Substrate processing method
By forming a protective film on the sidewalls and controlling the etching process with a cold substrate support, the method addresses sidewall shape defects in recesses by preventing reaction by-product adherence, achieving precise etching results.
Patent Information
- Application Number
- JP2020209374
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-17
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Existing methods for forming recesses in dielectric materials on semiconductor substrates suffer from shape defects on the sidewalls of the recesses due to the adherence of reaction by-products during etching.
A method involving the formation of a protective film on the sidewalls of recesses, followed by controlled etching of the recess bottom while suppressing the adherence of reaction by-products, and maintaining a substrate support temperature at -40°C or lower during the etching process.
This method effectively suppresses shape defects such as bowing on the sidewalls of the recesses by preventing the formation of shoulders caused by reaction by-products, ensuring precise etching.
Smart Images

Figure 0007583601000001 
Figure 0007583601000002 
Figure 0007583601000003
Abstract
Description
[Technical field]
[0001] An exemplary embodiment of the present disclosure relates to a method for processing a substrate. [Background technology]
[0002] US Patent No. 5,999,333 discloses a method for forming an etched recess in a dielectric material on a semiconductor substrate. In the method, a first plasma containing an etching reactant is generated and the substrate is exposed to the first plasma to partially etch a recess in the dielectric material. A protective film is then deposited on the sidewalls of the recess using atomic layer deposition. Etching and deposition are repeated until the recess is etched to its final depth. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] U.S. Patent No. 9,378,971 Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique for suppressing defects in the shape of the sidewalls of recesses formed by etching. [Means for solving the problem]
[0005] In one exemplary embodiment, a substrate processing method is provided, which includes the steps of: (a) providing a substrate having a film to be etched on a substrate support, in which a recess is formed, (b) forming a protective film on a sidewall of the recess, (c) generating plasma from a processing gas after (b) to etch a bottom of the recess, and (d) performing a sequence including (b) and (c) one or more times, in which (c) includes a first step of etching the bottom of the recess while suppressing the formation of a shoulder caused by a reaction by-product generated in the etching adhering to the sidewall, and a second step of further etching the bottom of the recess by controlling the temperature of the substrate support to −40° C. or less after the first step. Effect of the Invention
[0006] According to one exemplary embodiment, it is possible to suppress defects in the shape of the sidewalls of a recess formed by etching. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a flow diagram of a substrate processing method according to one exemplary embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a portion of an example substrate. [Diagram 3] FIG. 3 is a schematic diagram of an example of a substrate processing apparatus. [Figure 4] FIG. 4(a) is a diagram for explaining an example of a process for providing a substrate having an etching target film in which a recess is formed, and FIG. 4(b) is a partially enlarged cross-sectional view of the example substrate in a state after the process has been performed. [Diagram 5] FIG. 5 is a partially enlarged cross-sectional view of the example substrate in a step of forming a protective film on a side wall of a recess. [Figure 6] FIG. 6(a) is a diagram for explaining an example of the first stage of a process for etching the bottom of a recess, and FIG. 6(b) is a partially enlarged cross-sectional view of an example substrate in a state after the first stage has been performed. [Figure 7]FIG. 7(a) is a diagram for explaining an example of the second stage of the process for etching the bottom of a recess, and FIG. 7(b) is a partially enlarged cross-sectional view of an example substrate in a state after the second stage has been performed. [Figure 8] FIG. 8 is a partially enlarged cross-sectional view of the example substrate after a process of performing a sequence including etching and formation of a protective film one or more times. [Figure 9] FIGS. 9(a) to 9(e) are diagrams showing schematic examples of the shape of the sidewall of a recess formed by etching. [Figure 10] FIGS. 10(a) to 10(c) are diagrams showing schematic examples of the shape of the sidewall of a recess formed by etching. [Figure 11] FIGS. 11(a) to 11(d) are diagrams showing schematic examples of the shape of the sidewall of a recess formed by etching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Various exemplary embodiments are described below.
[0009] In one exemplary embodiment, a substrate processing method includes the steps of: (a) providing a substrate having a film to be etched on a substrate support, the film having a recess formed therein; (b) forming a protective film on a sidewall of the recess; (c) after (b), generating plasma from a processing gas to etch a bottom of the recess; and (d) performing a sequence including (b) and (c) one or more times, in which (c) includes a first step of etching the bottom of the recess while suppressing the formation of a shoulder caused by a reaction by-product generated in the etching adhering to the sidewall; and a second step of further etching the bottom of the recess by controlling a temperature of the substrate support to −40° C. or less after the first step.
[0010] According to the above method, it is possible to suppress shape defects (bowing) on the sidewalls of the recess formed by etching.
[0011] The formation of the shoulder may be inhibited by inhibiting the reaction by-products from adhering to the sidewalls and / or by removing the reaction by-products that have adhered to the sidewalls.
[0012] In the first stage, etching may be performed with the temperature of the substrate support set to a temperature higher than -40°C.
[0013] The film to be etched may be a silicon-containing film, the process gas may contain a halogen-containing gas not containing carbon atoms and nitrogen atoms and an oxygen-containing gas, and in the first stage, etching may be performed in a state where a ratio of a flow rate of the oxygen-containing gas to a total flow rate of the halogen-containing gas and the oxygen-containing gas is set to a first ratio, and in the second stage, etching may be performed in a state where the ratio is set to a second ratio greater than the first ratio.
[0014] The halogen-containing gas may include at least one gas selected from the group consisting of SF6 gas, Cl2 gas, and HBr gas.
[0015] The oxygen-containing gas may include O2 gas.
[0016] The silicon-containing film may include a silicon film or a silicon germanium film.
[0017] The first ratio may be equal to or less than 35%, which can significantly reduce defects in the shape of the sidewall of the recess formed by etching.
[0018] The step (a) is a process for providing the substrate having the recess formed thereon by etching the film to be etched while controlling the temperature of the substrate support to −40° C. or less, and the etching conditions in the step (a) may be the same as the etching conditions in the second step.
[0019] The duration of the second stage may be up to six times the duration of the first stage.
[0020] The recess etched in the first step may have an etching depth of 1 μm or less.
[0021] In the step (c), the first stage may be switched to the second stage while plasma is being generated.
[0022] The steps (a) to (d) may be carried out in situ.
[0023] Various exemplary embodiments will now be described in detail with reference to the drawings, in which the same or corresponding parts are designated by the same reference numerals.
[0024] Fig. 1 is a flow diagram of a substrate processing method according to an example embodiment. The substrate processing method (hereinafter referred to as "method MT") shown in Fig. 1 is performed to etch a region in a substrate. Fig. 2 is an enlarged cross-sectional view of a portion of an example substrate. The substrate W shown in Fig. 2 may have a region RE and a mask MK.
[0025] The region RE is a film to be etched in the method MT. In the substrate W shown in FIG. 2, a mask MK is provided on the region RE. The mask MK is patterned. That is, the mask MK provides one or more openings OP that partially expose the region RE. The width of the openings OP provided by the mask MK may be, for example, 100 nm or less. The distance between adjacent openings OP may also be, for example, 100 nm or less.
[0026] The region RE may contain silicon and / or germanium. The region RE may include a silicon-containing film. The silicon-containing film may include at least one of a silicon film, a silicon germanium film, a silicon oxide film, and a silicon nitride film. The silicon-containing film may be a multilayer film including a silicon film and a silicon germanium film. The silicon-containing film may contain at least one of single crystal silicon, silicon containing a dopant, and silicon germanium.
[0027] The mask MK may include at least one of a silicon oxide film, a silicon nitride film, a silicon carbide film, an organic film, and a metal film. The organic film may include at least one of a SOC (Spin On Carbon) film and an amorphous carbon film. The metal film may contain tungsten or titanium.
[0028] In one embodiment, the method MT is performed using a substrate processing apparatus. An example substrate processing apparatus is shown in FIG 3. The substrate processing apparatus shown in FIG 3 is an inductively-coupled plasma (ICP) apparatus 10.
[0029] The plasma processing apparatus 10 includes a chamber 12. The chamber 12 is made of a metal containing Al (aluminum) or Y (yttrium). For example, the chamber 12 is made of Al2O3 or Y2O3. The chamber 12 has, for example, a substantially cylindrical shape. An internal space 12c in which processing is performed is provided within the chamber 12.
[0030] A substrate support 14 is disposed below the internal space 12c. The substrate support 14 is configured to hold a substrate W placed thereon. The substrate W is, for example, a semiconductor wafer.
[0031] The substrate support 14 can be supported by a support 13. The support 13 extends upward from the bottom of the chamber 12 within the internal space 12c. The support 13 can be substantially cylindrical. The support 13 can be made of an insulating material such as quartz.
[0032] The substrate support 14 includes an electrostatic chuck 16 and a lower electrode 18. The lower electrode 18 includes a first plate 18a and a second plate 18b. The first plate 18a and the second plate 18b are made of a metal such as aluminum. The first plate 18a and the second plate 18b are, for example, substantially cylindrical. The second plate 18b is disposed on the first plate 18a. The second plate 18b is electrically connected to the first plate 18a.
[0033] The electrostatic chuck 16 is disposed on the second plate 18b. The electrostatic chuck 16 includes an insulating layer and a thin-film electrode disposed in the insulating layer. A DC power supply 22 is electrically connected to the thin-film electrode of the electrostatic chuck 16 via a switch 23. The electrostatic chuck 16 generates an electrostatic force from a DC voltage of the DC power supply 22. The electrostatic chuck 16 attracts and holds the substrate W by the generated electrostatic force.
[0034] In the plasma processing apparatus 10, an edge ring ER is disposed on the second plate 18b and around the second plate 18b so as to surround the outer periphery of the substrate W and the electrostatic chuck 16. The edge ring ER serves to improve the uniformity of the process. The edge ring ER is made of, for example, silicon.
[0035] A flow path 24 is formed in the second plate 18b. A heat exchange medium such as a refrigerant is supplied to the flow path 24 from a temperature adjustment unit (e.g., a chiller unit) disposed outside the chamber 12 for temperature control. The temperature adjustment unit adjusts the temperature of the heat exchange medium. The heat exchange medium is supplied from the temperature adjustment unit to the flow path 24 through a pipe 26a. The heat exchange medium supplied from the temperature adjustment unit to the flow path 24 through the pipe 26a is returned to the temperature adjustment unit through a pipe 26b. After the temperature adjustment by the temperature adjustment unit, the heat exchange medium is returned to the flow path 24 in the substrate support 14. In this manner, the temperature of the substrate support 14, i.e., the temperature of the substrate W, can be adjusted.
[0036] The plasma processing apparatus 10 further includes a gas supply line 28 that extends through the substrate support 14 to the upper surface of the electrostatic chuck 16. A heat exchange gas, such as helium (He) gas, is supplied from a heat exchange gas supply mechanism through the gas supply line 28 to the space between the upper surface of the electrostatic chuck 16 and the lower surface of the substrate W. The heat exchange gas promotes heat exchange between the substrate support 14 and the substrate W.
[0037] Alternatively, a heater HT may be disposed in the substrate support 14. The heater HT is a heating device. The heater HT is embedded in, for example, the second plate 18b or the electrostatic chuck 16. The heater HT is connected to a heater power supply HP. The heater power supply HP supplies power to the heater HT, thereby adjusting the temperature of the substrate support 14 and, in turn, the temperature of the substrate W.
[0038] A bias power supply 30 is connected to the lower electrode 18 of the substrate support 14. The bias power supply 30 generates a bias power used to attract ions to the substrate W. In one embodiment, the bias power supply 30 may be a radio frequency power supply that generates radio frequency (RF) power as the bias power. When a radio frequency power supply is used as the bias power supply 30, the frequency of the bias power is, for example, within a range of 400 kHz to 40.68 MHz. In one example, the frequency of the bias power may be 13.56 MHz. In this embodiment, the bias power supply 30 is connected to the lower electrode 18 via a matching box 32. The matching box 32 includes a circuit that performs matching between the output impedance from the bias power supply 30 and the impedance on the load side, i.e., the lower electrode 18 side.
[0039] The plasma processing apparatus 10 further includes a shield 34 removably attached to the inner wall of the chamber 12. The shield 34 is also disposed so as to surround the outer periphery of the support 13. The shield 34 prevents by-products generated by the processing from adhering to the chamber 12. The shield 34 may be an aluminum member coated with a ceramic such as Y2O3.
[0040] An exhaust path is formed between the substrate support 14 and the side wall of the chamber 12. The exhaust path is connected to an exhaust port 12e formed at the bottom of the chamber 12. The exhaust port 12e is connected to an exhaust device 38 via a pipe 36. The exhaust device 38 includes a pressure adjustment unit and a vacuum pump such as a turbo molecular pump (TMP). A baffle plate 40 is disposed in the exhaust path, i.e., between the substrate support 14 and the side wall of the chamber 12. The baffle plate 40 has a plurality of through holes penetrating the baffle plate 40 in the thickness direction. The baffle plate 40 may be an aluminum member whose surface is coated with ceramics such as Y2O3.
[0041] An opening is formed in the upper side of the chamber 12. The opening is closed by a dielectric window 42. The dielectric window 42 is made of quartz or the like. The dielectric window 42 is, for example, a flat plate.
[0042] A gas supply port 12i is formed in the side wall of the chamber 12. The gas supply port 12i is connected to a gas supply unit 44 via a gas supply pipe 46. The gas supply unit 44 supplies various gases used in processing to the internal space 12c. The gas supply unit 44 includes a plurality of gas sources 44a, a plurality of flow rate controllers 44b, and a plurality of valves 44c. Although not shown in FIG. 1, a different gas supply port may be provided for each gas to be supplied to prevent the gases from being mixed together.
[0043] The multiple gas sources 44a include gas sources for various gases, which will be described later. One gas source may supply one or more gases. The multiple flow rate controllers 44b may be mass flow controllers (MFCs). The flow rate controllers 44b realize flow rate control by pressure control. Each gas source included in the multiple gas sources 44a is connected to a gas supply port 12i via a corresponding one of the multiple flow rate controllers 44b and a corresponding one of the multiple valves 44c. The position of the gas supply port 12i is not particularly limited. For example, the gas supply port 12i may be formed in the dielectric window 42 instead of the sidewall of the chamber 12.
[0044] An opening 12p is formed in the sidewall of the chamber 12. The opening 12p serves as a path for loading and unloading the substrate W. The substrate W is loaded from the outside into the internal space 12c of the chamber 12 through the opening 12p, and is unloaded from the internal space 12c to the outside of the chamber 12. A gate valve 48 is provided on the sidewall of the chamber 12, and is capable of opening and closing the opening 12p.
[0045] An antenna 50 and a shield 60 are disposed on the chamber 12 and the dielectric window 42. The antenna 50 and the shield 60 are disposed outside the chamber 12. In one embodiment, the antenna 50 includes an inner antenna element 52A and an outer antenna element 52B. The inner antenna element 52A is a spiral coil disposed in the center of the dielectric window 42. The outer antenna element 52B is a spiral coil disposed on the dielectric window 42 and on the outer periphery side of the inner antenna element 52A. The inner antenna element 52A and the outer antenna element 52B are each made of a conductive material such as copper, aluminum, stainless steel, or the like.
[0046] The inner antenna element 52A and the outer antenna element 52B are gripped and held together by a plurality of clamps 54. Each of the clamps 54 is rod-shaped. The clamps 54 extend radially from approximately the center of the inner antenna element 52A to the outer periphery of the outer antenna element 52B.
[0047] The antenna 50 is covered with a shield 60. The shield 60 includes an inner shield wall 62A and an outer shield wall 62B. The inner shield wall 62A has a cylindrical shape. The inner shield wall 62A is disposed between the inner antenna element 52A and the outer antenna element 52B and surrounds the inner antenna element 52A. The outer shield wall 62B has a cylindrical shape. The outer shield wall 62B is disposed outside the outer antenna element 52B and surrounds the outer antenna element 52B.
[0048] A disk-shaped inner shield plate 64A is disposed on the inner antenna element 52A. The inner shield plate 64A covers the opening of the inner shield wall 62A. A flat ring-shaped outer shield plate 64B is disposed on the outer antenna element 52B. The outer shield plate 64B covers the opening between the inner shield wall 62A and the outer shield wall 62B.
[0049] The shapes of the shield wall and shield plate included in the shield 60 are not limited to those described above. For example, the shield wall of the shield 60 may be a prism having a rectangular cross section.
[0050] The inner antenna element 52A and the outer antenna element 52B are connected to the high frequency power source 70A and the high frequency power source 70B, respectively. The inner antenna element 52A and the outer antenna element 52B are supplied with power of the same or different frequencies from the high frequency power source 70A and the high frequency power source 70B, respectively. When high frequency power is supplied from the high frequency power source 70A to the inner antenna element 52A, an induction magnetic field is generated in the internal space 12c, which excites the gas in the internal space 12c to generate plasma above the center of the substrate W. On the other hand, when high frequency power is supplied from the high frequency power source 70B to the outer antenna element 52B, an induction magnetic field is generated in the internal space 12c, which excites the gas in the internal space 12c to generate plasma in a ring shape above the outer periphery of the substrate W. The high frequency power source 70A and the high frequency power source 70B constitute an example of a plasma generating unit.
[0051] The electrical length of each of inner antenna element 52A and outer antenna element 52B is adjusted according to the frequency output from high frequency power supply 70A and high frequency power supply 70B. Therefore, the positions of inner shield plate 64A and outer shield plate 64B in the z-axis direction are adjusted independently by actuators 68A and 68B.
[0052] The plasma processing apparatus 10 further includes a control unit 80. The control unit 80 is, for example, a computer including a processor, a storage unit such as a memory, an input unit, a display, and the like. The control unit 80 operates based on a control program and recipe data stored in the storage unit, and controls each unit of the plasma processing apparatus 10. For example, the control unit 80 controls a plurality of flow rate controllers 44b, a plurality of valves 44c, an exhaust device 38, high frequency power supplies 70A and 70B, a bias power supply 30, a matching box 32, a heater power supply HP, and the like. The control unit 80 reads out a program or data from the storage unit and controls each unit of the plasma processing apparatus 10, thereby performing plasma processing of a plasma processing method according to an embodiment, which will be described later.
[0053] Method MT will be described in detail with reference to Fig. 1 again. In the following description, method MT will be described with reference to Figs. 4 to 8, taking as an example a case where the substrate W shown in Fig. 2 is processed using the plasma processing apparatus 10. Note that other substrate processing apparatuses may be used in method MT. Other substrates may be processed in method MT.
[0054] The method MT may include steps ST0, ST1, ST2, ST3, and ST4. Steps ST0 to ST4 may be performed in this order. The method MT may be performed with the substrate W placed on the substrate support 14. The method MT may be performed while maintaining a reduced pressure environment in the internal space 12c of the chamber 12, and without removing the substrate W from the internal space 12c. That is, in steps ST1 to ST4, the substrate W may be processed in-situ. In one embodiment, the method MT may start with step ST0.
[0055] In step ST0, the temperature of the substrate support 14 is controlled to −40° C. or lower. The temperature of the substrate support 14 can be controlled by a coolant supplied to the flow path 24. Step ST0 may be performed in steps ST1 to ST4, except for the first stage of step ST3.
[0056] In step ST1, a substrate W (see FIG. 4(b)) having a region RE in which a recess R1 is formed is provided. The recess R1 may be, for example, a hole or a trench. In one embodiment, the recess R1 is formed by partially etching the region RE. The region RE may be etched using plasma. In one embodiment, step ST1 is a step of providing a substrate W in which a recess R1 is formed by etching the region RE while controlling the temperature of the substrate support 14 to −40° C. or less.
[0057] Fig. 4(a) is a diagram for explaining an example of step ST1 of providing a substrate W having an etching target film in which a recess R1 is formed. Fig. 4(b) is a partially enlarged cross-sectional view of the example substrate W in a state after the step ST1 is performed. In step ST1, as shown in Fig. 4(a), a plasma P1 is generated from a processing gas in a chamber 12.
[0058] The process gas may include a halogen-containing gas. The halogen-containing gas may be free of carbon and nitrogen atoms. The halogen-containing gas may include at least one of a bromine-containing gas, a chlorine-containing gas, and a fluorine-containing gas. The bromine-containing gas may include HBr gas. The chlorine-containing gas may include Cl2 gas. The fluorine-containing gas may include SF6 gas. The process gas may include an oxygen-containing gas. The oxygen-containing gas may include, for example, O2 gas.
[0059] In step ST1, etching may be performed in a state in which the temperature of the substrate support 14 that supports the substrate W is set to a low temperature, for example, below −50° C. or below −40° C. The control unit 80 controls the temperature adjustment mechanism of the plasma processing apparatus 10 so as to set the temperature of the substrate support 14 to a designated temperature.
[0060] In step ST1, as shown in FIG. 4(a), chemical species from plasma P1 are supplied to substrate W, and region RE is partially etched by the chemical species. In step ST1, region RE is etched to a position between the upper surface of region RE and the lower surface of region RE. The upper surface of region RE is the surface of region RE exposed from the opening of mask MK. When step ST1 is performed, as shown in FIG. 4(b), recess R1 is formed so as to extend from mask MK into region RE. Recess R1 has sidewall R1s and bottom R1b. The width WD of recess R1 is the distance between a pair of sidewalls R1s facing each other. The width WD of recess R1 may be, for example, 100 nm or less. The distance between adjacent recesses R1 may also be, for example, 100 nm or less.
[0061] In step ST1, the control unit 80 controls the exhaust device 38 to set the pressure of the gas in the chamber 12 to a designated pressure. The control unit 80 controls the gas supply unit 44 to supply a processing gas into the chamber 12. The control unit 80 controls the plasma generation unit to generate plasma P1 from the processing gas. In one embodiment, in step ST1, the control unit 80 controls the high frequency power supply 70A, the high frequency power supply 70B, and the bias power supply 30 to supply high frequency power and bias power.
[0062] The recess R1 may be provided in advance in the region RE of the substrate W by a method other than etching.
[0063] 5 is a partially enlarged cross-sectional view of an example of the substrate W in step ST2 of forming a protective film PF on a sidewall R1s of the recess R1. In step ST2, as shown in FIG. 5, the protective film PF is formed on the sidewall R1s of the recess R1. The protective film PF may also be formed on the bottom R1b of the recess R1 and the surface of the mask MK. The protective film PF may have a first thickness on the sidewall R1s of the recess R1 and a second thickness smaller than the first thickness on the bottom R1b of the recess R1 and the surface of the mask MK. The protective film PF may contain, for example, a silicon oxide film.
[0064] The protective film PF may be formed by atomic layer deposition (ALD), chemical vapor deposition (CVD), or physical vapor deposition (PVD). The CVD may be a plasma enhanced CVD, or a CVD using heat, light, or the like. In step ST2 using the CVD method, a film forming gas is supplied into the chamber 12. In step ST2 using the CVD method, plasma may be generated from the film forming gas in the chamber 12.
[0065] In step ST2 by the ALD method, a precursor layer is formed on the surface of the substrate W. A first gas is used to form the precursor layer. The first gas includes a substance that constitutes the precursor layer. The precursor layer may be formed without generating plasma from the first gas. Alternatively, the precursor layer may be formed using chemical species from plasma generated from the first gas.
[0066] The first gas includes monosilane (SiH4), disilane (Si2H6), silicon chloride, chlorosilane, or silicon fluoride. Silicon chloride is, for example, silicon tetrachloride (SiCl4), hexachlorodisilane (Si2Cl6), etc. Chlorosilanes are, for example, trichlorosilane (HSiCl3), dichlorosilane (H2SiCl2), chlorotrimethylsilane ((CH3)3SiCl), etc. Silicon fluoride is, for example, silicon tetrafluoride (SiF4), etc.
[0067] The control unit 80 controls the gas supply unit 44 to supply the first gas into the chamber 12. The control unit 80 controls the exhaust device 38 to set the pressure of the gas in the chamber 12 to a designated pressure. When plasma is to be generated, the control unit 80 controls the plasma generating unit to generate plasma from the first gas in the chamber 12. In one embodiment, to generate plasma from the first gas, the control unit 80 controls the high frequency power supply 61 and / or the bias power supply 62 to supply high frequency power HF and / or high frequency power LF.
[0068] After the precursor layer is formed, purging of the internal space 12c may be performed. The control unit 80 may control the exhaust device 38 to evacuate the internal space 12c. The control unit 80 may control the gas supply unit 44 to supply an inert gas into the chamber 12. By performing the purging, the first gas in the chamber 12 may be replaced with the inert gas. By performing the purging, excess substances adsorbed on the substrate W may be removed. As a result of the purging, the precursor layer may be formed on the substrate W as a monolayer.
[0069] After the purge is performed, a protective film PF is formed from the precursor layer. A second gas may be used to form the protective film PF. The second gas includes reactive species that react with a material constituting the precursor layer to form the protective film PF from the precursor layer. The second gas includes an oxygen-containing gas (e.g., H2 gas). The protective film PF may be formed without generating plasma from the second gas. Alternatively, the protective film PF may be formed using chemical species from plasma generated from the second gas. Alternatively, the precursor layer may be activated by heat, light, or the like.
[0070] The control unit 80 controls the gas supply unit 44 to supply the second gas into the chamber 12. The control unit 80 controls the exhaust device 38 to set the pressure of the gas in the chamber 12 to a specified pressure. When plasma is generated, the control unit 80 controls the plasma generation unit to generate plasma from the second gas in the chamber 12. In one embodiment, to generate plasma from the second gas, the control unit 80 controls the high frequency power supply 70A, the high frequency power supply 70B, and / or the bias power supply 30 to supply high frequency power. Alternatively, the control unit 80 may control the heater power supply HP to heat the substrate W for activation of the precursor layer. Alternatively, the control unit 80 may control a light source to irradiate the substrate W with light for activation of the precursor layer.
[0071] After the protective film PF is formed, the internal space 12c may be purged, so that the second gas in the chamber 12 may be replaced with an inert gas.
[0072] By repeating the formation and purging of the precursor layer, the thickness of the protective film PF can be adjusted.
[0073] Step ST3 includes a first stage and a second stage. Step ST3 starts in the first stage. The second stage is performed after the first stage. Step ST3 may include one or more stages performed after the second stage.
[0074] Fig. 6(a) is a diagram for explaining an example of a first stage of step ST3 for etching the bottom R1b of the recess R1. Fig. 6(b) is a partially enlarged cross-sectional view of the example substrate W in a state after the first stage has been performed. Fig. 7(a) is a diagram for explaining an example of a second stage of step ST3 for etching the bottom R1b of the recess R1, and Fig. 7(b) is a partially enlarged cross-sectional view of the example substrate W in a state after the second stage has been performed.
[0075] In the first stage, as shown in FIG. 6, the bottom R1b of the recess R1 is etched while suppressing the formation of a shoulder caused by the adhesion of reaction by-products generated by etching to the sidewall R1s. The formation of the shoulder is suppressed by suppressing the adhesion of reaction by-products to the sidewall R1s and / or removing the reaction by-products attached to the sidewall R1s. In one embodiment, a plasma P2 is generated from a process gas in the chamber 12, and the bottom R1b of the recess R1 is etched. In one embodiment, the bottom R1b of the recess R1 is etched by chemical species from the plasma P2. The type of process gas in the first stage may be the same as that in step ST1.
[0076] In the second stage, the bottom R1b of the recess R1 is further etched as shown in Fig. 7. A plasma P3 is generated from the process gas in the chamber 12 to etch the bottom R1b of the recess R1. In one embodiment, the bottom R1b of the recess R1 is etched by chemical species from the plasma P3. The type of process gas in the second stage may be the same as that in the first stage.
[0077] In step ST3, while plasma is being generated, the etching may be switched from the first stage to the second stage. The etching conditions in the second stage may be the same as the etching conditions in step ST1.
[0078] In one embodiment, in the first stage, etching may be performed with the temperature of the substrate support 14 set to a first temperature T1. The first temperature T1 may be, for example, higher than -40°C or higher than -30°C. The first temperature T1 may be -20°C or lower. In the second stage, etching may be performed with the temperature of the substrate support 14 set to a second temperature T2 lower than the first temperature T1. The second temperature T2 may be, for example, lower than -50°C or lower than -40°C. The second temperature T2 may be -100°C or higher. In this embodiment, the type and flow rate of the gas contained in the process gas in the first stage may be the same as the type and flow rate of the gas contained in the process gas in the second stage. In the first and second stages, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas not containing carbon atoms and nitrogen atoms may be greater than 35%, greater than 30%, or greater than 25%.
[0079] In another embodiment, in the first stage, etching may be performed in a state where the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas not containing carbon atoms and nitrogen atoms and the oxygen-containing gas is set to a first ratio RT1. The first ratio RT1 may be 35% or less, 30% or less, or 25% or less. In the second stage, etching may be performed in a state where the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas not containing carbon atoms and nitrogen atoms and the oxygen-containing gas is set to a second ratio RT2. The second ratio RT2 is greater than the first ratio RT1. The second ratio RT2 may be greater than 35%, greater than 30%, or greater than 25%. In this embodiment, the temperature of the substrate support 14 in the first stage may be the same as the temperature of the substrate support 14 in the second stage. The temperature of the substrate support 14 in the first stage and the second stage may be, for example, less than −50° C. or less than −40° C.
[0080] The duration of the first stage may be, for example, 10 seconds or more and 30 seconds or less. The duration of the second stage may be, for example, 30 seconds or more and 60 seconds or less. The duration of the second stage may be 1 time or more, or 6 times or less, the duration of the first stage. The etching depth of the recess R1 formed during the first stage may be, for example, 100 nm or more or 200 nm or more, and 1 μm or less or 500 nm or less.
[0081] In step ST3, the control unit 80 controls the temperature adjustment mechanism of the plasma processing apparatus 1 to set the temperature of the substrate support 14 to a specified temperature. The control unit 80 controls the exhaust unit 38 to set the pressure of the gas in the chamber 12 to a specified pressure. The control unit 80 controls the gas supply unit 44 to supply a process gas containing a specified type and flow rate of gas into the chamber 12. The control unit 80 controls the plasma generation unit to generate plasma P3 from the process gas. In one embodiment, the control unit 80 controls the high frequency power supply 70A, the high frequency power supply 70B, and the bias power supply 30 to supply high frequency power and bias power.
[0082] 8 is a partially enlarged cross-sectional view of an example of the substrate W in a state after execution of step ST4 in which a sequence including etching and formation of a protective film PF is performed one or more times. In step ST4, step ST2 of forming a protective film PF and step ST3 of etching the bottom R1b of the recess R1 are repeated. Step ST4 is performed until the number of repetitions reaches a threshold value. Step ST4 is performed until the depth DP of the recess R1 reaches a desired depth, as shown in FIG. 8. After step ST4, the depth DP is, for example, 3 μm or more. After step ST4, the aspect ratio of the recess R1 may be 30 or more. When step ST4 is completed, the method MT is completed.
[0083] According to the method MT, it is possible to suppress shape defects (bowing) of the side walls R1s of the recesses R1 formed by etching.
[0084] The mechanism by which bowing of the sidewall R1s of the recess R1 is suppressed is thought to be as follows, but is not limited to this. If the bottom of the recess is etched with the temperature of the substrate support 14 set to a constant temperature, bowing may occur on the sidewall of the recess formed by etching. Alternatively, if the bottom of the recess is etched with the flow rate of the oxygen-containing gas set to a constant rate, bowing may occur on the sidewall of the recess formed by etching.
[0085] The mechanism by which bowing occurs is believed to be as follows, but is not limited to this. When the bottom of a recess is etched while the temperature of the substrate support 14 and the flow rate of the oxygen-containing gas are constant, in the early stages of etching, reaction by-products produced by etching adhere to the side walls of the recess, forming shoulders that protrude inward from the side walls. The size of the shoulders increases as the temperature of the substrate support 14 decreases, and as the flow rate of the oxygen-containing gas increases. In subsequent etching, etching proceeds laterally starting from the shoulders, causing bowing.
[0086] On the other hand, in the above method MT, the bottom R1b of the recess R1 is etched in the first stage while suppressing the formation of a shoulder. More specifically, the bottom R1b of the recess R1 is etched under conditions that suppress the adhesion of reaction by-products to the sidewall R1s of the recess R1 during etching, or that remove the reaction by-products attached to the sidewall R1s by etching. To perform such etching, for example, the temperature of the substrate support 14, the type, mixture ratio and flow rate of the process gas, the pressure in the chamber, the magnitude of the high frequency power and the bias power, etc. are controlled. In one example, the bottom R1b of the recess R1 is etched in a state where the temperature of the substrate support 14 is set to a relatively high first temperature T1. Alternatively, the bottom R1b of the recess R1 is etched in a state where the flow rate of the oxygen-containing gas is set to a relatively low first rate RT1 in the first stage. As a result, the above-mentioned shoulder portion is less likely to form in the first stage (initial stage of etching), and lateral etching starting from the shoulder portion is suppressed, so that the occurrence of bowing is suppressed even after the second stage is completed (after etching is completed).
[0087] Normally, if the temperature of the substrate support 14 is −40° C. or lower at the beginning of etching, shape defects that may occur on the sidewalls of the recesses formed by etching become worse. On the other hand, in the above-described method MT, the temperature of the substrate support 14 is set to a relatively high first temperature T1 in the first stage. This makes it possible to suppress shape defects on the sidewalls R1s of the recesses R1 formed by etching.
[0088] When the width of the recess is small, etching does not proceed linearly downward, which may cause shape defects on the sidewall of the recess. Even in such a case, the method MT can suppress shape defects on the sidewall R1s of the recess R1 formed by etching.
[0089] When the aspect ratio of a recess is large, etching may not proceed linearly downward, which may cause shape defects on the sidewalls of the recess. Even in such a case, the method MT can suppress shape defects on the sidewalls R1s of the recess R1 formed by etching.
[0090] Although various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various additions, omissions, substitutions, and modifications may be made. In addition, elements in different embodiments can be combined to form other embodiments.
[0091] For example, the substrate processing apparatus used to perform the method MT may be any type of plasma processing apparatus. For example, the substrate processing apparatus used to perform the method MT may be an inductively coupled plasma processing apparatus other than the plasma processing apparatus 10. The substrate processing apparatus used to perform the method MT may be a capacitively coupled plasma processing apparatus, an ECR (electron cyclotron resonance) plasma processing apparatus, or a plasma processing apparatus that uses surface waves such as microwaves to generate plasma.
[0092] The substrate processing apparatus used to perform the method MT may include a first chamber for forming a protective film and a second chamber for performing etching, instead of a single chamber. In this case, the substrate W may be transferred between the first and second chambers in a reduced pressure environment. Alternatively, the substrate W may be removed from the reduced pressure environment, transferred between the first and second chambers under atmospheric pressure, and then returned to the reduced pressure environment.
[0093] Various experiments performed to evaluate Method MT will be described below, but the experiments described below are not intended to limit the present disclosure.
[0094] (First experiment)
[0095] In the first experiment, five sample substrates having the same structure as the substrate W shown in FIG. 2 were prepared. Each sample substrate had a silicon-containing film and a mask provided on the silicon-containing film. The silicon-containing film was a silicon single crystal film. In the first experiment, a plasma processing apparatus having the same structure as the plasma processing apparatus 10 in FIG. 3 was used to generate plasma from a processing gas and etch the silicon-containing film of each sample substrate.
[0096] The first sample substrate was subjected to a first etching for 60 seconds, and then, after an interval of 80 seconds, a second etching for 60 seconds was performed. In each of the first and second etchings, the temperature of the substrate support 14 was -50°C. High frequency power was supplied from the high frequency power source 70A to the inner antenna element 52A, and high frequency power was supplied from the high frequency power source 70B to the inner antenna element 52A. In addition, bias power was supplied from the bias power source 30 to the lower electrode 18. In each of the first and second etchings, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 35%. Note that HBr gas and SF6 gas were used as the halogen-containing gas.
[0097] The etching conditions for the second sample substrate were the same as those for the first sample substrate, except that the temperature of the substrate support 14 was -45°C.
[0098] The etching conditions for the third sample substrate were the same as those for the first sample substrate, except that the temperature of the substrate support 14 was −40° C. and the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the first etching was 37%.
[0099] The etching conditions for the fourth sample substrate were the same as those for the first sample substrate, except that the temperature of the substrate support 14 was −35° C. and the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the first etching was 38%.
[0100] The etching conditions for the fifth sample substrate were the same as those for the first sample substrate, except that the temperature of the substrate support 14 was -20°C and the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the first etching was 40%.
[0101] 9(a) to 9(e) are diagrams showing schematic examples of the shapes of the sidewalls of recesses formed by etching. FIG. 9(a) to 9(e) show cross sections of the first to fifth sample substrates, respectively. It can be seen from FIG. 9 that the occurrence of bowing in the sidewalls of the recesses is suppressed as the temperature of the substrate support 14 increases. When the temperature of the substrate support 14 is higher than -40°C, the occurrence of bowing is significantly suppressed.
[0102] (Second experiment)
[0103] In the second experiment, three sample substrates having the same structure as the substrate W shown in FIG. 2 were prepared. Each sample substrate had a silicon-containing film and a mask provided on the silicon-containing film. The silicon-containing film was a silicon single crystal film. In the second experiment, a plasma processing apparatus having the same structure as the plasma processing apparatus 10 in FIG. 3 was used to generate plasma from a processing gas and etch the silicon-containing film of each sample substrate.
[0104] The first sample substrate was subjected to a first etching for 60 seconds, and then, after an interval of 80 seconds, a second etching for 20 seconds was performed. In each of the first and second etchings, the temperature of the substrate support 14 was -50°C. High frequency power was supplied from the high frequency power source 70A to the inner antenna element 52A, and high frequency power was supplied from the high frequency power source 70B to the inner antenna element 52A. In addition, bias power was supplied from the bias power source 30 to the lower electrode 18. In the first etching, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 35%. In the second etching, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 40%. In both the first etching and the second etching, HBr gas and SF6 gas were used as the halogen-containing gas.
[0105] The etching conditions for the second sample substrate were the same as those for the first sample substrate, except that the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the second etching was 35%.
[0106] The etching conditions for the third sample substrate were the same as those for the first sample substrate, except that the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the second etching was 25%.
[0107] Fig. 10 (a) to (c) are diagrams showing schematic examples of the shape of the sidewall of a recess formed by etching. Fig. 10 (a) to (c) show cross sections of the first to third sample substrates, respectively. Fig. 10 shows that the occurrence of a shoulder SH formed on the sidewall of a recess is suppressed as the ratio of the flow rate of O2 gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas decreases. When the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas is 25% or less, the occurrence of a shoulder SH is significantly suppressed.
[0108] (Third experiment)
[0109] In the third experiment, four sample substrates having the same structure as the substrate W shown in FIG. 2 were prepared. Each sample substrate had a silicon-containing film and a mask provided on the silicon-containing film. The silicon-containing film was a silicon single crystal film. In the third experiment, a plasma processing apparatus having the same structure as the plasma processing apparatus 10 in FIG. 3 was used to generate plasma from a processing gas and etch the silicon-containing film of each sample substrate.
[0110] As in the second experiment, the first sample substrate was subjected to a first etching for 60 seconds, and then, after an interval of 80 seconds, a second etching for 20 seconds was performed. After that, a third etching for 40 seconds was performed. In each of the first to third etchings, the temperature of the substrate support 14 was -50°C. High frequency power was supplied from the high frequency power source 70A to the inner antenna element 52A, and high frequency power was supplied from the high frequency power source 70B to the inner antenna element 52A. In addition, bias power was supplied from the bias power source 30 to the lower electrode 18. In the first etching, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 35%. In the second etching, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 40%. In the third etching, the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas was 35%. In both the first etching and the second etching, HBr gas and SF6 gas were used as the halogen-containing gas.
[0111] The etching conditions for the second sample substrate were the same as those for the first sample substrate, except that the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the second etching was 35%.
[0112] The etching conditions for the third sample substrate were the same as those for the first sample substrate, except that the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the second etching was 30%.
[0113] The etching conditions for the fourth sample substrate were the same as those for the first sample substrate, except that the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas in the second etching was 25%.
[0114] Fig. 11 (a) to (d) are diagrams showing examples of the shape of the sidewall of the recess formed by etching. Fig. 11 (a) to (d) show cross sections of the first to fourth sample substrates, respectively. Fig. 11 shows that the occurrence of bowing on the sidewall of the recess is suppressed as the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas decreases. When the ratio of the flow rate of the oxygen-containing gas to the total flow rate of the halogen-containing gas and the oxygen-containing gas is 30% or less, the occurrence of bowing is significantly suppressed.
[0115] From the foregoing, it will be understood that various embodiments of the present disclosure have been described herein for purposes of illustration, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Accordingly, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims. [Explanation of symbols]
[0116] 12: chamber; 14: substrate support; P1, P2, P3: plasma; PF: protective film; R1: recess; R1b: bottom; R1s: side wall; W: substrate.
Claims
1. (a) providing a substrate having a film to be etched, the film having a recess formed therein, on a substrate support; (b) forming a protective film on a side wall of the recess; (c) after (b), generating plasma from a processing gas to etch the bottom of the recess; (d) performing a sequence including (b) and (c) one or more times; Including, The (c) is a first step of etching a bottom of the recess while suppressing the formation of a shoulder caused by a reaction by-product generated by the etching being attached to the sidewall; a second step of further etching the bottom of the recess by controlling the temperature of the substrate support to −40° C. or less after the first step; Including, In the first stage, etching is performed with the temperature of the substrate support set to a temperature higher than -40°C.
2. (a) providing a substrate having a film to be etched, the film having a recess formed therein, on a substrate support; (b) forming a protective film on a side wall of the recess; (c) after (b), generating plasma from a processing gas to etch the bottom of the recess; (d) performing a sequence including (b) and (c) one or more times; Including, The (c) is a first step of etching a bottom of the recess while suppressing the formation of a shoulder caused by a reaction by-product generated by the etching being attached to the sidewall; a second step of further etching the bottom of the recess by controlling the temperature of the substrate support to −40° C. or less after the first step; Including, the film to be etched is a silicon-containing film; the processing gas includes a halogen-containing gas that does not include carbon atoms and nitrogen atoms and an oxygen-containing gas; In the first stage, etching is performed in a state where a ratio of a flow rate of the oxygen-containing gas to a total flow rate of the halogen-containing gas and the oxygen-containing gas is set to a first ratio; In the second stage, etching is performed with the ratio set to a second ratio greater than the first ratio.
3. The halogen-containing gas is SF 6 Gas, Cl 2 3. The method of claim 2, further comprising at least one selected from the group consisting of a nitrogen gas and a hydrogen gas.
4. The oxygen-containing gas is O 2 The method of claim 2 or 3, further comprising a gas.
5. 5. The substrate processing method according to claim 2, wherein the silicon-containing film includes a silicon film or a silicon germanium film.
6. The substrate processing method according to claim 2, wherein the first ratio is equal to or less than 35%.
7. A substrate processing method described in any one of claims 1 to 6, wherein formation of the shoulder is suppressed by suppressing adhesion of the reaction by-products to the side wall and / or by removing the reaction by-products adhered to the side wall.
8. The step (a) is a step of providing the substrate having the recess formed thereon by etching the etching target film in a state in which the temperature of the substrate support is controlled to −40° C. or less; 8. The substrate processing method according to claim 1, wherein the etching conditions in the step (a) are the same as the etching conditions in the second step.
9. 9. The substrate processing method according to claim 1, wherein a period of the second stage is six times or less than a period of the first stage.
10. 10. The substrate processing method according to claim 1, wherein the recess is etched to a depth of 1 μm or less in the first step.
11. 11. The substrate processing method according to claim 1, wherein in (c), the first stage is switched to the second stage while plasma is being generated.
12. The substrate processing method according to any one of claims 1 to 11, wherein the steps (a) to (d) are carried out in-situ.
Citation Information
Patent Citations
Method of manufacturing deep and perpendicular structure to silicon substrate
JP1996250466A
Plasma etching method
JP2013021192A
Etching method and etching apparatus
JP2016213427A
Substrate processing method and substrate processing apparatus
JP2020141103A
Technique to deposit sidewall passivation for high aspect ratio cylinder etch
US9378971B1