Resin composition
The resin composition, featuring a copolymer of polysilane and vinyl monomer with UV-absorbing additives, addresses the limitations of conventional resist films by enhancing UV absorption and heat resistance, enabling high-speed and precise UV laser processing for semiconductor dicing.
Patent Information
- Application Number
- JP2020210793
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-18
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Conventional resist films made of PVA or similar materials have poor heat resistance and low UV laser absorption, limiting high-speed and high-precision processing, and increasing the film thickness exacerbates these issues.
A resin composition comprising a copolymer of a first polysilane and a vinyl monomer, with a second polysilane block of higher molecular weight, and incorporating ultraviolet absorbing monomers like benzotriazole or benzophenone skeletons, enhances UV absorption and heat resistance.
Enables high-speed and high-precision UV laser processing with improved film strength and adhesion, allowing for efficient plasma dicing of semiconductor wafers.
Smart Images

Figure 0007583603000001 
Figure 0007583603000002 
Figure 0007583603000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition, and in particular to a resin composition for use as an ultraviolet laser processing resist. [Background technology]
[0002] Dicing is performed to divide a semiconductor wafer into individual devices. Dicing is generally performed by scribing or sawing. In recent years, plasma dicing, which etches a predetermined portion of a wafer using plasma, has been attracting attention.
[0003] In plasma dicing, a mask made of a resist film is formed on the wafer, and the parts of the wafer exposed through the mask are then plasma etched to separate them into individual devices. The mask must be able to accurately form the pattern for etching, and also be able to protect the elements on the wafer from the plasma.
[0004] The mask can be formed by patterning a photoresist film using standard lithography operations. However, this method has a problem with the cost of mask formation. It has also been considered to form a mask by directly patterning a resist film made of polyvinyl alcohol (PVA) using an ultraviolet (UV) laser instead of a photoresist film (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-165963 A Summary of the Invention [Problem to be solved by the invention]
[0006] Conventional resist films made of PVA and the like have poor heat resistance and low UV laser absorption, which means that processing speeds cannot be increased and high-precision processing is difficult. Adding UV absorbers to resist films has also been considered, but increasing the amount added causes precipitation of the UV absorbers, making it difficult to sufficiently improve UV laser absorption. Furthermore, adding UV absorbers does not solve the problem of low heat resistance of resist films.
[0007] Furthermore, to protect the elements on the wafer from plasma, the resist film needs to be sufficiently thick. However, in the case of conventional resist films made of PVA, increasing the thickness of the film further reduces processability, making it difficult to make the film sufficiently thick.
[0008] An object of the present disclosure is to realize an ultraviolet laser processing resist that can be processed at high speed and with high precision. [Means for solving the problem]
[0009] One embodiment of the resin composition for ultraviolet laser processing resist of the present disclosure contains an ultraviolet-absorbing copolymer having a first block consisting of a first polysilane and a second block which is a copolymer of a vinyl monomer and contains ultraviolet-absorbing monomer units derived from an ultraviolet-absorbing monomer having ultraviolet absorbing properties, and a second polysilane having a molecular weight larger than that of the first polysilane.
[0010] In one embodiment of the resin composition for ultraviolet laser processing resist, the weight average molecular weight of the second polysilane is 10,000 or more and 50,000 or less, and the proportion of the second polysilane can be 5 parts by mass or more and less than 45 parts by mass per 100 parts by mass of the ultraviolet absorbing copolymer.
[0011] In one embodiment of the resin composition for an ultraviolet laser processing resist, the ultraviolet absorbing monomer can have any one of a benzotriazole skeleton, a benzophenone skeleton, and a triazine skeleton.
[0012] In one embodiment of the resin composition for ultraviolet laser processing resist, the proportion of the ultraviolet absorbing monomer unit in the entire ultraviolet absorbing copolymer can be 3 mass% or more and 70 mass% or less, and the proportion of the first polysilane in the entire ultraviolet absorbing copolymer can be 30 mass% or more and 97 mass% or less.
[0013] In one embodiment of the resin composition for ultraviolet laser processing resist, the ultraviolet transmittance at a wavelength of 355 nm can be 2% or less.
[0014] The resist agent of the present disclosure contains the resin composition of the present disclosure and a solvent. Effect of the Invention
[0015] According to the resin composition of the present disclosure, it is possible to realize an ultraviolet laser processing resist that can be processed at high speed and with high precision. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The resist agent of this embodiment contains a resin composition (resist polymer) and a solvent. The resist agent of this embodiment can be directly patterned by an ultraviolet (UV) laser, and can be used, for example, to form a mask for plasma dicing. The resist polymer contained in the resist agent of this embodiment contains an ultraviolet absorbing copolymer having an ultraviolet absorbing effect, which contains a first polysilane, and a second polysilane.
[0017] The ultraviolet absorbing copolymer of this embodiment has a first block made of a first polysilane, and a second block made of a polymer of a vinyl monomer and having ultraviolet absorbing properties.
[0018] The first block is made of a first polysilane, has a main chain formed by silicon-silicon bonds, and has an organic substituent on the side chain. The main chain formed by silicon-silicon bonds may be linear or branched, or may have a ring structure. The organic substituent on the side chain is not particularly limited, and can be preferably an alkyl group, an aryl group, an aralkyl group, or the like. The alkyl group may be linear or branched, or may have a ring structure. It may also be an organic substituent containing a heteroatom. The molecular weight of the polysilane, which is the first block, is not particularly limited, but from the viewpoint of handleability as a resist agent, the number average molecular weight (Mn) is preferably 500 or more, more preferably 800 or more, and preferably 3000 or less, more preferably 2500 or less. The weight average molecular weight (Mw) is preferably 800 or more, more preferably 1000 or more, and preferably 4000 or less, more preferably 3000 or less.
[0019] The second block is made of a polymer of a vinyl monomer, and at least a part of the monomer units constituting the second block is an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having an ultraviolet absorbing group. Therefore, the second block has an ultraviolet absorbing effect. The ultraviolet absorbing group is not particularly limited, but can be, for example, a benzotriazole skeleton, a benzophenone skeleton, or a triazine skeleton. The ultraviolet absorbing monomer may have a vinyl group and an ultraviolet absorbing group, but from the viewpoint of polymerization and the like, an acrylic monomer that is an acrylic acid ester derivative (acrylate) or a methacrylic acid ester derivative (methacrylate) is preferable. Specifically, as the ultraviolet absorbing monomer, 3-(2H-benzotriazol-2-yl)-4-hydroxyphenethyl=methacrylate, 2-(4-benzoyl-3-hydroxyphenoxy)ethyl acrylate, or 2-[4-(4,6-diphenyl)-[1,3,5]triazin-2-yl]-3-hydroxy-phenoxy}-ethylprop-2-enoate, etc. can be used. In the following, acrylate or methacrylate will be referred to as (meth)acrylate.
[0020] The ultraviolet absorbing copolymer containing the first block and the second block can be prepared by mixing and reacting the first polysilane with the ultraviolet absorbing monomer. Radicals can be generated in the first polysilane by irradiation with ultraviolet light, etc., so that the ultraviolet absorbing monomer can be copolymerized with the first polysilane.
[0021] The proportion of the first block in the entire ultraviolet absorbing copolymer is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more, from the viewpoint of heat resistance, and is preferably 97% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, from the viewpoint of exerting an ultraviolet absorbing effect.
[0022] The proportion of the monomer units derived from the ultraviolet absorbing monomer in the entire ultraviolet absorbing copolymer is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and even more preferably 15% by mass or more, from the viewpoint of exerting an ultraviolet absorbing effect, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less, from the viewpoint of heat resistance.
[0023] The ultraviolet absorbing copolymer may contain a monomer unit derived from an ultraviolet non-absorbing monomer that does not have an ultraviolet absorbing group such as a benzotriazole skeleton and does not exhibit ultraviolet absorbing properties. The ultraviolet non-absorbing monomer is not particularly limited, but may be an acrylic monomer such as a (meth)acrylic acid ester or a (meth)acrylamide derivative. By adding a (meth)acrylic acid alkyl ester having an alkyl group with 4 or more carbon atoms, the resist film can be made flexible to improve adhesion to the wafer, and the processability can be further improved. In addition, by adding a hydrocarbon monomer that has a higher plasma etching resistance than polysilane, the plasma resistance of the resist film can be improved.
[0024] The non-UV-absorbing monomer can be copolymerized with the UV-absorbing monomer to form a constituent unit of the second block, or may be included in the UV-absorbing copolymer as a constituent unit of a block different from the second block.
[0025] The proportion of monomer units derived from ultraviolet non-absorbing monomers in the entire ultraviolet absorbing copolymer is preferably 15 mass % or less, and more preferably 10 mass % or less.
[0026] The proportions of the first block, the second block and each monomer unit are based on the amounts charged when polymerizing the ultraviolet absorbing copolymer, but can also be determined by composition analysis of the ultraviolet absorbing copolymer.
[0027] The second polysilane to be mixed with the ultraviolet absorbing copolymer has a higher molecular weight than the first polysilane constituting the first block. Specifically, the weight average molecular weight (Mw) of the second polysilane is preferably 10,000 or more, more preferably 11,000 or more, from the viewpoint of improving the heat resistance and film strength of the resist agent. In addition, from the viewpoint of the coatability (coating liquid viscosity) of the resist agent, it is preferably 50,000 or less, more preferably 20,000 or less.
[0028] By adding the second polysilane having a higher molecular weight than the first polysilane, the heat resistance and film strength of the resist film formed can be improved. This improves the crack resistance of the resist film and its adhesion to the film formation surface. Even when a relatively thick resist film is formed, high-speed processing can be performed.
[0029] The resist film using the resist polymer of this embodiment can be laser processed at a processing speed of more than 600 mm / s, and can be processed satisfactorily even at 700 mm / s or 800 mm / s, and shows sufficient processability up to about 1000 mm / s. Laser processing at a processing speed of 600 mm / s or less is also possible.
[0030] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer in the resist polymer of this embodiment is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, from the viewpoint of heat resistance and film strength, and is preferably 45 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less, from the viewpoint of coatability.
[0031] The resist agent of this embodiment can be prepared by dissolving the ultraviolet absorbing copolymer and the second polysilane in a solvent, or by mixing a solution in which the ultraviolet absorbing copolymer is dissolved with a solution in which the second polysilane is dissolved.
[0032] The solvent is not particularly limited as long as it can dissolve the resist polymer, and may be, for example, toluene, tetrahydrofuran, methyl ethyl ketone, propylene glycol monomethyl ether acetate, cyclohexanone, etc. The solvent may be a mixed solvent containing a plurality of solvents.
[0033] The proportion of the resist polymer in the entire resist agent can be adjusted depending on the thickness of the resist film to be formed, etc., but is preferably 10 mass % or more, more preferably 25 mass % or more, and preferably 70 mass % or less, more preferably 60 mass % or less.
[0034] The resist agent may not contain any components other than the resist polymer and the solvent, but may contain other components. Examples of other components include additive components such as leveling agents, light stabilizers, and antioxidants, and polymer components such as acrylic resins, polyester resins, and epoxy resins. The ratio of other components is 10 parts by mass or less, more preferably 5 parts by mass or less, per 100 parts by mass of the resist polymer. In addition, the resist agent may contain residues such as unpolymerized polysilane and vinyl polymer when the first polymer and the second polymer are polymerized.
[0035] The resist agent of this embodiment can be coated on the surface of a wafer by a method such as spin coating to form a resist film. The formed resist film can be patterned by removing street portions by irradiation with a UV laser. The patterned resist film can be used as a mask to irradiate the wafer with plasma and etch the wafer, thereby performing dicing of the wafer. The thickness of the resist film formed on the surface of the wafer is not particularly limited, but is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 25 μm or more from the viewpoint of resist properties, and is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less from the viewpoint of laser processability.
[0036] The wavelength of the UV laser light used for patterning the resist agent of this embodiment is not particularly limited, but may be about 200 nm to 400 nm, and preferably 355 nm. The frequency of the laser light is also not particularly limited, but may be, for example, about 1 kHz to 300 kHz, and a high frequency is preferable from the viewpoint of high speed processing.
[0037] The resist agent of the present embodiment can be processed at high speed even if the resist film is thick. Therefore, it is particularly excellent as a resist agent for forming a resist film for plasma dicing of a wafer. In addition, it can be used as a protective film for processes that require heat resistance, such as a resist agent that can be laser patterned, not limited to plasma dicing of a wafer. EXAMPLES
[0038] The resin composition of the present disclosure will be described in more detail below using examples. The following examples are illustrative and are not intended to limit the present invention.
[0039] <Formation of resist film> The prepared resist agent was applied to the surface of a silicon wafer (φ8 inch, thickness 700 μm) using a spin coater, and the solvent was dried to form a resist film. The rotation speed of the spin coater was 200 rpm, and the thickness of the resist film was 30 μm.
[0040] <Evaluation of liquid stability over time> The prepared resin solution was placed in a transparent, sealed container and allowed to stand at room temperature for 7 days, after which the appearance of the resin solution and the presence or absence of precipitate were visually observed and the liquid stability over time was evaluated according to the following evaluation criteria.
[0041] (Evaluation Criteria) A: The solution is free of turbidity and precipitate.
[0042] B: Slight cloudiness but no sediment.
[0043] C: Separation or precipitation is observed.
[0044] <Evaluation of heat resistance> 5 g of the produced resin solution was placed in an aluminum cup and dried in an oven at 100°C for 180 minutes to evaporate the solvent. The non-volatile components remaining in the aluminum cup were measured for 10% weight loss temperature using a thermogravimetric differential thermal analyzer (TG-DTA). The measurement conditions were a temperature rise rate of 20°C / min and heating from 30°C to 600°C in a nitrogen atmosphere. The measurement results were evaluated for heat resistance according to the following evaluation criteria.
[0045] (Evaluation Criteria) A: The 10% weight loss temperature is 250℃ or higher.
[0046] B: The 10% weight loss temperature is 200°C or higher and less than 250°C.
[0047] C: 10% weight loss temperature is less than 200°C.
[0048] <Evaluation of coating surface quality> The surface condition of the formed resist film was visually observed and the coating surface quality was evaluated according to the following evaluation criteria.
[0049] (Evaluation Criteria) A: The coating is uniform and free of irregularities.
[0050] B: Slight unevenness (citrus peel) is observed.
[0051] C: The coating has defects such as cracks and graininess.
[0052] <Evaluation of laser processability> The surface of the formed resist film was patterned using a UV laser processing device (AL300P, manufactured by Tokyo Seimitsu) to create a checkerboard pattern with a line width of 15 μm, line length of 15 mm, and a pitch of 1 mm. The processing conditions were laser wavelength: 355 nm, pulse width: <15 ns, and frequency: 50 kHz. The processing speed was 600 mm / sec or 800 mm / sec. The laser-processed portion was observed at a magnification of 200 times using a microscope, and the laser processability was evaluated according to the following evaluation criteria.
[0053] (Evaluation Criteria) A: There is no peeling of the coating film at the laser processed edge, and no resist residue.
[0054] B: A small amount of resist residue remains on the laser processed edge.
[0055] C: Part of the resist film remains in the laser irradiated area, or defects such as peeling of the coating film or cracks are found on the laser processed edge.
[0056] <Evaluation of resist properties> After evaluating the laser processability, a plasma etching process was performed from the resist film side using a plasma etching device. The processing conditions were as follows: plasma source: ICP plasma power 2200 W, process gas: SF6 gas, gas pressure: 2 Pa, processing time: 7 minutes. The surface of the resist film after the plasma etching process was observed at 200 times magnification using a microscope, and the resist properties were evaluated according to the following evaluation criteria.
[0057] (Evaluation Criteria) A: There is no erosion of the resist film by plasma etching.
[0058] B: Erosion by plasma etching is observed, but there is no exposure of the silicon wafer.
[0059] C: The resist film disappears, and exposure of the silicon wafer is observed.
[0060] <Measurement of UV transmittance> The prepared resin solution was applied to the surface of a polyethylene terephthalate (PET) film with a thickness of 50 μm using a spin coater to form a resin film. The film thickness after drying of the resin film was 10 μm. The transmittance of ultraviolet light with a wavelength of 355 nm was measured for the PET film on which the resin film was formed using a spectrophotometer. The transmittance of the resin film was obtained by subtracting the transmittance of the PET film before forming the resin film as a blank.
[0061] (Example 1) The ultraviolet-absorbing copolymer having an ultraviolet-absorbing action containing polysilane was a copolymer of a first polysilane and a methacrylate-based ultraviolet-absorbing monomer having a benzotriazole skeleton. As the first polysilane, one having a number average molecular weight (Mn) of 900 and a weight average molecular weight (Mw) of 1100 (Oxsol SI-20-10, manufactured by Osaka Gas Chemical Co., Ltd.) was used. The ultraviolet-absorbing monomer was (3-(2H-benzotriazol-2-yl)-4-hydroxyphenethyl methacrylate, RUVA-93, manufactured by Otsuka Chemical Co., Ltd.). 44.2 g of the first polysilane and 15.8 g of the ultraviolet-absorbing monomer were dissolved in 40 g of toluene and copolymerized to obtain a solution of the ultraviolet-absorbing copolymer. The copolymerization was carried out by irradiating with ultraviolet light for 60 minutes using a high-pressure mercury lamp (UV intensity: 170 mW / cm 2 ) with the liquid temperature set at 60 °C to 70 °C under a nitrogen stream.
[0062] When the polymer separated from the obtained UV-absorbing copolymer solution by gel permeation chromatography (GPC) was analyzed by infrared spectroscopy (IR), a spectrum was obtained that was a composite of the spectrum of the polysilane and the spectrum of the UV-absorbing monomer. 1 HNMR spectroscopy confirmed the peaks of acrylic polymer chains at chemical shifts of 0.5 ppm to 4.5 ppm. From these results, it was determined that the obtained ultraviolet absorbing copolymer was a copolymer of polysilane and an ultraviolet absorbing monomer. The Mw of the obtained ultraviolet absorbing copolymer was 3900.
[0063] The second polysilane used had a number average molecular weight (Mn) of 2100 and a weight average molecular weight (Mw) of 12700 (Oxol SI-10-10, manufactured by Osaka Gas Chemicals). 3.2 g of the second polysilane was dissolved in 23.2 g of toluene to prepare a solution of the second polysilane.
[0064] A resist agent was prepared by mixing a solution of the ultraviolet absorbing copolymer and a solution of the second polysilane. The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer in the resist agent was 5.3 parts by mass. The solid content ratio of the ultraviolet absorbing copolymer and the second polysilane in the resist agent was 50% by mass. The obtained resist agent was evaluated for liquid stability over time, coating surface quality, laser processability, resist properties, heat resistance, and UV transmittance. The liquid stability over time was A, the coating surface quality of the resist film was A, the laser processability was A when the processing speed was 600 mm / s and B when it was 800 mm / s, the resist properties were A, the heat resistance was A, and the UV transmittance was 0%.
[0065] Example 2 The same procedure as in Example 1 was carried out except that 6.7 g of the second polysilane was dissolved in 26.7 g of toluene to prepare a solution of the second polysilane.
[0066] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 11.2 parts by mass, and the ratio of solids in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0067] Example 3 The same procedure as in Example 1 was carried out except that 15.0 g of the second polysilane was dissolved in 35.0 g of toluene to prepare a solution of the second polysilane.
[0068] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 25.0 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0069] Example 4 The same procedure as in Example 1 was carried out except that 25.7 g of the second polysilane was dissolved in 45.7 g of toluene to prepare a solution of the second polysilane.
[0070] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 42.8 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was B, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0071] Example 5 The procedure was the same as in Example 2, except that an ultraviolet absorbing copolymer was polymerized from 57.0 g of the first polysilane and 3.0 g of the ultraviolet absorbing monomer.
[0072] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 11.2 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A when the processing speed was 600 mm / s and B when it was 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0073] Example 6 The procedure was the same as in Example 2, except that an ultraviolet absorbing copolymer was polymerized from 18.0 g of the first polysilane and 42.0 g of the ultraviolet absorbing monomer.
[0074] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 11.2 parts by mass, and the ratio of solid content in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was B, and the UV transmittance was 0%.
[0075] Example 7 The procedure was the same as in Example 2, except that the first polysilane had a number average molecular weight (Mn) of 1100 and a weight average molecular weight (Mw) of 1800 (Oxol SI-10-20, manufactured by Osaka Gas Chemicals).
[0076] The ratio of the second polysilane to 100 parts by mass of the ultraviolet absorbing copolymer was 11.2 parts by mass, and the ratio of solids in the resist agent was 50% by mass. The liquid stability over time was A, the coating surface quality was A, the laser processability was A at both processing speeds of 600 mm / s and 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0077] The conditions and evaluation results of Examples 1 to 7 are shown in Table 1.
[0078] [Table 1]
[0079] (Reference example 1) The ultraviolet absorbing copolymer was prepared by dissolving 52.5 g of polysilane and 22.5 g of ultraviolet absorbing monomer in 75 g of toluene and copolymerizing them, and the resist agent was prepared without adding the second polysilane. The resist film was evaluated with a thickness of 10 μm.
[0080] The liquid stability over time was A, the coating surface quality was A, the laser processability was A at a processing speed of 600 mm / s and B at 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0081] (Reference example 2) The same procedure as in Reference Example 1 was repeated, except that the evaluation was performed with the resist film having a thickness of 30 μm.
[0082] The liquid stability over time was A, the coating surface quality was A, the laser processability was A when the processing speed was 600 mm / s and C when it was 800 mm / s, the resist property was A, the heat resistance was A, and the UV transmittance was 0%.
[0083] The conditions and evaluation results of Reference Examples 1 and 2 are shown in Table 2.
[0084] [Table 2]
[0085] Comparative Example 1 The resist agent was prepared by dissolving 75.0 g of polyvinyl alcohol (PVA-205, manufactured by Kuraray) in 75.0 g of distilled water.
[0086] The liquid stability over time was A, the coating surface quality was A, the laser processability was C at a processing speed of 600 mm / s, the resist property was A, the heat resistance was C, and the UV transmittance was 90%. Note that the processability at a processing speed of 800 mm / s was not evaluated.
[0087] Comparative Example 2 The resist agent was prepared by dissolving 75.0 g of polysilane (Ogsol SI-20-10, manufactured by Osaka Gas Chemicals) in 75.0 g of toluene.
[0088] The liquid stability over time was A, the coating surface quality was A, the laser processability was C at a processing speed of 600 mm / s, the resist property was B, the heat resistance was A, and the UV transmittance was 63%. Note that the processability at a processing speed of 800 mm / s was not evaluated.
[0089] Comparative Example 3 The procedure was the same as in Example 1, except that the resist agent was a solution of 52.5 g of polysilane (Oxol SI-20-10, manufactured by Osaka Gas Chemicals) and 22.5 g of a benzotriazole-based ultraviolet absorber (2-(2-hydroxy-5-t-butylphenyl)benzotriazole, Tinuvin PS, manufactured by BASF Japan) dissolved in 75.0 g of toluene. The liquid stability over time was C, the coating surface quality was C, and other items could not be evaluated.
[0090] The conditions and evaluation results of Comparative Examples 1 to 3 are shown in Table 3.
[0091] [Table 3]
[0092] Comparative Example 4 The procedure was the same as in Example 1, except that a solution of 3.2 g of an acrylic resin (Dianal BR-113, manufactured by Mitsubishi Chemical) having a number average molecular weight of 30,000 was dissolved in 23.2 g of toluene was used instead of the solution of the second polysilane. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.
[0093] Comparative Example 5 The procedure was the same as in Comparative Example 4, except that 57.0 g of the first polysilane and 3.0 g of the ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to prepare an ultraviolet absorbing copolymer solution. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.
[0094] Comparative Example 6 The procedure was the same as in Comparative Example 4, except that 18.0 g of the first polysilane and 42.0 g of the ultraviolet absorbing monomer were dissolved in 40 g of toluene and copolymerized to prepare an ultraviolet absorbing copolymer solution. The liquid stability over time was B, the coating surface quality was C, and other items could not be evaluated.
[0095] Comparative Example 7 The procedure was the same as in Example 1, except that instead of the solution of the second polysilane, a solution containing 3.2 g of a polyester resin (Vylon UR-1400, manufactured by Toyobo) having a number average molecular weight of 40,000 and toluene was added to the solution to adjust the amount of solvent to 23.2 g was used. The liquid stability over time was rated C, the coating surface quality was rated C, and other items could not be evaluated.
[0096] The conditions and evaluation results of Comparative Examples 4 to 7 are shown in Table 4.
[0097] [Table 4] [Industrial Applicability]
[0098] INDUSTRIAL APPLICABILITY The resin composition of the present disclosure has excellent laser processability and is useful as an ultraviolet laser processing resist, etc.
Claims
1. an ultraviolet absorbing copolymer having a first block made of a first polysilane and a second block which is a copolymer of a vinyl monomer and contains an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having an ultraviolet absorbing effect; A second polysilane having a molecular weight greater than that of the first polysilane, The resin composition for a resist for ultraviolet laser processing, wherein the ultraviolet absorbing monomer has any one of a benzotriazole skeleton, a benzophenone skeleton, and a triazine skeleton.
2. A resin composition for ultraviolet laser processing resist as described in claim 1, having an ultraviolet transmittance of 2% or less at a wavelength of 355 nm.
3. An ultraviolet absorbing copolymer having a first block composed of a first polysilane and a second block which is a copolymer of a vinyl monomer and contains an ultraviolet absorbing monomer unit derived from an ultraviolet absorbing monomer having an ultraviolet absorbing effect; A second polysilane having a molecular weight greater than that of the first polysilane, A resin composition for use as a resist for ultraviolet laser processing, having an ultraviolet transmittance of 2% or less at a wavelength of 355 nm.
4. A resin composition for ultraviolet laser processing resist as described in claim 3, wherein the ultraviolet absorbing monomer has any one of a benzotriazole skeleton, a benzophenone skeleton, and a triazine skeleton.
5. The weight average molecular weight of the second polysilane is 10,000 or more and 50,000 or less, The proportion of the second polysilane is 5 parts by mass or more and less than 45 parts by mass with respect to 100 parts by mass of the ultraviolet absorbing copolymer. The resin composition for ultraviolet laser processing resist according to any one of claims 1 to 4.
6. a ratio of the ultraviolet absorbing monomer unit to the entire ultraviolet absorbing copolymer is 3 mass% or more and 70 mass% or less, The resin composition for ultraviolet laser processing resist according to any one of claims 1 to 5, wherein the proportion of the first polysilane in the entire ultraviolet absorbing copolymer is 30 mass% or more and 97 mass% or less.
7. A resist agent comprising the resin composition according to any one of claims 1 to 6 and a solvent.
Citation Information
Patent Citations
Method for forming pattern on substrate by ultraviolet laser beams
JP1991109553A
Preparation of polysilane block copolymer
JP1997255785A
Silicon-based positive resist composition, and patterning method
JP2002226664A
Ultraviolet curable ultraviolet-shielding resin composition
JP2006307151A
Pattern-forming method, photosensitive adhesive sheet, method for forming light shielding pattern on lens sheet, method and device for manufacturing transmission-type screen, transmission type screen and projection-type image display device
JP2007017790A