Semiconductor device and its manufacturing method

The semiconductor device with trench-based gettering elements addresses the limitations of conventional gettering methods by enhancing gettering efficiency through thermal expansion and ion implantation, effectively trapping heavy metals and expanding the region for semiconductor element formation.

JP7583507B2Active Publication Date: 2024-11-14NISSHINBO MICRO DEVICES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020072076
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-14
Publication Date
2024-11-14
Estimated Expiration
2040-04-14

AI Technical Summary

Technical Problem

Conventional gettering methods, such as intrinsic and extrinsic gettering, face limitations in forming sufficient gettering sites due to density constraints and loss of gettering effect from annealing processes, leading to inadequate immobilization of heavy metal impurities in semiconductor devices.

Method used

A semiconductor device with a gettering element featuring first and second trench portions of differing depths, filled with insulating material and stress relaxation portions, is designed to enhance gettering efficiency by creating gettering regions on the semiconductor surface, utilizing thermal expansion and ion implantation to trap heavy metals.

Benefits of technology

The solution improves gettering efficiency by forming gettering sites that can trap heavy metals like iron, thickening the region for semiconductor element formation, and maintaining the gettering effect without affecting the semiconductor elements, while being compatible with standard manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583507000001
    Figure 0007583507000001
  • Figure 0007583507000002
    Figure 0007583507000002
  • Figure 0007583507000003
    Figure 0007583507000003
Patent Text Reader

Abstract

To provide a semiconductor device that comprises a gettering element on a surface in a semiconductor region where a semiconductor element is to be formed, and to provide a method of manufacturing the same.SOLUTION: In a gettering element 2, a first trench 4 having a first depth and a second trench 5 having a second depth deeper than the first depth are opposedly arranged on a surface in a semiconductor region 3. The first trench 4 is filled with an insulation material (a silicon oxide 6). The second trench 5 has an inner surface coated with the insulation material, and the coated inner surface serves as a stress alleviation part (polysilicon). Heat treatment on the semiconductor region 3 having such a structure causes defects generated from the vicinity of the first trench 4, which turn into a gettering site for forming a gettering region 8.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device having a gettering element and a method for manufacturing the same. [Background technology]

[0002] Heavy metal impurities mixed into a semiconductor region generate noise and leakage current, so it is necessary to immobilize the heavy metal impurities by forming a gettering site in the semiconductor region. Known methods for gettering heavy metal impurities include the intrinsic gettering method (IG method) in which oxygen is precipitated inside a silicon substrate and the oxygen precipitates (bulk micro defects: BMD) are used as gettering sites, and the extrinsic gettering method (EG method) in which mechanical distortion is applied to the back surface of a silicon substrate using a sandblasting method or the like, or a polycrystalline silicon film or the like is formed to use the gettering site (e.g., Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 3-84931 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when the density of BMD is increased, the region (DZ layer: Denuded Zone) where semiconductor elements can be formed becomes narrow, so there is a limit to the density of BMD that can be formed. In addition, when a process for annealing and eliminating micro defects such as COPs (crystal originated defects) on the silicon surface is performed using a reducing gas, mechanical distortion formed on the back surface of a silicon substrate using a sandblasting method or the like is eliminated, and the gettering effect is lost. Furthermore, when a polycrystalline silicon film is formed, if the polysilicon is single-crystallized by an annealing process during the process, the gettering effect is lost. Thus, the conventional IG method and EG method have a problem that sufficient gettering sites cannot be formed. In view of the above circumstances, the present invention aims to provide a semiconductor device provided with a gettering element on the surface of a semiconductor region where semiconductor elements are formed, and a method for manufacturing the same. [Means for solving the problem]

[0005] In order to achieve the above object, the present invention relates to a semiconductor device having a gettering element, The gettering element is A first trench portion having a first depth and a second trench portion having a second depth deeper than the first depth are disposed opposite each other on a surface of a semiconductor region. And so, The first trench portion is filled with an insulating material, the second trench portion has an inner surface covered with the insulating material, and the inside surrounded by the insulating material serves as a stress relief portion, and the second depth is deeper than a depth of a gettering region formed in the semiconductor region between the first trench portion and the second trench portion and is a depth that prevents the gettering region from spreading from the second trench portion to the semiconductor region on the opposite side to the gettering region. The second trench portion surrounds the first trench portion so as to eliminate any influence on the semiconductor element formed therearound. It is characterized by:

[0006] The invention according to claim 2 of the present application is characterized in that, in the semiconductor device according to claim 1, the semiconductor region is made of silicon, the insulating material is made of silicon oxide, and the stress relaxation portion is made of polysilicon or a void.

[0007] The invention according to claim 3 of the present application is characterized in that in the semiconductor device according to claim 1 or 2, the gettering region includes an impurity-implanted region.

[0008] The invention according to claim 4 of the present application is a method for manufacturing a semiconductor device having a gettering element, comprising the steps of: forming an etching mask having a first opening with a first opening width for forming a first trench portion in a region on the surface of the semiconductor region where the gettering element is to be formed and a second opening with a second opening width wider than the first opening width for forming a second trench portion, and using the etching mask to etch away a part of the exposed semiconductor region to form a first trench portion with the first opening width and a first depth, and a second trench portion with the second opening width and a second depth deeper than the first depth; forming an insulating material in the first trench portion, filling the first trench portion with the insulating material and covering an inner surface of the second trench portion with the insulating material to form a region filled with the insulating material; and leaving a region in the second trench portion that is not filled with the insulating material as a void or filling it with a stress relaxation material to form a stress relaxation portion, and then heat-treating the semiconductor region to form a gettering region in the semiconductor region between the first trench portion and the second trench portion, the semiconductor region being shallower than a depth of the second trench portion. the semiconductor region is made of silicon, the insulating material is made of silicon oxide, and the stress relaxation material is made of polysilicon. 4. A method for manufacturing a semiconductor device comprising the steps of:

[0010] Claims of the present application 5 The invention according to claim Book 4 In the above-mentioned method for manufacturing a semiconductor device, the step of forming the gettering region includes a step of ion-implanting an impurity into at least the semiconductor region that is to become the gettering region, and then performing the heat treatment. Effect of the Invention

[0011] In the semiconductor device of the present invention, the gettering element can be disposed on the surface of the semiconductor region where the semiconductor element is formed, so that the gettering efficiency can be improved. In addition, a general gettering region can be disposed on a semiconductor substrate or an epitaxial substrate at a position away from the surface of the semiconductor region, so that the region where the semiconductor element can be formed (DZ layer) can be made thick, which is advantageous in that various semiconductor elements can be formed.

[0012] The gettering element of the present invention can have both gettering sites generated due to thermal expansion and gettering sites generated due to ion implantation, and has the advantage of being able to increase the gettering efficiency.

[0013] The method for manufacturing a semiconductor device of the present invention can be carried out using only the normal manufacturing process for semiconductor devices, and can therefore be carried out easily with a high yield. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is an explanatory diagram of a gettering element of the semiconductor device of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of a gettering element according to the first embodiment of the present invention. [Diagram 3] 3A to 3C are explanatory diagrams of a method for manufacturing the gettering element according to the first embodiment of the present invention. [Figure 4] 3A to 3C are explanatory diagrams of a method for manufacturing the gettering element according to the first embodiment of the present invention. [Diagram 5] 3A to 3C are explanatory diagrams of a method for manufacturing the gettering element according to the first embodiment of the present invention. [Figure 6] 3A to 3C are explanatory diagrams of a method for manufacturing the gettering element according to the first embodiment of the present invention. [Figure 7] 3A to 3C are explanatory diagrams of a method for manufacturing the gettering element according to the first embodiment of the present invention. [Figure 8] FIG. 4 is an explanatory diagram of a gettering element according to a second embodiment of the present invention. [Figure 9] 5A to 5C are explanatory diagrams of a method for manufacturing a gettering element according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention relates to a semiconductor device having a gettering element on the surface of a semiconductor region of a silicon substrate, a silicon epitaxial substrate, an SOI substrate, etc., and a method for manufacturing the same. EXAMPLES

[0016] First, a first embodiment of the present invention will be described. Fig. 1 shows a schematic diagram of a case where a gettering element 2 of this embodiment is arranged in a scribe region 1 where a semiconductor substrate (wafer) on which semiconductor elements are formed is cut and removed in a lattice shape while leaving a semiconductor element forming region when forming semiconductor devices by dividing the semiconductor substrate (wafer) on which semiconductor elements are formed. As shown in Fig. 1, a plurality of gettering elements 2 can be arranged along the scribe region 1.

[0017] Fig. 2 is an explanatory diagram of an individual gettering element 2, showing a cross-sectional view in a direction perpendicular to the longitudinal direction of the gettering element 2 shown in Fig. 1. As shown in Fig. 2, the gettering element 2 of this embodiment has a first trench portion 4 and a second trench portion 5 on the surface of a semiconductor region 3 such as an epitaxial layer on a semiconductor substrate, and the first trench portion 4 is surrounded by the second trench portion 5 formed at a predetermined distance apart.

[0018] The opening dimension of the first trench portion 4 is narrower than the opening dimension of the second trench portion 5. Furthermore, the depth of the first trench portion 4 is shallower than the depth of the second trench portion 5.

[0019] 2, the inside of the first trench portion 4 is filled only with silicon oxide 6, the inside of the second trench portion 5 is covered on the surface with silicon oxide 6, and the region not filled with silicon oxide 6 is filled with polysilicon 7. The polysilicon 7 on the surface of the second trench portion 5 is in an oxidized state by a heat treatment to be described later.

[0020] A gettering region 8 resulting from thermal expansion is formed between the first trench portion 4 and the second trench portion 5. The gettering region 8 will be described in detail in the following description of the manufacturing method.

[0021] Next, a method for manufacturing the gettering element 2 shown in Fig. 2 will be described. In a region of the semiconductor region 3 where the gettering element is to be formed, an etching mask 11 is formed that has a first opening 9 with a predetermined width (corresponding to the first opening width) for forming a first trench portion and a second opening 10 with a predetermined width (corresponding to the second opening width and wider than the first opening width) for forming a second trench portion (Fig. 3). When silicon oxide is used as this etching mask 11, a silicon oxide film is formed on the entire surface of the semiconductor region 3, and the first opening 9 and the second opening 10 are formed by a normal photolithography method. The first opening 9 is arranged so as to be surrounded by the second opening 10.

[0022] Thereafter, the semiconductor region 3 exposed in the first opening 9 and the second opening 10 is dry-etched using the etching mask 11. As shown in FIG. 4, this etching can simultaneously form a first trench portion 4 etched from the first opening 9 with a first opening width and a second trench portion 5 etched from the second opening 10 with a second opening width. As shown in FIG. 4, the depth of the first trench portion 4 is formed shallower than the depth of the second trench portion 5. The depths of the first trench portion 4 and the second trench portion 5 can be formed with good reproducibility by setting the first opening width of the first opening 9 and the second opening width of the second opening 10 to a predetermined width. It is also possible to form the first trench portion 4 and the second trench portion 5 separately.

[0023] Thereafter, a silicon oxide film 12 is formed on the entire surface by low pressure CVD. The thickness of the silicon oxide film 12 is set so that the first trench portion 4 is filled with the silicon oxide film 12, and the second trench portion 5 is not filled with the silicon oxide film 12, leaving a gap 13 (FIG. 5).

[0024] In order to fill the void remaining inside the second trench portion 5, a polysilicon film 14 is formed on the entire surface (FIG. 6). When forming the silicon oxide film 12 in the second trench portion 5, it is possible to increase the thickness of the silicon oxide film 12 so that the opening of the second trench portion 5 is blocked with the silicon oxide film and a void (corresponding to the stress relaxation portion) is left inside. In this case, the step of forming the polysilicon film can be omitted. Alternatively, when forming the polysilicon film 14, it is also possible to form the polysilicon film 14 so that the opening of the second trench portion 5 is blocked with the polysilicon film 14 and a void (corresponding to the stress relaxation portion) is left inside.

[0025] The polysilicon film 14, silicon oxide film 12, and etching mask 11 covering the surface of the semiconductor region 3 are removed to expose the surface of the semiconductor region 3. Then, a heat treatment is performed at 1100° C. for about 100 minutes. This heat treatment causes the semiconductor region 3 and the like to expand thermally. Here, since the thermal expansion coefficient of the silicon oxide film 12 filled in the first trench portion 4 is smaller than that of the semiconductor region 3 made of silicon, stress is concentrated at the interface between the semiconductor region 3 surrounded by the second trench portion 5 and the silicon oxide film 12 of the first trench portion 4. On the other hand, since the second trench portion 5 is filled with the polysilicon film 14 (corresponding to a stress relief material), the stress concentrated at the interface between the semiconductor region 3 and the silicon oxide film 12 of the second trench portion 5 is relieved. As a result, defects (dislocations or lattice distortion) (shown by dotted lines in FIG. 7) are generated from the first trench portion 4, and these defects extend in the direction of the second trench portion 5. As a result of observing the generated defect, it was confirmed that the defect extended obliquely downward from the sidewall of the first trench portion 4 and stopped at the sidewall of the second trench portion 5, as shown in FIG. 7. This defect functions as a gettering site 15.

[0026] By appropriately setting the depth of the second trench portion 5 in this manner, it is possible to form a gettering region 8 in which gettering sites 15 are concentrated in the semiconductor region 3 surrounded by the second trench portion 5. In other words, the depth of the second trench portion 5 is set so that the gettering region 8 is not formed by spreading to the semiconductor region 3 outside the second trench portion 5 (the opposite side to the gettering region 8). To achieve this, it is necessary to set the depths of the first trench portion 4 and the second trench portion 5, and further to set the first opening width of the first opening 9 and the second opening width of the second opening 10 described in FIG.

[0027] The gettering region 8 thus formed traps heavy metal impurities such as iron (Fe) that diffuse during heat treatment in the manufacturing process of the semiconductor device, and can reduce the effects of the heavy metal impurities in the semiconductor element formation region. In this embodiment, the gettering element 2 having the gettering region 8 is disposed in the scribe region 1 as shown in Fig. 1, so that the gettering element 2 is not disposed in the completed semiconductor device.

[0028] Incidentally, in the gettering element 2 of this embodiment, the gettering region 8 is formed in a region surrounded by the second trench portion 5 as shown in Fig. 7, so that the gettering region 8 does not affect the semiconductor element even if it is disposed in the semiconductor element formation region. Furthermore, heavy metal impurities once gettered will not be released again unless a high-temperature, long-time heat treatment step is performed after the heat treatment for forming the gettering region 8. Therefore, the gettering element 2 of the present invention may be formed either in the semiconductor element formation region or in the semiconductor region 3 outside the semiconductor element formation region, such as a scribe region.

[0029] When the gettering element 2 is formed in the scribe region 1, the second trench portion 5 may be disposed only in the region parallel to the extension direction of the scribe region 1, and the first trench portion 4 may not be surrounded by the second trench portion 5. In this case, the gettering site 15 is formed extending in the extension direction of the scribe region 1 where the second trench portion 5 is not present, but there is no effect on the semiconductor element formation region and no problem occurs. In this case, the first trench portion 4 needs to be shaped so that stress that causes defects due to thermal expansion is efficiently applied to the first trench portion 4. On the other hand, when the gettering element 2 is formed in the semiconductor element formation region, it is preferable to surround the first trench portion 4 with the second trench portion 5 in order to eliminate the effect on the semiconductor element formed around it. EXAMPLES

[0030] Next, a second embodiment will be described. As shown in FIG. 8, the gettering element 2A of this embodiment is different from the first embodiment described above in that an impurity implanted region 16 is added to the gettering region 8 in which the gettering site 15A is formed. This impurity implanted region 16 is a conventionally known gettering region. This embodiment can combine a gettering site formed in a relatively deep region generated from the first trench portion 4 and a gettering site formed in a relatively shallow region generated by ion implantation from the surface, and is expected to improve the gettering efficiency.

[0031] Next, a method for manufacturing the gettering element 2A shown in Fig. 8 will be described. As in the first embodiment, an etching mask 11 is formed in a region of the semiconductor region 3 where the gettering element is to be formed, the etching mask 11 including a first opening 9 having a predetermined width (corresponding to the first opening width) for forming a first trench portion and a second opening 10 having a predetermined width (corresponding to the second opening width, wider than the first opening width) for forming a second trench portion (Fig. 3).

[0032] Thereafter, the semiconductor region 3 exposed in the first opening 9 and the second opening 10 is dry etched using the etching mask 11. As shown in FIG. 4, this etching allows the first trench portion 4 etched from the first opening 9 with the first opening width and the second trench portion 5 etched from the second opening 10 with the second opening width to be simultaneously formed. The depth of the first trench portion 4 is formed shallower than the depth of the second trench portion 5. The depths of the first trench portion 4 and the second trench portion 5 can be formed with good reproducibility by setting the first opening width of the first opening 9 and the second opening width of the second opening 10 to a predetermined width. It is also possible to form the first trench portion 4 and the second trench portion 5 separately.

[0033] Thereafter, a silicon oxide film 12 is formed on the entire surface by low pressure CVD. The thickness of the silicon oxide film 12 is set so that the first trench portion 4 is filled with the silicon oxide film 12, and the second trench portion 5 is not filled with the silicon oxide film 12, leaving a gap 13 (FIG. 5).

[0034] In order to fill the void remaining inside the second trench portion 5, a polysilicon film 14 is formed on the entire surface (FIG. 6). When forming the silicon oxide film 12 in the second trench portion 5, it is possible to thicken the silicon oxide film to block the opening of the second trench portion 5 and leave a void inside. In this case, the process of forming the polysilicon film can be omitted. Alternatively, when forming the polysilicon film 14, it is possible to block the opening of the second trench portion 5 with the polysilicon film 14 and form the film so that a void remains inside. In either case in this embodiment, it is preferable to form the film so that the opening is not exposed on the surface of the semiconductor region 3 in order to form an ion implantation mask described later.

[0035] The polysilicon film 14, the silicon oxide film 12 and the etching mask 11 formed on the surface of the semiconductor region 3 are removed to expose the surface of the semiconductor region 3. Then, an ion implantation mask 17 is formed so as to open the semiconductor region 3 in the region surrounded by the second trench portion 5 where the impurity implantation region is to be formed (FIG. 9).

[0036] A high concentration of phosphorus ions is implanted into the exposed semiconductor region 3 using an ion implantation mask 17 to form crystal distortion. Thereafter, the ion implantation mask 17 is removed and heat treatment is performed. This heat treatment makes it easier for defects to occur due to the crystal distortion formed by the ion implantation. These defects function as gettering sites. Furthermore, as explained in the first embodiment above, the semiconductor region 3 etc. thermally expands, and defects (shown by dotted lines in FIG. 8) occur from the first trench portion 4, and these defects extend in the direction of the second trench portion 5. The generated defects extend obliquely downward from the sidewall of the first trench portion 4 and stop at the sidewall of the second trench portion 5, functioning as gettering sites 15A.

[0037] In this embodiment, a gettering region 8A having a gettering site caused by ion implantation and a gettering site caused by thermal expansion can be formed. As with the gettering element 2 described in the first embodiment, the gettering region 8A shown in FIG. 8 can be formed in the semiconductor region 3 surrounded by the second trench portion 5 by appropriately setting the depth of the second trench portion 5.

[0038] The gettering region 8A thus formed traps heavy metal impurities such as iron (Fe) that diffuse during heat treatment in the manufacturing process of the semiconductor device, and can reduce the effects of the heavy metal impurities in the semiconductor element formation region. In this embodiment, the gettering element 2 having the gettering region 8 is disposed in the scribe region 1 as shown in Fig. 1, so that the gettering element 2 is not disposed in the completed semiconductor device.

[0039] However, as shown in Fig. 8, the gettering region 8A of the gettering element 2A of this embodiment is formed in a region surrounded by the second trench portion 5, so that the gettering region 8A does not affect the semiconductor element even if it is disposed in the semiconductor element formation region. Furthermore, the heavy metal impurities once gettered will not be released again unless a high-temperature, long-time heat treatment step is performed after the heat treatment for forming the gettering region 8A. Therefore, the gettering element 2A of the present invention may be formed either in the semiconductor element formation region or in the semiconductor region 3 outside the semiconductor element formation region, such as a scribe region.

[0040] When the gettering element 2A is formed in the scribe region 1, the second trench portion 5 may be disposed only in the region parallel to the extension direction of the scribe region 1, and the first trench portion 4 may not be surrounded by the second trench portion 5. In this case, the gettering site 15A is formed extending in the extension direction of the scribe region 1 where the second trench portion 5 is not present, but there is no effect on the semiconductor element formation region and no problem occurs. In this case, it is necessary to make the shape such that the stress that causes defects due to thermal expansion is efficiently applied to the first trench portion 4. On the other hand, when the gettering element 2A is formed in the semiconductor element formation region, it is preferable to surround the first trench portion 4 with the second trench portion 5 in order to eliminate the effect on the semiconductor element formed around it.

[0041] Although the embodiments of the present invention have been described above, it goes without saying that the present invention is not limited to the above embodiments. Although an example of forming silicon oxide to fill the first trench portion 4 by low pressure CVD has been described, it is possible to change to a method of thermally oxidizing a semiconductor region made of silicon. In addition, the materials of the semiconductor region, the insulating material, and the stress relaxation portion can be appropriately changed within a range in which a gettering site caused by thermal expansion can be formed. [Explanation of symbols]

[0042] 1: scribe region, 2, 2A: gettering element, 3: semiconductor region, 4: first trench portion, 5: second trench portion, 6: silicon oxide, 7: polysilicon, 8, 8A: gettering region, 9: first opening, 10: second opening, 11: etching mask, 12: silicon oxide film, 13: gap, 14: polysilicon film, 15, 15A: gettering site, 16: impurity implantation region, 17: ion implantation mask

Claims

1. In a semiconductor device having a gettering element, the gettering element is configured such that a first trench portion having a first depth and a second trench portion having a second depth deeper than the first depth are disposed opposite to each other on a surface of a semiconductor region; the first trench portion is filled with an insulating material; the second trench portion has an inner surface covered with the insulating material, and an inner portion surrounded by the insulating material serves as a stress relaxation portion; the second depth is deeper than a depth of a gettering region formed in the semiconductor region between the first trench portion and the second trench portion, and is a depth that prevents the gettering region from spreading from the second trench portion to the semiconductor region on an opposite side to the gettering region; The second trench portion surrounds the first trench portion so as to eliminate any influence on a semiconductor element formed in the vicinity.

2. 2. The semiconductor device according to claim 1, wherein said semiconductor region is made of silicon, said insulating material is made of silicon oxide, and said stress relaxation portion is made of polysilicon or a void.

3. 3. The semiconductor device according to claim 1, The semiconductor device according to claim 1, wherein the gettering region includes an impurity-implanted region.

4. A method for manufacturing a semiconductor device including a gettering element, comprising the steps of: a step of forming an etching mask having a first opening with a first opening width for forming a first trench portion in a region on the surface of the semiconductor region where the gettering element is to be formed and a second opening with a second opening width wider than the first opening width for forming a second trench portion, and using the etching mask to etch away a part of the exposed semiconductor region to form a first trench portion with the first opening width and a first depth, and a second trench portion with the second opening width and a second depth deeper than the first depth; forming an insulating material in the first trench portion and the second trench portion, filling the first trench portion with the insulating material and covering an inner surface of the second trench portion with the insulating material to form a region filled with the insulating material; a step of leaving a region in the second trench portion that is not filled with the insulating material as a void or filling it with a stress relaxation material to form a stress relaxation portion, and then heat treating the semiconductor region to form a gettering region in the semiconductor region between the first trench portion and the second trench portion, the semiconductor region being shallower than a depth of the second trench portion; 2. A method for manufacturing a semiconductor device, comprising the steps of: forming a semiconductor region on a substrate; forming a first insulating material on the substrate; and forming a first stress relaxation material on the substrate.

5. 5. The method of manufacturing a semiconductor device according to claim 4, 2. A method for manufacturing a semiconductor device, wherein the step of forming the gettering region includes a step of ion-implanting an impurity into the semiconductor region that is to become the gettering region, and then performing the heat treatment.

Citation Information

Patent Citations

  • Gettering of semiconductor substrate

    JP1991084931A

  • Manufacture of silicon wafer and semiconductor device

    JP1993062867A

  • Manufacture of semiconductor device

    JP1994291178A

  • Semiconductor device and method for manufacturing it

    JP2002134512A

  • Semiconductor device

    JP2009158588A