Decorative film, decorative molded body, decorative panel, and electronic device
A decorative film with multiple optical reflective layers and cholesteric liquid crystal compounds achieves high brightness, chroma, and rich color changes, addressing the limitations of conventional decorative technologies.
Patent Information
- Application Number
- JP2022550638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-17
- Filing Date
- 2021-09-17
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-09-17
AI Technical Summary
Existing decorative films and molded bodies lack high brightness, high chroma, and rich color changes depending on the viewing direction, with conventional methods such as hot stamp foils and cholesteric liquid crystal layers providing insufficient color variation.
A decorative film with multiple optical reflective layers, each having different diffuse reflectance, and optionally including a printed layer between them, utilizing cholesteric liquid crystal compounds to achieve high glitter and rich color changes based on viewing angle.
The solution provides a decorative film with high brightness, high chroma, and significant color changes based on viewing direction, enhancing design impact and visual appeal.
Smart Images

Figure 0007583055000017 
Figure 0007583055000018 
Figure 0007583055000019
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a decorative film, a decorated molded body, a decorated panel, and an electronic device. [Background technology]
[0002] A decorated molded body is known in which a decorative film is placed on the surface of a resin molded body to color the surface of the resin molded body in a desired hue or to provide a desired pattern on the surface of the resin molded body. The decorated molded body is obtained, for example, by placing a decorative film in a mold in advance and then injection molding a base resin into the mold, and has a structure in which the decorative film is integrated with the surface of the resin molded body. The process of placing a decorative film in a mold in advance and then injection molding the base resin is generally referred to as film insert molding or simply insert molding. The decorated molded body may also be manufactured by attaching a decorative film to the molded body after molding.
[0003] As a conventional hot stamp foil, JP 2001-105795 A describes a hot stamp foil characterized in that a cholesteric liquid crystal polymer layer having a selective reflection wavelength range in visible light is laminated as a transfer layer. In addition, JP 2017-97114 A describes improving retroreflectivity by subjecting the cholesteric liquid crystal layer to uneven processing. Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a decorative film that has high glitter, high saturation, and rich color variation depending on the viewing direction. Another problem to be solved by another embodiment of the present disclosure is to provide a decorated molded body using the above decorative film. Another problem to be solved by another embodiment of the present disclosure is to provide a decorative panel using the above decorative film. A problem to be solved by another embodiment of the present disclosure is to provide an electronic device using the above decorative panel. [Means for solving the problem]
[0005] The present disclosure includes the following aspects. <1> The optical reflecting layer has a base material and an optical reflection layer that exhibits color by optical interference or structural color, and at least two optical reflection layers are laminated. A decorative film in which the diffuse reflectance of each optical reflection layer is different from each other, or a printed layer is laminated between each optical reflection layer. <2> At least one of the optical reflection layers is a layer containing a cholesteric liquid crystal compound. <1> The decorative film according to claim 1. <3> <1> or <2> A decorated molded body comprising the decorative film according to claim 1. <4> <1> or <2> A decorative panel comprising the decorative film according to claim 1. <5> <4> An electronic device comprising the decorative panel according to claim 1. Effect of the Invention
[0006] According to one embodiment of the present disclosure, it is possible to provide a decorative film that has high glitter, high saturation, and rich color variation depending on the viewing direction. According to another embodiment of the present disclosure, a decorated molded body using the above decorative film is provided. According to another embodiment of the present disclosure, a decorative panel using the above decorative film is provided. According to another embodiment of the present disclosure, there is provided an electronic device using the above-mentioned decorative panel. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a decorative film according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a decorative film according to the present disclosure. [Diagram 3]FIG. 3 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. [Figure 6] FIG. 6 is a schematic cross-sectional view showing an example of a decorative panel according to the present disclosure. [Figure 7] FIG. 7 is a schematic plan view showing an example of a transparent body having a concave-convex structure according to the present disclosure. [Figure 8] FIG. 8 is a schematic perspective view of a transparent body having a concave-convex structure according to the present disclosure. [Figure 9] FIG. 9 is a schematic diagram showing a black image pattern as an example of a printed layer according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the decorative film, the decorative molded body, the decorative panel, and the electronic device according to the present disclosure will be described. However, the present disclosure is not limited to the following embodiments, and can be implemented with appropriate modifications within the scope of the purpose of the present disclosure. When describing the embodiments of the present disclosure with reference to the drawings, the description of overlapping components and symbols may be omitted. Components indicated by the same symbols in the drawings are the same components. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.
[0009] In the present disclosure, when a group (atomic group) is represented without indicating whether it is substituted or unsubstituted, it includes both those that have no substituent and those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituent (an unsubstituted alkyl group) but also an alkyl group that has a substituent (a substituted alkyl group). In the present disclosure, "light" means actinic rays or radiation. In the present disclosure, "actinic rays" or "radiation" refers to, for example, the emission line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light (EUV light: extreme ultraviolet light), X-rays, and electron beams (EB). Unless otherwise specified, "exposure" in this disclosure includes not only exposure to the emission line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light, X-rays, EUV light, and the like, but also exposure to particle beams such as electron beams and ion beams. In this disclosure, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0010] In this disclosure, (meth)acrylate refers to acrylate and methacrylate, and (meth)acrylic refers to acrylic and methacrylic. In the present disclosure, the weight average molecular weight (Mw) of the resin component, the number average molecular weight (Mn) of the resin component, and the dispersity (also referred to as molecular weight distribution) (Mw / Mn) of the resin component are defined as polystyrene-equivalent values measured using a Gel Permeation Chromatography (GPC) device (HLC-8120GPC manufactured by Tosoh Corporation) (solvent: tetrahydrofuran, flow rate (sample injection amount): 10 μL, column: TSK gel Multipore HXL-M manufactured by Tosoh Corporation, column temperature: 40° C., flow rate: 1.0 mL / min, detector: refractive index detector).
[0011] In the present disclosure, the amount of each component in a composition means, when a plurality of substances corresponding to each component are present in the composition, the total amount of the corresponding substances present in the composition, unless otherwise specified. In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In the present disclosure, the term "total solid content" refers to the total mass of the components excluding the solvent from the entire composition of the composition. Also, the term "solid content" refers to the components excluding the solvent from the entire composition of the composition, and may be, for example, solid or liquid at 25°C. Also, in the present disclosure, combinations of two or more preferred aspects are more preferred aspects.
[0012] (Decorative film) The decorative film according to an embodiment of the present disclosure has a substrate and an optical reflection layer that develops color by optical interference or structural color, and at least two or more optical reflection layers are laminated. Furthermore, in the decorative film according to an embodiment of the present disclosure, the optical reflection layers have different diffuse reflectances from each other, or a printed layer is laminated between the optical reflection layers.
[0013] The use of the decorative film according to one embodiment of the present disclosure is not particularly limited, and can be used, for example, to decorate electronic devices (e.g., wearable devices and smartphones), home appliances, audio products, computers, displays, in-vehicle products, watches, accessories, optical components, doors, window glass, and building materials. In particular, the decorative film according to one embodiment of the present disclosure can be suitably used to decorate electronic devices (e.g., wearable devices and smartphones). In addition, the decorative film according to one embodiment of the present disclosure is also excellent in three-dimensional moldability, and is therefore suitable as a decorative film for molding used in molding such as three-dimensional molding and insert molding, and is more suitable as a decorative film for three-dimensional molding.
[0014] Conventionally, for example, printing, painting, deposition, or plating has been used for surface decoration used in items such as home appliances, electronic devices, and mobile phones. However, for example, from the viewpoints of functionality, environmental load, and reupholstery, decoration techniques using decorative films have come to be widely used. On the other hand, new designs are required due to the expansion of user preferences. In particular, changes in color (e.g., color and subtle shades) depending on the viewing angle are one of the designs that are required, and the introduction of decoration techniques to obtain such designs has been required. In addition, JP 2001-105795 A describes a hot stamp foil in which a cholesteric liquid crystal polymer layer is laminated as a transfer layer, but the color change depending on the viewing direction may be insufficient. In addition, JP 2017-97114 A describes improving retroreflectivity by applying uneven processing to a cholesteric liquid crystal layer, but does not mention its use as a decorative film and its effects.
[0015] As a result of intensive research, the inventors have found that a decorative film having the above-mentioned configuration provides a decorative film that has high brilliance, high saturation, and a wide range of color changes depending on the viewing direction (e.g., useful as a material for decorated molded bodies).
[0016] The decorative film of the present disclosure has a plurality of optical reflection layers laminated thereon. By laminating a plurality of optical reflection layers, a decorative film having high glittering properties can be provided.
[0017] In one embodiment, the decorative film according to the present disclosure has optical reflective layers each having a different diffuse reflectivity. The different diffuse reflectivity allows the reflected color of each optical reflective layer to be viewed independently, and provides a highly impactful design with rich hues (i.e., high saturation) and a large color change depending on the viewing angle (i.e., a wide range of color changes depending on the viewing direction).
[0018] In another aspect, the decorative film according to an embodiment of the present disclosure has a print layer between each of the optical reflection layers of the plurality of optical reflection layers. By having the print layer, the print layer absorbs the complementary color light transmitted from the upper optical reflection layer, and the color of each optical reflection layer can be visually recognized without mixing with the lower optical reflection layer. The combination of the color of the print layer and the reflected color expands the range of hue expression, and as a result, a design with a large color change depending on the viewing angle (i.e., a rich color change depending on the viewing direction) and a rich color (i.e., high saturation) can be provided.
[0019] In the present disclosure, "rich in color variation depending on the viewing direction" means, for example, that there is a large change in color when the object is viewed from a perpendicular angle to the surface direction of the object and when the object is viewed from an angle of 45 degrees to the surface direction of the object. The above-mentioned effect is preferable in that it can improve the impact of the design.
[0020] The decorative film according to the present disclosure will be described in detail below.
[0021] <Base material> The decorative film according to one embodiment of the present disclosure has a substrate. The substrate may be a support. As the substrate, for example, a substrate conventionally known as a substrate used for molding such as three-dimensional molding and insert molding can be used without particular limitation, and may be appropriately selected according to suitability for molding. In addition, the shape and material of the substrate are not particularly limited, and may be appropriately selected as desired. From the viewpoint of ease of molding and chipping resistance, the substrate is preferably a resin substrate, more preferably a resin film.
[0022] Specific examples of the substrate include resin films containing resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), acrylic resin, urethane resin, urethane-acrylic resin, polycarbonate (PC), acrylic-polycarbonate resin, triacetyl cellulose (TAC), cycloolefin polymer (COP), and acrylonitrile / butadiene / styrene copolymer resin (ABS resin). Among these, the substrate is preferably polyethylene terephthalate (PET), acrylic resin, polycarbonate, or polypropylene from the viewpoint of moldability and strength, and more preferably polyethylene terephthalate (PET), acrylic resin, or polycarbonate. The substrate may also be a laminated resin substrate of two or more layers. For example, a laminated film containing an acrylic resin layer and a polycarbonate layer is preferably used.
[0023] The substrate may contain additives as necessary. Examples of such additives include lubricants (e.g., mineral oil, hydrocarbons, fatty acids, alcohols, fatty acid esters, fatty acid amides, metal soaps, natural waxes, and silicones), inorganic flame retardants (e.g., magnesium hydroxide and aluminum hydroxide), halogen-based organic flame retardants, phosphorus-based organic flame retardants, organic or inorganic fillers (e.g., metal powder, talc, calcium carbonate, potassium titanate, glass fiber, carbon fiber, and wood powder), antioxidants, ultraviolet inhibitors, lubricants, dispersants, coupling agents, foaming agents, colorants, and engineering plastics other than the above-mentioned resins. Examples of engineering plastics include polyolefins, polyesters, polyacetals, polyamides, and polyphenylene ethers.
[0024] The substrate may be a commercially available product. Examples of commercially available products include Technoloy (registered trademark) series (acrylic resin film or acrylic resin / polycarbonate resin laminated film, manufactured by Sumitomo Chemical Co., Ltd.), ABS film (manufactured by Okamoto Corporation), ABS sheet (manufactured by Sekisui Seikei Kogyo Co., Ltd.), Teflex (registered trademark) series (PET film, manufactured by Teijin Film Solutions Co., Ltd.), Lumirror (registered trademark) easy moldable type (PET film, manufactured by Toray Industries, Inc.), and Pure Thermo (polypropylene film, manufactured by Idemitsu Unitech Co., Ltd.).
[0025] The thickness of the substrate is determined according to, for example, the use and handling of the molded product to be produced, and is not particularly limited.The lower limit of the thickness of the substrate is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, and particularly preferably 30 μm or more.The upper limit of the thickness of the substrate is preferably 500 μm or less, more preferably 200 μm or less, and particularly preferably 100 μm or less.
[0026] <Optical reflective layer> A decorative film according to an embodiment of the present disclosure has an optical reflection layer that develops color by optical interference or structural color, and at least two optical reflection layers are laminated.
[0027] Examples of the optical reflection layer include a layer containing a cholesteric liquid crystal compound (hereinafter also referred to as a "cholesteric liquid crystal layer"), a layer containing flat metal particles, an optical multilayer film, a metal thin film, and a layer containing a chromic material. Among the above-mentioned optical reflection layers, from the viewpoint of easily obtaining brilliance, a layer containing a cholesteric liquid crystal layer, a metal thin film (hereinafter sometimes referred to as a "mirror layer"), or an optical multilayer film is preferred, a cholesteric liquid crystal layer or a metal thin film is more preferred, and a cholesteric liquid crystal layer is particularly preferred. In addition, from the viewpoint of easily obtaining brilliance, at least one layer of the optical reflection layers is preferably a cholesteric liquid crystal layer.
[0028] The material of the metal thin film is preferably a metal that is difficult to oxidize, such as In, Ag, or Zn, and the thin film layer is preferably formed using a gas phase method such as deposition or sputtering process. In is more preferable from the viewpoint of high brightness.
[0029] <<Liquid crystal composition>> The cholesteric liquid crystal layer is a layer containing a cholesteric liquid crystal compound, and is formed by curing a liquid crystal composition. The liquid crystal composition is a composition containing a cholesteric liquid crystal compound. As the cholesteric liquid crystal compound used in the present disclosure, it is preferable to use at least a cholesteric liquid crystal compound having one ethylenically unsaturated group or one cyclic ether group from the viewpoint of molding processability and temporary support peelability. The liquid crystal composition for forming the cholesteric liquid crystal layer contains, for example, a cholesteric liquid crystal compound having one ethylenically unsaturated group or one cyclic ether group in an amount of 25% by mass or more based on the total solid content of the liquid crystal composition, and may further contain other components (for example, a chiral agent, an alignment control agent, a polymerization initiator, and an alignment assistant).
[0030] -Cholesteric liquid crystal compound having one ethylenically unsaturated group or one cyclic ether group- The liquid crystal composition preferably contains, as a cholesteric liquid crystal compound, 25% by mass or more of a cholesteric liquid crystal compound having one ethylenically unsaturated group or one cyclic ether group (hereinafter also referred to as a "specific liquid crystal compound").
[0031] The ethylenically unsaturated group in the specific liquid crystal compound is not particularly limited, and may be, for example, a (meth)acryloxy group, a (meth)acrylamide group, a vinyl group, a vinyl ester group, or a vinyl ether group. From the viewpoint of reactivity, the ethylenically unsaturated group is preferably a (meth)acryloxy group, a (meth)acrylamide group, or an aromatic vinyl group, more preferably a (meth)acryloxy group or a (meth)acrylamide group, and particularly preferably a (meth)acryloxy group.
[0032] The cyclic ether group in the specific liquid crystal compound is not particularly limited, but from the viewpoint of reactivity, it is preferably an epoxy group or an oxetanyl group, and particularly preferably an oxetanyl group.
[0033] From the viewpoints of reactivity and suppression of changes in reflectance and color after molding, the specific liquid crystal compound is preferably a cholesteric liquid crystal compound having one ethylenically unsaturated group. More preferably, the liquid crystal composition contains 25% by mass or more of the cholesteric liquid crystal compound having one ethylenically unsaturated group based on the total solid content of the liquid crystal composition.
[0034] The specific liquid crystal compound may have both an ethylenically unsaturated group and a cyclic ether group in one molecule, but the number of ethylenically unsaturated groups is one, or the number of cyclic ether groups is one. In addition, as long as the number of ethylenically unsaturated groups in the specific liquid crystal compound is one, for example, the specific liquid crystal compound may be a compound having one ethylenically unsaturated group and one or more cyclic ether groups.
[0035] When the liquid crystal composition contains a cholesteric liquid crystal compound having one ethylenically unsaturated group, the liquid crystal composition preferably contains a radical polymerization initiator, and more preferably contains a photoradical polymerization initiator, from the viewpoint of suppressing changes in reflectance and color after molding.
[0036] When the liquid crystal composition contains a cholesteric liquid crystal compound having one cyclic ether group, from the viewpoint of suppressing changes in reflectance and color tone after molding, the liquid crystal composition preferably contains a cationic polymerization initiator, and more preferably contains a photocationic polymerization initiator.
[0037] From the viewpoint of suppressing changes in reflectance and color after molding, the specific liquid crystal compound is preferably a cholesteric liquid crystal compound having both an ethylenically unsaturated group and a cyclic ether group, and more preferably a cholesteric liquid crystal compound having one ethylenically unsaturated group and one cyclic ether group.
[0038] The specific liquid crystal compound may be a rod-shaped liquid crystal compound or a discotic liquid crystal compound as long as it has a liquid crystal structure. The specific liquid crystal compound is preferably a rod-shaped liquid crystal compound from the viewpoints of ease of adjusting the pitch of the helical structure in the cholesteric liquid crystal layer and suppressing changes in reflectance and color after molding.
[0039] As the rod-shaped liquid crystal compound, azomethines, azoxys, cyanobiphenyls, cyanophenyl esters, benzoates, cyclohexane carboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, or alkenylcyclohexylbenzonitriles are preferably used. In addition to the above-mentioned low molecular weight liquid crystal compounds, liquid crystalline polymer compounds can also be used. As the rod-shaped liquid crystal compound, the following compounds are described in "Makromol. Chem., Vol. 190, p. 2255 (1989)"; "Advanced Materials 5, p. 107 (1993)”, U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, WO 1995 / 022586, WO 1995 / 024455, WO 1997 / 000600, WO 1998 / 023580, WO 1998 / 052905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and JP-A-2001-328973, compounds having one ethylenically unsaturated group or one cyclic ether group can be used. Furthermore, as the rod-shaped liquid crystal compound, for example, a compound having one ethylenically unsaturated group or one cyclic ether group among the compounds described in JP-A-11-513019 and JP-A-2007-279688 can be preferably used. The cholesteric liquid crystal layer is more preferably a layer in which the orientation of the rod-shaped liquid crystal compound is fixed by polymerization.
[0040] As the discotic liquid crystal compound, for example, among the compounds described in JP-A-2007-108732 or JP-A-2010-244038, a compound having one ethylenically unsaturated group or one cyclic ether group can be preferably used.
[0041] Specific examples of the specific liquid crystal compound include, but are not limited to, the compounds shown below.
[0042] [ka]
[0043] [ka]
[0044] [ka]
[0045] [ka]
[0046] [ka]
[0047] [ka]
[0048] [ka]
[0049] The liquid crystal composition may contain one specific liquid crystal compound alone or two or more specific liquid crystal compounds. The content of the specific liquid crystal compound is preferably 25% by mass or more based on the total solid content of the liquid crystal composition. When the content of the specific liquid crystal compound is 25% by mass or more, a decorative film with small change in reflectance after molding can be obtained. In addition, from the viewpoint of suppressing change in reflectance and change in color after molding, the content of the specific liquid crystal compound is preferably 30% by mass or more based on the total solid content of the liquid crystal composition, more preferably 40% by mass or more, even more preferably 60% by mass or more and 99% by mass or less, and particularly preferably 80% by mass or more and 98% by mass or less.
[0050] -Other cholesteric liquid crystal compounds- The liquid crystal composition may contain other cholesteric liquid crystal compounds (hereinafter, simply referred to as "other liquid crystal compounds") other than the specific liquid crystal compound. Examples of the other liquid crystal compounds include cholesteric liquid crystal compounds having no ethylenically unsaturated group and no cyclic ether group, cholesteric liquid crystal compounds having two or more ethylenically unsaturated groups and no cyclic ether group, cholesteric liquid crystal compounds having two or more cyclic ether groups and no ethylenically unsaturated group, and cholesteric liquid crystal compounds having two or more ethylenically unsaturated groups and two or more cyclic ether groups. From the viewpoint of suppressing changes in reflectance and color after molding, the other liquid crystal compound is preferably at least one compound selected from the group consisting of cholesteric liquid crystal compounds having no ethylenically unsaturated group and no cyclic ether group, cholesteric liquid crystal compounds having two or more ethylenically unsaturated groups and no cyclic ether group, and cholesteric liquid crystal compounds having two or more cyclic ether groups and no ethylenically unsaturated group, more preferably at least one compound selected from the group consisting of cholesteric liquid crystal compounds having no ethylenically unsaturated group and no cyclic ether group, cholesteric liquid crystal compounds having two ethylenically unsaturated groups and no cyclic ether group, and cholesteric liquid crystal compounds having two cyclic ether groups and no ethylenically unsaturated group, and particularly preferably at least one compound selected from the group consisting of cholesteric liquid crystal compounds having no ethylenically unsaturated group and no cyclic ether group, and cholesteric liquid crystal compounds having two ethylenically unsaturated groups and no cyclic ether group.
[0051] As the other liquid crystal compound, a known cholesteric liquid crystal compound can be used. As the rod-shaped liquid crystal compound among the other liquid crystal compounds, for example, those described in "Makromol. Chem., Vol. 190, p. 2255 (1989)" and "Advanced Materials 5, p. 107 (1993)," U.S. Pat. No. 4,683,327, U.S. Pat. No. 5,622,648, U.S. Pat. No. 5,770,107, WO 1995 / 022586, WO 1995 / 024455, WO 1997 / 000600, WO 1998 / 023580, WO 1998 / 052905, JP-A-1-272551, JP-A-6-16616, JP-A-7-110469, JP-A-11-80081, and JP-A-2001-328973 can be used. Furthermore, as the rod-shaped liquid crystal compound in the other liquid crystal compounds, for example, the compounds described in JP-T-11-513019 or JP-A-2007-279688 can be preferably used. As the discotic liquid crystal compound in the other liquid crystal compounds, for example, the compounds described in JP-A-2007-108732 or JP-A-2010-244038 can be preferably used.
[0052] The liquid crystal composition may contain one or more of the other liquid crystal compounds. From the viewpoint of suppressing changes in reflectance and color tone after molding, the content of the other liquid crystal compounds is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 40% by mass or less, and particularly preferably 5% by mass or less, based on the total solid content of the liquid crystal composition. The lower limit of the content of the other liquid crystal compounds is 0% by mass.
[0053] -Chiral agents (optically active compounds)- From the viewpoint of ease of forming a cholesteric liquid crystal layer and ease of adjusting the pitch of the helical structure, the liquid crystal composition preferably contains a chiral agent (i.e., an optically active compound). The chiral agent has a function of inducing a helical structure in the cholesteric liquid crystal layer. The chiral agent may be selected according to the purpose, since the twist direction or helical pitch of the helical structure induced by the liquid crystal compound varies. The chiral agent is not particularly limited, and known compounds (for example, compounds described in "Liquid Crystal Device Handbook", Chapter 3, Section 4-3, Chiral Agents for TN (twisted nematic) and STN (Super-twisted nematic), p. 199, edited by the 142nd Committee of the Japan Society for the Promotion of Science, 1989), isosorbide, and isomannide derivatives can be used. The chiral agent generally contains an asymmetric carbon atom, but axially asymmetric compounds or planarly asymmetric compounds that do not contain an asymmetric carbon atom can also be used as the chiral agent. Preferred examples of the axially asymmetric compound or the planarly asymmetric compound include a binaphthyl compound, a helicene compound, and a paracyclophane compound.
[0054] From the viewpoint of suppressing the change in reflectance after molding, the liquid crystal composition preferably contains a chiral agent having a polymerizable group, and more preferably contains a chiral agent containing a polymerizable group and a chiral agent without a polymerizable group. The polymerizable group is not particularly limited as long as it is a polymerizable group, but from the viewpoint of reactivity and suppressing the change in reflectance after molding, it is preferably an ethylenically unsaturated group or a cyclic ether group, and more preferably an ethylenically unsaturated group. The preferred aspects of the ethylenically unsaturated group and the cyclic ether group in the chiral agent are the same as the preferred aspects of the ethylenically unsaturated group and the cyclic ether group in the specific liquid crystal compound described above.
[0055] When the chiral agent has an ethylenically unsaturated group or a cyclic ether group, from the viewpoints of reactivity and suppression of change in reflectance after molding, it is preferable that the ethylenically unsaturated group or cyclic ether group of the specific liquid crystal compound and the ethylenically unsaturated group or cyclic ether group of the chiral agent are the same type of group (for example, an ethylenically unsaturated group, preferably a (meth)acryloxy group), and it is more preferable that they are the same group.
[0056] From the viewpoints of reactivity and suppression of change in reflectance after molding, the chiral agent having a polymerizable group is preferably a chiral agent having two or more polymerizable groups, more preferably a chiral agent having two or more ethylenically unsaturated groups or a chiral agent having two or more cyclic ether groups, and particularly preferably a chiral agent having two or more ethylenically unsaturated groups.
[0057] The chiral agent may be a cholesteric liquid crystal compound.
[0058] As described later, when the magnitude of the helical pitch of the cholesteric liquid crystal layer is controlled by light irradiation during the production of the cholesteric liquid crystal layer, the liquid crystal composition preferably contains a chiral agent (hereinafter also referred to as a "photosensitive chiral agent") that is sensitive to light and can change the helical pitch of the cholesteric liquid crystal layer. The photosensitive chiral agent is a compound that changes its structure by absorbing light and can change the helical pitch of the cholesteric liquid crystal layer. As such a compound, a compound that causes at least one of a photoisomerization reaction, a photodimerization reaction, and a photodecomposition reaction is preferable. A compound that causes a photoisomerization reaction refers to a compound that causes stereoisomerization or structural isomerization by the action of light. Examples of compounds that cause a photoisomerization reaction include azobenzene compounds and spiropyran compounds. Also, a compound that causes a photodimerization reaction refers to a compound that causes an addition reaction between two groups and is cyclized by light irradiation. Examples of compounds that cause a photodimerization reaction include cinnamic acid derivatives, coumarin derivatives, chalcone derivatives, and benzophenone derivatives. The light is not particularly limited, and examples thereof include ultraviolet light, visible light, and infrared light.
[0059] A preferred example of the photosensitive chiral agent is a chiral agent represented by the following formula (CH1): The chiral agent represented by the following formula (CH1) can change the orientation structure, such as the helical pitch (e.g., helical period and twist period) of the cholesteric liquid crystal phase, depending on the amount of light upon irradiation.
[0060] [ka]
[0061] In formula (CH1), Ar CH1 and Ar CH2 each independently represents an aryl group or a heteroaromatic ring group; R CH1 and R CH2 each independently represents a hydrogen atom or a cyano group.
[0062] Ar in formula (CH1) CH1 and Ar CH2is preferably an aryl group. CH1 and Ar CH2 The total number of carbon atoms in the aryl group in is preferably 6 to 40, and more preferably 6 to 30. The aryl group may have a substituent. Examples of the substituent include preferably a halogen atom, an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, a hydroxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyloxy group, a carboxy group, a cyano group, or a heterocyclic group, and more preferably a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, a hydroxy group, an acyloxy group, an alkoxycarbonyl group, or an aryloxycarbonyl group.
[0063] Ar CH1 and Ar CH2 is preferably an aryl group represented by the following formula (CH2) or formula (CH3).
[0064] [ka]
[0065] In formula (CH2) and formula (CH3), R CH3 and R CH4 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heterocyclic group, an alkoxy group, a hydroxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyloxy group, a carboxy group, or a cyano group; L CH1 and L CH2 each independently represents a halogen atom, an alkyl group, an alkoxy group, or a hydroxy group, nCH1 represents an integer of 0 to 4, nCH2 represents an integer of 0 to 6, and * represents the bonding position with C forming an ethylenically unsaturated bond in formula (CH1).
[0066] R in formula (CH2) and formula (CH3) CH3 and R CH4are each independently preferably a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an aryl group, an alkoxy group, a hydroxy group, an alkoxycarbonyl group, an aryloxycarbonyl group, or an acyloxy group, more preferably an alkoxy group, a hydroxy group, or an acyloxy group, and particularly preferably an alkoxy group. L in formula (CH2) and formula (CH3) CH1 and L CH2 are preferably each independently an alkoxy group having 1 to 10 carbon atoms or a hydroxy group. In the formula (CH2), nCH1 is preferably 0 or 1. In the formula (CH3), nCH2 is preferably 0 or 1.
[0067] Ar of formula (CH1) CH1 and Ar CH2 The total number of carbon atoms in the heteroaromatic ring group in is preferably 4 to 40, more preferably 4 to 30. The heteroaromatic ring group may have a substituent. As the substituent, for example, a halogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkoxy group, a hydroxy group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyloxy group, or a cyano group is preferable, and a halogen atom, an alkyl group, an alkenyl group, an aryl group, an alkoxy group, or an acyloxy group is more preferable. As the heteroaromatic ring group, a pyridyl group, a pyrimidinyl group, a furyl group, or a benzofuranyl group is preferable, and a pyridyl group or a pyrimidinyl group is more preferable.
[0068] In formula (CH1), R CH1 and R CH2 are each preferably independently a hydrogen atom.
[0069] The liquid crystal composition may contain one chiral agent alone or two or more chiral agents. The content of the chiral agent can be appropriately selected according to the structure of the specific liquid crystal compound used and the desired pitch of the helical structure. From the viewpoints of ease of forming a cholesteric liquid crystal layer, ease of adjusting the pitch of the helical structure, and suppression of reflectance change after molding, the content of the chiral agent is preferably 1% by mass or more and 20% by mass or less, more preferably 2% by mass or more and 15% by mass or less, and particularly preferably 3% by mass or more and 10% by mass or less, based on the total solid content of the liquid crystal composition.
[0070] When the liquid crystal composition contains a chiral agent having a polymerizable group as a chiral agent, the content of the chiral agent having a polymerizable group is, from the viewpoint of suppressing a change in reflectance after molding, preferably from 0.2 mass % to 15 mass % relative to the total solid content of the liquid crystal composition, more preferably from 0.5 mass % to 10 mass %, even more preferably from 1 mass % to 8 mass %, and particularly preferably from 1.5 mass % to 5 mass %.
[0071] When the liquid crystal composition contains a chiral agent that does not have a polymerizable group as a chiral agent, the content of the chiral agent that does not have a polymerizable group is preferably from 0.2 mass % to 20 mass % inclusive, more preferably from 0.5 mass % to 15 mass % inclusive, and particularly preferably from 1.5 mass % to 10 mass % inclusive, relative to the total solid content of the liquid crystal composition, from the viewpoint of suppressing changes in reflectance after molding.
[0072] In addition, the pitch of the helical structure of the cholesteric liquid crystal in the cholesteric liquid crystal layer, and the selective reflection wavelength and its range described below can be easily changed not only by the type of liquid crystal compound used, but also by adjusting the content of the chiral agent. Although it cannot be said in general, when the content of the chiral agent in the liquid crystal composition is doubled, the pitch may be halved and the center value of the selective reflection wavelength may also be halved.
[0073] -Polymerization initiator- The liquid crystal composition preferably contains a polymerization initiator, and more preferably contains a photopolymerization initiator.
[0074] When the liquid crystal composition contains a cholesteric liquid crystal compound having one ethylenically unsaturated group, the liquid crystal composition preferably contains a radical polymerization initiator, and more preferably contains a photoradical polymerization initiator, from the viewpoint of suppressing changes in reflectance and color after molding.
[0075] When the liquid crystal composition contains a cholesteric liquid crystal compound having one cyclic ether group, from the viewpoint of suppressing changes in reflectance and color tone after molding, the liquid crystal composition preferably contains a cationic polymerization initiator, and more preferably contains a photocationic polymerization initiator.
[0076] The liquid crystal composition preferably contains, as the polymerization initiator, only either a radical polymerization initiator or a cationic polymerization initiator.
[0077] As the polymerization initiator, a known polymerization initiator can be used. In addition, the polymerization initiator is preferably a photopolymerization initiator capable of initiating a polymerization reaction by ultraviolet irradiation. Examples of the photopolymerization initiator include α-carbonyl compounds (described in U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ether compounds (described in U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (described in U.S. Pat. No. 2,722,512), polynuclear quinone compounds (described in U.S. Pat. Nos. 3,046,127 and 2,951,758), a combination of triaryl imidazole dimer and p-aminophenyl ketone (described in U.S. Pat. No. 3,549,367), acridine compounds and phenazine compounds (described in JP-A-60-105,667 and U.S. Pat. No. 4,239,850), and oxadiazole compounds (described in U.S. Pat. No. 4,212,970).
[0078] As the photoradical polymerization initiator, a known photoradical polymerization initiator can be used. Preferred examples of the photoradical polymerization initiator include an α-hydroxyalkylphenone compound, an α-aminoalkylphenone compound, and an acylphosphine oxide compound.
[0079] As the cationic photopolymerization initiator, a known cationic photopolymerization initiator can be used. Preferred examples of the cationic photopolymerization initiator include an iodonium salt compound and a sulfonium salt compound.
[0080] The liquid crystal composition may contain one type of polymerization initiator alone or two or more types. The content of the polymerization initiator can be appropriately selected according to the structure of the specific liquid crystal compound used and the desired pitch of the helical structure. From the viewpoints of ease of forming a cholesteric liquid crystal layer, ease of adjusting the pitch of the helical structure, polymerization rate, and strength of the cholesteric liquid crystal layer, the content of the polymerization initiator is preferably 0.05% by mass or more and 10% by mass or less, more preferably 0.05% by mass or more and 5% by mass or less, even more preferably 0.1% by mass or more and 2% by mass or less, and particularly preferably 0.2% by mass or more and 1% by mass or less, based on the total solid content of the liquid crystal composition.
[0081] -Crosslinking agent- The liquid crystal composition may contain a crosslinking agent to improve the strength and durability of the cholesteric liquid crystal layer after curing. As the crosslinking agent, for example, a crosslinking agent that cures with ultraviolet light, heat, or moisture can be suitably used. The crosslinking agent is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include polyfunctional acrylate compounds such as trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate; epoxy compounds such as glycidyl (meth)acrylate and ethylene glycol diglycidyl ether; aziridine compounds such as 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate] and 4,4-bis(ethyleneiminocarbonylamino)diphenylmethane; isocyanate compounds such as hexamethylene diisocyanate and biuret type isocyanate; polyoxazoline compounds having an oxazoline group in the side chain; and alkoxysilane compounds such as vinyltrimethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane. In addition, a known catalyst can be used according to the reactivity of the crosslinking agent, and the productivity can be improved in addition to improving the strength and durability of the cholesteric liquid crystal layer.
[0082] The liquid crystal composition may contain one type of crosslinking agent alone or two or more types of crosslinking agents. From the viewpoint of strength and durability of the cholesteric liquid crystal layer, the content of the crosslinking agent is preferably from 1% by mass to 20% by mass, more preferably from 3% by mass to 15% by mass, based on the total solid content of the liquid crystal composition.
[0083] -Multifunctional polymerizable compound- From the viewpoint of suppressing the change in reflectance after molding, the liquid crystal composition preferably contains a polyfunctional polymerizable compound, and more preferably contains a polyfunctional polymerizable compound having the same type of polymerizable group. Examples of the polyfunctional polymerizable compound include the cholesteric liquid crystal compound having two or more ethylenically unsaturated groups and no cyclic ether group, the cholesteric liquid crystal compound having two or more cyclic ether groups and no ethylenically unsaturated group, and the cholesteric liquid crystal compound having two or more ethylenically unsaturated groups and two or more cyclic ether groups, the chiral agent having two or more polymerizable groups, and the crosslinking agent.
[0084] The liquid crystal composition preferably contains, as a polyfunctional polymerizable compound, at least one compound selected from the group consisting of a cholesteric liquid crystal compound having two or more ethylenically unsaturated groups and no cyclic ether group, a cholesteric liquid crystal compound having two or more cyclic ether groups and no ethylenically unsaturated group, and a chiral agent having two or more polymerizable groups, and more preferably contains a chiral agent having two or more polymerizable groups.
[0085] The liquid crystal composition may contain one type of polyfunctional polymerizable compound alone or two or more types. From the viewpoint of suppressing a change in reflectance after molding, the content of the polyfunctional polymerizable compound is preferably 0.5% by mass to 70% by mass, more preferably 1% by mass to 50% by mass, even more preferably 1.5% by mass to 20% by mass, and particularly preferably 2% by mass to 10% by mass, based on the total solid content of the liquid crystal composition.
[0086] -Other additives- The liquid crystal composition may contain additives other than the above-mentioned components as necessary. As the additives, known additives can be used, and examples thereof include surfactants, polymerization inhibitors, antioxidants, horizontal alignment agents, ultraviolet absorbers, light stabilizers, colorants, and metal oxide particles.
[0087] The liquid crystal composition may also contain a solvent. The solvent is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent is preferably used. The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ketones (e.g., methyl ethyl ketone and methyl isobutyl ketone), alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers. The solvent may be used alone or in combination of two or more. Among these, ketones are particularly preferred when considering the burden on the environment. The above-mentioned components may also function as a solvent.
[0088] The content of the solvent in the liquid crystal composition is not particularly limited, and may be adjusted to a content of the solvent that provides desired coating properties. The content of the solid content relative to the total mass of the liquid crystal composition is not particularly limited, but is preferably 1% by mass to 90% by mass, more preferably 5% by mass to 80% by mass, and particularly preferably 10% by mass to 80% by mass. The content of the solvent in the liquid crystal composition at the time of curing to form a cholesteric liquid crystal layer is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less, relative to the total solid content of the liquid crystal composition. The content of the solvent in the cholesteric liquid crystal layer obtained by curing the liquid crystal composition is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less, relative to the total mass of the cholesteric liquid crystal layer.
[0089] - Application and curing of liquid crystal composition - In forming a cholesteric liquid crystal layer, the liquid crystal composition is used by, for example, applying it onto an object (for example, the above-mentioned substrate and the alignment layer described below). The liquid crystal composition can be applied, for example, by making the liquid crystal composition into a solution state using a solvent, or by heating it into a liquid such as a molten liquid, and then by an appropriate method such as a roll coating method, a gravure printing method, or a spin coating method. The liquid crystal composition can also be applied by various methods such as a wire bar coating method, an extrusion coating method, a direct gravure coating method, a reverse gravure coating method, and a die coating method. In addition, the liquid crystal composition can be discharged from a nozzle using an inkjet device to form a coating film (meaning a film-like liquid crystal composition formed by application).
[0090] After the liquid crystal composition is applied, the liquid crystal composition is cured to form a cholesteric liquid crystal layer. The liquid crystal composition is cured to maintain and fix the alignment state of the molecules of the cholesteric liquid crystal compound (for example, the above-mentioned specific liquid crystal compound). The liquid crystal composition is preferably cured by a polymerization reaction of a polymerizable group (for example, an ethylenically unsaturated group or a cyclic ether group) possessed by the cholesteric liquid crystal compound. When a solvent is used as a component of the liquid crystal composition, it is preferable to dry the coating film by a known method after the liquid crystal composition is applied and before the polymerization reaction for curing. For example, the coating film may be dried by leaving it to stand, or the coating film may be dried by heating. It is sufficient that the cholesteric liquid crystal compound in the liquid crystal composition is aligned after the application and drying of the liquid crystal composition.
[0091] -Layer structure of cholesteric liquid crystal layer- From the viewpoint of suppressing changes in reflectance after molding, the decorative film according to an embodiment of the present disclosure preferably has two or more cholesteric liquid crystal layers. The compositions of the two or more cholesteric liquid crystal layers may be the same or different. When the decorative film according to an embodiment of the present disclosure has two or more cholesteric liquid crystal layers, the decorative film according to an embodiment of the present disclosure may have at least one layer formed by curing a liquid crystal composition containing a cholesteric liquid crystal compound (i.e., a specific liquid crystal compound) having one ethylenically unsaturated group or one cyclic ether group in an amount of 25% by mass or more relative to the total solid content of the liquid crystal composition. From the viewpoint of suppressing changes in reflectance after molding, it is preferable that each of the two or more cholesteric liquid crystal layers is a layer formed by curing a liquid crystal composition containing a cholesteric liquid crystal compound having one ethylenically unsaturated group or one cyclic ether group in an amount of 25% by mass or more relative to the total solid content of the liquid crystal composition.
[0092] Furthermore, for example, when the decorative film according to one embodiment of the present disclosure has two cholesteric liquid crystal layers, it is preferable to have a cholesteric liquid crystal layer on each side of the substrate from the viewpoint of suppressing changes in reflectance after molding.
[0093] <<Selective reflectivity of optical reflective layer>> The optical reflection layer preferably has a central wavelength of selective reflection wavelength in the range of 300 nm to 1,500 nm. In the present disclosure, the "central wavelength of selective reflection wavelength" refers to the minimum and minimal value of the light transmittance of the target object (e.g., the optical reflection layer). min (unit:%), the half-value transmittance T is expressed by the following formula 1 / 2 The average value of two wavelengths (unit: %) is shown. However, the first of the two wavelengths is the T min The second of the two wavelengths is the maximum wavelength in the wavelength range that includes wavelengths shorter than the wavelength that shows the above T minThe transmittance is the minimum wavelength in a wavelength range including wavelengths longer than the wavelength at which the selective reflection wavelength is observed. The transmittance is measured using a spectrophotometer (e.g., Shimadzu Corporation, spectrophotometer UV-2100). The central wavelength of the selective reflection wavelength may be in the range of 380 nm or more and 780 nm or less, or in the range of more than 780 nm and 1,500 nm or less. Formula for calculating half-value transmittance: T 1 / 2 =100-(100-T min )÷2
[0094] The optical reflective layer preferably has a maximum reflection wavelength in the wavelength range of 380 nm to 1,500 nm. From the viewpoint of use in a decorative film, the wavelength range including the maximum reflection wavelength is preferably 380 nm to 1,200 nm, more preferably 400 nm to 1,000 nm, and particularly preferably 420 nm to 900 nm.
[0095] The decorative film according to one embodiment of the present disclosure has two or more optical reflection layers laminated together, and in one embodiment, the optical reflection layers have different diffuse reflectances. The diffuse reflectance is defined by the following relational expression using the absolute reflectance (Rs) measured from a direction perpendicular to the film plane (0°) and the integral reflectance (Rd). Formula for calculating diffuse reflectance: (Rd-Rs) / Rd For example, the measurement can be performed using a spectrophotometer V-670 manufactured by JASCO Corporation.
[0096] Possible means for controlling the diffuse reflectivity of the optical reflection layer include giving the optical reflection layer an uneven structure, and when the optical reflection layer is made of cholesteric liquid crystal, possible methods include controlling the anisotropy of the alignment film to control the degree of alignment of the liquid crystal.
[0097] The decorative film according to the embodiment of the present disclosure provides a decorative film that exhibits a high saturation reflected color. In order to achieve high saturation, the optical reflection layer preferably has a maximum reflected wavelength in the wavelength range of 420 nm to 780 nm. The saturation (C *ab) can be calculated uniquely from the reflectance spectrum. For example, it can be calculated using the integrated reflectance spectrum measured with a spectrophotometer V-670 manufactured by JASCO Corporation, using the color diagnosis software (color evaluation (color diagnosis) program) that comes with the device. In this case, the CIE1976L is calculated based on the XYZ color system calculated according to JIS Z 8701:1999 with a light source of D65 and a visual field of 2°. * a * b * displayed in color space.
[0098] The thickness of each optical reflective layer is not particularly limited and may be, for example, 0.5 μm to 10.0 μm, or 1.0 μm to 8.0 μm. When the thickness is 0.5 μm or more, good visibility of the decoration is easily obtained, and when the thickness is 10.0 μm or less, defects and distortions of the reflective film are suppressed and a uniform reflected color is easily obtained.
[0099] <Alignment layer> The decorative film according to an embodiment of the present disclosure may have an alignment layer in contact with the cholesteric liquid crystal layer. The alignment layer is used to align the molecules of the liquid crystal compound in the liquid crystal composition when forming a layer containing a liquid crystal compound (hereinafter also referred to as a "liquid crystal layer"). Since the alignment layer is used, for example, when forming the liquid crystal layer, a decorative film that does not include a liquid crystal layer may or may not include an alignment layer.
[0100] The alignment layer can be provided, for example, by rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound (e.g., SiO2), or by forming a layer having microgrooves. Furthermore, alignment layers that generate an alignment function by applying an electric field, a magnetic field, or light irradiation are also known. Depending on the material of the lower layer such as the support and the liquid crystal layer, the lower layer can be directly aligned (e.g., rubbing) to function as an alignment layer without providing an alignment layer. An example of such a support that can be the lower layer is polyethylene terephthalate (PET). In addition, when a layer (hereinafter referred to as the "upper layer" in this paragraph) is laminated directly on the liquid crystal layer, the lower liquid crystal layer may act as an alignment layer to align the liquid crystal compound for the preparation of the upper layer. In such a case, the liquid crystal compound in the upper layer can be aligned without providing an alignment layer or performing a special alignment treatment (e.g., rubbing treatment).
[0101] As preferred examples of the alignment layer, a rubbed alignment layer and a photoalignment layer will be described below.
[0102] <<Rubbing treatment alignment layer>> The rubbing treatment alignment layer is an alignment layer to which alignment is imparted by rubbing treatment. Examples of polymers that can be used in the rubbing treatment alignment layer include, for example, methacrylate copolymers, styrene copolymers, polyolefins, polyvinyl alcohol, and modified polyvinyl alcohols described in paragraph 0022 of JP-A-8-338913, as well as poly(N-methylolacrylamide), polyesters, polyimides, vinyl acetate copolymers, carboxymethylcellulose, and polycarbonates. A silane coupling agent can be used as the polymer. As the polymer that can be used in the rubbing treatment alignment layer, water-soluble polymers (e.g., poly(N-methylolacrylamide), carboxymethylcellulose, gelatin, polyvinyl alcohol, and modified polyvinyl alcohol) are preferred, gelatin, polyvinyl alcohol, or modified polyvinyl alcohol are more preferred, and polyvinyl alcohol or modified polyvinyl alcohol is particularly preferred.
[0103] In the method of orienting a liquid crystal compound using a rubbed alignment layer, for example, a composition for forming a cholesteric liquid crystal layer (one form of a liquid crystal composition) is applied to the rubbed surface of the rubbed alignment layer to orient the molecules of the liquid crystal compound. Thereafter, if necessary, a polymer contained in the alignment layer is reacted with a polyfunctional monomer contained in the cholesteric liquid crystal layer, or a crosslinking agent is used to crosslink the polymer contained in the alignment layer, thereby forming a cholesteric liquid crystal layer. The thickness of the alignment layer is preferably in the range of 0.1 μm to 10 μm.
[0104] -Rubbing treatment- The surface of the alignment layer, support, or other layer to which the composition for forming a cholesteric liquid crystal layer is applied may be subjected to a rubbing treatment, if necessary. The rubbing treatment can generally be carried out by rubbing the surface of a film mainly composed of a polymer in a certain direction with paper or cloth. General methods for rubbing treatment are described, for example, in "Liquid Crystal Handbook" (published by Maruzensha, October 30, 2000).
[0105] The rubbing density can be changed by the method described in "Liquid Crystal Handbook" (published by Maruzensha). The rubbing density (L) is quantified by the following formula (A). Formula (A): L=Nl(1+2πrn / 60v) In formula (A), N is the number of rubbings, l is the contact length of the rubbing roller, π is the circular constant, r is the radius of the roller, n is the rotation speed of the roller (rpm), and v is the stage movement speed (per second).
[0106] In order to increase the rubbing density, the number of rubbings may be increased, the contact length of the rubbing roller may be increased, the radius of the roller may be increased, the number of rotations of the roller may be increased, or the stage moving speed may be decreased, whereas in order to decrease the rubbing density, the opposite may be done. In addition, the description of Japanese Patent No. 4052558 may be referred to for the conditions of the rubbing treatment.
[0107] <<Photo alignment layer>> The photo-alignment layer is an alignment layer to which alignment is imparted by light irradiation. Photo-alignment materials used in the photo-alignment layer are described in many documents. Examples of photo-alignment materials include azo compounds described in JP 2006-285197 A, JP 2007-76839 A, JP 2007-138138 A, JP 2007-94071 A, JP 2007-121721 A, JP 2007-140465 A, JP 2007-156439 A, JP 2007-133184 A, JP 2009-109831 A, Japanese Patent No. 3883848 A, and Japanese Patent No. 4151746 A, and azo compounds described in JP 2002-229039 A. Preferred examples include aromatic ester compounds, maleimide and / or alkenyl-substituted nadiimide compounds having photo-orientable units described in JP-A-2002-265541 and JP-A-2002-317013, photo-crosslinkable silane derivatives described in JP-A-4205195 and JP-A-4205198, and photo-crosslinkable polyimides, polyamides, or esters described in JP-T-2003-520878, JP-T-2004-529220, and JP-T-4162850. Particularly preferred are azo compounds, photo-crosslinkable polyimides, polyamides, or esters.
[0108] For example, a layer formed from the above material is irradiated with linearly polarized light or non-polarized light to produce a photo-alignment layer. In the present disclosure, "irradiation with linearly polarized light" refers to an operation for causing a photo-reaction in a photo-alignment material. The wavelength of the light used varies depending on the photo-alignment material used, and is not particularly limited as long as it is a wavelength necessary for the photo-reaction. Preferably, the peak wavelength of the light used for photoirradiation is 200 nm to 700 nm, and more preferably, the peak wavelength of the light is ultraviolet light of 400 nm or less.
[0109] Examples of light sources used for light irradiation include commonly used light sources, such as lamps (e.g., tungsten lamps, halogen lamps, xenon lamps, xenon flash lamps, mercury lamps, mercury xenon lamps, and carbon arc lamps), various lasers (e.g., semiconductor lasers, helium-neon lasers, argon ion lasers, helium cadmium lasers, and YAG (yttrium aluminum garnet) lasers), light-emitting diodes, and cathode ray tubes.
[0110] As a means for obtaining linearly polarized light, a method using a polarizing plate (e.g., an iodine polarizing plate, a dichroic dye polarizing plate, and a wire grid polarizing plate), a method using a prism-based element (e.g., a Glan-Thompson prism) and a reflective polarizer utilizing the Brewster angle, or a method using light emitted from a polarized laser light source can be adopted. Also, a filter and a wavelength conversion element may be used to selectively irradiate only light of a required wavelength.
[0111] When the light to be irradiated is linearly polarized, a method is adopted in which the light is irradiated vertically or obliquely to the upper or lower surface of the alignment layer. The incident angle of the light varies depending on the photo-alignment material, but is preferably 0° to 90° (vertical), more preferably 40° to 90°. When non-polarized light is used, the non-polarized light is irradiated obliquely to the upper or lower surface of the alignment layer. The incident angle of the non-polarized light is preferably 10° to 80°, more preferably 20° to 60°, and particularly preferably 30° to 50°. The irradiation time is preferably 1 minute to 60 minutes, more preferably 1 minute to 10 minutes.
[0112] <Resin layer> The decorative film according to an embodiment of the present disclosure preferably has a resin layer between the substrate and the optical reflection layer. For example, when pressure is applied to the optical reflection layer to impart a concave-convex structure, the resin layer is deformed, so that the optical reflection layer can easily follow the concave-convex structure used as a mold.
[0113] The thickness of the resin layer is preferably from 0.2 μm to 100 μm, more preferably from 0.5 μm to 70 μm, and further preferably from 1.0 μm to 50 μm.
[0114] The elastic modulus of the resin layer at 25° C. is preferably 0.000001 GPa to 3 GPa, more preferably 0.00001 to 1 GPa, and even more preferably 0.0001 to 0.5 GPa. The elastic modulus is measured by a nanoindenter device (for example, Nanoindenter G200, manufactured by KLA Corporation).
[0115] The resin layer preferably contains a binder resin as a main component. The binder resin is not limited, and any known resin can be used. From the viewpoint of obtaining a desired color, the binder resin is preferably a transparent resin, and specifically, a resin having a total light transmittance of 80% or more is preferable. The total light transmittance can be measured by a spectrophotometer (for example, a spectrophotometer UV-2100 manufactured by Shimadzu Corporation).
[0116] The binder resin is not limited, and known resins can be used. Examples of the binder resin include acrylic resin, silicone resin, polyester, urethane resin, and polyolefin. The binder resin may be a homopolymer of a specific monomer, or a copolymer of a specific monomer and another monomer.
[0117] The binder resin may be used alone or in combination of two or more. From the viewpoint of moldability, the content of the binder resin in the resin layer is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 60% by mass, and particularly preferably 20% by mass to 60% by mass, based on the total mass of the resin layer.
[0118] A known pressure sensitive adhesive or bonding agent may also be used for the resin layer.
[0119] <<Adhesive>> Examples of the adhesive include acrylic adhesives, rubber adhesives, and silicone adhesives. Examples of the adhesive include acrylic adhesives, ultraviolet (UV) curing adhesives, and silicone adhesives, as described in "Evaluation of Properties of Release Papers, Release Films, and Adhesive Tapes and Technology for Controlling Them," Information Agency, 2004, Chapter 2. In this disclosure, the acrylic adhesive refers to an adhesive containing a polymer of a (meth)acrylic monomer (i.e., a (meth)acrylic polymer). When the resin layer contains an adhesive, the resin layer may further contain a tackifier.
[0120] <<Adhesive>> Examples of the adhesive include urethane resin adhesives, polyester adhesives, acrylic resin adhesives, ethylene vinyl acetate resin adhesives, polyvinyl alcohol adhesives, polyamide adhesives, and silicone adhesives. In terms of higher adhesive strength, urethane resin adhesives and silicone adhesives are preferred.
[0121] <<Method of forming resin layer>> The method of forming the resin layer is not limited. The resin layer can be formed, for example, by using a composition for forming a resin layer. The composition for forming a resin layer can be prepared, for example, by mixing the raw materials of the resin layer. The method of applying the composition for forming a resin layer can be, for example, the same method as the application method of the liquid crystal composition.
[0122] <<Additives>> The resin layer may contain additives, if necessary, in addition to the above components. The additives are not limited, and known additives can be used. Examples of the additives include surfactants described in paragraph 0017 of Japanese Patent No. 4502784 and paragraphs 0060 to 0071 of Japanese Patent Publication No. 2009-237362, thermal polymerization inhibitors (also called polymerization inhibitors, preferably phenothiazine) described in paragraph 0018 of Japanese Patent No. 4502784, and additives described in paragraphs 0058 to 0071 of Japanese Patent Publication No. 2000-310706.
[0123] <Print layer> The decorative film according to an embodiment of the present disclosure has two or more optical reflection layers laminated thereon, and a printed layer is laminated between each of the optical reflection layers. The printed layer is a layer on which an image pattern is printed, and can be printed using a UV inkjet printer, such as Acuity (registered trademark) 1600 manufactured by Fujifilm Corporation.
[0124] <Colored layer> The decorative film according to an embodiment of the present disclosure preferably has a colored layer. In addition, in an embodiment, the decorative film is preferably a decorative film for visually recognizing the colored layer through the cholesteric liquid crystal layer. The colored layer may be a colored layer (i.e., not colorless and transparent). The colored layer is preferably an opaque colored layer (preferably a colored layer having a total light transmittance of 10% or less). The color of the colored layer may be black, gray, white, red, orange, yellow, green, blue, or purple. A black colored layer is preferable because the intensity of reflected light is small and color changes are more emphasized.
[0125] The colored layer may be a layer obtained by curing a polymerizable compound, or may be a layer containing a polymerizable compound and a polymerization initiator. From the viewpoint of storage stability and adhesion between the colored layer and other layers, the colored layer is preferably a layer obtained by curing a polymerizable compound, and more preferably a layer obtained by curing at least a bifunctional or trifunctional polymerizable compound having at least one partial structure selected from the group consisting of a urethane bond and an alkyleneoxy group having 2 or 3 carbon atoms.
[0126] <<Coloring agent>> From the viewpoint of visibility, the colored layer preferably contains a colorant, and from the viewpoint of durability, it is more preferable that the colorant contains a pigment. The colorant is not particularly limited, and a colorant having a desired hue can be appropriately selected and used. Examples of the colorant include pigments and dyes, and pigments are preferable. In addition, the pigment is preferably a particulate pigment. As the pigment, various inorganic pigments and organic pigments known in the art can be used.
[0127] Examples of inorganic pigments include those described in paragraphs 0015 and 0114 of JP-A-2005-7765. Specific examples of inorganic pigments include white pigments (e.g., titanium dioxide, zinc oxide, lithopone, precipitated calcium carbonate, white carbon, aluminum oxide, aluminum hydroxide, and barium sulfate) and black pigments (e.g., carbon black, titanium black, titanium carbon, iron oxide, and graphite). Known chromatic pigments such as iron oxide, barium yellow, cadmium red, and chrome yellow can also be used.
[0128] Examples of the organic pigment include those described in paragraph 0093 of JP-A-2009-256572. Specific examples of the organic pigment include red pigments such as CI Pigment Red 177, 179, 224, 242, 254, 255, and 264, yellow pigments such as CI Pigment Yellow 138, 139, 150, 180, and 185, orange pigments such as CI Pigment Orange 36, 38, and 71, green pigments such as CI Pigment Green 7, 36, and 58, blue pigments such as CI Pigment Blue 15:6, and purple pigments such as CI Pigment Violet 23.
[0129] In addition, the colored layer may contain particles of a pigment having light transmittance and light reflectance (so-called glittering pigment) as a pigment. When the method for forming the colored layer includes a step of exposing the colored layer to light, the glittering pigment is preferably used within a range that does not interfere with curing by exposure.
[0130] The colorants may be used alone or in combination of two or more. In addition, inorganic pigment particles and organic pigment particles may be used in combination. The content of the colorant in the colored layer is preferably 1% by mass to 50% by mass, more preferably 5% by mass to 50% by mass, and even more preferably 10% by mass to 40% by mass, based on the total mass of the colored layer, from the viewpoints of expressing a desired hue (for example, suppressing whitening) and maintaining the shape conformability of the colored layer to the mold. Here, "whitening" in the present disclosure refers to a change in the colored layer to exhibit a whitish color with a matte feel.
[0131] <<Polymerizable compounds>> The colored layer used in the present disclosure may contain a polymerizable compound. The polymerizable compound is a compound having a polymerizable group.
[0132] Examples of the polymerizable group include an ethylenically unsaturated group and an epoxy group, and from the viewpoint of curability, etc., an ethylenically unsaturated group is preferable, and a (meth)acryloxy group is more preferable. Moreover, the polymerizable group is preferably a radically polymerizable group.
[0133] The polymerizable compound is preferably a bifunctional or trifunctional polymerizable compound having at least one partial structure selected from the group consisting of a urethane bond, a urea bond, an alkyleneoxy group having 2 or 3 carbon atoms, and a hydrocarbon group having 6 to 12 carbon atoms (hereinafter also referred to as a "specific polymerizable compound"), and more preferably a compound containing a urethane bond in the partial structure.
[0134] -Bifunctional or trifunctional polymerizable compound having a urethane bond- The bifunctional or trifunctional polymerizable compound having a urethane bond (hereinafter also referred to as "specific polymerizable compound 1") is preferably a urethane oligomer. The nitrogen atom in the urethane bond may be disubstituted (one of the groups on the nitrogen atom is a hydrogen atom) or trisubstituted. In addition, the specific polymerizable compound 1 preferably has a urethane resin chain.
[0135] The urethane oligomer is preferably a urethane (meth)acrylate oligomer. The urethane (meth)acrylate oligomer can be, for example, an aliphatic urethane (meth)acrylate and an aromatic urethane (meth)acrylate. For details, Oligomer Handbook (supervised by Junji Furukawa, published by The Chemical Daily Co., Ltd.) can be referred to, and the urethane oligomer described therein can be appropriately selected according to purpose and used to form a colored layer.
[0136] The molecular weight of the urethane oligomer, which is a type of specific polymerizable compound 1, is preferably 800 to 2,000, and more preferably 1,000 to 2,000.
[0137] As the urethane (meth)acrylate oligomer, which is one type of specific polymerizable compound 1, a commercially available product may be used. Commercially available urethane (meth)acrylate oligomers include, for example, U-2PPA and UA-122P manufactured by Shin-Nakamura Chemical Co., Ltd.; CN964A85, CN964, CN959, CN962, CN963J85, CN965, CN982B88, CN981, CN983, CN991, CN991NS, CN996, CN996NS, CN9002, CN9007, CN9178, and CN9893 manufactured by Sartomer Japan Co., Ltd.; and EBECRYL230, EBECRYL270, EBECRYL284, EBECRYL4858, EBECRYL210, EBECRYL8402, EBECRYL8804, and EBECRYL8800-20R manufactured by Daicel-Allnex Corporation (all of which are trade names). In addition, "EBECRYL" is a registered trademark.
[0138] <<Dispersant>> From the viewpoint of improving the dispersibility of the pigment contained in the colored layer, the colored layer may contain a dispersant. By including a dispersant in the colored layer, the dispersibility of the pigment in the colored layer formed is improved, and the hue of the resulting decorative film can be made uniform.
[0139] The dispersant can be appropriately selected depending on the type and shape of the pigment, but is preferably a polymer dispersant. Examples of the polymer dispersant include silicone polymers, acrylic polymers, and polyester polymers.
[0140] When it is desired to impart heat resistance to the decorative film, it is preferable to use, for example, a silicone polymer such as a graft type silicone polymer as a dispersant.
[0141] The weight average molecular weight of the dispersant is preferably from 1,000 to 5,000,000, more preferably from 2,000 to 3,000,000, and particularly preferably from 2,500 to 3,000,000. When the weight average molecular weight is 1,000 or more, the dispersibility of the pigment is further improved.
[0142] As the dispersant, commercially available products may be used. Examples of commercially available products include EFKA 4300 (acrylic polymer dispersant) from BASF Japan, Homogenol L-18, Homogenol L-95, and Homogenol L-100 from Kao Corporation, Pers 20000 and Solsperse 24000 from Lubrizol Japan, and DISPERBYK-110, DISPERBYK-164, DISPERBYK-180, and DISPERBYK-182 from BYK-Chemie Japan. Note that "Homogenol", "Solsperse", and "DISPERBYK" are all registered trademarks.
[0143] When the colored layer contains a dispersant, the dispersant may contain only one type of dispersant, or may contain two or more types of dispersants. The content of the dispersant is preferably 1 part by mass to 30 parts by mass with respect to 100 parts by mass of the colorant.
[0144] <<Polymerization initiator>> The colored layer may contain a polymerization initiator. As the polymerization initiator, a photopolymerization initiator is preferable from the viewpoint of increasing sensitivity to light exposure. As the photopolymerization initiator, for example, the polymerization initiator described in paragraphs 0031 to 0042 of JP2011-95716A and the oxime-based polymerization initiator described in paragraphs 0064 to 0081 of JP2015-014783A can be used.
[0145] Specific examples of the photopolymerization initiator include 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyloxime) (e.g., IRGACURE® OXE-01, manufactured by BASF), [9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethan-1-one-1-(O-acetyloxime) (e.g., IRGACURE® OXE-02, manufactured by BASF), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (e.g., IRGACURE® 379EG, manufactured by BASF), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (e.g., IRGACURE® 907 ... hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methyl-propan-1-one (e.g., IRGACURE (registered trademark) 127, manufactured by BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1 (e.g., IRGACURE (registered trademark) 369, manufactured by BASF), 2-hydroxy-2-methyl-1-phenylpropan-1-one (e.g., IRGACURE (registered trademark) 1173, manufactured by BASF), 1-hydroxycyclohexyl phenyl ketone (e.g., IRGACURE (registered trademark) 184, manufactured by BASF), 2,2-dimethoxy-1,2-diphenylethane-1-one (e.g., IRGACURE (registered trademark) 651, manufactured by BASF), and an oxime ester polymerization initiator (trade name: Lunar 6 (manufactured by DKSH Japan Co., Ltd.), 2,4-diethylthioxanthone (for example, Kayacure DETX-S, manufactured by Nippon Kayaku Co., Ltd.), and fluorene oxime polymerization initiators DFI-091 and DFI-020 (both manufactured by Daito Chemistry Co., Ltd.).
[0146] Among these, from the viewpoint of enhancing the curing sensitivity, it is preferable to use an initiator other than a halogen-containing polymerization initiator such as a trichloromethyltriazine-based compound, and an oxime-based polymerization initiator such as an α-aminoalkylphenone-based compound, an α-hydroxyalkylphenone-based compound, or an oxime ester-based compound is more preferable.
[0147] The content of the polymerization initiator is preferably from 0.1 to 15 parts by mass, and more preferably from 0.5 to 10 parts by mass, relative to 100 parts by mass of the polymerizable compound.
[0148] <<Binder resin>> The colored layer preferably contains a binder resin from the viewpoint of reducing the cure shrinkage of the colored layer. The binder resin is not particularly limited, and a known resin can be appropriately selected. The binder resin is preferably a transparent resin from the viewpoint of obtaining a desired hue, and specifically, a resin having a total light transmittance of 80% or more is preferable. The total light transmittance can be measured by a spectrophotometer (for example, a spectrophotometer UV-2100 manufactured by Shimadzu Corporation).
[0149] Examples of the binder resin include acrylic resin, silicone resin, polyester resin, urethane resin, and olefin resin. Among them, from the viewpoint of transparency, acrylic resin, silicone resin, or polyester resin is preferable, and acrylic resin or silicone resin is more preferable. Furthermore, from the viewpoint of heat resistance, silicone resin is preferable.
[0150] In the present disclosure, the term "acrylic resin" refers to a resin containing a structural unit derived from an acrylic monomer having a (meth)acryloyl group. The term "(meth)acryloyl group" is a concept that includes a methacryloyl group and an acryloyl group. The acrylic resin includes, for example, a homopolymer of acrylic acid, a homopolymer of methacrylic acid, a homopolymer of an acrylic acid ester, a homopolymer of a methacrylic acid ester, a copolymer of acrylic acid and other monomers, a copolymer of methacrylic acid and other monomers, a copolymer of an acrylic acid ester and other monomers, a copolymer of a methacrylic acid ester and other monomers, and a urethane-modified copolymer having a urethane skeleton in the side chain. Examples of the acrylic resin include a glycidyl methacrylate adduct of a cyclohexyl methacrylate / methyl methacrylate / methacrylic acid copolymer, a random copolymer of benzyl methacrylate / methacrylic acid, a copolymer of allyl methacrylate / methacrylic acid, and a copolymer of benzyl methacrylate / methacrylic acid / hydroxyethyl methacrylate.
[0151] As the silicone resin, known silicone resins can be used, for example, methyl-based straight silicone resin, methylphenyl-based straight silicone resin, acrylic resin-modified silicone resin, ester resin-modified silicone resin, epoxy resin-modified silicone resin, alkyd resin-modified silicone resin, and rubber-based silicone resin. Among them, methyl-based straight silicone resin, methylphenyl-based straight silicone resin, acrylic resin-modified silicone resin, or rubber-based silicone resin is preferred, and methyl-based straight silicone resin, methylphenyl-based straight silicone resin, or rubber-based silicone resin is more preferred.
[0152] As the silicone resin, commercially available products may be used, and examples of commercially available products include KR-300, KR-311, KR-251, X-40-2406M, and KR-282 manufactured by Shin-Etsu Chemical Co., Ltd.
[0153] Examples of the polyester resin include linear saturated polyesters synthesized from an aromatic dibasic acid or its ester-forming derivative and a diol or its ester-forming derivative. Specific examples of linear saturated polyesters include polyethylene terephthalate, polyethylene isophthalate, polybutylene terephthalate, poly(1,4-cyclohexylene dimethylene terephthalate), and polyethylene-2,6-naphthalate.
[0154] The content of the binder resin is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 60% by mass, and even more preferably 20% by mass to 60% by mass, based on the total mass of the colored layer, from the viewpoint of reducing the cure shrinkage of the colored layer. The ratio of the total amount of the binder resin to the total amount of the polymerizable compounds including the specific polymerizable compound, i.e., the total amount of the polymerizable compounds / the total amount of the binder resin, is preferably 0.3 to 1.5, and more preferably 0.5 to 1.0.
[0155] <<Other ingredients>> The colored layer may contain additives as necessary in addition to the above components. As the additives, known additives can be used, for example, surfactants described in paragraph 0017 of Japanese Patent No. 4502784 and paragraphs 0060 to 0071 of Japanese Patent Publication No. 2009-237362, thermal polymerization inhibitors (also called polymerization inhibitors, preferably phenothiazine) described in paragraph 0018 of Japanese Patent No. 4502784, and other additives described in paragraphs 0058 to 0071 of Japanese Patent Publication No. 2000-310706.
[0156] <<Formation of colored layer>> The method of forming the colored layer is not particularly limited, but it is preferable to form the colored layer using a composition for forming a colored layer. The composition for forming a colored layer preferably contains a colorant, and more preferably contains a colorant and an organic solvent. The composition for forming a colored layer may further contain other components described above. The composition for forming a colored layer can be prepared, for example, by mixing an organic solvent and a component contained in the colored layer, such as a colorant. The content of the components contained in the colored layer is described as the content (mass%) relative to the total mass of the colored layer, but when these components are contained in the composition for forming a colored layer, the content is to be read as the content (mass%) relative to the total solid content of the composition for forming a colored layer.
[0157] In addition, when the composition for forming a colored layer contains a pigment as a colorant, it is preferable to prepare a pigment dispersion containing the pigment and its dispersant in advance and use this pigment dispersion to prepare the composition for forming a colored layer, from the viewpoint of further enhancing the uniform dispersibility and dispersion stability of the pigment.
[0158] The color layer forming composition may be one prepared in advance by the above-mentioned method, or a commercially available product may be used, or the color layer forming composition may be prepared immediately before coating.
[0159] -Organic solvents- As the organic solvent, any organic solvent that is commonly used can be used without any particular limitation.Specific examples of the organic solvent include esters, ethers, ketones, aromatic hydrocarbons, and the like.In addition, methyl ethyl ketone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, cyclohexanol, methyl isobutyl ketone, ethyl lactate, methyl lactate, and the like, which are the same as the solvents described in paragraphs 0054 and 0055 of U.S. Patent Application Publication No. 2005 / 282073, can also be suitably used as the organic solvent in the colored layer forming composition. Among them, 1-methoxy-2-propyl acetate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, diethylene glycol monoethyl ether acetate (ethyl carbitol acetate), diethylene glycol monobutyl ether acetate (butyl carbitol acetate), propylene glycol methyl ether acetate, methyl ethyl ketone, etc. are preferably used as organic solvents in the colored layer forming composition. These organic solvents may be used alone or in combination of two or more. The content of the organic solvent is not particularly limited, but is preferably 5% by mass to 90% by mass, more preferably 30% by mass to 70% by mass, based on the total mass of the colored layer forming composition (for example, coating liquid).
[0160] <Adhesive layer> The decorative film according to an embodiment of the present disclosure preferably has an adhesive layer from the viewpoint of adhesion to the housing to which the decorative film is attached or adhesion between layers. The material of the adhesive layer is not particularly limited and can be appropriately selected depending on the purpose. For example, the adhesive layer may be a layer containing a known pressure-sensitive adhesive or adhesive.
[0161] <<Adhesive>> Examples of the adhesive include acrylic adhesives, rubber adhesives, and silicone adhesives. Examples of the adhesive include the acrylic adhesives, ultraviolet (UV) curing adhesives, and silicone adhesives described in Chapter 2 of "Evaluation of Properties of Release Paper / Release Film and Adhesive Tape and Technology for Controlling Them," Information Agency, 2004. When the adhesive layer contains an adhesive, the adhesive layer may further contain a tackifier.
[0162] <<Adhesive>> Examples of adhesives include urethane resin adhesives, polyester adhesives, acrylic resin adhesives, ethylene vinyl acetate resin adhesives, polyvinyl alcohol adhesives, polyamide adhesives, silicone adhesives, etc. From the viewpoint of higher adhesive strength, urethane resin adhesives and silicone adhesives are preferred.
[0163] In the decorative film according to one embodiment, the relationship between the thickness (T2) of the colored layer, the thickness (T3) of the optical reflection layer (preferably a cholesteric liquid crystal layer), and the thickness (T4) of the adhesive layer preferably satisfies T4<10(T2+T3). By satisfying the above relationship, a decorative film that is thin and has excellent glitter and visibility can be obtained. More preferably, T4<8(T2+T3), even more preferably, T4<5(T2+T3), and particularly preferably, T4<3(T2+T3).
[0164] <<How to form an adhesive layer>> The method of forming the adhesive layer is not particularly limited, and examples thereof include a method of laminating a protective film on which an adhesive layer is formed so that the adhesive layer contacts an object (e.g., an optical reflection layer, an alignment layer, or a colored layer), a method of laminating an adhesive layer alone so that the adhesive layer contacts an object (e.g., an optical reflection layer, an alignment layer, or a colored layer), and a method of applying a composition containing a pressure-sensitive adhesive or adhesive onto an object (e.g., an optical reflection layer, an alignment layer, or a colored layer). A known method can be used as the lamination method. A preferred application method is the same as the application method of the liquid crystal composition.
[0165] The thickness of the adhesive layer in the decorative film is preferably 2 μm to 40 μm, more preferably 3 μm to 25 μm, further preferably 4 μm to 20 μm, and particularly preferably 4 μm to 15 μm, from the viewpoint of achieving both adhesive strength and handleability.
[0166] <Other layers> The decorative film according to an embodiment of the present disclosure may have layers other than those described above. Examples of the other layers include a self-repairing layer, an antistatic layer, an antifouling layer, an anti-electromagnetic wave layer, and a conductive layer, which are layers known in decorative films. The other layers in the decorative film according to an embodiment of the present disclosure can be formed by a known method. For example, a method of applying a composition (layer-forming composition) containing the components contained in these layers in a layer form and drying it can be mentioned.
[0167] <<Cover film>> The decorative film according to an embodiment of the present disclosure may have a cover film as the outermost layer on the optical reflection layer side based on the substrate for the purpose of preventing dirt, etc. The cover film may be made of any material that is flexible and has good peelability, and examples of such materials include resin films. Examples of such resin films include polyethylene films. The cover film is introduced into the decorative film by, for example, attaching it to an object (for example, an optical reflection layer). The method of attaching the cover film is not particularly limited, and examples of such methods include known attachment methods, and examples of such methods include a method of laminating the cover film on the object (for example, an optical reflection layer).
[0168] <Layer structure of decorative film> An example of the layer structure of the decorative film will be described with reference to Figs. 1 and 2. However, the layer structure of the decorative film is not limited to the layer structure shown in each figure. Fig. 1 is a schematic cross-sectional view showing an example of the layer structure of the decorative film according to the present disclosure. The decorative film 20 shown in Fig. 1 has a substrate 22, a mirror layer (optical reflection layer) 24 on the substrate 22, an alignment layer 26 on the mirror layer 24, a cholesteric liquid crystal layer (optical reflection layer) 28 on the alignment layer 26, and an adhesive layer 30 on the cholesteric liquid crystal layer 28.
[0169] Fig. 2 is a schematic cross-sectional view showing an example of the layer structure of the decorative film according to the present disclosure. The decorative film 50 shown in Fig. 2 has a mirror layer (optical reflection layer) 32, a substrate 34 on the mirror layer 32, a resin layer 36 on the substrate 34, an alignment layer 38 on the resin layer 36, and a cholesteric liquid crystal layer (optical reflection layer) 40 on the alignment layer 38.
[0170] <Method of manufacturing decorative film> The manufacturing method of the decorative film according to the embodiment of the present disclosure is not limited. For example, a decorative film having at least a substrate and two or more optical reflection layers can be manufactured by providing an optical reflection layer and, if necessary, a layer other than the optical reflection layer on a substrate. The above-mentioned methods can be used to form each layer. It is also possible to manufacture a plurality of laminates including two or more layers in advance and stack the plurality of laminates.
[0171] (Decoration method and decoration) The decoration method according to an embodiment of the present disclosure is not particularly limited as long as it is a decoration method using a decorative film according to an embodiment of the present disclosure. For example, the decoration method according to an embodiment of the present disclosure preferably includes a step of attaching the surface of the decorative film on the optical reflection layer side to the convex surface of the transparent body by a lamination or molding process. The decorative object according to an embodiment of the present disclosure is preferably a decorative object using a decorative film according to an embodiment of the present disclosure, and is preferably a decorative object obtained by a decorative method according to an embodiment of the present disclosure.
[0172] (Decorative molding) The decorated molded body according to one embodiment of the present disclosure includes the decorated film according to one embodiment of the present disclosure. That is, the decorated molded body according to one embodiment of the present disclosure has a base material and an optical reflection layer that develops color by optical interference or structural color, and at least two or more optical reflection layers are laminated, and the diffuse reflectivity of each optical reflection layer is different, or a printed layer is laminated between each optical reflection layer.
[0173] <Base material> The decorated molded body according to one embodiment of the present disclosure includes a substrate. For example, the substrate described in the above "decorative film" section can be used as the substrate. The preferred embodiment of the substrate is the same as the preferred embodiment of the substrate described in the above "decorative film". The substrate may have an uneven structure.
[0174] <Optical reflective layer> The decorated molded body according to one embodiment of the present disclosure includes at least two optical reflection layers. The optical reflection layer described in the above "Decorative Film" section can be used as the optical reflection layer. The preferred embodiment of the optical reflection layer is the same as the preferred embodiment of the optical reflection layer described in the above "Decorative Film" section. In one embodiment, the optical reflection layer is preferably a layer containing cholesteric liquid crystal.
[0175] <Resin layer> The decorative molded body according to an embodiment of the present disclosure preferably includes a resin layer between the substrate and the optical reflection layer. The resin layer particularly contributes to the formation of a linear convex structure in the optical reflection layer. For example, the resin layer can improve the conformability of the optical reflection layer to a surface having a linear convex structure (i.e., a linear convex surface) used as a mold for imparting a linear convex structure to the optical reflection layer. As a result, a desired linear convex structure can be easily imparted to the optical reflection layer.
[0176] The resin layer may be the same as that described in the "decorative film" section above. The preferred embodiment of the resin layer is the same as that described in the "decorative film" section above. The resin layer may have a linear convex structure. The resin layer preferably has the same convex structure as that of the optical reflection layer.
[0177] The thickness of the resin layer is preferably 0.5 to 10 times, more preferably 0.8 to 8 times, and particularly preferably 1 to 5 times, the depth of the linear convex structure of the optical reflecting layer.
[0178] <Colored layer> The decorated molded body according to one embodiment of the present disclosure preferably includes a colored layer. As the colored layer, the colored layer described in the above "decorative film" section can be used. The preferred embodiment of the colored layer is the same as the preferred embodiment of the colored layer described in the above "decorative film". The colored layer may have a linear convex structure.
[0179] The position of the colored layer is not limited. In an embodiment, the colored layer is preferably disposed between the substrate and the optical reflection layer. That is, the decorated molded body according to an embodiment preferably includes the substrate, the colored layer, and the optical reflection layer in this order. In an embodiment, the colored layer is preferably disposed on the opposite side of the substrate to the optical reflection layer. That is, the decorated molded body according to an embodiment preferably includes the colored layer, the substrate, and the optical reflection layer in this order.
[0180] <Alignment layer> The decorated molded body according to an embodiment of the present disclosure may include an alignment layer. The alignment layer is preferably in contact with an optical reflection layer (preferably a cholesteric liquid crystal layer). As the alignment layer, the alignment layer described in the above "Decorative Film" section can be used. A preferred embodiment of the alignment layer is the same as the preferred embodiment of the alignment layer described in the above "Decorative Film". The alignment layer may have a linear convex structure.
[0181] <Adhesive layer> The decorated molded body according to one embodiment of the present disclosure may include an adhesive layer. The adhesive layer may be disposed on the surface of the decorated molded body. The adhesive layer may be disposed between any two layers included in the decorated molded body. As the adhesive layer, the adhesive layer described in the above "Decorative Film" section may be used. A preferred embodiment of the adhesive layer is the same as the preferred embodiment of the adhesive layer described in the above "Decorative Film" section. The adhesive layer may have a linear convex structure.
[0182] <Other layers> The decorated molded body according to an embodiment of the present disclosure may include layers other than the layers described above. For example, the other layers may be the layers described in the "decorative film" section above.
[0183] In an embodiment, the decorated molded body according to an embodiment of the present disclosure preferably includes a substrate, an optical reflection layer, and a transparent body having a surface with a concave-convex structure, in this order. For example, by observing the decorated molded body in a direction from the transparent body to the substrate, a user can observe a color that is highly lustrous and has a wide variety of colors depending on the viewing direction. The transparent body is preferably in contact with an optical reflection layer (preferably a cholesteric liquid crystal layer). The transparent body may be in contact with the optical reflection layer via another layer (e.g., an orientation layer). The convex surface of the transparent body is preferably facing the optical reflection layer. Examples of the transparent body include transparent resins, glass, prisms, etc., and examples of the transparent bodies shown in Figures 7 and 8 include the transparent bodies.
[0184] <Layer structure of decorated molded body> Examples of the layer structure of the decorated molded body will be described with reference to Figures 3, 4, and 5. However, the layer structure of the decorated molded body is not limited to the layer structures shown in each figure.
[0185] Fig. 3 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. The decorated molded body 70 shown in Fig. 3 has, in this order, a substrate 22, a mirror layer (optical reflection layer) 24, an alignment layer 26, a cholesteric liquid crystal layer (optical reflection layer) 28, an adhesive layer 30, and a transparent body 60 having a concave-convex structure. The transparent body 60 is one form of a transparent body.
[0186] Fig. 4 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. The decorated molded body 80 shown in Fig. 4 has, in this order, a mirror layer (optical reflection layer) 32, a substrate 34, a resin layer 36, an alignment layer 38, a cholesteric liquid crystal layer (optical reflection layer) 40, and a transparent body 60 having a concave-convex structure.
[0187] Fig. 5 is a schematic cross-sectional view showing an example of a decorated molded body according to the present disclosure. The decorated molded body 90 shown in Fig. 5 has, in this order, a mirror layer (optical reflection layer) 32, a substrate 34, a resin layer 36, a cholesteric liquid crystal layer (optical reflection layer) 40, an alignment layer 38, and a transparent body 60 having a concave-convex structure.
[0188] <Manufacturing method of decorated molded body> The manufacturing method of the decorated molded body according to one embodiment of the present disclosure is preferably a method using the decorative film according to one embodiment of the present disclosure. The manufacturing method of the decorated molded body according to one embodiment of the present disclosure preferably includes a step of attaching the decorative film to a transparent body having an uneven structure on the optical reflection layer side. The decorative film according to one embodiment of the present disclosure is also excellent in three-dimensional moldability, and can be suitably used for manufacturing the decorated molded body, and is particularly suitable for manufacturing the decorated molded body by at least one molding selected from the group consisting of thermal lamination, three-dimensional molding, and insert molding. In addition, according to the decorative film according to one embodiment of the present disclosure, it is also possible to make a decorated molded body by attaching it to a molded body after molding. When producing a decorated molded body, by using the decorative film according to one embodiment of the present disclosure, it becomes possible to apply it to molds with more complex shapes, smaller shapes, etc., and the range of uses of the decorated molded body can be expanded. The layer structure of the decorated molded body obtained using the decorative film reflects the layer structure of the decorative film. In other words, the decorated molded body obtained using the decorative film includes each layer contained in the decorative film.
[0189] In addition, three-dimensional molding is also suitable as a molding method. For example, three-dimensional molding is preferably exemplified by thermoforming, vacuum molding, pressure molding, and vacuum pressure molding. The vacuum molding method is not particularly limited, but a method in which three-dimensional molding is performed in a heated state under vacuum is preferred. Vacuum refers to a state in which the pressure inside the room is reduced to a vacuum degree of 100 Pa or less. The temperature during three-dimensional molding may be appropriately set according to the molding substrate used, but is preferably a temperature range of 60°C or higher, more preferably a temperature range of 80°C or higher, and even more preferably a temperature range of 100°C or higher. The upper limit of the temperature during three-dimensional molding is preferably 200°C. The temperature during three-dimensional molding refers to the temperature of the molding substrate used for three-dimensional molding, and is measured by attaching a thermocouple to the surface of the molding substrate.
[0190] Vacuum molding can be carried out using vacuum molding techniques that are widely known in the molding field. For example, vacuum molding may be carried out using Formech 508FS manufactured by Nippon Touki Kogyo Co., Ltd.
[0191] The manufacturing method of the decorated molded body will be specifically described below. The manufacturing method of the decorated molded body according to one embodiment of the present disclosure preferably includes a step of preparing a decorative film having at least a substrate and two or more optical reflection layers, and a step of contacting the optical reflection layer with a surface having a concave-convex structure, applying a pressure of 0.01 MPa or more to the optical reflection layer, and imparting the concave-convex structure to the optical reflection layer. The surface having the concave-convex structure functions as a mold for imparting the concave-convex structure to the optical reflection layer. By contacting the optical reflection layer with the surface having the concave-convex structure and applying pressure to the optical reflection layer, the optical reflection layer is deformed along the surface having the concave-convex structure. As a result, the concave-convex structure is imparted to the optical reflection layer.
[0192] The layer structure of the decorative film may be determined according to the layer structure of the intended decorated molded body. For example, by using a decorative film having a base material, an optical reflection layer, a resin layer between the base material and the optical reflection layer, and another optical reflection layer on the surface opposite to the side having the resin layer of the base material, a decorated molded body including the base material, the resin layer, and the optical reflection layer in this order can be obtained.
[0193] The surface having the linear convex structure is defined by the outer surface of various articles. The surface having the concave-convex structure may be, for example, the surface of a mold, or may be the surface of an article other than a mold.
[0194] In the process of bringing the optical reflection layer into contact with the surface having a linear convex structure, the optical reflection layer may be brought close to the surface having a concave-convex structure, or the surface having the linear convex structure may be brought close to the optical reflection layer. The optical reflection layer may be brought into contact with the surface having the linear convex structure via another layer (e.g., an alignment layer).
[0195] The pressure applied to the optical reflection layer is preferably 0.1 Mpa or more, more preferably 0.3 Mpa or more, and particularly preferably 0.5 Mpa or more. The upper limit of the pressure applied to the optical reflection layer is not limited. The upper limit of the pressure applied to the optical reflection layer may be determined, for example, according to the processability of the optical reflection layer and the thickness of the decorative film. The pressure applied to the optical reflection layer is preferably 10 Mpa or less, more preferably 3 Mpa or less, and particularly preferably 1 Mpa or less.
[0196] The method of applying pressure to the optical reflection layer is not limited, and any known method can be used. Examples of the pressure application method include a method using compressed air and a method using a press machine.
[0197] In the method for producing a decorated molded body, for example, a transparent body having a surface with the above-mentioned uneven structure (i.e., an uneven surface) may be used as an article having a surface with an uneven structure. For example, a method for producing a decorated molded body according to an embodiment preferably includes a step of preparing a decorative film having at least a substrate and an optical reflection layer having a central wavelength of selective reflection wavelength in the range of 300 nm to 1,500 nm, and a step of contacting the optical reflection layer with the surface with the uneven structure by superposing a transparent body having a surface with an uneven structure and the decorative film, applying a pressure of 0.01 Mpa or more to the optical reflection layer, and imparting a linear convex structure to the optical reflection layer. After imparting a linear convex structure to the optical reflection layer, the transparent body may or may not be removed. When the transparent body is not removed, the transparent body is disposed, for example, as an outer layer of the decorated molded body.
[0198] <Application> The uses of the decorated molded body obtained as described above are not particularly limited, and the decorated molded body can be used for various articles. Particularly suitable uses of the decorated molded body include the interior and exterior of electronic devices (e.g., wearable devices and smartphones), the interior and exterior of automobiles, the interior and exterior of electrical products, and packaging containers.
[0199] (Decorative panel) The decorative panel according to an embodiment of the present disclosure includes a decorative film according to an embodiment of the present disclosure. The decorative film in the decorative panel is synonymous with the decorative film described in the "Decorative Film" section above.
[0200] The decorative panel can be manufactured, for example, by bonding the surface of the optical reflection layer side of the decorative molded body to the surface of the member that will be the surface layer of the decorative panel. For example, a glass panel can be used as the member that will be the surface layer of the decorative panel. For example, the above-mentioned adhesive layer can be used to bond the decorative molded body to the member that will be the surface layer of the decorative panel. The decorative molded body may be used alone as the decorative panel without combining it with other members.
[0201] An example of the layer structure of the decorative panel will be described with reference to FIG. 6. However, the layer structure of the decorative panel is not limited to the layer structure shown in FIG. 6. FIG. 6 is a schematic cross-sectional view showing an example of a decorative panel according to the present disclosure. The decorative panel 100 shown in FIG. 6 has, in this order, a mirror layer (optical reflection layer) 32, a base material 34, a resin layer 36, a cholesteric liquid crystal layer (optical reflection layer) 40, an alignment layer 38, a transparent body 60 having a concave-convex structure, an adhesive layer 42, and a glass panel 44.
[0202] The shape of the decorative panel is not limited. The shape of the decorative panel may be determined, for example, according to the application. The decorative panel may be, for example, flat. The decorative panel may also have a curved surface.
[0203] The decorative panel can be used, for example, for the interior and exterior of various articles (for example, electronic devices, automobiles, and electrical products). For example, when the decorative panel 100 shown in Fig. 6 is used as a housing for an electronic device, it is preferable to arrange the mirror layer 32, the base material 34, the resin layer 36, the cholesteric liquid crystal layer 40, the alignment layer 38, the transparent body 60 having a concave-convex structure, the adhesive layer 42, and the glass panel 44 from the inside to the outside of the housing. By observing the decorative panel 100 in the direction from the glass panel 44 to the mirror layer 32, the user can observe high brilliance and a rich variety of colors depending on the viewing direction.
[0204] (Electronic Devices) An electronic device according to an embodiment of the present disclosure includes a decorative panel according to an embodiment of the present disclosure. Examples of the electronic device include a wearable device and a smartphone. The decorative panel in the electronic device is synonymous with the decorative panel described in the above "Decorative Panel". The decorative panel is preferably used as a housing for the electronic device.
[0205] The method for manufacturing the electronic device is not limited, and a known method can be used. When a decorative panel is used as a housing for the electronic device, various electronic components of the electronic device can be accommodated inside the housing including the decorative panel, thereby manufacturing the electronic device including the decorative panel. EXAMPLES
[0206] The present disclosure will be described in more detail below with reference to examples. The scope of the present disclosure is not limited to the specific examples shown below.
[0207] Example 1 <Preparation of the support> As the supports, two sheets of Cosmoshine (registered trademark) A4100 (PET, thickness: 50 μm, film having an easy-adhesion layer on one side, manufactured by Toyobo Co., Ltd., A4 size) were prepared. Hereinafter, the two supports are referred to as Support 1A and Support 1B, respectively.
[0208] [Composition of Coating Solution 1 for Forming Orientation Layer] Modified polyvinyl alcohol as shown below: 28 parts by weight Citric acid ester (AS3, manufactured by Sankyo Chemical Co., Ltd.): 1.2 parts by mass Photopolymerization initiator (Irgacure 2959, manufactured by BASF): 0.84 parts by weight Glutaraldehyde: 2.8 parts by weight ·Water: 699 parts by mass Methanol: 226 parts by weight
[0209] Modified polyvinyl alcohol (The numbers to the right of each unit in the following compounds indicate the molar ratio.)
[0210] [ka]
[0211] <Preparation of Laminate 1-1> On the surface of the support 1A on which the easy-adhesion layer was not formed, the coating solution 1 for forming an alignment layer was applied by a wire bar coater. Then, the applied coating solution 1 for forming an alignment layer was dried at 100° C. for 120 seconds to prepare an alignment layer 1 having a layer thickness of 0.5 μm.
[0212] <Formation of Cholesteric Liquid Crystal Layer 1> The prepared alignment layer 1 was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1,000 rpm (revolutions per minute), conveying speed: 10 m / min, number of reciprocations: 1) in a direction rotated 31.5° counterclockwise from the short side direction of the alignment layer 1. The components contained in the coating solution 1 for forming a cholesteric liquid crystal layer shown below were stirred and dissolved in a container kept at 25° C. to prepare the coating solution 1 for forming a cholesteric liquid crystal layer (liquid crystal composition 1).
[0213] [Composition of Coating Solution 1 for Forming Cholesteric Liquid Crystal Layer] Methyl ethyl ketone: 150.6 parts by weight ·Liquid crystal compound 1 (rod-shaped liquid crystal compound): 92 parts by mass Photopolymerization initiator A (IRGACURE 907, manufactured by BASF): 0.50 parts by mass Chiral agent A: 4.00 parts by weight Chiral agent B: 4.00 parts by weight The following surfactant F1: 0.027 parts by weight
[0214] Liquid crystal compound 1 (monofunctional): The following rod-shaped liquid crystal compound. In the case of radical polymerization, even if an oxetanyl group (cationically polymerizable functional group) is attached, it is defined as monofunctional because it has only one acryloxy group (radical polymerizable group). The same applies to cationic polymerization.
[0215] [ka]
[0216] Chiral agent A (bifunctional): the following compound
[0217] [ka]
[0218] Chiral agent B (zero functionality): the following compound. In the following compound, Bu represents an n-butyl group.
[0219] [ka]
[0220] Surfactant F1: The following compound
[0221] [ka]
[0222] The prepared cholesteric liquid crystal layer forming coating solution 1 was applied to the rubbed surface of the alignment layer 1 using a wire bar coater and dried at 85° C. for 120 seconds. The exposure dose for the surface of the cholesteric liquid crystal layer of the formed laminate was 70 mJ / cm 2 .2 The entire surface was exposed to i-line light to produce a cholesteric liquid crystal layer 1 having a thickness of 3.0 μm.
[0223] The prepared cholesteric liquid crystal layer forming coating solution 1 was applied to the surface of the above-mentioned alignment layer 1 that had been subjected to the rubbing treatment using a wire bar coater, and dried at 85° C. for 120 seconds. The exposure dose for the surface of the cholesteric liquid crystal layer of the formed laminate was 70 mJ / cm 2 2 A laminate 1-1 was formed by forming a cholesteric liquid crystal layer 1 having a thickness of 3.0 μm through exposure to (i-line). The laminate 1-1 has a support 1A, an alignment layer 1, and a cholesteric liquid crystal layer 1 in this order.
[0224] <Preparation of Laminate 1-2> An acrylic adhesive (SK Dyne SG-50Y, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied to the surface of the separately prepared Cosmoshine (registered trademark) A4100 (i.e., support 1B) on which the easy-adhesion layer was formed, using a comma coater, and dried at 120°C for 2 minutes to form a resin layer 1 (adhesive layer) with a layer thickness of 20 μm, thereby forming a laminate 1-2. The laminate 1-2 has a support 1B and a resin layer 1.
[0225] <Preparation of Laminate 1-3> The laminate 1-1 and the laminate 1-2 were bonded together using a laminator so that the resin layer 1 was in contact with the cholesteric liquid crystal layer 1. The PET film on the laminate 1-1 side (i.e., the support 1A) was peeled off to obtain a laminate 1-3 in which the support 1B / resin layer 1 / cholesteric liquid crystal layer 1 / alignment layer 1 were laminated in this order.
[0226] <Preparation of Laminate 1-4> After corona treatment was performed on the surface of the alignment layer 1 of the laminate 1-3 using a tabletop corona treatment device (TEC-8XA, manufactured by Kasuga Seiki Co., Ltd., set output 70 W, operation speed 1 m / min, number of times: 5 reciprocations), a transparent body (thickness 50 μm, width 140 mm, length 70 mm) having an uneven pattern shown in FIG. 7 was used as a mold, and the surface of the alignment layer 1 of the laminate 1-3 was brought into contact with the convex surface of the transparent body, and pressure molding (TOM molding) was performed to form a laminate 1-4. For the pressure molding, a TOM molding machine NGF-0510-R (manufactured by Fuse Vacuum Co., Ltd.) was used, the molding temperature was 120° C., and the stretching ratio was 30% at the highest part. The pressure in the pressure molding was 0.3 MPa. The diffuse reflectance of the cholesteric liquid crystal layer 1 laminated on the uneven pattern was measured through the alignment layer 1 and was 75%. The diffuse reflectance measured through the alignment layer 1 is the same as the diffuse reflectance measured without the alignment layer 1 .
[0227] <Preparation of Molded Body 1> A layer of indium (50 nm) was formed on the support 1B of the laminate 1-4 using a vacuum sputtering device (VEP-1000, manufactured by ULVAC), and a mirror layer 1 was laminated to form a molded body 1 (i.e., a decorated molded body). The molded body 1 has a mirror layer 1, a support 1B, a resin layer 1, a cholesteric liquid crystal layer 1, and an alignment layer 1, in this order. Separately, an indium sputtered layer was formed on Cosmoshine (registered trademark) A4100 (PET, thickness: 50 μm, film having an easy-adhesion layer on one side, manufactured by Toyobo Co., Ltd., A4 size) under the same conditions as above, and the diffuse reflectivity of the mirror layer 1 was evaluated to be 4%.
[0228] Example 2 <Formation of Cholesteric Liquid Crystal Layer 2> Instead of forming a mirror layer 1, a coating liquid for forming an alignment layer 1 was applied to the support 1B of the laminate 1-4 of Example 1 using a wire bar coater. The applied coating liquid for forming an alignment layer 1 was then dried at 100° C. for 120 seconds to prepare an alignment layer 2 having a layer thickness of 0.5 μm. The prepared alignment layer 2 was subjected to a rubbing treatment (rayon cloth, pressure: 0.1 kgf (0.98 N), rotation speed: 1,000 rpm (revolutions per minute), conveying speed: 10 m / min, number of times: 1 round trip) in a direction rotated 31.5° counterclockwise based on the short side direction of the alignment layer 2. The components contained in the coating liquid for forming a cholesteric liquid crystal layer 2 shown below were stirred and dissolved in a container kept at 25° C. to prepare a coating liquid for forming a cholesteric liquid crystal layer 2 (liquid crystal composition 2).
[0229] [Composition of Coating Solution 2 for Forming Cholesteric Liquid Crystal Layer] Methyl ethyl ketone: 150.6 parts by weight ·Liquid crystal compound 1 (rod-shaped liquid crystal compound): 92 parts by mass Photopolymerization initiator A (IRGACURE 907, manufactured by BASF): 0.50 parts by mass Chiral agent A: 2.50 parts by weight Chiral agent B: 2.50 parts by weight Surfactant F1: 0.027 parts by weight
[0230] The prepared cholesteric liquid crystal layer forming coating solution 2 was applied to the rubbed surface of the alignment layer 2 using a wire bar coater, and dried at 85° C. for 120 seconds. The exposure dose for the surface of the cholesteric liquid crystal layer of the formed laminate was 70 mJ / cm 2 2 The entire surface was exposed to (i-line) to form a cholesteric liquid crystal layer 2 having a layer thickness of 8.0 μm. The diffuse reflectance of the formed cholesteric liquid crystal layer 2 was measured.
[0231] Furthermore, Nax Real 642 (mirror black, manufactured by Nippon Paint Co., Ltd.) was applied onto the cholesteric liquid crystal layer 2 using a wire bar coater and dried at 100°C for 120 seconds to form a colored layer 2 with a layer thickness of 8.0 μm, thereby producing a decorative panel 2. The diffuse reflectance of the cholesteric liquid crystal layer 1 was measured through the alignment layer 1. The diffuse reflectance measured through the alignment layer 1 is the same as the diffuse reflectance measured without the alignment layer 1.
[0232] Example 3 After forming the alignment layer 1 of Example 1, a laminate 3-1 was formed in the same manner as the laminate 1-1 of Example 1, except that a cholesteric liquid crystal layer-forming coating solution 1 was applied onto the alignment layer 1 without performing a rubbing treatment, and then dried to form a cholesteric liquid crystal layer 3. The laminate 3-1 has a support 1A, an alignment layer 1, and a cholesteric liquid crystal layer 3 in this order. The diffuse reflectance of the formed cholesteric liquid crystal layer 3 was measured.
[0233] A layer of indium (50 nm) was formed on the surface of the support 1A of the laminate 3-1 opposite to the cholesteric liquid crystal layer 3 using a vacuum sputtering device (VEP-1000, manufactured by ULVAC, Inc.), and a mirror layer 3 was laminated to form a molded body 3 (i.e., a decorated molded body). The molded body 3 has the mirror layer 3, the support 1A, the alignment layer 1, and the cholesteric liquid crystal layer 1 in this order. The diffuse reflectance of the mirror layer 1 was 4%, similar to that of the mirror layer 1 evaluated in Example 1.
[0234] Example 4 A laminate 4-4 was formed in the same manner as in the laminate 1-4 of Example 1, except that the cholesteric liquid crystal layer forming coating liquid 1 was replaced with the cholesteric liquid crystal layer forming coating liquid 2. An acrylic adhesive (SK Dyne SG-50Y, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied to the surface of the support 1B of the laminate 4-4 opposite to the surface on which the easy-adhesion layer was formed, using a comma coater, and dried at 120°C for 2 minutes to form an adhesive layer 4 having a layer thickness of 20 μm. Furthermore, the adhesive layer 4 was bonded to the surface of the molded body 1 of Example 1 opposite to the mirror layer 1 (i.e., the surface of the alignment layer 1 of the molded body 1 of Example 1) using a laminator to produce a molded body 4 (i.e., a decorated molded body). The diffuse reflectance of the mirror layer 1 was 4%, which was the same as that of the mirror layer 1 evaluated in Example 1. The diffuse reflectance of the cholesteric liquid crystal layer 1 and the cholesteric liquid crystal layer 2 was measured before the molded body 1 and the laminate 4-4 were bonded together. The diffuse reflectance of the cholesteric liquid crystal layer 1 was measured through the alignment layer 1 of the molded body 1, and the diffuse reflectance of the cholesteric liquid crystal layer 2 was measured through the alignment layer 1 of the laminate 4-4. The diffuse reflectance measured through the alignment layer 1 is the same as the diffuse reflectance measured without the alignment layer 1.
[0235] Example 5 A laminate 5-1 was formed in the same manner as the laminate 1-1 in Example 1. A laminate 5-2 was formed in the same manner as the laminate 1-1 in Example 1, except that the cholesteric liquid crystal layer forming coating liquid 2 was used. A black image pattern (printed layer) shown in FIG. 9 was printed on the surface of the laminate 5-1 on which the easy-adhesion layer was formed, using Acuity1600 (manufactured by Fujifilm Corporation, UV inkjet printer, resolution 320 dpi), to produce a laminate 5-3. Furthermore, an acrylic adhesive (SK Dyne SG-50Y, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied on the printed surface of the laminate 5-3 using a comma coater, and dried at 120°C for 2 minutes to form an adhesive layer 5 having a layer thickness of 20 μm. Furthermore, the surface of the laminate 5-2 on which the cholesteric liquid crystal layer 2 was formed and the adhesive layer 5 were bonded together using a laminator to form a laminate 5-4. Nax Real 642 (mirror black, manufactured by Nippon Paint Co., Ltd.) was applied using a wire bar coater to the surface of the support 1A in the laminate 5-2 portion of the laminate 5-4 opposite the side having the orientation layer 1A, and dried at 100°C for 120 seconds to form a colored layer 5 with a layer thickness of 8.0 μm, and the decorative panel 5 was produced. The diffuse reflectance of the cholesteric liquid crystal layer 1 and the cholesteric liquid crystal layer 2 was measured before the laminate 5-2 and the laminate 5-3 were bonded together.
[0236] Example 6 A layer of indium (50 nm) was formed on the printed surface (printed layer) of the laminate 5-3 of Example 5 using a vacuum sputtering apparatus (VEP-1000, manufactured by ULVAC), and a mirror layer 5 was laminated to form a decorative panel 6. The diffuse reflectance of the mirror layer 5 was 4%, similar to that of the mirror layer 1 evaluated in Example 1.
[0237] Comparative Example 1 A layer of indium (50 nm) was formed on the surface of Cosmoshine (registered trademark) A4100 (PET, thickness: 50 μm, film having an easy-adhesion layer on one side, manufactured by Toyobo Co., Ltd., A4 size) on which the easy-adhesion layer was formed, using a vacuum sputtering device (VEP-1000, manufactured by ULVAC, Inc.), and thereby mirror layer 1-B was laminated to form molded body 1-B. The diffuse reflectance of the mirror layer 1-B was 4%, similar to that of the mirror layer 1 evaluated in Example 1.
[0238] Comparative Example 2 A layer of indium (50 nm) was formed on the surface of the support 1A of the laminate 5-1 in Example 5 on which the easy-adhesion layer was formed, using a vacuum sputtering apparatus (VEP-1000, manufactured by ULVAC), and a mirror layer 2-B was laminated thereon to form a molded body 2-B. The diffuse reflectance of the mirror layer 2-B was 4%, similar to that of the mirror layer 1 evaluated in Example 1.
[0239] <Performance evaluation> -Diffuse reflectance- The absolute reflectance (Rs) and the integrated reflectance (Rd) were measured in the direction perpendicular to the substrate at wavelengths of 380 nm to 1,100 nm using a spectrophotometer V-670 manufactured by JASCO Corporation, and the diffuse reflectance (Rd-Rs) / Rd value of each optical reflection layer was calculated. The diffuse reflectance is the value at the wavelength that gives the highest reflectance among the maximum values of the reflection spectrum.
[0240] -Glitter- The reflectance of the molded body 1, the decorative panels 2, 5 and 6, the molded bodies 3 and 4, and the laminates 1-B and 2-B (hereinafter sometimes referred to as "molded bodies, etc.") was measured in the wavelength range of 380 nm to 1,100 nm from a direction perpendicular to the upper pattern of the panel using a spectrophotometer V-670 manufactured by JASCO Corporation. The reflectance is the highest maximum value of the reflection spectrum. The "upper pattern of the panel" refers to the alignment layer 1 for molded body 1 and decorated panel 2, the cholesteric liquid crystal layer 3 for molded body 3, the alignment layer 1 (on cholesteric liquid crystal layer 2) for molded body 4, the cholesteric liquid crystal layer 1 for decorated panels 5 and 6, the film for laminate 1-B, and the cholesteric liquid crystal layer 1 for laminate 2-B.
[0241] For the molded body, the surface (140 mm x 70 mm) of the upper pattern of the panel in plan view was divided into 10 mm areas (98 places), and the reflectance of the center of each area was measured. The evaluation criteria are as follows. The practical levels were A, B, and C, and the brilliance was judged to be high. As an evaluation result, C is preferable, B is more preferable, and A is particularly preferable. <<Evaluation Criteria>> A: There is an area on the surface where the reflectance differs by 40% or more. B: There are areas within the plane where the reflectance differs by 30% or more and less than 40%, but there are no areas where the reflectance differs by 40% or more. C: There are areas within the plane where the reflectance differs by 15% or more and less than 30%, and there are no areas where the reflectance differs by 30% or more. D: There is no area in the plane where the reflectance differs by 15% or more.
[0242] -Saturation- The reflectance spectrum of the molded body was measured in the wavelength range of 380 nm to 780 nm from the direction perpendicular to the upper pattern of the panel using a spectrophotometer V-670 manufactured by JASCO Corporation. The saturation C * ab was calculated.
[0243] The reflectance of the center of each of the 10 mm-sized areas (98 locations) mentioned above in the evaluation of glitter was measured. The evaluation criteria are as follows. The practical levels are A, B, and C, and the saturation is judged to be high. <<Evaluation Criteria>> A: There is an area on the surface with a saturation of 40 or more. B: There is an area within the surface where the saturation is 25 or more and less than 40. C: There is an area on the surface where the saturation difference is 10 or more and less than 25. D: The in-plane saturation is less than 10 in all cases.
[0244] - Viewing angle dependence of color (evaluation of whether a large change in color occurs depending on the viewing angle) - The molded products were evaluated based on the following criteria for the change in color when viewed from angles of 0° and 45° (e.g., yellow at 0° and blue at 45°) when the direction perpendicular to the surface direction of the upper pattern of the panel is taken as 0°. The practical levels were A, B, and C, and it was determined that there was a wide change in color depending on the viewing direction. As an evaluation result, C is preferable, B is more preferable, and A is particularly preferable. <<Evaluation Criteria>> A: There is a large change in color when viewed from a 0° angle and when viewed from a 45° angle. B: A change in color can be seen when viewed from a 0° direction and a 45° direction. C: A slight change in color is observed when viewed from a 0° direction and a 45° direction. D: There is almost no change in color when viewed from a 0° direction and when viewed from a 45° direction.
[0245] The evaluation results of Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 1. In Tables 1 and 2, "reflective layer" means "optical reflective layer".
[0246] [Table 1]
[0247] [Table 2]
[0248] The disclosure of Japanese Patent Application No. 2020-156576, filed on September 17, 2020, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. The optical reflecting layer has a base material and an optical reflection layer that exhibits color by optical interference or structural color, and the optical reflecting layer is laminated in at least two layers, The optical reflection layers have different diffuse reflectivities, or a print layer is laminated between the optical reflection layers; At least two of the optical reflection layers contain a cholesteric liquid crystal compound, A decorative film having a layer containing the cholesteric liquid crystal compound on each side of the substrate.
2. A decorated molded body comprising the decorative film according to claim 1.
3. A decorative panel comprising the decorative film according to claim 1 .
4. An electronic device comprising the decorative panel according to claim 3 .
Citation Information
Patent Citations
Authenticity identifying body and authenticity identifiable base material
JP2006153990A
Patch transferring medium
JP2010120230A
Transfer foil for in-mold having embossed layer serving also as hard coat layer, method of manufacturing the same and injection molded article
JP2012201016A
Thermal compression bonding film containing cholesteric liquid crystal layer and application of the same
JP2015072410A
Run-flat tire
JP2020203574A