Lithium potassium elemental oxide compounds as Li superionic conductors, solid electrolytes, and coating layers for lithium metal and lithium ion batteries

Lithium-potassium element oxide compounds with formulas (I) to (IV) address safety and stability issues in lithium-ion batteries by offering high conductivity and low activation energy, enhancing battery performance and safety.

JP7582823B2Active Publication Date: 2024-11-13MARYLAND COLLEGE PARK UNIV OF +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020153091
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-13
Filing Date
2020-09-11
Publication Date
2024-11-13
Estimated Expiration
2040-09-11

AI Technical Summary

Technical Problem

Current lithium-ion batteries face safety risks due to flammable organic solvents and dendrite formation, and existing solid-state lithium conductors lack stability and cost-effectiveness, failing to meet all requirements for high conductivity, low activation energy, and electrochemical stability.

Method used

Development of lithium-potassium element oxide compounds with specific formulas (I) to (IV) as solid electrolytes, exhibiting high Li+ conductivity (10-22 mS/cm) and low activation energy (0.15-0.50 eV), suitable for use in solid-state lithium batteries and protective coating layers.

Benefits of technology

The lithium-potassium element oxide compounds provide enhanced mechanical and thermal stability, preventing dendrite formation and improving charge/discharge rates, while being cost-effective and easy to synthesize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582823000007
    Figure 0007582823000007
  • Figure 0007582823000008
    Figure 0007582823000008
  • Figure 0007582823000009
    Figure 0007582823000009
Patent Text Reader

Abstract

To identify a range of further materials which have high Li ion conductivity and low electron conductivity and are suitable as a solid state electrolyte for a lithium ion battery and / or suitable as a protective coating layer or a component of an electrode active material; and provide a solid state lithium ion battery and / or lithium metal battery containing a solid state Li ion electrolyte membrane and / or electrode containing the material.SOLUTION: Solid-state lithium ion electrolytes of lithium potassium element oxide based compounds are provided which contain an anionic framework capable of conducting lithium ions. The element atoms are Ir, Sb, I, Nb and W. The activation energy of the lithium potassium element oxide compounds is from 0.15 to 0.50 eV, and the conductivity is 10-3 to 22 mS / cm at 300K.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Names of the parties to the joint research agreement The subject matter disclosed herein is the result of collaborative research conducted under a Cooperative Research Agreement between Toyota Motor Engineering and Manufacturing North America, Inc., 6565 Headquarters Drive W1-3C, Plano, Texas, 75024, and the University of Maryland, College Park, 2130 Mitchell Bldg. 7999 Regents Dr., College Park, Maryland, 20742.

[0002] Field of the Disclosure The present disclosure relates to novel lithium potassium elemental oxide compounds useful as Li superionic conductors, solid electrolytes comprising the novel lithium potassium elemental oxide compounds, and electrode coating layers for Li metal and Li ion batteries comprising the novel lithium potassium elemental oxide compounds, the elements of which may be one or more selected from Ir, Sb, I, Nb, and W. [Background technology]

[0003] background Li-ion batteries have traditionally dominated the portable electronics market, but the safety risks associated with conventional Li-ion batteries, which contain flammable organic solvents as components of the electrolyte, have raised concerns that may limit or prevent the use of Li-ion batteries in large-scale energy storage applications.

[0004] By replacing the flammable organic liquid electrolyte with a solid Li-conducting phase, this safety issue can be mitigated and further benefits such as improved mechanical and thermal stability can be realized. The solid Li-conducting phase is usually called a solid Li-ion conductor or solid electrolyte, and its main function is to conduct the Li-ion current while blocking the direct movement of electrons between the electrodes inside the battery. +It is to conduct ions from the anode side to the cathode side during discharge and from the cathode side to the anode side during charging.

[0005] Also, in lithium batteries constructed with non-aqueous electrolytes, dendritic lithium metal structures are known to form protruding from the anode to the cathode during repeated charge-discharge cycles, and if such dendritic structures protrude into the cathode and short-circuit the battery, energy can be rapidly released, resulting in ignition of the organic solvent.

[0006] Therefore, there has been great interest and great efforts in discovering new solid-state Li-ion conducting materials that can lead to all-solid-state lithium batteries. 14 ZnGeO 16 ), NASICON (Li 1.3 Al 0.3 Ti 1.7 (PO4)3), perovskites (e.g., La 0.5 Li 0.5 TiO3), Garnet (Li7La3Zr2O 12 ), LiPON (for example, Li 2.88 PO 3.73 N 0.14 ), as well as, for example, Li3PS4, Li7P3S 11 , and LGPS(Li 10 GeP2S 12 The focus has been primarily on ionically conducting oxides, such as sulfides, e.g.

[0007] Recent progress has led to solid-state Li-ion conductors with conductivities of 1–10 mS / cm, which is comparable to the conductivities of liquid-phase electrolytes, and therefore there is great interest in discovering new solid-state Li-ion conductors.

[0008] Effective lithium-ion solid conductors have high Li at room temperature. + Generally, this Li + Conductivity is 10-6 Furthermore, for use over a wide range of operating temperatures that may occur in the environment, the Li + The activation energy of migration should be low. In addition, the material should have good stability against chemical, electrochemical, and thermal decomposition. The solid conductor material should be stable in terms of electrochemical decomposition reactivity with the chemical composition of the anode and cathode, unlike many of the non-aqueous solvents used traditionally. The material should have low grain boundary resistance for use in solid-state batteries. Ideally, the material should be easy to synthesize and its cost should not be high. Unfortunately, there is no currently known lithium-ion solid electrolyte that meets all of these requirements. For example, Li 10 GeP2S 12 has the state-of-the-art Li conductivity, but does not meet the electrochemical stability requirements and is expensive due to its Ge content. The manufacturing method and structure of the battery require high Li + It is believed that there is a need for environmentally stable composite materials that have electrical conductivity and low activation energy.

[0009] The standard redox potential of Li / Li+ is -3.04 V, so lithium metal is one of the strongest reducing agents available. Thus, Li metal can reduce most of the known cationic species to a lower oxidation state. Because of the strong reducing power of lithium metal in the anode, it is often necessary to use solid Li ions containing cationic moieties different from the lithium ion. + When in contact with a conductor, lithium reduces this cationic species, decreasing its oxidation state and degrading the solid conductor.

[0010] For example, the expression: Li3PS4 The conductor of P in the formula 5+ Therefore, Li + When it comes into contact with Li metal, reduction occurs according to the following equation (Non-Patent Document 1):

[0011] Li3PS4+5Li → P+4Li2S P+3Li → Li3P Similarly, Li 10 GeP2S 12 It has already been reported that when it comes into contact with lithium metal, it decomposes according to the following equation (Non-Patent Document 1).

[0012] Li 10 GeP2S 12 +10Li → 2P+8Li2S+Li4GeS4 P+3Li → Li3P 4Li4GeS4+31Li → 16Li2S+Li 15 Ge4 Li 10 GeP2S 12 Ge 4+ and P 5+ each of which is reduced as described above.

[0013] In another example, the second cation La 3+ and Zr 4+ Contains Li7La3Zr2O 12 When it comes into contact with lithium metal, it undergoes chemical decomposition according to the following chemical formula (Non-Patent Document 1):

[0014] 6Li7La3Zr2O 12 +40Li → 4Zr3O+41Li2O+9La2O3 Zr3O+2Li → Li2O+3Zr La2O3+6Li → 2La+3Li2O Thus, many current and previously known solid Li-ion conductors have stability problems when in contact with a Li metal anode.

[0015] The inventors of the present application have been investigating lithium compounds that can be used in the future as solid Li+ conductors, and previous results of such investigations are disclosed in U.S. Patent No. 6,233,436, filed June 19, 2017, U.S. Patent No. 6,233,436, filed November 7, 2017, U.S. Patent No. 6,233,436, filed June 20, 2018, U.S. Patent No. 6,233,436, filed August 28, 2018, U.S. Patent No. 6,233,436, filed September 26, 2018, U.S. Patent No. 6,233,436, filed September 27, 2018, U.S. Patent No. 6,233,436, filed October 10, 2018, U.S. Patent No. 6,233,436, filed October 9, 2018, and U.S. Patent No. 6,233,436, filed January 31, 2019. However, research continues to discover additional materials with maximum efficiency, high stability, low cost, and easy handling and manufacturing. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] U.S. Application Serial No. 15 / 626,696 [Patent Document 2] US No. 15 / 805,672 [Patent Document 3] U.S. Application No. 16 / 013,495 [Patent Document 4] U.S. Application Serial No. 16 / 114,946 [Patent Document 5] U.S. Application Serial No. 16 / 142,217 [Patent Document 6] U.S. Application Serial No. 16 / 144,157 [Patent Document 7] U.S. Application Serial No. 16 / 153,335 [Patent Document 8] U.S. Application Serial No. 16 / 155,349 [Patent Document 9] U.S. Application Serial No. 16 / 264,294 [Patent Document 10] U.S. Application Serial No. 15 / 597,651 [Patent Document 11] Weppner et al. (US8092941) [Non-patent literature]

[0017] [Non-Patent Document 1] J.Mater.Chem.A,2016,4,3253-3266 [Non-Patent Document 2] Ceder et al., Nature Materials, 14, 2015, 1026-1031 [Non-Patent Document 3] Nature Materials, 14, 2015, 2016 [Non-Patent Document 4] Mo et al., First Principles Study on Electrochemical and Chemical Stability of the Solid Electrolyte-Electrode Interfaces in All-Solid-State Li-ion Batteries (to be published in Journal of Materials Chemistry A) [Non-Patent Document 5] Hautier et al., Inorg. Chem. 2011, 50, 656-663 [Non-Patent Document 6] Bai et al.,ACS Appl.Energy Mater.2018,1,1626-1634 [Non-Patent Document 7] He et al.,Phys.Chem.Chem.Phys.,2015.17,18035 [Non-Patent Document 8] Monatshefte fuer Chemie,100,295-303,1969 [Non-Patent Document 9] Journal of Solid State Chemistry,128,1997,241 [Non-Patent Document 10] Zeitschrift fuer Naturforschung B,50,1995,1061 [Non-Patent Document 11] Journal of Solid State Chemistry 130,1997,90 [Non-Patent Document 12] Journal of Alloys and Compounds,645,2015,S174 [Non-Patent Document 13] Z.Naturforsch.51b,199652 5 Summary of the Invention [Problem to be solved by the invention]

[0018] It is therefore an object of the present application to identify a variety of further materials with high Li-ion conductivity and low electronic conductivity that are suitable as solid electrolytes for lithium-ion batteries and / or as components of protective coating layers or electrode active materials.

[0019] It is a further object of the present application to provide a solid state lithium ion battery and / or lithium metal battery comprising a solid state Li-ion electrolyte membrane and / or electrodes containing said material. [Means for solving the problem]

[0020] Overview of the embodiment These and other objects are provided by embodiments of the present application, a first embodiment of which is a solid-state lithium ion electrolyte comprising a compound represented by formulas (I), (II), (III), and (IV): Li y (M1) x1 KMO6(I) wherein M is selected from the group consisting of Ir, Sb, I, Nb, and W, x1 is a number greater than 0 and less than 6, y is a value such that charge neutrality of the above formula is obtained, and M1 is at least one element different from Li selected from the elements of Groups 1, 2, 13, and transition metals; Li y K 1-x2 (M2) x2 MO6(II) wherein x2 is a number greater than 0 and less than 1, y is a value such that charge neutrality of the above complex formula is obtained, and M2 is at least one element different from K selected from the elements of groups 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and 13; Li y KM 1-x3 (M3) x3 O6(III) In the formula, x3 is a number greater than 0 and less than 1, y is a value such that charge neutrality of the formula is obtained, and M3 is at least one element different from M selected from the elements of groups 1 to 13; and Li6KMO6(V) The present invention relates to a solid-state lithium-ion electrolyte comprising at least one material selected from the group of materials consisting of the compounds of the formula:

[0021] In one aspect of the first embodiment, the lithium ions (Li + ) conductivity is 10 at 300K -3 ~22mS / cm.

[0022] In another aspect of the first embodiment, the activation energy of the compounds of formulae (I) to (IV) is 0.15 to 0.50 eV.

[0023] A second embodiment includes a solid-state lithium battery including an anode, a cathode, and a solid-state lithium-ion electrolyte located between the anode and the cathode, the solid-state lithium-ion electrolyte including at least one material according to the first embodiment and aspects thereof.

[0024] In a particular aspect of the second embodiment, the solid-state lithium battery may be a lithium metal battery or a lithium ion battery.

[0025] In a third embodiment, an electrode is provided having a current collector, an electrode active material, and a coating layer made of a material according to any of formulas (I)-(IV) described in the above-described embodiments and aspects thereof.

[0026] In a fourth embodiment, an electrode is provided having a current collector and an active layer comprising an electrode active material and a material according to any of formulas (I)-(IV) described in the embodiments and aspects thereof described above.

[0027] A fifth embodiment includes a lithium battery including any of the solid electrolytes and / or electrodes according to the embodiments described above.

[0028] The above description provides a general introduction and summary of the present disclosure, and is not intended to limit the disclosure unless otherwise specified. Preferred embodiments and further advantages of the present disclosure can be best understood by referring to the following detailed description and the accompanying drawings. [Brief description of the drawings]

[0029] [Figure 1] This is the crystal structure of Li6KIrO6. [Diagram 2] Calculated XRD analysis for Li6KIrO6 based on Cu-Kα radiation at wavelength 1.54184 Å. [Diagram 3] 3 is a table showing the main peaks and relative intensities for the XRD analysis of FIG. 2. [Figure 4] This is the crystal structure of Li6KNbO6. [Diagram 5] Calculated XRD analysis for Li6KNbO6 based on Cu-Kα radiation at wavelength 1.54184 Å. [Figure 6] 6 is a table showing the main peaks and relative intensities for the XRD analysis of FIG. 5. [Figure 7] This is the crystal structure of Li6KSbO6. [Figure 8]Calculated XRD analysis for Li6KSbO6 based on Cu-Kα radiation at wavelength 1.54184 Å. [Figure 9] 9 is a table showing the main peaks and relative intensities for the XRD analysis of FIG. 8. [Figure 10] This is the crystal structure of Li6KIO6. [Figure 11] Calculated XRD analysis for Li6KIO6 based on Cu-Kα radiation at wavelength 1.54184 Å. [Figure 12] 12 is a table showing the main peaks and relative intensities for the XRD analysis of FIG. 11. [Figure 13] This is the crystal structure of Li6KWO6. [Figure 14] Calculated XRD analysis for Li6KWO6 based on Cu-Kα radiation at wavelength 1.54184 Å. [Figure 15] 15 is a table showing the main peaks and relative intensities for the XRD analysis of FIG. 14. [Figure 16] This is an Arrhenius plot of Li7IrO6 by AIMD simulation. [Figure 17] This is an Arrhenius plot of Li7.33Sn0.33Ir0.67O6 by AIMD simulation. [Figure 18] This is an Arrhenius plot of Li6.17KNb0.83Zr0.17O12 by AIMD simulation. [Figure 19] This is an Arrhenius plot of Li6.33KNb0.67Sn0.33O12 by AIMD simulation. [Figure 20] This is an Arrhenius plot of Li6.5KNb0.5Zr0.5O12 by AIMD simulation. [Figure 21] This is an Arrhenius plot of Li6.67KNb0.33Zr0.67O12 by AIMD simulation. [Figure 22] This is an Arrhenius plot of Li6.33KSb0.67Sn0.33O12 by AIMD simulation. [Figure 23] This is an Arrhenius plot of Li6.33KI0.67Sn0.33O12 by AIMD simulation. [Figure 24] This is an Arrhenius plot of Li6.33KW0.67Sn0.33O12 by AIMD simulation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Description of the Preferred Embodiments Throughout this description, the terms "electrochemical cell" and "battery" may be used interchangeably unless the context of the description clearly distinguishes between electrochemical cells and batteries. Additionally, the terms "solid electrolyte" and "solid ionic conductor" may be used interchangeably unless a clear distinction is made between the two.

[0031] In the chemical formulas provided, the term "less than" refers to a value less than the full value of the number shown. Thus, "less than" may refer to a value up to the number shown multiplied by 0.9. For example, if the number shown is 3, then a number less than 3 may be 2.7. The term "greater than 0" may refer to an existing positive value, and such a value may be as small as 0.01.

[0032] Valid Li + The structural features of the conductive crystal lattice were reported by Ceder et al. + Li, an ionic conductor 10 GeP2S 12 and Li7P3S 11 has been described in which it has been shown that the sulfur sublattices of these two materials match very well with the bcc lattice structure. Furthermore, adjacent tetrahedrally coordinated Li + Li between lattice sites + It has also been shown that ion hopping provides the pathway with the lowest activation energy.

[0033] The present inventors are investigating new lithium composite compounds to identify materials with properties that can serve as solid electrolytes in solid-state lithium batteries. In this ongoing research and effort, the present inventors have developed and implemented a methodology to identify composite materials that have chemical and structural properties that the present inventors have indicative of lithium ion conductivity and that are suitable for use as solid electrolytes for lithium ion batteries.

[0034] To qualify as a solid electrolyte for practical applications, a material must meet several specific criteria. First, it must be stable at room temperature, typically 10 -6 First, the material should exhibit a desirable Li-ion conductivity of 0.1 S / cm or higher. Second, the material should have good stability against chemical, electrochemical, and thermal decomposition. Third, the material should have low grain boundary resistance for use in solid-state batteries. Fourth, the material should be easy to synthesize and its cost should not be high.

[0035] To meet the criteria of this methodology and qualify as a solid electrolyte for practical applications, the material must be able to withstand temperatures typically of 10 -6 It is required to exhibit a desirable Li-ion conductivity of greater than or equal to 1.5 S / cm. Therefore, a first-principles molecular dynamics simulation study was applied to calculate the diffusivity of Li-ions in the lattice structure of selected potassium lithium tantalate materials. To speed up the simulation, the calculations were performed at high temperatures and the effect of excess Li or Li vacancies was considered. Aliovalent substitution of cations or anions may be evaluated to create excess Li or Li vacancies. Thus, partial substitution of K or Ta with aliovalent cationic species, for example, creates Li vacancies while simultaneously compensating for charge neutrality with Li vacancies or excess Li.

[0036] The diffusion coefficient at 300K was calculated by equation (I). D=D0exp(-E a / k b T) Equation (I) In the formula, D0, E a , and k b are the frequency factor, activation energy, and Boltzmann constant, respectively. The conductivity is related to the calculated diffusivity according to equation (II):

[0037] σ=D 300 ρe 2 / k b T Equation (II) where ρ is the volume density of Li ions and e is the unit charge.

[0038] The anion lattice of Li-ion conductors has been shown to conform to a specific lattice type (see Non-Patent Document 3). + The anion lattice of the ionic conductor is Li, which is known to have high conductivity. + It is compared to the anion lattice of an ionic conductor.

[0039] Therefore, selected lithium potassium iridium oxide compounds were compared with Li-containing compounds reported in the Inorganic Crystal Structure Database (FIZ Karlsruhe ICSD - https: / / icsd.fiz-karlsruhe.de) and their lattices were matched with known Li-ion conductors by comparative evaluation using the anion lattice matching method described in co-pending patent application WO 2017 / 052364, filed May 17, 2017, which the inventors developed for this purpose.

[0040] Using the anion lattice matching method described in co-pending US Patent No. 5,999,943, the atomic coordinate set of the lattice structure of the compound may be transformed into a coordinate set of an anion-only lattice. The anions of this lattice are replaced with the anions of a comparison material, and the resulting unit cell is rescaled. X-ray diffraction data of the transformed anion-only lattice may be simulated, and an n x 2 matrix may be generated from the simulated diffraction data. From this n x 2 matrix, quantitative structural similarity values ​​may be obtained.

[0041] The purpose of anion lattice matching is to obtain high Li +The goal of this study is to further identify compounds that are most likely to exhibit solid Li conductivity. + It is expected to be suitable as a conductor.

[0042] First-principles molecular dynamics (AIMD) simulations were then applied to predict the conductivity of the target lithium potassium tantalate. The initial structure was statically relaxed and set at an initial temperature of 100 K. The structure was then heated at a constant rate over 2 ps to the target temperature (750–1150 K) by velocity scaling. The total time for the AIMD simulations ranged from 200 to 400 ps. The conductivity of Li at different temperatures in the range of 750–1150 K was calculated. + The diffusivity follows an Arrhenius type relationship.

[0043] In their research, the inventors have found that compounds based on aliovalent substitution of Li6KIrO6 have properties of great interest as lithium ion conductors. The chemical compositions of interest were further evaluated for structural stability based on evaluating the phase equilibrium of a given phase of the studied composition by analyzing the composition phase diagram constructed using the pymatgen computational package. The phase equilibrium of a given solid electrolyte was determined by constructing the convex hull of the energies of all relevant phases in the composition phase diagram. The energy minimum E eq Phase equilibria at composition C, corresponding to (C), were identified by comparing the energies of all relevant phases in the composition space. The phase stability of the investigated phases was calculated as the decomposition energy ΔE of a given phase according to Eq. III. D and its phase equilibrium was evaluated.

[0044] ΔE D (phase)=E eq (C)-E(phase) (Equation III) ΔE D is a negative number indicating the energy value above the envelope. DA β-direction constant of −50 or less was deemed to be sufficiently stable to justify AIMD computational studies. The method for this analysis is described by Mo et al. (Non-Patent Document 4), the disclosure of which is incorporated herein by reference.

[0045] Suitable elements for aliovalent substitution may be selected using the ion substitution probability determined by the method described by Hautier et al. (Non-Patent Document 5), in which candidate dopants may be selected by an ion substitution probability model built on data mining of all known inorganic crystalline materials. Dopants that are expected to be able to create vacancies or interstitials in a particular material were included. Structures with energetically unfavorable dopants may be filtered out and excluded during phase stability calculations. The configurations of sublattices, dopants, and vacancies or interstitials were determined by the computational methods described herein. Such methods have been reported, for example, in the following reports: Non-Patent Document 6 Non-Patent Document 7 It is described in.

[0046] By applying equation (I) above, the diffusivity at 300K can be determined, and then the conductivity can be determined using the relationship between conductivity and diffusivity in equation (II). Table 1 shows the activation energies and room temperature conductivities determined for a series of compounds studied. The Li + Arrhenius plots of the diffusivity are shown in Figures 4 to 20. The activation energies and lithium ion conductivities determined for these materials confirm that these materials are suitable materials for the solid electrolyte and Li-ion conductor according to the present disclosure.

[0047] [Table 1]

[0048] Thus, in one embodiment, the present disclosure provides a solid-state lithium ion electrolyte comprising: Liy (M1) x1 KMO6(I) wherein M is selected from the group consisting of Ir, Sb, I, Nb, and W, x1 is a number greater than 0 and less than 6, y is a value such that charge neutrality of the above formula is obtained, and M1 is at least one element different from Li selected from the elements of Groups 1, 2, 13, and transition metals; Li y K 1-x2 (M2) x2 MO6(II) wherein x2 is a number greater than 0 and less than 1, y is a value such that charge neutrality of the above complex formula is obtained, and M2 is at least one element different from K selected from the elements of groups 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and 13; Li y KM 1-x3 (M3) x3 O6(III) In the formula, x3 is a number greater than 0 and less than 1, y is a value such that charge neutrality of the formula is obtained, and M3 is at least one element different from M selected from the elements of Groups 1 to 13; The present invention provides a solid-state lithium-ion electrolyte comprising at least one material selected from the group of materials consisting of the compounds

[0049] The compounds of formulas (I) to (III) are represented by the general formula (IV): Li6KMO6(IV) wherein at least one of Li, K, and M is aliovalently substituted as described above. The compound of formula (IV) and the materials of formulas (I), (II), and (III) comprise a crystal lattice having a trigonal structure.

[0050] The crystal structure of Li6KIrO6 is shown in Figure 1. The calculated X-ray diffraction analysis for Li6KIrO6, obtained based on Cu-Kα radiation of wavelength 1.54184 Å, is shown in Figure 2, and a table showing the main peak positions (2θ) is shown in Figure 3.

[0051] The crystal structure of Li6KNbO6 is shown in Figure 4. The calculated X-ray diffraction analysis for Li6KNbO6, obtained based on Cu-Kα radiation of wavelength 1.54184 Å, is shown in Figure 5, and a table showing the main peak positions (2θ) is shown in Figure 6.

[0052] The crystal structure of Li6KSbO6 is shown in Figure 7. The calculated X-ray diffraction analysis for Li6KSbO6, obtained based on Cu-Kα radiation of wavelength 1.54184 Å, is shown in Figure 8, and a table showing the main peak positions (2θ) is shown in Figure 9.

[0053] The crystal structure of Li6KIO6 is shown in Figure 10. The calculated X-ray diffraction analysis for Li6KIO6, obtained based on Cu-Kα radiation of wavelength 1.54184 Å, is shown in Figure 11, and a table showing the main peak positions (2θ) is shown in Figure 12.

[0054] The crystal structure of Li6KWO6 is shown in Figure 13. The calculated X-ray diffraction analysis for Li6KWO6, obtained based on Cu-Kα radiation of wavelength 1.54184 Å, is shown in Figure 14, and a table showing the main peak positions (2θ) is shown in Figure 15.

[0055] The inventors have found that the resulting doped materials according to formulas (I)-(I-III) retain the crystal structure of the base compounds (I-IV) and have activation energies and conductivities associated with the base compounds. Based on the measurement methods described above, the lithium ion (Li + ) conductivity is 10 at 300K -3The activation energy of the materials of formula (I), (II), (III), and (IV) may be 0.15 to 0.50 eV, preferably 0.25 eV to 0.40 eV.

[0056] The synthesis of the compounds according to the embodiments described above can be carried out by solid-phase reaction of selected precursor materials (stoichiometric amounts). Examples of solid-phase synthesis methods are described, for example, in each of the following papers: i) 8, ii) 9, iii) 10, iv) 11, v) 12, vi) 13, and vii) 11. Those skilled in the art are well able to use such methods to prepare the composite compounds according to the embodiments disclosed herein.

[0057] In further embodiments, the present application includes solid-state lithium-ion batteries that include the solid electrolytes described above. Solid-state batteries according to these embodiments, including metal-metal solid-state batteries, may have higher charge / discharge rate capabilities and power densities than conventional batteries, and promise to achieve high power and energy densities.

[0058] Thus, in a further embodiment, there is provided a solid-state battery comprising an anode, a cathode, and a solid-state lithium-ion electrolyte between the anode and the cathode according to embodiments described above.

[0059] The anode may be any anode structure conventionally used in lithium ion batteries. Generally, such materials are +Ions can be inserted and extracted. Examples of anode active materials can include graphite, hard carbon, lithium titanate (LTO), tin / cobalt alloy, and silicon / carbon composite. In one aspect, the anode can include a current collector and a coating of lithium ion active material on the current collector. Standard current collector materials include, but are not limited to, aluminum, copper, nickel, stainless steel, carbon, carbon paper, and carbon cloth. In one aspect with the solid lithium ion conductive material advantageously described in the first and second embodiments, the anode can be lithium metal or lithium metal alloy, optionally coated on a current collector. In one aspect, the anode can be a sheet of lithium metal that serves as both the active material and the current collector.

[0060] The cathode structure may be any of those conventionally used in lithium ion batteries, including, but not limited to, lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium iron phosphate (LiFePO4), and complex lithium metal oxides such as lithium nickel manganese cobalt oxide. Other active cathode materials may include elemental sulfur and complex metal sulfides. The cathode may include current collectors such as copper, aluminum, and stainless steel.

[0061] In one embodiment, the active cathode material may be a transition metal, preferably silver or copper. Such transition metal based cathodes may not include a current collector.

[0062] In a further set of embodiments, electrodes containing the solid electrolyte material of formulas (I)-(IV) are also disclosed. Thus, in preparing the electrodes, the active material described above may be physically mixed with the solid electrolyte material before application to a current collector, or the solid electrolyte material may be applied as a coating layer over the applied active material. In either embodiment, the presence of a lithium ion superconductor on or in the electrode structure may improve the performance of the electrode and may serve to protect conventional solid electrolytes, especially when applied as a coating layer.

[0063] Thus, one embodiment of the present disclosure includes a cathode comprising a current collector and a layer of cathode active material applied to the current collector, where at least one of the following is true: i) the cathode active material applied to the current collector is a physical mixture containing at least one of the solid electrolyte materials of formulas (I)-(IV) described above; ii) the layer of cathode active material applied to the current collector is coated with a layer comprising at least one of the solid electrolyte materials of formulas (I)-(IV). Cathodes where both elements i) and ii) are true are also included in the present disclosure.

[0064] In a related embodiment, the disclosure includes an anode comprising a current collector and a layer of anode active material applied to the current collector, where at least one of the following is true: i) the anode active material applied to the current collector is a physical mixture containing at least one of the solid electrolyte materials of Formulas (I)-(IV) described above; ii) the layer of anode active material applied to the current collector is coated with a layer comprising at least one of the solid electrolyte materials of Formulas (I)-(IV).

[0065] A battery comprising a cathode described in any of the above embodiments, an anode described in any of the above embodiments, or both an anode and a cathode according to the above embodiments is also an embodiment of the present disclosure.

[0066] The above description is presented to enable one of ordinary skill in the art to make and use the invention, and is provided in the context of a particular application and its requirements. Various modifications to the preferred embodiment will be apparent to those skilled in the art, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the invention. Thus, the present invention is not intended to be limited to the embodiments described, but is to be accorded the widest scope consistent with the principles and features disclosed herein. In this regard, certain embodiments within the scope of the invention may not represent all of the benefits of the invention broadly considered.

Claims

1. A solid-state lithium ion electrolyte, Formula (III): Li y KM 1-x3 (M3) x3 O 12 (III) wherein M is selected from the group consisting of Sb, I, Nb, and W; x3 is a number greater than 0 and less than 1; y is a value such that charge neutrality is obtained in the formula; M3 is an aliovalent substitute for M and is at least one element different from M selected from the elements of groups 1 to 13, and is Sn or Zr; The material comprises a compound of The lithium ion (Li + ) Conductivity is 10 at 300K -3 .about.22 mS / cm, solid-state lithium-ion electrolyte.

2. A solid-state lithium ion electrolyte, Formula (IVa): Li 6 KIrO 6 (Iva) and an X-ray diffraction analysis obtained on said material based on Cu-Kα radiation of wavelength 1.54184 Å shows the following: 【Table 1】 A solid lithium ion electrolyte comprising a peak having a relative intensity of 10 or more relative to an intensity of 100 of the maximum peak.

3. A solid-state lithium ion electrolyte, Formula (IVb): Li 6 KNbO 6 (IVb) and an X-ray diffraction analysis obtained on said material based on Cu-Kα radiation of wavelength 1.54184 Å shows the following: 【Table 2】 A solid lithium ion electrolyte comprising a peak having a relative intensity of 10 or more relative to an intensity of 100 of the maximum peak.

4. A solid-state lithium ion electrolyte, Formula (IVc): Li 6 KSbO 6 (IVc) and an X-ray diffraction analysis obtained on said material based on Cu-Kα radiation of wavelength 1.54184 Å shows the following: 【Table 3】 A solid lithium ion electrolyte comprising a peak having a relative intensity of 10 or more relative to an intensity of 100 of the maximum peak.

5. A solid-state lithium ion electrolyte, Formula (IVd): Li 6 K.I.O. 6 (I) and an X-ray diffraction analysis obtained on said material based on Cu-Kα radiation of wavelength 1.54184 Å shows the following: 【Table 4】 2. The solid lithium ion electrolyte of claim 1, further comprising a peak having a relative intensity of 10 or more relative to an intensity of 100 of the maximum peak of said solid lithium ion electrolyte.

6. A solid-state lithium ion electrolyte, Formula (IVe): fi) 6 .﯀ 6 (()) and an X-ray diffraction analysis obtained on said material based on Cu-Kα radiation of wavelength 1.54184 Å shows the following: 【Table 5】 A solid lithium ion electrolyte comprising a peak having a relative intensity of 10 or more relative to an intensity of 100 of the maximum peak.

7. The lithium ion (Li + ) Conductivity is 10 at 300K -3 The solid lithium ion electrolyte according to any one of claims 2 to 6, wherein the solid lithium ion electrolyte has a conductivity of up to 22 mS / cm.

8. The solid lithium ion electrolyte according to any one of claims 1 to 6, wherein the activation energy of the material is 0.15 to 0.50 eV.

9. The solid state lithium ion electrolyte of any one of claims 1 to 6, wherein the material comprises a trigonal crystal structure.

10. 1. A solid-state lithium battery, comprising: An anode; A cathode; a solid-state lithium ion electrolyte located between the anode and the cathode; The solid lithium ion electrolyte is the solid lithium ion electrolyte according to any one of claims 1 to 6. A solid lithium battery.

11. 11. The solid-state lithium battery of claim 10, wherein the solid-state lithium battery is a lithium metal battery or a lithium ion battery.

12. 1. An electrode for a solid-state lithium battery, comprising: A current collector; an electrode active layer on the current collector; 7. An electrode, wherein the electrode active layer comprises the solid-state lithium ion electrolyte according to claim 1.

13. 1. An electrode for a solid-state lithium battery, comprising: A current collector; an electrode active layer on the current collector; a coating layer on the electrode active layer; An electrode, wherein a coating layer on the electrode active layer comprises the solid lithium ion electrolyte according to any one of claims 1 to 6.

14. 13. A solid-state lithium battery comprising the electrode of claim 12, wherein the solid-state lithium battery is a lithium ion battery or a lithium metal battery.

15. 14. A solid-state lithium battery comprising the electrode of claim 13, wherein the solid-state lithium battery is a lithium ion battery or a lithium metal battery.

Citation Information

Patent Citations

  • Compounds with mixed anions as solid Li-ion conductors

    US10511054B2

  • Lithium metal sulfides as lithium super-ionic conductors

    US10854916B2

  • Lithium bismuth oxide compounds as Li super-ionic conductor, solid electrolyte, and coating layer for Li metal battery and Li-ion battery

    US11152640B2

  • Lithium metal nitrides as lithium super-ionic conductors

    US11581572B2

  • System and method to quantify structural properties and predict bulk properties of inorganic materials

    US20180336288A1