Catalyst system, method for hydrocracking feedstock oil containing heavy gas oil fraction using the same, and hydrocracking apparatus

A catalyst system with specific zeolite ratios and bed arrangements enhances both middle distillate yield and hydrocracking activity, addressing the inefficiencies of existing hydrocracking methods for heavy gas oil fractions.

JP7583538B2Active Publication Date: 2024-11-14IDEMITSU KOSAN CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020111904
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-29
Publication Date
2024-11-14
Estimated Expiration
2040-06-29

AI Technical Summary

Technical Problem

Existing methods for hydrocracking heavy gas oil fractions struggle to achieve a high yield of middle distillates (120°C to 360°C) while maintaining excellent hydrocracking activity, leading to instability and higher production costs.

Method used

A catalyst system comprising a packed bed A with a zeolite ratio of 12% or more and a packed bed B with a zeolite ratio of less than 12%, arranged in specific ratios (R A /R B from 20/80 to 95/5, where bed A contacts the heavy gas oil fraction first, utilizing catalyst A's high hydrocracking activity and catalyst B's high middle distillate selectivity to balance both properties.

Benefits of technology

The catalyst system achieves a high middle distillate yield and hydrocracking activity, allowing for stable and cost-effective production of middle distillates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583538000001
    Figure 0007583538000001
  • Figure 0007583538000002
    Figure 0007583538000002
Patent Text Reader

Abstract

To provide a catalyst system that achieves both a high intermediate fraction yield and a hydrocracking activity, and a hydrocracking method and hydrocracking apparatus for a raw material oil containing a heavy gas oil fraction using the catalyst system.SOLUTION: There is provided a catalyst system that performs hydrocracking of a raw material oil containing a heavy gas oil fraction. The catalyst system comprises: a packed bed A composed of a catalyst A with a zeolite ratio of 12% or more; and a packed bed B composed of a catalyst B with a zeolite ratio of less than 12%, in which the packed bed of the catalyst A is filled so as to be in contact with the heavy gas oil fraction at first, so that a ratio (RA / RB) between a rate of the packed layer A (RA) and a rate of the packed layer B (RB) is adjusted to 20 / 80 to 80 / 20. There is also provided a hydrocracking method and hydrocracking apparatus using the catalyst system.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst system, a method for hydrocracking feedstock containing a heavy gas oil fraction using the same, and a hydrocracking apparatus. [Background technology]

[0002] Heavy gas oil fractions such as oil refinery gas oil (AGO) and vacuum gas oil (VGO) obtained by distilling crude oil under atmospheric pressure or vacuum are fractions that are used for various purposes such as kerosene, automobile fuel, lubricant base oil, etc., after undergoing refining processes such as hydrocracking. Various methods have been investigated for hydrocracking (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a method for producing a lubricating base oil, which includes, in order, a first step of catalytically cracking a feedstock oil containing aromatic hydrocarbons with a hydrocracking catalyst containing zeolite to produce a catalytically cracked oil, and a second step of contacting the feedstock oil with a hydrocracking catalyst containing an amorphous solid acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-66227 A Summary of the Invention [Problem to be solved by the invention]

[0005] Since the above-mentioned heavy gas oil fraction is used for important applications such as kerosene, base stock for automobile fuel (gasoline base stock), lubricant base oil, etc. after hydrocracking, there is a demand for more inexpensive and stable production and supply of fractions suitable for these applications. Therefore, it is necessary to study the type of catalyst used for hydrocracking, reaction conditions, and various other aspects to improve the yield of the desired fraction or to improve hydrocracking activity.

[0006] Therefore, the present invention focuses on middle distillates having a boiling point of 120°C to 360°C, which are mainly used as kerosene and diesel and are heavily used in the above-mentioned applications among the heavy light oil fractions, and aims to provide a catalyst system that can realize a stable supply of middle distillates at lower cost by increasing the yield of the middle distillate and maintaining excellent hydrocracking activity when hydrocracking a heavy light oil fraction, i.e., a catalyst system that achieves both a high yield of middle distillate and hydrocracking activity, and further a method and an apparatus for hydrocracking a feedstock containing a heavy light oil fraction using the catalyst system. [Means for solving the problem]

[0007] As a result of intensive research into solving the above problems, the present inventors have found that the problems can be solved by the following invention. That is, the present invention provides a catalyst system having the following configuration, and further a method for hydrocracking a feedstock oil containing a heavy gas oil fraction and a hydrocracking apparatus using the catalyst system.

[0008] 1. A catalytic system for hydrocracking a feedstock oil containing a heavy gas oil fraction, comprising: a packed bed A composed of a catalyst A having a zeolite ratio of 12% or more; and a packed bed B composed of a catalyst B having a zeolite ratio of less than 12%. A ) and the ratio of the filling layer B (R B ) and the ratio (R A / R B The packed bed A is packed so that the packed bed A first comes into contact with the heavy gas oil fraction so that the ratio of the packed bed A to the heavy gas oil fraction is 20 / 80 to 95 / 5. 2. A method for hydrocracking a feedstock containing a heavy gas oil fraction, using the catalyst system described in 1 above. 3. A hydrocracking unit for feedstock containing a heavy gas oil fraction, comprising the catalyst system described in 1 above. Effect of the Invention

[0009] According to the present invention, it is possible to provide a catalyst system which achieves both a high yield of middle distillates and high hydrocracking activity, and further, a method for hydrocracking a feedstock oil containing a heavy gas oil fraction using the catalyst system, and a hydrocracking apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a catalyst system, a hydrocracking method, and a hydrocracking apparatus according to an embodiment of the present invention (hereinafter, sometimes simply referred to as "the present embodiment") will be specifically described. Note that in this specification, the numerical values ​​of "less than," "more than," and "to" in describing a numerical range are numerical values ​​that can be arbitrarily combined, and the numerical values ​​in the examples are numerical values ​​that can be used as upper or lower limits.

[0011] [Catalyst system] The catalyst system of the present embodiment is a catalyst system for hydrocracking a feedstock oil containing a heavy gas oil fraction, in which a packed bed A composed of a catalyst A having a zeolite ratio of 12% or more and a packed bed B composed of a catalyst B having a zeolite ratio of less than 12% are arranged such that the packed bed A has a ratio (R A ) and the ratio of the filling layer B (R B ) and the ratio (R A / R B The packed bed A is packed so that it first comes into contact with the heavy gas oil fraction so that the ratio of the packed bed A to the heavy gas oil fraction is 20 / 80 to 95 / 5.

[0012] Catalyst A having a zeolite ratio of 12% or more is characterized by a higher hydrocracking activity but an insufficient middle distillate selectivity, while catalyst B having a zeolite ratio of less than 12% is characterized by a higher middle distillate selectivity but an insufficient hydrocracking activity. In the catalyst system of this embodiment, catalyst A and catalyst B having such characteristics are mixed in the above ratio (R A / R B) are used in combination, and the packed beds of the catalysts are arranged so that the feedstock containing a heavy gas oil fraction is passed through packed bed A of catalyst A followed by packed bed B of catalyst B, thereby making it possible to improve the advantages of each catalyst while compensating for their disadvantages, and as a result, it is possible to achieve both a high middle distillate yield and high hydrocracking activity. In this specification, the middle distillate refers to a fraction having a boiling point of 120°C to 360°C as described above, and includes fractions usually called gas oil and kerosene.

[0013] The inventors found that middle distillate selectivity tends to depend on the performance of the packed bed of the catalyst that comes into contact with the feedstock containing heavy gas oil fractions later. By arranging packed bed B of catalyst B, which has higher middle distillate selectivity, so that the feedstock comes into contact with packed bed A of catalyst A later than packed bed A of catalyst B, the advantage of catalyst B's higher middle distillate selectivity is fully obtained, while the disadvantage of catalyst B's lower hydrocracking activity is compensated for by catalyst A, which has the advantage of higher hydrocracking activity, making it possible to achieve both a high middle distillate yield and hydrocracking activity. In addition, by adjusting the proportion of packed bed A of catalyst A to the above proportion (R A / R B It was also found that by making the ratio 20 / 80 to 95 / 5, i.e., 20% or more, the middle distillate yield properties can be maintained at a high level, and by making it 95% or less, a high level of hydrocracking activity can be obtained. In this way, by achieving both a high middle distillate yield and hydrocracking activity, it has become possible to hydrocracking heavy gas oil fractions more cheaply and stably (over the long term).

[0014] [Catalyst A] Catalyst A is a catalyst characterized by having a zeolite ratio of 12% or more, and is a catalyst having superior hydrocracking activity compared to catalyst B described below. In this specification, the zeolite ratio means the content of zeolite in the catalyst carrier.

[0015] Preferred examples of catalyst A include catalysts in which an active metal is supported on a support containing a zeolite, such as ultra-stable Y-type zeolite (also referred to as "USY zeolite") or metal-supported USY zeolite, and a porous inorganic oxide, such as alumina, silica-alumina, silica, alumina-boria, alumina-zirconia, or alumina-titania, with the zeolite ratio being 12% or more.

[0016] (Zeolite) The zeolite is more preferably a metal-supported USY zeolite, and for example, a preferred example of the metal-supported USY zeolite is a USY zeolite supported with at least one metal selected from Groups 3 to 16 of the periodic table. In particular, iron-supported USY zeolite, which supports iron as the metal, is preferred.

[0017] The USY zeolite and metal-supported USY zeolite can be produced, for example, by the following method. As the raw material for USY zeolite, Y zeolite having a ratio (molar ratio) of silica to alumina, that is, SiO2 / Al2O3 of 4.5 or more, preferably 5.0 or more, and Na2O of 2.4 mass % or less, preferably 1.8 mass % or less is used. First, the above-mentioned Y-type zeolite is subjected to a steaming treatment to obtain USY zeolite. Here, the conditions for the steaming treatment may be appropriately selected according to various circumstances, but it is preferable to perform the treatment in the presence of steam at a temperature of 510°C to 810°C. Steam may be introduced from the outside, or physically adsorbed water or crystal water contained in the Y-type zeolite may be used. In addition, a mineral acid is added to the USY zeolite obtained by the steaming treatment, and the mixture is mixed and stirred to dealuminate the zeolite structural framework, and the aluminum that has fallen off is washed and removed by the steaming and mineral acid treatment.

[0018] Various types of mineral acids can be used here, but hydrochloric acid, nitric acid, sulfuric acid, etc. are commonly used. In addition, inorganic acids such as phosphoric acid, perchloric acid, peroxodisulfonic acid, dithioic acid, sulfamic acid, nitrososulfonic acid, etc., and organic acids such as formic acid, trichloroacetic acid, trifluoroacetic acid, etc. can also be used. The amount of these mineral acids used is about 0.5 to 20 mol, preferably 3 to 16 mol, per 1 kg of USY zeolite. The mineral acid concentration is 0.5 to 50 mass % solution, preferably 1 to 20 mass % solution. The treatment temperature is room temperature to 100°C, preferably 50 to 100°C. The treatment time is 0.1 to 12 hours.

[0019] Next, a metal salt solution is added to this system to support the metal on the USY zeolite. Examples of the support method include a mixing and stirring treatment, a dipping method, and an impregnation method, and the like, with the mixing and stirring treatment being preferred. The metal is preferably at least one metal from Groups 3 to 16 of the periodic table. Specifically, preferred examples include yttria and lanthanum from Group 3 of the periodic table, zirconium and titanium from Group 4, vanadium, niobium and thallium from Group 5, chromium, molybdenum and tungsten from Group 6, manganese and rhenium from Group 7, iron, ruthenium and osmium from Group 8, cobalt, rhodium and iridium from Group 9, nickel, palladium and platinum from Group 10, copper from Group 11, zinc and cadmium from Group 12, aluminum and gallium from Group 13, tin from Group 14, phosphorus and antimony from Group 15, and selenium from Group 16. Among these, At least one metal selected from the group consisting of Groups 4, 7, 8, 9 and 10 is more preferred, with titanium, manganese, iron, cobalt, nickel, palladium and platinum being even more preferred, and iron being particularly preferred.

[0020] As the salts of various metals, sulfates and nitrates are preferable. When performing the metal salt solution treatment, the treatment temperature varies depending on the situation and cannot be unequivocally defined, but the treatment temperature is usually about 30° C. to 100° C., preferably 50° C. to 80° C., and the treatment time is usually about 0.1 to 12 hours, preferably 0.5 to 5 hours.

[0021] The loading of these metals is preferably carried out simultaneously with the dealumination of the zeolite structural framework, and may be carried out at a pH of 2.0 or less, preferably 1.5 or less. The iron salt may be ferrous sulfate, ferric sulfate, etc., with ferric sulfate being preferred. The iron sulfate may be added as is, but is preferably added as a solution. The solvent used in this case may be any solvent capable of dissolving the iron salt, with water, alcohol, ether, ketone, etc. being preferred. The concentration of the iron sulfate added is usually 0.02 to 10.0 mol / L, preferably 0.05 to 5.0 mol / L.

[0022] When a mineral acid and an iron sulfate are added to treat a crystalline aluminosilicate, the slurry ratio, that is, treatment solution volume (liters) / aluminosilicate mass (kg) is conveniently in the range of 1 to 50, and particularly preferably 5 to 30. The iron-loaded crystalline aluminosilicate obtained by the above treatment is further washed with water and dried, if necessary. In this manner, USY zeolite and metal-supported USY zeolite can be produced.

[0023] (Porous inorganic oxide) Preferred examples of the porous inorganic oxide to be combined with zeolite include alumina, silica-alumina, silica, alumina-boria, alumina-zirconia, alumina-titania, etc., and among these, alumina as the main component is preferred. In this specification, the term "main component" refers to a content of 50% by mass or more, preferably 70% by mass, and more preferably 80% by mass, based on the porous inorganic oxide (100% by mass).

[0024] As the alumina, boehmite gel, alumina sol, and alumina produced from these are preferably used. Alumina is preferable because it can support the active metal in a highly dispersed manner, and the alumina described below is particularly preferable because it can easily optimize the pore distribution of the catalyst.

[0025] Particularly preferred alumina is one that is produced through a process of obtaining alumina hydrate (boehmite gel) as an intermediate by a neutralization reaction of an aqueous solution containing an aluminum salt, and has a relative peak height of boehmite crystals in X-ray diffraction analysis (XRD) of 65 to 85. If the relative peak height is 65 or more, the average pore diameter of the alumina does not become excessively small, thereby improving the desulfurization activity of the catalyst for heavy light oil fractions, and if it is 85 or less, the average pore diameter of the alumina does not become excessively large, thereby improving the cracking activity of the catalyst.

[0026] In the present invention, the relative peak height of the boehmite crystal of the alumina hydrate is calculated from the peak heights (peak heights) of the alumina (boehmite) of the standard material and the sample material at 2θ: 10° to 20° using an X-ray diffractometer, and the calculated value is calculated from the formula (1) described below. Specifically, the value is measured by the following method.

[0027] (Method of measuring relative peak height) Using an X-ray diffractometer, the alumina (boehmite) peak heights of the standard material and the sample material were measured, and the relative peak heights were calculated using the following formula (1). Relative peak height = (B / A) x 100 (1) In the formula, A represents the measured value of the peak height of the standard material (manufactured by Sasol, trade name: Catapal D), and B represents the measured value of the peak height of the sample material. The conditions for the X-ray diffraction measurement are as follows. Measuring device: Rigaku (RINT-2100) Measurement conditions: Target: Cu Filter:Ni Voltage: 30kV Current: 14mA Scan speed: 1° / min, Full scall: 1000cps, Number of smoothing points: 19 Scan angle(2θ):10°~20° How to measure Peak High: In the broken line profile, tangents were drawn to the background on both sides of the peak, and then a perpendicular line was drawn from the peak top to determine the height from the background to the peak top, and these values ​​were taken as the peak heights. Note that the measuring device is not limited to the above model, and an equivalent device may be used.

[0028] Alumina satisfying the above conditions can be produced, for example, by the following method, that is, (1) a step of reacting an aqueous solution containing an aluminum salt with a neutralizing agent to obtain an alumina hydrate (boehmite) having a pH of 6 to 11, and then (2) a step of washing, aging, drying, and kneading the alumina hydrate.

[0029] In the above method, aluminum sulfate, aluminum nitrate, aluminum chloride, etc. can be used as the aluminum salt, and sodium aluminate, potassium aluminate, caustic soda, ammonia, etc. can be used as the neutralizing agent. The pH of the alumina hydrate is preferably slightly alkaline, specifically, pH 7 to 10, from the viewpoint of facilitating the production of a hydrate having a desired particle size.

[0030] In the washing step (2), washing is performed thoroughly. For example, if aluminum sulfate is used as the aluminum salt, the sulfate radicals (SO4 2- It is preferable to carry out the aging process so that the remaining amount is 1 mass % or less, and more preferably 0.7 mass % or less. The temperature of the aging process is 80 to 160°C, preferably 90 to 100°C, and the kneading time is preferably 1 to 24 hours, and more preferably 2 to 12 hours. As the above-mentioned method for producing alumina, it is preferable to adopt the method described in Japanese Patent No. 3755826.

[0031] (Zeolite ratio) The zeolite ratio of catalyst A is 12% or more, that is, when the carrier of catalyst A contains the above-mentioned zeolite and porous inorganic oxide, the content of the zeolite is 12% or more, preferably 14% or more, more preferably 15% or more, and even more preferably 18% or more. There is no particular upper limit, but from the viewpoint of improving the middle distillate yield and hydrocracking activity, it may be about 45% or less, preferably 40% or less, more preferably 30% or less, and even more preferably 25% or less. The support of catalyst A is preferably composed of the above-mentioned zeolite and porous inorganic oxide, i.e., the sum of the two components is preferably 100% by mass, but may contain other components such as clay minerals and phosphorus, as long as the improvement in the middle distillate yield and hydrocracking activity is not hindered. In this case, the content of the other components is usually about 30% by mass or less, and preferably 25% by mass or less. When the content of the other components is within the above range, the effect of using the components can be easily obtained, and the improvement in the middle distillate yield and hydrocracking activity can also be achieved.

[0032] The carrier of catalyst A is prepared by, for example, forming a slurry of zeolite such as the above USY zeolite or metal-supported USY zeolite with water, and forming a slurry of a gel or sol-like porous inorganic oxide with water, and thoroughly mixing these with a kneader, etc. From the viewpoint of more efficiently preparing the carrier, the water content in each slurry state is preferably 30 to 80 mass %, more preferably 40 to 70 mass %, for the crystalline aluminosilicate slurry, and preferably 50 to 90 mass %, more preferably 55 to 85 mass %, for the porous inorganic oxide slurry. The zeolite and the porous inorganic oxide are mixed and kneaded, and then molded into a shape of 1 / 12 inch to 1 / 32 inch in diameter and 1.5 mm to 6 mm in length into a cylindrical, trilobe or quadruple lobe shape. The molded product is then dried at 30 to 200°C for 0.1 to 24 hours, and then calcined at 300 to 750°C (preferably 450 to 700°C) for 1 to 10 hours (preferably 2 to 7 hours), to obtain a carrier for catalyst A.

[0033] (active metal) The active metal used in the hydrocracking catalyst is preferably at least one metal selected from the group 6, 8, 9 and 10 of the periodic table. Here, the metal belonging to Group 6 of the periodic table is preferably molybdenum or tungsten, and the metal belonging to Groups 8 to 10 is preferably nickel or cobalt. As a combination of two types of metals, it is preferable to use a combination of a metal of Group 6 with a metal of Groups 8 to 10, and specifically, nickel-molybdenum, cobalt-molybdenum, nickel-tungsten, cobalt-tungsten, etc. are preferably mentioned, among which cobalt-molybdenum and nickel-molybdenum are preferable, and nickel-molybdenum is particularly preferable.

[0034] The amount of the metals supported as the active components is not particularly limited and may be appropriately selected depending on various conditions such as the properties of the feed oil, the desired hydrocracking activity, and the yield of middle distillates. Generally, the amount of the Group 6 metal supported is 0.5 to 30 mass %, preferably 5 to 20 mass %, of the entire catalyst, and the amount of the Group 8 to 10 metal supported is 0.1 to 20 mass %, preferably 1 to 10 mass %, of the entire catalyst. There is no particular limitation on the method for supporting the above metal components on the carrier, and for example, known methods such as impregnation, kneading, and coprecipitation can be used. The above metal components supported on the carrier are usually dried at 30 to 200°C for 0.1 to 24 hours, and then calcined at 250 to 700°C (preferably 300 to 650°C) for 1 to 10 hours (preferably 2 to 7 hours) to complete the catalyst.

[0035] [Catalyst B] Catalyst B is a catalyst characterized by having a zeolite ratio of less than 12%, and is a catalyst superior to Catalyst A in middle distillate selectivity. Preferred examples of catalyst B include catalysts in which an active metal is supported on a support containing a zeolite, such as ultra-stable Y-type zeolite (also referred to as "USY zeolite") or metal-supported USY zeolite, and a porous inorganic oxide, such as alumina, silica-alumina, silica, alumina-boria, alumina-zirconia, or alumina-titania, with the zeolite ratio being less than 12%.

[0036] The zeolite, porous inorganic oxide, and active metal in catalyst B are the same as those described for the zeolite, porous inorganic oxide, and active metal in catalyst A. The properties of catalyst B are the same as those described for catalyst A, but catalysts A and B differ in the ratio of zeolite contained in the carrier. In this way, by using two types of catalysts with different zeolite ratios in combination, as described above, it is possible to utilize the advantages of each catalyst and at the same time complement each other's disadvantages, resulting in a high middle distillate yield and hydrocracking activity.

[0037] As described above, the zeolite ratio of catalyst B must be less than 12%, and is preferably 11% or less from the viewpoint of improving the middle distillate yield and hydrocracking activity. There is no particular lower limit, and the zeolite ratio is usually 1% or more, preferably 3% or more, and more preferably 5% or more. The support for catalyst B may be prepared by blending zeolite and porous inorganic oxide so that the zeolite ratio is less than 12%, and thoroughly mixing the mixture in a kneader or the like to form a slurry, and may be prepared according to the method described as the method for producing the support for catalyst A. The active metal may also be supported according to the method described as the method for producing catalyst A.

[0038] [Ratio of packed bed A to packed bed B] In the catalyst system of this embodiment, the packed bed A composed of the catalyst A and the packed bed B composed of the catalyst B are mixed at a ratio (R A ) and the ratio of the packed bed B (R B ) and the ratio (R A / R BThe above ratio (R A / R B ) is less than 20 / 80, i.e., the ratio of packed bed A (R A ) is less than 20, and the ratio of packed bed B (R B ) exceeds 80, excellent hydrocracking activity cannot be obtained. A / R B ) is greater than 95 / 5, i.e., the ratio of packed bed A (R A ) is more than 95, and the ratio of packed bed B (R B ) is less than 5, excellent middle distillate selectivity cannot be obtained. From the viewpoint of improving the middle distillate yield and hydrocracking activity, the ratio is preferably 25 / 75 or more, more preferably 35 / 65 or more, even more preferably 45 / 55 or more, still more preferably 55 / 45 or more, and the upper limit is preferably 90 / 10 or less, more preferably 85 / 15 or less, even more preferably 80 / 20 or less, and still more preferably 75 / 25 or less.

[0039] [Arrangement of packed bed A and packed bed B] In the catalyst system of this embodiment, it is necessary that packed bed A is packed so as to come into contact with the feed oil containing the heavy gas oil fraction first, that is, packed bed B is packed next to packed bed A. Therefore, in the catalyst system of this embodiment, the feed oil containing the heavy gas oil fraction is passed through packed bed A and then through packed bed B. If they are not packed in this way, it is not possible to utilize the respective advantages of catalyst A and catalyst B while simultaneously compensating for each other's disadvantages, and a high middle distillate yield and hydrocracking activity cannot be obtained.

[0040] In the catalyst system of this embodiment, there are no limitations on the manner in which packed beds A and B are packed, so long as packed bed A is first in contact with the heavy light oil fraction that serves as the feedstock oil. However, from the viewpoint of saving space, it is preferable that they are provided in order in one reactor.

[0041] [Desulfurization / Denitrification Catalyst Layer] The catalyst system of the present embodiment may have a layer filled with a desulfurization and denitrification catalyst, that is, a desulfurization and denitrification catalyst layer, as necessary. The desulfurization / denitrification catalyst is not particularly limited as long as it is a catalyst that generally has desulfurization activity and denitrification activity, and commercially available products can be used. For example, a hydrogenation catalyst in which cobalt-molybdenum, nickel-molybdenum, or the like is supported as an active metal on an inorganic composite oxide support made of aluminum, silicon, phosphorus (e.g., diphosphorus pentasulfide, etc.) can be used.

[0042] When a desulfurization / denitrification catalyst is used, the desulfurization / denitrification catalyst bed is preferably provided so as to come into contact with the heavy gas oil fraction serving as the feedstock oil prior to the packed bed A. This improves the yield of middle distillates and hydrocracking activity, and also improves the life span of catalysts A and B, making it possible to supply the heavy gas oil fraction more cheaply and stably. In this case, the desulfurization and denitrification catalyst bed is preferably provided in a reactor separate from the packed bed A and the packed bed B from the viewpoint of maintenance and the like.

[0043] (raw oil) The feedstock oil of the catalyst system of this embodiment includes a heavy gas oil fraction. Examples of the heavy gas oil fraction include heavy gas oil (AGO), vacuum gas oil (VGO), and mixtures thereof obtained by atmospheric distillation and vacuum distillation of crude oil. In addition, the uncracked fraction (UCO) produced after hydrocracking any of heavy gas oil (AGO), vacuum gas oil (VGO), and mixtures thereof can also be used as the feedstock oil.

[0044] The properties of these feedstocks are not particularly limited as long as they contain the above-mentioned heavy gas oil fraction. For example, the density (15°C) is usually 0.800 g / cm 3 More than 1.000g / cm 3 It is sufficient if it is less than 0.820 g / cm3, preferably 0.820 g / cm3 3 More than 0.950g / cm 3 Less than or equal to 0.850 g / cm 3 More than 0.900g / cm 3The sulfur content is usually 1.0 mass% or more and 2.9 mass% or less, and preferably 1.5 mass% or more and 2.8 mass% or less, and the nitrogen content is usually 100 mass ppm or more and 1000 mass ppm or less, and preferably 300 mass ppm or more and 750 mass ppm or less. When the content is within the preferred range, the catalyst system of the present embodiment is easy to function, and the middle distillate yield and hydrocracking activity are easily improved. In addition, the distillation properties of the feedstock oil (JIS K2254:1998 (Petroleum products - Distillation test methods)), namely, the initial boiling point, 10% by volume distillation temperature, 50% by volume distillation temperature, 90% by volume distillation temperature and end point are usually 240°C or more and 290°C or less, 340°C or more and 380°C or less, 410°C or more and 450°C or less, 475°C or more and 510°C or less, and 530°C or more and 570°C or less, respectively. In the catalyst system of this embodiment, any oil having these properties and including middle distillates can be used as the feedstock oil, without being limited to the above-mentioned fractions.

[0045] The feedstock oil used in the catalyst system of this embodiment is not particularly limited as long as it contains a heavy light oil fraction, and fractions having the above properties or fractions containing intermediate distillates can also be used. However, the content of heavy light oil fraction contained in the feedstock oil is preferably 70 mass% or more, more preferably 85 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass%, i.e., it is even more preferable that the feedstock oil is a heavy light oil fraction.

[0046] (Hydrogenolysis conditions) The conditions in the catalyst system of this embodiment are as follows. By carrying out hydrocracking under the following conditions, it is possible to improve the middle distillate yield and hydrocracking activity. In the hydrocracking process, at the inlet of the feed oil, i.e., the upstream side of the packed bed A of the catalyst A, the hydrogen pressure is usually 9.0 MPa or more and 19.0 MPa or less, preferably 10.0 MPa or more and 16.0 MPa or less, more preferably 10.5 MPa or more and 13.0 MPa or less, and the LHSV is usually 0.1 h -1 Over 9.0 hours -1 Less than 0.3h, preferably-1 Over 5.0 hours -1 Less than 0.5 hours, preferably 0.5 hours -1 Over 3.0 hours -1 The reaction temperature is usually 310° C. or higher and 450° C. or lower, preferably 330° C. or higher and 420° C. or lower, more preferably 350° C. or higher and 400° C. or lower, and the hydrogen / feedstock ratio is usually 300 Nm 3 / kL or more 2000Nm 3 / kL or less, preferably 500 Nm 3 / kL or more 1800Nm 3 / kL or less, more preferably 650Nm 3 / kL or more 1500Nm 3 / kL or less, more preferably 800Nm 3 / kL or more 1300Nm 3 / kL or less, and even more preferably 900 Nm 3 / kL or more 1100Nm 3 / kL or less.

[0047] When a desulfurization / denitrification catalyst layer is provided, the nitrogen content at the outlet of the desulfurization / denitrification catalyst layer is usually adjusted to 1 mass ppm or more and 20 mass ppm or less, preferably 3 mass ppm or more and 17 mass ppm or less, and more preferably 5 mass ppm or more and 15 mass ppm or less. Note that the nitrogen content is an adjustment target, and does not necessarily have to be within the above range at all times.

[0048] When the catalyst system of this embodiment is used to hydrocrack feedstock, the temperature at the outlet of the catalyst system (also referred to as hydrocracking temperature (WAT: Weight Average Temperature)) is adjusted so that the middle distillate yield at the outlet of the catalyst system is usually in the range of 55 mass% to 70 mass%, preferably 60 mass% to 65 mass%. In this case, the hydrocracking temperature (WAT) is usually set to a low temperature of 360°C to less than 378°C, 365°C to 375°C, or 368°C to 373°C. In other words, the catalyst system of this embodiment can maintain the above-mentioned low temperatures because it achieves both a high middle distillate yield and hydrocracking activity.

[0049] [Hydrogenation cracking method] The hydrocracking method of the present embodiment is a method for hydrocracking a feedstock oil containing a heavy gas oil fraction, using the catalyst system of the present embodiment described above. The catalyst system of this embodiment employed in the hydrocracking method of this embodiment is as described above. Similarly, the catalyst system may have a desulfurization / deoxidization catalyst layer.

[0050] The feedstock oil containing a heavy gas oil fraction employed in the hydrocracking method of this embodiment is the same as the feedstock oil containing a heavy gas oil fraction described as being used in the catalyst system of this embodiment, and the hydrocracking conditions are also the same as the hydrocracking conditions described as being used in the catalyst system of this embodiment.

[0051] [Hydrocracking unit] The hydrocracker of this embodiment is equipped with the catalyst system of this embodiment described above. The catalyst system of the present embodiment employed in the hydrocracking method of the present embodiment is as described above, and may also have a desulfurization / denitrification catalyst layer. Also, it is preferable that the packed bed A of catalyst A and the packed bed B of catalyst B are packed in a single reactor, and the desulfurization / denitrification catalyst layer may be provided in a reactor other than the single reactor.

[0052] The feedstock oil that can be hydrocracked in the hydrocracking unit of this embodiment is the same as the feedstock oil containing the heavy gas oil fraction described as being used in the catalyst system of this embodiment, and the hydrocracking conditions are also the same as the hydrocracking conditions described as being used in the catalyst system of this embodiment. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0054] [Evaluation method] 1.Middle distillate yield The middle distillate yields in the examples and comparative examples were evaluated according to the following criteria. A higher middle distillate yield indicates higher catalyst performance. A rating of D is a failure. A: The yield of middle distillate was 46.0% by mass or more. B: The yield of the middle distillate was 45.8% by mass or more and less than 46.0% by mass. C: The yield of the middle distillate was 45.5% by mass or more and less than 45.8% by mass. D: The yield of the middle distillate was less than 45.5% by mass. 2. Hydrocracking activity In the examples and comparative examples, the hydrocracking temperature (WAT: Weight Average Temperature) was adjusted so that the hydrocracking rate at the outlet of the second reaction tower packed with packed bed A of catalyst A and packed bed B of catalyst B was 62 mass %. The hydrocracking temperature (WAT) was evaluated according to the following criteria. The lower the WAT, the higher the hydrocracking activity of the catalyst. D is a failure. A: The WAT was below 370℃. B: WAT was greater than 370℃ and less than 373℃. C: WAT was greater than 373℃ and less than 378℃. D: WAT was over 378°C.

[0055] ( Comparative Example 3 ) The feedstock oil used was a mixed oil containing heavy gas oil (AGO), vacuum gas oil (VGO) and uncracked oil (UCO) in a volume ratio of 4:3:3, and having the properties shown in Table 1. A first reaction tower packed with a desulfurization / denitrification catalyst and having a desulfurization / denitrification catalyst layer, and a second reaction tower packed with a packed bed A of catalyst A and a packed bed B of catalyst B in a ratio of 50 / 50 were prepared, and a bench facility for a hydrocracking unit was prepared in which these reaction towers were connected so that the mixed oil was passed through the first reaction tower and the second reaction tower in that order, and the packed bed A was passed first. Operating conditions: LHSV=1.0h -1The hydrogen partial pressure was adjusted to 11.0 MPa, the nitrogen content at the outlet of the first reactor was adjusted to 5 to 15 mass ppm, and the hydrocracking temperature (WAT: Weight Average Temperature) of the packed bed A of catalyst A and the packed bed B of catalyst B was adjusted so that the hydrocracking rate was 62 mass%. The yields of naphtha fraction (boiling point 120 ° C or less), middle fraction (boiling point 120 to 360 ° C), and uncracked oil fraction (boiling point 360 ° C or more) were measured by gas chromatographic distillation for the hydrocracked feed oil at the outlet of the second reactor. The middle fraction yield and the temperature (WAT) of the hydrocracking catalyst layer are shown in Table 2. The evaluation of the middle fraction yield and hydrocracking activity is also shown in Table 2.

[0056] [Table 1]

[0057] Example 2 Comparative Example 3 In the second reaction tower, the ratio of the packed bed A to the packed bed B was set to 70 / 30, Comparative Example 3 The yield of middle distillate and the yield of hydrocracking are shown in Table 2.

[0058] (Comparative Examples 1 and 2) Comparative Example 3 Except that the ratio of the packed bed A and the packed bed B in the second reaction tower was as shown in Table 2, Comparative Example 3 The yield of middle distillate and the yield of hydrocracking are shown in Table 2.

[0059] [Table 2]

[0060] From the results of the examples, it was confirmed that by setting the ratio of packed bed A to packed bed B within the range of 20 / 80 to 95 / 5, it is possible to achieve both a middle distillate yield and hydrocracking activity at a high level in a well-balanced manner. On the other hand, in Comparative Example 1, in which only packed bed A was used, the hydrocracking activity was high due to the characteristics of catalyst A, but the middle distillate yield was poor, while in Comparative Example 2, in which only packed bed B was used, the middle distillate yield was high due to the characteristics of catalyst B, but the hydrocracking activity was poor.

Claims

1. A catalyst system for hydrocracking a feedstock oil containing a heavy gas oil fraction, comprising: a packed bed A composed of a catalyst A having a zeolite ratio of 12 mass% or more in a catalyst carrier; and a packed bed B composed of a catalyst B having a zeolite ratio of less than 12 mass% in a catalyst carrier, the packed bed A being arranged such that the ratio (R A ) and the ratio of the filling layer B (R B ) and the volume ratio (R A / R B a ratio of the packed bed A to the heavy light oil fraction is 55 / 45 to 95 / 5; the zeolite in the carrier of the catalyst A and the catalyst B is a metal-supported USY zeolite supporting at least one metal selected from Groups 3 to 16 of the Periodic Table; the catalyst A and the catalyst B each have a Group 6 metal and a Group 8 to 10 metal as active metals, the amount of the Group 6 metal supported is 0.5 to 30 mass% of the entire catalyst, and the amount of the Group 8 to 10 metal supported is 0.1 to 20 mass% of the entire catalyst.

2. The catalyst system according to claim 1 , further comprising a desulfurization / denitrification catalyst layer provided upstream of said packed bed A so as to be in contact with said heavy gas oil fraction.

3. The catalyst system according to claim 1 or 2, wherein at least the packed bed A and the packed bed B are provided in one reactor.

4. 4. The catalyst system according to claim 3, wherein the desulfurization catalyst layer is provided in a reactor separate from the first reactor.

5. The ratio (R A / R B 5. The catalyst system according to claim 1, wherein the ratio of the benzene ring to the benzene ring is 55 / 45 to 75 / 25.

6. The catalyst system according to any one of claims 1 to 5, wherein the feedstock oil is at least one selected from the group consisting of heavy gas oil (AGO) and vacuum gas oil (VGO).

7. 7. The catalyst system of claim 6, wherein the feedstock further comprises uncracked oil (UCO).

8. A method for hydrocracking a feedstock containing a heavy gas oil fraction, using the catalyst system according to any one of claims 1 to 7.

9. A hydrocracking unit for feedstock containing a heavy gas oil fraction, comprising the catalyst system according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Exchanging of hydrocarbon oil

    JP1991181595A

  • Hydrocracking of hydrocarbon feedstock

    JP1995268363A

  • Iron-containing crystalline alumino-silicate

    JP2000086233A

  • Process for producing lubricant base oil

    JP2017066227A