degree of flame resistance, a resin foam with a sufficient thickness must be used, so it was not usable for applications such as battery cases that require both high flame resistance and fire resistance, as well as light weight and space saving. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-80629 A Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, the problem that the present invention aims to solve is to provide a molding material that is lightweight and thin-walled while having excellent flame resistance and strength, and that can be suitably used for molded products such as battery cases, and a battery case using the same. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that a laminate having a core layer (A) made of a foam, an outer layer (B) made of a fiber-reinforced plastic, and a metal layer (C), with the metal layer (C) located between the core layer (A) and the outer layer (B), has the characteristics of being lightweight and thin yet excellent in flame resistance and strength, and can be used for various molded products including battery cases, and have completed the present invention.
[0007] That is, the present invention relates to (I) a laminate having a core layer (A) made of a foam, an outer layer (B) made of a fiber-reinforced plastic, and a metal layer (C), wherein the metal layer (C) is located between the core layer (A) and the outer layer (B).
[0008] The present invention further relates to (II) the laminate according to the above (I), wherein the core layer (A) is formed by compressing a foam in the thickness direction.
[0009] The present invention further relates to (III) the laminate according to (II) above, wherein the core layer (A) has a compressibility of 40% or more in terms of thickness.
[0010] The present invention further relates to (IV) the laminate according to the above (II) or (III), wherein the aspect ratio of foam cells of the core layer (A) is 2 or more.
[0011] The present invention further relates to (V) the laminate according to any one of (I) to (IV) above, wherein the outer layer (B) is obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r), and the matrix resin is a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), or a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
[0012] The present invention further relates to (VI) the laminate according to any one of (I) to (V) above, wherein the metal layer (C) is aluminum.
[0013] The present invention further relates to (VII) a method for producing the laminate described in any one of (I) to (VI) above, which comprises hot molding a precursor obtained by laminating a core layer (A) made of a foam, an outer layer (b) made of a prepreg containing a reinforcing fiber (f) and a matrix resin (r), and a metal layer (C).
[0014] The present invention further relates to (VIII) a method for producing the laminate described in any one of (I) to (VI), wherein the core layer (A), the outer layer (B) made of fiber-reinforced plastic, and the metal layer (C) are bonded together using an adhesive.
[0015] The present invention further relates to (IX) a battery case using the laminate described in any one of (I) to (VI). Effect of the Invention
[0016] According to the present invention, it is possible to provide a laminate which is lightweight and thin while having excellent flame resistance and strength, and which can be suitably used for molded products such as battery cases, and a battery case using the laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below.
[0018] The laminate of the present invention is characterized in that it has a core layer (A) made of a foam, an outer layer (B) made of a fiber-reinforced plastic, and a metal layer (C), and that the metal layer (C) is located between the core layer (A) and the outer layer (B).
[0019] As the foam to be the core layer (A), foams made of various resin materials can be used without any particular limitation. Examples of the resin materials include polyurethane resin, phenol resin, melamine resin, acrylic resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polystyrene resin, styrene acrylic resin, ABS resin, polyphenylene ether resin, polyetherimide resin, polymethyl methacrylate resin, polymethacrylimide resin, etc. The foaming method and foaming agent used for these resin materials are not particularly limited, and those foamed by a known and commonly used foaming agent and foaming method can be used. Among them, bead foams are preferable because the resulting laminate has better flame resistance, and bead foams of polystyrene resin are more preferable.
[0020] The bead foam can be produced, for example, by a method in which a foaming gas is injected into particles made of the various resin materials, the particles are heated to pre-expand, and the resulting foam beads are foamed under heat and pressure. The average particle size of the foam beads is preferably in the range of 0.5 to 5 mm, since the resulting laminate has better flame resistance and strength. Examples of the foaming gas include propane, butane, and pentane, and the amount of gas injected is preferably 5 to 7 mass % of the foam beads. The expansion ratio is preferably 40 to 70 times, since the resulting laminate has better flame resistance and strength. The density of the foam is preferably 0.01 to 0.07 g / cm, since the laminate has a good balance of light weight, flame resistance, and strength. 3 It is preferable that the range is 100%.
[0021] In the bead foam, a functional coating agent is applied to the surface of the foamable beads, which are the raw material, to impart desired performance to the resulting foam. Examples of the functional coating agent include a flame retardant coating agent and a heat-resistant coating agent. Among them, a resin bead foam having a flame retardant coating agent applied to the surface is preferred, since the resulting laminate has better flame retardancy. Examples of the flame retardant coating agent include a phosphorus atom-containing compound, a halogen atom-containing compound, a nitrogen atom-containing compound, a hydrated metal compound, a borate, a metal oxide, a silicone compound, and the like, as a flame retardant.
[0022] The core layer (A) of the present invention may be a foam as it is, or may be a foam compressed in the thickness direction. In particular, the core layer (A) is preferably a foam compressed in the thickness direction, since the resulting laminate is thin and has sufficient flame resistance. When the core layer (A) is a foam compressed in the thickness direction, the compression ratio of the foam is preferably 40% or more, more preferably 75% or more, and particularly preferably 85% or more, in terms of thickness, since the resulting laminate is thin and has sufficient flame resistance. Also, it is preferably 97% or less, and more preferably 95% or less. Also, the aspect ratio of the foam cells is preferably 1.7 or more, more preferably 4 or more, and particularly preferably 6.7 or more, since the resulting laminate is thin and has sufficient flame resistance. Also, it is preferably 30 or less, and more preferably 20 or less. The aspect ratio of the foam cells may be either an actual value measured by observing the cross section of the foam with a microscope, or a calculated value calculated from the compression ratio. Aspect ratio = 1 / [1-compression ratio(%) / 100]
[0023] The thickness of the core layer (A) is preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm, since the resulting laminate has an excellent balance of flame resistance, strength, and light weight. The core layer (A) may be formed of only one layer, or may be formed of multiple layers. When the core layer (A) is multiple layers, each layer may be formed of the same type of foam, or each layer may be formed of different types of foam. Some layers may be uncompressed foam, and some layers may be compressed foam. Even when the core layer (A) is multiple layers, the total thickness of the core layer (A) is preferably in the range of 0.5 to 5 mm, more preferably in the range of 1 to 3 mm.
[0024] The outer layer (B) made of the fiber reinforced plastic is specifically obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r).
[0025] Examples of the reinforcing fiber (f) include carbon fiber, glass fiber, silicon carbide fiber, alumina fiber, boron fiber, metal fiber, aramid fiber, vinylon fiber, tetron fiber, and other organic fibers. These may be used alone or in combination of two or more. Among these, carbon fiber or glass fiber is preferred because it can provide a laminate with higher strength.
[0026] As the carbon fiber, various types of fibers such as polyacrylonitrile, pitch, and rayon can be used. Among these, polyacrylonitrile-based fibers are preferred because they provide carbon fibers with higher strength.
[0027] The shape of the reinforcing fiber (f) is not particularly limited, and examples thereof include reinforcing fiber tows in which reinforcing fiber filaments are converged, unidirectional materials in which reinforcing fiber tows are aligned in one direction, woven fabrics, short-cut reinforcing fibers, and nonwoven fabrics and papers made of short-cut reinforcing fibers. When the reinforcing fiber (f) is a fabric, examples thereof include a plain weave, twill weave, satin weave, or non-crimped fabric, which is a sheet in which fiber bundles are aligned in one direction, or a sheet laminated at different angles, stitched to prevent unraveling. When short-cut reinforcing fibers are used as the reinforcing fibers (f), it is preferable to use those cut to 2.5 to 50 mm, since this improves the flowability in the mold during molding and the appearance of the molded product. Among these, it is preferable to use unidirectional materials or woven fabrics as the reinforcing fibers, since this results in a higher-strength outer layer (B). When using a prepreg using unidirectional materials as the reinforcing fibers, a stronger outer layer (B) can be obtained by stacking multiple sheets in a quasi-isotropic manner, for example, with the fiber directions alternating between 0° and 90°.
[0028] Weight of reinforcing fiber (f) (fiber 1m 2 There is no particular restriction on the weight per unit area, and a wide variety of weights per unit area can be used. The optimum value also differs depending on the reinforcing fiber (f). In general, a weight per unit area of 30 to 650 g / m is used because it provides an excellent balance between the uniformity of the fiber width of the reinforcing fiber (f) and the impregnation with the matrix resin (r). 2 In the case where the reinforcing fiber (f) is a glass fiber, it is preferable that the thickness is in the range of 50 g / m 2 It is preferable that the thickness is 100 g / m or more. 2 More preferably, it is 600 g / m or more. 2 It is preferable that the thickness is less than 350 g / m 2 It is more preferable that the reinforcing fiber (f) is a carbon fiber. 2 It is preferable that the thickness is 80 g / m or more. 2 More preferably, it is 300 g / m or more. 2 It is preferable that the thickness is less than 200 g / m 2 It is more preferable that:
[0029] The content of the reinforcing fibers (f) in the prepreg is preferably 40% by mass or more, more preferably 50% by mass or more, since this results in a stronger outer layer (B), and is preferably 90% by mass or less, more preferably 80% by mass or less.
[0030] The matrix resin (r) can be impregnated into the reinforcing fiber (f) and can be molded by heating or the like, and a wide variety of resins can be used without any particular limitations. Among them, a thermosetting resin composition is preferable from the viewpoint of ease of handling. Furthermore, since the obtained outer layer (B) has high strength, is easy to handle, and is excellent in moldability into various shapes, it is preferable that the resin composition contains a urethane reaction component formed by an isocyanate group and a hydroxyl group, and that a polymerizable unsaturated group is present in the resin composition. Examples of such resin compositions include a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), and a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
[0031] In the present invention, a (meth)acrylate compound refers to a compound having either or both of an acryloyl group and a methacryloyl group, a (meth)acryloyl group refers to either or both of an acryloyl group and a methacryloyl group, and a (meth)acrylic acid refers to either or both of acrylic acid and methacrylic acid.
[0032] Examples of the polyisocyanate compound (r1) include aliphatic diisocyanate compounds such as butane diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and dimer acid diisocyanate; alicyclic diisocyanate compounds such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate; tolylene diisocyanate, Examples of the isocyanate include aromatic diisocyanate compounds such as xylylene diisocyanate, tetramethyl xylylene diisocyanate, lysine diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate; and modified isocyanurate compounds, biuret modified compounds, allophanate modified compounds, carbodiimide modified compounds, urethane imine modified compounds, and polyol modified compounds modified with polyols such as diethylene glycol and dipropylene glycol. These compounds may be used alone or in combination. Among these, aromatic diisocyanate compounds and various modified compounds thereof are preferred because they provide an outer layer (B) with excellent heat resistance. When multiple types of polyisocyanate compounds (r1) are used in combination, the proportion of aromatic diisocyanate compounds and their various modified products relative to the total mass of polyisocyanate compounds (r) is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0033] The polyhydroxy(meth)acrylate compound (r2) may, for example, be a (meth)acrylate compound obtained by reacting an epoxy resin with (meth)acrylic acid.
[0034] Examples of the epoxy resin include diglycidyloxybenzene, diglycidyloxynaphthalene, aliphatic epoxy resins, biphenol type epoxy resins, bisphenol type epoxy resins, novolac type epoxy resins, alicyclic epoxy resins, glycidylamine type epoxy resins, heterocyclic type epoxy resins, glycidyl ester type epoxy resins, triphenolmethane type epoxy resins, phenol or naphthol aralkyl type epoxy resins, phenylene or naphthylene ether type epoxy resins, oxodoridone modified epoxy resins, and brominated epoxy resins thereof. The epoxy resin may be an epoxy resin obtained by extending the above-mentioned specific examples with an extender.
[0035] Examples of the aliphatic epoxy resin include various aliphatic polyol compounds and polyglycidyl ethers of one or more of these alkylene oxide adducts with epihalohydrin. Examples of the aliphatic polyol compounds include ethylene glycol, propylene glycol, 1,3-propanediol, 2-methylpropanediol, 1,2,2-trimethyl-1,3-propanediol, 2,2-dimethyl-3-isopropyl-1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1, Examples of the diol compounds include aliphatic diol compounds such as 6-hexanediol, 1,4-bis(hydroxymethyl)cyclohexane, and 2,2,4-trimethyl-1,3-pentanediol; alicyclic diol compounds such as 2,2-bis(4-hydroxyphenyl)propane; and aliphatic polyol compounds with three or more functional groups such as trimethylolethane, trimethylolpropane, glycerin, hexanetriol, pentaerythritol, ditrimethylolpropane, and dipentaerythritol.
[0036] Examples of the biphenol type epoxy resin include biphenol compounds such as biphenol and tetramethylbiphenol, and polyglycidyl ethers of one or more of these alkylene oxide adducts with epihalohydrin.
[0037] Examples of the bisphenol type epoxy resin include bisphenol compounds such as bisphenol A, tetrabromobisphenol A, bisphenol F, bisphenol S, bisphenol fluorene, and biscresol fluorene, and alkylene oxide adducts thereof which are polyglycidyl etherified with epihalohydrin.
[0038] The novolac type epoxy resin may be, for example, a novolac resin formed from one or more of various phenolic compounds such as phenol, dihydroxybenzene, cresol, xylenol, naphthol, dihydroxynaphthalene, bisphenol, or biphenol, which is polyglycidyl etherified with epihalohydrin.
[0039] Examples of the alicyclic epoxy resin include those obtained by hydrogenating the biphenol compounds or bisphenol compounds, and those obtained by polyglycidyl etherifying one or more of the alkylene oxide adducts thereof with epihalohydrin, as well as 3,4-epoxy-6-methylcyclohexylmethyl-3,4-epoxy-6-methylcyclohexanecarboxylate, 1-epoxyethyl-3,4-epoxycyclohexane, and the like.
[0040] Examples of the glycidylamine type epoxy resin include N,N-diglycidylaniline, triglycidylaminophenol, tetraglycidylxylenediamine, and 4,4'-methylenebis[N,N-diglycidylaniline].
[0041] Examples of the heterocyclic epoxy resin include 1,3-diglycidyl-5,5-dimethylhydantoin and triglycidyl isocyanurate.
[0042] Examples of the glycidyl ester type epoxy resin include diglycidyl phthalate, diglycidyl tetrahydrophthalate, diglycidyl-p-oxybenzoate, and glycidyl dimerate.
[0043] Examples of the extender for the epoxy resin include the above-mentioned various biphenol compounds and hydrogenated products thereof, the above-mentioned various bisphenol compounds and hydrogenated products thereof, dibasic acid compounds, and acid group-containing polyester resins.
[0044] Among these, the bisphenol type epoxy resin is preferred because it is excellent in impregnation into the reinforcing fiber (f) and in the strength of the resulting outer layer (B), etc. In this case, the epoxy equivalent of the epoxy resin is preferably in the range of 150 to 600 g / equivalent, and more preferably in the range of 200 to 450 g / equivalent.
[0045] The reaction between the epoxy resin and (meth)acrylic acid can be carried out by heating at a temperature of about 60 to 140° C. in the presence of any esterification catalyst. If necessary, a reaction solvent or a polymerization inhibitor may be added. The reaction ratio between the epoxy resin and (meth)acrylic acid is preferably such that the molar ratio of the functional groups of both [carboxy group / epoxy group] is in the range of 0.6 to 1.1.
[0046] When the bisphenol type epoxy resin is used as the epoxy resin, the hydroxyl value of the resulting (meth)acrylate compound is preferably 50 to 200 mg / KOH, and the (meth)acryloyl group equivalent is preferably in the range of 300 to 600 g / equivalent.
[0047] The polyhydroxy(meth)acrylate compound (r2) may be used alone or in combination of two or more. When two or more polyhydroxy(meth)acrylate compounds (r2) are used in combination, the ratio of the bisphenol type epoxy resin (meth)acrylate compound to the total mass of the polyhydroxy(meth)acrylate compound (r2) is preferably 50 mass% or more, more preferably 70 mass% or more, and particularly preferably 80 mass% or more.
[0048] Examples of the monohydroxy(meth)acrylate compound (r3) include hydroxyethyl(meth)acrylate, hydroxypropyl(meth)acrylate, hydroxybutyl(meth)acrylate, trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, (poly)oxyalkylene(meth)acrylate compounds having (poly)oxyalkylene chains such as (poly)oxyethylene chains, (poly)oxypropylene chains, and (poly)oxytetramethylene chains introduced into these molecular structures, and lactone-modified (meth)acrylate compounds having (poly)lactone structures introduced into these molecular structures. These may be used alone or in combination.
[0049] Among them, monohydroxymono(meth)acrylate compounds are preferred, and hydroxyethyl(meth)acrylate is more preferred, because they provide an excellent balance between the impregnation of the reinforcing fiber (f) and the strength of the resulting outer layer (B). When a plurality of monohydroxy(meth)acrylate compounds (r3) are used in combination, the proportion of hydroxyethyl(meth)acrylate to the total mass of the monohydroxy(meth)acrylate compounds (r3) is preferably 50% by mass or more, more preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0050] Examples of the polyhydroxy compound (r4) include dihydroxybenzene, dihydroxynaphthalene, the various aliphatic polyols mentioned above, biphenol compounds, bisphenol compounds, their alkylene oxide adducts, and lactone-modified compounds. These may be used alone or in combination. Among them, alkylene oxide adducts of bisphenol compounds are preferred because they provide an excellent balance between the impregnation of the reinforcing fibers (f) and the strength of the resulting outer layer (B). The average number of moles of alkylene oxide added is preferably in the range of 2 to 10 moles.
[0051] When multiple types of polyhydroxy compounds (r4) are used in combination, the ratio of the alkylene oxide adduct of a bisphenol compound to the total mass of the polyhydroxy compounds (r4) is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0052] In the resin composition (1), the molar ratio (NCO / OH) of the isocyanate group contained in the polyisocyanate compound (r1) to the hydroxyl group contained in the polyhydroxy(meth)acrylate compound (r2) is preferably in the range of 0.3 to 1.2, more preferably in the range of 0.4 to 1.1, and particularly preferably in the range of 0.5 to 1.0, in order to provide an excellent prepreg in terms of ease of handling, moldability, etc.
[0053] In the resin composition (2), the molar ratio (NCO / OH) of the isocyanate group contained in the polyisocyanate compound (r1) to the total of the hydroxyl group contained in the monohydroxy(meth)acrylate compound (r3) and the polyhydroxy compound (r4) is preferably in the range of 0.7 to 1.3, more preferably in the range of 0.8 to 1.1, and particularly preferably in the range of 0.8 to 1.0, in order to provide excellent ease of handling and moldability of the prepreg. The molar ratio (r3 / r4) of the monohydroxy(meth)acrylate compound (r3) to the polyhydroxy compound (r4) is preferably in the range of 40 / 60 to 80 / 20, and more preferably in the range of 50 / 50 to 70 / 30, in order to provide further improved heat resistance and curability.
[0054] The resin compositions (1) and (2) may contain a polymerizable unsaturated group-containing compound other than the polyhydroxy(meth)acrylate compound (r2) and the monohydroxy(meth)acrylate compound (r3). Specific examples thereof include aliphatic mono(meth)acrylate compounds such as methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, isodecyl(meth)acrylate, lauryl(meth)acrylate, isotridecyl(meth)acrylate, n-stearyl(meth)acrylate, ethylene glycol(meth)acrylate alkyl ether, and propylene glycol(meth)acrylate alkyl ether; alicyclic mono(meth)acrylate compounds such as cyclohexyl(meth)acrylate, isobornyl(meth)acrylate, adamantyl mono(meth)acrylate, dicyclopentenyloxyethyl(meth)acrylate, and dicyclopentanyl methacrylate; glycidyl(meth)acrylate, tetrahydrofurfuryl acrylate, and the like. heterocyclic ring-containing mono(meth)acrylate compounds such as benzyl (meth)acrylate, phenyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenoxybenzyl (meth)acrylate, benzyl benzyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, and other aromatic ring-containing mono(meth)acrylate compounds; (poly)oxyalkylene-modified mono(meth)acrylate compounds in which a polyoxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the various mono(meth)acrylate monomers mentioned above; lactone-modified mono(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the various mono(meth)acrylate compounds mentioned above;Aliphatic di(meth)acrylate compounds such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate; 1,4-cyclohexanedimethanol di(meth)acrylate, norbornane di(meth)acrylate, norbornane dimethanol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate. alicyclic di(meth)acrylate compounds such as biphenol di(meth)acrylate and bisphenol di(meth)acrylate; aromatic ring-containing di(meth)acrylate compounds such as biphenol di(meth)acrylate and bisphenol di(meth)acrylate; polyoxyalkylene-modified di(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the above-mentioned various di(meth)acrylate compounds; lactone-modified di(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the above-mentioned various di(meth)acrylate compounds. Meth)acrylate compounds; aliphatic tri(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate and glycerin tri(meth)acrylate; (poly)oxyalkylene-modified tri(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the aliphatic tri(meth)acrylate compounds; lactone-modified compounds in which a (poly)lactone structure has been introduced into the molecular structure of the aliphatic tri(meth)acrylate compounds tri(meth)acrylate compounds; tetrafunctional or higher aliphatic poly(meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc.; tetrafunctional or higher (poly)oxyalkylene-modified poly(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the aliphatic poly(meth)acrylate compounds;Examples of the poly(meth)acrylate compound include tetrafunctional or higher lactone-modified poly(meth)acrylate compounds in which a (poly)lactone structure is introduced into the molecular structure of the aliphatic poly(meth)acrylate compound. These may be used alone or in combination of two or more kinds.
[0055] Among these, since they provide an excellent balance between the impregnation into the reinforcing fibers (f) and the strength of the resulting outer layer (B), preferred are difunctional or higher (meth)acrylate compounds having a molecular weight in the range of 150 to 600. When a plurality of types of other polymerizable unsaturated group-containing compounds are used in combination, the ratio of difunctional or higher (meth)acrylate compounds having a molecular weight in the range of 150 to 600 to the total mass of other polymerizable unsaturated group-containing compounds is preferably 50 mass% or more, more preferably 80 mass% or more, and particularly preferably 90 mass% or more.
[0056] When other polymerizable unsaturated group-containing compounds are used in the resin composition (1), the blending amount is preferably 40 mass% or less, more preferably 30 mass% or less, based on the total mass of the polyisocyanate compound (r1) and the polyhydroxy(meth)acrylate compound (r2), in order to obtain an excellent balance between the impregnation property into the reinforcing fiber (f) and the strength of the resulting outer layer (B). When other polymerizable unsaturated group-containing compounds are used in the resin composition (2), the blending amount is preferably 40 mass% or less, more preferably 30 mass% or less, based on the total mass of the polyisocyanate compound (r1), the monohydroxy(meth)acrylate compound (r3), and the polyhydroxy compound (r4).
[0057] The resin compositions (1) and (2) may contain a polymerization initiator. The polymerization initiator may be any of the general types without any particular limitation, but is preferably an organic peroxide. Examples of organic peroxides include diacyl peroxide compounds, peroxyester compounds, hydroperoxide compounds, ketone peroxide compounds, alkyl perester compounds, percarbonate compounds, and peroxyketals. These may be used alone or in combination. Among them, those having a temperature of 60° C. or higher for obtaining a 10-hour half-life are preferred because they shorten the molding time. In addition, when a laminate is manufactured by the manufacturing methods 1 and 3 described below, and particularly when the core layer (a) or the core layer (A) is a polystyrene foam, those having a 10-hour half-life temperature of 90° C. or lower are preferred, more preferably 80° C. or lower, and particularly preferably 70° C. or lower are preferred, in order to avoid molding defects due to swelling of the polystyrene foam. Examples of such polymerization initiators include 1,6-bis(t-butylperoxycarbonyloxy)hexane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-amylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, t-butylperoxydiethyl acetate, t-butylperoxyisopropyl carbonate, t-butylperoxy2-ethylhexyl carbonate, t-amylperoxyisopropyl carbonate, and t-amylperoxy2-ethylhexyl. Examples of the polymerization initiator include butyl peroxy 2-ethylhexanoate, di-tert-butyl peroxy isopropyl carbonate, di-tert-butyl peroxy hexahydroterephthalate, t-amyl peroxy trimethylhexanoate, t-amyl peroxy isononaate, t-hexyl peroxy 2-ethylhexanoate, n-butyl 4,4-di(t-butylperoxy)valerate, 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, t-butyl peroxy 2-ethylhexanoate, and t-butyl peroxy pivalate. The amount of the polymerization initiator added is preferably in the range of 0.5 to 3% by mass based on the total mass of the polymerizable unsaturated group-containing compound in the resin composition.
[0058] The resin compositions (1) and (2) may contain other components in addition to the various compounds described above, such as thermoplastic resins, polymerization inhibitors, curing accelerators, fillers, low shrinkage agents, mold release agents, thickeners, viscosity reducers, pigments, antioxidants, plasticizers, flame retardants, antibacterial agents, UV stabilizers, reinforcing materials, and photocuring agents.
[0059] Examples of the thermoplastic resin include polyamide resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polycarbonate resin, urethane resin, polypropylene resin, polyethylene resin, polystyrene resin, acrylic resin, polybutadiene resin, polyisoprene resin, and resins modified by copolymerization, etc. These may be used alone or in combination of two or more.
[0060] Examples of the polymerization inhibitor include hydroquinone, trimethylhydroquinone, pt-butylcatechol, t-butylhydroquinone, toluhydroquinone, p-benzoquinone, naphthoquinone, hydroquinone monomethyl ether, phenothiazine, copper naphthenate, copper chloride, etc. These may be used alone or in combination of two or more.
[0061] Examples of the curing accelerator include metal soaps such as cobalt naphthenate, cobalt octenate, vanadyl octenate, copper naphthenate, and barium naphthenate, and metal chelate compounds such as vanadyl acetylacetate, cobalt acetylacetate, and iron acetylacetonate. Examples of amines include N,N-dimethylamino-p-benzaldehyde, N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, N-ethyl-m-toluidine, triethanolamine, m-toluidine, diethylenetriamine, pyridine, phenylmorpholine, piperidine, and diethanolaniline. These may be used alone or in combination of two or more.
[0062] The fillers are roughly classified into inorganic compounds and organic compounds. Fillers are components added mainly for the purpose of adjusting the physical properties such as strength, elastic modulus, impact strength, and fatigue durability of molded products.
[0063] Examples of the inorganic compounds include calcium carbonate, magnesium carbonate, barium sulfate, mica, talc, kaolin, clay, celite, asbestos, barite, baryta, silica, silica sand, dolomite limestone, gypsum, aluminum fine powder, hollow balloons, alumina, glass powder, aluminum hydroxide, kansui stone, zirconium oxide, antimony trioxide, titanium oxide, molybdenum dioxide, and iron powder. Examples of the organic compounds include natural polysaccharide powders such as cellulose and chitin, and synthetic resin powders. Examples of the synthetic resin powder include organic powders composed of hard resins, soft rubbers, elastomers, or polymers (copolymers), and particles having a multilayer structure such as a core-shell type. Specific examples of the synthetic resin powder include particles composed of butadiene rubber, acrylic rubber, urethane rubber, silicone rubber, and the like, polyimide resin powder, fluororesin powder, and phenolic resin powder. These may be used alone or in combination of two or more types.
[0064] Examples of the release agent include zinc stearate, calcium stearate, paraffin wax, polyethylene wax, carnauba wax, etc. Preferred are paraffin wax, polyethylene wax, carnauba wax, etc. These may be used alone or in combination of two or more.
[0065] Examples of the thickener include metal oxides and hydroxides such as magnesium oxide, magnesium hydroxide, calcium oxide, and calcium hydroxide, and acrylic resin-based fine particles. These thickeners can be used alone or in combination of two or more kinds.
[0066] Examples of the flame retardant include a phosphorus atom-containing compound, a halogen atom-containing compound, a nitrogen atom-containing compound, a hydrated metal compound, a borate, a metal oxide, a silicone compound, etc. These flame retardants can be used alone or in combination of two or more kinds.
[0067] The method for producing the prepreg is not particularly limited, but examples thereof include a method in which each component of the matrix resin (r) is mixed using a known mixer such as a static mixer, a power mixer, a planetary mixer, or a kneader, and then the matrix resin (r) is impregnated into the reinforcing fiber (f), which is then sandwiched between release films and rolled using a rolling machine. When the matrix resin (r) is impregnated into the reinforcing fiber (f), it may be heated appropriately.
[0068] When the resin compositions (1) and (2) are used as the matrix resin (r), the sheet after rolling is allowed to stand at room temperature to 50° C. to cause a urethane reaction between the isocyanate groups and the hydroxyl groups in the resin composition, thereby making it possible to obtain a prepreg having excellent storage stability and ease of handling. When the resin compositions (1) and (2) are used as the matrix resin (r), the resin composition may be one in which the urethane reaction has progressed partially during the preparation process of the resin composition.
[0069] The thickness of the prepreg is preferably 0.02 mm or more, more preferably 0.05 mm or more, because this allows for easy handling and excellent moldability, and is preferably 1.0 mm or less, more preferably 0.5 mm or less.
[0070] The outer layer (B) can be obtained by hot molding the prepreg. An example of the hot molding method is, for example, a method in which a plurality of prepregs are laminated and placed in a mold preheated to 110°C to 160°C, molded by a compression molding machine, and cured while maintaining a molding pressure of 0.1 to 10 MPa. Furthermore, a manufacturing method is preferred in which a mold having a shear edge is used, a mold temperature is 130°C to 160°C, a molding pressure is maintained at 1 to 8 MPa, and hot compression molding is performed for 1 to 3 minutes per mm of thickness of the molded product. The number of prepregs to be laminated can be arbitrarily set in consideration of the balance between moldability and the strength of the obtained outer layer (B), but is preferably in the range of 1 to 20 sheets because of its excellent light weight. In addition, the orientation of the prepregs when laminating them can be arbitrarily set in consideration of the desired strength, but it is preferable to laminate them so that they are quasi-isotropic. For example, it is preferable to laminate them in order so that the fiber directions are alternated between 0° and 90°. From the viewpoint of the balance between the strength and the light weight of the resulting laminate, the thickness of the outer layer (B) is preferably 0.1 mm or more, more preferably 0.4 mm or more, and particularly preferably 0.6 mm or more, and is preferably 2.0 mm or less, and more preferably 1.5 mm or less.
[0071] The metal layer (C) can be made of various metal foils or thin metal films without any particular limitations. Specific metal species include, for example, aluminum, chromium, gold, silver, copper, titanium, iron, and stainless steel. These metals may be used as metal foils or tapes with metal foils, or may be formed into films by methods such as vapor deposition, plating, and sputtering. The thickness of the metal layer (C) is preferably 0.006 mm or more, and more preferably 0.01 mm or more, because the resulting laminate has an excellent balance between flame resistance and light weight. Also, it is preferably 0.2 mm or less, and more preferably 0.1 mm or less.
[0072] In the laminate of the present invention, the metal layer (C) is located between the core layer (A) and the outer layer (B). The metal layer (C) may be present on only one side of the core layer (A) or on both sides. In addition, three or more metal layers (C) may be present in the laminate. The metal layer (C) may be adjacent to the core layer (A) or the outer layer (B), or both, and other layers may be present between the metal layer (C) and the core layer (A), between the metal layer (C) and the outer layer (B), or both. Examples of the other layers include a resin layer and an adhesive layer. In the laminate of the present invention, the core layer (A), the outer layer (B), and the metal layer (C) may each be multi-layered. In any case, the ratio of the total thickness of the core layer (A), the outer layer (B), and the metal layer (C) to the total thickness of the laminate is preferably 80% or more, more preferably 85% or more.
[0073] The method for producing the laminate of the present invention is not particularly limited, and the laminate can be produced by a wide variety of methods depending on the application and desired shape of the laminate. As some specific examples, the following three production methods can be mentioned. These production methods will be described below. (Production Method 1) A method for producing a laminate by hot molding a precursor obtained by laminating a core layer (A) made of a foam, an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r), and a metal layer (C). (Production method 2) A method for producing a laminate in which the core layer (A), the outer layer (B) made of fiber-reinforced plastic, and the metal layer (C) are bonded together using an adhesive
[0074] The manufacturing method 1 is a method of hot-molding a precursor in which a core layer (A) made of a foam, an outer layer (b) made of a prepreg containing a reinforcing fiber (f) and a matrix resin (r), and the metal layer (C) are laminated. As described above, the core layer (A) may be a compressed foam, and in this case, a pre-compressed one may be used as the core layer (A), or an uncompressed one may be used and compressed during hot-molding. Also, as described above, the outer layer (b) is preferably a layer of a plurality of prepregs, specifically, 1 to 20 prepregs are preferably laminated. The lamination direction when laminating the prepregs can be arbitrarily set in consideration of the desired strength, but it is preferable to laminate them so as to be quasi-isotropic, and for example, it is preferable to laminate them in order so that the fiber directions are alternately 0° and 90°. The core layer (A), the outer layer (b), and the metal layer (C) may be directly laminated, or other layers such as adhesive layers may be provided between them. Furthermore, when producing a laminate by Production Method 1, in order to prevent the foam constituting the core layer (a) from further foaming in the heat forming step, the moldable temperature of the prepreg constituting the outer layer (b) is preferably 140°C or lower, and more preferably 110°C or lower.
[0075] In the above-mentioned manufacturing method 1, the molding conditions are not particularly limited, but examples thereof include a method of molding at a temperature of 80 to 140°C and a pressure of 0.1 to 6 MPa for several minutes to several tens of minutes. If necessary, a mold release agent may be applied to the mold, and the precursor is preferably filled in the center of the mold. In addition, the thickness of the laminate may be adjusted using a spacer or the like so that the thickness of the laminate is a predetermined thickness.
[0076] The manufacturing method 2 is a method of bonding the core layer (A), the outer layer (B), and the metal layer (C) using an adhesive. The core layer (A), the outer layer (B), and the metal layer (C) used in the manufacturing method 2 are as described above. The adhesive used in the manufacturing method 2 is not particularly limited and is selected according to the application and desired shape of the laminate, and examples thereof include acrylic resin-based, urethane resin-based, rubber-based, polyester resin-based, epoxy resin-based, cyanoacrylate resin-based, silicone resin-based, and modified silicone resin-based adhesives. The adhesive may be in any form, such as one-liquid liquid, two-liquid liquid, sheet, or double-sided tape.
[0077] In the manufacturing method 3, the molding conditions are not particularly limited, but examples include a method of molding at a temperature of 80 to 140°C and a pressure of 0.1 to 6 MPa for several minutes to several tens of minutes. If necessary, a mold release agent may be applied to the mold, and the precursor is preferably filled in the center of the mold. In addition, the thickness of the laminate may be adjusted using a spacer or the like so that the thickness of the laminate is a predetermined thickness.
[0078] The laminate of the present invention is characterized by being lightweight yet having excellent flame resistance and strength, and therefore can be suitably used for various applications such as aerospace aircraft components, railway vehicle components, housing equipment components, electronic equipment components, medical equipment components, home appliance components, and automobile components, in addition to battery cases. EXAMPLES
[0079] The present invention will now be described in more detail with reference to examples and comparative examples. In the following, "parts" and "%" are by weight unless otherwise specified.
[0080] Production Example 1: Production of prepreg (1) In a 1L flask equipped with a thermometer, nitrogen and air inlet tubes, a cooling condenser, and a stirrer, epoxy resin (DIC Corporation's "Epicron 152"), 365 parts by mass of tetrabromobisphenol A type epoxy resin (epoxy equivalent 365 g / equivalent, bromine content 48.1% by mass), 84 parts by mass of methacrylic acid, and 0.18 parts by mass of t-butylhydroquinone as a polymerization inhibitor were charged, and the temperature was raised to 95°C under a gas flow of a 1:1 mixture of nitrogen and air. 0.9 parts by mass of triphenylphosphine was added as a catalyst, the temperature was raised to 105°C, and the reaction was carried out for 12 hours. When the acid value became 1 or less, the reaction was terminated. After cooling to around 80°C, the mixture was removed from the reaction vessel to obtain epoxy methacrylate (1). The hydroxyl value of this resin was 135 mgKOH / g. The (meth)acryloyl group equivalent of this resin was 450 g / equivalent.
[0081] Diphenylmethane diisocyanate (13 parts by mass, "Lupranate MI" manufactured by BASFINOAC Polyurethanes Co., Ltd.), 80 parts by mass of the epoxy (meth)acrylate resin (1) obtained above, 20 parts by mass of an ethylenically unsaturated monomer (butanediol dimethacrylate), and 11.3 parts by mass of a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide, 10-hour half-life temperature 87°C) were mixed to obtain a matrix resin (1). Using a prepreg manufacturing device, glass fibers ("ER1620F" manufactured by Nippon Electric Glass Co., Ltd., glass fiber basis weight 162 g / m) were mixed. 2 ) was impregnated with matrix resin (1) so that the resin mass content was 35%, to obtain a prepreg (1) with a thickness of 0.13 mm.
[0082] Production Example 2: Production of prepreg (2) Diphenylmethane diisocyanate (13 parts by mass, "Lupranate MI" manufactured by BASFINOAC Polyurethanes Co., Ltd.), 80 parts by mass of the epoxy (meth)acrylate resin (1) obtained in Production Example 1, 20 parts by mass of an ethylenically unsaturated monomer (butanediol dimethacrylate), and 18.1 parts by mass of a polymerization initiator ("Trigonox 421-70" manufactured by Kayaku Akzo Co., Ltd., organic peroxide, 10-hour half-life temperature 65°C) were mixed to obtain a matrix resin (2). Using a prepreg manufacturing device, glass fibers ("ER1620F" manufactured by Nippon Electric Glass Co., Ltd., glass fiber basis weight 162 g / m) were mixed. 2 ) was impregnated with matrix resin (2) so that the resin mass content was 35%, to obtain a prepreg (2) with a thickness of 0.13 mm.
[0083] Production Example 3: Production of prepreg (3) A mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, content of polymethylene polyphenyl polyisocyanate: 55 to 65 mass parts), 100 mass parts of hydroxyethyl methacrylate, 24 mass parts of ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl equivalent: 164 g / equivalent), 31 mass parts of ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl equivalent: 204 g / equivalent), and 2.1 mass parts of polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide) were mixed to obtain a matrix resin (2). Using a prepreg manufacturing device, glass fiber ("ER1620F" manufactured by Nippon Electric Glass Co., Ltd., glass fiber weight 162g / m 2 ) was impregnated with matrix resin (3) so that the resin mass content was 35%, to obtain a prepreg (3) with a thickness of 0.13 mm.
[0084] Production Example 4: Production of prepreg (4) A mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, content of polymethylene polyphenyl polyisocyanate: 55 to 65% by mass) was mixed with 100 parts by mass of hydroxyethyl methacrylate, 59 parts by mass of ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent: 164 g / equivalent) with 24 parts by mass, ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl group equivalent: 204 g / equivalent) with 31 parts by mass, and a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide) with 2.1 parts by mass to obtain a matrix resin (3). Using a prepreg manufacturing device, carbon fiber ("T700SC" manufactured by Toray Industries, Inc., carbon fiber basis weight: 100 g / m 2 ) was impregnated with matrix resin (4) so that the resin mass content was 34%, to obtain a prepreg (4) with a thickness of 0.1 mm.
[0085] Production Example 5 Production of prepreg (5) A mixture of polymethylene polyphenyl polyisocyanate and diphenylmethane diisocyanate ("Millionate MR-200" manufactured by Tosoh Corporation, content of polymethylene polyphenyl polyisocyanate: 55 to 65% by mass) of 100 parts by mass, hydroxyethyl methacrylate of 59 parts by mass, ethylene oxide adduct of bisphenol A ("Newpol BPE-20" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl equivalent: 164 g / equivalent) of 24 parts by mass, ethylene oxide adduct of bisphenol A ("Newpol BPE-40" manufactured by Sanyo Chemical Industries, Ltd., hydroxyl equivalent: 204 g / equivalent) of 31 parts by mass, and a polymerization initiator ("Trigonox 122-C80" manufactured by Kayaku Akzo Co., Ltd., organic peroxide) of 2.1 parts by mass were mixed to obtain a matrix resin (3). Using an SMC manufacturing device, carbon fibers were cut into 1 / 2 inch pieces and randomly scattered (Toray Industries, Inc. "T700SC", carbon fiber weight 1150g / m 2 ) was impregnated with matrix resin (4) so that the resin mass content was 43%, to obtain a prepreg (5) with a thickness of 1.6 mm.
[0086] Examples 1 to 7 and Comparative Example 1 The laminates (1) to (7) and the laminate (1') were produced in the following manner and subjected to various evaluation tests. The evaluation results of each laminate are shown in Table 1.
[0087] Example 1: Production of Laminate (1) The prepreg (1) obtained in Production Example 1 was cut into sizes of 298 mm x 218 mm and 298 mm x 218 mm, and four sheets were laminated in order so that the fiber directions of the prepreg were alternated between the 0° direction and the 90° direction. This was filled into the center of a flat plate mold coated with a mold release agent, and compression molded under conditions of a pressure of 4 MPa, an upper mold temperature of 140°C, a lower mold temperature of 135°C, and a molding time of 3 minutes to obtain an outer layer (B1) of 300 mm x 220 mm x 0.5 mm. The flexural modulus of the outer layer (B1) measured in accordance with JIS K 7017 was 24.6 GPa. A 10 mm thick polystyrene foam board (Ushiomatex Co., Ltd. "Varishield"; a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm 3 The foam (expansion ratio: 60 times) was cut into a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of upper mold temperature 30°C, lower mold temperature 30°C, and molding time 5 minutes to obtain a core layer (A1) of 300 mm x 220 mm x 2 mm. The compression ratio of the core layer (A1) in the thickness direction was 80%, and the specific gravity was 0.20 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 5. An aluminum foil tape ("Aluminum Tape Strong" manufactured by Kimura MonotaRO Co., Ltd., total thickness of the tape: 0.2 mm, aluminum foil thickness: 0.025 mm) was attached to one side of the core layer (A1). Furthermore, the outer layers (B1) were attached one by one to both sides of the aluminum foil tape using flame-retardant double-sided tape ("No. 5011N" manufactured by Nitto Denko Corporation) to obtain a laminate (1).
[0088] Example 2: Production of Laminate (2) In the same manner as in Example 1, the core layer (A1) and the outer layer (B1) were obtained. Aluminum foil tape ("Aluminum Tape Strong" manufactured by Kimura MonotaRO Co., Ltd., total tape thickness 0.2 mm, aluminum foil thickness 0.025 mm) was attached to both sides of the core layer (A1). Furthermore, the outer layers (B1) were attached one by one to both sides of the aluminum foil tape using flame-retardant double-sided tape ("No. 5011N" manufactured by Nitto Denko Corporation) to obtain a laminate (2).
[0089] Example 3: Production of laminate (3) The prepreg (1) obtained in Production Example 1 was cut into sizes of 298 mm x 218 mm and 298 mm x 218 mm, and three sheets were laminated in order so that the fiber direction of the prepreg was alternated between the 0° direction and the 90° direction. This was filled into the center of a flat plate mold coated with a release agent, and compression molded in a compression molding machine under conditions of a pressure of 4 MPa, an upper mold temperature of 140°C, a lower mold temperature of 135°C, and a molding time of 3 minutes to obtain an outer layer (B2) with a width of 300 mm x 220 mm x 0.35 mm. The flexural modulus of the outer layer (B2) measured in accordance with JIS K 7017 was 24.6 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm 3 The foam (expansion ratio: 60 times) was cut to a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of upper mold temperature 30°C, lower mold temperature 30°C, and molding time 5 minutes to obtain a core layer (A2) of 300 mm x 220 mm x 1.5 mm. The compression ratio in the thickness direction of the core layer (A2) was 92.5%, and the specific gravity was 0.53 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 13.3. Aluminum foil tape ("Aluminum Tape Strong" manufactured by Kimura MonotaRO Co., Ltd., total thickness of the tape: 0.2 mm, thickness of the aluminum foil portion: 0.025 mm) was attached to both sides of the core layer (A2). Furthermore, the outer layer (B2) was attached to both sides of the aluminum foil tape using a flame-retardant double-sided tape ("No. 5011N" manufactured by Nitto Denko Corporation), to obtain a laminate (3).
[0090] Example 4: Production of Laminate (4) The prepreg (3) obtained in Production Example 3 was cut into sizes of 298 mm x 218 mm and 298 mm x 218 mm, and eight sheets were laminated in order so that the fiber directions of the prepreg were alternated between the 0° direction and the 90° direction. This was filled into the center of a flat plate mold coated with a release agent, and compression molded in a compression molding machine under conditions of a pressure of 4 MPa, an upper mold temperature of 140°C, a lower mold temperature of 135°C, and a molding time of 3 minutes to obtain an outer layer (B3) with a width of 300 mm x 220 mm x 1 mm. The flexural modulus of the outer layer (B3) measured in accordance with JIS K 7017 was 23.2 GPa. A 20 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm 3 The foam (expansion ratio: 60 times) was cut to a size of 298 mm x 218 mm, filled into the center of a flat plate mold, and compression molded under the conditions of upper mold temperature 30°C, lower mold temperature 30°C, and molding time 5 minutes to obtain a core layer (A3) of 300 mm x 220 mm x 2 mm. The compression ratio of the core layer (A3) in the thickness direction was 90%, and the specific gravity was 0.40 g / m 3 The aspect ratio of the foam cells calculated from the compressibility was 10. Aluminum foil tape ("Aluminum Tape Strong" manufactured by Kimura MonotaRO Co., Ltd., total thickness of the tape: 0.2 mm, thickness of the aluminum foil portion: 0.025 mm) was attached to both sides of the core layer (A3). Furthermore, the outer layers (B3) were attached one by one to both sides of the aluminum foil tape using flame-retardant double-sided tape ("No. 5011N" manufactured by Nitto Denko Corporation) to obtain a laminate (4).
[0091] Example 5: Production of laminate (5) The prepreg (4) obtained in Production Example 4 was cut into sizes of 298 mm x 218 mm and 298 mm x 218 mm, and 10 sheets were laminated in order so that the fiber direction of the prepreg was alternated between the 0° direction and the 90° direction. The prepreg was filled into the center of a flat plate mold coated with a release agent, and compression molded in a compression molding machine under conditions of a pressure of 4 MPa, an upper mold temperature of 140°C, a lower mold temperature of 135°C, and a molding time of 3 minutes to obtain an outer layer (B4) with a width of 300 mm x 220 mm x 1 mm. The flexural modulus of the outer layer (B4) measured in accordance with JIS K 7017 was 61.5 GPa. The core layer (A3) was obtained in the same manner as in Example 4. Aluminum foil tape ("Aluminum Tape Strong" manufactured by Kimura MonotaRO Co., Ltd., total tape thickness 0.2 mm, aluminum foil thickness 0.025 mm) was attached to both sides of the core layer (A3). Furthermore, the outer layers (B3) were attached one by one to both sides of the aluminum foil tape using flame-retardant double-sided tape ("No. 5011N" manufactured by Nitto Denko Corporation) to obtain a laminate (5).
[0092] Example 6: Production of laminate (6) A polystyrene foam plate with aluminum foil on both sides ("Bari-shield with aluminum foil on both sides" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, thickness 20 mm, density 0.04 g / cm 3 A prepreg (2) obtained in Production Example 2 was cut to a size of 298 mm x 218 mm and 298 mm x 218 mm on both sides of the cut sheet, and four sheets were laminated in order so that the fiber directions of the prepreg were alternately 0° and 90°. The prepreg was filled in the center of a flat plate mold coated with a mold release agent, and a 3 mm spacer was placed. The laminate was compression molded under the conditions of a pressure of 4 MPa, an upper mold temperature of 105°C, a lower mold temperature of 100°C, and a molding time of 5 minutes to obtain a laminate (6) of 300 mm x 220 mm x 3 mm. The laminate (6) had a core layer (A4) of 2 mm thick, an outer layer (B4) of 0.47 mm thick, and a metal layer of 0.03 mm thick. A molded article identical to the outer layer (B4) of the obtained laminate (6) was produced, and the bending modulus of the outer layer was 24.6 GPa when this molded article was measured in accordance with JIS K 7017. The molded article was produced by cutting the prepreg (2) obtained in Production Example 2 to the same size as above, laminating four sheets in the same manner, filling the center of the flat plate mold, and appropriately adjusting the filling amount, pressure, and the like.
[0093] Example 7: Production of laminate (7) The prepreg (5) obtained in Production Example 5 was cut to a size of 290 mm x 212 mm. One cut prepreg was filled into the center of a flat plate mold coated with a release agent, and compression molded under conditions of a pressure of 10 MPa, an upper mold temperature of 145°C, a lower mold temperature of 145°C, and a molding time of 3 minutes to obtain an outer layer (B4) of 300 mm x 220 mm x 1.5 mm. The flexural modulus of the outer layer (B4) measured in accordance with JIS K 7017 was 29 GPa. A laminate (7) was obtained in the same manner as in Example 2, except that the outer layer (B4) obtained was used instead of the outer layer (B1).
[0094] Comparative Example 1: Production of Laminate (1') In the same manner as in Example 1, an outer layer (B1) was obtained. A 2 mm thick polystyrene foam board ("BariShield" manufactured by Ushiomatex Co., Ltd., a styrene bead foam with a flame retardant coating on the surface, density 0.04 g / cm 3 The foam (expansion ratio: 60 times) was cut into a size of 300 mm x 220 mm to form a core layer (A5). Using a flame-retardant double-sided tape (No. 5011N, manufactured by Nitto Denko Corporation), one outer layer (B1) was attached to each side of the core layer (A5) to obtain a laminate (1').
[0095] Evaluation of laminate thickness The total thickness of the core layer (A), outer layer (B), and metal layer (C) was evaluated as the thickness of the laminate. Note that in this evaluation, the thickness of the double-sided tape and the adhesive layer of the aluminum foil tape used in the manufacturing process of the laminate were not included in the thickness of the laminate.
[0096] Measurement of specific gravity of laminate The specific gravity was evaluated by dividing the total weight of the core layer (A) and the outer layer (B) by the volume of the laminate. Note that in this evaluation, the weight and volume of the double-sided tape and aluminum foil tape used in the manufacturing process of the laminate were not included in the weight and volume of the laminate.
[0097] Flame resistance evaluation Using a gas burner, the flame was applied to the center of one side of the laminate, and the position of the flame was adjusted so that the temperature of the direct flame in contact with the laminate was 1000°C, and the laminate was heated for 6 minutes. The surface temperature of the center of the side of the laminate that was not heated with a direct flame was measured, and the maximum temperature during heating was used for evaluation. The lower the maximum temperature, the better the flame resistance.
[0098] Evaluation of laminate strength The bending stiffness (D) was calculated as an index showing the strength of the laminate and evaluated. The bending stiffness (D) was calculated using the following formula. D = ((E1 × t1) × (E2 × t2) × (T + tc) 2 ) / 4λ(E1×t1+E2×t2) Here, E is the bending modulus of elasticity of the outer layer (B) [kN / mm 2 ] (upper layer E1, lower layer E2), t is the thickness [mm] of the outer layer (B) (upper layer t1, lower layer t2), tc is the thickness [mm] of the core layer (A), and T is the thickness [mm] of the laminate. λ is 1-(Poisson's ratio) 2 where 0.99 is used as the coefficient for anisotropic materials. The average value for steel plate is 4.5kN mm 2 Anything above that was rated as an A, and anything below that was rated as a B.
[0099] [Table 1]
[0100] As shown in Table 1, the laminates of Examples 1 to 7, each having a foam core layer (A), a fiber-reinforced plastic outer layer (B), and a metal layer (C), are all lightweight and thin, yet excellent in flame resistance and strength. In particular, the maximum temperature during heating in the flame resistance evaluation was 240°C, so that in the molded articles, particularly battery cases, using the laminates of Examples 1 to 7, the temperature of the battery case can be prevented from becoming excessively high even when the battery generates abnormal heat, ensuring safety.
[0101] On the other hand, the laminate of Comparative Example 1, which has a core layer (A) made of a foam and an outer layer (B) made of a fiber-reinforced plastic but does not have a metal layer (C), is inferior in flame resistance to the laminates of Examples 1 to 7. In particular, since the maximum temperature during heating in the flame resistance evaluation was 320°C, the battery case using the laminate of Comparative Example 1 cannot prevent the temperature of the battery case from becoming excessively high when the battery generates excessive heat.
Claims
1. The foamed foam has a core layer (A) made of a foam, an outer layer (B) made of a fiber-reinforced plastic, and a metal layer (C), and the metal layer (C) is located between the core layer (A) and the outer layer (B); The foam is a polyethylene resin bead foam having a flame retardant coating applied to its surface, The core layer (A) is formed by compressing the foam in the thickness direction, the compression rate of the core layer (A) is 40% or more in terms of thickness, and the aspect ratio of the foam cells of the core layer (A), which is represented by the following formula, is 2 or more. Aspect ratio = 1 / [1 - compression ratio (%) / 100]
2. 2. The laminate according to claim 1, wherein the outer layer (B) is obtained by hot molding a prepreg containing reinforcing fibers (f) and a matrix resin (r), and the matrix resin is a resin composition (1) containing a polyisocyanate compound (r1) and a polyhydroxy(meth)acrylate compound (r2), or a resin composition (2) containing a polyisocyanate compound (r1), a monohydroxy(meth)acrylate compound (r3), and a polyhydroxy compound (r4).
3. 2. The laminate according to claim 1, wherein the metal layer (C) is aluminum.
4. 3. The method for producing a laminate according to claim 1 or 2, comprising the step of hot-molding a precursor obtained by laminating a core layer (A) made of a foam, an outer layer (b) made of a prepreg containing reinforcing fibers (f) and a matrix resin (r), and a metal layer (C).
5. The method for producing a laminate according to claim 1 or 2, wherein the core layer (A), the outer layer (B) made of fiber-reinforced plastic, and the metal layer (C) are bonded together using an adhesive.
6. A battery case using the laminate according to claim 1 or 2.
Citation Information
Patent Citations
Method for producing flame-retardant styrene-based resin foam molded product
JP1993339416A
Laminated panel and panel for housing
JP2012240302A
Carbon fiber composite material and method for producing the same
JP2016002723A
Lightweight board, manufacturing method thereof, and structural material
JP2022080629A
Polypropylene resin foamed sheet, method for producing polypropylene resin foamed sheet, and adhesive sheet
WO2016088438A1