Carbon dioxide fixation method
By producing powdered dry ice and incorporating it into cement compositions with carbonated water, the method enhances carbon dioxide fixation and cement strength, addressing the limitations of existing carbon dioxide immobilization techniques.
Patent Information
- Application Number
- JP2021030185
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing methods for fixing carbon dioxide in cement compositions are limited in their ability to immobilize significant amounts of CO2, and there is a need for more effective techniques to enhance carbon dioxide fixation.
A method involving the production of powdered dry ice by reducing the pressure of liquefied carbon dioxide, forming block-shaped dry ice, and mixing it with cement and water to create a cement composition that fixes carbon dioxide, utilizing carbonated water to enhance fixation.
The method significantly increases the amount of carbon dioxide fixed in cement compositions while maintaining or improving the strength of the cement, as demonstrated by the higher CO2 fixation and compressive strength results compared to traditional methods.
Smart Images

Figure 0007583644000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for fixation of carbon dioxide. [Background technology]
[0002] In recent years, reducing carbon dioxide emissions has become an important issue in order to prevent global warming. In relation to this, technology is being considered in which carbon dioxide captured from exhaust gases generated in cement manufacturing plants is fixed in concrete or the like. For example, Patent Document 1 describes a method for producing CO2-absorbing precast concrete, which contains one or two of γ-CS (symbol γ) and steel slag powder (symbol B) as powder components, and Portland cement (symbol C), and the total of γ and B in the total content of γ, B, and C is 25 to 95 mass%, and the water-cement ratio W / C is 80 to 250%, and is poured into a formwork. After demolding, one or more holes that allow ventilation are drilled in the solidified concrete, and the solidified concrete is carbonation-cured in an atmosphere with a CO2 concentration of 5 to 95%, forming a carbonation region from the surface (excluding the surface inside the hole) to a depth of 20 mm or more (however, in the entire thickness of the part with a thickness of less than 20 mm), and also forming a carbonation region from the surface inside the hole. In this method, combustion exhaust gas discharged from a factory or facility can be used as a source of carbon dioxide used for carbonation curing.
[0003] Furthermore, as a method of mixing and fixing carbon dioxide gas into concrete, Patent Document 2 describes a method for mixing carbon dioxide gas into concrete, which is characterized by controlling and reducing the pressure of liquefied carbon dioxide gas pumped from a carbon dioxide gas storage facility to turn it into powdered dry ice, and then spraying this powdered dry ice into the concrete and mixing it therein. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-168436 A [Patent Document 2] Japanese Patent Application Publication No. 11-324324 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method capable of fixing more carbon dioxide in a cement composition. [Means for solving the problem]
[0006] As a result of intensive research into solving the above problems, the present inventors have discovered a method for producing powdered dry ice by ejecting liquefied carbon dioxide gas from a liquefied carbon dioxide gas storage means, and compressing and storing the powdered dry ice in a molding container to produce a powdered dry ice having a bulk density of 0.30 to 1.00 g / cm. 3 The inventors have found that the above-mentioned object can be achieved by a method for fixation of carbon dioxide, the method including the steps of obtaining a block of dry ice having a diameter of about 100 mm and removing the block of dry ice from a molding vessel and mixing at least the block of dry ice or its crushed material with cement and water to obtain a cement composition in which carbon dioxide derived from the block of dry ice is fixed, and have completed the present invention. That is, the present invention provides the following [1] to [3]. [1] A carbon dioxide solidification process in which liquefied carbon dioxide gas is compressed and liquefied under conditions of reducing pressure at a pressure reduction rate sufficient to produce dry ice from a liquefied carbon dioxide gas storage means in which the liquefied carbon dioxide gas is stored, to obtain powdered dry ice; and a process in which the powdered dry ice is compressed and stored in a molding container to obtain a powdered dry ice having a bulk density of 0.30 to 1.00 g / cm. 3and a dry ice utilization step of extracting the block-shaped dry ice from the molding container, and then mixing at least the block-shaped dry ice or its crushed pieces with cement and water to obtain a cement composition in which carbon dioxide derived from the block-shaped dry ice is fixed. [2] The volume of the block of dry ice or its crushed material is 100 to 1,000 cm 3 The method for fixation of carbon dioxide according to [1] above. [3] The method for fixation of carbon dioxide according to [1] or [2] above, wherein the water is carbon dioxide-containing water. Effect of the Invention
[0007] According to the method for immobilizing carbon dioxide of the present invention, a larger amount of carbon dioxide can be immobilized in the cement composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The method for fixing carbon dioxide of the present invention includes a carbon dioxide solidification step of ejecting liquefied carbon dioxide gas (hereinafter, abbreviated as "liquefied carbon dioxide gas") from a liquefied carbon dioxide gas storage means storing pressurized liquefied carbon dioxide gas under conditions of reducing the pressure at a pressure reduction rate sufficient to produce dry ice, thereby obtaining powdered dry ice, and a carbon dioxide solidification step of compressing and storing the powdered dry ice in a molding container to obtain a powdered dry ice having a bulk density of 0.30 to 1.00 g / cm. 3 The method includes a dry ice molding step of obtaining a block of dry ice having the same shape as the internal space of the molding container, and a dry ice utilization step of removing the block of dry ice from the molding container, and then mixing at least the block of dry ice or its crushed pieces with cement and water to obtain a cement composition in which carbon dioxide derived from the block of dry ice is fixed. Each step will be explained in detail below.
[0009] [Carbon dioxide solidification process] This process is a process in which liquefied carbon dioxide gas is ejected from a liquefied carbon dioxide gas storage means that stores pressurized liquefied carbon dioxide gas under conditions in which the pressure is reduced at a rate of pressure reduction sufficient to produce dry ice, thereby obtaining powdered dry ice. When carbon dioxide gas that has been liquefied by pressurization is suddenly released through a nozzle or the like, the temperature of the carbon dioxide gas drops due to the Joule-Thomson effect, and dry ice is produced. For example, powdered dry ice can be obtained by ejecting the liquefied carbon dioxide gas stored in the liquefied carbon dioxide gas storage means under atmospheric pressure through a nozzle or the like connected to the liquefied carbon dioxide gas storage means. The temperature at which the liquefied carbon dioxide gas is ejected under atmospheric pressure is not particularly limited, but is usually room temperature (e.g., 20°C). The liquefied carbon dioxide gas storage means is not particularly limited as long as it is capable of storing liquefied carbon dioxide gas while maintaining it in a liquefied state, and examples thereof include a liquefied carbon dioxide gas cylinder, a liquefied carbon dioxide gas storage tank, etc.
[0010] [Dry ice molding process] In this process, the powdered dry ice obtained in the previous process is compressed and placed in a molding container to form a powder having a bulk density of 0.30 to 1.00 g / cm. 3 This is a process for obtaining a block of dry ice having the same shape as the internal space of the molding container. The molding container is not particularly limited in material or shape as long as it can accommodate powdered dry ice in its internal space. From the viewpoint of easily taking out the molded dry ice, the shape of the molding container is preferably a cylindrical or prismatic internal space, more preferably a cylindrical one.
[0011] An example of a method for compressing and storing powdered dry ice in a molding container is to use the pressure of the powdered dry ice ejected from a liquefied carbon dioxide gas storage means to feed the powdered dry ice into the molding container while simultaneously compressing it. Also, after powdered dry ice is poured into the molding container, the powdered dry ice in the molding container may be compressed using a press or the like.
[0012] The bulk density of block dry ice is 0.30 to 1.00 g / cm 3 , preferably 0.35 to 0.90 g / cm 3 , more preferably 0.45 to 0.80 g / cm 3 , particularly preferably 0.48 to 0.60 g / cm 3 The bulk density is 0.30 g / cm 3 If the bulk density is less than 1.00 g / cm, the block-shaped dry ice is easily crushed when the dry ice is mixed with cement or the like in the dry ice utilization step described below, and the dry ice is easily sublimated, resulting in a small amount of immobilized carbon dioxide. 3 If the temperature exceeds this range, it becomes difficult to mix the dry ice evenly into the cement composition.
[0013] The volume of the block of dry ice is preferably 100 to 1,000 cm. 3 , more preferably 200 to 950 cm 3 , and more preferably 300 to 900 cm 3 , particularly preferably 400 to 850 cm 3 If the volume above is 100 cm 3 If the volume is less than 1,000 g / cm, the block-shaped dry ice is easily crushed when the dry ice is mixed with cement or the like in the dry ice utilization step described below, and the dry ice is easily sublimated, resulting in a small amount of immobilized carbon dioxide. 3 If the temperature exceeds this range, it becomes difficult to mix the dry ice evenly into the cement composition.
[0014] [Dry ice usage process] This step involves removing the block-shaped dry ice from the molding vessel, and then mixing at least the block-shaped dry ice or its crushed pieces with cement and water to obtain a cement composition in which carbon dioxide derived from the block-shaped dry ice is fixed. The amount of block-shaped dry ice or crushed pieces to be mixed will vary depending on the bulk density and volume of the dry ice, the amount of cement to be mixed, etc., but may be one piece or two or more pieces. Depending on the shape and size of the mixing means such as a mixer, the block-shaped dry ice taken out of the molding vessel may be crushed and the resulting crushed material may be mixed with cement or the like. The volume of the crushed material is set to 100 cm3 or less in order to prevent the dry ice from being easily crushed. 3 More than 200cm, preferably 200cm 3 That's all. The amount of block-shaped dry ice or crushed pieces thereof (however, two or more block-shaped dry ice or crushed pieces thereof may be used, in which case the total amount) is preferably 100 to 250 kg, more preferably 120 to 230 kg, further preferably 140 to 200 kg, and particularly preferably 150 to 180 kg per ton of cement. If the amount is 100 kg or more, the amount of carbon dioxide fixed in the cement composition can be increased. If the amount is 250 kg or less, a decrease in the strength development of the cement composition can be prevented.
[0015] The above cement is not particularly limited, and examples thereof include various Portland cements such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, and low-heat Portland cement, mixed cements such as blast-furnace cement and fly ash cement, and ecocement, etc. These may be used alone or in combination of two or more.
[0016] The water is not particularly limited, and for example, tap water, industrial water, etc. can be used. The amount of water is not particularly limited, and may be any amount generally used in cement compositions such as paste, mortar, and concrete. From the viewpoint of fixing a large amount of carbon dioxide in the cement composition, carbon dioxide-containing water may be used as the water. In this specification, the term "carbonated water" refers to water containing carbon dioxide gas (gaseous carbon dioxide). Specific examples include carbonated water, carbon dioxide bubble-free water, water saturated with dry ice, and carbon dioxide fine bubble water having bubbles containing carbon dioxide gas (e.g., carbon dioxide microbubble water, carbon dioxide ultrafine bubble water, etc.). Carbonated water can be obtained, for example, by blowing carbon dioxide into water under high pressure. Water containing dissolved carbon dioxide without bubbles can be obtained, for example, by blowing carbon dioxide into water under normal pressure. Further, as the carbon dioxide gas or the carbon dioxide gas used as a raw material for the dry ice, a gas obtained by separating and recovering carbon dioxide from exhaust gas generated in cement production, etc. can be used. By using such a gas, it is possible to reduce the amount of carbon dioxide emitted in cement production, etc.
[0017] Furthermore, fine bubble water is water that contains air bubbles, and in which the proportion of air bubbles having a particle size of less than 100 μm is 50 vol% or more of the total volume (100 vol%) of the air bubbles. Examples of carbon dioxide fine bubble water containing bubbles containing carbon dioxide gas include carbon dioxide ultrafine bubble water in which the proportion of bubbles with a particle size of less than 1 μm is 50% or more by volume of the total bubble volume (100% by volume), and carbon dioxide microbubble water in which the proportion of bubbles with a particle size of 1 μm or more and less than 100 μm is 50% or more by volume of the total bubble volume (100% by volume). The gas constituting the bubbles contains carbon dioxide gas. The content of carbon dioxide gas in the gas constituting the bubbles is preferably 5% by volume or more, more preferably 20% by volume or more, and particularly preferably 40% by volume or more. If the content is 5% by volume or more, the amount of carbon dioxide fixed in the cement composition can be increased. As the gas constituting the bubbles, exhaust gas generated in cement production or the like, or gas obtained by separating and recovering carbon dioxide from the exhaust gas, or the like, may be used. By using the exhaust gas or gas obtained by separating and recovering carbon dioxide from the exhaust gas, or the like, the amount of carbon dioxide emitted in cement production or the like can be reduced.
[0018] The amount of carbon dioxide gas in the carbon dioxide-containing water is preferably 500 to 10,000 mg / L, more preferably 1,000 to 9,000 mg / L, even more preferably 1,500 to 9,000 mg / L, and particularly preferably 3,000 to 7,000 mg / L. If the concentration is 500 mg / L or more, the amount of carbon dioxide fixed in the cement composition can be increased. If the amount is 10,000 mg / L or less, the pH value when mixing the cement composition does not become excessively low, and the fluidity of the cement composition can be prevented from decreasing.
[0019] In this step, other materials may be mixed as necessary. Examples of other materials that may be mixed as necessary include fine aggregate, coarse aggregate, various admixtures such as air-entraining agents, water-reducing agents, air-entraining water-reducing agents, high-performance water-reducing agents, and high-performance air-entraining water-reducing agents, and various admixtures such as fly ash, silica fume, and ground granulated blast furnace slag.
[0020] The method for mixing each material is not particularly limited, and each material may be added at once and mixed, or a method in which water and a powdered or granular material other than block-shaped dry ice or crushed dry ice, such as cement, are mixed, and then water and the block-shaped dry ice or crushed dry ice are added to the obtained mixture and mixed. EXAMPLES
[0021] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Materials used] (1) Cement: ordinary Portland cement manufactured by Taiheiyo Cement Corporation (2) Water; Carbonated water (carbon dioxide content: 6,000 mg / liter) (3) Fine aggregate: mountain sand (4) Air-entraining water-reducing agent; product name "Master Polyhede 15S" manufactured by Pozzolith Corporation
[0022] [Example 1] Powdered dry ice was sprayed from a nozzle connected to a liquefied carbon dioxide gas cylinder into a cylindrical molding container with an internal space of 12 cm in diameter and 7 cm in height at 20°C under atmospheric pressure. The dry ice was compressed by the pressure of the spray from the nozzle. From the molding container, a cylindrical piece of dry ice with a diameter of 12 cm and a height of 7 cm (volume: 791 cm) 3 The bulk density of this cylindrical (block-shaped) dry ice is 0.87 g / cm 3 The cylindrical dry ice was crushed into three pieces of crushed dry ice (volume of each piece: 200 to 300 cm 3 degree) was obtained. Cement and carbonated water, which had been mixed with an AE water-reducing agent in advance, were poured into the mixer and mixed for 30 seconds, after which fine aggregate was poured into the mixer and mixed for 30 seconds. After that, the kneaded material adhering to the inner wall of the mixer was scraped off, and the mixture was mixed for 60 seconds. Next, crushed dry ice was poured into the mixer and mixed for 120 seconds to obtain mortar. The amounts of each material were determined so that the mass ratio of carbonated water to cement (carbonated water / cement) was 0.5, and the mass ratio of fine aggregate to cement (fine aggregate / cement) was 2.55. The amount of dry ice was determined to be 167 kg per ton of cement. The amount of AE water reducer was determined to be 0.7 parts by mass per 100 parts by mass of cement.
[0023] The compressive strength of the resulting mortar at ages of 1 day, 7 days, and 28 days was measured in accordance with JIS R 5201:2015 (Physical testing methods for cement). The amount of carbon dioxide fixed in the mortar was determined as the mass per ton of cement contained in the mortar by thermogravimetry-differential thermal analysis (TG-DTA). Specifically, from the measurement results of thermogravimetry-differential thermal analysis (TG-DTA), the decrease in mass in the endothermic peak range of about 550 to 800°C was determined to be due to decarbonation of calcium carbonate contained in the mortar, and the amount of carbon dioxide was calculated from the amount of the decrease.
[0024] [Examples 2 to 3] Dry ice having the bulk density shown in Table 1 was obtained in the same manner as in Example 1, except that the pressure of the spray from the nozzle was changed. Mortar was produced using the obtained dry ice in the same manner as in Example 1, and the compressive strength of the mortar and the amount of carbon dioxide fixed in the mortar were measured. [Comparative Example 1] Cement and water that had been mixed with an AE water-reducing agent were poured into the mixer and mixed for 30 seconds, after which fine aggregate was poured into the mixer and mixed for 30 seconds. Next, the kneaded material adhering to the inner wall of the mixer was scraped off, and the mixture was mixed for 180 seconds to obtain mortar. The mixing ratio of each material was set so that the mass ratio of water to cement (carbonated water / cement) was 0.5, and the mass ratio of fine aggregate to cement (fine aggregate / cement) was 2.55. The amount of AE water reducer was set to 0.7 parts by mass per 100 parts by mass of cement. The compressive strength of the obtained mortar and the amount of carbon dioxide fixed in the mortar were measured in the same manner as in Example 1.
[0025] [Comparative Example 2] A mortar was obtained in the same manner as in Example 1, except that, instead of the crushed dry ice, powdered dry ice having the same mass as the crushed dry ice was used. The mortar compressive strength and the amount of carbon dioxide fixed in the mortar at ages of 1 day, 7 days, and 28 days were measured in the same manner as in Example 1. Table 1 shows the mortar compressive strength at ages of 1 day, 7 days, and 28 days for each of Examples 1 to 3 and Comparative Examples 1 and 2, as well as the amount of carbon dioxide absorbed from the dry ice and carbonated water and fixed in the mortar. In Examples 1 to 3 and Comparative Examples 1 and 2, the amounts of carbon dioxide calculated from the TG-DTA measurements include that derived from calcium carbonate of limestone contained in cement, which is a raw material for mortar. Because the type and amount of cement used in Examples 1 to 3 and Comparative Examples 1 and 2 are the same, the amount of carbon dioxide absorbed from the dry ice and carbonated water and fixed in the mortar can be calculated by subtracting the amount of carbon dioxide in Comparative Example 1 (all of which is derived from the limestone contained in the cement, and the mass of carbon dioxide per ton of cement is 32.8 kg) from the amount of carbon dioxide in each of Examples 1 to 3 and Comparative Examples 2 and 3.
[0026] [Table 1]
[0027] From Table 1, it can be seen that in Examples 1 to 3, the amount of carbon dioxide per ton of cement (12.4 to 15.3 kg / ton) that was absorbed from the block dry ice and carbonated water and fixed in the mortar was greater than the amount of carbon dioxide per ton of cement (7.9 kg / ton) that was absorbed from the powdered dry ice and carbonated water and fixed in the mortar in Comparative Example 2. Furthermore, the compressive strength of the mortar at ages of 7 days and 28 days in Examples 1 to 3 (7 days: 36.3 to 37.2 N / mm 2 , 28th: 57.2~61.2N / mm 2 ) is the compressive strength of the mortar at ages of 7 days and 28 days in Comparative Examples 1 and 2 (7 days: 32.1 to 35.0 N / mm 2 , 28th: 50.2~51.2N / mm 2 ) is found to be larger than
Claims
1. a carbon dioxide solidification step of ejecting the liquefied carbon dioxide from a liquefied carbon dioxide storage means in which the liquefied carbon dioxide is stored under conditions of reducing the pressure at a pressure reduction rate sufficient to produce dry ice, thereby obtaining powdered dry ice; The powdered dry ice is compressed and stored in a molding container to produce a bulk density of 0.45 to 0.90 g / cm 3 a dry ice molding step of obtaining a block of dry ice having the same shape as the internal space of the molding container and a volume of 100 to 1,000 cm 3 ; The method includes a dry ice utilization step of removing the block-shaped dry ice from the molding vessel, and then mixing at least the block-shaped dry ice or crushed pieces of the dry ice obtained by crushing the block-shaped dry ice and having a volume of 100 cm3 or more, cement, and water to obtain a cement composition in which carbon dioxide derived from the block-shaped dry ice is fixed. A method for fixation of carbon dioxide, characterized in that in the dry ice utilization step, the amount of the block-shaped dry ice or the crushed dry ice is 100 to 250 kg per ton of cement.
2. 2. The method for fixation of carbon dioxide according to claim 1, wherein the water is carbon dioxide-containing water.
Citation Information
Patent Citations
Precast hollow concrete member and preparation method thereof
CN104420580A
Production of concrete for vegetation and precast concrete for vegetation
JP1996143382A
Method and device for mixing carbon dioxide with concrete
JP1999324324A
Method for producing dry ice aerosol
JP2003054929A
Apparatus for manufacturing dry ice
JP2006240918A