Ferroelectric film manufacturing method, ferroelectric film, and uses thereof

The method of sputtering ferroelectric films at low temperatures below 300°C forms films with a fluorite-type structure, addressing the high-temperature limitations of conventional methods and enabling the use of organic substrates, thus enhancing productivity and cost-effectiveness.

JP7582672B2Active Publication Date: 2024-11-13INSTITUTE OF SCIENCE TOKYO
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021516331
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-27
Publication Date
2024-11-13
Estimated Expiration
2040-04-27

AI Technical Summary

Technical Problem

Conventional methods for forming ferroelectric films require high temperatures of 300°C or higher, limiting the use of substrates to those with heat resistance and excluding organic materials, and existing low-temperature methods like hydrothermal synthesis are impractical due to being wet processes.

Method used

A method involving sputtering at substrate temperatures below 300°C, followed by a low-temperature thermal history or application of an electric field, to form a ferroelectric film with a crystalline metal oxide having a fluorite-type structure in a rectangular phase, allowing use on substrates with lower heat resistance, including organic materials.

Benefits of technology

Enables the production of ferroelectric films at lower temperatures, improving productivity and cost-effectiveness, and allowing the use of organic substrates, while maintaining ferroelectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582672000001
    Figure 0007582672000001
  • Figure 0007582672000002
    Figure 0007582672000002
  • Figure 0007582672000003
    Figure 0007582672000003
Patent Text Reader

Abstract

Provided are a method for forming a ferroelectric film of a metal oxide having a fluorite structure at a temperature lower than 300˚C and a ferroelectric film obtained at a low temperature. The present invention provides a method for producing a ferroelectric film containing a crystalline metal oxide having an orthorhombic phase fluorite structure by sputtering a target by a sputtering method while the temperature of a substrate is less than 300˚C so as to deposit a film of a metal oxide capable of forming an orthorhombic phase fluorite structure on the substrate, and ensuring that the thermal history of the resulting film is less than 300˚C or applying an electric field to the film after the deposition or after the thermal history. In addition, the present invention also provides the above ferroelectric film formed on an organic substrate, glass, or metal substrate intended only for low-temperature use, and a ferroelectric element, ferroelectric functional element, or device using the ferroelectric film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a ferroelectric film, the resulting ferroelectric film, and applications of the ferroelectric film, such as capacitors, electro-optical elements, memory elements, transistors, pyroelectric elements, and piezoelectric elements. [Background technology]

[0002] Known ferroelectric materials include barium titanate BaTiO3, lead zirconate titanate Pb(Zr,Ti)O3, (Pb,La)(Zr,Ti)O3, and BiFeO3. A ferroelectric is a type of dielectric material in which electric dipoles are aligned even in the absence of an external electric field, and the direction of the dipoles can be changed by an electric field. Ferroelectrics are dielectrics that have pyroelectricity and piezoelectricity in addition to ferroelectricity, and are therefore also used as capacitors, electro-optical elements, memory elements, transistors, pyroelectric elements, and piezoelectric elements. A piezoelectric material, which is a ferroelectric, is a material in which polarization proportional to the pressure appears when pressure is applied to the material, and conversely, the material deforms when an electric field is applied. Piezoelectrics are widely used as piezoelectric elements in ignition devices, sonar, speakers, etc.

[0003] Ferroelectric properties have been reported in films using HfO2-based solid solution materials, which are metal oxides with a fluorite structure of an orthorhombic phase (Non-Patent Documents 1, 2, etc.). Conventional ferroelectric materials are complex oxides with a perovskite-based structure, which have a large number of constituent elements (four or more), large fluctuations in composition and crystal structure, as well as problems such as the inclusion of toxic constituent elements, high vapor pressure, and difficulty in controlling the composition due to volatilization. On the other hand, ZrO2, HfO2-based solid solution materials have a fluorite structure and are simple oxides, which have a small number of constituent elements, small fluctuations in composition and crystal structure, excellent reproducibility, no need to use toxic constituent elements, and the possibility of forming films. Therefore, it is considered that the use of ferroelectric films made of fluorite-structure materials is high.

[0004] Known methods for forming inorganic ferroelectric films include sputtering, sol-gel, CVD (Chemical Vapor Deposition), PLD (Pulsed Laser Deposition), ALD (Atomic Layer Deposition), and hydrothermal synthesis (see, for example, Patent Document 1 and Patent Document 2). Among these known methods, except for hydrothermal synthesis, inorganic ferroelectric films cannot be obtained unless they are deposited at a high temperature of 300° C. or higher or annealed at a high temperature of 300° C. or higher after deposition. Therefore, in addition to problems of productivity and cost, there is a drawback in that the usable substrate must be heat-resistant, and organic substrates cannot be used. On the other hand, hydrothermal synthesis can obtain inorganic ferroelectrics at a temperature of 300° C. or lower, but has problems such as being unable to be used for some purposes due to being a wet process. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Re-tabled publication No. 2016-031986 [Patent Document 2] JP 2012-106902 A [Non-patent literature]

[0006] [Non-Patent Document 1] U. Schroeder et al, SCS, J. Solid State Sci.Technol.2013, Volume 1, Issue 2, Pages N69-N71 [Non-Patent Document 2] U. Schroeder et al, Japanese Journal of Applied Physics 53, 08LE01 (2014) Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, an object of the present invention is to provide a method for forming a ferroelectric film of a metal oxide having an orthorhombic fluorite structure at a low temperature of less than 300° C., the obtained ferroelectric film, and a functional element or device using the ferroelectric film. [Means for solving the problem]

[0008] In order to achieve the above object, the present invention provides at least the following aspects. (Aspect 1) A method for producing a ferroelectric film, comprising the steps of: setting a substrate temperature at less than 300°C; sputtering a target to deposit a metal oxide film capable of having an orthorhombic fluorite structure on the substrate; and subjecting the film to a subsequent thermal history of less than 300°C; or applying an electric field to the film after the deposition or thermal history, thereby producing a ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure. (Aspect 2) The method for producing a ferroelectric film according to aspect 1, wherein the metal of the metal oxide includes hafnium (Hf), zirconium (Zr), cerium (Ce), or two or more of these, or includes hafnium (Hf), zirconium (Zr), cerium (Ce), or two or more of these, and at least one metal element selected from aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). (Aspect 3) 3. The method for producing a ferroelectric film according to aspect 1 or 2, wherein the sputtering is carried out in an inert atmosphere having an oxygen partial pressure of less than 1%. (Aspect 4) The method for producing a ferroelectric film according to any one of aspects 1 to 3, wherein the substrate is any one of a substrate containing glass having a glass transition point of less than 300° C., a substrate containing a polymer organic layer, a substrate containing a metal layer having a softening temperature of less than 300° C., and the inside of a semiconductor device. (Aspect 5) A ferroelectric film obtained by the manufacturing method according to any one of aspects 1 to 4. (Aspect 6) A ferroelectric film comprising a crystalline metal oxide having an orthorhombic fluorite structure, provided on any one of a substrate comprising glass having a glass transition point of 300°C or less, a substrate comprising a polymer organic layer, and a substrate comprising a metal layer having a softening temperature of less than 300°C. (Aspect 7) The ferroelectric film according to aspect 5 or 6, wherein the metal of the metal oxide includes hafnium (Hf), zirconium (Zr), cerium (Ce), or two or more of these, or includes hafnium (Hf), zirconium (Zr), cerium (Ce), or two or more of these, and at least one metal element selected from aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). (Aspect 8) The ferroelectric film according to any one of aspects 5 to 7, further comprising a conductive film between the substrate and the ferroelectric film. (Aspect 9) A ferroelectric functional device comprising the ferroelectric film according to any one of aspects 5 to 8 and a pair of electrodes. (Aspect 10) 10. The ferroelectric functional element according to aspect 9, wherein the ferroelectric functional element is selected from the group consisting of a capacitor, an electro-optical element, a memory element, a transistor, a ferroelectric data storage, a pyroelectric element, and a piezoelectric element. (Aspect 11) 10. The ferroelectric functional element according to aspect 9, wherein the ferroelectric functional element is selected from the group consisting of an actuator, an inkjet head, a gyro sensor, a vibration power generating element, a surface acoustic wave resonator, a film bulk wave resonator, a piezoelectric mirror, and a piezoelectric sensor. Effect of the Invention

[0009] According to the present invention, there is provided a method for forming a ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure at a low temperature of less than 300° C. In addition, since a heat treatment at 300° C. or higher is not required, it is possible to improve productivity and costs, and also to use organic materials or soda glass having low heat resistance as a substrate, and further, it is possible to provide a novel ferroelectric functional element or device using these ferroelectric films or substrates. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic perspective view showing a unit cell of a fluorite structure. [Diagram 2] FIG. 2 is a schematic diagram of an example of a sputtering apparatus. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of a laminated structure including a ferroelectric film in a ferroelectric functional element. [Figure 4] FIG. 4 shows an example of a membrane capacitor. [Diagram 5] FIG. 5 shows an example of a ferroelectric memory. [Figure 6] FIG. 6 shows an example of the configuration of a field effect transistor including a ferroelectric material. [Figure 7] FIG. 7 shows a schematic diagram of an example of a pyroelectric power generation device. [Figure 8] FIG. 8 shows an example of an optical deflector using a ferroelectric material as an electro-optical element. [Figure 9] FIG. 9 is a cross-sectional view showing an example of a laminated structure of a piezoelectric element. [Figure 10] FIG. 10 shows a cross-sectional view of an example of an inkjet head. [Figure 11] FIG. 11 is a schematic diagram showing an example of a hard disk drive. [Figure 12] FIG. 12 is a schematic diagram illustrating an example of a gyro sensor. [Figure 13] FIG. 13 is a diagram illustrating the principle of vibration power generation. [Figure 14] FIG. 14 is a schematic diagram showing an example of a surface acoustic wave (SAW) resonator. [Figure 15]FIG. 15 is a schematic diagram showing an example of a membrane bulk acoustic resonator (FBAR). [Figure 16-1] FIG. 16-1 is a schematic diagram illustrating an example of a piezoelectric mirror. [Figure 16-2] FIG. 16-2 is a schematic diagram (continuation) showing an example of a piezoelectric mirror. [Figure 17] FIG. 17 is an X-ray diffraction analysis chart of the 7%YO1.5-93%HfO2 films obtained in Examples 1 to 4. [Figure 18] FIG. 18 is a chart showing the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 films obtained in Examples 1 to 4. [Figure 19] FIG. 19 is an X-ray diffraction analysis chart and a chart showing the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film obtained in Example 5. [Figure 20-1] FIG. 20-1 is an X-ray diffraction analysis chart and a chart showing the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film obtained in Example 6. [Figure 20-2] FIG. 20-2 shows the results of polarization measurement by PUND (Positive-up-negative-down) for the 7%YO1.5-93%HfO2 film obtained in Example 6. [Figure 21-1] FIG. 21-1 is an X-ray diffraction analysis chart and a chart showing the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film obtained in Example 7. [Figure 21-2] Figure 21-2(a) shows a bright-field transmission electron microscope image of the 7%YO1.5-93%HfO2 film on ITO / PET obtained in Example 7, Figure 21-2(b) shows a selected-area electron diffraction image of the 7%YO1.5-93%HfO2 film, and Figure 21-2(c) shows a dark-field transmission electron microscope image taken using 222 diffraction of Figure 21-2(b). [Figure 22] FIG. 22 is an X-ray diffraction analysis chart and a chart showing the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film obtained in Example 8. [Figure 23-1] FIG. 23-1 shows the polarization hysteresis measurement results (relationship between polarization and electric field) and X-ray diffraction analysis charts of the 7%YO1.5-93%HfO2 films obtained on some of the substrates (Pt / Si) in Example 9. [Figure 23-2] Figure 23-2 shows the polarization measurement results by PUND (Positive-up-negative-down) for a 7%YO1.5-93%HfO2 film on a Pt / Si substrate. [Figure 24] FIG. 24 shows the polarization hysteresis measurement results (relationship between polarization and electric field) and X-ray diffraction analysis charts of the 7%YO1.5-93%HfO2 films obtained on some of the substrates (ITO / Al2O3 (c-plane), SRO / STO) in Example 9. [Diagram 25] FIG. 25 is an X-ray diffraction analysis chart of the 7%YO1.5-93%HfO2 film obtained in Example 10. [Figure 26] FIG. 26 shows the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film (ITO / polyimide substrate) obtained in Example 11. [Figure 27] FIG. 27(a) shows a bright-field image of the 7%YO1.5-93%HfO2 film obtained in Example 12, FIG. 27(b) shows a selected-area electron diffraction image of the 7%YO1.5-93%HfO2 film, and FIG. 27(c) shows selected-area electron diffraction images of the ITO electrode and the YSZ100 substrate. [Figure 28] FIG. 28 shows the polarization hysteresis curve (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film having a thickness of 20 nm obtained in Example 14. [Figure 29] FIG. 29 shows an X-ray diffraction analysis chart and polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film having a thickness of 900 nm obtained in Example 15. [Diagram 30]Figure 30 shows X-ray diffraction analysis charts of the 7%YO1.5-93%HfO2 film and 5%YO1.5-95%HfO2 film obtained in Example 16. Figure 30(a) is a 2Theta-Psi map near the 110 superlattice diffraction in a 7%YO1.5-93%HfO2 film deposited at room temperature on an ITO / (111)YSZ plate. Figure 30(b) is a 2Theta-Psi map near the 110 superlattice diffraction in a 5%YO1.5-95%HfO2 film deposited at room temperature on an ITO / (111)YSZ substrate. [Diagram 31] Fig. 31 shows the polarization hysteresis measurement results (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film and the 5%YO1.5-95%HfO2 film obtained in Example 16. Fig. 31(a) shows the result of the polarization hysteresis measurement (relationship between polarization and electric field) of the 7%YO1.5-93%HfO2 film. Fig. 31(b) shows the result of the polarization hysteresis measurement (relationship between polarization and electric field) of the 5%YO1.5-95%HfO2 film. Fig. 31(c) and (d) show the applied voltage dependence of the residual polarization value Pr and the coercive field Ec of the 7%YO1.5-93%HfO2 film and the 5%YO1.5-95%HfO2 film. [Diagram 32] FIG. 32 shows the results of polarization hysteresis measurements (relationship between polarization and electric field) for the 7%YO1.5-93%HfO2 film obtained in Example 17 before and after annealing. [Diagram 33] 33(a) and (b) show the polarization hysteresis measurement results (relationship between polarization and electric field) of the 5%YO1.5-95%Hf0.75Zr0.25O2 film obtained in Example 18. [Diagram 34]FIG. 34(a) shows the polarization hysteresis measurement results of the 5%YO1.5-95%Hf0.75Zr0.25O2 film on the ITO / YSZ111 substrate obtained in Example 19, and FIG. 34(b) shows the polarization hysteresis measurement results (relationship between polarization and electric field) of the 5%YO1.5-95%Hf0.75Zr0.25O2 film on the ITO / YSZ100 substrate obtained in Example 19. FIG. 34(c) shows the polarization hysteresis measurement results (relationship between polarization and electric field) of the 5%YO1.5-95%Hf0.50Zr0.50O2 film on the ITO / YSZ111 substrate obtained in Example 20, and FIG. 34(d) shows the polarization hysteresis measurement results (relationship between polarization and electric field) of the 5%YO1.5-95%Hf0.75Zr0.25O2 film on the ITO / YSZ100 substrate obtained in Example 20. [Diagram 35] FIG. 35 shows the polarization hysteresis measurement results (relationship between polarization and electric field) of a 5%YO1.5-95%Hf0.50Zr0.50O2 film on a Pt / Si substrate obtained in Example 21 using different Pt deposition temperatures instead of ITO / YSZ. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (Method of manufacturing ferroelectric film) In a first aspect, the present invention provides a method for producing a ferroelectric film, characterized in that a film sputtering method is used to deposit a metal oxide film capable of having an orthorhombic fluorite structure on a substrate by setting a substrate temperature at less than 300°C and sputtering a target, and the film is subsequently subjected to a thermal history of less than 300°C, or an electric field is applied to the film after the deposition or after the thermal history, thereby producing a ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure.

[0012] Conventionally, when a ferroelectric film containing a metal oxide having an orthorhombic fluorite structure is formed by PLD or the like, the ferroelectric film is obtained by depositing the film at a high temperature of 300°C or more, or by depositing a metal oxide film and then annealing it at a high temperature of 300°C or more. A monoclinic phase is obtained by deposition at room temperature or less than 300°C. However, the present inventors have unexpectedly found that if a target having a raw material composition capable of forming an orthorhombic fluorite structure is used and the film is deposited by sputtering at a substrate temperature of less than 300°C, a ferroelectric film containing a metal oxide having a crystal with an orthorhombic fluorite structure can be formed without annealing at a high temperature of 300°C or more thereafter, or by applying an electric field to the film after deposition or thermal history, and in addition, such a ferroelectric film can be formed even on a substrate with a heat-resistant temperature of less than 300°C.

[0013] (Ferroelectric film) In the method for producing a ferroelectric film of the present invention, the ferroelectric film to be formed is a ferroelectric film containing a metal oxide of crystals having a fluorite structure of an orthorhombic (orthorhombic) phase.

[0014] The fluorite structure and the orthorhombic (orthorhombic) phase are widely known in crystallography. Figure 1 shows a unit cell of the fluorite structure. The crystals of the fluorite structure can have four crystal structures: cubic, tetragonal, orthorhombic, and monoclinic. The cubic, tetragonal, and orthorhombic crystals have right-angled quadrangular lattices with their crystal axes intersecting perpendicularly, but the cubic crystal has three axes of the same length, the tetragonal crystal has two axes of the same length and one axis of a different length, and the orthorhombic crystal has three axes of different lengths. In contrast, the monoclinic crystal has two crystal axes that do not intersect perpendicularly and the three axes of the same length. The ferroelectric film of the present invention has a fluorite structure of the orthorhombic phase. A ferroelectric film cannot be obtained unless the fluorite structure of the orthorhombic phase is used. There has been no report of forming a ferroelectric film of a metal oxide of the fluorite structure of the orthorhombic phase on a substrate at a temperature of less than 300°C without post-annealing. In addition, the orthorhombic phase and the orthorhombic phase are simply expressed differently, but are crystallographically the same crystal phase.

[0015] The fact that the ferroelectric film of the present invention has an orthorhombic fluorite structure may be confirmed by X-ray diffraction (the presence of superlattice reflection in wide-area reciprocal lattice mapping measurement). However, although the ferroelectric film of the present invention can be easily confirmed to have an orthorhombic and / or tetragonal phase by X-ray diffraction analysis, depending on the type of metal oxide, the difference in the axis length of the orthorhombic and / or tetragonal phase is so small that it may be impossible to distinguish between the orthorhombic and tetragonal phases depending on the type of X-ray diffraction device and the measurement accuracy. In such cases, the presence of the orthorhombic phase may be confirmed by examining the polarization hysteresis characteristics to see whether or not the film exhibits ferroelectricity. When the polarization hysteresis characteristic is confirmed as a result of the polarization hysteresis measurement, since an electric field is applied in the polarization hysteresis measurement, there are two cases: the film before the measurement is already in an orthorhombic phase, and the film before the measurement is in a tetragonal phase, but the application of an electric field for the measurement causes an electric field-induced phase transition to the orthorhombic phase. In either case, in the present invention, it is sufficient that the film exhibits ferroelectricity and is in an orthorhombic phase. Furthermore, even if the film after the film formation can be confirmed to be tetragonal, the ferroelectric film of the present invention may be one in which a phase change is induced to the orthorhombic phase by the application of an electric field, and the film exhibits ferroelectricity. The film exhibiting ferroelectricity is an orthorhombic phase, and is included in the ferroelectric film of the present invention.

[0016] When it is impossible to distinguish between the orthorhombic and tetragonal phases due to the type of X-ray diffraction device and the measurement accuracy, the crystal phase may be analyzed by an X-ray diffraction method with higher analytical accuracy (e.g., SPring 8, etc.). In addition, the applied electric field may be gradually increased and then gradually decreased while examining the polarization characteristics (hysteresis characteristics) and examining the changes in the polarization characteristics (hysteresis characteristics, especially the residual polarization value and the coercive field value) during the period, which may confirm that the film is in the orthorhombic phase after film formation and before the measurement of the hysteresis characteristics. The change in the polarization characteristic value that appears may be different between the case where the film is in the orthorhombic phase before the application of the electric field (especially an oriented film) and the case where a phase change is induced by the application of the electric field. In the former case (especially an oriented film), the applied electric field may be low to obtain the residual polarization value, whereas in the latter case, the applied electric field may be high to obtain the residual polarization value (electric induction from the tetragonal to the orthorhombic phase is necessary). For a film that is in the orthorhombic phase before the application of an electric field (hysteresis characteristic measurement), the applied electric field that shows the same remnant polarization value and coercive field value is the same or does not change much when the applied electric field is increased and decreased, but for a film that is in the tetragonal phase before the application of an electric field (hysteresis characteristic measurement), the applied electric field that shows the same remnant polarization value and coercive field value is higher when the applied electric field is increased and lower when the applied electric field is decreased, and a significant difference may be observed between them (see Example, Figure 32). However, for a film that is in the orthorhombic phase before the application of an electric field (hysteresis characteristic measurement) but has low orientation, an applied electric field is required to orient (polarize) it, and it may not show polarization hysteresis characteristics at a low applied electric field, so even if this measurement method cannot confirm that it is in the orthorhombic phase, there is a possibility that the film after film formation is in the orthorhombic phase.

[0017] Furthermore, the film of the present invention has a fluorite structure of an orthorhombic phase and exhibits ferroelectricity, and the ferroelectricity can be confirmed by polarization hysteresis measurement (relationship between polarization and electric field). The method of polarization hysteresis measurement (relationship between polarization and electric field) is well known. Films that exhibit ferroelectricity always exhibit piezoelectricity, and the piezoelectricity can also be confirmed by applying a voltage to a test piece and observing the expansion and contraction.

[0018] The film of the present invention is a ferroelectric film containing a crystal having a fluorite structure of an orthorhombic (orthorhombic) phase and a metal oxide exhibiting ferroelectricity. Such a metal oxide is preferably a metal oxide containing one of hafnium (Hf) oxide, zirconium (Zr) oxide, and cerium (Ce) oxide, or a solid solution of metal oxides containing two or more of them, or a metal oxide containing one or more of hafnium (Hf), zirconium (Zr), and cerium (Ce) and an additive or substitution element such as aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc.). Metal oxides containing one or more of hafnium (Hf), zirconium (Zr) and cerium (Ce), or metal oxides containing the above-mentioned additive or substitution elements, are known as metal oxides that can have a fluorite structure and exhibit an orthorhombic (orthorhombic) phase and ferroelectricity. Metal oxides containing these three metals, particularly Hf and Zr, are known to be capable of forming a complete solid solution with each other and have a high similarity in crystal structure. (References: See, for example, J. Amer. Ceram Soc., 37(10) 458 (1954).)

[0019] Metal oxides containing one or more of these elements Hf, Zr, and Ce are similar to each other and can form solid solutions with each other. However, it is also known that the inclusion of oxygen vacancies allows them to have an orthorhombic fluorite structure and to exhibit ferroelectricity.

[0020] In addition, it is preferable to use a metal oxide containing one or more metals selected from Hf, Zr, and Ce, and which is added or substituted with an element. Examples of elements that can be used as a substitute or added element (hereinafter also simply referred to as a substitute element) include elements that are solid-soluble in the above-mentioned metal oxides, such as aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc.).

[0021] The amount of these substitution elements depends on the type of metal oxide and substitution element, but may be an amount that forms a fluorite structure of an orthorhombic phase, and generally, the molar number of the substitution element (metal element) is preferably 0.1 to 10% or less than 15 mol%, and may be 4 to 9 mol%, based on the total of the metals in the entire metal oxide substituted with elements being 100 mol%. If the amount of element substitution is less than the above, the fluorite structure with a monoclinic phase may be stabilized. If the amount of element substitution is more than the above, the fluorite structure with a tetragonal phase or cubic phase may be stabilized.

[0022] The metal oxides to be substituted with elements in the above may be simple oxides such as hafnium oxide, zirconium oxide, and cerium oxide, or may be solid solutions between these metal oxides that have a fluorite structure. In the case of a solid solution between metal oxides, the ferroelectric film having a fluorite structure of the orthorhombic phase of the present invention can be obtained by elementally substituting aluminum, silicon, rare earth elements, etc. for the solid solution of the metal oxide. The amount of element substitution is preferably 0.1 to 10% or less by 10 mol%, more preferably 4 to 9 mol%, based on the total amount of metals in the entire solid solution of the metal oxides substituted with elements as above being 100 mol%.

[0023] In one preferred embodiment, the metal oxide contains at least one of hafnium (Hf) and zirconium (Zr), and further contains a substitution element such as aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), or a rare earth element. Hafnium (Hf) oxide and zirconium (Zr) oxide can be completely solid-soluble with each other, but in the case of zirconium (Zr) oxide alone, the molar number of the substitution element (metal element) is 0.5 to 5 mol%, more preferably 1 to 3 mol% or 1 to 2 mol%, based on the total of the metals in the entire element-substituted metal oxide being 100 mol%. In the case of hafnium (Hf) oxide alone, the molar number of the substitution element (metal element) is 3 to 12 mol%, more preferably 4 to 9% or 4 to 8 mol%, based on the total of the metals in the entire element-substituted metal oxide being 100 mol%. In the case of a solid solution of hafnium (Hf) oxide and zirconium (Zr) oxide, the substitution amount (range) is preferably weighted and added according to the solid solution ratio of Hf and Zr based on the above amount (range) of the substitution element in the case of hafnium (Hf) oxide alone and zirconium (Zr) oxide alone. Within these ranges, a ferroelectric film having a fluorite structure of an orthorhombic phase can be more easily manufactured by a sputtering method. If the molar ratio of Zr to Hf is r=Zr / (Zr+Hf), the number of moles is preferably within the range of [0.5+(3-0.5)r] to [5+(12-5)r], further preferably within the range of [1+(4-1)r] to [3+(9-3)r], or further preferably within the range of [1+(4-1)r] to [2+(8-2)r], assuming that the total of Zr and Hf is 100 mol %.

[0024] The ferroelectric film of the present invention must have an orthorhombic fluorite structure and exhibit ferroelectricity. Although ferroelectricity is considered to be a result of having an orthorhombic fluorite structure, the ferroelectric film of the present invention not only has an orthorhombic fluorite structure but also exhibits ferroelectricity.

[0025] The ferroelectric film formed by the manufacturing method of the present invention is a crystal having a fluorite structure of an orthorhombic phase that exhibits ferroelectricity, but it may be a polycrystal, a uniaxially oriented crystal, or even an epitaxial crystal. When a crystal film is grown on a crystal substrate, a uniaxially oriented crystal is one in which one crystal axis of the growing crystal and the crystal substrate are almost aligned, and an epitaxial crystal is one in which two crystal axes of the crystal are almost aligned. It is also possible to form a uniaxially oriented crystal in which each crystal grain is epitaxially grown by "local epitaxial growth", or a single crystal epitaxial crystal in which the epitaxially grown crystal grains have a substantial size. Furthermore, a uniaxially oriented crystal originally refers to the orientation of a crystal in relation to a crystal substrate, but the crystal orientation of a single crystal film separated from a crystal substrate may also be referred to as uniaxial orientation based on the unique crystal orientation of the obtained uniaxially oriented crystal.

[0026] The thickness of the ferroelectric film formed by the manufacturing method of the present invention is not particularly limited because a suitable thickness is adopted depending on the final use of the ferroelectric film, and may be, for example, 1 nm or more, 20 nm or more, or 100 nm or more, but may be preferably 300 nm or more, 500 nm or more, or 1 μm or more, particularly in the case of a piezoelectric body. It may further be 5 nm or more, or 10 nm or more. In addition, the upper limit is not limited, and may be, for example, 10 μm or less, 5 μm or less, 3 μm or less, or 1 μm or less. In one preferred embodiment, the thickness of the ferroelectric film is 5 nm to 1000 nm, more preferably 10 nm to 500 nm. In another preferred embodiment, the thickness of the ferroelectric film is 500 nm to 5 μm, more preferably 1 μm to 3 μm.

[0027] (Sputtering method) The present invention is characterized by using a sputtering method. In other deposition methods (deposition methods) such as a sol-gel method, a CVD (Chemical Vapor Deposition) method, a PLD (Pulsed Laser Deposition) method, and an ALD (Atomic Layer Deposition) method, except for hydrothermal methods, even if a metal oxide film having a fluorite structure is deposited, unless the substrate temperature is 300° C. or higher or the film is annealed at a temperature of 300° C. or higher after deposition, an orthorhombic phase or even a tetragonal fluorite structure cannot be obtained, resulting in a film that does not exhibit ferroelectricity. The present inventors have found, contrary to conventional knowledge and completely unexpectedly, that by using a sputtering method, a metal oxide film having an orthorhombic fluorite structure and exhibiting ferroelectricity can be formed even if the substrate temperature is less than 300° C., without the need for high-temperature annealing after deposition. According to the manufacturing method of the present invention, even if deposition is performed at a substrate temperature of less than 300°C and the subsequent thermal history is less than 300°C, it is possible to manufacture a ferroelectric film containing a metal oxide having a crystal with a fluorite-type structure in an orthorhombic phase by applying an electric field as the case may be, which is a novel technology not seen in the past.

[0028] The sputtering method is a deposition method in which a material such as a metal oxide or metal that is the raw material of the metal oxide to be deposited as a film is placed as a target in a vacuum chamber, and particles such as ions or electrons, for example, a gas ionized by applying a high voltage, for example, nitrogen gas or a rare gas (typically argon), are collided with the target to flick off the film raw material on the target surface with high energy, and the raw material that is flicked off with high energy reaches a substrate to form a film. Vapor phase deposition methods include a vapor deposition method in which the film raw material is heated and evaporated, and a pulsed laser deposition method (PLD) in which the film raw material is evaporated by irradiating a pulsed laser beam on the film raw material, and the like, which mainly utilizes heat to vaporize the raw material. However, for a film having a composition in which the monoclinic phase is stable at low temperatures, the effect of the present invention (a ferroelectric film containing a crystal of a metal oxide having an orthorhombic phase or a tetragonal fluorite structure at low temperatures) cannot be obtained unless the sputtering method is used, in which accelerated particles having high energy are collided with a target. In the deposition method and the PLD method, the raw material is vaporized using heat rather than bombarding a target with particles, and therefore the energy during deposition is low, which is thought to prevent the deposition of the ferroelectric film targeted by the present invention.

[0029] FIG. 2 shows a typical example of a sputtering apparatus 10. The sputtering apparatus 10 includes a vacuum chamber 1, a substrate 2 and a target 3 disposed in the vacuum chamber 1, a power supply 4 for applying a voltage between the substrate 2 and the target 3, an introduction system 5 for an atmospheric gas of the vacuum chamber 1, a heater (not shown) for heating the substrate 3, and a thermometer (not shown) for measuring the temperature of the substrate 2. The sputtering apparatus 10 may be configured as a magnetron sputtering apparatus by optionally providing a magnetron generator for the target 3. Usually, a high DC or AC voltage is applied between the substrate 2 and the target 3 to ionize the inert gas in the vacuum chamber 1, and the substrate 2 is biased to a potential higher than that of the target 3, so that the inert gas ions collide with the target and scatter the raw material on the target surface, and the scatter-scattered raw material reaches the substrate, so that the target material is deposited on the substrate surface in a state of higher energy than that of the thermal deposition method. The sputtering method of the present invention includes a reactive sputtering method in which a film is formed from a reaction product generated by a chemical reaction between a raw material sputtered from a target and a gas. Even in the reactive sputtering method, the raw material sputtered from the target with high energy is deposited on the substrate with high energy even if it chemically reacts with the gas in the atmosphere, so that it is possible to obtain a ferroelectric film containing a metal oxide of a crystal having an orthorhombic phase or a tetragonal fluorite structure that is not a stable phase at low temperatures. In the case of a sputtering method in the narrow sense that does not involve a chemical reaction (non-reactive sputtering method), an inert atmosphere is used and the atmosphere does not contain a gas reactive with the raw material, but it is permissible to include a small amount of oxygen gas in the atmospheric gas to stabilize the composition of the metal oxide to be formed.

[0030] The sputtering conditions used in the method for producing a ferroelectric film of the present invention may be any of the above-mentioned sputtering methods. The sputtering method used in the present invention may be any method for sputtering a target using particles such as ions or electrons, rather than heat, and includes a normal sputtering method in which an electric field is applied to generate plasma, as well as an ion beam sputtering method and an electron beam sputtering method. The sputtering method may be any of DC sputtering, AC sputtering, high frequency sputtering, magnetron sputtering, AC magnetron sputtering, ion beam sputtering, and ECR sputtering. One preferred embodiment of the sputtering method is DC sputtering or AC magnetron sputtering.

[0031] (target) The film formed in the present invention contains a metal oxide having an orthorhombic fluorite structure and exhibiting ferroelectricity, as described above. The target used in the present invention is a metal oxide and / or metal capable of forming such a metal oxide (having an orthorhombic fluorite structure and exhibiting ferroelectricity). In the non-reactive sputtering method, the target is preferably a metal oxide itself having the same composition as the metal oxide as described above, but may be a combination of a plurality of metal oxides whose average composition is the same as the metal oxide as described above. In the case of the reactive sputtering method, a metal can be used as the target, but in the non-reactive sputtering method, a metal may also be used as part of the target. The metal oxide formed by the sputtering method basically has the same composition as the target, but it is acceptable for the composition of the film sputtered, scattered from the target, and deposited on the substrate to change slightly from the composition (average composition) of the metal oxide of the target. In the sputtering method of the present invention, the change in the composition of the target substance between the target and the obtained film is usually slight and negligible. The molar amount of each metal element and oxygen is considered to be 2 to 3% or less, usually 1% or less, 0.5% or less, or even 0.02% or less.

[0032] In the method for producing a ferroelectric film of the present invention, the metal oxide constituting the target can preferably be, for example, hafnium oxide, zirconium oxide, cerium oxide, and metal oxides such as solid solutions thereof, or materials obtained by elementally substituting these metal oxides. Examples of elements that can be used as the substituting element include elements that are solid-soluble in the above-mentioned metal oxides, such as aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). In non-reactive sputtering, the target is preferably a metal oxide itself having such a composition, but may also be a composite of a plurality of metal oxides whose average composition coincides with the composition of the above-mentioned metal oxide. In particular, the substituting element may be a metal oxide that is integral with another metal oxide or is a single metal oxide, or may be a metal.

[0033] (Sputtering conditions) In the method for producing a ferroelectric film of the present invention, the substrate temperature during sputtering is less than 300°C. The substrate may be at room temperature without heating, but if it is heated to less than 300°C, the advantage of lower temperatures can be obtained compared to the conventional method of forming or annealing at a temperature of 300°C or more. One preferred embodiment is room temperature (e.g., 25°C). Another preferred embodiment is heating to a temperature less than 300°C, for example, heating to a temperature of 50°C or more, 100°C or more, less than 300°C, 250°C or less, or 150°C or less. A lower temperature is preferable to avoid adverse effects due to heat treatment, but it may be desirable to raise the temperature to a certain degree in order to improve the crystallinity of the film to be formed.

[0034] In the method for producing a ferroelectric film of the present invention, in the non-reactive sputtering, the atmosphere in the vacuum chamber is an inert atmosphere that does not react with the target material (raw material) that is ejected from the target, for example, a rare gas such as argon, xenon, krypton, helium, or nitrogen, and preferably a rare gas, particularly argon. Since the target and the film are metal oxides, a small amount of oxygen may be contained in order to stabilize the composition of the metal oxide. The content of oxygen gas contained in the inert atmosphere may be 10% or less, 5% or less, 1% or less, or 0.1% or less in terms of partial pressure in the atmosphere. However, in one embodiment of the present invention, it is most preferable that the atmosphere is composed of only an inert gas atmosphere and does not contain oxygen gas. In the non-reactive sputtering, even if oxygen gas is contained in the atmosphere, the partial pressure of oxygen gas in the inert gas is preferably less than 1%, 0.05% or less, or 0.01% or less.

[0035] In reactive sputtering, the atmosphere in the vacuum chamber is an oxygen-containing atmosphere. In addition to oxygen, the atmosphere may contain the above-mentioned inert gases, for example, rare gases such as argon, xenon, krypton, and helium, and nitrogen, preferably rare gases, especially argon. The ratio of the inert gas to oxygen is not limited, but may be 100:0 to 100:1, further 100:0 to 100:0.5, 100:0 to 100:0.1, or 100:0 to 100:0.01 in molar ratio.

[0036] In the method for producing a ferroelectric film of the present invention, the atmospheric pressure in the vacuum chamber is reduced to, for example, 10 to 200 mTorr.

[0037] In the method for producing a ferroelectric film of the present invention, the electric field applied between the substrate and the target may be, for example, DC or RF, etc. The electric field for ionizing an atmospheric gas such as argon may be direct current or high frequency, etc.

[0038] In the method for producing a ferroelectric film of the present invention, the power of sputtering is, for example, 0.06 to 2.47 W / cm based on the area of ​​the target. 2 , and 0.12 to 1.85 W / cm2 , 0.12~1.23W / cm 2 , 0.12~0.617W / cm 2 The higher the sputtering power, the more efficient the film formation (the greater the film thickness per unit time), but the crystallinity of the resulting film may decrease.

[0039] In the method for producing a ferroelectric film of the present invention, the sputtering time is not necessarily set because it depends on the film formation speed and the desired film thickness, but may be, for example, 1 minute to 300 minutes.

[0040] (Thermal history after deposition) In the manufacturing method of the present invention, a ferroelectric film is obtained by sputtering at a substrate temperature of less than 300° C., so the thermal history after film formation may also be less than 300° C. By having a thermal history of less than 300° C. during and after film formation, the ferroelectric film of the metal oxide of the present invention can be formed on the substrate without damaging the substrate, which has a heat resistance of less than 300° C. In one preferred embodiment, annealing is not required after sputtering, but in another preferred embodiment, annealing may be performed after sputtering at a temperature less than 300° C., for example, at a temperature of 50° C. or more, 100° C. or more, or at a temperature less than 300° C., 250° C. or less, or 150° C. or less.

[0041] (Electric field applied after deposition) In one embodiment of the manufacturing method of the present invention, a ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure may be obtained by forming a metal oxide film capable of having an orthorhombic fluorite structure by sputtering at a substrate temperature of less than 300° C., and applying an electric field after the film formation or thermal history at a thermal history of less than 300° C. In this embodiment, the film after deposition is tetragonal, and a phase change from the tetragonal to the orthorhombic phase is induced by the application of an electric field.

[0042] Unless the sputtering method is used, it is impossible to form a film of a metal oxide with a fluorite structure in which a phase change from the tetragonal phase to the orthorhombic phase (which is not a stable phase at low temperatures) can be induced by the application of an electric field during low-temperature film formation at less than 300°C and low-temperature thermal history.

[0043] The applied electric field depends on the crystal structure, crystal state, and film thickness of the film, and is not necessarily limited, but is generally 1 MV / cm or more, 3 MV / cm or more, 4 MV / cm or more, and preferably 5 MV / cm or more. It may also be 3 MV / cm or less. The applied electric field is preferably an alternating current, with a frequency of 1 to 100 kHz and an application time (number of cycles) of 1 cycle or more.

[0044] The application of the electric field may be carried out at room temperature, but also at elevated temperatures below 300° C., particularly temperatures not higher than either the deposition temperature or the post-deposition annealing temperature.

[0045] The mode and conditions of application of this electric field may be similar to the mode and conditions used in hysteresis analysis or polarization treatment of a ferroelectric film, or may be higher energy conditions than the conditions used in hysteresis analysis or polarization treatment, or may be lower energy conditions than the conditions used in hysteresis analysis or polarization treatment, depending on the film.

[0046] Furthermore, when the ferroelectric film produced in the present invention is used as a ferroelectric element or a ferroelectric functional element, it is preferable to carry out a polarization treatment.

[0047] In one embodiment, the poling process may be an electric field application process that induces a phase change from a tetragonal to an orthorhombic phase.

[0048] (Base) In the method for producing a ferroelectric film of the present invention, the substrate on which the ferroelectric film is deposited is not particularly limited, and any substrate that has been used as a substrate for forming a ferroelectric film similar to the ferroelectric film of the present invention can be used. For example, a substrate made of ceramic, semiconductor, metal, or organic material can be used. The ceramic may be conductive or insulating.

[0049] In the manufacturing method of the present invention, a crystalline substrate having a small crystal lattice mismatch with the ferroelectric film to be formed is preferably used as the substrate in order to enhance the crystallinity of the ferroelectric film to be formed. Preferred crystalline substrates include, for example, crystalline substrates having a cubic fluorite structure, a bixbyite structure, a pyrochlore structure, a diamond structure, a zinc blende structure, and a perovskite structure.

[0050] Examples of crystalline substrates with a cubic fluorite structure include yttria-stabilized zirconia (lattice constant a=about 5.15 Å), cerium oxide (lattice constant a=about 5.41 Å), and calcium fluoride (lattice constant a=about 5.466 Å).

[0051] Examples of crystal substrates with a bixbyite structure include indium oxide (lattice constant a = about 10.125 Å), indium tin oxide (lattice constant a = about 10.125 Å), scandium oxide (lattice constant a = about 9.845 Å), yttrium oxide (lattice constant a = about 10.604 Å), erbium oxide (lattice constant a = about 10.545 Å), thulium oxide (lattice constant a = about 10.49 Å), ytterbium oxide (lattice constant a = about 10.434 Å), and lutetium oxide (lattice constant a = about 10.363 Å). The lattice constants of the ferroelectric material with an orthorhombic fluorite structure and the crystal substrate may be in a multiple relationship.

[0052] Examples of crystalline substrates with the pyrochlore structure include Bi2Ru2O7 (lattice constant a = approximately 10.293 Å), rare earth ruthenium oxide R2Ru2O7 (R is a rare earth element), Bi2Ir2O7 (lattice constant a = approximately 10.323 Å), and rare earth iridium oxide R2Ir2O7 (R is a rare earth element).

[0053] Some semiconductors can also be used as crystal substrates. In particular, they can be used suitably if the lattice constant is suitable. For example, examples of semiconductors with diamond structure include silicon (lattice constant a = about 5.43 Å) and germanium (lattice constant a = about 5.6575 Å). Examples of compound semiconductors with zinc blende structure include III-V group compound semiconductors such as gallium arsenide (lattice constant a = about 5.6532 Å), aluminum arsenide (lattice constant a = about 5.656 Å), gallium phosphide (lattice constant a = about 5.450 Å), and aluminum phosphide (lattice constant a = about 5.451 Å), as well as II-IV group compound semiconductors such as beta zinc sulfide (lattice constant a = about 5.4109 Å) and zinc selenide (lattice constant a = about 5.451 Å).

[0054] In the ferroelectric film of the present invention, the above-mentioned crystalline substrate can be a film formed on a substrate such as an yttria-stabilized zirconia substrate or a single crystal silicon substrate.

[0055] The above-mentioned crystal substrate may be formed on a semiconductor, particularly a single crystal silicon substrate, and a cubic fluorite or bixbyite type epitaxial crystal film or the like may be further provided as a buffer layer between the crystal substrate and a semiconductor substrate such as a single crystal silicon substrate.

[0056] The crystal substrate on which the ferroelectric epitaxial film of the present invention is formed can be an electrode layer having electrical conductivity. Examples of the crystal substrate on which the ferroelectric film of the present invention can be formed and has electrical conductivity include pyrochlore structures such as Bi2Ru2O7, R2Ru2O7 (R is a rare earth element), Bi2Ir2O7, and rare earth iridium oxide R2Ir2O7 (R is a rare earth element). Indium tin oxide (ITO) is also electrically conductive, and the ferroelectric film of the present invention can be formed thereon. These electrically conductive pyrochlore structures and electrically conductive crystal substrates such as ITO can be formed on substrates such as yttria-stabilized zirconia substrates and single crystal silicon substrates.

[0057] In particular, as a structure for forming the ferroelectric film of the present invention on a semiconductor substrate such as silicon, when the semiconductor is represented by S, the ferroelectric epitaxial film by F, the metal by M, and the insulator by I, structures such as an MFS structure (e.g., M / F / Si), an MFIS structure (e.g., M / F / fluorite structure / Si, M / F / bixbite structure / Si), and an MFM(IS) structure (e.g., M / F / ITO / (fluorite structure or bixbite structure) / Si, M / F / conductive pyrochlore structure / (fluorite structure or bixbite structure) / Si) can be used. Here, the portion described as (fluorite structure or bixbite structure) is a buffer layer and can be omitted. FIG. 3 shows examples of stacked structures including the above-mentioned ferroelectric film in memories, resistive memories, transistors, capacitors, cooling devices, and pyroelectric devices as examples of ferroelectric elements or ferroelectric functional elements using the ferroelectric film. A ferroelectric element generally includes a ferroelectric film and a pair of electrodes, each of which is in direct or indirect contact with both sides of the ferroelectric film and electrically connected to the ferroelectric film.

[0058] Examples of semiconductors include diamond (lattice constant a = approximately 3.567 Å), silicon (lattice constant a = approximately 5.43 Å), and germanium (lattice constant a = approximately 5.6575 Å), which are semiconductors with a diamond structure; beta silicon carbide (lattice constant a = approximately 4.3596 Å), which is a compound semiconductor with a zinc blende structure; III-V compound semiconductors gallium arsenide (lattice constant a = approximately 5.6532 Å), aluminum arsenide (lattice constant a = approximately 5.656 Å), gallium phosphide (lattice constant a = approximately 5.450 Å), and aluminum phosphide (lattice constant a = approximately 5.451 Å); and II-IV compound semiconductors such as beta zinc sulfide (lattice constant a = approximately 5.4109 Å) and zinc selenide (lattice constant a = approximately 5.451 Å).

[0059] In the manufacturing method of the present invention, from the viewpoint of effectively utilizing the advantage that a ferroelectric film can be formed at a low temperature of less than 300°C, a film can be preferably formed on a substrate having a heat-resistant temperature of less than 300°C. Examples of substrates having a heat-resistant temperature of less than 300°C include organic resins, particularly organic resins having a glass transition temperature of less than 300°C, inorganic glass having a glass transition temperature of less than 300°C, such as soda glass, and metals having a softening temperature of less than 300°C, such as aluminum wiring layers, copper foils, and gold foils. If a ferroelectric film is formed on these low heat-resistant substrates by the low-temperature film-forming method of the present invention, it is preferable because the ferroelectric film can be formed on the low heat-resistant substrate without damaging the substrate. In addition, a substrate made of an organic resin having a glass transition temperature of less than 300°C can have flexibility, so that a flexible ferroelectric film can be obtained, and applications to new and unique uses are expected.

[0060] In a preferred embodiment of the present invention, the substrate may be a conductive substrate such as a metal, or may be a semiconductor or an insulator. According to the manufacturing method of the present invention, it is possible to form a ferroelectric film on a substrate made of various materials.

[0061] In a preferred embodiment of the present invention, a conductive film may be provided between the substrate and the ferroelectric film. The conductive film is preferable because it can function as an electrode layer for the ferroelectric film. Examples of such conductive films include ITO (indium tin oxide), metals such as platinum (Pt), Ir, Al, and Ag, and conductive ceramics such as TiN, IrO2, RuO2, SrRuO3, LaNiO3, and LaSrCoO3.

[0062] The thickness of the conductive film is not limited, but may be, for example, preferably 1 nm to 100 nm, more preferably 10 nm to 100 nm. The substrate having the conductive film is not particularly limited, and may be the above-mentioned low heat-resistant substrate of less than 300° C. When the conductive film is present between the substrate and the ferroelectric film, the substrate having the conductive film on its surface may be considered as a substrate (composite substrate) in its entirety in the film-forming method of the present invention.

[0063] In a preferred embodiment of the present invention, a conductive substrate such as a metal, as well as a semiconductor or insulator film may be present between the substrate and the ferroelectric film. The substrate having such a film on its surface can also be considered as a substrate (composite substrate) in its entirety in the film forming method of the present invention.

[0064] (Ferroelectric film-2) In a second aspect of the present invention, there is provided a ferroelectric film manufactured by the manufacturing method of the first aspect. The ferroelectric film is a ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure, and is the film described above as the ferroelectric film to be formed. A fluorite structure, orthorhombic phase, crystalline, ferroelectric film is also described.

[0065] The metal oxide of the ferroelectric film is a metal oxide formed on a substrate by the above manufacturing method. This metal oxide is a ferroelectric film of crystals having a fluorite structure of an orthorhombic phase. In addition, in the non-reactive sputtering method, this metal oxide may be identical to the composition of the metal oxide used as a target in the above manufacturing method, or the average composition of the combination of metal oxides. In the manufacturing method of a ferroelectric film of the present invention, the composition of the obtained film basically coincides with the composition of the target. However, this metal oxide does not have to be completely identical to the composition of the metal oxide used as a target in the above manufacturing method, or the average composition of the combination of metal oxides. Even if the composition of the film obtained during sputtering is slightly different from the composition of the target, it is sufficient as long as the obtained film is a ferroelectric film of a metal oxide of crystals having a fluorite structure of an orthorhombic phase.

[0066] In a preferred embodiment of the present invention, the metal oxide of the resulting ferroelectric film is a metal oxide as described above.

[0067] In a preferred embodiment of the present invention, the ferroelectric film obtained is on a substrate, and the substrate is not particularly limited, but more preferably the substrate is a low heat-resistant substrate having a heat resistance of less than 300° C., such as an organic resin, particularly an organic resin having a glass transition temperature of less than 300° C., an inorganic glass having a low heat resistance or an inorganic glass having a glass transition temperature of less than 300° C., such as soda glass, a metal having a low heat resistance or a metal having a softening temperature of less than 300° C., such as an aluminum wiring layer, copper foil, gold foil, etc. The substrate may be inside a semiconductor device. If a ferroelectric film can be formed inside a semiconductor device at a low temperature, it is preferable because it does not affect members or elements of the semiconductor device that are sensitive to high temperatures (e.g., impurity diffusion regions, aluminum wiring, etc.).

[0068] In a preferred embodiment of the present invention, a conductive film capable of functioning as an electrode layer may be present between the substrate and the ferroelectric film. Examples of such a conductive film include ITO (indium tin oxide), aluminum, and silver. There is no restriction on the thickness of the conductive film, but it may be, for example, preferably 1 nm to 100 nm, more preferably 10 nm to 100 nm. When a conductive film is present between the substrate and the ferroelectric film, this conductive film may be considered as the substrate, or the entire substrate having a conductive film on its surface may be considered as the substrate (composite substrate) in the film forming method of the present invention.

[0069] In a preferred embodiment of the present invention, a conductive substrate such as a metal, as well as a semiconductor or insulator film may be present between the substrate and the ferroelectric film. The film between the substrate and the ferroelectric film is preferably a film deposited by a sputtering method, a PLD method, a CVD method, or the like. The substrate having such a film on its surface can also be considered as a substrate (composite substrate) in its entirety in the film forming method of the present invention.

[0070] The ferroelectric film of the present invention may have an electrode layer on the film. The electrode layer on the ferroelectric film may be made of any material as long as it is conductive, such as ITO, Pt, or Ir.

[0071] In preferred embodiments of the present invention, the ferroelectric film may be within a variety of ferroelectric functional elements or devices, such as memories, transistors, capacitors, piezoelectric elements, cooling devices, pyroelectric devices, and the like.

[0072] (Ferroelectric elements, ferroelectric functional elements or devices) The ferroelectric film provided by the present invention can be applied to various ferroelectric elements, ferroelectric functional elements or devices such as capacitors, electro-optical elements, memory elements, transistors, piezoelectric elements and pyroelectric elements by utilizing the ferroelectric properties of the ferroelectric film.

[0073] The basic element utilizing ferroelectricity is constructed as a ferroelectric expression element that has a ferroelectric film and a pair of electrode layers in order to express the ferroelectric properties of the ferroelectric film and utilize the on / off switching of the ferroelectric properties.

[0074] (Membrane Capacitor) FIG. 4 shows an example of a film capacitor. The film capacitor according to the present invention includes at least one layer of an MIM structure consisting of a ferroelectric 14 replacing a normal dielectric, a first internal electrode 13 arranged on one main surface of the ferroelectric, and a second internal electrode 15 arranged on the other main surface of the ferroelectric, a first intermediate electrode 17a for electrically connecting the first internal electrode 13 to a first external electrode (not shown), and a second intermediate electrode 17b for electrically connecting the second internal electrode 15 to a second external electrode (not shown). FIG. 4 shows a case where the MIM structure is a single layer, but a plurality of MIM structures may be stacked. When a plurality of MIM structures are stacked, the internal electrode of one MIM structure can also serve as the internal electrode of the other MIM structure. The film capacitor further includes protective films 12, 16 arranged to cover the MIM structure, and the protective films 12, 16 are arranged to cover the MIM structure, and intermediate electrodes 17a, 17b penetrate the protective films. In FIG. 4, the film capacitor is formed on a support substrate 19 via a release layer 11, and a bonding resin 18 is formed on the first protective film 16. The intermediate electrodes 17a and 17b penetrate the first protective film 16, reach the interface between the first protective film 16 and the bonding resin 18, and extend along this interface toward one end face of the film capacitor. After penetrating the first protective film 16, the intermediate electrodes 17a and 17b may reach the interface with different bonding resins 18, or may reach the interface with the same bonding resin 18. At this time, they do not necessarily have to be exposed. It is preferable that the intermediate electrodes 17a and 17b are exposed to the end face of the protective film. A plurality of film capacitors fabricated on a support substrate 19 are prepared, the film capacitors are bonded to each other using a bonding technique, and the film capacitors are peeled off from one of the support substrates 19. The bonding and peeling steps are repeated the required number of times to fabricate a laminated film capacitor having a desired number of layers.

[0075] (Ferroelectric Memory) An example of a ferroelectric memory is shown in Figure 5. This ferroelectric memory is a 1T1C type (capacitor type) that combines a ferroelectric capacitor (C) with a MOS (metal oxide semiconductor) FET (T) for memory cell selection. There is also a 2C2T type based on this, which improves data reliability by polarizing two capacitors in opposite directions. There is also a 1T type (transistor type) that uses an MFS-FET or MFMIS-FET whose gate insulating film is made of a ferroelectric, but this is specifically called FFTAM and is distinguished from the others.

[0076] Referring to FIG. 5, the ferroelectric film 21 is sandwiched between a lower electrode 22 and an upper electrode 23 made of a conductive film on the top and bottom to form a capacitor. On the other hand, the MOSFET has a gate electrode layer 28 on a semiconductor region of a low concentration impurity region between a source 25 and a drain 26 made of a high concentration impurity region in a semiconductor layer 24, via a gate insulating film 27 made of an insulating film. One electrode (upper electrode 23) of the capacitor and one of the source and drain of the MOSFET (for example, the drain 26) are electrically connected by a via filling 29 and a wiring layer 30 to form a 1T1C type memory cell. Bit lines 31 and word lines 32 run vertically and horizontally in a lattice pattern on the semiconductor substrate, and memory cells are arranged at their intersections. In the example of FIG. 5, the lower electrodes 22 of the capacitor are connected to earth 33, the other of the source and drain of the MOSFET (source 25) is connected to the bit line 31, and the gate electrode layer 28 of the MOSFET is connected to the word line 32.

[0077] (Transistor) FIG. 6 shows an example of the configuration of a field effect transistor including a ferroelectric. FIG. 6(a) shows a schematic diagram of an MFS type transistor having a gate electrode 45 of a metal layer on a semiconductor layer 41 via a ferroelectric 44 between a source 42 and a drain 43 made of a high concentration impurity region of the semiconductor layer 41. FIG. 6(b) shows a schematic diagram of an MFMIS type transistor having a dielectric layer 46 on a semiconductor layer 41 between a source 42 and a drain 43 made of a high concentration impurity region of the semiconductor layer 41 to configure a MOSFET, and a conductive layer 47 of a metal layer, a ferroelectric 44-2, and a gate electrode 45 laminated on the dielectric layer 46 to configure a capacitor. In the MFMIS type transistor in FIG. 6(b), the MOSFET and the capacitor are laminated together, while FIG. 6(c) shows an FCG type transistor in which the MOSFET and the capacitor are not laminated together but are separated. In FIG. 6(c), the capacitor is made of a laminate of a conductive layer 48, a ferroelectric 44-2, and a gate electrode 45, and is electrically connected to the conductive layer 47 of the MOSFET via a wiring 49.

[0078] By replacing the gate insulating film of a normal MOSFET with a ferroelectric film, it is possible to construct a negative capacitance transistor (NCFET) that can increase the surface potential by utilizing the negative capacitance generated by the ferroelectric and make the subthreshold characteristics steeper. It is believed that the subthreshold characteristics can be made steeper by inverting the polarization of the ferroelectric layer, which is the gate insulating film.

[0079] It is also known that an excellent ferroelectric tunnel junction (FJT) memory can be realized by using a ferroelectric film as the dielectric layer 46 in the transistor shown in FIG. 6(b)(c). The FJT transistor constituting the ferroelectric tunnel junction (FJT) memory has a tunnel junction formed by a ferroelectric film at the junction between the semiconductor region between the source and drain and the gate. The FJT usually has an MFM structure sandwiched between electrodes, an MFIM structure with an insulator added, or a modified MIFIM or MFIFM structure. Furthermore, an MFTJ structure using a magnetic material in the M phase of the electrode is also used. Here, F stands for ferroelectric, M for metal, I for insulator, T for tunnel, and J for junction.

[0080] (Ferroelectric Data Storage) Similar to hard disks using ferromagnetic materials, it is possible to configure a hard disk type storage medium (ferroelectric data storage) using ferroelectrics. Ferroelectric data storage is a type of storage medium that uses ferromagnetic materials for hard disks (1 Tbit / inch 2 It has been attracting attention as a material that can improve the memory density even more than that of HfO2 (which is said to be limited to about 1000 times the density of HfO2). In particular, crystals with an orthorhombic fluorite structure such as HfO2 show high ferroelectricity even when the film thickness is thin, making them promising materials for ferroelectric data storage. Ferroelectric data storage has a structure in which ferroelectric films are stacked on a substrate via a common electrode layer, for example, and information is recorded by applying a voltage from above the ferroelectric data storage using a probe (opposite electrode) to form domains with upward or downward polarization.

[0081] (Pyroelectric element) 7 shows a schematic diagram of an example of a pyroelectric power generation device 50. A pyroelectric element 51 is formed by sandwiching a ferroelectric substance 52 between electrodes 53. When a time-varying heat source 54 acts on this pyroelectric element 51, a voltage that varies in response to the temperature change is generated in the ferroelectric substance 52, generating electricity.

[0082] It is also possible to configure an infrared sensor by utilizing the pyroelectric effect of ferroelectrics (the phenomenon in which an electric charge is generated on the surface of a material in response to a change in temperature). Infrared sensors using ferroelectrics are a type of thermal sensor that converts infrared rays into thermal energy and measures them. They do not require cooling and are sensitive to long wavelengths (far infrared region: 5 to 1000 μm), and are superior in terms of sensitivity, S / N, and responsiveness compared to other thermal sensors that use thermistors or thermocouples.

[0083] (Electro-optical element) Fig. 8 shows an example of an optical deflector using a ferroelectric as an example of an electro-optical element. The optical deflector has a positive electrode 62 and a negative electrode 63, which are parallel plates, formed on opposing surfaces of a ferroelectric 61. By applying a DC voltage between the positive electrode 62 and the negative electrode 63, incident light can be deflected in the direction in which the electric field is applied and output as outgoing light.

[0084] (Other ferroelectric functional elements or devices) It is clear that the ferroelectric functional element or device utilizing the ferroelectricity of the ferroelectric film of the present invention is not limited to the above-mentioned examples of capacitors, electro-optical elements, memory elements, transistors, ferroelectric data storage, and pyroelectric elements, but can be widely applied to various other ferroelectric functional elements or devices and various aspects thereof.

[0085] Furthermore, the ferroelectric film provided by the present invention is a piezoelectric material and can be applied to piezoelectric elements that utilize the piezoelectric properties and functional elements or devices that use piezoelectric materials.

[0086] (Piezoelectric element) Piezoelectric elements have a structure in which a piezoelectric body is sandwiched between electrode layers made of conductive layers in order to express the piezoelectric properties of ferroelectricity and utilize the on / off of the piezoelectric properties. An example of the laminated structure of a piezoelectric element 10 is shown in Fig. 9. In a piezoelectric element 70, a base 71 has a lower electrode 72, on which a piezoelectric body 73 and an upper electrode 74 are placed, and a buffer layer 75 may be placed between the base 71 and the lower electrode 72 as necessary.

[0087] (Piezoelectric sensor) A piezoelectric element can be a piezoelectric sensor without any change in structure. In a piezoelectric element, when a voltage is applied to a piezoelectric body sandwiched between electrodes, the piezoelectric body expands and contracts. Conversely, in a piezoelectric sensor, when the piezoelectric body expands and contracts, a voltage is generated between the electrodes sandwiching the piezoelectric body, and the pressure applied to the piezoelectric sensor can be detected from the voltage.

[0088] (Actuator) An actuator is a device that generates mechanical force by displacing the piezoelectric body itself (inverse piezoelectric effect) by applying a voltage to the piezoelectric element. The ferroelectric film of the present invention is promising as a flexible actuator because it can be formed on an organic substrate.

[0089] (Inkjet head) FIG. 10(a) shows a cross-sectional view of an example of an inkjet head 80. The inkjet head 80 has a piezoelectric element 82 on the wall surface of an ink pressurizing chamber 81 that is fluidly connected to an ink chamber (not shown). The piezoelectric element 82 is configured by laminating an upper electrode layer 82-1, a ferroelectric film 82-2, and a lower electrode layer 82-3, and is laminated on an elastic layer 82-4 that forms a part of the wall surface of the ink pressurizing chamber 81. Therefore, as shown in FIG. 10(b), when the piezoelectric element 82 is driven, the elastic layer 82-4 together with the piezoelectric element 82 is deformed toward the inside of the pressurizing chamber 83, whereby the ink in the pressurizing chamber 83 is pressurized and the ink is ejected from a nozzle 84.

[0090] (Hard disk drive head) Referring to FIG. 11(a), a hard disk drive 91 includes a main body 92 on which a hard disk 90 is rotatably mounted, and a hard disk drive head 93 for reading and writing information from and to the hard disk 91. FIG. 11(b) is an enlarged view of the rear side of the suspension part of the hard disk drive head 93, which includes a magnetic head 35 at the tip of a suspension 94, a piezoelectric microactuator 96, and a slider 97. FIG. 11(c) is an enlarged view of the magnetic head 95, which includes two piezoelectric microactuators 96 on both sides, sandwiching the magnetic head 95 and the slider 97. FIG. 11(d) shows the details of the piezoelectric microactuator 96, which includes a ceramic thin plate 98 and a piezoelectric element 99. The ceramic thin plate 98 rotates as the piezoelectric element 99 expands and contracts, and the slider 97 also rotates. In the hard disk drive head shown in FIG. 11, the magnetic head rotates horizontally at the tip of the suspension by the piezoelectric microactuator, but there is also a type in which the piezoelectric microactuator rotates vertically to rotate the magnetic head vertically.

[0091] (Gyro sensor) Fig. 12 shows an example of a gyro sensor 100. As shown in the perspective view of Fig. 12(a), the gyro sensor 100 is made of a base 101 and a pair of arms 102 extending from the base 101, and has a tuning fork structure. Fig. 12(b) shows an end view of the pair of arms 102 seen from the tip direction, and a pair of piezoelectric elements 103, 104 are formed on each of the main surfaces of the arms 102 made of silicon. In a state in which the arms 102 are vibrating in a direction connecting them to each other, the angular velocity of rotation can be obtained by detecting vibrations in a direction perpendicular to the direction connecting the arms 102 to each other.

[0092] (Vibration power generation device) 13 is a diagram explaining the principle of vibration power generation. In a vibration power generation device 110, one end of a piezoelectric element 112 is fixed to a body 111 in a vibrable form, and a weight 113 is attached to the tip of the piezoelectric element 112 to facilitate vibration of the piezoelectric element 112. When the piezoelectric element 112 vibrates, a voltage is generated in the piezoelectric element 112, and power is generated by utilizing this. The ferroelectric film of the present invention can be formed on a flexible organic substrate, and is therefore promising as an oscillator.

[0093] (SAW resonator) FIG. 14 shows an example of a surface acoustic wave (SAW) resonator. In the SAW resonator 120 of FIG. 14, two ports 122 and 123, i.e., input and output comb electrodes (IDT / Inter Digital Transducer) are arranged in the center of the main surface of a piezoelectric substrate 121, and reflectors 124 are installed on both ends of the two ports. Both sides of the piezoelectric substrate 121 may be made of a sound absorbing material instead of the reflectors 124. Alternatively, only a one-port comb electrode (IDT) may be provided in the center of the main surface of the piezoelectric substrate 121. In this case, one electrode 125 of the comb electrode (IDT) is for input, and the other electrode 126 is for output. When an electric signal is applied to the input IDT, a surface acoustic wave is generated there, and the surface acoustic wave propagates along the substrate surface and reaches the output IDT, where it is converted back into an electric signal. The resonant frequency (usually several tens of MHz to several GHz) is determined by the shape of the comb electrode (IDT). The reflector 124 reflects the surface acoustic wave.

[0094] (FBAR) An example of a film bulk acoustic resonator (FBAR / Film Bulk Acoustic Resonator) 130 is shown in Fig. 15. A cavity 132 is provided in a silicon substrate 131, and a piezoelectric element consisting of a lower electrode 133, a piezoelectric body 134, and an upper electrode 135 is formed in the portion where the cavity 132 opens on the main surface of the silicon substrate 131. The piezoelectric element vibrates in the bulk, that is, in the stacking direction (the up and down direction in the figure), and the resonant frequency is determined by the dimensions of the opening and the thickness of the piezoelectric body 134. Both SAW resonators and film bulk acoustic resonators form high-frequency (usually several tens of MHz to several GHz) resonators by utilizing the property that the speed of wave motion propagating in an elastic body is orders of magnitude slower than the propagation speed in space.

[0095] (Piezoelectric mirror) Examples of piezoelectric mirrors are shown in Fig. 16-1 and Fig. 16-2. Referring to Fig. 16-1(a), a piezoelectric mirror element 140 is connected to a first support 143 via a torsion bar 142 that rotatably holds a mirror 141. As shown in an enlarged view in Fig. 16-1(b), the first support 143 has piezoelectric elements 144 and 145 on both sides of the torsion bar 142. When a voltage of a resonant frequency is applied to the first and second piezoelectric elements 144 and 145, as shown in Fig. 16-1(c), the mirror 141 rotates around the torsion bar 142 as an axis due to the twisting of the torsion bar 142 associated with the expansion and contraction of the first and second piezoelectric elements 144 and 145 relative to the first support 143. Referring again to FIG. 16-1(a), the first support 143 has third piezoelectric elements 146 and fourth piezoelectric elements 147 alternately connected in a zigzag shape, and the outermost third and fourth piezoelectric elements 146, 147 are connected to the second support 148. FIG. 16-2(d) shows a schematic diagram of the deformation of the piezoelectric elements when the zigzag-connected third piezoelectric element 144 and fourth piezoelectric element 145 are driven, and the deformation of the third and fourth piezoelectric elements 146, 147 causes the first support 143 to rotate with respect to the second support 148 about the connecting portion as an axis. The rotation of the mirror 141 by the third and fourth piezoelectric elements 145 is perpendicular to the axial direction of the rotation of the first and second piezoelectric elements 144, 145 about the torsion bar 142 as an axis. Therefore, with this piezoelectric mirror element 140, the mirror 141 can rotate in both the up-down and left-right directions, and as a result, the reflection direction of the mirror 141 can also be changed in both the up-down and left-right directions. Therefore, as shown in Figure 16-2(e), it is possible for light ray 147 incident on the mirror 141 from the light source 146 to scan in both the up-down and left-right directions on the screen 148, i.e., across the entire screen.

[0096] (Other functional elements or devices using piezoelectric bodies) It is clear that the functional element or device using the piezoelectric material of the present invention is not limited to the above examples, but can also be applied to various devices using piezoelectric materials and various embodiments thereof, such as ultrasonic probes, ultrasonic transmitters, ultrasonic sensors, etc. EXAMPLES

[0097] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. (Ferroelectricity Measurement) In the following examples, the polarization hysteresis of the film (measurement of ferroelectricity) was measured using a ferroelectric tester (FCE-1A model, manufactured by Toyo Corporation). For the deposited film, an upper electrode was made of Pt by electron beam deposition, with a film thickness of 20 to 100 nm and a diameter of 50 to 100 μm.

[0098] Example 1 Film formation was carried out using a sputtering apparatus as shown in Fig. 2. This sputtering apparatus has a substrate holding means capable of being heated by a heater in a vacuum chamber, a target setting means, a thermometer, a gas supply port, an exhaust port for reducing pressure, and a power source for applying a voltage between the substrate and the target, and forms a film on the substrate by reducing the pressure inside the vacuum chamber and applying a voltage between the substrate and the target, which causes the ionized gas to sputter the target.

[0099] The substrate used was an ITO / YSZ111 substrate, which was a 500 μm thick (111)-oriented yttria-stabilized zirconia (Y10%-YSZ111) substrate with an ITO film of about 50 nm formed on it. The target was a mixture of 93 mol % hafnia (HfO2) and 7 mol % yttria (YO 1.5 ) mixed target (7%YO 1.5 The substrate temperature was set to 50°C, and the atmosphere in the chamber was first replaced with argon and then evacuated, after which it was set to an argon flow rate of 100sccm, oxygen of 0sccm, and pressure of 10mTorr. The sputtering power was set to 10-50W.

[0100] 7%YO on ITO / YSZ111 substrate 1.5 A film of 7% YO was deposited to a thickness of 160 nm. 1.5 The chart obtained by X-ray diffraction analysis of the -93% HfO2 film is shown in Figure 17(a). 1.5It was confirmed that the -93%HfO2 film (crystals with this composition are labeled YHO7 in the figure, and are the same in other figures) is polycrystalline, contains an epitaxial phase (single crystal layer) in some parts, and has a fluorite structure of the orthorhombic or tetragonal phase.

[0101] This 7%YO 1.5 The polarization hysteresis measurement results (relationship between polarization and electric field) of the -93% HfO2 polycrystalline film are shown in Fig. 18(a). 1.5 It was confirmed that the -93%HfO2 crystalline film exhibited ferroelectricity. After hysteresis measurement (applied electric field), 1.5 The -93%HfO2 polycrystalline film was confirmed to be in the orthorhombic phase because it exhibited ferroelectric properties.

[0102] (Example 2: Soda glass substrate) Except for changing the substrate from ITO / YSZ111 to ITO / soda glass, the deposition of Example 2 was carried out in the same manner as in Example 1. The ITO / soda glass substrate was a substrate in which an ITO film was deposited to a thickness of 150 nm on soda glass with a thickness of 1100 μm.

[0103] 7%YO deposited on ITO / soda glass substrate 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 17(b). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0104] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 18(b). 1.5 It was confirmed that the -93%HfO2 crystalline film exhibited ferroelectricity. After hysteresis measurements, 1.5 The -93%HfO2 polycrystalline film was confirmed to be in the orthorhombic phase because it exhibited ferroelectric properties.

[0105] (Example 3: Alkali-free glass substrate) Except for changing the substrate from ITO / YSZ111 to ITO / alkali-free-glass, the deposition of Example 3 was carried out in the same manner as in Example 1. The ITO / alkali-free glass substrate was a substrate in which an ITO film was deposited to a thickness of 150 nm on an alkali-free glass substrate having a thickness of 700 μm.

[0106] 7%YO deposited on ITO / alkali-free substrate 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 17(c). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0107] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 18(c). 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity. After hysteresis measurements, 1.5 The -93%HfO2 polycrystalline film was confirmed to be in the orthorhombic phase because it exhibited ferroelectric properties.

[0108] (Example 4: PET substrate) Except for changing the substrate from ITO / YSZ111 to ITO / polyethylene terephthalate (ITO / PET), the film formation of Example 4 was carried out in the same manner as in Example 1. The ITO / PET substrate was a substrate in which an ITO film of 150 nm was formed on a 150 μm-thick polyethylene terephthalate film (heat-resistant temperature 200° C.).

[0109] 7%YO deposited on ITO / PET substrate 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 17(d). 1.5It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0110] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 18(d). 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity. After hysteresis measurements, 1.5 The -93%HfO2 polycrystalline film was confirmed to be in the orthorhombic phase because it exhibited ferroelectric properties.

[0111] (Example 5: Room temperature and 100°C) The substrate temperature during sputtering was changed from 50°C to room temperature (unheated) and 100°C, and 7% YO 1.5 The deposition of Example 5 was carried out in the same manner as in Example 1, except that the thickness of the -93% HfO2 film was 50 nm when deposited at room temperature and 170 nm when deposited at 100°C.

[0112] 7%YO obtained at room temperature 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 19(a). 1.5 It was confirmed that the -93%HfO2 film had a fluorite structure of either the orthorhombic or tetragonal phase (denoted as O / T in the figure, the same below).

[0113] 7%YO obtained at room temperature 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 19(b). 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity. After hysteresis measurements, 1.5 The -93%HfO2 polycrystalline film was also confirmed to be in the orthorhombic phase, as it exhibited ferroelectricity.

[0114] 7%YO obtained at a substrate temperature of 100°C 1.5The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 19(c). 1.5 It was confirmed that the -93%HfO2 films had an orthorhombic or tetragonal fluorite structure, respectively.

[0115] 7%YO obtained with the substrate temperature set at 100°C 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 film are shown in Fig. 19(d). From Fig. 19(d), after the hysteresis measurement, 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity.

[0116] (Example 6: Room temperature, 150 nm) The substrate temperature during sputtering was changed from 50°C to room temperature (unheated), and 7% YO 1.5 The film formation of Example 6 was carried out in the same manner as in Example 2, except that the thickness of the -93% HfO2 film was set to 150 nm.

[0117] Obtained 7%YO 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 20-1(a). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0118] Obtained 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 film are shown in Figure 20-1(b). 1.5 The results of PUND (Positive-up-negative-down) polarization measurements of the -93% HfO2 film are shown below. These results confirmed that the film exhibits ferroelectricity.

[0119] (Example 7: Room temperature, 210 nm) The substrate temperature during sputtering was changed from 50°C to room temperature (unheated), and 7% YO 1.5The deposition of Example 7 was carried out in the same manner as in Example 4, except that the thickness of the -93% HfO2 film was set to 210 nm.

[0120] Obtained 7%YO 1.5 The chart obtained by X-ray diffraction analysis of the -93%HfO2 film is shown in Figure 21-1(a). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0121] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 film are shown in Figure 21-1(b). From Figure 21-1(b), after the hysteresis measurement, 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity.

[0122] Obtained 7%YO 1.5 Bright-field images of the -93% HfO2 film and ITO / PET substrate taken by a transmission electron microscope are shown in Figure 21-2(a). 1.5 The selected area electron diffraction image of the -93%HfO2 film is shown in Figure 21-2(b). The diffraction image in Figure 21-2(b) shows random spots, which indicates that the 7%YO 1.5 It was confirmed that the -93%HfO2 film was a polycrystalline film. Figure 21-2(c) shows a dark-field image of a transmission electron microscope imaged using 222 diffraction in Figure 21-2(b). 1.5 It was confirmed that the -93%HfO2 film was composed of columnar grains with a width of approximately 50 nm, and that the columnar grains were formed.

[0123] (Example 8: YSZ100 substrate) Substrate changed from (111)ITO / (111)YSZ to (100)ITO / (100)YSZ, 7%YO 1.5 Except for changing the thickness of the -93% HfO2 film to 16 nm and 50 nm, the film of Example 8 was formed in the same manner as in Example 1. The (100) ITO / (100) YSZ substrate was a substrate in which a (100) ITO film was formed on the (100) ITO using (100)-oriented YSZ.

[0124] A 7% YO film with a thickness of 16 nm was deposited on a (100) ITO / (100) YSZ substrate. 1.5 The chart obtained by X-ray diffraction analysis of the -93% HfO2 film is shown in Figure 22(a). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0125] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 22(b). 1.5 It was confirmed that the -93%HfO2 polycrystalline film exhibited ferroelectricity. After hysteresis measurements, 1.5 The -93%HfO2 polycrystalline film was also confirmed to be in the orthorhombic phase, as it exhibited ferroelectricity.

[0126] A 50 nm thick 7% YO film was deposited on a (100) ITO / (100) YSZ substrate. 1.5 The chart obtained by X-ray diffraction analysis of the -93% HfO2 film is shown in Figure 22(c). 1.5 It was confirmed that the -93%HfO2 film was polycrystalline and had a fluorite structure of either the orthorhombic or tetragonal phase, respectively.

[0127] This 7%YO 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 polycrystalline film are shown in Fig. 22(d). 1.5 -93%HfO2 polycrystalline film was confirmed to exhibit ferroelectricity. 1.5 The -93%HfO2 polycrystalline film was also confirmed to be in the orthorhombic phase, as it exhibited ferroelectricity.

[0128] (Example 9: Stainless steel, Al2O3 (c-plane), SRO / STO substrate) The substrate was changed from (111)ITO / (111)YSZ to stainless steel (SUS304), Pt / Si, ITO / Al2O3 (c-plane), and SRO / STO, respectively, and 7%YO 1.5 Except for the various -93%HfO2 films, the deposition of the film of Example 9 was carried out in the same manner as in Example 5, where the substrate temperature was room temperature. The Pt / Si substrate was a substrate in which a 110 nm thick (111)Pt was deposited on a (001)Si substrate, the ITO / Al2O3 (c-plane) was a substrate in which a 50 nm thick (111)ITO was deposited on an Al2O3 (c-plane) substrate, the SRO / STO was a substrate in which a conductive (111)SrRuO3 was deposited on a (111)SrTiO3, and the (111)YSZ was a (111)-oriented Y10%-YSZ substrate.

[0129] In particular, FIG. 23-1 to FIG. 24 show that the obtained 7% YO 1.5 It was confirmed that both -93%HfO2 films exhibited ferroelectricity through polarization hysteresis measurements (relationship between polarization and electric field). 1.5 In the -93% HfO2 film, X-ray diffraction analysis revealed that 7% 1.5 It was confirmed that the -93%HfO2 film is a polycrystalline film with a fluorite structure of the orthorhombic or tetragonal phase, and therefore, it was also confirmed to be in the orthorhombic phase because it showed ferroelectricity after the hysteresis measurement. 1.5 It was confirmed that the -93% HfO2 film exhibits ferroelectricity by measuring the polarization hysteresis (relationship between polarization and electric field).

[0130] Figure 23-1(a) shows a 7% YO film with a thickness of 150 nm formed on a Pt / Si substrate. 1.5 The X-ray diffraction analysis chart of -93%HfO2 film is shown. 1.5 It was confirmed that the -93%HfO2 film was polycrystalline with a fluorite structure of either the orthorhombic or tetragonal phase. Figure 23-1(b) and (c) show a 7% YO film with a thickness of 150 nm formed on a Pt / Si substrate. 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 film are shown in Figure 23-2. 1.5The results of PUND (Positive-up-negative-down) polarization measurements of the -93% HfO2 film are shown below. These results confirmed that the film exhibits ferroelectricity.

[0131] Figure 24(a) and (b) show a 7% YO film with a thickness of 50 nm formed on an ITO / Al2O3 (c-plane) substrate. 1.5 The X-ray diffraction analysis chart and polarization hysteresis measurement (relationship between polarization and electric field) results of -93%HfO2 film are shown. 1.5 It was confirmed that the -93%HfO2 film has an orthorhombic or tetragonal fluorite structure and exhibits ferroelectricity by hysteresis measurements. Figure 24(c) shows a 7% YO film with a thickness of 50 nm formed on an SRO / STO substrate. 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93% HfO2 film are shown below. It was confirmed that the film exhibits ferroelectricity.

[0132] (Example 10: Power 10W) Example 10 was carried out in the same manner as Example 1, except that the sputtering power was changed from 50 W to 10 W. 1.5 -93%HfO2 was analyzed by X-ray diffraction to find that 7%YO 1.5 It was confirmed that -93%HfO2 has a fluorite structure of orthorhombic or tetragonal phase, and that it exhibits ferroelectricity through polarization hysteresis measurements (relationship between polarization and electric field), and therefore that it is also orthorhombic. 1.5 The X-ray diffraction analysis chart of -93% HfO2 is shown.

[0133] (Comparative example 1: PLD) The film was formed using a pulsed laser deposition apparatus, which has a heater-heatable substrate holding means, a target installation means, a thermometer, and a gas supply port in a vacuum chamber, and forms a film on the substrate by irradiating the target with a pulsed laser beam from a laser emitter through a lens.

[0134] The substrate used was yttria-stabilized zirconia (Y10%-YSZ) with a (111) orientation, and the target used was a mixture of hafnia (HfO2) and 7 mol% yttrium (Y). The substrate temperature was set to room temperature. The atmosphere in the chamber was first replaced with argon and evacuated, and then the supply gas was changed to 0 sccm argon and 0.5 sccm oxygen, creating an oxygen atmosphere of 20 mTorr. The laser light was 3 J / cm 2 The target was irradiated with a 5 Hz pulsed KrF laser beam.

[0135] 7% YO on yttria-stabilized zirconia substrate 1.5 The resulting 7% YO 1.5 X-ray diffraction analysis of the -93% HfO2 film revealed that it was a crystal with a fluorite structure, but was in a monoclinic crystal phase and a paraelectric phase.

[0136] (Comparative example 2: PLD) The deposition of Comparative Example 1 was carried out in the same manner as in Comparative Example 1, except that the atmosphere in the chamber was first replaced with argon and evacuated, and then the supply gas was changed to 0.5 sccm of argon and 0 sccm of oxygen, creating an argon atmosphere of 20 mTorr.

[0137] 7%YO film formed on Y10%-YSZ substrate 1.5 X-ray diffraction analysis of the -93% HfO2 film revealed that it was a crystal with a fluorite structure, but in a monoclinic crystal phase, a paraelectric phase.

[0138] (Comparative example 3: PLD) The film of Comparative Example 3 was formed in the same manner as in Comparative Example 1 and Comparative Example 2, except that the substrate was changed from Y10%-YSZ to ITO / Glass.

[0139] 7%YO film formed on Y10%-YSZ substrate 1.5 X-ray diffraction analysis of the -93%HfO2 film revealed that 7%YO 1.5No peak of -93%HfO2 was observed, and the film was not crystallized.

[0140] (Example 11: Polyimide Substrate) The substrate was changed from ITO / YSZ111 to ITO / polyimide, and a 7%YO 1.5 Except for the various -93%HfO2 films, the deposition of the film of Example 11 was carried out in the same manner as in Example 5, in which the substrate temperature was room temperature (non-heated). The ITO / polyimide substrate was a polyimide substrate with a 15 nm (111) ITO film deposited thereon.

[0141] Obtained 7%YO 1.5 As shown in Figure 26, the -93%HfO2 film was confirmed to exhibit ferroelectricity by polarization hysteresis measurement (relationship between polarization and electric field). 1.5 In the -93% HfO2 film, X-ray diffraction analysis revealed that 7% 1.5 It was confirmed that the -93%HfO2 film was a polycrystal with a fluorite structure of the orthorhombic or tetragonal phase, and therefore, it was also confirmed to be in the orthorhombic phase because it exhibited ferroelectricity after the hysteresis measurement.

[0142] (Example 12: Epitaxial film) The substrate was changed from ITO / YSZ111 to YSZ100, and 7% YO with a thickness of 16 nm was deposited at room temperature. 1.5 Example 12 was carried out in the same manner as Example 1, except that a -93% HfO2 film was formed.

[0143] Obtained 7%YO 1.5 Bright-field images of the -93%HfO2 / ITO / YSZ100 in a transmission electron microscope are shown in Fig. 27(a). 1.5 The selected-area electron diffraction image of the -93% HfO2 film is shown in Figure 27(b), and the selected-area electron diffraction images of the ITO electrode and the YSZ100 substrate are shown in Figure 27(c). 1.5 It was confirmed that the -93% HfO2 film was crystallized directly above the ITO. 1.5 The atomic arrangement of the -93%HfO2 film is consistent with that of the ITO / YSZ100 substrate, so1.5 It was confirmed that the -93%HfO2 film was an epitaxial film lattice-matched to ITO.

[0144] (Example 13: Film thickness 20 nm) At room temperature (unheated), 7% YO with a film thickness of 20 nm 1.5 The deposition of Example 13 was carried out in the same manner as in Example 5, except that a -93% HfO2 film was deposited.

[0145] From the X-ray diffraction analysis chart, 7%YO 1.5 It was confirmed that the -93%HfO2 film was an epitaxial film and had a tetragonal fluorite structure. The results of measuring the polarization hysteresis of the film are shown in Figure 28. 1.5 It was confirmed that the -93%HfO2 film exhibited ferroelectricity and had an orthorhombic phase.

[0146] (Example 14: Film thickness 900 nm) At room temperature (unheated), the sputtering power was 100 W, and the film thickness was 900 nm. 1.5 The deposition of Example 14 was carried out in the same manner as in Example 5, except that a -93% HfO2 film was deposited.

[0147] The X-ray diffraction analysis chart and the polarization hysteresis measurement results of the obtained film are shown in FIG. 29, and it was confirmed that the film contained an orthorhombic phase and exhibited ferroelectricity.

[0148] Example 15: 5% YO 1.5 -95%HfO2 film) The target composition is 7%YO 1.5 -93%HfO2 and 5%YO 1.5 -95%HfO2, room temperature (non-heated), sputtering power 50W, 7%YO with a thickness of 16nm 1.5 -93% HfO2 film and 14nm 5% YO 1.5 The deposition of Example 15 was carried out in the same manner as in Example 5, except that a -95% HfO2 film was deposited.

[0149] Obtained 7%YO 1.5-93% HfO2 film and 5% YO 1.5 The X-ray diffraction analysis chart of the -95% HfO2 film is shown in FIG. 30, and the polarization hysteresis measurement results are shown in FIG. Figure 30(a) shows the 7% YO deposited at room temperature on the ITO / (111) YSZ substrate. 1.5 This is a 2Theta-Psi map of the 110 superlattice diffraction in a -93% HfO2 film. Since no 110 superlattice diffraction due to the orthorhombic phase was observed, this film was confirmed to be in the tetragonal phase.

[0150] On the other hand, Fig. 30(b) shows 5% YO deposited at room temperature on an ITO / (111) YSZ substrate. 1.5 This is a 2Theta-Psi map around the 110 superlattice diffraction in a -95% HfO2 film. Since the 110 superlattice diffraction originating from the orthorhombic phase was observed, this film was confirmed to be in the orthorhombic phase.

[0151] Figure 31(a) shows a 16 nm 7% YSZ thin film deposited at room temperature on an ITO / (111) YSZ substrate. 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -93%HfO2 film are shown in Fig. 31(a). 1.5 It was confirmed that the -93%HfO2 film exhibited ferroelectricity. In addition, crystal structure analysis confirmed that the film exhibited ferroelectricity even though it was in the tetragonal phase after deposition at room temperature, confirming an electric field-induced phase transition from the tetragonal phase to the orthorhombic phase.

[0152] Figure 31(b) shows a 14 nm 5% YSZ film deposited at room temperature on an ITO / (111) YSZ substrate. 1.5 The results of the polarization hysteresis measurement (relationship between polarization and electric field) of the -95%HfO2 film are shown in Fig. 31(b). 1.5 It was confirmed that the -95%HfO2 film exhibited ferroelectricity.

[0153] Figure 31(c) and (d) show 7%YO 1.5 -93% HfO2 film and 5% YO 1.5 The remanent polarization value Pr and the coercive field Ec of the -95%HfO2 film are shown as a function of applied voltage. 1.5-The remanent polarization value can be obtained by applying a voltage of about 5000 kV / cm to the 93% HfO2 film, whereas the remanent polarization value can be obtained by applying a voltage of about 5000 kV / cm to the 5% YO 1.5 -For the 95%HfO2 film, the residual polarization value can be obtained by applying a voltage of about 3000kV / cm. 1.5 In order for the -93%HfO2 film to exhibit ferroelectricity, a field-induced phase transition from the tetragonal phase to the orthorhombic phase is required, so the electric field required to obtain the remanent polarization value is 5%YO 1.5 -This is thought to have a higher possibility than the 95% HfO2 film.

[0154] In addition, in Figure 31(d), there is almost no difference in the remanent polarization value Pr and coercive field Ec when the applied voltage is increased (up) and decreased (down), suggesting that the crystal was in the orthogonal phase before the electric field was applied. In contrast, in Figure 31(c), there is a significant difference in the remanent polarization value Pr and coercive field Ec when the applied voltage is increased (up) and decreased (down), indicating that an electric field-induced transformation from the tetragonal phase to the orthogonal phase has occurred.

[0155] (Example 16: Annealing at 1000°C) In Example 6, 7% YO with a thickness of 16 nm 1.5 -93%HfO2 films were deposited on ITO / YSZ111 substrates and then annealed at 1000℃ for 10 seconds in an inert atmosphere. The results of measuring the polarization hysteresis of the film before and after annealing after deposition are shown in Figure 32. After deposition at room temperature, the film was in the tetragonal phase, but after application of an electric field, both before and after annealing, it was confirmed that the film was in the orthorhombic phase. As shown in Figure 32, there is no significant difference in the polarization hysteresis before and after annealing, and a ferroelectric film equivalent to the 1000°C annealed film was obtained by deposition at room temperature.

[0156] Example 17: Hf 0,75 Zr 0.25 O2 membrane) The same as in Example 1, except that the target contained hafnia (HfO2) and zirconia (ZrO2) in a molar ratio of 75:25, with 95 mol% Hf 0.75 Zr 0.25 O2 and 5 mol% yttria (YO 1.5) mixed target (5%YO 1.5 -95%Hf 0.75 Zr 0.25 O2) at room temperature (without heating the substrate), 1.5 -95%Hf 0.75 Zr 0.25 An O2 membrane was formed.

[0157] Obtained 27nm 5%YO 1.5 -95%Hf 0.75 Zr 0.25 The polarization hysteresis measurement results of the O2 film are shown in Figure 33(a). It was confirmed that a ferroelectric film with an orthorhombic phase of the fluorite structure was obtained.

[0158] Obtained 13.7 nm 5% YO 1.5 -95%Hf 0.75 Zr 0.25 The polarization hysteresis measurement results of the O2 film are shown in FIG. 33(b), and it was confirmed that a ferroelectric film with an orthorhombic phase of the fluorite structure was obtained.

[0159] (Example 18: 5% YO 1.5 -95%Hf 0.75 Zr 0.25 O2 film, ITO / YSZ100 substrate) In Example 18, the same procedure as in Example 17 was used, except that ITO / YSZ100 was used as the substrate instead of ITO / YSZ111, and a 5% YBCO film with a thickness of 27 nm was formed. 1.5 -95%Hf 0.75 Zr 0.25 An O2 membrane was formed.

[0160] Obtained 27nm 5%YO 1.5 -95%Hf 0.75 Zr 0.25 From the X-ray analysis chart and the polarization hysteresis measurement results, it was confirmed that the O2 film was a ferroelectric film with an orthorhombic phase of fluorite structure.

[0161] Figure 34(a) shows the 5% YO on the ITO / YSZ111 substrate. 1.5 -95%Hf 0.75 Zr 0.25The polarization hysteresis measurement results of the O2 film are shown in Fig. 34(b). 1.5 -95%Hf 0.75 Zr 0.25 The polarization hysteresis measurement results of the O2 film are shown.

[0162] Example 19: 5% YO 1.5 -95%Hf 0.50 Zr 0.50 O2 film, ITO / YSZ substrate) Example 19 was similar to Example 17, except that ITO / YSZ111 and ITO / YSZ100 were used as substrates, hafnia (HfO2) and zirconia (ZrO2) were included in a molar ratio of 50:50 as targets, and 5 mol % of yttria (YO) was added to the total of 95 mol % of hafnia (HfO2) and zirconia (ZrO2). 1.5 ) mixed target (5%YO 1.5 -95%Hf 0.50 Zr 0.50 O2) at room temperature (without heating the substrate), 1.5 -95%Hf 0.50 Zr 0.50 An O2 membrane was formed.

[0163] Obtained 33nm 5%YO 1.5 -95%Hf 0.50 Zr 0.50 It was confirmed from the X-ray analysis chart and the polarization hysteresis measurement results that the O2 film was a ferroelectric film with an orthorhombic phase of the fluorite structure on both the ITO / YSZ111 and ITO / YSZ100 substrates.

[0164] Figure 34(c) shows the 5% YO on the ITO / YSZ111 substrate. 1.5 -95%Hf 0.50 Zr 0.50 The polarization hysteresis measurement results of the O2 film are shown in Fig. 34(d). 1.5 -95%Hf 0.75 Zr 0.25 The polarization hysteresis measurement results of the O2 film are shown.

[0165] (Example 20: 5% YO 1.5 -95%Hf 0.50 Zr 0.50 O2 membrane, Pt / Si) In Example 20, the same procedure as in Example 19 was used, except that a Pt / Si substrate was used instead of an ITO / YSZ substrate, and a Pt film was deposited at a different temperature. 1.5 -95%Hf 0.50 Zr 0.50 An O2 membrane was formed.

[0166] Obtained 33nm 5%YO 1.5 -95%Hf 0.50 Zr 0.50 It was confirmed from the X-ray analysis chart and the polarization hysteresis measurement results that the O2 film was a ferroelectric film with an orthorhombic phase of the fluorite structure on both Pt / Si substrates.

[0167] Instead of ITO / YSZ as the substrate, 5%YO on Pt / Si substrate with different Pt deposition temperatures was used. 1.5 -95%Hf 0.50 Zr 0.50 The polarization hysteresis measurement results of the O2 film are shown in Figure 35(a) and (b), respectively. [Explanation of symbols]

[0168] 1. Vacuum chamber 2 Base 3. Target 4 Power supply 5 Gas introduction system 10 Sputtering equipment

Claims

1. A ferroelectric film containing a crystalline metal oxide having an orthorhombic fluorite structure is manufactured by sputtering a target at a substrate temperature of less than 300°C, depositing a metal oxide film capable of having an orthorhombic fluorite structure on the substrate, and then subjecting the film to a thermal history of less than 300°C, or by applying an electric field to the film after the deposition or thermal history. The metal of the metal oxide contains one or both of hafnium (Hf) and zirconium (Zr), or the metal of the metal oxide contains hafnium (Hf) and zirconium (Zr). a method for producing a ferroelectric film, the method comprising: adding one or both of hafnium (Hf) and zirconium (Zr) to at least one additional element selected from aluminum (Al), silicon (Si), strontium (Sr), barium (Ba) and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), the number of moles of the additional element being 15 mol % or less, with the total of all metals in the metal oxide containing the additional element being 100 mol %.

2. 2. The method for producing a ferroelectric film according to claim 1, wherein the sputtering is carried out in an inert atmosphere with an oxygen partial pressure of less than 1%.

3. 3. The method for producing a ferroelectric film according to claim 1, wherein the substrate is any one of a substrate containing glass having a glass transition point of less than 300°C, a substrate containing a polymer organic layer, a substrate containing a metal layer having a softening temperature of less than 300°C, and the inside of a semiconductor device.

4. 1. A ferroelectric film comprising a crystalline metal oxide having an orthorhombic fluorite structure, the ferroelectric film being provided on any one of a substrate comprising glass having a glass transition point of less than 300°C, a substrate comprising a polymer organic layer, and a substrate comprising a metal layer having a softening temperature of less than 300°C, wherein the metal of the metal oxide comprises one or both of hafnium (Hf) and zirconium (Zr), or one or both of hafnium (Hf) and zirconium (Zr) and at least one additional element selected from aluminum (Al), silicon (Si), strontium (Sr), barium (Ba), and rare earth elements (Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), and the number of moles of the additional element is 15 mol % or less, with the total of all metals in the metal oxide including the additional element being 100 mol %.

5. 5. The ferroelectric film according to claim 4, further comprising a conductive film layer between said substrate and said ferroelectric film.

6. A ferroelectric functional element comprising the ferroelectric film according to claim 4 or 5 and a pair of electrodes.

7. 7. The ferroelectric functional element according to claim 6, wherein the ferroelectric functional element is selected from the group consisting of a capacitor, an electro-optical element, a memory element, a transistor, a ferroelectric data storage, a piezoelectric element, and a pyroelectric element.

8. 7. The piezoelectric functional element according to claim 6, wherein the ferroelectric functional element is any one of an actuator, an inkjet head, a Jaoro sensor, a vibration power generation element, a surface acoustic wave resonator, a film bulk wave resonator, a piezoelectric mirror, and a piezoelectric sensor.

Citation Information

Patent Citations

  • Method for producing crystallized ceramic film and the ceramic film

    JP2001146421A

  • Manufacturing method for ferroelectric device, ferroelectric memory using the same, piezoelectric element, ink jet head, and ink jet printer

    JP2004096050A

  • Forming method of ferroelectric thin film and paraelectric thin film, and semiconductor device

    JP2009238842A

  • Method of manufacturing ceramic film, ferroelectric element and electronic component

    JP2011086819A

  • Perovskite-type oxide film, ferroelectric film using the same, ferroelectric device, and method for manufacturing perovskite-type oxide film

    JP2012106902A