Liquid crystal composition, optically anisotropic layer, optical film, polarizing plate, and image display device

The liquid crystal composition, featuring a reverse dispersion compound and optimized surfactant, addresses the challenges of uniformity and biodegradability in optically anisotropic layers, providing improved display device performance and environmental sustainability.

WO2024242041A1PCT designated stage expired Publication Date: 2024-11-28FUJIFILM CORP

Patent Information

Application Number
PCT/JP2024/018281
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-14
Filing Date
2024-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional liquid crystal compositions used in display devices face issues with uniform thickness and reflection control due to the adverse effects of polyfluoro group compounds, which have low biodegradability and cause cissing and wind unevenness during the formation of optically anisotropic layers.

Method used

A liquid crystal composition is developed that includes a reverse dispersion compound and a surfactant with specific structures, optimizing the surface energy and solubility parameters to form an optically anisotropic layer with suppressed repellency and wind unevenness without using polyfluoro group compounds.

Benefits of technology

The composition achieves uniform thickness and improved film quality in optically anisotropic layers, enhancing the performance of display devices while being environmentally friendly by avoiding polyfluoro compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018281_28112024_PF_FP_ABST
    Figure JP2024018281_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a liquid crystal composition that is capable of forming an optically anisotropic layer, in which pits and unevenness due to wind are suppressed during the formation of an inversely dispersive liquid crystal cured layer, without using a compound that has a polyfluoro group; an optically anisotropic layer; an optical film; a polarizing plate; and an image display device. An optically anisotropic layer according to the present invention is formed of a liquid crystal cured layer which is obtained by immobilizing the alignment state of a liquid crystal composition that contains an inversely dispersive compound (I) represented by formula (1), at least one liquid crystal compound, and a surfactant (II) that has a structure represented by formula (2) in each molecule, and the optically anisotropic layer satisfies the relationship of formula (3).
Need to check novelty before this filing date? Find Prior Art

Description

Liquid crystal composition, optically anisotropic layer, optical film, polarizing plate and image display device

[0001] The present invention relates to a liquid crystal composition, an optically anisotropic layer, an optical film, a polarizing plate and an image display device.

[0002] Conventionally, a circular polarizer consisting of a λ / 4 plate and a linear polarizer has been used in a display device to suppress the adverse effects of external light reflection. Examples of such a display device include an organic electroluminescence (EL) display device. Patent Document 1 discloses an embodiment of a circular polarizer using an optically anisotropic layer with reverse wavelength dispersion. A method of using a polymerizable compound exhibiting reverse wavelength dispersion to prepare an optically anisotropic layer with reverse wavelength dispersion is widely used because it enables accurate conversion of light wavelengths over a wide wavelength range and allows the optically anisotropic layer to be thin due to its high refractive index.

[0003] A change in the thickness of the optically anisotropic layer is accompanied by a change in retardation, which changes the color of the reflected light when the optically anisotropic layer is used as a circular polarizer in a display device. Therefore, these optically anisotropic layers are required to have a particularly uniform thickness in the plane. In order to achieve such a uniform thickness, it is required to apply the reverse dispersion liquid crystal composition uniformly when applying it to a substrate. In order to apply the composition uniformly, a polyfluoro group [-(CF 2 ) n It is known to use a liquid crystal composition containing a surfactant containing a group consisting of a reverse dispersion liquid crystal compound, a polymer surfactant having a repeating unit containing a polyfluoro group, and a solvent.

[0004] It is preferable to avoid the use of compounds having polyfluoro groups because they have low biodegradability, accumulate in living organisms and the environment, and may have long-term adverse effects on the human body and ecosystems. Patent Document 3 describes an embodiment using a liquid crystal composition containing a reverse dispersion liquid crystal compound, a polyacrylate-based surfactant, and a solvent.

[0005] JP 2015-200861 A JP 2020-052327 A JP 2021-152641 A

[0006] The present inventors have investigated the liquid crystal compositions and cured liquid crystal layers (optically anisotropic layers) described in Patent Document 3 and the like, and have found that, depending on the structure of the surfactant contained in the liquid crystal composition, repelling and wind unevenness may occur during the formation of the optically anisotropic layer.

[0007] Therefore, an object of the present invention is to provide a liquid crystal composition, an optically anisotropic layer, an optical film, a polarizing plate, and an image display device that can form an optically anisotropic layer in which repelling and wind unevenness are suppressed when forming a reverse dispersion liquid crystal cured layer, without using a compound having a polyfluoro group.

[0008] As a result of intensive research aimed at achieving the above object, the present inventors have found that by blending a predetermined surfactant into a liquid crystal composition for forming a reverse dispersion cured liquid crystal layer, an optically anisotropic layer can be formed in which repelling and wind unevenness are suppressed during the formation of the reverse dispersion cured liquid crystal layer, and have completed the present invention. That is, the present inventors have found that the above object can be achieved by the following configuration.

[0009] [1] An optically anisotropic layer comprising a cured liquid crystal layer obtained by fixing the alignment state of a liquid crystal composition containing a reverse dispersion compound (I) represented by formula (1) described below, at least one liquid crystal compound, and a surfactant (II) having a structure represented by formula (2) described below in its molecule, wherein the optically anisotropic layer satisfies the relationship represented by formula (3) described below. [2] The optically anisotropic layer according to [1], wherein the reverse dispersion compound (I) is a liquid crystal compound. [3] The optically anisotropic layer according to [1] or [2], wherein the surface free energy is 35 mN / m or less. [4] The optically anisotropic layer according to any one of [1] to [3], wherein the surface free energy is 24 mN / m or more. [5] The optically anisotropic layer according to any one of [1] to [4], wherein the surfactant (II) is a surfactant that, when a solution containing 0.08% by mass of the surfactant (II) and cyclopentanone and methyl ethyl ketone in a mass ratio of 4:1 is prepared, the surface tension of the solution is 22 mN / m or more. [6] The optically anisotropic layer according to [5], wherein the surfactant (II) is a surfactant that causes the surface tension of the solution to be 30 mN / m or less. [7] The optically anisotropic layer according to [6], wherein the surfactant (II) is a surfactant that causes the surface tension of the solution to be 27 mN / m or less. [8] The optically anisotropic layer according to any one of [1] to [7], wherein the surfactant (II) has a structure represented by formula (4) described below. [9] The optically anisotropic layer according to any one of [1] to [7], wherein the surfactant (II) has a structure represented by formula (5) described below.

[10] The optically anisotropic layer according to any one of [1] to [9], wherein, when the solubility parameter of the liquid crystal mixture is defined as a weighted average value obtained by multiplying the solubility parameters of all liquid crystal compounds contained in the liquid crystal composition by the content of each liquid crystal compound, the relative energy difference of the surfactant (II) with respect to the liquid crystal mixture in the solubility parameters is 6 to 12. Here, the relative energy difference means the difference between the solubility parameter of the surfactant (II) and the solubility parameter of the liquid crystal mixture.

[11] The optically anisotropic layer according to any one of [1] to [7] and

[10] , wherein the surfactant (II) is a polymer having a repeating unit A having a structure of formula (2) described below.

[12] The optically anisotropic layer according to

[11] , wherein the repeating unit A is a repeating unit having a structure represented by formula (6) described below.

[13] The optically anisotropic layer according to

[11] or

[12] , wherein the surfactant (II) is a polymer containing the repeating unit A in an amount of 40% by mass to 90% by mass.

[14] The optically anisotropic layer according to any one of

[11] to

[13] , wherein the surfactant (II) is a polymer having a weight-average molecular weight of 15,000 or less.

[15] The optically anisotropic layer according to

[10] , wherein the surfactant (II) is a polymer having a repeating unit A having a structure represented by formula (2) described below and a repeating unit B not having the structure represented by formula (2) described below, and wherein the relative energy difference in solubility parameter of the monomer of repeating unit B with respect to the liquid crystal mixture is 3 to 7. Here, the relative energy difference refers to the difference between the solubility parameter of the monomer of repeating unit B and the solubility parameter of the liquid crystal mixture.

[16] The optically anisotropic layer according to any one of

[11] to

[14] , wherein the surfactant (II) is a polymer having a repeating unit A and a repeating unit B not containing the structure of formula (2) described below, and the repeating unit B is a repeating unit containing a functional group that reacts with light or heat to form a crosslink.

[17] The optically anisotropic layer according to any one of

[11] to

[16] , wherein the surfactant (II) is a polymer having repeating units A with two or more different structures.

[18] The optically anisotropic layer according to [1], comprising two or more surfactants (II) with different structures.

[19] The optically anisotropic layer according to any one of [1] to

[18] , wherein the content of the surfactant (II) is 0.1 parts by mass or less per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, the 100 parts by mass of the liquid crystal compound, which is the basis for the content of the surfactant (II), refers to 100 parts by mass of the total amount of the liquid crystal compound, including the reverse dispersion compound (I).

[20] Ar in the formula (1) described below. 1 and Ar 2

[21] The optically anisotropic layer according to any one of [1] to

[19] , wherein each independently represents an aromatic ring selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8) described below. 1 and Ar 2each independently represent an aromatic ring selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8) described below.

[22] The optically anisotropic layer according to

[11] , wherein the surfactant (II) is a polymer having a repeating unit A and a repeating unit B not containing a structure represented by formula (2), and the repeating unit B is a repeating unit containing a structure represented by formula (7) described below.

[23] The optically anisotropic layer according to any one of [1] to

[22] , wherein the liquid crystal composition further contains a solvent, the solvent containing a high-boiling solvent having a boiling point of 130°C or higher, and the content of the high-boiling solvent is 150 parts by mass or more per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, the 100 parts by mass of the liquid crystal compound that is the basis for the content of the high-boiling solvent refers to 100 parts by mass of the total amount of the liquid crystal compound, including the reverse dispersion compound (I).

[24] The optically anisotropic layer according to

[11] , wherein the liquid crystal composition further contains a solvent, the solvent comprising a high-boiling solvent having a boiling point of 130°C or higher, and the content of the high-boiling solvent is 150 parts by mass or more per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, the 100 parts by mass of the liquid crystal compound, which is the basis for the content of the high-boiling solvent, refers to 100 parts by mass of the total amount of the liquid crystal compound, including the reverse dispersion compound (I).

[25] An optical film having the optically anisotropic layer according to any one of [1] to

[24] .

[26] A polarizing plate having the optically anisotropic layer according to any one of [1] to

[24] and a polarizer.

[27] The polarizing plate according to

[26] , further comprising a positive C plate.

[28] An image display device having the optically anisotropic layer according to any one of [1] to

[24] .

[29] A liquid crystal composition containing a reverse dispersion compound (I) represented by formula (1) described later, at least one liquid crystal compound, and a surfactant (II) having a structure represented by formula (2) described later in the molecule.

[30] The liquid crystal composition according to

[29] , wherein the content of the surfactant (II) is 0.1 parts by mass or less relative to 100 parts by mass of the liquid crystal compound.Here, 100 parts by mass of the liquid crystal compound, which is the basis for the content of the surfactant (II), refers to 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I) when the reverse dispersion compound (I) is a liquid crystal compound.

[31] Ar in formula (1) described later. 1 and Ar 2 each independently represent an aromatic ring selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8) described below.

[32] The liquid crystal composition according to any one of

[29] to

[31] , wherein the surfactant (II) is a polymer having a repeating unit A and a repeating unit B that does not contain a structure represented by formula (2) described below, and the repeating unit B is a repeating unit that contains a structure represented by formula (7):

[33] The liquid crystal composition according to any one of

[29] to

[32] , further comprising a solvent, the solvent including a high-boiling point solvent having a boiling point of 130°C or higher, and the content of the high-boiling point solvent is 150 parts by mass or more per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, 100 parts by mass of the liquid crystal compound, which is the basis for the content of the high-boiling point solvent, refers to 100 parts by mass of the total amount of the liquid crystal compound, including the reverse dispersion compound (I).

[0010] According to the present invention, it is possible to provide a liquid crystal composition, an optically anisotropic layer, an optical film, a polarizing plate, and an image display device, which are capable of forming an optically anisotropic layer in which repelling and wind unevenness are suppressed when forming a reverse dispersion liquid crystal cured layer.

[0011] FIG. 1 is a schematic cross-sectional view showing an example of an optical film.

[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the upper and lower limits. In this specification, the upper or lower limit of a numerical range described in a stepwise manner may be replaced with the upper or lower limit of another stepwise manner. In this specification, the upper or lower limit of a numerical range described in a stepwise manner may be replaced with a value shown in the Examples. In this specification, each component may be a single substance corresponding to the component, or two or more substances may be used in combination. When two or more substances are used in combination for each component, the content of that component refers to the total content of the substances used in combination, unless otherwise specified. In addition, in this specification, "(meth)acrylate" is a notation representing "acrylate" or "methacrylate", "(meth)acrylic" is a notation representing "acrylic" or "methacrylic", and "(meth)acryloyl" is a notation representing "acryloyl" or "methacryloyl". In addition, the bonding direction of the divalent group (e.g., -O-CO-) represented in this specification is not particularly limited, and for example, "L 1 -L 2 -L 3 In the bond 2 When is —O—CO—, L 1 The position where it is bonded to the side is *1, L 3 If the position bonded to the side is *2, then L 2 may be *1-O-CO-*2 or *1-CO-O-*2.

[0013] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and the thickness direction retardation, respectively, at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan OPMF-1 (manufactured by Optoscience). Specifically, by inputting the average refractive index ((nx + ny + nz) / 3) and the film thickness (d (μm)) into the AxoScan OPMF-1, the following slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d. Although R0(λ) is displayed as a numerical value calculated by the AxoScan OPMF-1, it means Re(λ).

[0014] In this specification, examples of the substituent (monovalent substituent) include the substituents described below in Substituent Group A. In this specification, the phrase "optionally having a substituent" includes not only an embodiment in which no substituent is present, but also an embodiment in which one or more substituents are present. <Substituent Group A> Examples of the substituent include halogen atoms (for example, fluorine atoms, chlorine atoms, and bromine atoms); alkyl groups (preferably linear, branched, or cyclic alkyl groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, and particularly preferably 1 to 8 carbon atoms, such as linear alkyl groups having 1 to 6 carbon atoms (for example, methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl groups), branched alkyl groups having 3 to 6 carbon atoms (for example, isopropyl, isobutyl, tert-butyl, sec-butyl, neopentyl, isohexyl, and 3-methylpentyl groups), and cyclic alkyl groups having 3 to 12 carbon atoms (for example, cyclopropyl, cyclopentyl, cyclohexyl, 1-norbornyl, and 1-adamantyl groups)); alkenyl groups (preferably alkenyl groups having 2 to 48 carbon atoms, more preferably 2 to 18 carbon atoms, such as vinyl groups, allyl groups, 1-butenyl groups, and 2-butenyl groups); alkynyl groups (preferably alkynyl groups having 2 to 6 carbon atoms, more preferably 2 to 4 carbon atoms, such as ethynyl groups, 1-propynyl groups, propargyl groups, 1-butynyl groups, and 2-butynyl groups); aryl groups (preferably aryl groups having 6 to 48 carbon atoms, more preferably 6 to 24 carbon atoms, such as phenyl groups, oligoaryl groups (naphthyl groups, anthryl groups), phenanthrenyl groups, fluorenyl groups, pyrenyl groups, triphenylenyl groups, and biphenyl groups); Heteroaryl groups (preferably heterocyclic groups having 1 to 32 carbon atoms, more preferably 1 to 18 carbon atoms, such as a 2-thienyl group, a 4-pyridyl group, a 2-furyl group, a 2-pyrimidinyl group, a 1-pyridyl group, a 2-benzothiazolyl group, a 1-imidazolyl group, a 1-pyrazolyl group, or a benzotriazol-1-yl group);arylalkyl groups (preferably arylalkyl groups having 7 to 15 carbon atoms, for example, benzyl group, phenethyl group, methylbenzyl group, phenylpropyl group, 1-methylphenylethyl group, phenylbutyl group, 2-methylphenylpropyl group, tetrahydronaphthyl group, naphthylmethyl group, naphthylethyl group, indenyl group, fluorenyl group, anthracenylmethyl group (anthrylmethyl group), phenanthrenylmethyl group (phenanthrylmethyl group)); silyl groups (preferably silyl groups having 3 to 38 carbon atoms, more preferably 3 to 18 carbon atoms, for example, trimethylsilyl group, triethylsilyl group, tributylsilyl group, t-butyldimethylsilyl group, t-hexyldimethylsilyl group); hydroxy groups; cyano groups; nitro groups; morpholino groups; Alkoxy groups (preferably alkoxy groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, methoxy, ethoxy, 1-butoxy, 2-butoxy, isopropoxy, t-butoxy, dodecyloxy, and cycloalkyloxy groups (for example, cyclopentyloxy and cyclohexyloxy)); aryloxy groups (preferably aryloxy groups having 6 to 48 carbon atoms, more preferably 6 to 24 carbon atoms, for example, phenoxy and 1-naphthoxy); alkenyloxy groups (preferably alkenyloxy groups having 2 to 6 carbon atoms, for example, vinyloxy, 1-propenyloxy, 2-n-propenyloxy (allyloxy), 1-n-butenyloxy, and prenyloxy); heterocyclic oxy groups (preferably heterocyclic oxy groups having 1 to 32 carbon atoms, more preferably 1 to 18 carbon atoms, such as a 1-phenyltetrazole-5-oxy group or a 2-tetrahydropyranyloxy group); silyloxy groups (preferably silyloxy groups having 1 to 32 carbon atoms, more preferably 1 to 18 carbon atoms, such as a trimethylsilyloxy group, a t-butyldimethylsilyloxy group or a diphenylmethylsilyloxy group); acyloxy groups (preferably acyloxy groups having 2 to 48 carbon atoms, more preferably 2 to 24 carbon atoms, such as an acetoxy group, a pivaloyloxy group, a benzoyloxy group, a dodecanoyloxy group, an acryloyloxy group or a methacryloyloxy group);hydroxyalkyleneoxy groups (preferably hydroxyalkyleneoxy groups having 2 to 10 carbon atoms, for example, a hydroxyethyleneoxy group); alkoxycarbonyloxy groups (preferably alkoxycarbonyloxy groups having 2 to 48 carbon atoms, more preferably 2 to 24 carbon atoms, for example, an ethoxycarbonyloxy group, a t-butoxycarbonyloxy group, or a cycloalkyloxycarbonyloxy group (for example, a cyclohexyloxycarbonyloxy group)); aryloxycarbonyloxy groups (preferably aryloxycarbonyloxy groups having 7 to 32 carbon atoms, more preferably 7 to 24 carbon atoms, for example, a phenoxycarbonyloxy group); carbamoyloxy groups (preferably carbamoyloxy groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, an N,N-dimethylcarbamoyloxy group, an N-butylcarbamoyloxy group, an N-phenylcarbamoyloxy group, or an N-ethyl-N-phenylcarbamoyloxy group); sulfamoyloxy groups (preferably sulfamoyloxy groups having 1 to 32 carbon atoms, more preferably 1 to 24 carbon atoms, such as an N,N-diethylsulfamoyloxy group or an N-propylsulfamoyloxy group); alkylsulfonyloxy groups (preferably alkylsulfonyloxy groups having 1 to 38 carbon atoms, more preferably 1 to 24 carbon atoms, such as a methylsulfonyloxy group, a hexadecylsulfonyloxy group or a cyclohexylsulfonyloxy group); arylsulfonyloxy groups (preferably arylsulfonyloxy groups having 6 to 32 carbon atoms, more preferably 6 to 24 carbon atoms, such as a phenylsulfonyloxy group); acyl groups (preferably acyl groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, such as a formyl group, an acetyl group, an acryloyl group, a methacryloyl group, a pivaloyl group, a benzoyl group, a tetradecanoyl group or a cyclohexanoyl group); an alkoxycarbonyl group (preferably an alkoxycarbonyl group having 2 to 48 carbon atoms, more preferably 2 to 24 carbon atoms, for example, a methoxycarbonyl group, an ethoxycarbonyl group, an octadecyloxycarbonyl group, a cyclohexyloxycarbonyl group, or a 2,6-di-tert-butyl-4-methylcyclohexyloxycarbonyl group);an aryloxycarbonyl group (preferably an aryloxycarbonyl group having 7 to 32 carbon atoms, more preferably an aryloxycarbonyl group having 7 to 24 carbon atoms, for example, a phenoxycarbonyl group); a carbamoyl group (preferably a carbamoyl group having 1 to 48 carbon atoms, more preferably a carbamoyl group having 1 to 24 carbon atoms, for example, a carbamoyl group, N,N-diethylcarbamoyl group, N-ethyl-N-octylcarbamoyl group, N,N-dibutylcarbamoyl group, N-propylcarbamoyl group, N-phenylcarbamoyl group, N-methyl-N-phenylcarbamoyl group, or N,N-dicyclohexylcarbamoyl group); an amino group (preferably an amino group having 32 or less carbon atoms, more preferably an amino group having 24 or less carbon atoms, for example, an amino group, a methylamino group, an N,N-dibutylamino group, a tetradecylamino group, a 2-ethylhexylamino group, or a cyclohexylamino group); anilino group (preferably an anilino group having 6 to 32 carbon atoms, more preferably 6 to 24 carbon atoms, for example, an anilino group, an N-methylanilino group); heterocyclic amino group (preferably a heterocyclic amino group having 1 to 32 carbon atoms, more preferably 1 to 18 carbon atoms, for example, a 4-pyridylamino group); carbonamido group (preferably a carbonamido group having 2 to 48 carbon atoms, more preferably 2 to 24 carbon atoms, for example, an acetamido group, a benzamido group, a tetradecanamido group, a pivaloylamido group, a cyclohexanamido group); ureido group (preferably a ureido group having 1 to 32 carbon atoms, more preferably 1 to 24 carbon atoms, for example, a ureido group, an N,N-dimethylureido group, an N-phenylureido group); imido group (preferably an imido group having 36 or less carbon atoms, more preferably 24 or less carbon atoms, for example, an N-succinimido group, an N-phthalimido group); an alkoxycarbonylamino group (preferably an alkoxycarbonylamino group having 2 to 48 carbon atoms, more preferably 2 to 24 carbon atoms, for example, a methoxycarbonylamino group, an ethoxycarbonylamino group, a t-butoxycarbonylamino group, an octadecyloxycarbonylamino group, or a cyclohexyloxycarbonylamino group); an aryloxycarbonylamino group (preferably an aryloxycarbonylamino group having 7 to 32 carbon atoms, more preferably 7 to 24 carbon atoms, for example, a phenoxycarbonylamino group);sulfonamido groups (preferably sulfonamido groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, methanesulfonamido groups, butanesulfonamido groups, benzenesulfonamido groups, hexadecanesulfonamido groups, and cyclohexanesulfonamido groups); sulfamoylamino groups (preferably sulfamoylamino groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, N,N-dipropylsulfamoylamino groups, and N-ethyl-N-dodecylsulfamoylamino groups); azo groups (preferably azo groups having 1 to 32 carbon atoms, more preferably 1 to 24 carbon atoms, for example, phenylazo groups and 3-pyrazolylazo groups); alkylthio groups (preferably alkylthio groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, methylthio groups, ethylthio groups, octylthio groups, and cyclohexylthio groups); an arylthio group (preferably an arylthio group having 6 to 48 carbon atoms, more preferably an arylthio group having 6 to 24 carbon atoms, for example, a phenylthio group); a heterocyclic thio group (preferably a heterocyclic thio group having 1 to 32 carbon atoms, more preferably a heterocyclic thio group having 1 to 18 carbon atoms, for example, a 2-benzothiazolylthio group, a 2-pyridylthio group, or a 1-phenyltetrazolylthio group); an alkylsulfinyl group (preferably an alkylsulfinyl group having 1 to 32 carbon atoms, more preferably an alkylsulfinyl group having 1 to 24 carbon atoms, for example, a dodecanesulfinyl group); an arylsulfinyl group (preferably an arylsulfinyl group having 6 to 32 carbon atoms, more preferably an arylsulfinyl group having 6 to 24 carbon atoms, for example, a phenylsulfinyl group); alkylsulfonyl groups (preferably alkylsulfonyl groups having 1 to 48 carbon atoms, more preferably 1 to 24 carbon atoms, for example, methylsulfonyl, ethylsulfonyl, propylsulfonyl, butylsulfonyl, isopropylsulfonyl, 2-ethylhexylsulfonyl, hexadecylsulfonyl, octylsulfonyl, and cyclohexylsulfonyl groups); arylsulfonyl groups (preferably arylsulfonyl groups having 6 to 48 carbon atoms, more preferably 6 to 24 carbon atoms, for example, phenylsulfonyl, and 1-naphthylsulfonyl groups);sulfamoyl groups (preferably sulfamoyl groups having 32 or less carbon atoms, more preferably 24 or less carbon atoms, for example, a sulfamoyl group, an N,N-dipropylsulfamoyl group, an N-ethyl-N-dodecylsulfamoyl group, an N-ethyl-N-phenylsulfamoyl group, an N-cyclohexylsulfamoyl group, or an N-(2-ethylhexyl)sulfamoyl group); phosphonyl groups (preferably phosphonyl groups having 1 to 32 carbon atoms, more preferably 1 to 24 carbon atoms, for example, a phenoxyphosphonyl group, an octyloxyphosphonyl group, or a phenylphosphonyl group); phosphinoylamino groups (preferably phosphinoylamino groups having 1 to 32 carbon atoms, more preferably 1 to 24 carbon atoms, for example, a diethoxyphosphinoylamino group, or a dioctyloxyphosphinoylamino group); epoxy groups; —NHCOCH; 3 ;-SO 2 NHC 2 H 4 OCH 3 ;-NHSO 2 CH 3 and the like, and two or more of these may be combined. These substituents may be further substituted with other substituents. When two or more substituents are present, they may be the same or different. If possible, they may be bonded to each other to form a ring.

[0015] [Liquid Crystal Composition] A liquid crystal composition is a composition that provides a coating layer that exhibits a liquid crystal phase within a predetermined temperature range. The liquid crystal composition of the present invention contains a reverse dispersion compound (I) represented by formula (1) described below, at least one liquid crystal compound, and a surfactant (II) (hereinafter also referred to as "specific surfactant") having a structure represented by formula (2) described below in its molecule. The reverse dispersion compound (I) may or may not exhibit liquid crystallinity. Furthermore, when the reverse dispersion compound (I) exhibits liquid crystallinity, the reverse dispersion compound (I) and the liquid crystal compound may be the same compound. However, in order to broaden the temperature range in which the liquid crystal phase is exhibited, it is preferable to further include a liquid crystal compound that does not exhibit reverse dispersion. The liquid crystal composition of the present invention is suitably used as a liquid crystal composition for forming a liquid crystal cured layer that constitutes the optically anisotropic layer of the present invention described below.

[0016] In the present invention, as described above, by blending a specific surfactant into the liquid crystal composition that forms the cured liquid crystal layer, repelling and wind unevenness can be suppressed during the formation of the cured liquid crystal layer, and an optically anisotropic layer with reverse dispersion properties and sufficient film thickness uniformity for application to a display device can be formed.

[0017] [Liquid Crystal Compound] The liquid crystal compound contained in the liquid crystal composition of the present invention is not particularly limited. The type of liquid crystal compound contained in the liquid crystal composition is not particularly limited. Generally, liquid crystal compounds can be classified into rod-shaped and discotic types based on their shape. Each type is further divided into low-molecular-weight and high-molecular-weight types. High-molecular-weight compounds generally refer to those with a degree of polymerization of 100 or more (Polymer Physics / Phase Transition Dynamics, Masao Doi, p. 2, Iwanami Shoten, 1992). Reverse dispersion liquid crystal compounds containing mesogenic groups as a branched structure are also known.

[0018] In the present invention, any liquid crystal compound can be used, but it is preferable to use a rod-shaped liquid crystal compound or a reverse dispersion liquid crystal compound, and it is more preferable to use two or more liquid crystal compounds selected from the group consisting of rod-shaped liquid crystal compounds and reverse dispersion liquid crystal compounds.

[0019] The liquid crystal compound is preferably a polymerizable liquid crystal compound having a polymerizable group. The polymerizable liquid crystal compound is preferably at least one polymerizable liquid crystal compound selected from the group consisting of polymerizable rod-shaped liquid crystal compounds and polymerizable reverse dispersion liquid crystal compounds. Examples of the polymerizable group include an acryloyl group, a methacryloyl group, an epoxy group, and a vinyl group. The alignment of the liquid crystal compound can be fixed by polymerizing a liquid crystal compound having such a polymerizable group in an aligned state. Note that, once the liquid crystal compound is fixed by polymerization, it no longer needs to exhibit liquid crystallinity.

[0020] [Reverse-Dispersion Compound (I)] The reverse-dispersion compound (I) contained in the liquid crystal composition of the present invention is a reverse-dispersion compound (I) represented by the following formula (1), and is preferably a liquid crystal compound. Here, reverse dispersion refers to "reverse wavelength dispersion," and a reverse-dispersion compound refers to a compound in which, when the in-plane retardation (Re) value at a specific wavelength (visible light range) of a retardation film produced using the compound is measured, the Re value remains the same or increases as the measured wavelength increases.

[0021] In the above formula (1), D 1 , D 2 , D 3 and D 4 each independently represents a single bond, or —CO—, —O—, —S—, —C(═S)—, or —CR 1 R 2 -, -CR 3 =CR 4 -, -NR 5 -, or a divalent linking group formed by a combination of two or more thereof, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 1 A G or SP G Also, A 1 , A 2 and A G each independently represents an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, or a divalent alicyclic hydrocarbon group which may have a substituent, provided that -CH 2 One or more of - may be substituted with -O-, -S- or -NH-. 1 , SP 2 and SP G each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, provided that —CH 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent.1 and L 2 each independently represents a monovalent organic group; 1 and L 2 At least one of Ar represents a polymerizable group. 1 and Ar 2 When at least one of the following is an aromatic ring represented by the following formula (Ar-4), L 1 and L 2 and L in the following formula (Ar-4): 3 and L 4 At least one of the groups represented by m represents a polymerizable group. In addition, m represents an integer of 0 to 2. When m is 2, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. Furthermore, l and n each independently represent 0 or an integer of 1 or more. When l is an integer of 2 or more, a plurality of A 1 may be the same or different, and a plurality of D 3 may be the same or different. When n is an integer of 2 or more, a plurality of D 4 may be the same or different, and a plurality of A 2 may be the same or different. p represents 0 or an integer of 1 or more. When p is an integer of 2 or more, a plurality of Ar 1 may be the same or different, and a plurality of D 2 When p is an integer of 2 or more and m is not 0, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. However, in the above formula (1), G 1 , D 1 and D 2 each represents a single bond; and 2 It is preferable to exclude embodiments in which represents a single bond and m represents 0.

[0022] In the above formula (1), D 1 , D 2 , D3 and D 4 Examples of the divalent linking group represented by one embodiment of the formula (I) include -CO-, -O-, -CO-O-, -C(=S)O-, and -CR 1 R 2 -, -CR 1 R 2 -CR 1 R 2 -, -O-CR 1 R 2 -, -CR 1 R 2 -O-CR 1 R 2 -, -CO-O-CR 1 R 2 -, -O-CO-CR 1 R 2 -, -CR 1 R 2 -O-CO-CR 1 R 2 -, -CR 1 R 2 -CO-O-CR 1 R 2 -, -NR 5 -CR 1 R 2 -, and -CO-NR 5 - and so on. 1 , R 2 and R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 1 , D 2 , D 3 and D 4 is preferably any one of a single bond, —CO—, —O—, and —CO—O—.

[0023] In the above formula (1), A 1 , A 2 and A G (G 1 A as one aspect of G The same applies hereinafter.) as an aromatic hydrocarbon ring, can be exemplified by an aromatic hydrocarbon ring having 6 to 20 carbon atoms, specifically a benzene ring, a naphthalene ring, an anthracene ring, a phenanthroline ring, etc. 1 , A2 and A G Examples of the aromatic heterocycle represented by one embodiment of the formula (1) include aromatic heterocycles having 5 to 20 carbon atoms, and specific examples thereof include a furan ring, a pyrrole ring, a thiophene ring, a pyridine ring, a thiazole ring, and a benzothiazole ring. 1 , A 2 and A G The divalent alicyclic hydrocarbon group represented by one embodiment of the formula (I) is preferably a 5-membered or 6-membered ring. The divalent alicyclic hydrocarbon group may be saturated or unsaturated, but is preferably a divalent saturated alicyclic hydrocarbon group. The -CH 2 One or more of the - may be substituted with -O-, -S-, or -NH-. Examples of such divalent alicyclic hydrocarbon groups include divalent alicyclic hydrocarbon groups having 5 to 12 carbon atoms, and specific examples include monocyclic hydrocarbon groups and bridged cyclic hydrocarbon groups, and more specific examples include those represented by the following formulas (g-1) to (g-10).

[0024] In addition, in the above formula (1), A 1 , A 2 and A G With regard to the above, examples of the substituent that the aromatic hydrocarbon ring, aromatic heterocycle, or divalent alicyclic hydrocarbon group may have include the substituents described in the above-mentioned Substituent group A, and among them, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferable.

[0025] In the above formula (1), SP 1 , SP 2 and SP G (G 1 SP as one aspect of GThe same applies hereinafter.) is a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, and is represented by, for example, a linear alkylene group having 1 to 20 carbon atoms or a branched alkylene group having 3 to 20 carbon atoms, a linear alkenylene group having 1 to 20 carbon atoms or a branched alkenylene group having 3 to 20 carbon atoms, or a linear alkynylene group having 1 to 20 carbon atoms or a branched alkynylene group having 3 to 20 carbon atoms. The linear alkylene group having 1 to 20 carbon atoms or a branched alkylene group having 3 to 20 carbon atoms is preferably an alkylene group having 1 to 12 carbon atoms, more preferably an alkylene group having 1 to 10 carbon atoms, and suitable examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group. As the linear alkenylene group having 1 to 20 carbon atoms or the branched alkenylene group having 3 to 20 carbon atoms, an alkenylene group having 2 to 10 carbon atoms is preferred, and an alkenylene group having 2 to 4 carbon atoms is more preferred, and a suitable example thereof is an ethenylene group. As the linear alkenylene group having 1 to 20 carbon atoms or the branched alkenylene group having 3 to 20 carbon atoms, an alkynylene group having 2 to 10 carbon atoms is preferred, and an alkynylene group having 2 to 4 carbon atoms is more preferred, and a suitable example thereof is an ethynylene group. In addition, in the case of SP 1 , SP 2 and SP G As described above, represents —CH which constitutes an aliphatic hydrocarbon group. 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)-, or -CO-. Examples of the substituent represented by Q include the substituents described in the above-mentioned substituent group A. Among them, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferable.

[0026] In the present invention, from the viewpoint of easily exhibiting liquid crystallinity, G 1 However, the above-mentioned A G or SP G Among them, A G In addition, it is preferable that G in the above formula (1) is 1represents a cycloalkane ring or a cycloalkene ring. Specific examples of the cycloalkane ring include a cyclohexane ring, a cycloheptane ring, a cyclooctane ring, a cyclododecane ring, and a cyclodocosane ring. Specific examples of the cycloalkene ring include a cyclobutene ring, a cyclopentene ring, a cyclohexene ring, a cycloheptene ring, a cyclooctene ring, a cyclopentadiene ring, and a cyclohexadiene ring.

[0027] In the above formula (1), L 1 and L 2 Examples of the monovalent organic group represented by the formula (I) include an alkyl group, an aryl group, a heteroaryl group, an alkoxy group, a cyano group, and a carboxy group. The alkyl group may be linear, branched, or cyclic, with linear being preferred. The alkyl group preferably has 1 to 30 carbon atoms, more preferably 1 to 20, and even more preferably 1 to 10. The aryl group may be monocyclic or polycyclic, with monocyclic being preferred. The aryl group preferably has 6 to 25 carbon atoms, more preferably 6 to 10. The heteroaryl group may be monocyclic or polycyclic. The number of heteroatoms constituting the heteroaryl group is preferably 1 to 3. The heteroatoms constituting the heteroaryl group are preferably nitrogen atoms, sulfur atoms, or oxygen atoms. The heteroaryl group preferably has 6 to 18 carbon atoms, more preferably 6 to 12. The alkyl group, aryl group, and heteroaryl group may be unsubstituted or may have a substituent. Examples of the substituent include the substituents described in the above-mentioned substituent group A, and among them, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferred.

[0028] In the above formula (1), L 1 and L 2The polymerizable group represented by at least one of the above is not particularly limited, but a polymerizable group capable of radical polymerization or cation polymerization is preferred. As the radical polymerizable group, known radical polymerizable groups can be used, and preferred examples include an acryloyloxy group or a methacryloyloxy group. In this case, the polymerization rate of an acryloyloxy group is generally known to be faster, and from the viewpoint of improving productivity, an acryloyloxy group is preferred, but a methacryloyloxy group can also be used as the polymerizable group. As the cationically polymerizable group, known cationically polymerizable groups can be used, and specific examples include an alicyclic ether group, a cyclic acetal group, a cyclic lactone group, a cyclic thioether group, a spiro orthoester group, and a vinyloxy group. Among these, an alicyclic ether group or a vinyloxy group is preferred, and an epoxy group, an oxetanyl group, or a vinyloxy group is particularly preferred. Particularly preferred examples of the polymerizable group include polymerizable groups represented by any of the following formulas (P-1) to (P-20): In the following formulae, Me represents a methyl group, and Et represents an ethyl group.

[0029]

[0030] In the present invention, the durability of the optically anisotropic layer formed is improved by reducing the L 1 and L 2 However, each of them is preferably a polymerizable group, and more preferably an acryloyloxy group or a methacryloyloxy group.

[0031] In the above formula (1), m represents an integer of 0 to 2, l and n each independently represent an integer of 0 or 1 or greater, and p represents an integer of 0 or 1 or greater. Here, m is preferably 0 or 1, and from the viewpoint of synthesis, it is more preferably 1. From the viewpoint of solubility and compatibility with other liquid crystal compounds, l and n are preferably integers of 0 to 2. p is preferably an integer of 0 to 2, and more preferably 0 or 1.

[0032] In the present invention, the liquid crystallinity is easily exhibited in a wide temperature range including room temperature, and the birefringence (Δn) is also increased. For this reason, in the above formula (1), both l and n represent 1, and A 1 and A 2 Preferably, each of these represents a benzene ring.

[0033] On the other hand, in the above formula (1), Ar 1 and Ar 2 Each of the groups independently represents an aromatic ring selected from the group consisting of groups represented by the following formulae (Ar-1) to (Ar-8): 3 or D 4 *2 represents the bonding position with D 1 or D 2 When l is 0, D 3 The bonding position with 1 When m is 0, *2 represents the bonding position with D 2 When n is 0, D 4 The bonding position with 2 represents the bonding position with

[0034] In the above formulas (Ar-1) and (Ar-2), Q 1 represents N or CH, and Q 2 is -S-, -O-, or -N(R 6 )-, R 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Y 1 represents a monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms which may have a substituent, a monovalent aromatic heterocyclic group having 3 to 12 carbon atoms which may have a substituent, or a monovalent alicyclic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent, and -CH 2 One or more of - may be replaced by -O-, -S- or -NH-. 6Specific examples of the alkyl group having 1 to 6 carbon atoms represented by one embodiment of the formula (1) include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group. 1 Examples of the monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms represented by one embodiment of the formula (I) include aryl groups such as a phenyl group, a 2,6-diethylphenyl group, and a naphthyl group. 1 Examples of the monovalent aromatic heterocyclic group having 3 to 12 carbon atoms represented by one embodiment of the formula (1) include heteroaryl groups such as a thienyl group, a thiazolyl group, a furyl group, and a pyridyl group, as well as groups formed by removing one hydrogen atom from an indole ring, a benzofuran ring, a benzothiophene ring, a benzimidazole ring, a benzothiazole ring, and a benzoxazole ring. 1 The aromatic heterocyclic group having 3 to 12 carbon atoms represented by Y is preferably a group obtained by removing one hydrogen atom from a benzofuran ring or a benzothiazole ring. 1 Examples of the monovalent alicyclic hydrocarbon group having 6 to 20 carbon atoms represented by one embodiment of the formula (I) include a cyclohexyl group, a cyclopentyl group, a norbornyl group, and an adamantyl group. 1 Examples of the substituent that may be possessed by include the substituents described in the above-mentioned substituent group A, and among them, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferable.

[0035] In addition, in the above formulas (Ar-1) to (Ar-8), Z 1 , Z 2 and Z 3 each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, a monovalent aromatic heterocyclic group having 6 to 20 carbon atoms, a halogen atom, a cyano group, a nitro group, -OR 7 , -NR 8 R 9 , -SR 10 , -COOR 11 , or -COR 12represents R 7 ~R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Z 1 and Z 2 may be bonded to each other to form an aromatic ring. As the monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, an alkyl group having 1 to 15 carbon atoms is preferred, an alkyl group having 1 to 8 carbon atoms is more preferred, specifically, a methyl group, an ethyl group, an isopropyl group, a tert-pentyl group (1,1-dimethylpropyl group), a tert-butyl group, or a 1,1-dimethyl-3,3-dimethyl-butyl group is further preferred, and a methyl group, an ethyl group, or a tert-butyl group is particularly preferred. Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include monocyclic saturated hydrocarbon groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclodecyl, methylcyclohexyl, and ethylcyclohexyl groups; monocyclic unsaturated hydrocarbon groups such as cyclobutenyl, cyclopentenyl, cyclohexenyl, cycloheptenyl, cyclooctenyl, cyclodecenyl, cyclopentadienyl, cyclohexadienyl, cyclooctadienyl, and cyclodecadiene; bicyclo[2.2.1]heptyl, bicyclo[2.2.2]octyl, and tricyclo[5.2.1.0]diene; 2,6 ] decyl group, tricyclo[3.3.1.1 3,7 ]decyl group, tetracyclo[6.2.1.1 3,6 .0 2,7 ] dodecyl group, adamantyl group, and other polycyclic saturated hydrocarbon groups. Specific examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a 2,6-diethylphenyl group, a naphthyl group, and a biphenyl group, with an aryl group having 6 to 12 carbon atoms (particularly a phenyl group) being preferred. Specific examples of the monovalent aromatic heterocyclic group having 6 to 20 carbon atoms include a 4-pyridyl group, a 2-furyl group, a 2-thienyl group, a 2-pyrimidinyl group, and a 2-benzothiazolyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, with a fluorine atom, a chlorine atom, and a bromine atom being preferred. On the other hand, R 7~R 12 Specific examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group.

[0036] Z 1 and Z 2 As described above, may be bonded to each other to form an aromatic ring. For example, Z 1 and Z 2 Examples of the structure in which the groups bond to each other to form an aromatic ring include a group represented by the following formula (Ar-1a): In the following formula (Ar-1a), *1 represents D in the above formula (1). 3 or D 4 *2 represents the bonding position with D in the above formula (1). 1 or D 2 When l is 0, D 3 The bonding position with 1 When m is 0, *2 represents the bonding position with D 2 When n is 0, D 4 The bonding position with 2 represents the bonding position with In the above formula (Ar-1a), Q 1 , Q 2 and Y 1 Examples of the alkyl group include those described above in relation to formula (Ar-1).

[0037] In the present invention, liquid crystallinity is easily exhibited, solubility is improved, and the durability of the optically anisotropic film to be formed is improved. For these reasons, Z 1 and Z 2 It is preferable that either one of Z in the above formulae (Ar-1) to (Ar-8) represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms (particularly a tert-butyl group). 1 represents a hydrogen atom, and Z 2It is preferred that represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms (particularly a tert-butyl group).

[0038] In addition, in the above formulas (Ar-3) and (Ar-4), A 3 and A 4 are each independently —O—, —N(R 13 represents a group selected from the group consisting of —, —S—, and —CO—; R 13 represents a hydrogen atom or a substituent. 13 Examples of the substituent represented by one embodiment of the formula (I) include the substituents described in the above-mentioned Substituent Group A, and among them, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferable.

[0039] In the formula (Ar-3), X represents a nonmetallic atom of Groups 14 to 16. However, the nonmetallic atom may have a hydrogen atom or a substituent bonded thereto. Examples of the nonmetallic atom of Groups 14 to 16 represented by X include an oxygen atom, a sulfur atom, a hydrogen atom, or a nitrogen atom bonded to a substituent [=N-R N1 , R N1 represents a hydrogen atom or a substituent.], a carbon atom to which a hydrogen atom or a substituent is bonded [═C(R C1 ) 2 , R C1 represents a hydrogen atom or a substituent.] Examples of the substituent include the substituents described in the above-mentioned substituent group A, and among them, preferred examples include an alkyl group, an alkoxy group, an alkyl-substituted alkoxy group, a cyclic alkyl group, an aryl group (for example, a phenyl group, a naphthyl group, etc.), a cyano group, an amino group, a nitro group, an alkylcarbonyl group, a sulfo group, and a hydroxyl group.

[0040] In addition, in the above formula (Ar-4), D 5 and D 6 each independently represents a single bond, or —CO—, —O—, —S—, —C(═S)—, or —CR 1 R 2 -, -CR 3 =CR 4 -, -NR 5 -, or a divalent linking group formed by a combination of two or more thereof, R1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. Here, the divalent linking group is D in the above formula (1). 1 , D 2 , D 3 and D 4 Examples of the above-described examples are the same as those described above.

[0041] In addition, in the above formula (Ar-4), SP 3 and SP 4 each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, provided that —CH 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent. Examples of the substituent represented by Q include the substituents described in the above-mentioned substituent group A, and among these, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferred. Here, the divalent aliphatic hydrocarbon group is a group represented by the formula (1) SP 1 , SP 2 and SP G Examples of the above-described examples are the same as those described above.

[0042] In addition, in the above formula (Ar-4), L 3 and L 4 each independently represents a monovalent organic group; 3 and L 4 and L in the above formula (1) 1 and L 2 At least one of the following represents a polymerizable group. Here, the monovalent organic group is L in the above formula (1). 1 and L 2 Examples of the polymerizable group include the same as those described above. 1 and L 2 Examples of the above-described examples are the same as those described above.

[0043] In the above formulas (Ar-5) to (Ar-8), Ax represents an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. In the above formulas (Ar-5) to (Ar-8), Ay represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. Here, the aromatic rings in Ax and Ay may have a substituent, and Ax and Ay may be bonded to form a ring. In addition, Q 3 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms which may have a substituent. Examples of Ax and Ay include those described in paragraphs

[0039] to

[0095] of WO 2014 / 010325. 3 Specific examples of the alkyl group having 1 to 20 carbon atoms represented by include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group. Examples of the substituent include the substituents described in the above-mentioned substituent group A, and among these, an alkyl group, an alkoxy group, an alkoxycarbonyl group, an alkylcarbonyloxy group, or a halogen atom is preferred.

[0044] In the present invention, the alignment property of the liquid crystal composition is improved by using Ar in the above formula (1). 1 and Ar 2 represents any one of aromatic rings selected from the group consisting of groups represented by the above formulae (Ar-1), (Ar-2), and (Ar-4) to (Ar-8).

[0045] The reverse dispersion compound (I) represented by the above formula (1) is a compound in which p in the above formula (1) is 0, for example, the general formula (1) described in JP-A-2010-084032 (particularly, the compounds described in paragraphs

[0067] to

[0073] ), the general formula (II) described in JP-A-2016-053709 (particularly, the compounds described in paragraphs

[0036] to

[0043] ), the general formula (1) described in JP-A-2016-081035 (particularly, the compounds described in paragraphs

[0043] to

[0055] ), and, paragraphs

[0025] to

[0056] of WO 2021 / 060427 include compounds described in.

[0046] In addition, as the reverse dispersion compound (1) represented by the above formula (1), compounds in which p in the above formula (1) is 1 include compounds represented by the following formulas (I) to (XII), and specifically, D 1 , G 1 and D 2 and K includes compounds having the groups shown in Tables 1 to 8 below, and D in the following formulas (VII) to (XII) 1 , G 1 , G 1 and D 2 and K are compounds having the groups shown in Table 9 below. 1 The "*" in groups such as these indicates the bonding position. In the following description, a compound represented by the following formula (I) and having the group shown in 1-1 in Table 1 below will be referred to as "compound (I-1-1)," and compounds having other structural formulas and groups will be referred to in the same manner. For example, a compound represented by the following formula (II) and having the group shown in 2-3 in Table 2 below can be referred to as "compound (II-2-3)." In addition, the group adjacent to the acryloyloxy group in compound (I-1-1) and the like represents a propylene group (a group in which a methyl group is substituted with an ethylene group), and represents a mixture of positional isomers in which the position of the methyl group differs.

[0047]

[0048]

[0049]

[0050]

[0051]

[0052]

[0053]

[0054]

[0055]

[0056] [Surfactant (II) (Specific Surfactant)] The surfactant (II) (specific surfactant) contained in the liquid crystal composition of the present invention is a compound having a structure represented by the following formula (2): Furthermore, the surfactant (II) preferably has three or more structures represented by the following formula (2), and more preferably has three to six structures represented by the following formula (2).

[0057]

[0058] In the above formula (2), * represents a bonding position. 21 , R 22 , and R 23each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group. Examples of alkyl groups include linear alkyl groups having 1 to 18 carbon atoms and branched or cyclic alkyl groups having 3 to 18 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. Examples of alkenyl groups include alkenyl groups having 2 to 12 carbon atoms. Specific examples include a vinyl group, a 1-propenyl group, a 1-butenyl group, a 1-methyl-1-propenyl group, a 1-cyclopentenyl group, and a 1-cyclohexenyl group. Examples of aryl groups include aryl groups having 6 to 12 carbon atoms. Specific examples include a phenyl group, an α-methylphenyl group, and a naphthyl group. Examples of alkylenearyl groups include alkylenearyl groups having 7 to 30 carbon atoms.

[0059] In the present invention, the surface tension of the liquid crystal composition is reduced, and wind unevenness can be further suppressed when forming the cured liquid crystal layer. 21 , R 22 , and R 23 However, it is preferable that each of them is an alkyl group.

[0060] In the present invention, the surfactant (II) is preferably a compound having a structure represented by the following formula (4), because the surface tension of the liquid crystal composition is reduced and wind unevenness can be further suppressed during the formation of the cured liquid crystal layer.

[0061] In the above formula (4), * represents a bonding position. 31 ~R 39 Each of the groups independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group. Specific examples of these groups are R 21 , R 22 , and R 23 Examples of the above-described examples are the same as those described above.

[0062] In the present invention, the surfactant (II) is also preferably a compound having a structure represented by the following formula (5), because the surface tension of the liquid crystal composition is reduced and wind unevenness can be further suppressed during the formation of the cured liquid crystal layer.

[0063] In the above formula (5), * represents a bonding position. 41 ~R 45 Each of the groups independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group. Specific examples of these groups are R 21 , R 22 , and R 23 ns represents an integer of 1 to 15. When ns is an integer of 2 to 15, a plurality of R 41 may be the same or different, and multiple R 42 may be the same or different.

[0064] <Control of Uneven Distribution of Specific Surfactant by HSP> In the present invention, the compatibility of surfactant (II) with the liquid crystal compound described above and the solvent described below can be controlled, thereby further suppressing wind unevenness and repelling. Specifically, in the present invention, the solubility parameter (HSP) obtained by the Hansen sphere method can be used to appropriately adjust the compatibility. That is, the solubility parameters (δD, δP, δH) of the solvent, liquid crystal compound, and surfactant are calculated using commercially available software (HSPiP-Hansen Solubility Parameters in Practice), and the relative energy difference ΔHSP (compound 1, compound 2) between any compound 1 and compound 2 is calculated as shown in the following formula (H1): Formula (H1) ΔHSP (compound 1, compound 2) = [{δD (compound 1) - δD (compound 2)}^2 + {δP (compound 1) - δP (compound 2)}^2 + {δH (compound 1) - δH (compound 2)}^2]^ (1 / 2) δD (compound 1): dispersion term of compound 1 δD (compound 2): dispersion term of compound 2 δP (compound 1): dipole-dipole term of compound 1 δP (compound 2): dipole-dipole term of compound 2 δH (compound 1): hydrogen bond term of compound 1 δH (compound 2): hydrogen bond term of compound 2

[0065] When the liquid crystal composition of the present invention contains two or more liquid crystal compounds (including the reverse dispersion compound (I) exhibiting liquid crystallinity), the solubility parameter of the mixture (defined as a "liquid crystal mixture") is determined by multiplying the solubility parameter of each liquid crystal compound by the content of each liquid crystal compound and averaging the weighted average. That is, the solubility parameter of the liquid crystal mixture is defined by the following formula: δD (liquid crystal mixture) = δD (liquid crystal compound 1) × composition ratio (liquid crystal compound 1) + δD (liquid crystal compound 2) × composition ratio (liquid crystal compound 2) + ... δP (liquid crystal mixture) = δP (liquid crystal compound 1) × composition ratio (liquid crystal compound 1) + δP (liquid crystal compound 2) × composition ratio (liquid crystal compound 2) + ... δH (liquid crystal mixture) = δH (liquid crystal compound 1) × composition ratio (liquid crystal compound 1) + δH (liquid crystal compound 2) × composition ratio (liquid crystal compound 2) + ... δD (liquid crystal compound i): dispersion force term of liquid crystal compound i δP (liquid crystal compound i): dipole-dipole force term of liquid crystal compound i δH (liquid crystal compound i): hydrogen bonding force term of liquid crystal compound i Composition ratio (liquid crystal compound i): mass ratio of liquid crystal compound i when the liquid crystal mixture is taken as 1

[0066] In the present invention, the relative energy difference between the liquid crystal mixture and the surfactant (II) is preferably 6 to 12, more preferably 6 to 11, even more preferably 6 to 9, and particularly preferably 7 to 9. Here, the relative energy difference of the surfactant (II) with respect to the liquid crystal mixture means the distance between the solubility parameter of the surfactant (II) and the solubility parameter of the liquid crystal mixture, i.e., the above-mentioned relative energy difference ΔHSP.

[0067] <Repeating Unit A> In the present invention, the surfactant (II) is preferably a polymer containing a repeating unit A having the structure of the above formula (2) (hereinafter also abbreviated as "specific polymer"), because this reduces the surface tension of the liquid crystal composition and can further suppress wind unevenness during the formation of a cured liquid crystal layer.

[0068] In the present invention, the repeating unit A is preferably a repeating unit containing a structure represented by the following formula (6), and it is more preferable that both the repeating unit A and a repeating unit B described later are repeating units containing a structure represented by the following formula (6).

[0069] In the above formula (6), * represents a bonding position. 51 and R 52 each independently represents a hydrogen atom or an alkyl group. 53 represents a hydrogen atom or a substituent. 5 is —O— or —NR Z - where R Z represents a hydrogen atom or a substituent.

[0070] Here, R 51 and R 52 Examples of the alkyl group represented by one embodiment of the formula (1) include a linear alkyl group having 1 to 18 carbon atoms, and a branched or cyclic alkyl group having 3 to 18 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. 51 and R 52 is preferably a hydrogen atom. 53 Examples of the substituent represented by one embodiment of the formula (1) include an alkyl group, an alkenyl group, an aryl group, or a substituent having a linking group and a structure represented by the formula (2) at the terminal. 2 -CO-L 1 -L 2 -(Si(R 11 ) (R 12 ) (R 13 ))m is also included. 1 is -O- or -NR Z - represents. 11 , R 12 , and R 13 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group; m represents an integer of 2 or more; L 2 represents an (m+1)-valent linking group. 53 is preferably an alkyl group, more preferably a linear alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group or an ethyl group. 53 is preferably a hydrogen atom or a methyl group.5 One aspect of the invention is represented by -NR Z -Regarding R Z The substituent represented by one embodiment of the group is preferably an alkyl group, more preferably a linear alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group or an ethyl group. 5 is preferably —O— or —NH—, and more preferably —O—.

[0071] In the present invention, the repeating unit A is preferably a repeating unit represented by the following formula (6-1), for the reasons that the surface tension of the liquid crystal composition is reduced and wind unevenness can be further suppressed during the formation of a cured liquid crystal layer while maintaining compatibility with the liquid crystal compound:

[0072]

[0073] In the above formula (6-1), R 51 , R 52 and R 53 and L 5 is the same as that explained in the above formula (6). 21 , R 22 , and R 23 is the same as that explained in the above formula (2). 21 may be the same or different, and multiple R 22 may be the same or different, and multiple R 23 may be the same or different. ms represents an integer of 2 or more. L 6 represents a ms+1-valent linking group.

[0074] In the above formula (7), ms is preferably an integer of 3 or more, more preferably an integer of 3 to 6, and even more preferably an integer of 3 to 5.

[0075] In the above formula (7), L 6Suitable examples of the ms+1-valent linking group represented by the formula (1) include ms+1-valent hydrocarbon groups having 1 to 10 carbon atoms which may have a substituent, in which some of the carbon atoms constituting the hydrocarbon group may be substituted with heteroatoms. Here, the substituent that the hydrocarbon group may have is preferably an alkyl group, more preferably a linear alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group or an ethyl group. Examples of heteroatoms include a silicon atom, an oxygen atom, and a nitrogen atom.

[0076] Specific examples of the repeating unit A include repeating units corresponding to the monomers represented by the following formulae K-1 to K-34. Bu represents a butyl group. In the examples described below, the monomer represented by the following formula K-1 will be referred to as "monomer K-1". The same applies to other monomers. The monomer represented by the following formula K-29 is represented by -(O-Si(CH 3 ) 2 Since this is a mixture of monomers with different numbers of )-, it is expressed as an average value with n ≈ 10. The same applies to the monomer represented by the following formula K-30.

[0077]

[0078]

[0079] In the present invention, the content of the repeating unit A in the specific polymer (surfactant (II)) is preferably 40% by mass or more and 90% by mass or less, and more preferably 50% by mass or more and 80% by mass or less, relative to the mass of the specific polymer. Here, when the content of the repeating unit A is 40% by mass or more, wind unevenness is further suppressed when the cured liquid crystal layer is formed, and when the content of the repeating unit A is 90% by mass or less, repelling is further suppressed when the cured liquid crystal layer is formed, and the orientation of the cured liquid crystal layer is further improved.

[0080] In the present invention, the surfactant (II) is preferably a polymer having repeating units A with two or more different structures, since this inhibits aggregation of the surfactant (II) and suppresses repelling.

[0081] <Repeating Unit B> In order to control the compatibility with the liquid crystal compound and the solvent described below and to adjust the surface tension in the process from coating to drying, the surfactant (II) is preferably a polymer (hereinafter also abbreviated as "specific copolymer") having, in addition to the repeating unit A, one or more repeating units B that do not contain the structure of the above formula (2). Here, when the surfactant (II) is a specific copolymer, it may be a random copolymer or a block copolymer, but from the viewpoint of compatibility with other components in the liquid crystal composition, it is preferably a random copolymer. Note that the surfactant (II) (specific surfactant) used in the examples described below is a random copolymer unless otherwise specified.

[0082] The structure of the main chain of the repeating unit B is not particularly limited, and may be a known structure, for example, a skeleton selected from the group consisting of (meth)acrylic, (meth)acrylamide, styrene, siloxane, cycloolefin, methylpentene, and aromatic ester. Among these, a skeleton selected from the group consisting of (meth)acrylic, (meth)acrylamide, siloxane, and cycloolefin is more preferred, and a (meth)acrylic skeleton or a (meth)acrylamide skeleton is even more preferred.

[0083] In the present invention, the relative energy difference of the monomer of repeating unit B with respect to the liquid crystal mixture is preferably 1 to 8, more preferably 3 to 7, and even more preferably 4 to 7. Here, the relative energy difference of the monomer of repeating unit B with respect to the liquid crystal mixture means the distance between the solubility parameter of the monomer of repeating unit B and the solubility parameter of the liquid crystal mixture, i.e., the above-mentioned relative energy difference ΔHSP.

[0084] In the present invention, it is preferable that the repeating unit B is a repeating unit containing a functional group that reacts with light or heat to form a crosslink. Examples of the functional group include radically polymerizable groups or cationically polymerizable groups, with radically polymerizable groups being preferred. Examples of the functional group include functional groups capable of forming covalent complexes with hydroxyl groups. Examples of the radically polymerizable group include known radically polymerizable groups, such as vinyl groups, allyl groups, vinyloxy groups, maleimide groups, allyloxy groups, (meth)acryloyl groups, (meth)acryloyloxy groups, and (meth)acrylamide groups. Among these, (meth)acryloyl groups or (meth)acryloyloxy groups are preferred. Examples of the cationically polymerizable group include known cationically polymerizable groups, such as alicyclic ether groups, cyclic acetal groups, cyclic lactone groups, cyclic thioether groups, spiro orthoester groups, and vinyloxy groups. Among these, an alicyclic ether group or a vinyloxy group is preferred, and an epoxy group, an oxetanyl group, or a vinyloxy group is more preferred. The functional group capable of forming a covalent bond complex with a hydroxyl group is a boronic acid group (-B(OH) 2 ) and a boronic ester group (—B(OR B1 ) 2 ) group is preferred. B1 R each independently represent a hydrogen atom, an alkyl group which may have a substituent, an aryl group which may have a substituent, or a heteroaryl group which may have a substituent, with a hydrogen atom or an alkyl group which may have a substituent being preferred. The alkyl group preferably has 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms. The aryl group preferably has 4 to 20 carbon atoms, more preferably 6 to 12 carbon atoms. An example of an aryl group is a phenyl group. The heteroaryl group preferably has 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms. Examples of heteroatoms contained in the heteroaryl group include an oxygen atom, a nitrogen atom, and a sulfur atom. B1 R may be bonded to each other to form a ring. B1 The number of members in the ring formed by bonding together is preferably 4 to 8, and more preferably 5 to 6.

[0085] The number of the functional groups contained in the repeating unit B is preferably 1 or more, more preferably 1 to 3, and even more preferably 1 or 2.

[0086] As the repeating unit B having the functional group, a repeating unit represented by the following formula (b1) is preferred in terms of superior compatibility with the liquid crystal compound.

[0087]

[0088] In formula (b1), R 51 , R 52 , R 53 , and L 5 is the same as that explained in the above formula (6-1).

[0089] In formula (b1), L 7 represents a single bond or a divalent linking group. Examples of the divalent linking group include divalent aliphatic hydrocarbon groups having 1 to 20 carbon atoms which may have a substituent. The aliphatic hydrocarbon group having 1 to 20 carbon atoms is preferably an alkylene group having 1 to 15 carbon atoms, more preferably an alkylene group having 2 to 8 carbon atoms. The -CH constituting the divalent aliphatic hydrocarbon group 2 One or more of the - may be independently substituted with a group selected from -O-, -S-, -CO-, and -N(Q)-. 2 - may be substituted. The definition and preferred embodiments of Q are as described above. 7 Among these, alkylene groups having 2 to 8 carbon atoms which may have a substituent, or *-(L 71 -O) n7 - * is preferred. * represents the bonding position. n7 represents an integer of 1 to 8. L 71 each independently represents an alkylene group having 1 to 6 carbon atoms which may have a substituent, and preferably an alkylene group having 2 to 4 carbon atoms which may have a substituent. 7 The divalent linking group represented by the formula (I) may be a group containing a mesogen group. Examples of the group containing a mesogen group include *-SP 1 -M 1 - * is preferred. * indicates the bonding position. SP1 represents a spacer group, M 1 represents a mesogenic group.

[0090] The spacer group is not particularly limited as long as it is a divalent linking group that does not contain a ring structure, and examples thereof include divalent chain aliphatic hydrocarbon groups having 1 to 20 carbon atoms. As the divalent chain aliphatic hydrocarbon group having 1 to 20 carbon atoms, an alkylene group having 1 to 15 carbon atoms is preferred, and an alkylene group having 1 to 8 carbon atoms is more preferred. Specific examples thereof include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a methylhexylene group, and a heptylene group. The —CH group constituting the divalent chain aliphatic hydrocarbon group 2 One or more of - may be independently substituted with a group selected from -O-, -S-, -CO-, and -N(Q)-. 2 - may be substituted. Q represents a hydrogen atom or a substituent. The substituent represented by Q is preferably an alkyl group, more preferably a linear alkyl group having 1 to 4 carbon atoms, and even more preferably a methyl group or an ethyl group. Among others, the spacer group is preferably *-(CH 2 -CH 2 -O) n1 - *, * - (CH 2 ) n2 -O-*, or *-(CH 2 ) n2 -O-CO-* is preferred. * represents the bonding position. n1 represents an integer of 1 to 4. n2 each independently represents an integer of 1 to 6, preferably an integer of 2 to 4.

[0091] Known mesogenic groups can be used as the mesogenic group. For example, see "Flussige Kristalle in Tabellen II" (VEB Deutsche Verlag fur Grundstoff Industrie, Leipzig, published in 1984), particularly pages 7 to 16, and "Liquid Crystal Handbook" edited by the Liquid Crystal Handbook Editorial Committee (Maruzen, published in 2000), particularly Chapter 3. The mesogenic group is preferably a group having at least one cyclic structure selected from the group consisting of an aromatic hydrocarbon group, a heterocyclic group, and an alicyclic group. In order to improve the degree of alignment of the liquid crystal compound, the mesogenic group is preferably a group having an aromatic hydrocarbon group or an alicyclic group, which may have a substituent; more preferably a group having two to four aromatic hydrocarbon groups, which may have a substituent; and even more preferably a group having three aromatic hydrocarbon groups, which may have a substituent. The substituent is preferably an alkyl group, an alkoxy group, an alkyl ester group, or an acetyl group, and more preferably a methyl group, a tert-butyl group, a methoxy group, or a methyl ester group.

[0092] Examples of the substituent that the divalent linking group may have include a hydroxy group, a halogen atom, an amino group, an alkyl group, an alkoxy group, an acyl group, an aryl group, a nitro group, a cyano group, an alkylcarbonyl group, and a sulfonyl group.

[0093] In formula (b1), P 1 represents a radically polymerizable group or a cationically polymerizable group. Preferred embodiments of the radically polymerizable group or the cationically polymerizable group are as described above.

[0094] Specific examples of repeating units having a polymerizable group include the repeating units shown below: In the repeating units shown below, n represents an integer of 1 or more (typically an integer of 1 to 6).

[0095]

[0096]

[0097] In the present invention, the repeating unit B is preferably a repeating unit containing a structure represented by the following formula (7), because it is easy to synthesize and has excellent controllability of the solubility parameter by adjusting np and nq below.

[0098] In the above formula (7), R 61 represents a hydrogen atom or a methyl group. 62 represents a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, np represents an integer of 1 to 4, and nq represents an integer of 1 to 100.

[0099] The repeating unit B is preferably a repeating unit having any one of a hydroxy group, a boronic acid group, a boronic acid ester group, a boronic acid amide group, an epoxy group, an oxetane group, a vinyl group, a styryl group, a (meth)acryloyl group (including a (meth)acrylamide group), a maleimide group, a naphthyl group, and a mesogenic group. Specific structures of the repeating unit B having a mesogenic group include compounds described in WO 2023 / 54164.

[0100] In the present invention, the content of the repeating unit B in the specific copolymer is preferably 0 to 50% by mass, more preferably 10 to 50% by mass, based on the mass of the specific copolymer.

[0101] In the present invention, the surfactant (II) is preferably a surfactant that inhibits aggregation of the surfactant (II) in the composition and suppresses repelling, and that, when a solution containing ethyl ketone in a 4:1 mass ratio is prepared, the surface tension of the solution is preferably 22 mN / m or more. Furthermore, since the surfactant (II) stabilizes the surface tension of the composition and suppresses wind unevenness, it is preferably a surfactant that causes the surface tension of the solution to be 30 mN / m or less, and more preferably a surfactant that causes the surface tension of the solution to be 27 mN / m or less. Here, the surface tension of the solution is measured twice using a static surface tensiometer (model number: CBVP-Z) manufactured by Kyowa Interface Science Co., Ltd.

[0102] The liquid crystal composition of the present invention preferably contains two or more surfactants (II) having different structures, since this inhibits aggregation of the surfactant (II) and suppresses repelling.

[0103] <Content> The content of surfactant (II) is preferably 0.01 to 10% by mass, more preferably 0.02 to 1% by mass, and even more preferably 0.04 to 0.5% by mass, relative to the total solid content (100% by mass) of the liquid crystal composition, from the viewpoint of achieving superior effects of the present invention. Furthermore, the content of surfactant (II) is preferably 0.1 parts by mass or less relative to 100 parts by mass of the liquid crystal compound, since this suppresses aggregation of the surfactant (II) and inhibits repelling and wind-induced unevenness. Here, the 100 parts by mass of the liquid crystal compound, which is the basis for the content of surfactant (II), refers to 100 parts by mass of the total amount of liquid crystal compound, including the reverse-dispersion compound (I), when the reverse-dispersion compound (I) is a liquid crystal compound.

[0104] <Molecular Weight> The weight-average molecular weight (Mw) of the surfactant (II) is preferably 7,000 to 40,000, more preferably 7,000 to 30,000, and even more preferably 7,000 to 15,000. When the weight-average molecular weight is 7,000 or more, wind unevenness during formation of the cured liquid crystal layer is further suppressed, and when the weight-average molecular weight is 15,000 or less, the orientation of the cured liquid crystal layer is further improved. Here, the weight-average molecular weight in the present invention is a value measured by gel permeation chromatography (GPC). Solvent (eluent): tetrahydrofuran. Apparatus name: EcoSEC HLC-8320GPC (manufactured by Tosoh Corporation). Column: Three columns, TSKgel SuperHZM-H, TSKgel SuperHZ4000, and TSKgel SuperHZ200 (all manufactured by Tosoh Corporation), were connected and used. Column temperature: 40°C. Sample concentration: 0.1% by mass. Flow rate: 0.35 ml / min. Calibration curve: A calibration curve using six samples of TSK standard polystyrene manufactured by Tosoh Corporation with Mw = 706,000 to 1,013 (Mw / Mn = 1.03 to 1.06) was used.

[0105] [Solvent] The liquid crystal composition of the present invention preferably contains a solvent from the viewpoint of workability, etc. Examples of the solvent include ketones (e.g., acetone, 2-butanone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone), ethers (e.g., dioxane, tetrahydrofuran, tetrahydropyran, dioxolane, tetrahydrofurfuryl alcohol, and cyclopentyl methyl ether), aliphatic hydrocarbons (e.g., hexane), alicyclic hydrocarbons (e.g., cyclohexane), aromatic hydrocarbons (e.g., benzene, toluene, xylene, and trimethylbenzene), halogenated carbons (e.g., dichloromethane, trichloromethane (chloroform), dichloroethane, dichlorobenzene, and chlorotoluene), and the like. Examples of suitable solvents include organic solvents such as ethanol, isopropanol, butanol, cyclohexanol, esters (e.g., methyl acetate, ethyl acetate, ethyl propionate, butyl acetate, and diethyl carbonate), alcohols (e.g., ethanol, isopropanol, butanol, and cyclohexanol), cellosolves (e.g., methyl cellosolve, ethyl cellosolve, and 1,2-dimethoxyethane), cellosolve acetates, sulfoxides (e.g., dimethyl sulfoxide), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, N-ethylpyrrolidone, and 1,3-dimethyl-2-imidazolidinone), and heterocyclic compounds (e.g., pyridine), as well as water. These solvents may be used alone or in combination of two or more.

[0106] Among these solvents, organic solvents are preferred, and ketones and / or esters are more preferred, because they provide a cured liquid crystal layer that has better alignment and improved heat resistance.

[0107] In the present invention, the solvent preferably contains a high-boiling solvent having a boiling point of 130° C. or higher, for the reason that the alignment of the liquid crystal composition is good. The content of the high-boiling solvent is preferably 150 parts by mass or more, and more preferably 150 to 1,000 parts by mass, per 100 parts by mass of the liquid crystal compound. Here, 100 parts by mass of the liquid crystal compound, which is the basis for the content of the high-boiling solvent, refers to 100 parts by mass of the total amount of the liquid crystal compound, including the reverse-dispersion compound (I), when the reverse-dispersion compound (I) is the liquid crystal compound.

[0108] [Polymerization Initiator] The liquid crystal composition of the present invention may contain a polymerization initiator. The polymerization initiator is not particularly limited, but is preferably a photosensitive compound, i.e., a photopolymerization initiator. Various compounds can be used as the photopolymerization initiator without any particular limitation. Examples of photopolymerization initiators include α-carbonyl compounds, acyloin ethers, α-hydrocarbon-substituted aromatic acyloin compounds, polynuclear quinone compounds, combinations of triarylimidazole dimers and p-aminophenyl ketones, acridines, phenazine compounds, oxadiazole compounds, o-acyloxime compounds, and acylphosphine oxide compounds. Commercially available photopolymerization initiators may also be used, including Irgacure-184, Irgacure-907, Irgacure-369, Irgacure-651, Irgacure-819, Irgacure-OXE-01, and Irgacure-OXE-02, all manufactured by BASF.

[0109] When the liquid crystal composition contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30% by mass, more preferably 0.1 to 10% by mass, based on the total solid content (100% by mass) of the liquid crystal composition.

[0110] [Optically Anisotropic Layer] The optically anisotropic layer of the present invention is an optically anisotropic layer comprising a cured liquid crystal layer obtained by fixing the alignment state of the liquid crystal composition of the present invention described above.

[0111] The orientation state of the liquid crystal compound in the cured liquid crystal layer of the present invention is preferably horizontal orientation. In this specification, "horizontal orientation" means that the major surface of the cured liquid crystal layer (or, when the cured liquid crystal layer is formed on a member such as a support or an alignment film, the surface of the member) and the long axis direction of the liquid crystal compound are parallel. However, strict parallelism is not required, and in this specification, it means an orientation in which the angle between the long axis direction of the liquid crystal compound and the major surface of the cured liquid crystal layer is less than 10°.

[0112] The optically anisotropic layer of the present invention is preferably a positive A plate. Here, a positive A plate is defined as follows. The positive A plate satisfies the relationship of the following formula (A1). The positive A plate exhibits a positive Rth value. The positive A plate is preferably used in combination with a positive C plate. That is, the positive C plate satisfies the relationship of the following formula (C1), where nx is the refractive index in the in-plane slow axis direction (the direction in which the in-plane refractive index is maximum), ny is the refractive index in the in-plane direction perpendicular to the in-plane slow axis, and nz is the refractive index in the thickness direction. The positive C plate exhibits a negative Rth value. nx>ny≒nz Formula (A1) nz>nx≒ny Formula (C1) Note that the above "≒" encompasses not only the case where the two are completely identical, but also the case where the two are substantially identical. Regarding "substantially the same," for a positive A plate, "ny ≒ nz" includes, for example, a case where (ny - nz) x d (where d is the film thickness) is -10 to 10 nm, preferably -5 to 5 nm, and "nx ≒ nz" includes, for example, a case where (nx - nz) x d (where d is the film thickness) is -10 to 10 nm, preferably -5 to 5 nm. Also, for a positive C plate, "nx ≒ ny" includes, for example, a case where (nx - ny) x d (where d is the film thickness) is 0 to 10 nm, preferably 0 to 5 nm.

[0113] When the liquid crystal cured layer of the present invention is a positive A plate, from the viewpoint of functioning as a λ / 4 plate, Re(550) is preferably 100 to 180 nm, more preferably 120 to 160 nm, even more preferably 130 to 150 nm, and particularly preferably 135 to 145 nm. Here, the "λ / 4 plate" is a plate having a λ / 4 function, specifically, a plate having a function of converting linearly polarized light of a certain wavelength into circularly polarized light (or circularly polarized light into linearly polarized light).

[0114] The thickness of the optically anisotropic layer is not particularly limited, but is preferably 0.1 to 10 μm, more preferably 0.5 to 5 μm.

[0115] The optically anisotropic layer of the present invention satisfies the relationship of the following formula (3): Re(450) / Re(550)<1.00 (3), where Re(450) represents the in-plane retardation of the optically anisotropic layer at a wavelength of 450 nm, and Re(550) represents the in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm.

[0116] The optically anisotropic layer of the present invention preferably has a surface free energy of 35 mN / m or less in order to prevent wind unevenness. For the same reason, the surface free energy is preferably 24 mN / m or more. Here, the surface free energy can be measured by the Kölbl-Wu method.

[0117] [Optical Film] The optical film of the present invention is an optical film having the optically anisotropic layer of the present invention described above. The structure of the optical film will be described with reference to Fig. 1. Fig. 1 is a schematic cross-sectional view showing an example of an optical film. Note that Fig. 1 is a schematic view, and the thickness relationships and positional relationships of the layers do not necessarily correspond to the actual ones, and the support and alignment film shown in Fig. 1 are both optional components.

[0118] The optical film 10 shown in FIG. 1 comprises, in this order, a support 16, an alignment film 14, and an optically anisotropic layer 12 composed of a cured liquid crystal layer formed by fixing the alignment state of the liquid crystal composition of the present invention. The optically anisotropic layer 12 may also be a laminate of two or more different cured liquid crystal layers. For example, when the polarizing plate of the present invention described below is used as a circular polarizing plate, or when the optical film of the present invention is used as an optical compensation film for an IPS (In-Plane-Switching) or FFS (Fringe-Field-Switching) liquid crystal display device, a laminate of a positive A plate and a positive C plate is preferred. Alternatively, the optically anisotropic layer may be peeled off from the support and used alone as an optical film. Various components used in the optical film are described in detail below.

[0119] [Support] The optical film may have a support as a substrate for forming the optically anisotropic layer. Such a support is preferably transparent. Specifically, it is preferable that the light transmittance thereof is 80% or more.

[0120] Examples of such supports include glass substrates and polymer films. Materials for the polymer film include cellulose-based polymers, acrylic polymers having acrylic acid ester polymers such as polymethyl methacrylate and lactone ring-containing polymers, thermoplastic norbornene-based polymers, polycarbonate-based polymers, polyester-based polymers such as polyethylene terephthalate and polyethylene naphthalate, styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers (AS resins), polyolefin-based polymers such as polyethylene, polypropylene, and ethylene-propylene copolymers, vinyl chloride-based polymers, amide-based polymers such as nylon and aromatic polyamides, imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinylidene chloride-based polymers, vinyl alcohol-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and polymers obtained by mixing these polymers.

[0121] The thickness of the support is not particularly limited, but is preferably 5 to 100 μm, more preferably 5 to 50 μm. The support may be peelable from the optical film.

[0122] [Alignment Film] In the optical film, the optically anisotropic layer is preferably formed on the surface of the alignment film. When the optical film has any of the above-mentioned supports, the alignment film may be sandwiched between the support and the optically anisotropic layer. In addition, the above-mentioned support may also serve as the alignment film. The alignment film may be peelable from the optical film. In addition, the alignment film may have optical anisotropy, and a positive C plate having an alignment function on its surface as shown in WO2021 / 166619 may be used as the alignment film.

[0123] The alignment film may be any film that has the function of aligning the polymerizable liquid crystal compound contained in the composition. The alignment film generally contains a polymer as its main component. Polymer materials for alignment films are described in numerous literatures, and many commercially available products are available. Preferred polymer materials for alignment films are polyvinyl alcohol, polyimide, or derivatives thereof, with modified or unmodified polyvinyl alcohol being more preferred.

[0124] It is also preferable to use a photo-alignment film as the alignment film, since it is possible to prevent the surface condition from being deteriorated by preventing contact with an object on the alignment film surface during the formation of the alignment film. The photo-alignment film is not particularly limited, but it can be an alignment film formed from a polymer material such as a polyamide compound or a polyimide compound described in paragraphs

[0024] to

[0043] of International Publication No. 2005 / 096041; a liquid crystal alignment film formed from a liquid crystal alignment agent having a cinnamoyl group described in Japanese Patent Application Laid-Open No. 2012-155308; and a product name LPP-JP265CP manufactured by Rolic Technologies, Inc., or the like.

[0125] The thickness of the alignment film is not particularly limited, but from the viewpoint of reducing surface irregularities that may be present on the support and forming a liquid crystal cured layer with a uniform film thickness, the thickness is preferably 0.01 to 10 μm, more preferably 0.01 to 1 μm, and even more preferably 0.01 to 0.5 μm.

[0126] [Another liquid crystal cured layer] In the optical film, the optically anisotropic layer of the present invention may be formed on the surface of another liquid crystal cured layer, or another liquid crystal cured layer may be formed on the surface of the optically anisotropic layer of the present invention. Here, examples of the other liquid crystal cured layer include a liquid crystal cured layer obtained by fixing the liquid crystal composition of the present invention described above in a desired alignment state. Further examples include a liquid crystal cured layer (light absorption anisotropic film) obtained by fixing the alignment state of a composition containing the above-mentioned liquid crystal compound, a polymerization initiator, a dichroic material, a surfactant, and a solvent.

[0127] [Ultraviolet Absorber] The optical film may contain an ultraviolet (UV) absorber in consideration of the influence of external light (particularly ultraviolet light). The ultraviolet absorber may be contained in the optically anisotropic layer, or may be contained in a member other than the optically anisotropic layer constituting the optical film. A suitable example of the member other than the optically anisotropic layer is a support. Any conventionally known ultraviolet absorber capable of exhibiting ultraviolet absorption properties can be used as the ultraviolet absorber. Among such ultraviolet absorbers, benzotriazole-based or hydroxyphenyltriazine-based ultraviolet absorbers are preferred from the viewpoint of high ultraviolet absorption and obtaining ultraviolet absorption ability (ultraviolet blocking ability) sufficient for use in image display devices. In addition, it is also preferred to use two or more ultraviolet absorbers with different maximum absorption wavelengths in combination in order to widen the ultraviolet absorption width.

[0128] Examples of ultraviolet absorbers that can be used include Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479, and Tinuvin 1577 (all manufactured by BASF).

[0129] [Polarizing Plate] The polarizing plate of the present invention comprises the optically anisotropic layer or optical film of the present invention described above and a polarizer. The polarizing plate of the present invention preferably further comprises a positive C plate, and more preferably comprises a positive C plate obtained by fixing the alignment state of a liquid crystal composition containing surfactant (II) having the structure represented by formula (2) described above. When the optically anisotropic layer is a positive A plate, the angle between the slow axis of the positive A plate and the absorption axis of the polarizer described below is preferably 30 to 60°, more preferably 40 to 50°, even more preferably 42 to 48°, and particularly preferably 45°, in terms of suitable application to circular polarizing plates and the like. Here, the "slow axis" refers to the direction in which the refractive index is maximized in the plane of the cured liquid crystal layer, and the "absorption axis" of the polarizer refers to the direction in which the absorbance is highest. When the liquid crystal cured layer (optically anisotropic layer) of the optical film is the optically anisotropic layer A described above, the absolute value of the angle between the in-plane slow axis of the second region formed by fixing the alignment state of the homogeneously aligned liquid crystal compound and the absorption axis of the polarizer is preferably 5 to 25°, more preferably 10 to 20°, in order to suitably apply the optically anisotropic layer A to circular polarizers and the like. The polarizing plate can also be used as an optical compensation film for an IPS-type or FFS-type liquid crystal display device. When the polarizing plate is used as an optical compensation film for an IPS-type or FFS-type liquid crystal display device, the optically anisotropic layer described above is preferably used as at least one plate of a laminate of a positive A plate and a positive C plate, and the angle between the slow axis of the positive A plate layer and the absorption axis of the polarizer described below is preferably orthogonal or parallel. Specifically, the angle between the slow axis of the positive A plate layer and the absorption axis of the polarizer described below is more preferably 0 to 5° or 85 to 95°. When the polarizing plate of the present invention is used in an image display device described later, the angle between the slow axis of the cured liquid crystal layer and the absorption axis of the polarizer described later is preferably parallel or perpendicular. In this specification, "parallel" does not require strict parallelism, but means that the angle between one axis and the other is less than 10°.Furthermore, in this specification, "orthogonal" does not require that they be strictly orthogonal, but rather means that the angle between one side and the other side is greater than 80° and less than 100°.

[0130] [Polarizer] The polarizer is not particularly limited as long as it has the function of converting light into specific linearly polarized light, and conventionally known absorption-type polarizers, reflective-type polarizers, and coated-type polarizers can be used. Examples of absorption-type polarizers include iodine-based polarizers, dye-based polarizers using dichroic dyes, and polyene-based polarizers. Iodine-based polarizers and dye-based polarizers include coated-type polarizers and stretched-type polarizers, and either can be used. However, polarizers produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching the resulting material are preferred. Examples of coated-type polarizers include polarizers containing a cured liquid crystal compound and a dichroic dye. Examples of reflective polarizers include polarizers stacked with thin films of different birefringence, wire-grid polarizers, and polarizers combining a cholesteric liquid crystal with a selective reflection region and a quarter-wave plate.

[0131] The thickness of the polarizer is not particularly limited, but is preferably from 3 to 60 μm, more preferably from 3 to 30 μm, and even more preferably from 3 to 10 μm.

[0132] [Adhesive Layer] In the polarizing plate of the present invention, an adhesive layer may be disposed between the optically anisotropic layer in the optical film and the polarizer. Examples of materials for forming the adhesive layer used for laminating the cured product and the polarizer include members formed of substances having a ratio of storage modulus G' to loss modulus G" (tan δ = G" / G') measured with a dynamic viscoelasticity measuring device of 0.001 to 1.5, and include so-called adhesives and substances that tend to creep. Examples of adhesives include, but are not limited to, polyvinyl alcohol-based adhesives.

[0133] [Adhesive Layer] The polarizing plate of the present invention may have an adhesive layer disposed between the optically anisotropic layer and the polarizer in the optical film. The adhesive layer used to laminate the cured product and the polarizer is preferably a curable adhesive composition that cures upon irradiation with active energy rays or heating. Examples of curable adhesive compositions include curable adhesive compositions containing a cationically polymerizable compound and curable adhesive compositions containing a radically polymerizable compound. The thickness of the adhesive layer is preferably 0.01 to 20 μm, more preferably 0.01 to 10 μm, and even more preferably 0.05 to 5 μm. When the thickness of the adhesive layer is within this range, lifting or peeling does not occur between the laminated protective layer or liquid crystal cured layer and the polarizer, and practically satisfactory adhesive strength is obtained. Furthermore, from the viewpoint of suppressing the generation of bubbles, the thickness of the adhesive layer is preferably 0.4 μm or more. For the adhesive layer, see, for example, paragraphs

[0062] to

[0080] of JP 2016-35579 A, ​​the contents of which are incorporated herein by reference.

[0134] [Easy-Adhesion Layer] The polarizing plate of the present invention may have an easy-adhesion layer disposed between the optically anisotropic layer and the polarizer in the optical film. From the viewpoints of excellent adhesion between the optically anisotropic layer and the polarizer and further suppressing the occurrence of cracks in the polarizer, the easy-adhesion layer may have a storage modulus of 1.0×10 at 85° C. 6 Pa ~ 1.0 x 10 7 Pa is preferable. Constituent materials of the easy-adhesion layer include polyolefin-based components and polyvinyl alcohol-based components. The thickness of the easy-adhesion layer is preferably 500 nm to 1 μm. For the easy-adhesion layer, for example, paragraphs

[0048] to

[0053] of JP 2018-36345 A can be referred to, and the contents thereof are incorporated herein by reference.

[0135] [Image display device] The image display device of the present invention is an image display device having the optical film of the present invention or the polarizing plate of the present invention. The display element used in the image display device is not particularly limited, and examples thereof include a liquid crystal cell, an organic electroluminescence (hereinafter abbreviated as "EL (Electro Luminescence)") display panel, and a plasma display panel. Of these, a liquid crystal cell and an organic EL display panel are preferred.

[0136] [Liquid Crystal Display Device] A liquid crystal display device, which is an example of an image display device, is a liquid crystal display device having the above-described polarizing plate and a liquid crystal cell. Of the polarizing plates provided on both sides of the liquid crystal cell, it is preferable to use the above-described polarizing plate as the front-side polarizing plate, and it is more preferable to use the above-described polarizing plate as the front-side and rear-side polarizing plates.

[0137] <Liquid Crystal Cell> The liquid crystal cell used in the liquid crystal display device is preferably in VA (Vertical Alignment) mode, OCB (Optically Compensated Bend) mode, IPS (In-Plane-Switching) mode, FFS (Fringe-Field-Switching) mode, or TN (Twisted Nematic) mode, but is not limited to these.

[0138] [Organic EL Display Device] An example of an organic EL display device, which is an example of an image display device, includes, from the viewing side, a polarizer, a λ / 4 plate made of the above-mentioned liquid crystal cured layer (optically anisotropic layer), and an organic EL display panel, in this order. The organic EL display panel is a display panel configured using organic EL elements in which an organic light-emitting layer (organic electroluminescence layer) is sandwiched between electrodes (between a cathode and an anode). The configuration of the organic EL display panel is not particularly limited, and a known configuration may be used.

[0139] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.

[0140] Comparative Example 1-1 An optically anisotropic layer containing a reverse dispersion compound, a liquid crystal compound and a specific surfactant, a positive C plate, and a circular polarizer and display device containing them were prepared as follows.

[0141] [Preparation of Support (Cellulose Acylate Film A1)] The following composition was charged into a mixing tank, stirred, and further heated at 90°C for 10 minutes. The resulting composition was then filtered through filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to prepare a dope. The solid content of the dope was 23.5% by mass, the amount of plasticizer added was the ratio relative to the cellulose acylate, and the solvent for the dope was methylene chloride / methanol / butanol = 81 / 18 / 1 (mass ratio).

[0142] ------------------------------------------------ Cellulose acylate dope -------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity average degree of polymerization 310) 100 parts by mass Sugar ester compound 1 (formula (S4) below) 6.0 parts by mass Sugar ester compound 2 (formula (S5) below) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) 351.9 parts by mass --------------------------------------------------

[0143]

[0144] The dope prepared above was cast using a drum film-forming machine. The dope was cast from a die onto a metal support cooled to 0°C, and the resulting web (film) was then peeled off from the drum. The drum was made of SUS (stainless steel). The cast web (film) was peeled off from the drum and dried for 20 minutes in a tenter apparatus, which clipped both ends of the web with clips while transporting the film at 30-40°C. The web was then post-dried by zone heating while being transported by a roll. The resulting web was knurled and wound up to form cellulose acylate film A1. The resulting cellulose acylate film A1 had a thickness of 40 μm, an in-plane retardation Re(550) of 1 nm at a wavelength of 550 nm, and a thickness-direction retardation Rth(550) of 25 nm at a wavelength of 550 nm.

[0145] [Preparation of Optical Film F1-1] A coating solution E1 for forming a photo-alignment film having the following composition was continuously coated on the above-mentioned cellulose acylate film A1 using a wire bar. The cellulose acylate film A1 on which the coating film was formed was dried with hot air at 140°C for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 , using an ultra-high pressure mercury lamp) to form a photo-alignment film E1 with a thickness of 0.7 μm, thereby obtaining a TAC film with a photo-alignment film.

[0146] -------------------------------------------------- Coating liquid E1 for forming photoalignment film -------------------------------------------------- - 100.00 parts by mass of polymer PA-2 (described below) - 5.00 parts by mass of thermal cationic polymerization initiator PAG-1 (described below) - 0.005 parts by mass of acid generator CPI-110TF (described below) - 16.50 parts by mass of isopropyl alcohol - 1072.00 parts by mass of butyl acetate - 268.00 parts by mass of methyl ethyl ketone --------------------------------------------------

[0147] Thermal cationic polymerization initiator PAG-1

[0148] Polymer PA-2 (weight average molecular weight: 45,000; in the following formula, the numerical value for each repeating unit represents the content (% by mass) of each repeating unit relative to all repeating units.)

[0149] Acid generator CPI-110TF

[0150] Composition F1-1 having the following composition was applied onto the photo-alignment film E1 using a bar coater. The coating film formed on the photo-alignment film E1 was heated to 120°C with hot air, then cooled to 60°C, and then irradiated with 100 mJ / cm at a wavelength of 365 nm using a high-pressure mercury lamp in a nitrogen atmosphere. 2 The coating film was irradiated with ultraviolet light of 500 mJ / cm 2 while being heated to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm, thereby fixing the alignment of the liquid crystal compound, and an optical film F1-1 having an optically anisotropic layer F1-1 was produced. The thickness of the optically anisotropic layer F1-1 was 2.9 μm, and Re(550) was 142 nm. The optically anisotropic layer F1-1 also satisfied the relationship Re(450)≦Re(550)≦Re(650). Re(450) / Re(550) was 0.82. The optically anisotropic layer corresponds to a so-called λ / 4 plate. The mixture of reverse dispersion compounds LA-1 to LA-3 and polymerizable liquid crystal compounds LC-1 to LC-4 contained in the following composition F1-1 is referred to as liquid crystal mixture A.

[0151] 0.16 parts by mass of polymerizable liquid crystal compound LC-3 below; 5.00 parts by mass of polymerizable liquid crystal compound LC-4 below; 0.50 parts by mass of polymerization initiator PI-1 below; 0.09 parts by mass of surfactant containing a polyacrylate compound as its main component (BYK-361N, manufactured by BYK Japan); 181.00 parts by mass of cyclopentanone; 181.00 parts by mass of methyl ethyl ketone. 54.00 parts by mass ――――――――――――――――――――――――――――――――

[0152] Reverse dispersion compound LA-1 (tBu represents a tertiary butyl group)

[0153] Reverse dispersion compound LA-2

[0154] Reverse dispersion compound LA-3

[0155] Polymerizable liquid crystal compound LC-1

[0156] Polymerizable liquid crystal compound LC-2

[0157] Polymerizable liquid crystal compound LC-3

[0158] Polymerizable liquid crystal compound LC-4 (Me represents a methyl group)

[0159] Polymerization initiator PI-1

[0160] [Preparation of Positive C Plate] Coating solution FC-1 for forming a positive C plate having the following composition was applied onto the above-mentioned cellulose acylate film A1, and the resulting coating film was aged at 60° C. for 60 seconds, and then exposed to a 70 mW / cm 2 An air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) was used, and the light output was 1000 mJ / cm 2 The alignment state was fixed by irradiating the liquid crystal compound with ultraviolet light of 1000 nm to vertically align the liquid crystal compound, thereby producing a positive C plate FC-1 having a thickness of 0.5 μm. The Rth(550) of the obtained positive C plate was −60 nm.

[0161] -------------------------------- Coating liquid FC-1 for forming positive C-plate -------------------------------- 83 parts by mass of the above liquid crystal compound LC-1 15 parts by mass of the above liquid crystal compound LC-2 2 parts by mass of the above liquid crystal compound LC-3 Polymerizable monomer (UA-601I, manufactured by Kyoeisha Chemical Co., Ltd.) 5 parts by mass Polymerization initiator (IrgacureOXE01, manufactured by BASF) 4 parts by mass 0.4 parts by mass of the following specific surfactant SC-1 1.2 parts by mass of the following vertical alignment agent S01 1.14 parts by mass of the following polymer M 494.9 parts by mass of methyl isobutyl ketone 95.0 parts by mass of 2-butanone 43.3 parts by mass --------------------------------

[0162] Vertical alignment agent S01

[0163] Polymer M (weight average molecular weight: 60,000, the value for each repeating unit indicates the content relative to the total repeating units)

[0164] Specific surfactant SC-1 (weight average molecular weight: 25,000)

[0165] [Fabrication of Circularly Polarizing Plate and Display Device] <Fabrication of Polarizer 1 with Protective Film> The surface of a support of cellulose triacetate film TJ25 "Z-TAC" (manufactured by Fujifilm; thickness: 25 μm) was subjected to alkaline saponification treatment. Specifically, the support was immersed in a 1.5 N sodium hydroxide aqueous solution at 55°C for 2 minutes, washed in a water wash bath at room temperature, and further neutralized with 0.1 N sulfuric acid at 30°C. After neutralization, the support was washed in a water wash bath at room temperature and further dried with hot air at 100°C to obtain a polarizer protective film. A roll-shaped polyvinyl alcohol film was stretched in the MD (machine direction) direction in an iodine aqueous solution and dried to obtain Polarizer 1 with a thickness of 14 μm. The polarizer protective film was attached to both surfaces of Polarizer 1 with PVA glue to produce Polarizer 1 with protective films.

[0166] <Preparation of UV adhesive 1> UV adhesive 1 was prepared having the following composition. --------------------------------------------------- UV adhesive 1 --------------------------------------------------- CEL2021P (manufactured by Daicel Corporation) 70 parts by mass 1,4-butanediol diglycidyl ether 20 parts by mass 2-ethylhexyl glycidyl ether 10 parts by mass CPI-100P 2.25 parts by mass ---------------------------------------------------

[0167] CPI-100P

[0168] <Preparation of adhesive sheet N1> 95 parts by mass of butyl acrylate and 5 parts by mass of acrylic acid were polymerized by solution polymerization to obtain an acrylic copolymer 1 having an average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 3.0. Next, relative to 100 parts by mass of the solid content of the acrylic copolymer 1, 10 parts by mass of a polyfunctional acrylate monomer (Aronix M-315, manufactured by Toagosei Co., Ltd.), 1 part by mass of a photopolymerization initiator (Irgacure 500, manufactured by BASF Corporation), 1 part by mass of trimethylolpropane tolylene diisocyanate (Coronate L, manufactured by Nippon Polyurethane Co., Ltd.), and 0.2 parts by mass of a silane coupling agent (KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed to prepare a solution (adhesive composition N1). Next, the prepared pressure-sensitive adhesive composition N1 was applied to a silicone resin-coated PET film (release film), dried at 90°C to remove the solvent, and irradiated with ultraviolet (UV) rays under the following conditions to prepare a pressure-sensitive adhesive sheet N1 having a 20 μm-thick pressure-sensitive adhesive layer N1. The storage modulus of the pressure-sensitive adhesive layer N1 was 0.6 MPa. (UV irradiation conditions) Fusion Inc. electrodeless lamp H bulb Illuminance: 600 mW / cm 2 ・Light intensity: 150mJ / cm 2 The UV illuminance and light quantity were measured using "UVPF-36" manufactured by Eye Graphics.

[0169] <Preparation of Circularly Polarizing Plate> The retardation layer (positive C plate) side of the positive C plate FC-1 prepared above was attached to the optically anisotropic layer F1-1 (positive A plate) side of the optical film F1-1 using the UV adhesive 1, and the photo-alignment film and cellulose acylate film A1 on the positive A plate side were removed to obtain an optically anisotropic layer-attached film 1. The protective film-attached polarizer 1 prepared above was attached to the optically anisotropic layer (positive A plate) side of the optically anisotropic layer-attached film 1 using the pressure-sensitive adhesive sheet N1, and the cellulose acylate film A1 on the positive C plate side was removed to complete a circularly polarizing plate. At this time, the attachment was performed so that the angle between the absorption axis of the polarizer included in the protective film-attached polarizer 1 and the slow axis of the positive A plate F1-1 included in the optically anisotropic layer-attached film 1 was 45°.

[0170] <Preparation of Organic EL Display Device> A GALAXY S4 manufactured by SAMSUNG equipped with an organic EL panel (organic EL display element) was disassembled, the touch panel with the circular polarizer was peeled off from the organic EL display device, and the circular polarizer was further peeled off from the touch panel to separate the organic EL display element, the touch panel, and the circular polarizer. Next, the separated touch panel was reattached to the organic EL display element, and the prepared circular polarizer was further attached to the touch panel via an adhesive SK2057 (manufactured by Soken Chemical & Engineering Co., Ltd.) so that the optically anisotropic layer side (positive C plate side) faced the panel side, thereby preparing an organic EL display device.

[0171] [Evaluation] [Wind Unevenness] Each optical film produced in Comparative Example 1-1 and each of the Examples and Comparative Examples described later was sandwiched between two polarizing plates arranged in a crossed Nicol configuration, and light was transmitted from bottom to top (toward the viewer), and the unevenness in brightness was observed. The observed unevenness was incorporated into an organic EL display device, and evaluated according to the following criteria. The results are shown in the tables described later. A: No unevenness was observed over the entire surface of the optical film. B: Weak unevenness was visible in part of the optical film, but not when incorporated into an organic EL panel. C: Unevenness was observed in part of the optical film, and was visible when incorporated into an organic EL panel, but was acceptable. D: Unevenness was observed in part of the optical film, and was strongly visible when incorporated into an organic EL panel, and was unacceptable.

[0172] [Cleaning] The number of cissings in the cured liquid crystal layer (optically anisotropic layer) of each optical film produced in Comparative Example 1-1 and each of the Examples and Comparative Examples described later was counted. Note that cissing refers to an area where no cured liquid crystal layer is formed. Cleaving refers to an area that remains dark even when a sample formed by laminating an optical film containing a cured liquid crystal layer and a support not containing a cured liquid crystal layer at a 90° offset is observed under crossed Nicols conditions using a polarizing microscope in transmission mode. Based on the results, evaluation was performed according to the following criteria. The results are shown in the tables described later. A: 5 cissings / m 2 Less than B: 5 repellings / m 2 More than 30 pieces / m 2 Less than C: 30 repellings / m 2More than this is unacceptable

[0173] [Measurement of Surface Free Energy] The surface free energy γ of the liquid crystal cured layer (optically anisotropic layer) of each optical film prepared in Comparative Example 1-1 and each Example and Comparative Example described later was calculated by the Kölbl-Wu method. The results are shown in the tables described later.

[0174] Comparative Examples 1-2 to 1-4 and Examples 1-1 to 1-16 Circularly polarizing plates and organic EL display devices of Comparative Examples 1-2 to 1-4 and Examples 1-1 to 1-16 were produced in the same manner as in Comparative Example 1-1, except that optical films F1-2 to F1-20 produced by the following method were used instead of optical film F1-1.

[0175] [Preparation of Optical Films F1-2 to F1-21] <Specific Surfactants SA-1 to SA-14> Specific surfactants SA-1 to SA-14 (all of which correspond to surfactant (II)) shown in Table 10 below were prepared.

[0176] Repeating unit A-1

[0177] Repeating unit A-2

[0178] Repeating unit B-1

[0179] Repeating unit B-2

[0180] Repeating unit B-3

[0181] Repeating unit B-4

[0182] Repeating unit B-5

[0183] <Preparation of Optical Films F1-2 to F1-20> Optical films F1-2 to F1-20 were prepared in the same manner as in Comparative Example 1-1, except that the blending amount of the surfactant BYK-361N (manufactured by BYK Japan) (i.e., a surfactant not corresponding to surfactant (II)) used in the preparation of optical film F1-1 in Comparative Example 1-1 was changed as shown in Table 11 below, or the surfactant BYK-361N was changed to specific surfactants SA-1 to SA-14 corresponding to surfactant (II) shown in Table 11 below.

[0184]

[0185] [Comparative Example 2-1] [Preparation of Optical Film F2-1] An optical film F2-1 having an optically anisotropic layer F2-1 was prepared in the same manner as in Comparative Example 1 (

[0160] to

[0179] ) of JP 2021-81651 A. Note that the liquid crystal mixture (1) shown in the above publication is referred to as liquid crystal mixture B. [Preparation of Circularly Polarizing Plate and Display Device] A circularly polarizing plate and an organic EL display device of Comparative Example 2-1 were prepared in the same manner as in Comparative Example 1-1, except that optical film F2-1 was used instead of optical film F1-1.

[0186] [Comparative Example 2-2 and Examples 2-1 to 2-16] Circularly polarizing plates and organic EL display devices of Comparative Example 2-2 and Examples 2-1 to 2-16 were produced in the same manner as in Comparative Example 2-1, except that optical films F2-2 and F2-5 to F2-20 produced by the following method were used instead of optical film F2-1.

[0187] [Preparation of Optical Films F2-2 and F2-5 to F2-20] Optical films F1-2 and F2-5 to F2-20 were prepared in the same manner as in Comparative Example 2-1, except that the amount of surfactant BYK-361N (manufactured by BYK Japan) (i.e., a surfactant not corresponding to surfactant (II)) used in the preparation of optical film F2-1 in Comparative Example 2-1 was changed as shown in Table 12 below, or that the surfactant BYK-361N was replaced with specific surfactants SA-1 to SA-14 corresponding to surfactant (II) shown in Table 12 below.

[0188]

[0189] [Examples 3-1 to 3-3] Circularly polarizing plates and organic EL display devices of Examples 3-1 to 3-3, which are also shown in Table 13 below, were produced in the same manner as in Comparative Example 1-1, except that optical films F3-1 to F3-3 produced by the following method were used instead of optical film F1-1.

[0190] [Preparation of Optical Film F3-1] An optical film F3-1 having an optically anisotropic layer F3-1 was prepared in the same manner as for optical film F1-1, except that the composition F1-1 used in the preparation of optical film F-1 was changed to the following composition F3-1. A mixture of reverse dispersion compounds LA-1 and LA-4 to LA-7 and polymerizable liquid crystal compound LC-4 shown in the following composition F3-1 was designated liquid crystal mixture C.

[0191] -------------------------------- Composition F3-1------------------------------------------------ - 26.0 parts by mass of the above reverse dispersion compound LA-1 - 20.0 parts by mass of the following reverse dispersion compound LA-4 - 24.0 parts by mass of the following reverse dispersion compound LA-5 - 5.0 parts by mass of the following reverse dispersion compound LA-6 - 12.0 parts by mass of the following reverse dispersion compound LA-7 - 13.0 parts by mass of the above polymerizable liquid crystal compound LC-4 - 0.5 parts by mass of the following polymerization initiator PI-1 - 0.06 parts by mass of the above surfactant SA-1 - 240.0 parts by mass of tetrahydrofuran - 60.0 parts by mass of cyclopentanone --------------------------------

[0192] Reverse dispersion compound LA-4

[0193] Reverse dispersion compound LA-5

[0194] Reverse dispersion compound LA-6

[0195] Reverse dispersion compound LA-7

[0196] [Preparation of Optical Film F3-2] Optical film F3-2 having an optically anisotropic layer F3-2 was prepared based on the method described in paragraphs

[0224] to

[0228] of Japanese Patent No. 6700468, except that BYK-361N blended as a leveling agent was replaced with the specific surfactant SA-1 (0.06 parts by mass). The liquid crystal mixture described in the above patent publication is referred to as liquid crystal mixture D.

[0197] [Preparation of Optical Film F3-3] An optical film F3-3 having an optically anisotropic layer F3-3 was prepared based on the method described in Example 1 of JP 2020-531615 A, except that the surfactant FluorN 561 contained in composition M-1 was changed to the specific surfactant SA-8 (0.06 parts by mass). Note that the mixture of compounds other than Irganox 1076, Darocure TPO, and FluorN 561 contained in composition M-1 in the above publication is referred to as liquid crystal mixture E.

[0198]

[0199] [Examples 4-1 to 4-11] Circularly polarizing plates and organic EL display devices of Examples 4-1 to 4-11 were produced in the same manner as in Comparative Example 1-1, except that optical films F4-1 to F4-11 produced by the following method were used instead of optical film F1-1.

[0200] [Preparation of Optical Films F4-1 to F4-11] <Specific Surfactant SA-15, etc.> Specific surfactants SA-15, etc. shown in Table 14 below (all surfactants corresponding to surfactant (II)) were prepared.

[0201] Repeating unit A-3 (Me represents a methyl group)

[0202] Repeating unit B-6

[0203] Surfactant SA-16

[0204] [Preparation of Optical Film F4-1] Optical film F4-1 having an optically anisotropic layer F4-1 was prepared in the same manner as for optical film F1-1, except that composition F1-1 used in the preparation of optical film F-1 was replaced with composition F4-1 below. A mixture of reverse dispersion compounds LA-8 and LA-9 and polymerizable liquid crystal compound LC-5 shown in composition F4-1 below is designated liquid crystal mixture F.

[0205] -------------------------------- Composition F4-1------------------------------------------------ 83.00 parts by mass of reverse dispersion compound LA-8 described below 14.00 parts by mass of reverse dispersion compound LA-9 described below 3.00 parts by mass of polymerizable liquid crystal compound LC-5 described below 0.50 parts by mass of polymerization initiator PI-1 described above 0.06 parts by mass of surfactant SA-7 described above Cyclopentanone 181.00 parts by mass Methyl ethyl ketone 54.00 parts by mass

[0206] Reverse dispersion compound LA-8

[0207] Reverse dispersion compound LA-9

[0208] Polymerizable liquid crystal compound LC-5

[0209] [Preparation of Optical Films F4-2 to F4-9] Optical films F4-2 to F4-9 were prepared in the same manner as for optical film F4-1, except that specific surfactant SA-7 was replaced with the surfactant type shown in Table 15 below.

[0210] [Preparation of Optical Film F4-10] Optical film F4-10 was prepared in the same manner as for optical film F4-1, except that composition F4-1 was replaced with composition F4-10 below. A mixture of reverse dispersion compounds LA-8 and LA-9 and polymerizable liquid crystal compound LC-5 shown in composition F4-10 below was designated liquid crystal mixture F, similar to composition F4-1.

[0211] -------------------------------- Composition F4-10------------------------------------------------ 83.00 parts by mass of the reverse dispersion compound LA-8 14.00 parts by mass of the reverse dispersion compound LA-9 3.00 parts by mass of the polymerizable liquid crystal compound LC-5 0.50 parts by mass of the polymerization initiator PI-1 0.06 parts by mass of the surfactant SA-7 Cyclopentanone 70.00 parts by mass Methyl ethyl ketone 230.00 parts by mass

[0212] [Preparation of Optical Film F4-11] Optical film F4-11 was prepared in the same manner as optical film F4-1, except that composition F4-1 was replaced with composition F4-11 below. The mixture of reverse dispersion compounds LA-10 and LA-11 shown in composition F4-11 below is designated liquid crystal mixture G.

[0213] Composition F4-11 ---------------------------------------------------------------- 99.97 parts by mass of reversed dispersion compound LA-10 described below 0.03 parts by mass of reversed dispersion compound LA-11 described below 0.50 parts by mass of polymerization initiator PI-1 described above 0.06 parts by mass of surfactant SA-7 described above Cyclopentanone 181.00 parts by mass Methyl ethyl ketone 54.00 parts by mass

[0214] Reverse dispersion compound LA-10

[0215] Reverse dispersion compound LA-11

[0216] [Evaluation of Alignment] The optical films produced in Examples 4-1 to 4-11, and the above-mentioned Examples 1-8, 1-12, 2-8, and 2-12 were sandwiched between two polarizing plates arranged in a crossed Nicol configuration, and the alignment was evaluated according to the following criteria. The results are shown in Table 15 below. A: The number of defects of 100 μm or more was one or less per square meter. B: The number of defects of 100 μm or more was more than one and not more than ten per square meter. C: The number of defects of 100 μm or more per square meter was 10 or more. D: Poor alignment over the entire surface.

[0217]

[0218] The results shown in Tables 10 to 15 above indicate that the use of a liquid crystal composition containing surfactant (II) can suppress repelling and wind-induced unevenness during the formation of a reverse-dispersion cured liquid crystal layer (see Examples in each table). Furthermore, the results shown in Table 15 above indicate that good alignment is achieved when 150 parts by mass or more of a high-boiling solvent having a boiling point of 130°C or higher is contained per 100 parts by mass of liquid crystal compound. This is presumably because the fluidity of the coating liquid (liquid crystal composition) is maintained longer after coating, promoting uneven distribution of surfactant (II). Furthermore, it is apparent that an optical film having an optically anisotropic layer formed by fixing the alignment state of a liquid crystal composition containing a reverse-dispersion compound having a group (aromatic ring) represented by formula (Ar-3) above exhibits poor alignment. This is presumably because the group (aromatic ring) represented by formula (Ar-3) has strong interactions such as π-π interactions, resulting in low fluidity of the liquid crystal and slow alignment.

[0219] 10 Optical film 12 Liquid crystal cured layer (optically anisotropic layer) 14 Alignment film 16 Support

Claims

1. An optically anisotropic layer comprising a liquid crystal cured layer obtained by fixing the alignment state of a liquid crystal composition containing a reverse dispersion compound (I) represented by the following formula (1), at least one liquid crystal compound, and a surfactant (II) having a structure represented by the following formula (2) in its molecule, wherein the optically anisotropic layer satisfies the relationship of the following formula (3). Here, in the formula (1), D 1 , D 2 , D 3 and D. 4 each independently represents a single bond, -CO-, -O-, -S-, -C(=S)-, or -CR 1 R 2 -, -CR 3 =CR 4 --, --NR 5 -, or a divalent linking group consisting of two or more of these, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 1 A G Or SP G Represents. A 1 , A 2 and A G each independently represents an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, or a divalent alicyclic hydrocarbon group which may have a substituent, provided that -CH 2 One or more of - may be replaced by -O-, -S- or -NH-. 1 , S.P. 2 and S.P. G each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent. 1 and L 2 each independently represents a monovalent organic group; L 1 and L 2 At least one of Ar represents a polymerizable group. 1 and Ar 2 When at least one of the following formula (Ar-4) is an aromatic ring, L 1 and L 2 And L in the following formula (Ar-4): 3 and L 4 At least one of the groups represents a polymerizable group. m represents an integer of 0 to 2. When m is 2, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. l and n each independently represent 0 or an integer of 1 or more. When l is an integer of 2 or more, a plurality of A 1 may be the same or different, and a plurality of D 3 may be the same or different. When n is an integer of 2 or more, a plurality of D 4 may be the same or different, and a plurality of A 2 may be the same or different. p represents 0 or an integer of 1 or more. When p is an integer of 2 or more, a plurality of Ar 1 may be the same or different, and a plurality of D 2 may be the same or different. When p is an integer of 2 or more and m is not 0, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. 1 and Ar 2 each independently represents an aromatic ring selected from the group consisting of groups represented by the following formulas (Ar-1) to (Ar-8): In the formulae (Ar-1) to (Ar-8), *1 represents D 3 Or D 4 *2 represents the bonding position with D 1 Or D 2 When l is 0, D 3 The bond position with 1 When m is 0, *2 represents a bonding position with D 2 When n is 0, D 4 The bond position with 2 It represents the bonding position with Q. 1 represents N or CH. 2 is -S-, -O-, or -N(R 6 )-, R 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 1 represents a monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms which may have a substituent, a monovalent aromatic heterocyclic group having 3 to 12 carbon atoms which may have a substituent, or a monovalent alicyclic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent, provided that -CH 2 One or more of - may be substituted with -O-, -S- or -NH-. 1 , Z 2 and Z 3 each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, a monovalent aromatic heterocyclic group having 6 to 20 carbon atoms, a halogen atom, a cyano group, a nitro group, -OR 7 , -NR 8 R 9 , -SR 10 , -COOR 11 or -COR 12 represents R 7 ~R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Z 1 and Z 2 may be bonded to each other to form an aromatic ring. 3 and A 4 Each independently represents -O-, -N(R 13 ) represents a group selected from the group consisting of -, -S-, and -CO-; R 13 represents a hydrogen atom or a substituent. X represents a nonmetallic atom of Groups 14 to 16. However, the nonmetallic atom may be bonded to a hydrogen atom or a substituent. D 5 and D. 6 each independently represents a single bond, -CO-, -O-, -S-, -C(=S)-, or -CR 1 R 2 -, -CR 3 =CR 4 --, --NR 5 -, or a divalent linking group consisting of two or more of these, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 3 and S.P. 4 each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent. 3 and L 4 each independently represents a monovalent organic group; L 3 and L 4 And L in the formula (1) 1 and L 2 At least one of these represents a polymerizable group. Ax represents an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. Ay represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. The aromatic rings in Ax and Ay may have a substituent, and Ax and Ay may be bonded to form a ring. Q 3 represents a hydrogen atom or an optionally substituted alkyl group having 1 to 20 carbon atoms. In the formula (2), * represents a bonding position. 21 , R 22 , and R 23 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group. In the formula (3), Re(450) represents the in-plane retardation of the optically anisotropic layer at a wavelength of 450 nm, and Re(550) represents the in-plane retardation of the optically anisotropic layer at a wavelength of 550 nm.

2. The optically anisotropic layer according to claim 1, wherein the reverse dispersion compound (I) is a liquid crystal compound.

3. The optically anisotropic layer according to claim 1, which has a surface free energy of 35 mN / m or less.

4. The optically anisotropic layer according to claim 1, having a surface free energy of 24 mN / m or more.

5. The optically anisotropic layer according to claim 1, wherein the surfactant (II) is a surfactant such that, when a solution containing 0.08% by mass of the surfactant (II) and cyclopentanone and methyl ethyl ketone in a mass ratio of 4:1 is prepared, the surface tension of the solution is 22 mN / m or more.

6. The optically anisotropic layer according to claim 5, wherein the surfactant (II) is a surfactant that gives the solution a surface tension of 30 mN / m or less.

7. The optically anisotropic layer according to claim 6, wherein the surfactant (II) is a surfactant that gives the solution a surface tension of 27 mN / m or less.

8. The optically anisotropic layer according to claim 1, wherein the surfactant (II) has a structure represented by the following formula (4): In the formula (4), * represents a bonding position. 31 ~R 39 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group.

9. The optically anisotropic layer according to claim 1, wherein the surfactant (II) has a structure represented by the following formula (5): In the formula (5), * represents a bonding position. 41 ~R 45 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group; ns represents an integer of 1 to 15; when ns is an integer of 2 to 15, a plurality of R 41 may be the same or different, and multiple R 42 may be the same or different.

10. The optically anisotropic layer according to claim 1, wherein, when the solubility parameter of a liquid crystal mixture is defined as a weighted average value obtained by multiplying the solubility parameters of all liquid crystal compounds contained in the liquid crystal composition by the content of each liquid crystal compound, the relative energy difference of the surfactant (II) with respect to the liquid crystal mixture in terms of the solubility parameters is 6 or more and 12 or less. Here, the relative energy difference means the distance between the solubility parameter of the surfactant (II) and the solubility parameter of the liquid crystal mixture.

11. The optically anisotropic layer according to claim 1, wherein the surfactant (II) is a polymer having a repeating unit A containing the structure of the formula (2).

12. The optically anisotropic layer according to claim 11, wherein the repeating unit A is a repeating unit containing a structure represented by the following formula (6): In the formula (6), * represents a bonding position. 51 and R 52 Each of R independently represents a hydrogen atom or an alkyl group. 53 represents a hydrogen atom or a substituent. 5 is -O- or -NR Z -, where R Z represents a hydrogen atom or a substituent.

13. The optically anisotropic layer according to claim 11, wherein the surfactant (II) is a polymer containing the repeating unit A in a proportion of 40% by weight or more and 90% by weight or less.

14. The optically anisotropic layer according to claim 11, wherein the surfactant (II) is a polymer having a weight average molecular weight of 15,000 or less.

15. The optically anisotropic layer according to claim 10, wherein the surfactant (II) is a polymer having a repeating unit A containing the structure of formula (2) and a repeating unit B not containing the structure of formula (2), and the relative energy difference of the monomer of the repeating unit B with respect to the liquid crystal mixture in terms of solubility parameter is 3 or more and 7 or less, wherein the relative energy difference means the distance between the solubility parameter of the monomer of the repeating unit B and the solubility parameter of the liquid crystal mixture.

16. The optically anisotropic layer according to claim 11, wherein the surfactant (II) is a polymer having the repeating unit A and a repeating unit B not containing the structure of formula (2), and the repeating unit B is a repeating unit containing a functional group that reacts with light or heat to form crosslinks.

17. The optically anisotropic layer according to claim 11, wherein the surfactant (II) is a polymer having two or more types of repeating units A having different structures.

18. The optically anisotropic layer according to claim 1, comprising the surfactant (II) having two or more different structures.

19. The optically anisotropic layer according to claim 1, wherein the content of the surfactant (II) is 0.1 parts by mass or less per 100 parts by mass of the liquid crystal compound, wherein the 100 parts by mass of the liquid crystal compound that is the basis for the content of the surfactant (II) is 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I) when the reverse dispersion compound (I) is a liquid crystal compound.

20. Ar in the above formula (1) 1 and Ar 2 each independently represents any one of aromatic rings selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8).

21. Ar in the above formula (1) 1 and Ar 2 each independently represents any one of aromatic rings selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8).

22. The optically anisotropic layer according to claim 11, wherein the surfactant (II) is a polymer having the repeating unit A and a repeating unit B not containing a structure represented by formula (2), and the repeating unit B is a repeating unit containing a structure represented by formula (7) below: In the formula (7), R 61 represents a hydrogen atom or a methyl group. 62 represents a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, np represents an integer of 1 to 4, and nq represents an integer of 1 to 100.

23. The optically anisotropic layer according to claim 1, wherein the liquid crystal composition further contains a solvent, the solvent includes a high-boiling point solvent having a boiling point of 130° C. or more, and the content of the high-boiling point solvent is 150 parts by mass or more per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, the 100 parts by mass of the liquid crystal compound that is the basis for the content of the high-boiling point solvent is 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I).

24. The optically anisotropic layer according to claim 11, wherein the liquid crystal composition further contains a solvent, the solvent includes a high-boiling point solvent having a boiling point of 130° C. or more, and the content of the high-boiling point solvent is 150 parts by mass or more per 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, the 100 parts by mass of the liquid crystal compound that is the basis for the content of the high-boiling point solvent is 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I).

25. An optical film having an optically anisotropic layer according to any one of claims 1 to 24.

26. A polarizing plate comprising the optically anisotropic layer according to any one of claims 1 to 24 and a polarizer.

27. The polarizing plate of claim 26, further comprising a positive C plate.

28. An image display device having the optically anisotropic layer according to any one of claims 1 to 24.

29. A liquid crystal composition comprising a reverse dispersion compound (I) represented by the following formula (1), at least one liquid crystal compound, and a surfactant (II) having a structure represented by the following formula (2) in its molecule. Here, in the formula (1), D 1 , D 2 , D 3 and D. 4 each independently represents a single bond, -CO-, -O-, -S-, -C(=S)-, or -CR 1 R 2 -, -CR 3 =CR 4 --, --NR 5 -, or a divalent linking group consisting of two or more of these, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 1 A G Or SP G Represents. A 1 , A 2 and A G each independently represents an aromatic hydrocarbon ring which may have a substituent, an aromatic heterocycle which may have a substituent, or a divalent alicyclic hydrocarbon group which may have a substituent, provided that -CH 2 One or more of - may be replaced by -O-, -S- or -NH-. 1 , S.P. 2 and S.P. G each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent. 1 and L 2 each independently represents a monovalent organic group; L 1 and L 2 At least one of Ar represents a polymerizable group. 1 and Ar 2 When at least one of the following formula (Ar-4) is an aromatic ring, L 1 and L 2 And L in the following formula (Ar-4): 3 and L 4 At least one of the groups represents a polymerizable group. m represents an integer of 0 to 2. When m is 2, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. l and n each independently represent 0 or an integer of 1 or more. When l is an integer of 2 or more, a plurality of A 1 may be the same or different, and a plurality of D 3 may be the same or different. When n is an integer of 2 or more, a plurality of D 4 may be the same or different, and a plurality of A 2 may be the same or different. p represents 0 or an integer of 1 or more. When p is an integer of 2 or more, a plurality of Ar 1 may be the same or different, and a plurality of D 2 may be the same or different. When p is an integer of 2 or more and m is not 0, a plurality of G 1 may be the same or different, and a plurality of D 1 may be the same or different. 1 and Ar 2 each independently represents an aromatic ring selected from the group consisting of groups represented by the following formulas (Ar-1) to (Ar-8): In the formulae (Ar-1) to (Ar-8), *1 represents D 3 Or D 4 *2 represents the bonding position with D 1 Or D 2 When l is 0, D 3 The bond position with 1 When m is 0, *2 represents a bonding position with D 2 When n is 0, D 4 The bond position with 2 It represents the bonding position with Q. 1 represents N or CH. 2 is -S-, -O-, or -N(R 6 )-, R 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 1 represents a monovalent aromatic hydrocarbon group having 6 to 12 carbon atoms which may have a substituent, a monovalent aromatic heterocyclic group having 3 to 12 carbon atoms which may have a substituent, or a monovalent alicyclic hydrocarbon group having 6 to 20 carbon atoms which may have a substituent, provided that -CH 2 One or more of - may be substituted with -O-, -S- or -NH-. 1 , Z 2 and Z 3 each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, a monovalent aromatic heterocyclic group having 6 to 20 carbon atoms, a halogen atom, a cyano group, a nitro group, -OR 7 , -NR 8 R 9 , -SR 10 , -COOR 11 or -COR 12 represents R 7 ~R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Z 1 and Z 2 may be bonded to each other to form an aromatic ring. 3 and A 4 Each independently represents -O-, -N(R 13 ) represents a group selected from the group consisting of -, -S-, and -CO-; R 13 represents a hydrogen atom or a substituent. X represents a nonmetallic atom of Groups 14 to 16. However, the nonmetallic atom may be bonded to a hydrogen atom or a substituent. D 5 and D. 6 each independently represents a single bond, -CO-, -O-, -S-, -C(=S)-, or -CR 1 R 2 -, -CR 3 =CR 4 --, --NR 5 -, or a divalent linking group consisting of two or more of these, R 1 ~R 5 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 12 carbon atoms. 3 and S.P. 4 each independently represents a single bond or a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms. 2 One or more of - may be substituted with -O-, -S-, -NH-, -N(Q)- or -CO-. Q represents a substituent. 3 and L 4 each independently represents a monovalent organic group; L 3 and L 4 And L in the formula (1) 1 and L 2 At least one of these represents a polymerizable group. Ax represents an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. Ay represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. The aromatic rings in Ax and Ay may have a substituent, and Ax and Ay may be bonded to form a ring. Q 3 represents a hydrogen atom or an optionally substituted alkyl group having 1 to 20 carbon atoms. In the formula (2), * represents a bonding position. 21 , R 22 , and R 23 each independently represents an alkyl group, an alkenyl group, an aryl group, or an alkylenearyl group.

30. The liquid crystal composition according to claim 29, wherein the content of the surfactant (II) is 0.1 parts by mass or less relative to 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, 100 parts by mass of the liquid crystal compound as the basis for the content of the surfactant (II) is 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I).

31. Ar in the above formula (1) 1 and Ar 2 each independently represents any one of aromatic rings selected from the group consisting of groups represented by formulas (Ar-1), (Ar-2), and (Ar-4) to (Ar-8).

32. The liquid crystal composition according to claim 29, wherein the surfactant (II) is a polymer having the repeating unit A and a repeating unit B not containing a structure represented by formula (2), and the repeating unit B is a repeating unit containing a structure represented by formula (7) below: In the formula (7), R 61 represents a hydrogen atom or a methyl group. 62 represents a hydrogen atom or an alkyl group having 1 to 18 carbon atoms, np represents an integer of 1 to 4, and nq represents an integer of 1 to 100.

33. The liquid crystal composition according to claim 29, further comprising a solvent, the solvent including a high-boiling point solvent having a boiling point of 130° C. or higher, and the content of the high-boiling point solvent is 150 parts by mass or more relative to 100 parts by mass of the liquid crystal compound. Here, when the reverse dispersion compound (I) is a liquid crystal compound, 100 parts by mass of the liquid crystal compound, which is the basis for the content of the high-boiling point solvent, refers to 100 parts by mass of the total amount of the liquid crystal compound including the reverse dispersion compound (I).

Citation Information

Patent Citations

  • Optical film, and polarizing plate and liquid crystal display using the same

    JP2007033712A

  • Polymerizable liquid crystal composition and optically anisotropic body produced using said composition, phase difference film, antireflection film and liquid crystal display element

    WO2016114047A1

  • Polymerizable composition and optically anistropic body using same

    WO2017057020A1

  • Polymerizable liquid-crystal composition, and optically anisotropic object and liquid-crystal display element both obtained using same

    WO2018003653A1

  • Composition for forming liquid crystal cured film and use of same

    WO2020218104A1

Cited By

  • Liquid crystal composition, light-absorbing anisotropic film, laminate, and image display device

    WO2025143020A1

  • copolymer

    WO2026071208A1