Composite resin molded body

A composite resin molded article with thermoplastic resins and a coloring agent promotes color development in fused portions, addressing the issue of color loss in thermal bonding, ensuring visible distinction and improved design.

JP7583151B2Active Publication Date: 2024-11-13エムエーライフマテリアルズ株式会社
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023508909
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-25
Filing Date
2022-03-04
Publication Date
2024-11-13
Estimated Expiration
2042-03-04

AI Technical Summary

Technical Problem

The risk of colored paint decomposition and adhesion loss during thermal bonding of nonwoven fabrics for absorbent articles, such as diapers and sanitary napkins, leads to difficulty in visually recognizing the fused portions due to lack of coloration.

Method used

A composite resin molded article is created by fusing a first resin molded body containing a thermoplastic resin without a coloring agent with a second resin molded body containing a thermoplastic resin that promotes color development, ensuring the fused portion is visibly distinct through chemical interaction of the coloring agent.

Benefits of technology

The fused portion of the composite resin molded article is easily recognizable by a distinct color tone, even without external coloring, enhancing visibility and design aesthetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583151000005
    Figure 0007583151000005
  • Figure 0007583151000006
    Figure 0007583151000006
  • Figure 0007583151000001
    Figure 0007583151000001
Patent Text Reader

Abstract

This composite resin molded body comprises a first resin molded body, a second resin molded body, and a fused part. The first resin molded body contains a first thermoplastic resin and a coloring agent. The second resin molded body contains a second thermoplastic resin and a color developing agent that promotes color development or color change of the coloring agent. In the fused part, a part of the first resin molded body and a part of the second resin molded body are fused.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a composite resin molded article. [Background technology]

[0002] Due to their excellent breathability and flexibility, thermally bonded nonwoven fabrics are widely used as topsheets for absorbent articles, including disposable diapers and sanitary napkins. It is known that thermally bonded nonwoven fabrics can be obtained by sandwiching a web containing fibers made of a thermoplastic resin between a heated embossing roll and a smooth roll to melt some of the fibers and bond them together. On the other hand, valley dyeing is known as a technique for enhancing the decorative effect by strengthening the contrast between a concave-convex pattern and its surroundings (Patent Document 1). Valley dyeing is a method in which a colored paint is applied to the convex parts of the pattern of an embossing roll to create a pattern on a substrate, and at the same time, the concave parts of the pattern on the substrate are colored.

[0003] Patent document 1: Japanese Patent Application Laid-open No. 53-24365 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when valley dyeing is used in the manufacturing method of the thermal bonded nonwoven fabric to enhance the decorative effect, the colored paint attached to the convex portion of the pattern of the embossing roll may be decomposed by the heat of the embossing roll. Therefore, the fused portion of the thermal bonded nonwoven fabric may not be colored as desired. The colored paint attached to the fused portion may fall off from the fused portion. As a result, the fused portion colored by valley dyeing may be difficult to see.

[0005] In view of the above circumstances, an object of the present disclosure is to provide a composite resin molding in which a fused portion is easily visible from the outside due to its color tone even if it is not colored. [Means for solving the problem]

[0006] Means for solving the above problems include the following embodiments. <1> A first resin molded body containing a first thermoplastic resin and a color former; A second resin molded body containing a second thermoplastic resin and a color developer that promotes color development or color change of the color developer; a fused portion at which a portion of the first resin molded body and a portion of the second resin molded body are fused to each other, <2> The first resin molding does not contain the color developer, The second resin molding does not contain the color former. <1> The composite resin molding according to claim 1. <3> the first resin molding includes a first fiber, The second resin molding includes a second fiber. <1> or <2> The composite resin molding according to claim 1. <4> the first resin molding is a first spunbond web containing the first fibers, the second resin molding is a second spunbond web containing the second fibers, The first spunbond web is laminated on one major surface of the second spunbond web. <3> The composite resin molding according to claim 1. <5> the first resin molding is a first fiber, the second resin molding is a second fiber, The first fibers and the second fibers constitute a mixed fiber spunbond web. <3> The composite resin molding according to claim 1. <6> The color former is contained within the first fiber, The color developer is contained in the second fiber. <3> ~ <5> 10. The composite resin molding according to claim 9, <7> The fused portion contains, at least inside thereof, a color-forming compound of the color former and the color developer. <1> ~ <6> 10. The composite resin molding according to claim 9, <8> The color former includes a leuco dye. <1> ~ <7> 10. The composite resin molding according to claim 9, Effect of the Invention

[0007] According to the present disclosure, a composite resin molding is provided in which the fused portion is easily visible from the outside due to its color tone even if it is not colored. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing an example of a manufacturing apparatus for a multilayer spunbonded nonwoven fabric according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a production apparatus for a mixed fiber spunbonded nonwoven fabric according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of a composite resin molded article according to the present disclosure will be described with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and description thereof will not be repeated. The following description of the configuration elements may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this disclosure, "mass%" and "weight%" are synonymous, and "parts by mass" and "parts by weight" are synonymous. In this disclosure, "%" indicating the amount of a component is based on mass unless otherwise specified. In the description of groups (atomic groups) in this specification, when there is no indication of whether substituted or unsubstituted, the indication encompasses both those having no substituents and those having a substituent. In this disclosure, the term "layer" includes cases where the layer is formed over the entire area when the area in which the layer exists is observed, as well as cases where the layer is formed over only a portion of the area. In the present disclosure, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the purpose of the step is achieved.

[0010] [Composite resin molded body] A composite resin molded body according to an embodiment of the present disclosure includes a first resin molded body, a second resin molded body, and a fused portion. The first resin molded body contains a first thermoplastic resin and a color former. The second resin molded body contains a second thermoplastic resin and a color former. The color former promotes color development or color change of the color former. The fused portion is formed by fusing a part of the first resin molded body and a part of the second resin molded body. The first resin molded body is preferably mainly composed of a first thermoplastic resin. The second resin molded body is preferably mainly composed of a second thermoplastic resin. The first resin molded body preferably does not contain a color former. The second resin molded body preferably does not contain a color former.

[0011] The term "color former" refers to a compound whose chemical structure changes as a result of chemical interaction with a color developer, and which develops or changes color. The term "color developer" refers to a compound that is colorless by itself, but that changes the chemical structure of a color former through chemical interaction with the color former, causing the color former to develop color or changing the color hue of the color former. "Containing a first thermoplastic resin as a main component" means that the content of the first thermoplastic resin in the first resin molded body is 50 mass % or more with respect to the total amount of the first resin molded body. The first resin molding "does not contain a colorant" means that the content of the colorant in the first resin molding, relative to the total amount of the first resin molding, is sufficiently low so as not to change the color tone of the first resin molding even in the presence of a color former, and is preferably 0.005 mass% or less, including 0 mass%. "Containing the second thermoplastic resin as a main component" means that the content of the second thermoplastic resin in the second resin molded body is 50 mass % or more with respect to the total amount of the second resin molded body. The second resin molding "does not contain a color former" means that the content of the color former in the second resin molding, relative to the total amount of the second resin molding, is sufficiently low so as not to change the color tone of the second resin molding even in the presence of a color developer, and is preferably 0.005 mass% or less, including 0 mass%. "Having compatibility" means that in an atmosphere in which the first thermoplastic resin and the second thermoplastic resin are melted, the melt of the first thermoplastic resin and the melt of the second thermoplastic resin are mixed together without being separated. From the viewpoint of efficiently expressing the chemical interaction between the color former contained in the first resin molded body and the color former contained in the second resin molded body, it is preferable that the compatibility between the first thermoplastic resin and the second thermoplastic resin is high. "Fusion" means that a portion of the first resin molded body and a portion of the second resin molded body melt and mix with each other, and the molten portions of the first resin molded body and the second resin molded body are integrated with each other. The "fused portion" refers to a portion where the first thermoplastic resin contained in the first resin molded body and the second thermoplastic resin contained in the second resin molded body are mixed with each other.

[0012] The composite resin molded product according to an embodiment of the present disclosure includes a fused portion in which a part of the first resin molded product and a part of the second resin molded product are fused together. Therefore, the fused portion is easily visible due to its color tone even if it is not colored from the outside. This is presumably due to the following reasons. When the color former and the color developer are mixed, the color former is likely to develop or change color. In one embodiment of the present disclosure, in the first resin molded body and the second resin molded body, the color former and the color developer are held in a separated state by the first thermoplastic resin and the second thermoplastic resin. Therefore, chemical interaction between the color former and the color developer is unlikely to occur. As a result, the first resin molded body and the second resin molded body are unlikely to develop or change color due to the color former. On the other hand, the fused portion is formed by heat fusing a part of the first resin molding and a part of the second resin molding. That is, when the fused portion is formed by heating, a state in which the color former and the color-developing agent temporarily coexist is formed in the fused portion. As a result, the chemical interaction between the color former and the color-developing agent becomes easier to work, and the fused portion develops or changes color due to the action of the color former. As a result, the fused and non-fused parts of the composite resin molding have different colors. The non-fused parts are the parts of the composite resin molding that are not fused. Therefore, the fused parts are easily visible due to their color even if they are not colored from the outside.

[0013] <Resin molded body> From the viewpoint of visibility, each of the first resin molded body and the second resin molded body may be a molded body molded in any shape. At least one of the first resin molding and the second resin molding may be a sheet-like product. That is, the first resin molding and the second resin molding may be sheet-like products, or only one of the first resin molding and the second resin molding may be a sheet-like product. Examples of the sheet-like material include a resin film and a nonwoven fabric sheet. When the first resin molding is a short sheet-like object (hereinafter referred to as the "first short sheet") and the second resin molding is a short sheet-like object (hereinafter referred to as the "second short sheet"), the composite resin molding may be a bag. The bag includes a first short sheet, a second short sheet, and a fused portion. The fused portion may be continuously formed along the outer peripheral edge of the main surface of the laminate. In the laminate, the first short sheet and the second short sheet are laminated such that the main surfaces of the first short sheet and the second short sheet face each other. This allows the user to easily know whether the bag is sealed or not by the difference in color tone between the fused portion and the non-fused portion. The main surface refers to each of a pair of surfaces having the largest area in the sheet-like object. When one of the first resin molded body and the second resin molded body is a sheet-like material and the other is not a sheet-like material, the composite resin molded body may be a packaging container. The packaging container may include a resin film, a tray, which is an example of a non-sheet-like material, and a fused portion. The tray has a recess for accommodating an item. The resin film covers the entire opening of the recess so as to form an accommodating space for the item between the resin film and the recess of the tray. The fused portion may be formed continuously so as to surround the recess. This allows the user to easily know whether the packaging container is sealed or not by the difference in color tone between the fused portion and the non-fused portion. Examples of the tray include a food tray.

[0014] From the viewpoint of visibility, it is preferable that the first resin molding contains first fibers, and the second resin molding contains second fibers. When the first resin molded body includes the first fiber and the second resin molded body includes the second fiber, the composite resin molded body may be a nonwoven fabric, a woven fabric, or a knitted fabric. From the viewpoint of visibility, the composite resin molded body is preferably a nonwoven fabric. The term "nonwoven fabric" refers to a fiber sheet, web, or batt in which the fibers are oriented in one direction or randomly and the fibers are bonded to each other by physical entanglement or fusion. The nonwoven fabric does not include paper, woven fabric, knitted fabric, tufts, and crepe felt. Examples of the nonwoven fabric include spunbonded nonwoven fabric, meltblown nonwoven fabric, and flash spun nonwoven fabric. The term "spunbonded nonwoven fabric" refers to a nonwoven fabric made by laminating a group of continuous fibers (filaments) spun from a spinneret by melting or dissolving a thermoplastic resin composition on a moving collecting member, and using one or more bonding methods. The bonding method includes heat compression bonding, which will be described later. The thermoplastic resin composition, the spinneret, and the moving collecting member will be described later. Examples of the woven fabric include plain weave fabric, twill weave fabric, satin weave fabric, etc. Each of the first fiber and the second fiber may be a long fiber or a short fiber.

[0015] It is preferable that the color former is contained in the first fiber, and the color developer is contained in the second fiber. This allows the fused portion to contain a reaction product of the color former and a reaction product of the color developer inside. As a result, the color or discoloration of the fused portion is less likely to change due to wear of the fused portion than when the fused portion is colored from the outside using a colored paint or the like.

[0016] From the viewpoint of visibility, it is preferable that the first resin molding contains a first spunbond web containing a first fiber, and the second resin molding contains a second spunbond web containing a second fiber. The term "spunbond web" refers to a web made by extruding a molten or dissolved thermoplastic resin composition from a spinneret and laminating continuous fibers (filaments) on a moving collecting member. The spunbond web differs from a spunbond nonwoven fabric in that the fibers constituting the spunbond web are not bonded to each other. When the first resin molding contains a first spunbond web containing a first fiber, and the second resin molding contains a second spunbond web containing a second fiber, the composite resin molding may be a multi-layer spunbond nonwoven fabric. The multi-layer spunbond nonwoven fabric may include a first fiber constituting the first spunbond web, a second fiber constituting the second spunbond web, and a fused portion. It is preferable that the first spunbond web is laminated on one main surface of the second spunbond web. The first fibers constituting the first spunbond web and the second fibers constituting the second spunbond web are each long fibers, the definition of which will be given later. The multi-layer spunbond nonwoven fabric will be described in detail later. Hereinafter, when the composite resin molding is a multi-layer spunbond nonwoven fabric, the composite resin molding may be referred to as a "multi-layer spunbond nonwoven fabric."

[0017] From the viewpoint of visibility, the composite resin molding is preferably a mixed fiber spunbond web. The mixed fiber spunbond web may be composed of each of the first fiber and the second fiber. The mixed fiber spunbond web includes the first fiber and the second fiber. When each of the first fiber and the second fiber constitutes a mixed fiber spunbond web, the composite resin molding is preferably a mixed fiber spunbond nonwoven fabric. The mixed fiber spunbond nonwoven fabric includes the first fiber and the second fiber constituting the mixed fiber spunbond web and a fused portion. Each of the first fiber constituting the mixed fiber spunbond web and the second fiber constituting the mixed fiber spunbond web is a long fiber. The mixed fiber spunbonded nonwoven fabric will be described in detail later. Hereinafter, when the composite resin molding is a mixed fiber spunbonded nonwoven fabric, the composite resin molding may be referred to as a "mixed fiber spunbonded nonwoven fabric."

[0018] <Fused part> The fused portion bonds the first resin molded body and the second resin molded body, and has a color tone different from that of the non-fused portion. The fused portion includes a reactant of the color former and a reactant of the color developer. The fused portion may include a first thermoplastic resin and a second thermoplastic resin. The fused portion may include an unreacted product of the color former and an unreacted product of the color developer. The fused portion may be formed in one place or in multiple places in the composite resin molding. The location where the fused portion is formed, the shape of the fused portion, etc. may be appropriately adjusted depending on the application of the composite resin molding, etc. When the composite resin molding is a nonwoven fabric, the fused portion is thinner (film-like) than the non-fused portion. If the area ratio of the fused portion is not 100%, it is appropriately adjusted depending on the application of the composite resin molding. When the composite resin molding is a nonwoven fabric, the area ratio of the fused portion is preferably 7% to 20%. The area ratio of the fused portion is determined by taking a test piece of 10 mm x 10 mm from the composite resin molding, observing the contact surface of the test piece with the embossing roll under an electron microscope (magnification: 100 times), and measuring the ratio of the area of ​​the fused portion to the area of ​​the observed composite resin molding.

[0019] The fused part preferably contains, at least inside, a color-developing compound of a color former and a coloring agent (i.e., a reaction product in which a color former and a coloring agent react to develop or change color, and the color former is a compound in which the color former develops or changes color.) As a result, the color development or discoloration of the fused part is caused by the color-developing compound produced by the reaction during heating, and therefore the fused part is less likely to change due to wear than when the fused part is colored from the outside using a colored paint or the like.

[0020] <Color difference(ΔE * )> The difference in color tone between the fused and unfused parts is the La standardized by the CIE (International Commission on Illumination). * b * c * Color difference (ΔE * ) Since the configuration of the fused portion before fusion is the same as the configuration of the non-fused portion, the difference in color tone between the fused portion and the non-fused portion can be regarded as the difference in color tone before and after fusion. The CIELab color space is * axis, a * axis and b * It is expressed in a three-dimensional coordinate system with mutually orthogonal axes. * The axis represents lightness. The L value ranges from 0 to 100, and the higher the L value, the brighter the light. * The positive axis represents redness. * The - axis direction represents green. * The positive axis represents yellowness. * The negative axis represents blueness. The color difference between two colors in the CIELAB color space (ΔE * ) defines the Euclidean distance between color coordinates (color specifications) in the CIELab color space.

[0021] ΔE before and after fusion * can be measured using a spectrophotometer. * Value, a1 * Value, b1 * value and L2 of the reflected light of the fused part * Value, a2 * Value, b2 *By measuring each value and applying these measurements to the following formula (A), ΔE * is required. ΔE * is an index of the change in color tone due to the color development or discoloration of the color former. * The higher the value, the better the visual contrast.

[0022] Formula (A): ΔE * =((L1 * -L2 * ) 2 +(a1 * -a2 * ) 2 +(b1 * -b2 * ) 2 ) 1 / 2

[0023] An example of a spectrophotometer is the "CM-3700A" manufactured by Konica Minolta, Inc.

[0024] From the perspective of visibility, ΔE * is preferably 3 to 120, more preferably 6 to 120, further preferably 8 to 120, particularly preferably 10 to 120, even more preferably 15 to 120, and still further preferably 20 to 120.

[0025] ΔL * The preferred range of varies depending on whether the color former before color development or color change (hereinafter referred to as "first color former") is achromatic or chromatic. "Achromatic" refers to white, gray, or black. "Chromatic" refers to all colors other than achromatic, and examples include red, yellow-red, yellow, yellow-green, green, blue-green, blue, blue-purple, purple, or red-purple. From the viewpoint of the difference in brightness before and after fusion, when the first color former is achromatic, ΔL * is preferably −100 to −15, more preferably −100 to −20, even more preferably −100 to −25, particularly preferably −100 to −30, and even more preferably −100 to −35. From the viewpoint of the difference in brightness before and after fusion, if the first color former is chromatic, ΔL *is preferably −100 to −90, more preferably −100 to −80, further preferably −100 to −70, and particularly preferably −100 to −60.

[0026] Δa * The preferred range of varies depending on the color of the first color former. When the first color is red, Δa * is preferably +15 or more, more preferably +20 or more, further preferably +25 or more, and particularly preferably +30 or more. * is preferably −15 or less, more preferably −20 or less, further preferably −25 or less, and particularly preferably −30 or less.

[0027] Δb * The preferred range of varies depending on the color of the first color former. When the color of the first color former is blue, Δb * is preferably −15 or less, more preferably −20 or less, even more preferably −25 or less, and most preferably −30 or less.

[0028] (Color formers and colorants) The combination of the color former and the color developer may be freely selected as long as the color former develops or changes color through chemical interaction with the color developer, and the first resin molded body, the second resin molded body, and the composite resin molded body can be molded normally. Specific examples include an oxidizing agent and a reducing agent, an acid and a base, and the like. From the viewpoint of safety and ease of handling, a combination of an acid and a base is preferred. That is, the chemical interaction between the color former and the color developer more preferably includes an acid-base reaction, and more preferably is an acid-base reaction.

[0029] (Color former) The color former is appropriately selected depending on the use of the composite resin molded body, the color tone developed by chemical interaction with the color developer, etc. From the viewpoint of emphasizing the color tone difference between the fused and non-fused parts of the composite resin molded body, the color former is preferably a dye that develops color from colorless to color rather than a dye that changes color from colored to colored, more preferably includes a leuco dye, and even more preferably is a leuco dye.

[0030] Examples of leuco dyes that develop color through an acid-base reaction include indolylphthalide compounds, indolephthalide compounds, fluoran compounds, triphenylmethanephthalide compounds, phenothiazine compounds, indolylazaphthalide compounds, triphenylmethane compounds, spiropyran compounds, triazene compounds, leucoauramine compounds, and rhodamine lactam compounds. Indolylazaphthalide compounds include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methyl-3-indolyl)-4-azaphthalide. Indolephthalide compounds include 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide. These leuco dyes are colorless or light-colored basic compounds that have a lactone ring in the molecule. These leuco dyes develop color when the lactone ring is cleaved by an acid, and become colorless or light-colored when the closed ring structure of the lactone ring is changed by a base. That is, the color-developing reaction of the leuco dye is reversible. These leuco dyes may be used alone or in combination of two or more kinds. When the composite resin molded product is a spunbonded nonwoven fabric, the leuco dye is preferably a compound that does not thermally decompose at 250° C. Spunbonded nonwoven fabrics include multilayer spunbonded nonwoven fabrics described below and mixed fiber spunbonded nonwoven fabrics described below. Spunbonded nonwoven fabrics may be exposed to an atmosphere at 250° C. during the manufacturing process of the spunbonded nonwoven fabric. Therefore, if the leuco dye is a compound that does not thermally decompose at 250° C., the fused portion is easily visible due to its color tone even if it is not colored from the outside. Examples of leuco dyes that do not undergo thermal decomposition at 250° C. include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methyl-3-indolyl)-4-azaphthalide and 3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide.

[0031] The content of the color former is appropriately selected depending on the shape of the first resin molded body and the like. When the first resin molding is a fiber, the content of the color former is preferably 0.01% by mass to 15% by mass, more preferably 0.1% by mass to 10% by mass, based on the total amount of the first resin molding. If the content of the color former is within the above range, the occurrence of molding defects such as thread breakage can be suppressed. If the content of the color former is within the above range, sufficient visibility can be imparted to the fused portion of the composite resin molding. When the first resin molding is a sheet-like product, the content of the color former is preferably 0.01% by mass to 15% by mass, more preferably 0.1% by mass to 10% by mass, based on the total amount of the first resin molding. If the content of the color former is within the above range, the occurrence of molding defects such as sheet breakage can be suppressed. If the content of the color former is within the above range, sufficient visibility can be imparted to the fused portion of the composite resin molding.

[0032] (Color developer) The color developer is appropriately selected depending on the type of color developer, etc. Examples of color-developing agents capable of coloring the basic leuco dye include phenolic compounds, higher fatty acids, aromatic carboxylic acids, etc. Examples of phenolic compounds include bisphenol S, 4-isopropoxyphenyl-4-hydroxyphenyl sulfone, etc. Examples of higher fatty acids include stearic acid, etc. These color-developing agents may be used alone or in combination of two or more. When the composite resin molded product is a spunbonded nonwoven fabric, the color developer is preferably a compound that does not thermally decompose at 250° C. Spunbonded nonwoven fabrics may be exposed to an atmosphere at 250° C. during the manufacturing process of the spunbonded nonwoven fabric. Therefore, if the color developer is a compound that does not thermally decompose at 250° C., the fused portion is easily visible due to its color tone even if it is not colored from the outside. Examples of color-developing agents that do not undergo thermal decomposition at 250° C. include bisphenol S, 4-isopropoxyphenyl-4-hydroxyphenyl sulfone, and stearic acid. The melting point of the colorant is preferably lower than the temperature at which the fused portion of the composite resin molding is formed (hereinafter referred to as the "fusion temperature"). This makes it easier for the colorant to melt when a portion of the first resin molding and a portion of the second resin molding are heated at the fusion temperature. Therefore, in the fused portion, the colorant and colorant are maintained in a more mixed state than when a colorant whose melting point is equal to or higher than the fusion temperature is used. In other words, the fused portion is more likely to develop color. As a result, the fused portion is more easily visible due to its color tone even if it is not colored from the outside. When the composite resin molding is a spunbond nonwoven fabric, the melting point of the colorant is preferably not more than 150° C. Examples of colorants having a melting point of not more than 150° C. include 4-isopropoxyphenyl-4-hydroxyphenylsulfone and stearic acid. When the composite resin molding is a spunbonded nonwoven fabric, from the viewpoint of moldability of the second resin molding, the color developer is preferably a higher fatty acid. When the color former is a basic leuco dye and it is desired to color the fused portion more strongly, it is preferable that the color former has a high acidity, i.e., a low acid dissociation constant (pKa). This makes it easier for the lactone ring of the leuco dye to open when the leuco dye and the color former are mixed together. In other words, the leuco dye is more likely to color.

[0033] The content of the color developer is appropriately selected depending on the shape of the second resin molded body and the like. When the second resin molding is a fiber, the content of the coloring agent is preferably 0.01% by mass to 15% by mass, more preferably 0.1% by mass to 10% by mass, based on the total amount of the second resin molding. If the content of the coloring agent is within the above range, the occurrence of molding defects such as thread breakage can be suppressed. If the content of the coloring agent is within the above range, sufficient visibility can be imparted to the fused portion of the composite resin molding. When the second resin molding is a sheet-like product, the content of the color developer is preferably 0.01% by mass to 15% by mass, more preferably 0.1% by mass to 10% by mass, based on the total amount of the second resin molding. If the content of the color developer is within the above range, the occurrence of molding defects such as sheet breakage can be suppressed. If the content of the color developer is within the above range, sufficient visibility can be imparted to the fused portion of the composite resin molding.

[0034] It is preferable that the first resin molding does not contain a coloring agent, and the second resin molding does not contain the coloring agent. This makes it possible to further enhance the contrast between the fused portion and the non-fused portion. As a result, the fused portion is more easily visible due to its color tone even if it is not colored from the outside.

[0035] (1st thermoplastic resin) The first thermoplastic resin is not particularly limited as long as it is a thermoplastic resin, and is appropriately selected depending on the application of the composite resin molded body. In particular, it is preferable that the first thermoplastic resin is transparent. As such a transparent thermoplastic resin, reference may be made to the resins described in "Encyclopedia of Plastic Materials Utilization" (edition number: first edition, published by: Industrial Research Association Encyclopedia Publishing Center, published date: October 20, 2001). Specifically, examples of the transparent thermoplastic resin include polyolefin, general purpose polystyrene (GPPS: General Purpose Polysthylene), polyvinyl chloride, polyamide, polyester, polycarbonate, methacrylic resin, and mixtures thereof. Examples of the polyolefin include propylene-based polymers, low density polyethylene (LDPE: Low Density Polyethylene), linear low density polyethylene (LLDPE: Linear Low Density Polyethylene), high density polyethylene (HDPE: High Density Polyethylene), and the like. Examples of the propylene-based polymer include propylene homopolymers and propylene copolymers.

[0036] In particular, when the first resin molding is a fiber, from the viewpoints of spinning stability during molding and stretch processability of the nonwoven fabric, it is preferable that the first thermoplastic resin contains a propylene-based polymer, and it is particularly preferable that it is a propylene-based polymer. The melting point (Tm) of the propylene homopolymer is preferably 155°C or higher, more preferably 157°C to 165°C. The melting point (Tm) of the propylene copolymer is preferably 130°C or higher and lower than 155°C, more preferably 130°C to 150°C. The propylene copolymer is preferably a copolymer of propylene and one or more α-olefins. The α-olefin is an α-olefin having 2 or more carbon atoms (excluding 3 carbon atoms), preferably an α-olefin having 2 to 8 carbon atoms (excluding 3 carbon atoms). Examples of the α-olefin having 2 or more carbon atoms include ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene. The melt flow rate (MFR) of the propylene polymer is not particularly limited as long as it can be melt-spun, but is usually 1 g / 10 min to 1000 g / 10 min, preferably 5 g / 10 min to 500 g / 10 min, and more preferably 10 g / 10 min to 100 g / 10 min. The melt flow rate of the propylene-based polymer is measured according to ASTM D-1238 under the conditions of 230° C. and a load of 2.16 kg.

[0037] The content of the first thermoplastic resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of the first resin molded body.

[0038] (Second thermoplastic resin) The second thermoplastic resin is not particularly limited as long as it is a thermoplastic resin, and is appropriately selected depending on the application of the composite resin molding. Examples of the second thermoplastic resin include those exemplified as the first thermoplastic resin. The second thermoplastic resin may be the same as or different from the first thermoplastic resin. The second thermoplastic resin preferably contains a propylene-based polymer, and is particularly preferably a propylene-based polymer.

[0039] The content of the second thermoplastic resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of the second resin molded body.

[0040] The first thermoplastic resin and the second thermoplastic resin preferably contain the above-mentioned transparent thermoplastic resin (e.g., polyolefin). This makes the first resin molded body, the second resin molded body, and the fused portion more transparent than in the first configuration. In the first configuration, each of the first thermoplastic resin and the second thermoplastic resin does not contain a transparent thermoplastic resin (e.g., polyolefin). In other words, the contrast between the fused portion and the non-fused portion caused by the color development or discoloration of the color former can be further enhanced. As a result, the fused portion is more easily visible due to its color tone even if it is not colored from the outside.

[0041] Each of the first resin molded body and the second resin molded body may contain other components as necessary within a range that does not impair the effects of one embodiment of the present disclosure. Examples of other components include sensitizers, antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antifogging agents, lubricants, dyes, pigments, light stabilizers, antiblocking agents, dispersants, nucleating agents, softeners, water repellents, fillers, natural oils, synthetic oils, waxes other than ethylene polymer wax, antibacterial agents, preservatives, matting agents, rust inhibitors, fragrances, defoamers, antifungal agents, insect repellents, etc. These other components may be contained inside the composite resin molded body or may be attached to the surface of the composite resin molded body.

[0042] [Multi-layer spunbond nonwoven fabric] Next, the multi-layer spunbonded nonwoven fabric will be described. As described above, the multilayer spunbond nonwoven fabric includes first fibers constituting a first spunbond web, second fibers constituting a second spunbond web, and fused portions. The first spunbond web is laminated on one main surface of the second spunbond web. In the fused portions, a portion of the first fibers and a portion of the second fibers are fused to each other. The first spunbond web is an example of a first resin molding, and the second spunbond web is an example of a second resin molding.

[0043] The multilayer spunbonded nonwoven fabric has a fused portion where a part of the first fibers constituting the first spunbonded web and a part of the second fibers constituting the second spunbonded web are fused together. Therefore, the fused portion is easily visible due to its color tone even if it is not colored from the outside. As a result, the multilayer spunbonded nonwoven fabric has excellent designability.

[0044] It is preferable that the color former is contained in the first fiber constituting the first spunbond web, and the color developer is contained in the second fiber constituting the second spunbond web. This allows the fused portion to contain a reaction product of the color former and a reaction product of the color developer therein. As a result, the color or discoloration of the fused portion is less likely to change due to wear of the fused portion than when the fused portion is colored from the outside using a colored paint or the like.

[0045] <First spunbond web> The first spunbond web preferably has a basis weight of 360 g / m 2 Less than 240 g / m 2 More preferably, 150 g / m 2 Less than 15 g / m 2 ~120g / m 2 , and more preferably 8 g / m 2 ~25g / m 2 The method for measuring the basis weight is the same as that described in the examples.

[0046] The average fiber diameter of the first fibers constituting the first spunbond web is preferably 1 μm to 50 μm, more preferably 1 μm to 40 μm, and even more preferably 1 μm to 30 μm. When the average fiber diameter of the first fibers constituting the first spunbond web is small, the entire fibers including the color former are easily melted, which is preferable from the viewpoint of improving the color visibility of the fused portion. The average fiber diameter is determined as follows: Ten test pieces measuring 10 mm x 10 mm are taken from the obtained spunbond nonwoven fabric, and the fiber diameter is read in μm units to one decimal place at a magnification of 20 times using a Nikon ECLIPSE E400 microscope. The diameter is measured at 20 random points on each test piece, and the average value is calculated.

[0047] The thickness of the first spunbond web is appropriately selected depending on the application of the multilayer spunbond nonwoven fabric, and is preferably 0.1 mm to 1.0 mm, more preferably 0.2 mm to 0.5 mm. If the thickness of the first spunbond web is within the above range, the melting efficiency of the spunbond web can be increased to promote the formation of fused parts, and an appropriate thickness can be imparted to the fused parts to improve color visibility. The method for measuring the thickness of the first spunbond web is the same as that described in the Examples.

[0048] <Second spunbond web> The basis weight of the second spunbond web is the same as the example of the basis weight of the first spunbond web. The basis weight of the second spunbond web may be the same as or different from the basis weight of the first spunbond web.

[0049] The average fiber diameter of the second fibers constituting the second spunbond web may be the same as the average fiber diameter of the first fibers constituting the first spunbond web. The average fiber diameter of the second fibers constituting the second spunbond web may be the same as or different from the average fiber diameter of the first fibers constituting the first spunbond web. If the average fiber diameter of the second fibers constituting the second spunbond web is small, the fibers including the color former are easily melted as a whole, which is preferable from the viewpoint of improving the color visibility of the fused portion.

[0050] The thickness of the second spunbond web is appropriately selected depending on the application of the multilayer spunbond nonwoven fabric, and is preferably 0.1 mm to 1.0 mm, more preferably 0.2 mm to 0.5 mm. If the thickness of the second spunbond web is within the above range, the melting efficiency of the spunbond web can be increased to promote the formation of fused parts, and an appropriate thickness can be imparted to the fused parts to improve color visibility. The method for measuring the thickness of the second spunbond web is the same as that described in the Examples.

[0051] <Other layers> The multilayer spunbond nonwoven fabric may have other layers in addition to the first spunbond web, the second spunbond web, and the fused portion. The other layers may be one layer or two or more layers. The other layers may be disposed on a surface adjacent to only one of the first spunbond web and the second spunbond web. The other layers may be disposed between the first spunbond web and the second spunbond web, so long as they do not inhibit the formation of the fused portion of the first spunbond web and the second spunbond web.

[0052] Examples of the other layer include a fiber assembly, a resin sheet, and a resin film. Examples of the fiber assembly include knitted fabrics, woven fabrics, and nonwoven fabrics other than the multilayer spunbonded nonwoven fabric according to one embodiment of the present disclosure (hereinafter simply referred to as "nonwoven fabric").

[0053] Examples of the nonwoven fabric include short fiber nonwoven fabric and long fiber nonwoven fabric. "Short fibers" refer to fibers having an average fiber length of 200 mm or less. The term "long fiber" refers to the "continuous filament" as generally used in the technical field, such as in the Nonwoven Fabric Handbook (compiled by INDA, Nonwoven Fabrics Association of America, Nonwoven Fabrics Information Co., Ltd., 1996). Examples of nonwoven fabrics include spunbond nonwoven fabrics, meltblown nonwoven fabrics, wet nonwoven fabrics, dry nonwoven fabrics, dry pulp nonwoven fabrics, flash spun nonwoven fabrics, spread nonwoven fabrics, etc. The fiber assembly may be a sheet-like material made of natural fibers such as cotton. Examples of the resin film include a polyolefin film, a polyester film, and a polyamide film. These other layers may be combined and laminated to the multi-layer spunbonded nonwoven fabric, for example, a multi-layer spunbonded nonwoven fabric, a resin film, and a fiber aggregate of natural fibers such as cotton may be laminated in this order.

[0054] When the multi-layer spunbonded nonwoven fabric requires breathability, the resin film to be laminated with the multi-layer spunbonded nonwoven fabric is preferably a breathable film or a moisture-permeable film. Examples of breathable films include thermoplastic elastomer films and porous films. Examples of thermoplastic elastomer films include polyurethane elastomers, polyester elastomers, and polyamide elastomers that have moisture permeability. The porous film is made by stretching a thermoplastic resin film containing inorganic particles or organic particles to make it porous. Examples of thermoplastic resins used for the porous film include polyolefins such as high-pressure low-density polyethylene, linear low-density polyethylene (LLDPE), high-density polyethylene, polypropylene, polypropylene random copolymers, and combinations thereof. When the multilayer spunbonded nonwoven fabric does not require breathability, the resin film to be laminated with the multilayer spunbonded nonwoven fabric may be a non-porous thermoplastic resin film, etc. The material of the non-porous thermoplastic resin film may be one or more selected from polyolefins (polyethylene, polypropylene, etc.), polyesters, and polyamides.

[0055] The method of laminating (bonding) other layers to the multilayer spunbond nonwoven fabric is not particularly limited, and examples thereof include heat fusion, mechanical entanglement, a method using an adhesive, extrusion lamination, etc. Heat fusion includes heat embossing and ultrasonic fusion. Mechanical entanglement includes needle punch and water jet. Adhesives include hot melt adhesives and urethane adhesives.

[0056] <Applications of multi-layer spunbond nonwoven fabric> The multi-layer spunbond nonwoven fabric can be used for textile products. The textile products are not particularly limited, and include absorbent articles, sanitary articles, medical articles, clothing materials, packaging materials, etc. Absorbent articles include, for example, disposable diapers, sanitary products, etc. Sanitary articles include, for example, sanitary masks, etc. Medical articles include, for example, bandages, etc.

[0057] [Mixed fiber spunbond nonwoven fabric] Next, the mixed fiber spunbonded nonwoven fabric will be described. As described above, the mixed fiber spunbonded nonwoven fabric includes the first fibers and the second fibers that constitute the mixed fiber spunbonded web, and the fused portions. The first fibers constituting the mixed fiber spunbonded web are an example of a first resin molded body, and the second fibers constituting the mixed fiber spunbonded web are an example of a second resin molded body.

[0058] The mixed fiber spunbonded nonwoven fabric has a fused portion where a part of the first fibers constituting the mixed fiber spunbonded web is fused to a part of the second fibers constituting the mixed fiber spunbonded web. Therefore, the fused portion is easily visible due to its color tone even if it is not colored from the outside. As a result, the mixed fiber spunbonded nonwoven fabric has excellent designability.

[0059] <Mixed fiber spunbond web> The mixed fiber ratio of the first thermoplastic resin is appropriately selected depending on the content of the color former in the first fiber constituting the mixed fiber spunbonded web and the content of the colorant in the second fiber constituting the mixed fiber spunbonded web, etc. The mixed fiber ratio of the first thermoplastic resin is preferably 20% by mass to 80% by mass, more preferably 40% by mass to 60% by mass.

[0060] The term "mixed fiber ratio" refers to the ratio of a specific type of fiber in a nonwoven fabric layer made of a mixture of two or more types of fibers, or the mixed ratio of various fibers in the nonwoven fabric layer. That is, the "mixed fiber ratio of the first fiber" in a mixed fiber spunbonded nonwoven fabric layer made of a first fiber and a second fiber is {mass of the first fiber in the first thermoplastic resin ÷ (mass of the first fiber + mass of the second fiber)}. The "mixed fiber ratio of the second fiber" is {mass of the second fiber ÷ (mass of the first fiber + mass of the second fiber)}. The term "different mixed fiber ratios" between spunbonded nonwoven fabric layers made of a first thermoplastic resin and a second thermoplastic resin means that the mixed ratios of the first thermoplastic resin and the second thermoplastic resin in each nonwoven fabric layer are different.

[0061] The average fiber diameter of the first fibers constituting the mixed fiber spunbonded web is preferably 50 μm or less, more preferably 40 μm or less, and further preferably 30 μm or less. When the average fiber diameter of the first fibers is small, the entire fibers including the color former are easily melted, which is preferable from the viewpoint of improving the color visibility of the fused portion.

[0062] The average fiber diameter of the second fibers constituting the mixed fiber spunbonded web may be the same as the average fiber diameter of the first fibers constituting the mixed fiber spunbonded web. The average fiber diameter of the second fibers constituting the mixed fiber spunbonded web may be the same as or different from the average fiber diameter of the first fibers constituting the mixed fiber spunbonded web. When the average fiber diameter of the second fibers is small, the fibers including the color former are easily melted as a whole, which is preferable from the viewpoint of improving the color visibility of the fused portion.

[0063] It is preferable that the color former is contained in the first fiber constituting the mixed spunbond web, and the color developer is contained in the second fiber constituting the mixed spunbond web. This allows the fused portion to contain a reaction product of the color former and a reaction product of the color developer therein. As a result, the color development or discoloration of the fused portion is less likely to change due to wear of the fused portion than when the fused portion is colored from the outside using a coloring paint or the like.

[0064] The basis weight of the mixed fiber spunbonded web can be selected depending on the application of the mixed fiber spunbonded nonwoven fabric. For example, in the application of sanitary materials such as diapers, the basis weight of the mixed fiber spunbonded nonwoven fabric is preferably 200 g / m from the viewpoint of softness and breathability. 2 Less than 100 g / m 2 Less than 80 g / m, more preferably 80 g / m 2 Less than 15 g / m 2 ~60g / m 2 It is.

[0065] The thickness of the mixed fiber spunbonded web is appropriately selected depending on the application of the mixed fiber spunbonded nonwoven fabric, and is preferably 0.1 mm to 1.0 mm, more preferably 0.2 mm to 0.5 mm. When the thickness of the mixed fiber spunbonded web is within the above range, the melting efficiency of the spunbonded web can be increased to promote the formation of fused parts, and an appropriate thickness can be imparted to the fused parts to improve color visibility. The method for measuring the thickness of the mixed fiber spunbonded web is the same as that described in the Examples.

[0066] <Other layers> The mixed fiber spunbonded nonwoven fabric may have other layers in addition to the mixed fiber spunbonded web and the fused parts. The other layers may be one layer or two or more layers.

[0067] The other layers include the same layers as those exemplified as the other layers described in the multi-layer spunbonded nonwoven fabric. Examples of a method for laminating (bonding) another layer to the mixed fiber spunbonded nonwoven fabric include the same methods as those exemplified as a method for laminating (bonding) another layer to the multilayer spunbonded nonwoven fabric described in the multilayer spunbonded nonwoven fabric.

[0068] <Applications of mixed fiber spunbond nonwoven fabric> The mixed fiber spunbonded nonwoven fabric can be used for textile products. The textile products are not particularly limited, and examples thereof include absorbent articles, sanitary articles, medical articles, clothing materials, packaging materials, etc. Examples of absorbent articles include disposable diapers, sanitary products, etc. Examples of sanitary articles include sanitary masks, etc. Examples of medical articles include bandages, etc.

[0069] <Manufacturing method of multi-layer spunbond nonwoven fabric> Next, an example of a method for producing a multilayer spunbonded nonwoven fabric will be described with reference to Fig. 1. Fig. 1 is a schematic diagram showing an example of a production apparatus for a multilayer spunbonded nonwoven fabric according to an embodiment of the present disclosure.

[0070] A preferred embodiment of the method for producing a multilayer spunbonded nonwoven fabric according to the present disclosure includes a first spinning step, a first web forming step, a second spinning step, a second web forming step, a thermocompression bonding step, and a winding step. The first spinning step, the first web forming step, the second spinning step, the second web forming step, the thermocompression bonding step, and the winding step are carried out in this order.

[0071] <Multi-layer spunbond nonwoven fabric manufacturing equipment> In the method for producing a multilayer spunbonded nonwoven fabric according to an embodiment of the present disclosure, a manufacturing apparatus 100 for a multilayer spunbonded nonwoven fabric is suitably used. As shown in FIG. 1, the multilayer spunbonded nonwoven fabric manufacturing apparatus 100 includes a first spinning section 10, a first web forming section 20, a second spinning section 30, a second web forming section 40, a thermocompression bonding section 50, and a winding section 60. The first spinning section 10 has a first extruder 11, a first spinneret 12, and a first ejector 13. The first extruder 11 melt-kneads the first thermoplastic resin composition and extrudes the melt of the first thermoplastic resin composition into the first spinneret 12. The first thermoplastic resin composition represents a raw material of the first resin molded body. The first spinneret 12 melt-spins the first thermoplastic resin composition to form the first continuous fiber group 1. The first ejector 13 stretches the first continuous fiber group 1. The first web forming section 20 has a moving collecting member 21, a first suction unit 22, and a pair of first compaction rolls 23. The moving collecting member 21 has a collecting surface for depositing the first continuous fiber group 1. The first suction unit 22 is used to efficiently collect the first continuous fiber group 1 on the collecting surface of the moving collecting member 21. The first suction unit 22 is provided below the collecting surface of the moving collecting member 21. The pair of first compaction rolls 23 press the first continuous fiber group 1 to form a first spunbond web 2. The second spinning section 30 has a second extruder 31, a second spinneret 32, and a second ejector 33. The second extruder 31 melt-kneads the second thermoplastic resin composition and extrudes the melt of the second thermoplastic resin composition into the second spinneret 32. The second thermoplastic resin composition represents the raw material of the second resin molded body. The second spinneret 32 ​​melt-spins the first thermoplastic resin composition to form the second continuous fiber group 3. The second ejector 33 stretches the second continuous fiber group 3. The second web forming section 40 has a second suction unit 41 and a pair of second compaction rolls 42. The second suction unit 41 is used to efficiently collect the second continuous fiber group 3 on the surface of the first spunbond web 2. The second suction unit 41 is provided below the collection surface of the moving collection member 21. The pair of second compaction rolls 42 integrates light fibers (the first spunbond web 2 and the second continuous fiber group 3) to enable the fibers to withstand subsequent processes (for example, heat bonding by an embossing roll 51, etc.). Specifically, the pair of second compaction rolls 42 presses the first spunbond web 2 and the second continuous fiber group 3 to form a laminated web 4. The laminated web 4 has a first spunbond web 2 and a second spunbond web. The first spunbond web 2 is laminated on one main surface of the second spunbond web. The thermocompression bonding unit 50 has an embossing roll 51 and a smooth roll 52. The embossing roll 51 and the smooth roll 52 thermocompress the laminated web 4. The embossing roll 51 is a metal roll with an engraved roll surface. The smooth roll 52 is a metal roll with a smooth roll surface. The winding section 60 has a winder 61. The winder 61 winds up the multilayer spunbond nonwoven fabric 5.

[0072] <First spinning process> In the first spinning step, the first thermoplastic resin composition is melt spun to form the first continuous fiber group 1. The first spinning step includes a known process of cooling and stretching the first continuous fiber group 1 before depositing the first continuous fiber group 1 on the collecting surface of the moving collecting member.

[0073] Specifically, the first thermoplastic resin composition is fed into a first extruder 11, and the melt of the first thermoplastic resin is extruded into a first spinneret 12. At this time, the heating temperature of the first extruder 11 is appropriately adjusted depending on the melting point of the first thermoplastic resin composition, and is preferably 200° C. to 250° C. The pressure when the melt of the first thermoplastic resin composition is extruded from the first extruder 11 is preferably 20 MPa to 80 MPa. Next, the first thermoplastic resin composition is melt spun by a first spinneret 12 to form a first continuous fiber group 1. The first continuous fiber group 1 is cooled by cooling air 14 and stretched by a first ejector 13. The temperature of the cooling air 14 is preferably 5° C. to 50° C. The wind speed of the cooling air 14 is preferably 100 m / min to 10,000 m / min.

[0074] <First web forming process> In the first web forming step, a first group of continuous fibers 1 is deposited on the collecting surface of a moving collecting member 21 to form a first spunbond web 2.

[0075] Specifically, the drawn first continuous fiber group 1 is efficiently collected on the collecting surface of the moving collecting member 21 by the first suction unit 22. The collected first continuous fiber group 1 is sandwiched between a pair of first compaction rolls 23, and a first spunbond web 2 is formed. The temperature of the pair of first compaction rolls 23 when pressing the first continuous fiber group 1 is preferably 100° C. to 120° C. The temperature of the compaction rolls when pressing the first continuous fiber group 1 is preferably lower than the melting point of the first thermoplastic resin.

[0076] <Second spinning process> In the second spinning step, the second thermoplastic resin composition is melt spun to form the second continuous fiber group 3. Similarly, the second spinning step also includes a known process of cooling and stretching the second continuous fiber group 3 before depositing the second continuous fiber group 3 on the first spunbond web 2.

[0077] Specifically, the second thermoplastic resin is fed into the second extruder 31, and the melt of the second thermoplastic resin is extruded. At this time, the heating temperature of the second extruder 31 is appropriately adjusted according to the melting point of the second thermoplastic resin, etc., and is preferably 200° C. to 250° C. The pressure when the melt of the second thermoplastic resin is extruded from the second extruder 31 is preferably 20 MPa to 80 MPa. Next, the second thermoplastic resin is melt-spun from a second spinneret 32 ​​to form a second continuous fiber group 3. The second continuous fiber group 3 is cooled by cooling air 34 and stretched by a second ejector 33. The temperature of the cooling air 34 is preferably 5° C. to 50° C. The wind speed of the cooling air 34 is preferably 100 m / min to 10,000 m / min.

[0078] <Second web forming process> In the second web forming step, a second continuous fiber group 3 is deposited on the first spunbond web 2 to form a second spunbond web, thereby forming a laminated web 4.

[0079] Specifically, the stretched second continuous fiber group 3 is efficiently collected on the first spunbond web 2 by the second suction unit 41. The collected second continuous fiber group 3 is sandwiched between a pair of second compaction rolls 42, and the laminated web 4 is formed. The temperature of the pair of second compaction rolls 42 when pressing the second continuous fiber group 3 is preferably 100° C. to 120° C. The temperature of the compaction rolls when pressing the second continuous fiber group 3 is preferably lower than the melting points of the first thermoplastic resin and the second thermoplastic resin.

[0080] <Thermocompression bonding process> In the thermocompression bonding step, the laminated web 4 is thermocompression bonded, thereby obtaining a multi-layered spunbonded nonwoven fabric 5. In other words, fused portions are formed in the laminated web 4.

[0081] Specifically, the laminated web 4 is sandwiched between an embossing roll 51 and a smooth roll 52 to form a multi-layer spunbond nonwoven fabric 5 . When pressing the laminated web 4, the surface temperatures of the embossing roll 51 and the smoothing roll 52 are preferably 140°C to 150°C. The pressure applied when pressing the laminated web 4 is preferably 700 MPa to 1200 MPa.

[0082] <Winding process> In the winding step, the multilayer spunbond nonwoven fabric 5 is wound and collected.

[0083] Specifically, the multi-layer spunbond nonwoven fabric 5 is wound up by a winder 61 .

[0084] (Method of manufacturing mixed fiber spunbond) Next, an example of a method for producing a mixed fiber spunbonded nonwoven fabric will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of a production apparatus for a mixed fiber spunbonded nonwoven fabric according to an embodiment of the present disclosure.

[0085] The method for producing a mixed fiber spunbonded nonwoven fabric according to an embodiment of the present disclosure includes a mixed fiber spinning step, a mixed fiber web forming step, a thermocompression bonding step, and a winding step. The mixed fiber spinning step, the mixed fiber web forming step, the thermocompression bonding step, and the winding step are carried out in this order.

[0086] <Mixed fiber spunbond nonwoven fabric manufacturing equipment> In the manufacturing method of the mixed fiber spunbonded nonwoven fabric according to the embodiment of the present disclosure, a manufacturing apparatus 200 for mixed fiber spunbonded nonwoven fabric is suitably used. As shown in FIG. 2, the manufacturing apparatus 200 for the mixed fiber multi-layer spunbonded nonwoven fabric includes a mixed fiber spinning unit 10A, a mixed fiber web forming unit 20A, a thermocompression bonding unit 50, and a winding unit 60. The mixed fiber spinning section 10A has a first extruder 11, a second extruder 15, a third spinneret 16, and a first ejector 13. The first extruder 11 melts and kneads the first thermoplastic resin composition, and extrudes the melt of the first thermoplastic resin composition into the third spinneret 16. The second extruder 15 melts and kneads the second thermoplastic resin composition, and extrudes the melt of the second thermoplastic resin composition into the third spinneret 16. The third spinneret 16 has a large number of spinning holes (nozzles) for each of the first thermoplastic resin composition and the second thermoplastic resin composition. The third spinneret 16 independently and simultaneously extrudes the first thermoplastic resin composition and the second thermoplastic resin composition from different spinning holes to form a third continuous fiber group 6. The first ejector 13 stretches the third continuous fiber group 6. The mixed fiber web forming section 20A has a moving collecting member 21, a first suction unit 22, and a pair of first compaction rolls .

[0087] <Mixed fiber spinning process> In the mixed fiber spinning process, the first thermoplastic resin composition and the second thermoplastic resin composition are each melt spun to form the third continuous fiber group 6. The mixed fiber spinning process includes a known process of cooling and stretching the third continuous fiber group 6 before depositing the third continuous fiber group 6 on the collecting surface of the moving collecting member 21.

[0088] Specifically, a first thermoplastic resin composition is fed into a first extruder 11, and a melt of the first thermoplastic resin composition is extruded into a third spinneret 16. At the same time, a second thermoplastic resin composition is fed into a third extruder 15, and a melt of the second thermoplastic resin composition is extruded into the third spinneret 16. In this case, the heating temperature and pressure of each of the first extruder 11 and the third extruder 15 may be the same as the heating temperature and pressure exemplified in the above-mentioned first spinning step. Next, each of the first thermoplastic resin composition and the second thermoplastic resin composition is melt spun from a third spinneret 16 to form a third continuous fiber group 6. The third continuous fiber group 6 is cooled by cooling air 14 and stretched by a first ejector 13.

[0089] <Mixed fiber web forming process> In the mixed fiber web forming process, the third continuous fiber group 6 is deposited on the collecting surface of the moving collecting member 21 to form a mixed fiber spunbonded web 7.

[0090] The mixed fiber web forming step can be carried out in the same manner as the first web forming step described above.

[0091] <Thermocompression bonding process> In the heat-bonding step, the mixed fiber spunbonded web 7 is heat-bonded. This results in a mixed fiber spunbonded nonwoven fabric 8. In other words, fused parts are formed in the mixed fiber spunbonded web 7.

[0092] The thermocompression bonding step is carried out in the same manner as the thermocompression bonding step of the above-mentioned multi-layer spunbonded nonwoven fabric manufacturing apparatus.

[0093] <Winding process> In the winding step, the mixed fiber spunbonded nonwoven fabric 8 is wound and recovered.

[0094] The winding step is carried out in the same manner as the winding step of the above-mentioned multi-layer spunbonded nonwoven fabric manufacturing apparatus. EXAMPLES

[0095] Hereinafter, the composite resin molded body of the present disclosure will be described with reference to examples, but the composite resin molded body of the present disclosure is not limited to the following embodiments in any way.

[0096] The physical properties and the like in the examples and comparative examples were measured by the following methods.

[0097] (1) Weight [g / m 2 〕 Ten test pieces measuring 100 mm (machine direction: MD) x 100 mm (direction perpendicular to machine direction: CD) were taken from the nonwoven fabrics obtained in the Examples and Comparative Examples. The test pieces were taken from 10 locations in the CD direction. Next, the mass [g] of each test piece was measured using a top-pan electronic balance (manufactured by Kensei Kogyo Co., Ltd.) in an environment of 20°C and a relative humidity of 50%. The average mass of each test piece was calculated. A 1m difference was calculated from the calculated average. 2 The weight per unit area of ​​each nonwoven fabric sample was calculated by converting the weight per unit area into mass [g] and rounding off to the nearest tenth. 2 〕.

[0098] (2) Thickness [mm] Ten test pieces of 100 mm (MD) x 100 mm (CD) were taken from the nonwoven fabrics obtained in the Examples and Comparative Examples. The test pieces were taken from the same locations as the test pieces for measuring the basis weight. Then, the thickness [mm] of each test piece was measured using a load-type thickness meter (manufactured by Ozaki Manufacturing Co., Ltd.) according to the method described in JIS L 1096:2010. The average thickness of each test piece was calculated and rounded off to one decimal place to obtain the thickness [mm] of each nonwoven fabric sample.

[0099] (3) Color difference [-] The L of reflected light in the non-fused and fused parts was measured using a spectrophotometer "CM-3700A" manufactured by Konica Minolta Inc. (SCE method, viewing angle 2 degrees, light source: CIE D65). * Value, a * value, and b * The value was measured, and the color difference before and after fusing was calculated using the color difference formula in the CIELab color space specified in JIS-P8150.

[0100] (4) Abrasion test [-] A friction test was conducted on the fused part of the laminated web using a Gakushin-type friction fastness tester (New model NR-100, manufactured by Daiei Scientific Instruments Co., Ltd.) in accordance with the friction fastness test method of JIS L 0849. In detail, a cloth tape (No. 1532, manufactured by Teraoka Seisakusho Co., Ltd.) was attached to the friction element side, and the fused part was rubbed back and forth 50 times in the MD direction with a load of 300g applied, and the abrasion resistance of the blue color of the fused part was evaluated according to the following criteria. Evaluation A: No damage to the blue color of the fused portion was observed. Rating B: Blue damage was observed in the fused area.

[0101] The components used in the examples and comparative examples are as follows. <Thermoplastic resin> Propylene homopolymer (MFR: 60g / 10min, melting point: 162℃) <Color former> Blue leuco dye: "Blue-63" (3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methyl-3-indolyl)-4-azaphthalide) manufactured by Yamamoto Chemical Industry Co., Ltd. Red leuco dye: "Red-40" (3,3-bis(1-n-butyl-2-methylindol-3-yl)phthalide) manufactured by Yamamoto Chemical Industry Co., Ltd. <Color developer> First coloring agent: Bisphenol S (melting point: 247°C, acid dissociation constant: 4.5) Second coloring agent: 4-isopropoxyphenyl-4-hydroxyphenyl sulfone (melting point 129°C, acid dissociation constant: 4.5) Third coloring agent: stearic acid (melting point 70°C, acid dissociation constant: 5.0)

[0102] Comparative Example 1 Propylene homopolymer (100 parts) and blue leuco dye (1 part) were mixed together to obtain a first feedstock. The first raw material was molded at 190° C. with a press film forming machine to obtain a first resin sheet having a thickness of 100 μm. When the first resin sheet was visually observed, the color tone of the first resin sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting of only a propylene homopolymer. A part of the first resin sheet was sandwiched in a batch type sealer and heat-pressurized to form a fused portion. The batch type sealer includes a pair of metal plates. The surface temperature of each of the pair of metal plates was 190° C. The pressure applied to the first resin sheet was 3 MPa. When the fused and non-fused parts of the first resin sheet were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0103] Comparative Example 2 A second resin sheet having a thickness of 100 μm was obtained in the same manner as in Comparative Example 1, except that a second raw material obtained by mixing a propylene homopolymer (100 parts) and a red leuco dye (1 part) was used instead of the first raw material. When the second resin sheet was visually observed, the color tone of the second resin sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting of only a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the second resin sheet. When the fused and non-fused parts of the second resin sheet were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0104] Comparative Example 3 A third resin sheet having a thickness of 100 μm was obtained in the same manner as in Comparative Example 1, except that a third raw material consisting of a mixture of propylene homopolymer (100 parts) and a first color developer (2 parts) was used instead of the first raw material. When the third resin sheet was visually observed, the color tone of the third resin sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting of only a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the third resin sheet. When the fused and non-fused parts of the third resin sheet were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0105] Comparative Example 4 A fourth resin sheet having a thickness of 100 μm was obtained in the same manner as in Comparative Example 1, except that a fourth raw material consisting of a mixture of propylene homopolymer (100 parts) and a second colorant (2 parts) was used instead of the first raw material. When the fourth resin sheet was visually observed, the color tone of the fourth resin sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting of only a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the fourth resin sheet. When the fused and non-fused parts of the fourth resin sheet were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0106] Comparative Example 5 A fifth resin sheet having a thickness of 100 μm was obtained in the same manner as in Comparative Example 1, except that a fifth raw material was used by mixing propylene homopolymer (100 parts) and a third colorant (2 parts) instead of the first raw material. When the fifth resin sheet was visually observed, the color tone of the fifth resin sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting of only a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the fifth resin sheet. When the fused and non-fused parts of the fifth resin sheet were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0107] Comparative Example 6 A sixth resin sheet having a thickness of 100 μm was obtained in the same manner as in Comparative Example 1, except that a sixth raw material consisting of a mixture of propylene homopolymer (100 parts), blue leuco dye (1 part), and a second colorant (2 parts) was used instead of the first raw material. When the sixth resin sheet was visually observed, the color tone of the sixth resin sheet was different from the color tone (colorless and transparent) of the transparent resin sheet consisting of only a propylene homopolymer, and the resin sheet was entirely blue. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the sixth resin sheet. When the fused and non-fused parts of the sixth resin sheet were visually observed, the color tone of the fused parts was blue, similar to the color tone (blue) of the non-fused parts.

[0108] Example 1 A first resin sheet containing a blue leuco dye was obtained in the same manner as in Comparative Example 1. A third resin sheet containing a first color developer was obtained in the same manner as in Comparative Example 3. The first resin sheet and the third resin sheet were superimposed to obtain a first laminate sheet. When the first laminate sheet was visually observed, the color tone of the first laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the first laminate sheet to obtain a first composite resin molding. When the fused and non-fused portions of the first composite resin molding were visually observed, the color tone of the fused portions was blue, which was different from the color tone (colorless and transparent) of the non-fused portions.

[0109] Example 2 A first resin sheet containing a blue leuco dye was obtained in the same manner as in Comparative Example 1. A fourth resin sheet containing a second color developer was obtained in the same manner as in Comparative Example 4. The first resin sheet and the fourth resin sheet were superimposed to obtain a second laminate sheet. When the second laminate sheet was visually observed, the color tone of the second laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the second laminate sheet to obtain a second composite resin molding. When the fused and non-fused portions of the second composite resin molding were visually observed, the color tone of the fused portions was dark blue, which was different from the color tone (colorless and transparent) of the non-fused portions. The color tone of the fused portion of the second composite resin molding was darker than the color tone of the fused portion of the first composite resin molding.

[0110] Example 3 A first resin sheet containing a blue leuco dye was obtained in the same manner as in Comparative Example 1. A fifth resin sheet containing a third color developer was obtained in the same manner as in Comparative Example 5. The first resin sheet and the fifth resin sheet were superimposed to obtain a third laminated sheet. When the third laminate sheet was visually observed, the color tone of the third laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the third laminate sheet to obtain a third composite resin molding. When the fused and non-fused portions of the third composite resin molding were visually observed, the color tone of the fused portions was pale blue, different from the color tone (colorless and transparent) of the non-fused portions. The color tone of the fused portion of the third composite resin molding was lighter than the color tone of the fused portion of the first composite resin molding.

[0111] Example 4 A second resin sheet containing a red leuco dye was obtained in the same manner as in Comparative Example 2. A third resin sheet containing a first color developer was obtained in the same manner as in Comparative Example 3. The second resin sheet and the third resin sheet were superimposed to obtain a fourth laminate sheet. When the fourth laminate sheet was visually observed, the color tone of the fourth laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the fourth laminate sheet to obtain a fourth composite resin molding. When the fused and non-fused portions of the fourth composite resin molding were visually observed, the color tone of the fused portions was red, which was different from the color tone (colorless and transparent) of the non-fused portions.

[0112] Example 5 A second resin sheet containing a red leuco dye was obtained in the same manner as in Comparative Example 2. A fourth resin sheet containing a second color developer was obtained in the same manner as in Comparative Example 4. The second resin sheet and the fourth resin sheet were superimposed to obtain a fifth laminate sheet. When the fifth laminate sheet was visually observed, the color tone of the fifth laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the fifth laminate sheet to obtain a fifth composite resin molding. When the fused and non-fused portions of the fifth composite resin molding were visually observed, the color tone of the fused portions was deep red, different from the color tone (colorless and transparent) of the non-fused portions. The color tone of the fused portion of the fifth composite resin molding was darker than the color tone of the fused portion of the fourth composite resin molding.

[0113] Example 6 A second resin sheet containing a red leuco dye was obtained in the same manner as in Comparative Example 2. A fifth resin sheet containing a third color developer was obtained in the same manner as in Comparative Example 5. The second resin sheet and the fifth resin sheet were superimposed to obtain a sixth laminate sheet. When the sixth laminate sheet was visually observed, the color tone of the sixth laminate sheet was colorless and transparent, similar to the color tone of the transparent resin sheet consisting only of a propylene homopolymer. In the same manner as in Comparative Example 1, a fused portion was formed in a part of the sixth laminate sheet to obtain a sixth composite resin molding. When the fused and non-fused portions of the sixth composite resin molding were visually observed, the color tone of the fused portions was pale red, different from the color tone (colorless and transparent) of the non-fused portions. The color tone of the fused portion of the sixth composite resin molding was lighter than the color tone of the fused portion of the fourth composite resin molding.

[0114] Example 7 In the same manner as in Example 1, a first laminate sheet was obtained. A part of the first laminate sheet was sandwiched in a roll-type press machine to form a fused portion, and a seventh composite resin molded body was obtained. The roll-type press machine was equipped with an engraved roll and a smooth roll. The engraved roll was a metal roll with an engraving on the roll surface. The smooth roll was a metal roll with a smooth roll surface. The surface temperatures of the engraved roll and the smooth roll were each 190°C. The pressure applied to the first laminate sheet was 700 MPa. When the fused and non-fused parts of the seventh composite resin molding were visually observed, the color tone of the fused parts was blue, which was different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the seventh composite resin molding where the engraving of the engraved roll was transferred (fused part) was blue.

[0115] Example 8 In the same manner as in Example 2, a second laminate sheet was obtained. In the same manner as in Example 7, a fused portion was formed in a part of the second laminate sheet to obtain an eighth composite resin molding. When the fused and non-fused parts of the eighth composite resin molding were visually observed, the color tone of the fused parts was dark blue, different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the eighth composite resin molding where the engraving of the engraved roll was transferred (fused part) was dark blue. The color tone of the fused portion of the eighth composite resin molding was darker than the color tone of the fused portion of the seventh composite resin molding.

[0116] Example 9 In the same manner as in Example 3, a third laminate sheet was obtained. In the same manner as in Example 7, a fusion-bonded portion was formed in a part of the third laminate sheet to obtain a ninth composite resin molding. When the fused and non-fused parts of the ninth composite resin molding were visually observed, the color tone of the fused parts was pale blue, different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the ninth composite resin molding where the engraving of the engraved roll was transferred (fused parts) was pale blue. The color tone of the fused portion of the ninth composite resin molding was lighter than the color tone of the fused portion of the seventh composite resin molding.

[0117] Example 10 In the same manner as in Example 4, a fourth laminate sheet was obtained. In the same manner as in Example 7, a fused portion was formed in a part of the fourth laminate sheet to obtain a tenth composite resin molding. When the fused and non-fused parts of the tenth composite resin molding were visually observed, the color tone of the fused parts was red, which was different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the tenth composite resin molding where the engraving of the engraved roll was transferred (fused part) was red.

[0118] Example 11 In the same manner as in Example 5, a fifth laminate sheet was obtained. In the same manner as in Example 7, a fused portion was formed in a part of the fifth laminate sheet to obtain an eleventh composite resin molding. When the fused and non-fused parts of the eleventh composite resin molding were visually observed, the color tone of the fused parts was dark red, different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the eleventh composite resin molding where the engraving of the engraved roll was transferred (fused parts) was dark red. The color tone of the fused portion of the eleventh composite resin molding was darker than the color tone of the fused portion of the tenth composite resin molding.

[0119] Example 12 In the same manner as in Example 6, a sixth laminate sheet was obtained. In the same manner as in Example 7, a fused portion was formed in a part of the sixth laminate sheet to obtain a twelfth composite resin molding. When the fused and non-fused parts of the 12th composite resin molding were visually observed, the color tone of the fused parts was pale red, which was different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the 12th composite resin molding where the engraving of the engraved roll was transferred (fused part) was pale red. The color tone of the fused portion of the twelfth composite resin molding was lighter than the color tone of the fused portion of the tenth composite resin molding.

[0120] Comparative Example 7 The first raw material was obtained in the same manner as in Comparative Example 1. The first raw material was melt-kneaded at 200°C and spun by a spunbond method. The resulting fibers were deposited on a collecting surface to obtain a first web. The basis weight of the first web was 10 g / m 2 The average fiber diameter of the fibers constituting the first web was 19 μm. When the first web was visually observed, the color tone of the first web was colorless and transparent, similar to the color tone of the nonwoven fabric made only of a propylene homopolymer. A part of the first web was sandwiched between an embossing roll device to form a fused portion. The embossing roll device includes an embossing roll 51 and a smooth roll 52. The surface temperatures of the embossing roll 51 and the smooth roll 52 were each 130°C. The pressure applied to the first web was 700 MPa. The engraving area ratio of the embossing roll 51 was 10%. The engraving area ratio of the embossing roll 51 indicates the ratio of the area of ​​the engraved portion (convex portion) to the total area of ​​the roll surface of the embossing roll 51. When the fused and non-fused parts of the first web were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0121] Comparative Example 8 The fourth raw material was obtained in the same manner as in Comparative Example 4. A second web was obtained in the same manner as in Comparative Example 7, except that the fourth raw material was used instead of the first raw material. When the second web was visually observed, the color tone of the second web was colorless and transparent, similar to the color tone of the nonwoven fabric consisting of only a propylene homopolymer. In the same manner as in Comparative Example 7, a fused portion was formed in the second web. When the fused and non-fused parts of the second web were visually observed, the color tone of the fused parts was colorless and transparent, similar to the color tone (colorless and transparent) of the non-fused parts.

[0122] Comparative Example 9 A seventh raw material was obtained by combining propylene homopolymer (100 parts), blue leuco dye (1 part), and a second color developer (1 part). A third web was obtained in the same manner as in Comparative Example 7, except that the seventh raw material was used instead of the first raw material. When the third web was visually observed, the color tone of the third web was different from the color tone of the nonwoven fabric made of only a propylene homopolymer, and the third web was entirely blue. In the same manner as in Comparative Example 7, a fused portion was formed in the third web. When the fused and non-fused parts of the third web were visually observed, the color tone of the fused parts was blue, similar to the color tone (blue) of the non-fused parts.

[0123] <Example 13> A first web was obtained in the same manner as in Comparative Example 7. A second web was obtained in the same manner as in Comparative Example 8. The first web and the second web were overlapped to obtain a web laminate. The total basis weight of the web laminate was 20 g / m 2 It was. In the same manner as in Comparative Example 7, a fused portion was formed in a part of the web laminate to obtain a thirteenth composite resin molding. When the fused and non-fused parts of the 13th composite resin molding were visually observed, the color tone of the fused parts was blue, which was different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the part of the 13th composite resin molding where the engraving of the embossing roll 51 was transferred (fused part) was blue.

[0124] <Example 14> The first raw material was obtained in the same manner as in Comparative Example 1. The propylene homopolymer (100 parts) and the second color developer (1 part) were mixed to obtain the eighth raw material. As shown in FIG. 8, the first raw material was fed into the first extruder 11, and the eighth raw material was fed into the third extruder 15, and they were melt-kneaded separately at 200°C. Using a spunbond nonwoven fabric molding machine having a third spinneret 16, melt spinning was performed by the spunbond method under the conditions of a resin temperature and a die temperature of the third spinneret 16 of 200°C, a cooling air temperature of 25°C, and a drawing air speed of 3500 m / min, and a third continuous fiber group 6 consisting of mixed long fibers was deposited on the collecting surface of a moving collecting member 21 to obtain a mixed fiber spunbond web 7. The mixed fiber spunbond web 7 is composed of a mixed fiber of color-developing fiber:color-exchangeable fiber in a ratio of 40:60 (mass%). The mixed fiber spunbond web 7 has a basis weight of 20 g / m 2 It was. The third spinneret 16 had a nozzle pattern in which the nozzle holes for the first raw material and the nozzle holes for the eighth raw material were alternately arranged. The nozzle diameter was 0.60 mmφ, and the ratio of the number of nozzles was 40:60 (nozzles for fibers made from the first raw material:nozzles for fibers made from the sixth raw material). When the mixed fiber spunbonded web 7 was visually observed, the color tone of the mixed fiber spunbonded web 7 was colorless, similar to the color tone of the fiber consisting of only propylene homopolymer. Next, in the same manner as in Comparative Example 7, a fused portion was formed in a part of the mixed fiber spunbonded web 7 to obtain a fourteenth composite resin molding. When the fused and non-fused parts of the fourteenth composite resin molding were visually observed, the color tone of the fused parts was blue, which was different from the color tone (colorless and transparent) of the non-fused parts. In other words, only the parts of the fourteenth composite resin molding where the engraving of the embossing roll 51 was transferred (fused parts) were blue.

[0125] Tables 1 and 2 show the visual color tones of the fused and non-fused parts in Examples 1 to 14 and Comparative Examples 1 to 9.

[0126] <Example 15> A laminated sheet in which a sheet containing a blue leuco dye and a sheet containing a color developer were overlapped was obtained in the same manner as in Example 2. A fused portion was formed in a part of the third laminated sheet in the same manner as in Comparative Example 1 to form a belt-like fused portion having a width of 10 mm.

[0127] <Example 16> In the same manner as in Example 13, a web containing a blue leuco dye and a web containing a color developer were overlapped to prepare a web having a total basis weight of 20 g / m 2 In the same manner as in Comparative Example 7, a fused portion was formed in a part of the web laminate to form a belt-like fused portion having a width of 10 mm.

[0128] The color tone of the fused portion and the color difference of the non-fused portion in Examples 15 and 16 are shown in Table 3.

[0129] <Example 17> In the same manner as in Example 16, a web laminate having fused portions formed therein was obtained.

[0130] <Comparative Example 10> A propylene homopolymer having a basis weight of 10 g / m was prepared in the same manner as in Comparative Example 7, except that only a propylene homopolymer was used as the raw material instead of the first raw material. 2 The fourth web was then stacked twice to obtain a total weight of 20 g / m 2 Thus, a web laminate of 1000 mm was obtained. A part of this web laminate was sandwiched in a batch sealer, and the laminated fourth webs were heat-pressed together to form a 10 mm-wide band-shaped fused portion. The surface temperature of each of the pair of metal plates of the batch sealer was 190° C. The pressure applied to the laminated web was 3 MPa. A blue oil-based paint was applied to the fused portion of the web laminate having the fused portion formed therein and dried so as to have the same color tone as the fused portion of Example 17. As a result, a blue coating film was formed on the fused portion.

[0131] An abrasion test was carried out for Example 17 and Comparative Example 10. The evaluation results of the abrasion test are shown in Table 4.

[0132] [Table 1]

[0133] [Table 2]

[0134] [Table 3]

[0135] [Table 4]

[0136] The composite resin molded body of Examples 1 to 14 includes a first resin molded body, a second resin molded body, and a fused portion. The first resin molded body contains a propylene homopolymer as a main component, a leuco dye, and does not contain a coloring agent. The second resin molded body contains a propylene homopolymer as a main component, a coloring agent, and does not contain a leuco dye. The fused portion is formed by fusing a part of the first resin molded body with a part of the second resin molded body. Therefore, the color tone of the fused portion was different from the color tone of the non-fused portion. As a result, it was found that in the composite resin molded bodies of Examples 1 to 14, the fused portion was easily visible due to its color tone even if it was not colored from the outside.

[0137] The melting point of the first coloring agent was higher than the fusion temperature. The melting point of the second coloring agent was lower than the fusion temperature. The fusion parts of the composite resin moldings of Examples 2, 5, 8, and 11, which contain the second coloring agent, were more strongly colored than the fusion parts of the composite resin moldings of Examples 1, 4, 7, and 10, which contain the first coloring agent. This shows that the fusion parts of the composite resin moldings can be more strongly colored by using a coloring agent whose melting point is lower than the fusion temperature.

[0138] The acidity of the first colorant was higher than that of the third colorant. The melting point of the first colorant was higher than the fusion temperature. The melting point of the third colorant was lower than the fusion temperature. The fusion parts of the composite resin molded bodies of Examples 1, 4, 7, and 10 containing the first colorant were more strongly colored than the fusion parts of the composite resin molded bodies of Examples 3, 6, 9, and 12 containing the third colorant. This shows that even if a colorant has a melting point lower than the heat fusion temperature, if the colorant has high acidity, the fusion parts can be more strongly colored than when a colorant with low acidity is used.

[0139] On the other hand, the resin sheets of Comparative Examples 1 to 6 and the webs of Comparative Examples 7 to 9 did not have either the first resin molding or the second resin molding. Therefore, the color tone of the fused portion was the same as the color tone of the non-fused portion. It was found that in the resin sheets of Comparative Examples 1 to 6 and the webs of Comparative Examples 7 to 9, the fused portion was not easily visible due to its color tone even if it was not colored from the outside.

[0140] The composite resin molding of Example 15 has a laminated sheet form. The composite molding of Example 16 is the same as that of Example 15, except that it has a multi-layer spunbonded nonwoven fabric form. Comparing Example 15 and Example 16, the color difference (ΔE) of the multilayer spunbonded nonwoven fabric of Example 16 was 23.37, while the color difference (ΔE) of the laminated sheet of Example 15 was 5.85. This result shows that the multilayer spunbonded nonwoven fabric of Example 16 had an improved visual contrast between the non-fused and fused parts compared to the laminated sheet of Example 15. L before and after fusion of the multi-layer spunbonded nonwoven fabric of Example 16 * The change in value of L * The change in the L value was larger than that of the non-fused portion of the spunbonded nonwoven fabric. This is presumably due to the fact that the non-fused portion of the spunbonded nonwoven fabric is made of fibers. In more detail, since fibers tend to scatter visible light, the change in the L value of the non-fused portion of the fiber * The value is relatively large. As a result, the L *The value is the L value of the fused part where the resin melts and becomes a film. * It is expected that the difference will become larger. Example 16 multilayer spunbond nonwoven fabric before and after fusion b * The change in value of b before and after fusing of the laminated sheet of Example 15 * The main reason for this is presumably that in Example 16, the first resin molded body containing a color former and the second resin molded body containing a color former are both in the form of fibers, and therefore melting and mixing easily occurs during fusion.

[0141] The disclosure of Japanese Patent Application No. 2021-051587, filed on March 25, 2021, is incorporated by reference in its entirety into this specification. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.

Claims

1. a first resin molded body containing a first thermoplastic resin and a color former; A second resin molded body containing a second thermoplastic resin and a color developer that promotes color development or color change of the color developer; a fused portion in which a portion of the first resin molded body and a portion of the second resin molded body are fused to each other, the fused portion indicates a portion where the first thermoplastic resin contained in the first resin molded body and the second thermoplastic resin contained in the second resin molded body are mixed with each other, the fused portion contains, at least inside thereof, a color-developing compound formed by the color-developing agent reacting with the color-developing agent to develop or change color, the first resin molding is a first spunbond web containing first fibers, the second resin molding is a second spunbond web containing second fibers; The first spunbond web is laminated on one major surface of the second spunbond web, the first fibers include the first thermoplastic resin; The second fibers include the second thermoplastic resin.

2. A first resin molded body containing a first thermoplastic resin and a color former; A second resin molded body containing a second thermoplastic resin and a color developer that promotes color development or color change of the color developer; a fused portion in which a portion of the first resin molded body and a portion of the second resin molded body are fused to each other, the fused portion indicates a portion where the first thermoplastic resin contained in the first resin molded body and the second thermoplastic resin contained in the second resin molded body are mixed with each other, the fused portion contains, at least inside thereof, a color-forming compound formed by the color-forming agent reacting with the color-developing agent to develop or change color; the first resin molding is a first fiber, the second resin molding is a second fiber, The first fibers and the second fibers constitute a mixed fiber spunbonded web.

3. The first resin molded body does not contain the color developer, The composite resin molding according to claim 1 or 2, wherein the second resin molding does not contain the color former.

4. The color former is contained within the first fiber, The composite resin molding according to any one of claims 1 to 3, wherein the color developer is contained within the second fibers.

5. The composite resin molding according to any one of claims 1 to 4, wherein the fused portion contains, at least inside thereof, a color-developing compound of the color former and the color developer.

6. The composite resin molding according to any one of claims 1 to 5, wherein the color former includes a leuco dye.

Citation Information

Patent Citations

  • Thermally color-changing nonwoven fabric

    JP1996027653A

  • Plastic card and production thereof

    JP1997011622A

  • Laminates containing absorbent articles and bonding patterns

    JP2009507556A

  • Method for manufacturing high-pressure tank

    JP2013119924A

  • Meltspun thermochromic fabrics

    US20030087566A1