Manufacturing method of semiconductor single crystal and manufacturing apparatus of semiconductor single crystal

By applying periodic fluctuations to the pulling speed synchronized with heater output fluctuations, the method stabilizes the V/G ratio, addressing the challenge of inconsistent quality in semiconductor single crystal production, achieving a high non-defective yield of 83%.

JP7583599B2Active Publication Date: 2024-11-14GLOBALWAFERS JAPAN
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020205347
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-10
Publication Date
2024-11-14
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

Existing methods for controlling the ratio of pulling speed to temperature gradient (V/G) in the Czochralski method are inadequate due to fluctuations in the temperature gradient, which are difficult to measure accurately and adjust in real-time, leading to inconsistent crystal quality.

Method used

A method and apparatus that apply periodic fluctuations to the pulling speed, synchronized with opposite-phase fluctuations in the heater output, with a controlled delay time, to stabilize the temperature gradient and maintain a constant V/G ratio, using a Czochralski method.

Benefits of technology

This approach enables the production of semiconductor single crystals with stable quality by effectively controlling the V/G ratio, reducing defects and improving the non-defective yield to 83% compared to conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583599000001
    Figure 0007583599000001
  • Figure 0007583599000002
    Figure 0007583599000002
  • Figure 0007583599000003
    Figure 0007583599000003
Patent Text Reader

Abstract

To provide a manufacturing method for semiconductor single crystal and a manufacturing apparatus for semiconductor single crystal that control a ratio of a lifting speed and a temperature gradient in a lifting process by a simple and highly versatile method.SOLUTION: There is provided a manufacturing method for semiconductor single crystal that employs a Czochralski method to lift a single crystal from a melt of a raw material while rearing it, and the manufacturing method comprises: using a heater to heat the melt so that the single crystal has its diameter kept constant; and imparting period variation which is equal in period to and opposite in phase from period variation TH of output of the heater to a lifting speed at which the single crystal is lifted. There is provided a manufacturing apparatus for semiconductor single crystal that lifts the single crystal from a melt of a raw material while rearing it, and the manufacturing apparatus comprises: a lifting machine which lifts the single crystal; the heater which heats the melt so that the diameter of the single crystal is kept constant; and a control part which imparts period variation equal in period to and opposite in phase from the period variation TH of the output of the heater to the lifting speed of the lifting machine.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing a semiconductor single crystal. [Background technology]

[0002] The Czochralski method is a typical method for manufacturing silicon single crystals (so-called silicon ingots) for semiconductor devices. When growing silicon ingots using the Czochralski method, defect-free single crystals are required, but the manufacturing conditions under which defect-free single crystals can be manufactured are extremely narrow. Examples of these manufacturing conditions include the ratio of the pulling speed and the temperature gradient.

[0003] The temperature gradient is the temperature change per unit length in the height direction of a single crystal near the solid-liquid interface, and the pulling speed is the speed at which the single crystal is pulled up. When the pulling speed is V and the temperature gradient is G, the defects formed during the production of a single crystal change sensitively depending on the ratio (V / G) of the pulling speed V to the temperature gradient G. For example, if the ratio (V / G) of the pulling speed V to the temperature gradient G is too large, vacancy type defects (void defects) are formed, and conversely, if the ratio (V / G) of the pulling speed V to the temperature gradient G is too small, interstitial silicon type defects (dislocation loops) are formed.

[0004] Therefore, in order to obtain single crystals of stable quality, it is necessary to control the ratio (V / G) of the pulling speed V to the temperature gradient G with high precision (see, for example, Patent Document 1). Since the pulling speed V can be precisely controlled mechanically, a common method for producing single crystals is to control the pulling speed V to be constant in order to achieve both stable crystal quality and planned production (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-337490 [Patent Document 2] Japanese Patent Application Publication No. 5-43386 [Patent Document 3] JP 2000-327486 A [Patent Document 4] JP 2000-281478 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the pulling speed V is controlled to be constant, the quality can vary in the crystal length direction. This is because the temperature gradient G during the pulling process is not constant but fluctuates. Although the temperature gradient G has been predicted by heat transfer calculations (see, for example, Patent Document 3), the temperature situation during the actual pulling process fluctuates from time to time due to various factors, making it difficult to achieve real-time control.

[0007] For this reason, some efforts have been made to measure the temperature gradient G using a temperature sensor (see, for example, Patent Document 4), but in reality, there are problems with large individual differences in the detection sensitivity of temperature sensors, and large differences in the dislocation rate between devices. In addition, since it is necessary to install a new sensor unit, there are also cases where the temperature measurement location cannot be adjusted depending on the installation method, resulting in limited flexibility in application. For this reason, it remains difficult to control V / G during the pulling process.

[0008] An object of the present invention is to provide a method for producing a semiconductor single crystal and an apparatus for pulling a semiconductor single crystal, in which the ratio (V / G) of the pulling speed V to the temperature gradient G during the pulling process is controlled in a simple and versatile manner. [Means for solving the problem]

[0009] In order to solve the above problems, one aspect of the present invention is a method for producing a semiconductor single crystal, which uses the Czochralski method to grow and pull a single crystal from a melt of a raw material, the method comprising the steps of: heating the melt using a heater so as to keep the diameter of the single crystal constant; and controlling a pulling speed for pulling the single crystal to have the same period and opposite phase to a periodic fluctuation in the output of the heater.and a delay time t [min] is added. Periodic fluctuation is added The delay time t [min] of the periodic fluctuation applied to the pulling speed is controlled within the range of t1≦t≦TH / 4, where TH [min] is the fluctuation period of the heater output and t1 [min] is the delay time of the fluctuation period of the heater temperature with respect to the heater output. do.

[0010] During a stable growth period in the process of pulling up a semiconductor single crystal, periodic fluctuations are observed in the temperature gradient G. In one embodiment of the method for producing a semiconductor single crystal of the present invention, periodic fluctuations are imparted to the pulling speed V to offset the periodic fluctuations in the temperature gradient G, thereby controlling the ratio (V / G) of the pulling speed V to the temperature gradient G, which has a significant effect on the occurrence of defects.

[0011] In addition, in one embodiment of the method for producing a semiconductor single crystal, the melt is heated using a heater so as to keep the diameter of the single crystal constant, and the periodic fluctuation has the same period and opposite phase to the periodic fluctuation of the heater output. In the method for producing a semiconductor single crystal, when the heater output is controlled so as to keep the crystal diameter constant, a relationship is established in which the temperature gradient G also fluctuates. In one embodiment of the method for producing a semiconductor single crystal, a periodic fluctuation having the same period and opposite phase to the periodic fluctuation of the heater output is applied to the pulling rate in order to offset the fluctuation of the temperature gradient G caused by controlling the heater output to keep the crystal diameter constant.

[0012] In addition, in one aspect of the present invention, the method for producing a semiconductor single crystal comprises heating the melt using a heater so as to keep the diameter of the single crystal constant, and the periodic fluctuation is a periodic fluctuation of the heater output with the same period and opposite phase as the periodic fluctuation, with a delay time added. The heater output and the crystal diameter of the ingot are linked, but have a time difference. Therefore, this delay time is added to the periodic fluctuation imparted to the pulling speed.

[0013] In addition, in the method for producing a semiconductor single crystal according to one embodiment of the present invention, when the fluctuation period of the heater output is TH [min], the delay time of the fluctuation period of the heater temperature relative to the heater output is t1 [min], and the delay time of the periodic fluctuation applied to the pulling speed is t [min], it is preferable to control the delay time t [min] of the periodic fluctuation applied to the pulling speed within the range of t1 ≦ t ≦ TH / 4. This is because within this range, it is possible to follow the change in the temperature gradient. Also, it is preferable to control the fluctuation width of the periodic fluctuation applied to the pulling speed within the range of ±0.1 [mm / min]. This is because within this range, the interface shape is not affected by the change in the ingot pulling speed.

[0014] Further, an apparatus for producing a semiconductor single crystal according to one aspect of the present invention is an apparatus for producing a semiconductor single crystal by using the Czochralski method to grow and pull a single crystal from a melt of a raw material, the apparatus comprising: a puller for pulling up the single crystal; a heater for heating the melt so as to keep the diameter of the single crystal constant; and a puller for controlling the pulling speed of the puller to have the same period and opposite phase to a periodic fluctuation of the output of the heater. and a delay time t [min] is added. and a control unit for applying a periodic fluctuation to the When the fluctuation period of the heater output is TH [min] and the delay time of the fluctuation period of the heater temperature with respect to the heater output is t1 [min], the control unit controls the delay time t [min] of the periodic fluctuation applied to the pulling speed within the range of t1≦t≦TH / 4. do.

[0015] By using such a semiconductor single crystal manufacturing apparatus, it is possible to offset the periodic fluctuation of the temperature gradient G by imparting periodic fluctuation to the pulling speed V, thereby controlling the ratio of the pulling speed V to the temperature gradient G (V / G), which has a significant effect on the occurrence of defects.

[0016] In one embodiment of the semiconductor single crystal manufacturing apparatus of the present invention, the melt is heated using a heater so as to keep the diameter of the single crystal constant, and the periodic fluctuation has the same period and opposite phase to the periodic fluctuation of the heater output. In one embodiment of the semiconductor single crystal manufacturing apparatus of the present invention, a periodic fluctuation having the same period and opposite phase to the periodic fluctuation of the heater output is applied to the pulling rate in order to offset the fluctuation of the temperature gradient G caused by controlling the heater output to keep the crystal diameter constant.

[0017] In one embodiment of the semiconductor single crystal manufacturing apparatus of the present invention, the melt is heated using a heater so as to keep the diameter of the single crystal constant, and the periodic fluctuation is a periodic fluctuation of the heater output with the same period and opposite phase as the periodic fluctuation, with a delay time added. The heater output and the crystal diameter of the ingot are linked, but there is a time difference. Therefore, this delay time is added to the periodic fluctuation imparted to the pulling speed.

[0018] In the semiconductor single crystal manufacturing apparatus according to one embodiment of the present invention, when the fluctuation period of the heater output is TH [min], the delay time of the fluctuation period of the heater temperature relative to the heater output is t1 [min], and the delay time of the periodic fluctuation applied to the pulling speed is t [min], it is preferable to control the delay time t [min] of the periodic fluctuation applied to the pulling speed within the range of t1 ≦ t ≦ TH / 4. This is because within this range, it is possible to follow the change in the temperature gradient. Also, it is preferable to control the fluctuation width of the periodic fluctuation applied to the pulling speed within the range of ±0.1 [mm / min]. This is because within this range, the interface shape is not affected by the change in the ingot pulling speed. Effect of the Invention

[0019] The present invention provides a method for producing a semiconductor single crystal and an apparatus for pulling a semiconductor single crystal, which controls the ratio (V / G) of the pulling speed V to the temperature gradient G during the pulling process in a simple and versatile manner. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a semiconductor single crystal manufacturing apparatus. [Diagram 2] FIG. 2 is a diagram showing temperature control of the raw material melt. [Diagram 3] FIG. 3 is a graph showing the relationship between the heater output and the pulling speed. [Figure 4] FIG. 4 is a diagram showing inspection results of the yield rate of the conventional example and the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the embodiment described below. In addition, in each drawing, the same or corresponding elements are appropriately assigned the same reference numerals. Furthermore, it should be noted that the drawings are schematic, and the dimensional relationship of each element, the ratio of each element, etc. may differ from the actual ones. There may also be parts in which the dimensional relationship and ratio differ between the drawings.

[0022] Fig. 1 is a diagram showing a schematic configuration of a semiconductor single crystal manufacturing apparatus. The semiconductor single crystal manufacturing apparatus 10 shown in Fig. 1 is an apparatus for manufacturing a semiconductor single crystal by a method generally called the Czochralski method. As shown in Fig. 1, the apparatus includes a furnace body 11, a crucible 12 arranged in the center of the furnace body 11, a heater 13 for heating the raw material melt in the crucible 12, and a winder 15 for winding up a wire for suspending a semiconductor single crystal (so-called an ingot 14) from the raw material melt in the crucible 12. The semiconductor single crystal manufacturing apparatus 10 is also provided with a sensor 16 for measuring the diameter of the grown ingot 14.

[0023] Furthermore, the semiconductor single crystal manufacturing apparatus 10 is equipped with a control unit 17 that controls various manufacturing conditions in the semiconductor single crystal manufacturing apparatus 10 according to information acquired from various sensors in the semiconductor single crystal manufacturing apparatus 10 and settings input by an operator. For example, the control unit 17 adjusts the output of the heater 13 in order to keep the diameter of the grown ingot 14, measured by the sensor 16, constant. The control unit 17 also controls the pulling speed at which the hoist 15 pulls up the ingot 14.

[0024] In addition, the semiconductor single crystal manufacturing apparatus 10 is configured to be able to rotate the crucible 12. That is, the crucible 12 is placed on a rotation / elevation mechanism 18, and is configured to rotate at a desired rotation speed and always maintain a constant distance between the lower end of the shield and the liquid surface. The semiconductor single crystal manufacturing apparatus 10 is also configured to be able to apply the so-called MCZ method (magnetic field applied Czochralski method), in which a magnetic field is applied to the raw material melt in order to precisely control the convection of the raw material melt in the crucible 12.

[0025] Fig. 2 shows the temperature control of the raw material melt. As shown in Fig. 2, the heater 13 cannot directly heat the raw material melt in the crucible 12, and even if the output of the heater 13 is changed, there is a time lag before the change is reflected in the temperature change of the raw material melt. Specifically, the crucible 12 is divided into a graphite crucible 12a and a quartz crucible 12b, and the heat of the heater 13 heats the graphite crucible 12a and the quartz crucible 12b in sequence to heat the raw material melt in the quartz crucible 12b, so it takes time from the change in the output of the heater 13 until the temperature of the raw material melt changes.

[0026] The time difference has an adverse effect on obtaining a single crystal of stable quality. That is, defects occurring during the growth of a single crystal are sensitive to the ratio (V / G) of the pulling speed V to the temperature gradient G, and defects will occur if the ratio (V / G) of the pulling speed V to the temperature gradient G is too large or too small. However, as described above, it takes time for the temperature gradient G to change from the change in the output of the heater 13 to the change in the temperature of the raw material melt, so it is difficult to keep the ratio (V / G) of the pulling speed V to the temperature gradient G within a certain range.

[0027] Therefore, in the semiconductor single crystal manufacturing method according to the embodiment of the present invention, a periodic variation is applied to the pulling speed for pulling up the ingot 14. For example, in the semiconductor single crystal manufacturing apparatus 10, this is realized by applying a periodic variation to the pulling speed that is the original control target when the control unit 17 controls the hoist 15. The periodic variation applied to the pulling speed can be determined, for example, as follows.

[0028] Figure 3 is a diagram showing the relationship between the output of heater 13 and the pulling speed. (a) in Figure 3 shows, from the top, the output of heater 13, the temperature of heater 13, and the crystal diameter. (b) in Figure 3 shows the pulling speed. These graphs shown in Figure 3 exemplify the periodic fluctuations observed during the stable growth period of a semiconductor single crystal.

[0029] 3(a), the output of heater 13 during the stable growth period of the semiconductor single crystal has periodic fluctuations. The temperature of the raw material melt in crucible 12 also fluctuates in accordance with this periodic fluctuation of the output of heater 13. At this time, if the temperature of the raw material melt increases, the temperature gradient G decreases, and if the temperature of the raw material melt decreases, the temperature gradient G increases.

[0030] Therefore, when the aim is to keep the ratio (V / G) of the pulling speed V to the temperature gradient G constant, the periodic fluctuation applied to the pulling speed V has the same period and the opposite phase to the periodic fluctuation of the output of the heater 13. In other words, when the output of the heater 13 is high, the pulling speed V is slowed down, and when the output of the heater 13 is low, the pulling speed V is fast.

[0031] As shown in Fig. 3(a), the output of heater 13 and the crystal diameter of ingot 14 are linked with a time lag. Using this property, the output of heater 13 is controlled so that the crystal diameter becomes constant. Specifically, the crystal diameter of ingot 14 is monitored using sensor 16, and the output of heater 13 is controlled so that the crystal diameter of ingot 14 measured using sensor 16 becomes constant. That is, the raw material melt is heated using heater 13 so as to keep the crystal diameter of ingot 14 constant, and the periodic fluctuation given to the pulling speed V has the same period and the opposite phase to the periodic fluctuation of the output of heater 13 at this time.

[0032] On the other hand, the output of the heater 13 and the crystal diameter of the ingot 14 are linked to each other, but there is a time lag. Therefore, the periodic fluctuation imparted to the pulling speed V is obtained by adding a delay time to the same period and opposite phase of the periodic fluctuation of the output of the heater 13 at this time. From this viewpoint, it is preferable to control the periodic fluctuation imparted to the pulling speed V so as to be within the following range.

[0033] First, the fluctuation period of the output of the heater 13 is TH [min], the delay time of the fluctuation period of the temperature of the heater 13 relative to the output of the heater 13 is t1 [min], and the delay time of the periodic fluctuation given to the pulling speed V is t [min]. Under these settings, the delay time t [min] of the periodic fluctuation given to the pulling speed V is controlled in the range of t1 ≦ t ≦ TH / 4. By controlling the delay time t [min] of the periodic fluctuation given to the pulling speed V in the range of t1 ≦ t ≦ TH / 4, it is possible to follow the change in the temperature gradient G. In addition, it is preferable to control the fluctuation width of the periodic fluctuation given to the pulling speed V within the range of ±0.1 [mm / min]. If the fluctuation width of the periodic fluctuation given to the pulling speed V is within the range of ±0.1 [mm / min], the interface shape is not affected by the change in the pulling speed of the ingot 14.

[0034] As described above, by controlling the periodic fluctuation applied to the pulling speed V, it is possible to offset the fluctuation in the temperature gradient G with the pulling speed V and maintain a constant ratio (V / G) of the pulling speed V to the temperature gradient G. This prevents the formation of defects that are sensitive to the ratio (V / G) of the pulling speed V to the temperature gradient G, and realizes a method for producing semiconductor single crystals of stable quality.

[0035] (Conventional Examples and Examples) Here, a description will be given of an experiment verifying the effects of the conventional example and the embodiment in which the above-described method for producing a semiconductor single crystal was implemented.

[0036] The manufacturing conditions common to the conventional example and the embodiment are as follows: a semiconductor single crystal of φ300 mm is grown with a charge of 350 kg, the distance between the lower end of the radiation shield and the liquid surface is 50 mm, the furnace atmosphere is argon (Ar) flow rate of 90 L / min, the furnace pressure is 65 torr, the crystal rotation speed is 10.0 rpm, the crucible rotation speed is 0.5 rpm, and the magnetic field strength of the transverse magnetic field is 3000 Gauss.

[0037] First, as a conventional manufacturing method, the pulling speed was set to V=0.55 [mm / min] (constant) and five semiconductor single crystals were manufactured in succession. At that time, the fluctuation period of the heater output was TH=86 [min], and the delay time of the fluctuation period of the heater temperature with respect to the heater output was t1=11 [min].

[0038] Thereafter, five semiconductor single crystals were successively manufactured in the same manner as in the manufacturing method of Example 1, with a pulling speed V=0.55[mm / min], a period T of the applied periodic fluctuation set to T=86[min], which is the same as the fluctuation period TH=86[min] of the heater output, a delay time of the periodic fluctuation set to t=0[min], and a fluctuation width of the periodic fluctuation set to within the range of V=±0.05[mm / min]. Note that this periodic fluctuation satisfies the requirement that it is in phase and opposite phase to the fluctuation period of the heater output, and the fluctuation width of the periodic fluctuation satisfies the range of ±0.1[mm / min].

[0039] Thereafter, as the manufacturing method of Example 2, five semiconductor single crystals were successively manufactured in the same manner, with a pulling speed V=0.55[mm / min], a period T of the applied periodic fluctuation set to T=86[min], which is the same as the fluctuation period TH=86[min] of the heater output, a delay time of the periodic fluctuation set to t=16[min], and a fluctuation width of the periodic fluctuation set to within the range of V=±0.05[mm / min]. Note that the periodic fluctuation satisfies the in-phase and anti-phase of the fluctuation period of the heater output, the delay time of the periodic fluctuation satisfies the range of t1≦t≦TH / 4, and the fluctuation width of the periodic fluctuation satisfies the range of ±0.1[mm / min].

[0040] Then, a yield rate inspection was performed on a total of 15 semiconductor single crystals from the conventional example and Examples 1 and 2. Here, the yield rate was defined as the percentage of the area in which defect-free crystals could be obtained from the entire length of the straight body of the manufactured semiconductor single crystal. FIG. 4 is a diagram showing the inspection results of the yield rates of the conventional example and Examples 1 and 2.

[0041] 4, the average yield rate of semiconductor single crystals produced using the conventional semiconductor single crystal production method was 60%, whereas the average yield rate of semiconductor single crystals produced using the semiconductor single crystal production method of Example 1 was 69%, and the average yield rate of semiconductor single crystals produced using the semiconductor single crystal production method of Example 2 was 83%. In other words, the semiconductor single crystal production method according to the present invention is a simple and highly versatile method that can control the ratio (V / G) of the pulling speed V and the temperature gradient G in the pulling process, and the semiconductor single crystal produced by this semiconductor single crystal production method has stable quality in the crystal length direction.

[0042] Although the present invention has been described based on the embodiments, the present invention is not limited to the above-mentioned embodiments. For example, the target value of the pulling speed V is not limited to being constant, and even when the pulling speed is controlled, the target value of the pulling speed V can be periodically changed. [Explanation of symbols]

[0043] 10. Semiconductor single crystal manufacturing equipment 11 Furnace body 12 Crucible 13. Heater 14 Ingot 15 Windlass 16 Sensors 17 Control Unit 18 Rotation and lifting mechanism

Claims

1. A method for producing a semiconductor single crystal by growing and pulling a single crystal from a melt of a raw material using the Czochralski method, comprising the steps of: Heating the melt using a heater so as to keep the diameter of the single crystal constant; imparting a periodic fluctuation to the pulling rate for pulling the single crystal, the periodic fluctuation having the same period and opposite phase to the periodic fluctuation of the heater output and having a delay time t [min] added thereto; a delay time t [min] of the periodic fluctuation imparted to the pulling rate is controlled in the range of t1≦t≦TH / 4, where TH [min] is the fluctuation period of the heater output and t1 [min] is the delay time of the fluctuation period of the heater temperature with respect to the heater output.

2. 2. The method for producing a single crystal according to claim 1, wherein the fluctuation width of the periodic fluctuation applied to the pulling rate is controlled within a range of ±0.1 [mm / min].

3. An apparatus for manufacturing semiconductor single crystals that uses the Czochralski method to grow and pull a single crystal from a melt of a raw material, comprising: A puller for pulling up the single crystal; a heater for heating the melt so as to keep the diameter of the single crystal constant; a control unit that applies a periodic fluctuation to the pulling speed of the pulling machine, the periodic fluctuation having the same period and opposite phase to the periodic fluctuation of the output of the heater, and having a delay time t [min] added thereto; Equipped with The apparatus for manufacturing semiconductor single crystals, wherein the control unit controls the delay time t [min] of the periodic fluctuation applied to the pulling rate within the range of t1≦t≦TH / 4, where TH [min] is the fluctuation period of the heater output and t1 [min] is the delay time of the fluctuation period of the heater temperature with respect to the heater output.

4. 4. The apparatus for producing a single crystal according to claim 3, wherein the control unit controls the fluctuation width of the periodic fluctuation applied to the pulling rate within a range of ±0.1 [mm / min].

Citation Information

Patent Citations

  • Method for pulling up single crystal

    JP1993043386A

  • Silicon single crystal almost free from crystal defect and its production

    JP1996337490A

  • Pulling up of single crystal

    JP1997208377A

  • Single crystal ingot production apparatus and method

    JP2000281478A

  • Production of silicon wafer and method for growing silicon single crystal

    JP2000327486A