Polyester film and device containing same
A biaxially oriented coextruded polyester film with a copolyester base layer and PET outer layers addresses the need for improved thermoformable materials by providing enhanced chemical and mechanical properties, enabling high-temperature thermoforming without microcracking and maintaining shape retention, suitable for electronic device applications.
Patent Information
- Application Number
- JP2020526269
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-11-13
- Filing Date
- 2018-11-13
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2038-11-13
AI Technical Summary
There is a need for improved thermoformable materials with enhanced chemical and scuff resistance, mechanical properties, and printability, while maintaining thermoformability, particularly in polycarbonate films used in electronic devices such as touch screens, and requiring ease of production and reduced thickness.
A biaxially oriented coextruded polyester film comprising a copolyester base layer and polyethylene terephthalate outer layers, with specific compositional and structural characteristics, including a copolyester derived from terephthalic acid and isophthalic acid, which provides excellent thermoformability, chemical resistance, and mechanical strength, and can be thermoformed at high temperatures without microcracking.
The film exhibits high optical clarity, excellent chemical resistance, scratch resistance, and mechanical properties, with improved thermoformability and dimensional stability, allowing it to be thermoformed at high temperatures and retain its shape, while being thinner than conventional polycarbonate films.
Smart Images

Figure 0007583610000001 
Figure 0007583610000002 
Figure 0007583610000003
Abstract
Description
[Technical field]
[0001] The present invention relates to thermoformable polyester films and their use in electronic devices, particularly in the touch screen interfaces of such devices. [Background technology]
[0002] Polymeric films have been widely used in screens, including touch screens for electronic devices, due to their advantageous combination of mechanical strength, dimensional stability and optical properties. The primary applications of such devices are in the automotive, home appliance and consumer electronics markets, where consumers have a greatly increased demand for more design flexibility and interaction with products through touch screen interfaces, especially through capacitance. In-mold electronics (IME) or in-mold decoration (IMD) technology utilizes polymeric films for the assembly of such screens using injection molded parts. A specific embodiment of such technology is film insert molding (FIM), where a film is printed, formed and filled by injection molding. These processes allow labeling and graphic indicia to be applied to plastic parts during the molding process, and also allow components to be integrated into a single unit. Applications for this technology are varied and include automotive and industrial instrument panels, displays, home appliance instrument panels, medical device instrument panels, consumer electronics body parts, and automotive interior decoration.
[0003] Polycarbonate (PC) film has traditionally been utilized for such applications due to its excellent thermoformability, printability and optical transparency, and is the current industry standard. Typically, the polymer film is printed with information and / or graphic indicia on the inner surface before being thermoformed, and then infilled with plastic material in an injection molding process, resulting in a rigid module, typically at least about 1 mm thick, with the graphic indicia layer being protected behind the film. Once thermoformed, the film should exhibit no or minimal relaxation in high temperature and / or humid conditions to avoid loss of the thermoformed shape. Thermoformed films should also exhibit good chemical resistance. Thermoformed films should also exhibit good abrasion resistance, which is usually imparted to polycarbonate thermoformable films by application of an additional hard coat to the film surface. Summary of the Invention
[0004] However, there is a need for improved thermoformable materials. In particular, there is a need to improve the chemical resistance and / or abrasion resistance and / or mechanical properties of thermoformable films, and to simplify manufacturing, while at least maintaining the thermoformable properties of currently available films, in particular known polycarbonate films. The mechanical property in particular sought to be improved is flex resistance. The films should also exhibit good or improved printability, in particular with conductive inks. It is also desirable to reduce the thickness of thermoformable polymeric films. It is an object of the present invention to address one or more of the problems mentioned above. According to a first aspect of the invention, there is provided a thermoformable biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first polyester outer layer A1 and a second polyester outer layer A2, said outer layers being arranged on opposite surfaces of said base layer, (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of about 5 to about 20 mol % of the acid fraction of the copolyester, the copolyester comprising at least 90% by weight of the total weight of the base layer; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) A polyester film is provided, wherein the thickness of the base layer comprises at least 90% of the total thickness of the coextruded multilayer polyester film.
[0005] The inventors have unexpectedly found that polyester films can provide excellent thermoformability while retaining the high optical transparency required for use as screens in electronic devices, and the high dimensional stability required to withstand the high temperatures encountered during device fabrication.The thermoformable polyester film of the present invention can be thermoformed at the high thermoforming temperatures used for conventional polycarbonate films, can withstand downstream processing, and does not develop microcracks.The polyester film exhibits excellent chemical resistance, abrasion resistance, and mechanical properties, especially flex resistance.In addition, the thermoformable polyester film has a higher modulus compared to polycarbonate, and is thinner and exhibits the required mechanical strength. The biaxially oriented coextruded polyester films described herein are self-supporting films or sheets, by which is meant a film or sheet that can exist independently without a supporting base. In the present invention, both the base layer and each of the outer layers are self-supporting. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006] The polyester forming the multilayer film is preferably a synthetic linear polyester. The polyester is preferably a thermoplastic polyester. Suitable polyesters are obtained by condensing one or more dicarboxylic acids or their lower alkyl (up to 6 carbon atoms) diesters with one or more diols. The dicarboxylic acid component contains at least one aromatic dicarboxylic acid, preferably terephthalic acid (TA). Isophthalic acid (IPA) is also present in the copolyester of the base layer. The diol is preferably selected from aliphatic diols, preferably from ethylene glycol (EG). The polyester resins forming the film (i.e., the polyesters and copolyesters described in more detail below) are the major components of the layers of the multilayer film, and account for at least 50% by weight of the total weight of a given layer, preferably at least 65% by weight, typically at least 80% by weight, more typically at least 85% by weight of the total weight of a given layer.
[0007] Each of the polyester outer layers A1 and A2 comprises PET. PET is a crystalline polyester. Preferably, the polyester is a homopolyester, i.e., it contains only one glycol, namely ethylene glycol, and one aromatic dicarboxylic acid, namely terephthalic acid. The polyester of the outer layers may contain small amounts of one or more residues derived from other dicarboxylic acids and / or diols, but if such small amounts are present, the total amount of other dicarboxylic acid(s) is preferably 5.0 mol % or less, preferably 3.0 mol % or less, preferably 2.0 mol % or less, preferably 1.5 mol % or less, preferably 1.0 mol % or less, and / or the total amount of other diol(s) is preferably 5.0 mol % or less, preferably 3.0 mol % or less, preferably 2.0 mol % or less, preferably 1.5 mol % or less, preferably 1.0 mol % or less, of the total diol fraction of the polyester. Preferably, PET (preferably PET homopolyester) is the only polyester in the outer layers A1 and A2. The polyester preferably constitutes at least 50% by weight of the total weight of the outer layer, preferably at least 65%, preferably at least 80%, preferably at least 85%, preferably at least 90%, preferably at least 95%, preferably at least 98%, preferably at least 99%, preferably substantially all of the total weight of the outer layer. In one advantageous embodiment, the or each outer layer consists or essentially consists of said polyester. The polyester itself preferably has an intrinsic viscosity of at least about 0.60, typically no more than 0.70, typically no more than 0.65.
[0008] Preferably, the copolyester of the base layer is derived from a monomer selected from the group consisting of terephthalic acid (TA), a second aromatic dicarboxylic acid, and ethylene glycol, the monomers from which said copolyester is derived being terephthalic acid (TA), a second aromatic dicarboxylic acid, and ethylene glycol. Preferably, the copolyester contains ethylene glycol as the only diol. The copolyester may contain minor amounts of one or more residues derived from other diols, but when such minor amounts are present, the total amount of said other diol(s) is preferably 5.0 mol % or less, preferably 3.0 mol % or less, preferably 2.0 mol % or less, preferably 1.5 mol % or less, preferably 1.0 mol % or less of the total diol fraction of the copolyester. The second aromatic dicarboxylic acid preferably contains a single aromatic ring, and is preferably isophthalic acid (IPA). The second aromatic dicarboxylic acid is present in an amount of about 5 to about 20 mol %, preferably about 8 to about 16 mol %, preferably about 10 to about 14 mol %, preferably about 12 mol %, of the acid fraction of the copolyester.
[0009] The copolyester of the base layer preferably has a crystalline melting point (Tm) within the range of about 210 to about 240°C, preferably about 215 to about 235°C, preferably about 220 to about 230°C. The copolyester of the base layer preferably has a glass transition temperature (Tg) within the range of about 60 to about 90°C, preferably about 65 to about 85°C, and preferably about 70 to about 80°C. The intrinsic viscosity of the copolyester itself is preferably at least about 0.60, preferably at least about 0.65, preferably no more than 0.70. The copolyester of the base layer preferably has a lower melting point than the polyester of the outer layer, and preferably the melting point of the copolyester is at least about 10°C, preferably at least about 25°C, preferably at least about 40°C, lower than the melting point of the polyester of the outer layer, and preferably at least about 60°C, preferably at least about 50°C, lower than the melting point of the polyester of the outer layer. The copolyester constitutes at least 90% by weight, preferably at least 95% by weight, preferably at least 98% by weight, preferably at least 99% by weight, preferably substantially all, of the total weight of the base layer. In one advantageous embodiment, the base layer consists or essentially consists of said copolyester.
[0010] The formation of the polyesters and copolyesters described herein above is conveniently carried out by condensation or transesterification in a known manner, generally at temperatures up to about 295° C. In a preferred embodiment, solid state polymerization can be used to increase the intrinsic viscosity of the polyester to the desired value, for example, using a fluidized bed, such as a nitrogen fluidized bed or a vacuum fluidized bed, using a rotary vacuum dryer, using conventional techniques well known in the art. In the following description of polymer and film manufacture, the term "polyester" should be understood to include "copolyester." The formation of the multilayer polyester film of the present invention is carried out by conventional coextrusion techniques well known in the art. Generally speaking, the coextrusion process involves coextrusion of each polyester composition through independent orifices of a multi-orifice die followed by joining of the still molten layers, or preferably by single-channel coextrusion in which the molten streams of each polyester are first joined in a channel leading to a manifold of the die and then extruded together from the orifice of the die under streamline flow conditions without intermixing, thereby resulting in a superposed film. Thus, the copolyester of the base layer and the polyesters of the outer layers (A1) and (A2) are coextruded. The extrusion is generally carried out at a temperature in the range of about 250 to about 300° C., followed by quenching the extrudate and orienting the quenched extrudate. Preferably, the copolyester forming the base layer is extruded at a temperature lower than that used for extrusion of the polyester forming the outer layer. Preferably, the polyester forming the outer layer is extruded at a temperature of about 260 to about 300°C, preferably about 260 to about 280°C.
[0011] Orientation may be performed by any process known in the art for producing oriented films, such as tubular or flat film processes. Biaxial orientation is performed by stretching in two mutually perpendicular directions in the plane of the film to achieve a satisfactory combination of mechanical and physical properties. In a tubular process, simultaneous biaxial orientation can be accomplished by extruding a thermoplastic polyester tube, which is then quenched, reheated, and then expanded by internal gas pressure to induce transverse orientation and stretched at a rate to induce longitudinal orientation. In a preferred flat film process, the polyester forming the film is extruded through a slot die and quickly quenched on a chilled casting drum to ensure that the polyester is quenched to an amorphous state. Orientation is then performed by stretching the quenched extrudate in at least one direction at a temperature above the glass transition temperature of the polyester materials (i.e., both the copolyester of the base layer and the polyester of the outer layers). Sequential orientation can be performed by stretching the flat, quenched extrudate first in one direction, usually the machine direction, i.e., forward through the machine that stretches the film, and then in the transverse direction. Forward stretching of the extrudate is conveniently performed over a set of rotating rolls or between two pairs of nip rolls, and then transverse stretching is performed in a tentering device. Stretching is generally performed so that the dimensions of the oriented film are 2 to 5 times, more preferably 2.5 to 4.5 times, preferably 2.5 to 3.5 times, and more preferably about 3.0 to about 3.4 times its original dimensions in the or each direction of stretching. Typically, stretching is performed at a temperature above the Tg of the polyester, preferably about 15° C. above the Tg. If orientation is required in only one direction, larger stretch ratios (e.g., up to about 8 times) can be used. Equal stretch in the machine and transverse directions is not necessary, although this may be preferred if balanced properties are desired.
[0012] The stretched film can be, and preferably is, dimensionally stabilized by heat setting at supported dimensions at a temperature above the glass transition temperature of the polyesters but below their melting temperature which induces the desired crystallization of the polyesters. During heat setting, a small dimensional relaxation is preferably performed in the transverse direction (TD) by a procedure known as "toe-in". In the present invention, the dimensional relaxation during heat setting is preferably within the range of about 0 to about 10.0%, preferably about 2.0 to about 10.0%, preferably 6.0% or less, preferably 5.0% or less, preferably 4.0% or less, preferably within the range of about 2.0 to about 4.0%. Similar dimensional relaxation in the process or machine direction (MD) is difficult to achieve because low tension in the running direction is required, making control and winding of the film problematic. The actual heat setting temperature and time will vary depending on the composition of the film and its desired final heat shrinkage, but should not be selected to substantially degrade the toughness properties of the film, such as tear resistance. Within these constraints, a heat-setting temperature of about 165 to 245°C is generally desirable, preferably about 230°C or less, preferably about 220°C or less, preferably about 215°C or less, preferably about 185 to about 215°C, preferably about 190 to about 210°C. In a particularly preferred embodiment, at least a portion of the heat-setting step is carried out at a temperature in the range of about 205 to about 215°C, preferably about 210°C. In a particularly preferred embodiment, the heat-setting is carried out in a multi-zone (preferably 3 or 4 zones) crystallizer, preferably the temperature of the final zone is lower than that of the first zone, preferably each zone is at a successively lower temperature within the above range, preferably the first zone is at a temperature in the range of about 205 to about 215°C, and the final zone is at a temperature in the range of about 165 to about 215°C, preferably in the range of about 165 to about 200°C, preferably in the range of about 165 to about 190°C, preferably in the range of about 170 to about 190°C. In the process of making the films of the present invention, the combination of toe-in and heat-set temperatures referred to above is important in producing the desired crystallinity, dimensional stability, chemical and mechanical properties.
[0013] After heat setting, the film is typically quickly quenched to induce the desired crystallinity in the polyester material. The film can be further stabilized through the use of an in-line relaxation stage. Alternatively, the relaxation treatment can be performed offline. In this additional step, the film is heated at a lower temperature and at much lower MD and TD tensions than in the heat-set stage. The tensions the film is subjected to are low tensions, typically less than 5 kg / m, preferably less than 3.5 kg / m, more preferably in the range of 1 to about 2.5 kg / m, and typically in the range of 1.5 to 2 kg / m of film width. Due to the relaxation process controlling the film speed, the decrease in film speed (and therefore the relaxation of strain) is typically in the range of 0 to 2.5%, preferably 0.5 to 2.0%. There is no increase in the transverse dimensions of the film during the heat stabilization step. The temperature to be used for the heat stabilization step can be varied depending on the desired combination of properties of the final film, with higher temperatures producing better properties, i.e. less residual shrinkage. Temperatures of 135-250°C are generally desirable, preferably 150-230°C, and more preferably 170-200°C. The duration of heating will depend on the temperature used but is typically in the range of 10-40 seconds, with durations of 20-30 seconds being preferred. This heat stabilization process can be carried out by a variety of methods, including flat and vertical configurations and either "off-line" as a separate process step or "in-line" as a continuation of the film manufacturing process. Films so processed will exhibit less thermal shrinkage than those produced in the absence of such post-heat-set relaxation.
[0014] Thus, in a second aspect of the present invention, there is provided a process for producing the thermoformable polyester film described herein, comprising the steps of: (i) co-extruding said copolyester base layer B, said first polyester outer layer A1 and said second polyester outer layer A2 such that said outer layers are disposed on opposing surfaces of said base layer; (ii) quenching the extrudate; (iii) stretching the quenched extrudate in at least one direction at a temperature above the glass transition temperature of the polyester material; and (iv) heat setting the stretched film at a temperature in the range of about 185°C to about 215°C, during which dimensional relaxation in the transverse dimensions of the film occurs in the range of about 2% to about 10%. A process is provided that includes:
[0015] The preferences disclosed herein above for the first aspect of the invention also apply to the second aspect. The base layer and / or one or both outer layers may also contain one or more additives conventionally used in the manufacture of polymeric films. Thus, agents such as crosslinkers, dyes, fillers, pigments, lubricants, radical scavengers, heat stabilizers, antioxidants, UV stabilizers, hydrolysis stabilizers, flame retardants and inhibitors, antiblocking agents, surfactants, lubrication aids, gloss improvers, prodegradants, viscosity modifiers and dispersion stabilizers may be incorporated as appropriate. Such components may be introduced into the polymer in a conventional manner. For example, by mixing with the monomer reactants from which the film-forming polymer is derived, or the components may be mixed with the polymer by somersaulting or dry blending, or by compounding in an extruder, followed by cooling and usually subdivision into granules or chips. Milling techniques may also be used.
[0016] In particular, the layers may contain one or more UV stabilizers, especially when the multilayer film is intended for use in exterior applications.UV stabilizers are particularly advantageous in outer layers, especially in layers that are exposed to the atmosphere during use (i.e., disposed on or forming the outer surface of the screen or electronic device that contains it).Typically, the UV stabilizer is an organic UV stabilizer, such as the organic UV stabilizers disclosed in WO-2012 / 123699-A, the disclosure of which is incorporated herein by reference.A preferred class of UV stabilizers is hydroxyphenyltriazines, especially hydroxyphenyltriazine compounds of formula (II):
[0017] [ka] (II) In the formula (II), R is selected from the group consisting of hydrogen, halogen, and C1-C 12 C1-C substituted with alkoxy 18 alkyl, C2-C6 alkyl, or benzyl; R 4 and R 5 is independently selected from hydrogen, alkyl, alkoxy or phenyl. R is preferably C-C 12 alkyl or benzyl, more preferably C3-C6 alkyl, especially hexyl. 4 and R 5 is preferably hydrogen. A particularly preferred UV stabilizer is 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyl)oxy-phenol, which is commercially available from BASF as Tinuvin™ 1577, which is a compound of formula (II) above, in which R is CH 13 and R 4 and R 5 are both H. A further particularly preferred UV stabilizer is 2-(2'-hydroxyphenyl)-4,6-diphenyltriazine, which is commercially available from BASF as Tinuvin™ 1600, which is a triazine of formula (II) above, where R is CHCH(CH)CH and R4 is phenyl, and R 5 is hydrogen.
[0018] The amount of UV stabilizer is preferably in the range of 0.1% to 10% by weight, more preferably 0.2% to 7% by weight, more preferably 0.6% to 4% by weight, in particular 0.8% to 2% by weight, and in particular 0.9% to 1.2% by weight, relative to the total weight of the layer. The presence of one or more antioxidants in the layer, especially in the outer layer, may also be particularly advantageous. The base layer is preferably free of antioxidants. Suitable antioxidants include hindered phenols, secondary aromatic amines and hindered amines, such as Tinuvin™ 770 (Ciba-Geigy) disclosed in WO-2012 / 123699-A, the disclosure of which is incorporated herein by reference. The concentration of the antioxidant present in the layer is preferably in the range of 50 ppm to 5000 ppm, more preferably in the range of 300 ppm to 1500 ppm, particularly in the range of 400 ppm to 1200 ppm, especially in the range of 450 ppm to 600 ppm of the polymer of the layer.
[0019] Layers, especially outer layers, especially layers that are exposed to the atmosphere during use (i.e., disposed on or forming the outer surface of the screen or electronic device containing it), may also contain one or more hydrolysis stabilizers. The base layer is preferably free of hydrolysis stabilizers. Any conventional hydrolysis stabilizer in the art may be used. Preferred hydrolysis stabilizers are glycidyl esters of branched monocarboxylic acids, the monocarboxylic acids having 5 to 50 carbon atoms, the glycidyl esters being present in the form of their reaction products with at least a portion of the end groups of the polymer. Such compounds are disclosed in WO-2011 / 030098-A, the disclosure of which is incorporated herein by reference. The total amount of hydrolysis stabilizer present in the layer is preferably within the range of about 0.10 to about 5.0 mol%, more preferably about 0.20 to about 2.5 mol%, more preferably about 0.25 to about 1.5 mol%, more preferably about 0.35 to about 1.0 mol%, based on the amount of polymer in the layer. Preferred glycidyl esters are esters having the formula (I):
[0020] [ka] (I) In formula (I): R 1 and R 2 are independently selected from alkyl; R 3 is selected from hydrogen and alkyl, preferably alkyl; base R 1 , R 2 and R 3 The total number of carbon atoms in the alkyl group is 3 to 48, preferably 3 to 23, preferably 3 to 13, preferably 6 to 10, preferably 7 to 9, and preferably 8. In formula (I), preferably R 1 and R 2 At least one of R is methyl. More preferably, R 1 is methyl, R 2 is an alkyl group containing at least two carbon atoms.
[0021] When a mixture of glycidyl esters is used in a given layer of the film, each of the glycidyl esters preferably is substituted according to formula (I) with the alkyl group R in each glycidyl ester of the mixture. 1 , R 2 and R 3 are independently selected such that the total number of carbon atoms in the In formula (I), preferably, R 1 is methyl, R 2 and R 3 is R 2 and R 3 wherein the total number of carbon atoms in R is 2 to 47, preferably 2 to 22, preferably 2 to 12, preferably 5 to 9, preferably 6 to 8. 2 and R 3 The total number of carbon atoms in is 7. In a further embodiment, the mixture of these preferred glycidyl esters preferably has an alkyl group R 1 , R 2 and R 3 The total number of carbon atoms in the alkyl group is used so that they are the same. As used herein, the term "alkyl" preferably refers to a group of the formula [-C n H 2n+1 ] refers to an unsubstituted straight-chain acyclic hydrocarbon group. The layers, especially the outer layers, may also contain particulate fillers, which may improve handling and flexibility during manufacture. The base layer is preferably free of fillers. Particulate fillers, if present, are typically particulate inorganic fillers, such as metal or semi-metal oxides, such as alumina, titania, talc and silica (especially precipitated or diatomaceous silica and silica gel), calcined china clay and alkali metal salts, such as calcium and barium carbonates and sulfates. The particulate inorganic fillers are preferably finely divided and their volume distribution median particle diameter (equivalent spherical diameter corresponding to 50% of the volume of all particles read on a cumulative distribution curve for the volume % of the particles to their diameters - often referred to as the "D(v,0.5)" value) is preferably in the range of 0.01 to 5 μm, more preferably 0.05 to 1.5 μm, especially 0.15 to 1.2 μm. Preferably, at least 90% by volume, more preferably at least 95% of the inorganic filler particles are within the range of ±0.8 μm, especially ±0.5 μm, of the volume distribution median particle diameter. The particle size of the filler particles can be measured by electron microscopy, Coulter counter, sedimentation analysis and static or dynamic light scattering. Techniques based on laser light diffraction are preferred.
[0022] Preferably, the coextruded polyester film described herein is optically transparent, since the intended end use of the film, as described herein, requires transparency and good aesthetic appearance. As used herein, the term "optically transparent" preferably means a % scattered visible light (haze) of 4.0% or less, preferably 3.5% or less, preferably 3.0 or less, more preferably 2.5% or less, more preferably 2.0% or less, especially 1.5% or less, and / or a total luminous transmittance (TLT) of at least 80%, preferably at least 85%, more preferably at least about 88%, preferably at least about 90% for light in the visible range (400 nm to 700 nm). In this embodiment, a filler may be present in the outer layer, but if present, it is contained only in small amounts, generally not exceeding 0.5% by weight of the layer, preferably less than 0.2% by weight, and in such an embodiment, the filler (if present) is preferably silica. The incorporation of such small amounts of filler into the outer layers is known to improve the flexing properties of the film (i.e., the film does not clog or jam when wound into a roll) without unacceptable degradation in haze or other optical properties. In another embodiment, acceptable flexing properties may be provided by an optically clear coating on one of the two surfaces of the film. Preferably, one or both of the outer layers, preferably both, do not contain particulate fillers, i.e., the layers are preferably unfilled. In the preferred thermoformable films of the present invention, neither the base layer nor the outer layers contain particulate fillers, i.e., the layers are preferably unfilled.
[0023] The total thickness of the film is preferably in the range of 25 to 400 μm, more preferably at least 50 μm, more preferably at least 75 μm, more preferably at least 100 μm, preferably not more than 350 μm, preferably not more than 300 μm, more preferably in the range of about 100 to 300 μm, especially 150 to 250 μm. The thickness of each of the first and second outer layers (A1) and (A2) is preferably about 25 μm or less, preferably about 15 μm or less, preferably about 10 μm or less, preferably about 8 μm or less, preferably about 5 μm or less, and preferably at least about 0.5 μm, preferably at least about 1 μm, preferably at least about 2 μm, preferably at least about 3 μm, preferably within the range of about 1 to about 10 μm, preferably about 3 to about 8 μm.
[0024] The thickness of the copolyester base layer exceeds the thickness of each of the first and second outer layers (A1) and (A2). The thickness of the copolyester base layer is preferably at least 90%, more preferably at least 92%, preferably at least 95%, and preferably not more than about 98%, preferably in the range of about 92% to about 98%, of the total thickness of the film. In the biaxially oriented coextruded film disclosed herein, the outer layers are preferably disposed directly on the opposite surfaces of a single base layer.Preferably, the coextruded film itself consists of three layers, namely the base layer and the two outer layers, i.e. only three layers are formed by the coextrusion process.The outer layers A1 and A2 can be the same or different, preferably the same, i.e. symmetrical films are preferred.The coextruded film therefore preferably exhibits an ABA layer structure.
[0025] Preferably, a functional layer selected from an adhesion-promoting layer and an ink-receiving layer is disposed on one or both of the outer layers (A1 and / or A2) of the coextruded polyester film to improve adhesion of the outer layer(s) to a subsequently applied layer or ink. Suitable such functional layers are well known in the art. In the following discussion, the outer layer of the coextruded polyester film that faces outward (i.e., toward the exterior of the electronic device) when the film is placed in the electronic device is referred to as outer layer A1, and the outer layer of the coextruded polyester film that faces inward (i.e., toward the interior of the electronic device and its electronic components) when the film is placed in the electronic device is referred to as outer layer A2. The subsequently applied layer may be a graphic indicator layer, such layer being preferably applied to the outer layer (A2) that is disposed facing inward in the electronic device. The graphic indicator layer may be applied by conventional printing processes such as offset, gravure, silk screen, flexographic, thermal transfer printing (TTP) or laser transfer printing (LTP). Any suitable ink may be used, including solvent-based inks, with conductive inks being particularly useful. As used herein, the term "graphic indicator layer" refers to pictorial and alphanumeric information.
[0026] The subsequently applied layer may be a hard coat or other protective layer, which is preferably applied to the outer layer (A1) disposed facing outward in the electronic device. Hard coats and protective layers are well known in the art. A suitable adhesion promoting layer (particularly suitable for promoting adhesion to a hardcoat or protective layer) comprises an acrylic resin. As used herein, the term "acrylic resin" refers to a resin that includes at least one acrylic and / or methacrylic component. The acrylic resin is suitably thermosetting.
[0027] Suitable acrylic resins preferably comprise at least one monomer derived from an ester of acrylic acid and / or an ester of methacrylic acid, and / or a derivative thereof. Preferably, the acrylic resin comprises more than 50 mol%, preferably less than 98 mol%, more preferably in the range of 60-97 mol%, particularly 70-96 mol%, and especially 80-94 mol% of at least one monomer derived from an ester of acrylic acid and / or an ester of methacrylic acid, and / or a derivative thereof. Preferred acrylic resins comprise alkyl esters of acrylic acid and / or methacrylic acid, where the alkyl group contains up to 10 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, hexyl, 2-ethylhexyl, heptyl, and n-octyl. Preferably, the acrylic resin comprises an alkyl acrylate (preferably ethyl acrylate and / or butyl acrylate) and an alkyl methacrylate (preferably methyl methacrylate), preferably the acrylic resin comprises ethyl acrylate and methyl methacrylate. The acrylate monomer is preferably present in a ratio within the range of 20-80 mol% (preferably 30-65 mol%), and the methacrylate monomer is preferably present in a ratio within the range of 20-80 mol% (preferably 20-60 mol%). Other monomers suitable for use in preparing the acrylic resins, preferably copolymerized as optional additional monomers together with said esters of acrylic acid and / or methacrylic acid and / or their derivatives, include acrylonitrile, methacrylonitrile, halo-substituted acrylonitriles, halo-substituted methacrylonitriles, acrylamide, methacrylamide, N-methylol acrylamide, N-ethanol acrylamide, N-propanolacrylamide, N-methacrylamide, N-ethanol methacrylamide, N-methylacrylamide, N-tertiary butylacrylamide, hydroxyethyl methacrylate, glycidyl acrylate, glycidyl methacrylate, dimethylaminoethyl methacrylate, itaconic acid, itaconic anhydride and half esters of itaconic acid. Other optional monomers include vinyl esters such as vinyl acetate, vinyl chloroacetate and vinyl benzoate, vinylpyridine, vinyl chloride, vinylidene chloride, maleic acid, maleic anhydride, styrene and derivatives of styrene such as chlorostyrene, hydroxystyrene and alkylated styrenes, where the alkyl group contains from 1 to 10 carbon atoms.
[0028] A preferred acrylic resin is derived from three monomers and contains 35-60 mol % (preferably 40-50 mol %) ethyl acrylate, 30-55 mol % (preferably 40-50 mol %) methyl methacrylate, and 2-20 mol % (preferably 5-10 mol %) acrylamide or methacrylamide, preferably in a molar ratio of about 46 / 46 / 8% ethyl acrylate / methyl methacrylate / acrylamide or methacrylamide, respectively. Preferably, the polymer is thermosetting, for example in the presence of about 25% by weight of a methylated melamine-formaldehyde resin.
[0029] Further preferred acrylic resins are derived from four monomers and include copolymers comprising the comonomers (a) 35-40 mol % of an alkyl acrylate, (b) 35-40 mol % of an alkyl methacrylate, (c) 10-15 mol % of a monomer containing a free carboxyl group, and (d) 15-20 mol % of a monomer containing a sulfonic acid group and / or their salts. Ethyl acrylate is a particularly preferred monomer (a) and methyl methacrylate is a particularly preferred monomer (b). Monomer (c) contains a free carboxyl group (i.e. a carboxyl group other than that which takes part in the polymerization reaction in which the copolymer is formed) and suitably comprises a copolymerizable unsaturated carboxylic acid, preferably selected from acrylic acid, methacrylic acid, maleic acid, and / or itaconic acid (preferably from acrylic acid and itaconic acid). The sulfonic acid group monomers (d) may also be present as free acids and / or their salts, for example as ammonium, substituted ammonium, or alkali metal, for example lithium, sodium or potassium salts. The sulfonate groups do not participate in the polymerization reaction in which the copolymer resin is formed. The sulfonic acid group monomer is preferably aromatic, more preferably p-styrenesulfonic acid and / or its salts.
[0030] Mass average molecular weight of acrylic resin (M W ; measured as described herein) can vary over a wide range, but is preferably within the range of 10,000 to 1,000,000, and more preferably 50,000 to 200,000. The acrylic resin component preferably constitutes at least 30% by weight, more preferably in the range of 40 to 99% by weight, particularly 50 to 85% by weight, and especially 70 to 80% by weight, based on the total weight of the layer. The acrylic resin is preferably the major component of said layer. The composition from which the acrylic resin layer is derived suitably also contains a crosslinking agent. The crosslinking agent functions to improve adhesion to the polyester outer layer. The crosslinking agent should also function to internally crosslink the acrylic resin layer to provide solvent resistance. Suitable crosslinking agents include epoxy resins, alkyd resins, amine derivatives such as hexamethoxymethylmelamine, and / or condensation products of amines such as melamine, diazines, urea, cyclic ethylene urea, cyclic propylene urea, thiourea, cyclic ethylene thiourea, alkyl melamines, aryl melamines, benzoguanamines, guanamines, alkyl guanamines and aryl guanamines with aldehydes such as formaldehyde. A useful condensation product is the condensation product of melamine with formaldehyde. The condensation product may be alkoxylated. The crosslinking agent may be suitably used in an amount up to 70%, preferably 1-60% by weight, more preferably 15-50% by weight, especially 20-30% by weight, based on the total weight of the layer. A catalyst is preferably utilized to promote the crosslinking action of the crosslinking agent. Preferred catalysts for crosslinking melamine formaldehyde include paratoluenesulfonic acid, maleic acid, morpholinium paratoluenesulfonate, and ammonium nitrate stabilized by reaction with a base.
[0031] The composition from which the acrylic layer is derived may contain a plasticizer to aid in film formation and handling. Any suitable plasticizer may be used, such as phthalates, such as alkyl benzyl phthalates, dialkyl adipates, and m,p-cresol propoxylates. The composition from which the adhesion-promoting layer (preferably the acrylic resin mentioned above) is derived is generally insoluble in water. Typically, such a composition is applied to the polyester outer layer as a coating composition in the form of an aqueous dispersion.
[0032] The composition from which the adhesion-promoting layer (preferably the acrylic resin mentioned above) is derived may be applied to the polyester outer layer, typically in the form of a coating composition, before, during or after the stretching process in the production of an oriented film. The coating composition is preferably applied to the polyester outer layer between the two stages (longitudinal and transverse) of the biaxial stretching process. The film to be coated is heated (e.g., in the heat-setting stage described herein above) to drive off the diluent of the composition (usually water, although organic solvent(s) can be used in addition or instead), and to coalesce the coating to form a continuous and uniform layer, and to help promote crosslinking of the crosslinkable coating composition. Any suitable conventional coating technique may be used, such as dip coating, bead coating, reverse roller coating or slot coating. The coating composition is preferably applied to the polyester base layer at a concentration of about 0.05 to 5 mg / dm 2 , especially 0.1 to 2.0 mg / dm 2 The composition is applied at a dry coat weight in the range of 1000:1.
[0033] The ink-receiving layer is preferably a polyurethane coating. Preferably, the polyurethane is dispersible in water. Suitable polyurethanes are available as NeoRez® (from DSM); Dispurez® (from Incorez); Bayhydrol® (from BASF); Hauthane® (from Hauthaway); Witcobond® (from Chemtura (Lanxess)); Alberdingk® (from Alberdingk Boley); Takelac® (from Mitsui Chemicals); Solucote® (from FitzChem) and Cydrothane® (from Cytec (Solvay)). The coating techniques for the adhesion-promoting layer described above apply analogously for the ink-receiving layer. The coating composition is preferably an aqueous composition, such as an aqueous dispersion. Crosslinkers, such as those described herein above, can also be incorporated into the composition.
[0034] The thickness of the functional layers described herein before (especially the adhesion-promoting or ink-receiving layers) is preferably 1.5 μm or less, more preferably in the range of 0.01 to 1.0 μm, especially 0.02 to 0.5 μm. The thermoformable biaxially oriented coextruded films described herein exhibit excellent mechanical strength. Preferably, the coextruded film has a compressibility of at least 10.0 kgf / mm in each of the machine and transverse directions of the film. 2 , preferably at least 11.0 kgf / mm 2 , preferably at least 12.0 kgf / mm 2 , preferably at least 13.0 kgf / mm 2 , preferably at least 13.5 kgf / mm 2 , preferably at least 14.0 kgf / mm 2 The ultimate tensile strength (UTS) of the material is shown. Preferably, the coextruded film exhibits an elongation at break (ETB) of at least 150%, preferably at least 160%, preferably at least 170%, preferably at least 180%, in each of the machine and transverse directions of the film.
[0035] Preferably, the coextruded film has a compressibility of at least 8.0 kgf / mm in each of the machine and transverse directions of the film. 2 , preferably at least 8.2 kgf / mm 2 , preferably at least 8.4 kgf / mm 2 , preferably at least 8.6 kgf / mm 2 , preferably at least 8.8 kgf / mm 2 , preferably at least 9.0 kgf / mm 2 The F5 value (stress at 5% elongation) is shown. The coextruded polyester films described herein preferably exhibit low shrinkage. Preferably, the shrinkage at 150°C for 30 minutes is 3.0% or less, preferably 2.5% or less, preferably 2.0% or less, preferably 1.5% or less in the machine dimension (MD) of the film, and 3.0% or less, preferably 2.5% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less in the transverse dimension (TD). Preferably, the shrinkage at 190°C for 5 minutes is 5.0% or less, preferably 4.5% or less, preferably 4.0% or less, preferably 3.5% or less in the machine dimension of the film, and 5.0% or less, preferably 4.5% or less, preferably 4.0% or less, preferably 3.5% or less, preferably 3.0% or less, preferably 2.5% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less in the transverse dimension of the film. Preferably, the shrinkage in the transverse dimensions of the film is lower than the shrinkage in the machine dimensions of the film, thus preferably the shrinkage at 190°C for 5 minutes is preferably 2.5% or less, preferably 2.0% or less, preferably 1.5% or less, preferably 1.0% or less in the transverse dimensions of the film.
[0036] It will be appreciated that the terms "longitudinal" and "transverse" of a film refer to the direction in which the film was stretched during its manufacture. The term "machine direction" is also used herein to refer to the longitudinal direction. The coextruded films described herein exhibit excellent thermoformability. The thermoforming process involves heating the film to a temperature above the Tg of the material but below the crystalline melting point of the material (if it has any crystallinity) and then applying a deforming force to the material while it is in a softened, rubbery, solid state. The film is then cooled to a temperature below its Tg, after which it must retain the deformation introduced while it was in the softened, rubbery state. Thermoformability therefore requires that the cooled and deformed film retains the deformed shape after such a thermoforming process.
[0037] The evaluation of the thermoformability of a film may also include an evaluation of the quality of the finished thermoformed film, particularly the accuracy of the replication of the designed features, especially the replication of sharp 90° edges. Thus, polycarbonate films are known to exhibit excellent thermoformability, resulting in accurate formation of shapes throughout the designed features, along with the ability to replicate sharp 90° edges. In contrast, while conventional polyester films can be thermoformed, they do not have the capacity for higher degrees of deformation (known as "draw"), are not successful in replicating sharp 90° edges (forming rounded edges instead), and exhibit crack and / or hole formation and / or stress-induced whitening during the thermoforming process. Thus, conventional polyester films are only suitable for shallow-draw applications, particularly those with less aggressive features (i.e., not requiring replication of sharp 90° edges). As used herein, the terms "shallow draw", "medium draw" and "deep draw" refer to deformation around the part less than 5 mm from the plane of the flat film, deformation about 5-10 mm from the plane of the flat film, and deformation greater than 10 mm from the plane of the flat film, respectively.
[0038] Thermoformability is indicated by the stress-strain curve at a temperature above the glass transition temperature of the material (see, for example, "Thermoforming" by James L. Throne (Pub. Karl Heuser Verlag, Munich 1987; ISBN 3-446-14699-7)). Thermoformable polymer films are characterized by a relatively low force required to stretch the film above its Tg and a relatively high elongation when compared with standard polymer films. The assessment of thermoformability is preferably achieved by measuring one or more of the Young's modulus, yield stress and post-yield modulus of the film at a temperature above the Tg, in particular the yield stress and post-yield modulus, as described herein below. Measurement of these parameters at various temperatures above the Tg generally indicates the thermoformability of the film, but the stress-strain behavior is only of substantial importance at the temperature of the thermoforming process, which depends on factors such as the identity and thickness of the film, the degree of deformation (or "stretching") required, and the magnitude and rate of deformation strain applied. More fundamentally, thermoformability requires that the deformed film retains the deformed shape once cooled, as described above. An important property of a thermoformable film is therefore the relaxation of the stress induced at the processing temperature after stretching the film to the desired strain. The property is usually expressed as the percentage of the stress retained after a specified length of time (in seconds) or as the time required to relax the stress by a specified percentage, and in a thermoformable film, the values of these parameters should be as low as possible, as is well known in the art (see, for example, "Viscoelastic Properties of Polymers"; John D. Ferry, page 8 et seq., 3rd Ed, Wiley, NY; ISBN 0-471-04894-1; and "Mechanical Properties of Solid Polymers", IM Ward, 2nd Ed., John Wiley).
[0039] In the thermoformable films of the present invention, the elongation (strain) at break (ETB) should exceed the elongation experienced during the thermoforming process and / or the tensile strength at maximum elongation (UTS) should exceed the yield stress. Preferably, the thermoformable films disclosed herein exhibit an elongation (strain) at break of greater than 220% in both the machine direction (MD) and transverse direction (TD) when measured at 130°C. The polyester films disclosed herein can also be evaluated for thermoformability by comparison with standard polycarbonate films and / or standard unfilled PET films. Such evaluation is suitably performed by optical microscopy. The evaluation is preferably performed using a "medium draw" around the part. Preferably, the evaluation can also be performed using a "deep draw" around the part.
[0040] The coextruded films described herein are preferably thermoformable at a temperature in the range of about 130°C to about 200°C, preferably at least about 135°C, preferably at least about 140°C, preferably at least about 150°C, preferably up to about 195°C, preferably from about 160°C to about 190°C, more preferably from about 160°C to about 180°C. In the coextruded films described herein, the morphology of the copolyester base layer is preferably different from that of the outer PET layers. Advantageously, the copolyester base layer exhibits a crystallinity lower than that of either of the PET outer layers. Preferably, the copolyester base layer exhibits a crystallinity (X C-外部 ) which is at least 40% lower, preferably at least 45% lower, C-ベース ). In other words, (X C-外部 )-(X C-ベース ) / (X C-外部 ) × 100≧40%, preferably ≧45%. C-外部 )-(X C-ベース ) / (X C-外部)×100 is about 70% or less, preferably about 60% or less, preferably about 55% or less, preferably about 50% or less. The crystallinity of each layer is calculated from the enthalpy of fusion measured by differential scanning calorimetry (DSC). Preferably, the crystallinity (X C-外部 ) are independently at least about 25%, preferably at least about 28%, preferably at least about 30%, and preferably no more than about 50%, typically no more than about 45%, more typically no more than about 40%, and more typically no more than about 35%. Preferably, the crystallinity (X C-ベース ) is less than 25%, preferably about 20% or less, preferably about 18% or less, preferably about 17% or less, typically about 16% or less, preferably at least about 5%, more preferably at least about 10%.
[0041] The film described herein above is particularly useful as a screen in electronic devices, particularly as a touch screen, particularly as a touch screen via capacitance.As mentioned above, such screens find utility in the automotive, home appliance and consumer electronics markets.Generally, the utility of the film extends beyond screens and can also include automotive and industrial instrument panels, displays, home appliance instrument panels, medical device instrument panels, consumer electronics body parts, and automotive interior decoration. According to a third aspect of the invention there is provided an electronic device comprising a touch screen interface, the outer surface of said touch screen interface being a thermoformed biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first outer polyester layer A1 and a second outer polyester layer A2, said outer layers being disposed on opposing surfaces of said base layer, (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of about 5 to about 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) an electronic device is provided, wherein the thickness of the base layer is at least 90% of the total thickness of the coextruded multilayer polyester film.
[0042] The thermoformed biaxially oriented coextruded polyester film in an electronic device is produced by thermoforming the thermoformable biaxially oriented coextruded polyester film described herein above. Preferably, the thermoforming is carried out at a film temperature in the range of about 130°C to about 200°C, preferably at least about 135°C, preferably at least about 140°C, preferably at least about 150°C, preferably 195°C or less, preferably about 160°C to about 190°C, more preferably about 160°C to about 180°C. Preferably, thermoforming is carried out by preheating the film for about 1 to about 15 seconds and then thermoforming at elevated pressure, preferably about 20 to about 150 bar (preferably not more than about 120 bar, preferably not more than about 110 bar, preferably about 30 to about 100 bar), preferably for about 1 to about 15 seconds. The elevated pressure required for the thermoforming step is preferably provided by high pressure air. Heating of the film can be carried out by contact heating or by using heated air.
[0043] In one preferred embodiment, the film is preheated (preferably for about 1 to about 15 seconds, typically about 2 to about 4 seconds) by pressing it against a heated platen with high pressure air (preferably in the range of 3 to 5 bar), followed by the application of a forming pressure (preferably about 35 bar) to thermoform the film around the former. In a further preferred embodiment, preheating is performed in a chamber separate from the chamber in which the film is formed into the desired shape. Thus, after preheating the film in the preheating chamber (preferably for about 1 to about 15 seconds), the film is passed into the forming chamber where the forming mold is closed and air pressure is applied. Forming is performed by applying high pressure heated air (up to 150 bar, preferably up to about 120 bar, preferably up to about 110 bar, and typically about 100 bar) to one side of the film to press it onto the forming tool.
[0044] Preferably, the process of forming the molded part comprises: (1) A step of arbitrarily printing a graphic display layer on a film (2) optionally functionalizing the film by placing on the film surface any electronic circuitry required for the end use, particularly printed electronic circuitry; (3) thermoforming the (optionally printed and / or functionalized) film; (4) cutting the thermoformed film into its desired shape prior to injection molding; and (5) providing a molded part by an injection molding process, preferably by placing the thermoformed film into a mold in an injection molding machine and filling the molded resin. Includes. In the injection molding step, the molding resin may be any polymeric resin suitable for use in injection molding, such as polycarbonate, acrylonitrile butadiene styrene (ABS) or polyester, preferably polycarbonate or polycarbonate / ABS. Injection molding is usually performed in a separate machine from the thermoforming machine. In the finished molded part, the printed graphic indicator layer is preferably encapsulated between the film and the molding resin.
[0045] The thermoformed biaxially oriented coextruded polyester film is preferably oriented in the electronic device such that the first polyester outer layer A1 is disposed facing outward in the device and the second polyester outer layer A2 is disposed facing inward in the device. Preferably, the second polyester outer layer A2 has a first and second surface, the first surface being adjacent to the base layer B and the second surface having a graphic indicator layer disposed thereon, preferably, as described herein above, an adhesion promoting layer or ink receiving layer is disposed on the second surface of the second polyester outer layer A2 prior to application of the graphic indicator layer. Preferably, the first polyester outer layer A1 has a first and second surface, the first surface being adjacent to the base layer B and the second surface having a hard coat or protective layer disposed thereon, preferably, as described herein above, an adhesion promoting layer is disposed on the second surface of the first polyester outer layer A1 prior to application of the hard coat or protective layer. The touchscreen interface is preferably in the form of an injection molded module comprising said touchscreen interface, suitably comprising an inner portion or layer of injection molded polymeric material and an outer portion or layer of said thermoformed biaxially oriented coextruded polyester film.
[0046] Injection molding can be carried out using any conventional injection molding technique known in the art and using any suitable thermoplastic or thermoset polymeric material. Polycarbonate is one example of a suitable injection molding material for use in the present invention. The touch screen is preferably a capacitance-mediated touch screen, and such screens are widely known and used in the art. The capacitance-mediated touch screen is preferably associated with a transparent conductive layer, such as indium tin oxide. As described above, any electronic circuitry and conductive inks are preferably disposed on the surface of the coextruded polyester film of the present invention. Thus, the electronic circuitry is suitably located between the thermoformed polyester film and the recessed injection molding material. According to a fourth aspect of the present invention there is provided the use of the biaxially oriented coextruded polyester film described herein as a thermoformable film, in particular in the manufacture of an electronic device including a touch screen interface, wherein the outer surface of said touch screen interface is a thermoformed biaxially oriented coextruded polyester film produced by thermoforming said thermoformable biaxially oriented coextruded polyester film. According to a fifth aspect of the invention there is provided a method of manufacturing an electronic device including a touch screen interface comprising the steps of: (i) thermoforming a thermoformable biaxially oriented coextruded polyester film as described herein to produce a thermoformed biaxially oriented coextruded polyester film; and (ii) providing the thermoformed biaxially oriented coextruded polyester film as part of the touch screen interface in an electronic device. A method is provided, comprising:
[0047] In a fifth embodiment manufacturing method, the thermoformed biaxially oriented coextruded polyester film is provided as part of the touchscreen interface by forming an injection molded module that includes the touchscreen interface, whereby the injection molded module includes an inner portion or layer of injection molded polymeric material and an outer portion or layer of the thermoformed biaxially oriented coextruded polyester film, and providing the injection molded module as part of an electronic device. The preferences disclosed herein above for the first, second and third aspects of the invention also apply to the fourth and fifth aspects.
[0048] Measurement of properties The following analyses were used to characterize the films described herein: (i) Transparency may be assessed by measuring the total luminance transmittance (TLT) through the total thickness of the film and the haze (% of transmitted visible light that is scattered) using an M57D spherical transmittance meter (diffuse system) in accordance with ASTM D1003. (ii) Intrinsic viscosity can be measured by solution viscometry according to ASTM D5225-98 (2003) (in units of dL / g) using a Viscotek™ Y-501C relative viscometer using a 0.5% by weight solution of the polyester in o-chlorophenol at 25° C. (see, e.g., Hitchcock, Hammons & Yau in American Laboratory (August 1994) “The dual-capillary method for modern-day viscometry”), and calculating the intrinsic viscosity using Billmeyer’s single point method: η=0.25η red +0.75(lnη rel ) / c where: η=intrinsic viscosity (dL / g), η rel = relative viscosity, c = concentration (g / dL), and η red = reduced viscosity (dL / g), which is (η rel -1) / c is equivalent to (η sp It can also be expressed as / c, where η sp is the specific viscosity).
[0049] (iii) Heat shrinkage is assessed on film samples of dimensions 200 mm x 10 mm cut at specific orientations relative to the machine and transverse directions of the film and marked for visual measurement. The shrinkage of the longer dimension of the sample (i.e. the 200 mm dimension) is tested, i.e. the test sample of dimension 200 mm is oriented along the machine direction of the film, corresponding to the film direction for assessment of shrinkage in the machine direction. After the specimen is heated to a given temperature (by placing it in an oven heated to that temperature) and held for a given time interval, it is cooled to room temperature and its dimensions are remeasured manually. Heat shrinkage is calculated and expressed as a percentage of the original length. (iv) Layer thickness is measured with a Mercer 122D gauge. (v) Ultimate Tensile Strength (UTS), Elongation at Break (ETB) and F5 value (stress at 5% elongation) are measured in accordance with test method ASTM D882. Five strips (10 mm + / - 0.5 mm) of film (100 mm in length) are cut along the machine direction using a straight edge and a calibrated specimen cutter. Each specimen is tested using an Instron testing machine using pneumatic grips with rubber jaws. Testing is performed at ambient conditions. The crosshead speed (speed of separation) is 25 mm.min. -1 The strain rate is 50%. The elongation at break (ε B (%))teeth: ε B (%) = (elongation at break / L0) x 100 where L0 is the original length of the sample between the grips.
[0050] (vi) Thermoformability can be assessed from the stress-strain curve above the glass transition temperature of the polymer with reference to the parameters Young's modulus, yield stress, and post-yield modulus. ·Young's modulus is a measure of the stiffness of a given material. It represents the rate of change of stress with strain and can be determined experimentally from the initial slope of the stress-strain curve during a tensile test. Young's modulus is therefore the ratio of the tensile strength to the elongation below the yield stress. Preferably, it is calculated as the highest ratio between 0% and 10% elongation. Yield stress can be determined from the stress-strain curve exhibited during tensile testing and represents the stress at which permanent deformation of a strained specimen begins to occur, i.e., the tensile stress above which the material stretches beyond the bounds of recovery. Preferably, it is calculated as the stress at which the tensile to elongation ratio falls by 60% from its highest value (i.e., Young's modulus). Desirably, the yield stress should be as close to zero as possible at the processing temperature of the thermoforming process.
[0051] · Post-yield modulus is a measure of strain hardening of a given material and is the slope of the stress-strain curve when the material is strained beyond the yield point. Increasing stress is required to produce additional deformation. Thus, the post-yield modulus coefficient is the ratio of the tensile strength to the elongation beyond the yield stress (and below the elongation at break). Preferably, it is calculated as the average ratio between the elongations (%) in the range E1 to E2, where: (i) 10≦(E2-E1)≦20; (ii) 60≦E2≦120; and (iii) 50≦E1≦100 (this range is typically between 60% and 80%, but in some cases between 40% and 60%, or 50% and 60%, or 100% and 120%, depending on the shape of the curve). Desirably, the post-yield modulus should be as close to zero as possible in the processing region of interest, i.e., in the strain and temperature region utilized in the thermoforming process.
[0052] Young's modulus, yield stress and post-yield modulus are suitably measured at various temperatures: 25°C; Tg; Tg+50°C; and Tg+100°C. Five dog-bone shaped strips (500 mm long) of film (10 mm ± 0.5 mm at the centre of the strip) are cut along the machine direction using a straight edge and a calibrated specimen cutter. The same procedure is repeated for the transverse direction. Each specimen is tested using an Instron Model 3111 Materials Testing Machine using pneumatic grips with rubber jaws and a hot box. Temperature is varied as required. Crosshead speed (speed of separation) is 25 mm.min. -1 The strain rate is 50%. The elongation is preferably measured by video recording the distance between two black spots previously marked on the strip. (vii) Relaxation of a thermoformed film at elevated temperature and / or humid conditions may be tested by accelerated aging of the thermoformed film in an environmental oven at 85°C and 85% relative humidity for 60 minutes or more. (viii) Glass transition temperature (T g ), crystalline melting point (T m ) and crystallinity (X c) was measured by differential scanning calorimetry (DSC) using a Perkin Elmer Hyper8500 DSC. Unless otherwise stated, measurements were performed according to the method described in ASTM E1356-98 following standard test method. Samples (5 mg) were kept under an atmosphere of dry nitrogen for the duration of the scan.
[0053] The thermal properties of the polymer / copolymer samples were examined by heat-cool-reheat scans using the following method: - Equilibrate at -30°C for 2 minutes - Heat from -30°C to 300°C at 20°C / min (first heating scan) - Equilibrate at 300°C for 2 minutes - Cool from 300°C to -30°C at 20°C / min (first cooling scan) - Equilibrate at -30°C for 2 minutes - Heat from -30°C to 300°C at 20°C / min (second heating scan) The value of Tg was determined as the extrapolated onset temperature of the glass transition observed in the DSC scan (heat flow (W / g) versus temperature (°C)) as described in ASTM E1356-98. The value of Tm was determined as the peak of the transition from the second heating scan of the DSC scan.
[0054] The thermal properties of the film samples, especially the crystallinity, were examined by heating scan only using the following method: - Equilibrate at 0°C for 2 minutes - Heat from 0°C to 300°C at 20°C / min Crystallinity (X c ) from the experimental value of enthalpy of fusion (ΔHm) using the equation: X c = ΔH m / ΔH m ° Calculated by (In the formula: H m = experimental enthalpy of fusion calculated from the integral of the melting endotherm; H m° = theoretical enthalpy of fusion of the corresponding poly(alkylene-carboxylate) homopolymer (i.e., without any minor amounts of comonomer) at 100% crystallinity. Thus, for the PET-based copolyesters of the base layer and PET outer layers of the preferred inventive film, ΔH m ° is the theoretical melting enthalpy of 100% crystalline PET polymer (140 J / g) as defined in the literature (B. Wunderlich, Macromolecular Physics, Academic Press, New York, (1976)). The present invention is further illustrated by the following examples, which are not intended to limit the invention described above. Modifications of detail can be made without departing from the scope of the invention. EXAMPLES
[0055] Example 1 A multilayer film including a base layer B of PET-based copolyester containing IPA (IPA:TA:EG molar ratio was 12:88:100; IV=0.67; unfilled) and two outer layers A1 and A2 of PET (IV=0.65; unfilled) was extruded and cast using a standard melt coextrusion system. The coextrusion system was assembled using two independently operating coextruders that fed the molten polymers separately to a standard coextrusion block or joined at a junction where these streams met. From the coextrusion block, the molten streams were transferred to a conventional, flat film extrusion die that allowed the film-like melt to be cast from a common coextrusion die at 275° C. and then quenched at temperature on a rotating chilled metal drum. The cast film was collected at a process speed of about 3.3 m / min and had a width of about 635 mm. The cast extrudate was stretched in the direction of extrusion to about 3.2 times its original dimension at a temperature of 78°C. The line speed was about 12 m / min. The cooled and stretched film was then passed through a tenter oven at a temperature of 105°C where it was dried and stretched in the transverse direction to about 3.0 times its original dimension. The biaxially stretched film was heat set in a three-zone crystallizer sequentially at temperatures of 210, 190 and 180°C in the transverse direction under about 8% dimensional relaxation. The final film had an average thickness of about 212 μm and contained three layers with ABA structure, with the outer layers (A1) and (A2) having an average thickness of about 6 μm. The film was tested according to the methods described herein. The crystallinity (Xc) of the base layer was less than 20%. Other results are shown in Table 1 below.
[0056] Thermoforming was performed on film samples with dimensions 610 mm x 436 mm. The film samples were molded using a preheat pressure of 5.5 bar (80 psi) with platen temperatures ranging from 177 to 200 °C and preheat times ranging from 2 to 12 seconds. The mold pressure was 34.4 bar (500 psi). The film performed well as a thermoformable film, with best results obtained at platen temperatures of 177 to 190 °C. However, at a thermoforming temperature of 200 °C, the thermoformed film shows signs of wrinkling and excessive shrinkage in some areas. A further series of thermoforming tests using the film of Example 1 was carried out using various thermoforming conditions. As a result, film samples with dimensions 300 x 210 mm were heated at a temperature of 260°C for preheat times ranging from 10 to 16 seconds, resulting in film temperatures of 137 to 160°C, with the best results being observed at a film temperature of 158°C. Film samples were cast under pressures of 50 to 120 bar with high pressure durations of 3 to 10 seconds. The film performed well as a thermoformable film. Best results were observed with high pressure durations towards the lower end of the range, preferably about 3 seconds. With regard to pressure, best results were observed at pressures of about 110 bar or less, preferably about 100 bar. At a pressure of 120 bar, signs of whitening and cracking were observed in some areas. As previously described herein, the molded parts were typically made from thermoformed films that were then filled with polycarbonate resin at a resin temperature of 290° C. using an Arburg 470C Allrounder 1500-350 injection molding machine.
[0057] Example 2 A multilayer film comprising a base layer B of IPA-containing PET-based copolyester (IPA:TA:EG molar ratio was 12:88:100; IV=0.65; unfilled) and two outer layers A1 and A2 of PET (IV=0.65; unfilled) was extruded and cast using a standard melt coextrusion system as described for Example 1. The cast film was collected at a process speed of about 3 m / min and had a width of about 620 mm. The cast extrudate was stretched in the direction of extrusion to about 3.2 times its original dimension at a temperature of 78° C. The linear speed was 11 m / min. The cooled and stretched film was then passed through a tenter oven at a temperature of 105° C., where the film was dried and stretched in the transverse direction to about 3.4 times its original dimension. The biaxially stretched film was heat set in a three-zone crystallizer at temperatures of 210, 210 and 190°C successively under dimensional relaxation of about 3% in the transverse direction. The average thickness of the final film was about 200 μm and contained three layers with ABA structure, with the average thickness of the outer layers (A1) and (A2) being about 5 μm. The film was tested according to the methods described herein and the results are shown in Table 1 below.
[0058] Thermoforming was carried out on film samples with dimensions of 300 x 210 mm. The film samples were preheated at a temperature of 260°C for 15 seconds to a film temperature of 158°C. The film samples were molded at a pressure of 100 bar with a high pressure duration of 3 seconds. The film performed well as a thermoformable film. Following thermoforming, a molded part was prepared by filling with polycarbonate resin as described for Example 1. An additional sample of the film of Example 2 was printed with black ink and then thermoformed under the same preheat temperature / time / forming pressure as before, except the film temperature was increased to 165° C. The film performed excellently as a thermoformable film.
[0059] Further samples of the film of Example 2 were thermoformed using film samples with dimensions 610 mm x 436 mm. The film samples were molded at a platen temperature of 177°C using a preheat pressure of 5.5 bar (80 psi) with a preheat time of 3 seconds. The molding pressure was 34.4 bar (500 psi). The film performed well as a thermoformable film. The film also showed good chemical resistance. In a 24-hour solvent test using various solvent systems at room temperature, the film passed the test with methylene chloride, isopropyl alcohol, cyclohexanone, ethyl acetate, concentrated HCl, acetone, xylene, and toluene. In this test, failure consisted of any irremovable coloring, haze, or blistering. Only with 40% NaOH aqueous solution did the film show any evidence of these characteristics. In addition, the film was tested for chemical resistance to various household agents (bleach; furniture polish; Windowlene®; sunscreen SPF30; mosquito repellent spray (50% DEET); WD40 oil; Flash® floor cleaner; fabric softener; car wax cleaner; and antibacterial spray) at room temperature and 50°C for 1 hour and 24 hours. In all cases, the film passed the test.
[0060] Example 3 A multilayer film comprising a base layer B of IPA-containing PET-based copolyester (IPA:TA:EG molar ratio was 12:88:100; IV=0.63) and two outer layers A1 and A2 of PET (IV=0.65; unfilled) was extruded and cast using a standard melt coextrusion system as described in Example 1. The cast film was collected at a process speed of about 2.8 m / min and had a width of about 710 mm. The cast extrudate was stretched in the direction of extrusion to about 3.2 times its original dimension at a temperature of 78° C. The linear speed was 9.5 m / min. The cooled and stretched film was then passed through a tenter oven at a temperature of 105° C., where the film was dried and stretched in the transverse direction to about 3.7 times its original dimension. The biaxially stretched film was heat set in a three-zone crystallizer, successively at temperatures of 210, 210 and 190° C., with a dimensional relaxation of about 4% in the transverse direction. The final film had an average thickness of about 185 μm and contained three layers with ABA structure, with the outer layers (A1) and (A2) having an average thickness of about 6 μm. Thermoforming was performed on film samples with dimensions 210 mm x 300 mm. The film samples were molded at a platen temperature of 177°C using a preheat time of 3 seconds and a preheat pressure of 5.5 bar (80 psi). The molding pressure was 34.4 bar (500 psi). The film performed well as a thermoformable film.
[0061] Comparative Example 1 A monolayer, unfilled PET film (IV=0.65) was extruded and cast using a standard melt coextrusion system as described in Example 1. The cast film was collected at a process speed of about 8 m / min and had a width of about 800 mm. The cast extrudate was stretched in the direction of extrusion to about 3.4 times its original dimension at a temperature of 82° C. The linear speed was 27 m / min. The cooled and stretched film was then passed through a tenter oven at a temperature of 125° C., where it was dried and stretched in the transverse direction to about 3.8 times its original dimension. The biaxially stretched film was heat set in a four-zone crystallizer at temperatures of 232, 232, 232 and 170° C. in succession, with a dimensional relaxation of about 2.4% in the transverse direction. The average thickness of the final film was about 175 μm. The film was tested according to the methods described herein. The crystallinity was 31%. Other results are shown in Table 1 below. Attempts to thermoform several samples of this film were made using film samples measuring 610 mm x 436 mm and varying thermoforming conditions. Film samples were molded using a preheat pressure of 5.5 bar (80 psi) with a platen temperature of 177°C and preheat times ranging from 2 to 15 seconds. The molding pressure was 34.4 bar (500 psi). The film did not perform acceptably as a thermoformable film.
[0062] [Table 1] In Table 1 above, Control 1 is a 250 μm polycarbonate film. Next, another preferred embodiment of the present invention will be described. 1. A thermoformable biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first polyester outer layer A1 and a second polyester outer layer A2, said outer layers being disposed on opposite surfaces of said base layer; (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of about 5 to about 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer constitutes at least 90% of the total thickness of the coextruded multilayer polyester film; Polyester film. 2. The film described in 1 above, wherein the second aromatic dicarboxylic acid is present in the copolyester in an amount of about 8 to about 16 mol %, preferably about 10 to about 14 mol %, and preferably about 12 mol %, of the acid fraction of the copolyester. 3. The film of claim 1 or 2, wherein the copolyester is derived from terephthalic acid, a second aromatic dicarboxylic acid, and ethylene glycol. 4. The film described in any one of 1 to 3 above, wherein the second aromatic dicarboxylic acid is isophthalic acid (IPA). 5. The film described in any one of 1 to 4 above, wherein the copolyester of the base layer exhibits a crystalline melting point (Tm) in the range of 210 to 240°C and at least 10°C lower than the crystalline melting point of the outer layer polyester, and / or a glass transition temperature (Tg) in the range of 60 to 90°C. 6. The film according to any one of 1 to 5 above, wherein the total thickness of the film is about 50 to about 350 μm. 7. A film according to any one of claims 1 to 6, exhibiting shrinkage of 3.0% or less at 150°C in each of the machine and lateral dimensions of the film; and / or exhibiting shrinkage of 5.0% or less at 190°C in each of the machine and lateral dimensions of the film. 8. The film according to any one of claims 1 to 7, exhibiting a haze of 3.0% or less and / or a total light transmittance (TLT) of at least 85%. 9. The film of any one of claims 1 to 8, wherein the base layer does not contain particulate filler, and preferably the outer layer does not contain particulate filler. 10. At least 10.0 kgf / mm in each of the longitudinal and transverse directions of the film 2 and / or an ultimate tensile strength (UTS) of at least 150% in each of the longitudinal and transverse directions of the film, and / or an elongation at break (ETB) of at least 8.0 kgf / mm 2 10. The film according to any one of the above 1 to 9, which exhibits an F5 value (stress at 5% elongation) of. 11. The film according to any one of claims 1 to 10, wherein a functional layer is disposed on one or both of the outer layers (A1 and / or A2) of the coextruded polyester film, said functional layer being selected from an adhesion promoting layer and an ink receiving layer. 12. The film according to claim 11, wherein the adhesion-promoting layer comprises an acrylic resin and is preferably disposed on the outer layer (A1). 13. The film of claim 11 or 12, wherein the subsequently applied layer is a protective or hardcoat layer applied to the adhesion-promoting layer disposed on the outer layer (A1). 14. The film according to any one of the above items 11 to 13, wherein the ink-receiving layer comprises polyurethane and is preferably disposed on the outer layer (A2). 15. The film of any one of claims 11 to 14, wherein the subsequently applied layer is a graphic-bearing layer applied to the ink-receiving layer disposed on the outer layer (A2). 16. The film according to any one of the above items 11 to 15, wherein the thickness of the functional layer is 1.5 μm or less, preferably in the range of 0.01 to 1.0 μm, particularly 0.02 to 0.5 μm. 17. The film according to any one of the above 1 to 16, which is thermoformable at a temperature within the range of 130°C to 200°C, preferably at least about 135°C, preferably at least 140°C, preferably at least about 150°C, preferably about 150°C to about 195°C, preferably 160°C to 190°C, and more preferably 160°C to 180°C. 18. The base layer of the copolyester exhibits a crystallinity lower than that of any of the outer layers, preferably [(X C-OUTER )-(X C-BASE ) / (X C-OUTER ) × 100] is at least 40%, preferably at least 45%, preferably 70% or less, preferably 60% or less, preferably 55% or less, preferably 50% or less, C-BASE is the crystallinity of the base layer of the copolyester, and X C-OUTER 18. The film according to any one of claims 1 to 17, wherein x is the crystallinity of the outer layer, and the crystallinity of the layer is calculated from the enthalpy of fusion measured by differential scanning calorimetry. 19. The crystallinity (X) of each of the outer layers C-OUTER ) is independently in the range of 25% to 50%, and / or the crystallinity (X C-BASE 19. The film according to any one of claims 1 to 18, wherein the crystallinity of the layer is calculated from the enthalpy of fusion measured by differential scanning calorimetry. 20. An electronic device comprising a touch screen interface, the outer surface of the touch screen interface being a thermoformed biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first outer polyester layer A1 and a second outer polyester layer A2, the outer layers being disposed on opposing surfaces of the base layer; (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of about 5 to about 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer constitutes at least 90% of the total thickness of the coextruded multilayer polyester film; electronic equipment. 21. The electronic device of claim 20, wherein the film is oriented in the device such that the first polyester outer layer A1 is positioned facing outward from the device and the second polyester outer layer A2 is positioned facing inward toward the device, the second polyester outer layer A2 having first and second surfaces, the first surface adjacent base layer B and the second surface having a graphic display layer disposed thereon. 22. The electronic device of claim 20 or 21, which is or includes an injection molded module including the touch screen interface, the injection molded module further including an outer portion or layer of the thermoformed biaxially oriented coextruded polyester film, the outer portion or layer including an inner portion or layer of injection molded polymeric material and optionally having a graphic display layer disposed on an inner surface thereof. 23. The electronic device according to claim 20, 21 or 22, wherein the touch screen interface is a capacitance mediated touch screen interface. 24. The electronic device of claim 23, further comprising a transparent conductive layer, preferably indium tin oxide. 25. The electronic device described in any one of claims 20 to 24, wherein the thermoformed biaxially oriented coextruded polyester film is produced by thermoforming the thermoformable biaxially oriented coextruded polyester film described in any one of claims 1 to 19. 26. Use of a biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first polyester outer layer A1 and a second polyester outer layer A2, said outer layers being arranged directly on the opposing surfaces of the base layer, as a thermoformable film, (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of about 5 to about 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer constitutes at least 90% of the total thickness of the coextruded multilayer polyester film; use. 27. The use according to claim 26 in the manufacture of an electronic device including a touch screen interface, wherein the outer surface of the touch screen interface is a thermoformed biaxially oriented coextruded polyester film produced by thermoforming the thermoformable biaxially oriented coextruded polyester film. 28. A method of manufacturing an electronic device including a touch screen interface, comprising: (i) thermoforming a thermoformable biaxially oriented coextruded polyester film as described herein to produce a thermoformed biaxially oriented coextruded polyester film; and (ii) providing the thermoformed biaxially oriented coextruded polyester film as part of the touch screen interface in an electronic device. A method comprising: 29. The method of claim 28, wherein the thermoformed biaxially oriented coextruded polyester film is provided as part of the touchscreen interface by forming an injection molded module that includes the touchscreen interface, whereby the injection molded module further includes an outer portion or layer of the thermoformed biaxially oriented coextruded polyester film that includes an inner portion or layer of injection molded polymeric material and optionally has a graphic display layer disposed on an inner surface thereof. 30. A process for producing a thermoformable polyester film according to any one of claims 1 to 19, comprising the steps of: (i) co-extruding said copolyester base layer B, said first polyester outer layer A1 and said second polyester outer layer A2 such that said outer layers are disposed on opposing surfaces of said base layer; (ii) quenching the extrudate; (iii) stretching the quenched extrudate in at least one direction at a temperature above the glass transition temperature of the polyester material; and (iv) heat setting the stretched film at a temperature in the range of about 165°C to about 215°C, during which dimensional relaxation in the lateral dimensions of the film occurs in the range of about 2% to about 10%. The process includes: 31. The process of claim 30, wherein at least a portion of the heat setting step is carried out at a temperature within the range of about 205 to about 215°C, preferably about 210°C. 32. The process according to claim 31 or 32, wherein the heat setting is carried out in a multi-zone crystallizer, the temperature of the final zone being lower than the temperature of the first zone, preferably the first zone being at a temperature of about 205 to about 215°C and the final zone being at a temperature preferably within the range of about 170 to about 190°C.
Claims
1. 1. An electronic device comprising a touch screen interface, the outer surface of the touch screen interface being a thermoformed biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first outer polyester layer A1 and a second outer polyester layer A2, the outer layers being disposed on opposing surfaces of the base layer; (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of 5 to 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer accounts for at least 90% of the total thickness of the coextruded multilayer polyester film; electronic equipment.
2. 2. The electronic device of claim 1, wherein the film is oriented in the device such that the first polyester outer layer A1 is positioned facing outward from the device and the second polyester outer layer A2 is positioned facing inwardly toward the device, the second polyester outer layer A2 having first and second surfaces, the first surface adjacent a base layer B and the second surface having a graphic display layer disposed thereon.
3. 3. The electronic device of claim 1 or 2, which is or includes an injection molded module that includes the touch screen interface, the injection molded module including an inner portion or layer of injection molded polymeric material and further including an outer portion or layer of the thermoformed biaxially oriented coextruded polyester film.
4. 4. The electronic device of claim 3, further comprising a graphic display layer disposed on an interior surface thereof.
5. The electronic device according to any one of claims 1 to 4, wherein the touchscreen interface is a capacitance mediated touchscreen interface.
6. 6. The electronic device of claim 5 further comprising a transparent conductive layer.
7. 7. The electronic device of claim 6, wherein the transparent conductive layer is indium tin oxide.
8. the copolyester is derived from terephthalic acid, a second aromatic dicarboxylic acid and ethylene glycol; and / or The electronic device according to any one of claims 1 to 7, wherein the second aromatic dicarboxylic acid is isophthalic acid (IPA).
9. 1. A thermoformable biaxially oriented coextruded polyester film for use as a touch screen in an electronic device, comprising a base layer B of a copolyester, a first polyester outer layer A1 and a second polyester outer layer A2, said outer layers being disposed on opposing surfaces of said base layer, (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of 5 to 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer constitutes at least 90% of the total thickness of the coextruded multilayer polyester film; the second aromatic dicarboxylic acid is isophthalic acid (IPA) and the film exhibits a haze of 4.0% or less; Thermoformable biaxially oriented coextruded polyester film.
10. 10. The thermoformable biaxially oriented coextruded polyester film for use as a touch screen in an electronic device according to claim 9, wherein the copolyester is derived from terephthalic acid, isophthalic acid and ethylene glycol.
11. The electronic device of any one of claims 1 to 8, wherein the second aromatic dicarboxylic acid is present in the copolyester in an amount of 8 to 16 mol % of the acid fraction of the copolyester.
12. 12. The electronic device according to claim 1, wherein the copolyester of the base layer exhibits a crystalline melting point (Tm) in the range of 210-240°C and at least 10°C lower than the crystalline melting point of the outer layer polyester, and / or the copolyester of the base layer exhibits a glass transition temperature (Tg) in the range of 60-90°C.
13. The electronic device according to any one of claims 1 to 8, 11 or 12, wherein the thermoformed film has a total thickness of 50 to 350 μm.
14. 14. The electronic device of any one of claims 1-8 or 11-13, wherein the thermoformed film exhibits shrinkage of 3.0% or less at 150°C in each of the film's machine and lateral dimensions; and / or shrinkage of 5.0% or less at 190°C in each of the film's machine and lateral dimensions.
15. The electronic device of any one of claims 1-8 or 11-14, wherein the thermoformed film exhibits a haze of 3.0% or less and / or a total light transmittance (TLT) of at least 85%.
16. The electronic device of any one of claims 1 to 8 or 11 to 15, wherein the base layer does not contain particulate filler.
17. The thermoformed film has a strength of at least 10.0 kgf / mm in each of the machine and cross directions of the film. 2 The electronic device of any one of claims 1 to 8 or 11 to 16, exhibiting an ultimate tensile strength (UTS) of
18. The electronic device of any one of claims 1-8 or 11-17, wherein the thermoformed film exhibits an elongation at break (ETB) of at least 150% in each of the machine and cross directions of the film.
19. The thermoformed film has a strength of at least 8.0 kgf / mm in each of the machine and cross directions of the film. 2 The electronic device according to any one of claims 6, 7, or 11 to 18, wherein the electronic device exhibits an F5 value (stress at 5% elongation) of 0.05 to 0.05%.
20. The electronic device of any one of claims 1 to 8 or 11 to 19, wherein the base layer is free of particulate filler and the outer layer is free of particulate filler.
21. 21. The electronic device of claim 1, wherein a functional layer is disposed on one or both of the outer layers (A1 and / or A2) of the thermoformed coextruded polyester film, the functional layer being selected from an adhesion promoting layer and an ink receiving layer.
22. 22. The electronic device of claim 21, wherein the adhesion promoting layer comprises an acrylic resin.
23. 23. The electronic device according to claim 22, wherein the adhesion promoting layer is disposed on the outer layer (A1).
24. The electronic device according to any one of claims 21 to 23, wherein the subsequently applied layer is a protective or hard coat layer applied to the adhesion promoting layer disposed on the outer layer (A1).
25. The electronic device of any one of claims 21 to 24, wherein the ink-receiving layer comprises a polyurethane.
26. 26. The electronic device of claim 25, wherein the ink-receiving layer is disposed on an outer layer (A2).
27. An electronic device according to any one of claims 21 to 26, wherein the subsequently applied layer is a graphic display layer which is applied to an ink receiving layer disposed on the outer layer (A2).
28. The electronic device according to any one of claims 21 to 27, wherein the functional layer has a thickness of 1.5 µm or less.
29. The electronic device of any one of claims 1-8 or 11-28, wherein the thermoformed film is thermoformable at a temperature in the range of 130°C to 200°C.
30. The electronic device of any one of claims 1-8 or 11-29, wherein the copolyester base layer of the thermoformed film exhibits a lower crystallinity than any of the outer layers.
31. [(X C-OUTER ) - (X C-BASE ) / (X C-OUTER ) × 100] is at least 40%, and X C-BASE is the crystallinity of the copolyester base layer of the thermoformed film, and X C-OUTER 31. The electronic device of claim 30, wherein: .times. ...
32. [(X C-OUTER ) - (X C-BASE ) / (X C-OUTER ) × 100] is 70% or less, C-BASE is the crystallinity of the copolyester base layer of the thermoformed film, and X C-OUTER 32. The electronic device of claim 30 or 31, wherein x is the crystallinity of the outer layer of the thermoformed film, the crystallinity of the layer being calculated from the enthalpy of fusion measured by differential scanning calorimetry.
33. The crystallinity (X C-OUTER ) is independently in the range of 25% to 50%, and / or the crystallinity (X C-BASE 29. The electronic device of claim 1, wherein the crystallinity of the layer is calculated from the enthalpy of fusion measured by differential scanning calorimetry.
34. 1. Use of a biaxially oriented coextruded polyester film comprising a base layer B of a copolyester, a first polyester outer layer A1 and a second polyester outer layer A2 as a thermoformable material for a touch screen in an electronic device, said outer layers being arranged directly on opposite surfaces of said base layer, (i) the base layer B comprises a copolyester derived from terephthalic acid (TA) and a second aromatic dicarboxylic acid and one or more diols, the second aromatic dicarboxylic acid being present in the copolyester in an amount of 5 to 20 mol % of the acid fraction of the copolyester; (ii) the polyester of each of said outer layers A1 and A2 is selected from polyethylene terephthalate (PET); (iii) the thickness of the base layer accounts for at least 90% of the total thickness of the coextruded multilayer polyester film; Use, The second aromatic dicarboxylic acid is isophthalic acid (IPA) and the film exhibits a haze of 4.0% or less.
35. 35. The use of claim 34 in the manufacture of an electronic device comprising a touch screen interface, wherein an outer surface of the touch screen interface is a thermoformed biaxially oriented coextruded polyester film produced by thermoforming the thermoformable biaxially oriented coextruded polyester film.
36. 1. A method of manufacturing an electronic device including a touch screen interface, comprising: (i) thermoforming the thermoformable biaxially oriented coextruded polyester film of claim 9 or 10 to produce a thermoformed biaxially oriented coextruded polyester film; and (ii) providing the thermoformed biaxially oriented coextruded polyester film as part of the touch screen interface in an electronic device. A method comprising:
37. 37. The method of claim 36, wherein the thermoformed biaxially oriented coextruded polyester film is provided as part of the touchscreen interface by forming an injection molded module that includes the touchscreen interface, whereby the injection molded module includes an interior portion or layer of injection molded polymeric material and further includes an exterior portion or layer of the thermoformed biaxially oriented coextruded polyester film.
38. 40. The method of claim 37, wherein an outer portion or layer of said thermoformed biaxially oriented coextruded polyester film has a graphic indicator layer disposed on an inner surface thereof.
39. A method for producing a thermoformable polyester film according to claim 9 or 10, comprising the steps of: (i) co-extruding said copolyester base layer B, said first polyester outer layer A1 and said second polyester outer layer A2 such that said outer layers are disposed on opposing surfaces of said base layer; (ii) quenching the extrudate; (iii) stretching the quenched extrudate in at least one direction at a temperature above the glass transition temperature of the polyester material; and (iv) heat setting the stretched film at a temperature in the range of 165-215° C., during which dimensional relaxation in the transverse dimensions of the film occurs in the range of 2% to 10%. A method comprising:
40. At least a portion of the heat-setting step is carried out at a temperature in the range of 205-215°C; and / or 40. The method of claim 39, wherein heat-setting is carried out in a multi-zone crystallizer, the temperature of the final zone being lower than the temperature of the first zone.
41. 41. The method of claim 40, wherein the first section is at a temperature of 205 to 215°C and the final section is at a temperature within the range of 170 to 190°C.
Citation Information
Patent Citations
Laminated light diffusing film
JP2002182013A
Biaxially oriented polyester film for molding member
JP2007111877A
Transparent conductive film and touch panel including the same
JP2017062609A