Laminate, manufacturing method thereof, and soundproofing member

A laminate with a urethane foam layer and thermoplastic resin layer addresses the issue of insufficient sound insulation and rigidity in existing urethane-based materials by ensuring continuous open bubbles and specific density ranges, achieving effective soundproofing and shape retention.

JP7583580B2Active Publication Date: 2024-11-14BRIDGESTONE CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020186631
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-09
Publication Date
2024-11-14
Estimated Expiration
2040-11-09

AI Technical Summary

Technical Problem

Existing soundproofing materials using urethane foam in molds often result in closed cells, leading to insufficient sound insulation and rigidity, making it difficult to maintain shape and fix the member to noise sources.

Method used

A laminate comprising a urethane foam layer with continuous and open bubbles and a thermoplastic resin layer, with specific density and thickness ranges, ensuring rigidity and excellent soundproofing properties against high-frequency sounds.

Benefits of technology

The laminate maintains rigidity, is lightweight, and provides superior soundproofing, especially against high-frequency sounds, while maintaining shape integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583580000001
    Figure 0007583580000001
  • Figure 0007583580000002
    Figure 0007583580000002
  • Figure 0007583580000003
    Figure 0007583580000003
Patent Text Reader

Abstract

To provide a laminate that keeps rigidity, is light in weight and is particularly soundproofed against high frequency noise and a soundproof member, and a method for producing the laminate.SOLUTION: A laminate has a urethane foamed layer including continuous and opened cells and having a flow resistance of 350,000 N s / m4 or less and a density of 10 kg / m3 or more, and a thickness more than 15 mm, and a resin layer containing a thermoplastic resin. The laminate has a density of 70 kg / m3 or more, and a modulus of 0.01 N m2 or more as measured at 10 mm width.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a method for producing the same, and a soundproofing member. [Background technology]

[0002] The use of composites of resin and urethane for the purpose of sound absorption and sound insulation has been investigated. For example, Patent Document 1 discloses a sound-absorbing and cushioning material that is used primarily as a sound-absorbing and cushioning material for building interior materials and the like, such as wall materials, in which an adhesive layer is formed on one side of a synthetic resin foam sheet having sound-absorbing and cushioning properties, and a straight concave pressure distortion line is formed on the sheet. Furthermore, Patent Document 2 discloses that in order to obtain a sound-absorbing member with excellent sound-absorbing properties in the low frequency range, the rear surface of a coated porous sound-absorbing material is partially attached to a base with an attachment area ratio of 5 to 70%, and integrated with the base. Patent Document 3 discloses a method of inserting a resin and foaming urethane in a mold in order to obtain an engine cover with excellent soundproofing and vibration-proofing effects. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-210108 [Patent Document 2] Japanese Patent Application Publication No. 10-8591 [Patent Document 3] JP 2003-27958 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when urethane is foamed in a mold as in Patent Document 3, the urethane foam layer has a skin layer, and the air bubbles of the urethane foam are closed and not open, so that the sound insulation properties are not sufficient. Also, the surface of the member is a fiber sheet, a thin film, etc., so the rigidity is insufficient. When the rigidity of the member is insufficient, it is difficult to maintain the shape of the member, and the shape of the member cannot be utilized to fix the member to the housing of the noise source.

[0005] An object of the present invention is to provide a laminate and a soundproofing member that maintain rigidity, are lightweight, and have excellent soundproofing properties, particularly against high-frequency sounds, as well as a method for manufacturing said laminate, and an object of the present invention is to achieve this object. [Means for solving the problem]

[0006] <1> It has continuous and open cells, and the flow resistance is 350,000N·s / m 4 and density is 10kg / m 3 A urethane foam layer having a thickness of more than 15 mm; A resin layer containing a thermoplastic resin; and has a density of 70 kg / m 3 or more, and the modulus measured at a width of 10 mm is 0.01 N m 2 The laminate is as described above.

[0007] <2> The thickness of the urethane foam layer is 50 mm or less. <1> The laminate according to claim 1. <3> The thickness is 20 to 55 mm. <1> or <2> The laminate according to claim 1. <4> The surface density of the resin layer is 0.15 to 0.50 g / cm 2 is <1> ~ <3> 13. The laminate according to claim 12 . <5> The density of the laminate is 250 kg / m 3 is less than or equal to <1> ~ <4> 13. The laminate according to claim 12 . <6> The thermoplastic resin includes at least one selected from the group consisting of polyamide-based thermoplastic resins and polyolefin-based thermoplastic resins. <1> ~ <5> 13. The laminate according to claim 12 . <7> The urethane foam layer is adjacent to the resin layer. <1> ~ <6> 13. The laminate according to claim 12 .

[0008] <8> <1> ~ <7> 13. A soundproofing member using the laminate according to any one of claims 1 to 12.

[0009] <9> A method for manufacturing a laminate, comprising the steps of placing a urethane slab in a mold having a gate, clamping the mold, and then injecting a thermoplastic resin into the mold to form a resin layer containing the thermoplastic resin while simultaneously bonding the resin layer and a urethane foam layer. Effect of the Invention

[0010] According to the present invention, it is possible to provide a laminate and a soundproofing member that maintain rigidity, are lightweight, and have excellent soundproofing properties, particularly against high-frequency sounds, as well as a method for producing the laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] <Laminate> The laminate of the present invention has continuous and open cells and a flow resistance of 350,000 N·s / m 4 and density is 10kg / m 3 or more, comprising a urethane foam layer having a thickness of more than 15 mm and a resin layer containing a thermoplastic resin, and having a density of 70 kg / m 3 or more, and the modulus measured at a width of 10 mm is 0.01 N m 2 That's all. The laminate of the present invention may have layers other than the urethane foam layer and resin layer of the above-mentioned configuration, but from the viewpoint of suppressing peeling between the layers in high temperature and high humidity environments, it is preferable that the urethane foam layer is adjacent to the resin layer. The laminate of the present invention has continuous and open cells and a flow resistance of 350,000 N·s / m 4 and density is 10kg / m 3By providing a urethane foam layer having a thickness of more than 15 mm, the product has excellent soundproofing properties against high-frequency sounds. In addition, by providing a resin layer containing a thermoplastic resin, the product can maintain rigidity while being lightweight, and has a density of 70 kg / m 3 or more, and the modulus of the laminate measured at a width of 10 mm is 0.01 N m 2 That's all.

[0012] (Modulus) The modulus of the laminate measured over a width of 10 mm was 0.01 N m 2 That's all. In order to further improve the rigidity of the laminate, the modulus of the 10 mm wide laminate is 0.02 N m 2 It is preferable that the value is equal to or greater than 0.03 N·m. 2 More preferably, it is equal to or greater than this. There is no particular upper limit for the modulus of the laminate, but it is usually 0.07 N m 2 It is preferable that the value is less than 0.06 N·m. 2 It is more preferable that: The modulus of the laminate can be measured by the following method.

[0013] The laminate is cut into test pieces 100 mm long and 10 mm wide. After cutting out the resin layer by grinding, the urethane can be cut with a blade, or it can be cut out all at once using a water jet. The end of the resin layer of the test piece is clamped and fixed with metal fittings such as clips, and the test piece is placed with the resin layer facing up on a three-point bending jig (compliant with JIS K7171 (2010)) set with a support distance of L = 105 mm, and a three-point bending test is performed by applying force with an indenter to the surface of the resin layer of the test piece. The stiffness can be calculated from the slope of the test force and displacement. The modulus of the laminate (EI) [N·mm] is calculated from the load applied by the indenter (W) [N], the deflection of the test piece (δ) [mm], and the support distance (L) [mm] using the following formula: 2 ] can be calculated. EI = [(ΔW / Δδ) × L 3 〕 / (48) Note that ΔW / Δδ is calculated from the initial slope of the three-point bending test.

[0014] (density) The laminate has a density of 70 kg / m 3 That's all. The density of the laminate (ρL) is 70 kg / m 3 If it is less than this, the laminate cannot obtain sufficient rigidity. The density of the laminate is 75 kg / m 3 It is preferable that the resistance is 85 kg / m or more. 3 More preferably, the density of the laminate is 250 kg / m or more. 3 The following is the result. The density of the laminate can be measured by a method in accordance with JIS K 7112 (1999).

[0015] (Thickness) The thickness (TL) of the laminate is preferably 20 to 55 mm. When the thickness of the laminate is 20 mm or more, the rigidity of the laminate can be further improved, and when the thickness is 55 mm or less, the laminate can be made lighter. The thickness of the laminate is more preferably 22 mm or more, and even more preferably 25 mm or more, and more preferably 50 mm or less, and even more preferably 45 mm or less.

[0016] (area density) The surface density of the laminate is 0.17 to 0.70 g / cm 2 It is preferable that: The surface density (ρAL) of the laminate is 0.17 g / cm 2 By setting the value at or above 0.70g / cm3, soundproofing against high frequency sounds can be improved. 2 By keeping the weight below 100g, the increase in mass can be suppressed. The surface density of the laminate is 0.20 g / cm 2 More preferably, it is 0.22 g / cm or more. 2 It is more preferable that the surface density of the laminate is 0.60 g / cm or more. 2 More preferably, it is 0.55 g / cm or less. 2It is even more preferable that: The surface density of the laminate can be measured with a scale after it has been processed into a predetermined shape using a punching blade or the like.

[0017] [Urethane foam layer] The urethane foam layer has open, continuous cells and a flow resistance of 350,000 N·s / m 4 and density is 10kg / m 3 or more and has a thickness of more than 15 mm. When the air bubbles in the urethane foam layer are continuous and open, the urethane foam layer is likely to absorb high-frequency sounds. When the air bubbles are, for example, cylindrical holes, one side of the holes may be open, or the entire holes may be open, and from the viewpoint of enhancing the soundproofing effect, it is preferable that the entire holes are open. However, when the urethane foam layer is adjacent to, for example, a resin layer, the air bubbles on the resin layer side of the urethane foam layer are usually not open.

[0018] (flow resistance) Flow resistance is an index that indicates the difficulty of air flow through the urethane foam layer, and is 350,000N·s / m 4 If it exceeds this value, the soundproofing effect against high frequency sounds cannot be achieved. In order to further improve the soundproofing effect of the laminate against high frequency sounds, the flow resistance of the urethane foam layer is set to 300,000N·s / m 4 Preferably less than 200,000N·s / m 4 More preferably, it is 100,000 N·s / m 4 It is even more preferable that: The lower limit of the flow resistance of the urethane foam layer is not particularly limited, but is preferably 500 N·s / m 4 More than 800N·s / m is preferable. 4 More preferably, it is 1,000N·s / m 4 More preferably, it is equal to or greater than this. The flow resistance can be measured, for example, by a flow resistance measuring device manufactured by Nihon Onkyo Engineering Co., Ltd. In the manufacture of the laminate, the flow resistance of the urethane slab used as the raw material for the urethane foam layer and the flow resistance of the urethane foam layer of the manufactured laminate usually remain the same and are equivalent to each other.

[0019] (Thickness) The thickness (Tu) of the urethane foam layer is greater than 15 mm. If the thickness of the urethane foam layer is less than 15 mm, the soundproofing effect against high frequency sounds cannot be improved. The thickness of the urethane foam layer is preferably 50 mm or less in order to make the laminate lighter. The thickness of the urethane foam layer is more preferably 17 mm or more, and even more preferably 20 mm or more, and more preferably 45 mm or less, and even more preferably 40 mm or less.

[0020] (density) The density of the urethane foam layer (ρu) is 10 kg / m 3 That's all. The density of the urethane foam layer is 10 kg / m 3 If the density is less than 90 kg / m, the soundproofing effect against high frequency sounds cannot be improved. There is no particular upper limit to the density, but from the viewpoint of suppressing an increase in the mass of the laminate, it is preferable that the density is 90 kg / m 3 It is preferable that: The density of the urethane foam layer is 17kg / m 3 More preferably, it is 20 kg / m or more. 3 It is more preferable that the density of the urethane foam layer is 85 kg / m or more. 3 More preferably, it is 80 kg / m or less. 3 It is even more preferable that: The density of the urethane foam layer can be measured by a method conforming to the apparent density measuring method of JIS K7222 (2005).

[0021] (shear modulus) The shear modulus (E) of the urethane foam layer is 300,000N / m2 It is preferable that: The shear modulus of the urethane foam layer is 300,000N / m 2 By keeping the shear modulus at 50 N / m or less, the soundproofing effect against high frequency sounds can be improved. There is no particular lower limit for the shear modulus, but it is usually 50 N / m 2 That's all. The shear modulus of the urethane foam layer is 60,000N / m 2 More preferably, it is 70,000N / m or more. 2 The shear modulus of the urethane foam layer is more preferably 250,000 N / m or more. 2 More preferably, it is equal to or less than 200,000 N / m 2 It is even more preferable that: The shear modulus of elasticity of the urethane foam layer can be measured using an elasticity measuring system manufactured by Nihon Onkyo Engineering Co., Ltd., and the elasticity is measured from the vibration transmission characteristics by vibrating the sample while applying a shear force. In addition, in producing the laminate, the shear modulus of elasticity of the urethane slab used as the raw material of the urethane foam layer and the shear modulus of elasticity of the urethane foam layer of the produced laminate usually do not change and are equivalent to each other.

[0022] (Number of cells) The urethane foam layer preferably has a cell number of 20 to 80 cells / 25 mm. A cell count of 20 cells / 25 mm or more can improve the soundproofing effect against high frequency sounds, while a cell count of 80 cells / 25 mm or less can suppress a decrease in rigidity. The number of cells in the urethane foam layer is preferably 25 cells / 25 mm or more, more preferably 30 cells / 25 mm or more, and more preferably 65 cells / 25 mm or less, and even more preferably 60 cells / 25 mm or less. The cell number of the urethane foam layer can be measured by the method described in Appendix 1 of JIS K6400-1 (2004).

[0023] (porosity) The porosity of the urethane foam layer is preferably 0.90 or more. When the porosity of the urethane foam layer is 0.90 or more, the soundproofing effect against high frequency sounds can be improved. The porosity is usually less than 1.00. The porosity of the urethane foam layer is more preferably 0.92 or more, and further preferably 0.95 or more. The porosity of the urethane foam layer is expressed as the volume of the voids, V V , the bulk volume is VT, and the porosity is Φ=V V / V T However, this can be easily calculated from the true density and bulk density of the input material. In the production of the laminate, the porosity of the urethane slab used as the raw material for the urethane foam layer is usually the same as the porosity of the urethane foam layer of the produced laminate.

[0024] (area density) The surface density of the urethane foam layer (ρAu) is 0.01 to 0.30 g / cm 2 It is preferable that: When the surface density of the urethane foam layer is within the above range, the sound absorbing performance can be improved. The surface density of the urethane foam layer is 0.02 g / cm 2 More preferably, it is 0.03 g / cm or more. 2 It is more preferable that the surface density of the urethane foam layer is 0.27 g / cm or more. 2 More preferably, it is 0.25 g / cm or less. 2 It is even more preferable that: The surface density of the urethane foam layer can be calculated by cutting it to a fixed length and measuring it with a scale or the like.

[0025] The urethane foam may be an ether-based urethane foam or an ester-based urethane foam. The term "ether-based urethane" refers to a urethane in which the main component of the polyol constituting the urethane (80 mol % or more of the total polyol) is a polyether polyol. The term "ester-based urethane" refers to a urethane in which the main component of the polyol constituting the urethane (80 mol % or more of the total polyol) is a polyester polyol. From the viewpoint of water resistance and moisture resistance, the urethane foam is preferably an ether-based urethane foam. In the ether-based urethane, the polyol may contain an ester group, but the ester group content in the total polyol is preferably 20 mol% or less. The polyol may be a single polyether polyol, or a mixture of one or more polyols other than polyether polyols.

[0026] In the present invention, the urethane foam can be obtained, for example, by using water as a blowing agent in a urethane synthesis reaction, which reacts with polyisocyanate to generate carbon dioxide. In order to obtain continuous and open cells, the urethane foam may be sufficiently expanded and then cut in the thickness direction. Flow resistance of 350,000N·s / m 4 To achieve this, the thickness of the urethane can be increased or the number of cells can be reduced. The density of the urethane foam is 10 kg / m 3 In order to achieve the above amount, the amount of water added to the urethane synthesis reaction may be appropriately adjusted. It also has continuous and open bubbles, and the flow resistance is 350,000N·s / m 4 and density is 10kg / m 3 As described above, a commercially available urethane foam having a thickness of more than 15 mm may be used.

[0027] [Resin Layer] The resin layer includes a thermoplastic resin. The laminate of the present invention has excellent rigidity due to the inclusion of a resin layer. The resin layer can be obtained, for example, by melt-kneading a resin composition containing a thermoplastic resin and molding the mixture in a mold. From the viewpoint of further improving the soundproofing effect against high frequency sounds, the resin layer may be a foamed resin layer.

[0028] (density) The density of the resin layer (ρr) is 300 to 2000 kg / m 3 It is preferable that the density is 300 kg / m 3 If the density is 2000 kg / m or more, the rigidity of the laminate can be further improved. 3 If the density is less than 1000 kg / m, the sound absorbing effect is not easily affected. 3 More preferably, it is 1200 to 1800 kg / m 3 It is more preferable that:

[0029] (thermoplastic resin) Examples of the thermoplastic resin include polyolefin-based thermoplastic resins, polystyrene-based thermoplastic resins, polyamide-based thermoplastic resins, and polyester-based thermoplastic resins. Examples of the polyolefin-based thermoplastic resin include polyethylene resin, polypropylene resin (propylene homopolymer), random copolymer or block copolymer of propylene and α-olefin, etc. Examples of the α-olefin include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, etc. Examples of the polystyrene-based thermoplastic resin include polystyrene, AS resin, ABS resin, and PMMA resin. Examples of the polyamide-based thermoplastic resin include polyamide 6, polyamide 66, polyamide 666, polyamide 11, polyamide 12, and the like. Examples of the polyester-based thermoplastic resin include polyethylene terephthalate, polybutylene terephthalate, and polyacrylate. The thermoplastic resin may be used alone or in combination of two or more kinds.

[0030] Among the above, from the viewpoints of rigidity and versatility, the thermoplastic resin preferably includes one or more selected from the group consisting of polyamide-based thermoplastic resins and polyolefin-based thermoplastic resins, more preferably includes one or more selected from the group consisting of polyamide-based thermoplastic resins and polypropylene resins, and further preferably is a polyamide-based thermoplastic resin.

[0031] From the viewpoint of further improving the rigidity of the laminate, the thermoplastic resin has a polystyrene-equivalent number average molecular weight (Mn) of preferably 5,000 to 10,000,000, more preferably 7,000 to 1,000,000, and further preferably 10,000 to 1,000,000. The number average molecular weight is measured, for example, by gel permeation chromatography using a refractometer as a detector, and is calculated in terms of polystyrene using monodisperse polystyrene as the standard. From the viewpoint of suppressing thermal decomposition of the thermoplastic resin, the melting point of the thermoplastic resin is preferably 250° C. or lower. The melting point of the thermoplastic resin is usually 120° C. or higher. The melt flow rate (MFR) of the thermoplastic resin is preferably 1 to 40 g / 10 min, and more preferably 5 to 30 g / 10 min, at 190° C. and a load of 2.16 kg, from the viewpoints of rigidity and ease of production of the laminate. The MFR may be measured according to a method conforming to JIS K7210-1 (2014).

[0032] The composition containing a thermoplastic resin may contain modifiers such as foaming agents, extenders, colorants, ultraviolet absorbers, antioxidants, fire retardants, antifungal agents, plasticizers, coupling agents, electrically conductive fillers, magnetic fillers, thermally conductive fillers, antistatic agents, and elastic fine particles, as necessary.

[0033] (area density) The surface density (ρAr) of the resin layer is 0.15 to 0.80 g / cm 2 It is preferable that: The surface density of the resin layer is 0.15 g / cm 2By setting the value to 0.50g / cm or more, rigidity can be ensured. 2 By satisfying the above condition, a lightweight laminate can be obtained. The surface density of the resin layer is 0.20 g / cm 2 The surface density of the resin layer is preferably 0.50 g / cm or more. 2 More preferably, it is 0.30 g / cm or less. 2 It is even more preferable that: The surface density of the resin layer can be calculated by subtracting the surface density of the urethane to be added from the surface density of the laminate. The surface density of the laminate can be calculated by cutting the laminate to a fixed size, weighing it, and then performing the calculation.

[0034] (Thickness) The thickness (Tr) of the resin layer is preferably 0.50 to 5.00 mm. When the thickness of the resin layer is 0.50 mm or more, the rigidity of the laminate can be further improved, and when the thickness is 5.00 mm or less, the laminate can be made lighter. The thickness of the resin layer is more preferably 0.85 mm or more, and even more preferably 1.10 mm or more, and more preferably 3.20 mm or less, and even more preferably 2.80 mm or less.

[0035] <Method of manufacturing laminate> The method for producing the laminate of the present invention is not particularly limited as long as it is a method capable of laminating the above-mentioned urethane foam layer and resin layer. However, it is preferable that the urethane foam layer and the resin layer are not laminated via an adhesive or a pressure sensitive adhesive, and the urethane foam layer is laminated adjacent to the resin layer. By laminating the urethane foam layer adjacent to the resin layer, the urethane foam layer and the resin layer are unlikely to peel off even if the laminate is placed in a high temperature environment, a high humidity environment, or the like. The laminate in which the urethane foam layer is laminated so as to be adjacent to the resin layer can be produced, for example, by the following method.

[0036] This manufacturing method involves placing a urethane slab in a mold having a gate, closing the mold, and then injecting thermoplastic resin into the mold to form a resin layer containing the thermoplastic resin while simultaneously bonding the resin layer and the urethane foam layer.

[0037] The mold is a container-like metal mold that fits together, and usually has a convex upper mold (core) and a concave lower mold (cavity). Either the upper mold or the lower mold has a gate that can inject molten resin into the cavity. The gate is preferably connected to a cylinder that can melt-knead a resin composition containing a thermoplastic resin. The gate is connected to a locating ring via a runner and a sprue, and is connected to the nozzle of the cylinder of the injection molding machine by the locating ring. In order to control the thickness of the resin layer, a spacer may be provided in the concave mold, or may be of a nesting type that can be easily replaced. A spacer may also be provided on the pressure receiving part. In addition, an ejector may be provided on the lower mold so that the manufactured laminate can be easily removed from the mold.

[0038] It is preferable to heat the upper and lower dies in advance before placing the urethane slab in the die. When the temperature of the die on the urethane side is Tu and the temperature of the die on the side on which the resin layer is formed is Tr, Tr and Tu differ depending on the type of molten resin to be injected, but for example, Tr may be set to 40 to 100°C and Tu may be set to 20 to 80°C.

[0039] Typically, a urethane slab is placed inside a lower mold (cavity) that has a gate. The urethane slab has continuous and open cells and a flow resistance of 350,000N·s / m 4 The following urethane foam may be processed into a slab (block) of the desired shape. The shape of the urethane slab is usually the same as the bottom shape of the lower mold (cavity), but it may be a shape that covers part of the bottom shape of the cavity. The thickness of the urethane slab may be in the same range as the thickness of the urethane foam layer of the laminate.

[0040] Next, the upper die is lowered or the lower die is raised to perform clamping. At this time, it is preferable that the die is maintained at a predetermined cavity distance (L0). The cavity interval (L0) can be adjusted by controlling the size of the spacer. The cavity interval (L0) differs depending on the mass of the urethane slab and the mass of the molten resin, but may be set to, for example, 0.5 to 3.5 mm.

[0041] After the mold is closed, a thermoplastic resin is injected into the mold. Specifically, it is preferable to inject a resin composition containing a thermoplastic resin molten at a predetermined cylinder temperature (Ts) into the mold from a gate at a predetermined injection speed (v) while the mold is completely closed. Then, it is preferable to apply a holding pressure (P) to the molten resin to fill the mold with the resin, and to cool and hold it in this state for a predetermined cooling time (Tc). Here, the cylinder temperature (Ts) may vary depending on the melting point of the thermoplastic resin, but may be, for example, 150 to 250° C. The injection speed (v) may be, for example, 10 to 80 mm / s, and the holding pressure (P) may be, for example, 3 to 50 MPa. The cooling time (Tc) may vary depending on the size of the molded product, but may be, for example, 10 to 150 seconds.

[0042] Next, the upper die is slowly raised or the lower die is slowly lowered to remove the molded product (laminate) from the metal mold. The molded product may be removed using an ejector or by utilizing the end or protrusion of the molded product.

[0043] <Soundproofing materials> The soundproofing material of the present invention is formed using the laminate of the present invention. Therefore, the soundproofing material of the present invention maintains its rigidity and has excellent soundproofing properties against high frequency sounds. The soundproofing material of the present invention is suitable for parts, products, etc. that require rigidity and soundproofing against high-frequency sounds. Examples of such parts include vehicle parts, building parts, etc. As an example of a vehicle part, the soundproofing material can be used for an engine cover. EXAMPLES

[0044] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0045] <Material> 1. Urethane slab As a material for forming a urethane foam layer, a urethane slab having the properties shown in Table 1 was prepared. Urethane 1 to Urethane 3 in Table 1 are the following products. The properties of Urethane 1 to Urethane 3 shown in Table 1 are the values ​​listed in the manufacturer's specifications.

[0046] Urethane 1: Ether-based urethane foam, Bridgestone polyurethane foam "TP" Urethane 2: Ether-based urethane foam, Bridgestone polyurethane foam "VO" Urethane 3: Ether-based urethane foam, Bridgestone polyurethane foam "DO"

[0047] Urethane 4 to Urethane 5 in Table 1 are virtual urethane slabs obtained by simulation. The properties of Urethane 4 to Urethane 5 shown in Table 1 are the set values ​​used in the simulation. The simulation was performed using laminated structure acoustic characteristic prediction software, product name "STRATI-ARTZ", manufactured by Nihon Acoustic Engineering Co., Ltd.

[0048] [Table 1]

[0049] 2.Thermoplastic resin As a material for forming a resin layer, the following thermoplastic resin was prepared. PA: Polyamide thermoplastic resin, polyamide 6, manufactured by Unitika Ltd., product name "UBE Unitika Nylon A3130"

[0050] <Manufacture of Laminate> Example 1 A container-like mold having a convex upper mold (core) and a concave lower mold (cavity) that fit together is used. The bottom surface of the lower mold has a gate that can inject molten resin into the cavity. A cylinder that can melt and knead a resin composition containing a thermoplastic resin is connected to the gate. The gate is connected to a locating ring via a runner and a sprue, and is connected to the nozzle of the cylinder of the injection molding machine by the locating ring.

[0051] Cut the urethane slab (urethane 1) to a length of 200 mm, width of 200 mm, and thickness of 30 mm, and place the urethane slab in the center of the lower mold (cavity). With the mold completely closed, the cylinder temperature (Ts) is set to 180°C and molten polyamide thermoplastic resin (PA) is injected from the gate into the lower mold. After that, a low dwell pressure (P) is applied to the molten resin to fill the mold so that the thickness of the urethane layer in the laminate after molding is the value shown in Table 2. In this state, it is cooled and held for 60 seconds. After the thermoplastic resin has hardened, the upper die is slowly raised and the molded product is removed. In this manner, the molded article (laminate 1) of Example 1 is produced. The laminate 1 is a two-layered body consisting of a resin layer of a polyamide thermoplastic resin (PA) and a urethane foam layer of a urethane 1.

[0052] [Examples 2 to 4] Except for changing the type of thermoplastic resin and the type of urethane slab as shown in Table 2, the laminates of Examples 2, 3, and 4 were manufactured in the same manner as Example 1 so that the thickness of the urethane layer in the laminate after molding would be the value shown in Table 2. The laminate 2 is a two-layered body consisting of a resin layer of a polyamide thermoplastic resin (PA) and a urethane foam layer of urethane 2. The laminate 3 is a two-layered body consisting of a resin layer of polyamide thermoplastic resin (PA) and a urethane foam layer of urethane 3. Laminate 4 is a two-layered body consisting of a resin layer of polyamide thermoplastic resin (PA) and a urethane foam layer of urethane 2, but differs from laminate 2 in that the resin layer is thicker.

[0053] Comparative Example 1 In Comparative Example 1, a molded article 101 was produced that had only a resin layer without a urethane foam layer. Molded product 101 was produced under the same conditions as those set in Example 3, without using a urethane slab. The molded article 101 is a single layer body made of a resin layer of polyamide thermoplastic resin (PA).

[0054] Comparative Example 2 As the molded article 102 of Comparative Example 2, a single layer body consisting of a urethane foam layer of Urethane 2 was used.

[0055] [Comparative Examples 3 to 6] Except for changing the type of thermoplastic resin and the type of urethane slab to those shown in Table 2, laminates 103 to 106 of Comparative Examples 3 to 6 were manufactured in the same manner as in Example 1 so that the thickness of the urethane layer in the laminate after molding would be the value shown in Table 2.

[0056] Table 2 shows the thickness configuration, surface density and density of the laminates or molded articles of the examples and comparative examples. The areal density of the molded products of Comparative Examples 1 and 2 was measured by cutting the molded products to a fixed size and then weighing them. The areal density of the laminates of the other Examples and Comparative Examples was estimated from the type of resin, the type of urethane, and the thickness of the resin and urethane after pressing.

[0057] [Table 2]

[0058] <Evaluation> The soundproofing properties, modulus and rigidity of the laminates and molded articles of the Examples and Comparative Examples were confirmed by the following methods. The results are shown in Table 3.

[0059] 1. Soundproofing evaluation (measurement using a sound-absorbing box) The molded articles 101 and 102 of Comparative Examples 1 and 2 were used as test specimens. A sound-absorbing box measuring 500 mm x 800 mm x 700 mm in height and with one side open was placed with the opening facing up, and a speaker was placed inside the sound-absorbing box. The opening of the sound-absorbing box was then blocked with a board having a 200 mm x 200 mm opening in the center. At this time, the position of the board was adjusted so that the opening was directly above the speaker. Furthermore, the opening of the board was blocked with a test specimen, and the gap was blocked with tape. The laminate and molded product having a urethane foam layer had the urethane foam layer side facing the speaker, and the molded product 101 without a urethane foam layer had the resin layer facing the speaker. A microphone was placed outside the sound-absorbing box, 20 cm away from the test specimen, and sound (4 kHz) was emitted from a speaker, and the intensity of the sound detected by the microphone was measured. The sound intensity when there is no test object is I 0 The sound intensity when the test specimen is present is I S The transmission loss (sound-absorbing box, 200 mm) was calculated using the following formula. Transmission loss (sound absorption box, 200mm) = 10Log(I S / I 0 ) The transmission losses of the laminates of Examples 1 to 4 and Comparative Examples 3 to 6 were estimated from the above measured data.

[0060] The larger the transmission loss value, the better the soundproofing properties. The results of the transmission loss (sound-absorbing box, 200 mm) of 47.0 dB or more were evaluated as ○ (good), and the results of less than 47.0 dB were evaluated as × (bad). These are shown in Table 3.

[0061] 2.Mass The molded products of Comparative Examples 1 and 2 were processed into a circle having a diameter of 40 mm, and the masses were measured. The results are shown in Table 3. The masses of the laminates in Examples 1 to 4 and Comparative Examples 3 to 6 were calculated based on the set values ​​in the simulation. The results are shown in Table 3 as follows: a mass of 5.5 g or less is rated as ○ (good); a mass of more than 5.5 g and less than 10.0 g is rated as △ (acceptable range); and a mass of more than 10.0 g is rated as × (bad).

[0062] 3. Modulus of laminate or molded product The molded articles of Comparative Examples 1 and 2 were cut to a width of 10 mm, and the modulus was measured by the following method. The molded product was cut into test pieces measuring 100 mm in length and 10 mm in width. The pieces were cut using a water jet. The end of the resin layer of the test piece was clamped and fixed with metal fittings such as clips, and the test piece was placed with the resin layer facing up on a three-point bending jig (compliant with JIS K7171 (2010)) set with a support distance of L = 105 mm, and a three-point bending test was performed by applying force to the surface of the resin layer of the test piece with an indenter. The rigidity was calculated from the slope of the test force and displacement. The modulus (EI) of the molded product [N·mm] was calculated using the load applied by the indenter (W) [N], the deflection of the test piece (δ) [mm], and the support distance (L) [mm] using the following formula: 2 ] was calculated. EI = [(ΔW / Δδ) × L 3 〕 / (48) Note that ΔW / Δδ was calculated from the initial inclination in the three-point bending test. The moduli of the laminates of Examples 1 to 4 and Comparative Examples 3 to 6 were estimated from the above measured data.

[0063] 4. Rigidity evaluation The rigidity evaluation was carried out on the laminate and molded article having the resin layer. The molded products 101 and 102 of Comparative Examples 1 and 2 were given projections and recesses to fix the shapes, and an evaluation of whether the shapes could be sufficiently maintained is shown in Table 3. In addition, for the other laminates and molded products, calculations were performed using the set values ​​of the simulation, and the evaluations were inferred from the test results of the molded products 101 and 102, and are shown in Table 3. ○: Sufficient shape retention and good rigidity ×: Shape cannot be sufficiently maintained, and rigidity is poor.

[0064] The modulus (EI) [N mm] was calculated from the load (W) [N] applied by the indenter, the deflection (δ) [mm] of the test piece, and the distance between supports (L) [mm] using the following formula: 2 ] was calculated. EI = [(ΔW / Δδ) × L 3 〕 / (48) In addition, ΔW / Δδ is calculated from the slope of the three-point bending test.

[0065] 5. Overall Judgment In the results of the transmission loss, mass, 10 mm width modulus, and stiffness evaluation, cases in which an x ​​rating was given were judged as x (bad) overall, and cases in which no x rating was given were judged as o (good) overall. The results are shown in Table 3.

[0066] [Table 3]

[0067] As can be seen from Table 3, the material has continuous and open cells and a flow resistance of 350,000 N·s / m 4 and density is 10kg / m 3 The laminate of the embodiment having a urethane foam layer having a thickness of more than 15 mm and a resin layer containing a thermoplastic resin has a density of 70 kg / m 3 or more, and the modulus measured at a width of 10 mm is 0.01 N m 2 As described above, the transmission loss is larger than that of the molded product of the comparative example, the soundproofing is excellent, the light weight is maintained, and the rigidity is excellent. [Industrial Applicability]

[0068] The laminate of the present invention maintains rigidity, is lightweight, and has excellent soundproofing properties, particularly against high-frequency sounds, and is therefore suitable for use as vehicle parts and building parts, and is particularly suitable for use as soundproof covers and engine covers.

Claims

1. It has continuous and open cells and a flow resistance of 350,000 N.s / m 4 The following urethane foam: A resin composition containing a thermoplastic resin; A laminate having a urethane foam layer and a resin layer, The density of the laminate is 70 kg / m 3 More than 250kg / m 3 The modulus measured at a width of 10 mm is 0.01 N m or less. 2 That's all. The thickness of the urethane foam layer of the laminate is 30 mm or more, The density of the urethane foam layer of the laminate is 10 kg / m 3 That's all. The modulus measured over a width of 10 mm was calculated by placing a test piece cut out from the laminate to a length of 100 mm and a width of 10 mm, with the resin layer facing up, on a three-point bending jig with a support distance set to 105 mm, and applying force with an indenter to the surface of the resin layer of the test piece to perform a three-point bending test.

2. 2. The laminate according to claim 1, wherein the urethane foam layer of the laminate has a thickness of 50 mm or less.

3. 3. The laminate according to claim 1 or 2, which has a thickness of 55 mm or less.

4. The surface density of the resin layer is 0.15 to 0.50 g / cm 2 The laminate according to any one of claims 1 to 3, wherein

5. The laminate according to any one of claims 1 to 4, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyamide-based thermoplastic resins and polyolefin-based thermoplastic resins.

6. The laminate according to any one of claims 1 to 5, wherein the urethane foam layer of the laminate is adjacent to the resin layer of the laminate.

7. A soundproofing material using the laminate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Sheet frame and its manufacture

    JP1981027331A

  • Sound-absorption member

    JP1998008591A

  • Composite molding with excellent sound absorbing qualities and its manufacture

    JP1998264339A

  • Sound absorbing / Cushioning material

    JP1999210108A

  • Thin layer laminate with sound absorption

    JP2002505209A