Wafer placement table
By employing metal matrix composites or low thermal expansion metals with ceramic materials and high thermal conductivity bonding layers, the wafer mounting table achieves cost-effective and durable heat removal, addressing the high manufacturing costs and thermal stress issues of conventional designs.
Patent Information
- Application Number
- JP2021166081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-08
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-10-08
AI Technical Summary
Conventional wafer mounting tables face high manufacturing costs due to the use of expensive materials like metal matrix composites (MMC) and low thermal expansion metals, which are difficult to process and costly to form coolant flow paths, leading to increased production expenses.
The use of metal matrix composite materials or low thermal expansion metals for the cooling base material, combined with a ceramic material for the grooved or perforated base material, and a high thermal conductivity metal bonding layer, reduces manufacturing costs while maintaining effective heat removal and minimizing thermal stress.
This configuration lowers manufacturing costs by utilizing less expensive materials and near net shape technologies, enhances heat removal capacity, and reduces the likelihood of damage from thermal stress, ensuring efficient and durable wafer processing.
Smart Images

Figure 0007583698000001 
Figure 0007583698000002 
Figure 0007583698000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer stage. [Background technology]
[0002] Conventionally, a wafer mounting table is known in which a ceramic base material such as alumina in which an electrostatic adsorption electrode is embedded and a cooling base material made of a metal such as aluminum are bonded via a resin layer (see, for example, Patent Document 1). With such a wafer mounting table, the effect of the thermal expansion difference between the ceramic base material and the cooling base material can be alleviated by the resin layer. A wafer mounting table is also known in which a ceramic base material and a cooling base material having a coolant flow path are bonded using a metal bonding layer instead of a resin layer (see, for example, Patent Documents 2 and 3). Since the metal bonding layer has a higher thermal conductivity than the resin layer, it can realize the heat extraction capacity required when processing a wafer with high-power plasma. On the other hand, since the metal bonding layer has a larger Young's modulus and a lower stress relaxation property than the resin layer, it is almost impossible to alleviate the effect of the thermal expansion difference between the ceramic base material and the cooling base material. In Patent Documents 2 and 3, a metal matrix composite (MMC) having a small difference in thermal expansion coefficient from the ceramic base material is used as the material of the cooling base material in order to make it less likely to break due to the thermal expansion difference. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 4-287344 [Patent Document 2] Patent No. 5666748 [Patent Document 3] Patent No. 5666749 Summary of the Invention [Problem to be solved by the invention]
[0004] However, MMC is more expensive than metals such as aluminum, is difficult to process, and requires high costs for forming the coolant flow paths, which can increase the manufacturing cost of the wafer mounting table.Instead of MMC, it is possible to use a low-thermal expansion metal material that has a small difference in thermal expansion coefficient from the ceramic base material, but the low-thermal expansion metal material is also expensive, is difficult to process, and requires high costs for forming the coolant flow paths, which can increase the manufacturing cost of the wafer mounting table.
[0005] The present invention has been made to solve the above problems, and has as its main object to reduce the manufacturing cost of a wafer mounting table that has high heat removal capacity and is less susceptible to breakage. [Means for solving the problem]
[0006] The first wafer mounting table of the present invention comprises: a ceramic substrate having a wafer mounting surface on an upper surface thereof and incorporating an electrode; A cooling substrate having a refrigerant flow path formed therein; a metal bonding layer bonding the lower surface of the ceramic substrate and the upper surface of the cooling substrate; Equipped with The cooling substrate comprises a ceiling substrate made of a metal matrix composite material or a low thermal expansion metal material which constitutes the ceiling of the refrigerant flow path, a grooved substrate made of a ceramic material having the same main component as the ceramic substrate and having a flow path groove on its upper surface which constitutes the bottom and side walls of the refrigerant flow path, and a metal ceiling joining layer which joins the lower surface of the ceiling substrate to the upper surface of the grooved substrate.
[0007] In the first wafer mounting table of the present invention, among the cooling base materials, MMC or a low thermal expansion metal material is used for the ceiling base material, while a ceramic material that is relatively inexpensive and can form flow channel grooves at a relatively low cost by near net shape technology or the like is used for the grooved base material. This reduces the manufacturing cost of the wafer mounting table. In addition, as the bonding layer between the ceramic base material and the ceiling base material and between the ceiling base material and the grooved base material, a metal bonding layer with high thermal conductivity is used instead of a resin layer with low thermal conductivity. This results in a high ability to draw heat from the wafer (heat extraction ability). Furthermore, since the main component of the ceramic material constituting the grooved base material is the same as the main component of the ceramic material constituting the ceramic base material, the grooved base material has a small absolute value of the difference in linear thermal expansion coefficient with the ceramic base material. Therefore, the ceramic base material, the ceiling base material, and the grooved base material have a small absolute value of the difference in linear thermal expansion coefficient between them, and even if the stress relaxation property of the bonding layer is low, problems are unlikely to occur.
[0008] In this specification, a low thermal expansion metal material is one having a linear thermal expansion coefficient of 10×10 at 40 to 400°C. -6 / K or less, and is 9.0 x 10 -6 / K or less is preferable, and 8.0×10 -6 / K or less is more preferable. In this specification, the linear thermal expansion coefficient obtained by measuring the length at 40°C and 400°C is referred to as the linear thermal expansion coefficient at 40 to 400°C. In this specification, the main component refers to a component that occupies 50 mass% or more of the total components contained, preferably 70 mass% or more, and more preferably 90 mass% or more. In this specification, the present invention may be described using up and down, left and right, front and back, etc., but up and down, left and right, front and back are merely relative positional relationships. Therefore, when the orientation of the wafer mounting table is changed, up and down may become left and right, or left and right may become up and down, but such cases are also included in the technical scope of the present invention.
[0009] In the first wafer-mounting table of the present invention, the metal matrix composite material or low thermal expansion metal material constituting the ceiling base material and the ceramic material constituting the grooved base material have an absolute value of difference in linear thermal expansion coefficient at 40 to 400°C of 1.5 × 10 from the ceramic material constituting the ceramic base material. -6 / K or less. In this way, even if the stress relaxation property of the bonding layer is low, problems are less likely to occur.
[0010] In the first wafer mounting table of the present invention, the ceramic material constituting the ceramic substrate may be alumina, and the ceramic material constituting the grooved substrate may be alumina having a lower purity than the alumina constituting the ceramic substrate, thereby making it possible to manufacture the grooved substrate at a lower cost.
[0011] The second wafer mounting table of the present invention is a ceramic substrate having a wafer mounting surface on an upper surface thereof and incorporating an electrode; A cooling substrate having a refrigerant flow path formed therein; a metal bonding layer bonding the lower surface of the ceramic substrate and the upper surface of the cooling substrate; Equipped with The cooling substrate comprises a ceiling substrate made of a metal matrix composite material or a low thermal expansion metal material that constitutes the ceiling of the refrigerant flow path, a perforated substrate made of a ceramic material having the same main component as the ceramic substrate and having flow path holes that penetrate in the vertical direction and that constitute the side walls of the refrigerant flow path, a bottom substrate that constitutes the bottom of the refrigerant flow path, a metal ceiling joining layer that joins the underside of the ceiling substrate to the upper side of the perforated substrate, and a bottom joining layer that joins the underside of the perforated substrate to the upper side of the bottom substrate.
[0012] In the second wafer mounting table of the present invention, MMC or a low thermal expansion metal material is used for the ceiling substrate among the cooling substrates, while a ceramic material that is relatively inexpensive and can form flow passage holes at a relatively low cost by near net shape technology or the like is used for the perforated substrate. This reduces the manufacturing cost of the wafer mounting table. In addition, as the bonding layer between the ceramic substrate and the ceiling substrate and between the ceiling substrate and the perforated substrate, a metal bonding layer with high thermal conductivity is used instead of a resin layer with low thermal conductivity. This results in a high ability to draw heat from the wafer (heat extraction ability). Furthermore, since the main component of the ceramic material constituting the perforated substrate is the same as the main component of the ceramic material constituting the ceramic substrate, the perforated substrate has a small absolute value of the difference in linear thermal expansion coefficient with the ceramic substrate. Therefore, the absolute value of the difference in linear thermal expansion coefficient between the ceramic substrate, the ceiling substrate, and the perforated substrate is small, and even if the stress relaxation property of the bonding layer is low, problems are unlikely to occur.
[0013] In the second wafer mounting table of the present invention, the bottom substrate may be made of a metal matrix composite material or a low thermal expansion metal material, and the bottom bonding layer may be made of metal. In this way, since the absolute value of the difference in linear thermal expansion coefficient between the material constituting the ceramic substrate and the material constituting the bottom substrate is small, the influence of the difference in linear thermal expansion coefficient between the ceramic substrate and the ceiling substrate or the perforated substrate, and the influence of the difference in linear thermal expansion coefficient between the ceiling substrate or the perforated substrate and the bottom substrate are canceled, and warping and damage of the wafer mounting table 10 can be suppressed. Therefore, the degree of freedom of the material constituting the ceiling substrate or the perforated substrate is increased. In addition, since the perforated substrate and the bottom substrate are bonded with a metal bonding layer, the bonding between the ceramic substrate and the ceiling substrate and the bonding between the ceiling substrate and the perforated substrate can be performed simultaneously, and the wafer mounting table can be efficiently manufactured.
[0014] In the second wafer mounting table of the present invention, the metal matrix composite material or low thermal expansion metal material constituting the ceiling base material and the ceramic material constituting the perforated base material are The fee is The absolute value of the difference in linear thermal expansion coefficient between the ceramic material constituting the ceramic base material and the ceramic material at 40 to 400°C is 1.5 × 10 -6 / K or less. In this way, even if the stress relaxation property of the bonding layer is low, problems are less likely to occur.
[0015] In the second wafer support of the present invention, the ceramic material constituting the ceramic substrate may be alumina, and the ceramic material constituting the perforated substrate may be alumina having a lower purity than the alumina constituting the ceramic substrate, thereby making it possible to manufacture the perforated substrate at a lower cost. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a vertical cross-sectional view of the wafer mounting table 10 installed in the chamber 94. [Diagram 2] FIG. [Diagram 3] 1 is a cross-sectional view of the wafer mounting table 10 cut by the upper surface of a grooved substrate 83 as viewed from above. [Figure 4] 5A to 5C are diagrams showing the manufacturing process of the wafer mounting table 10. [Diagram 5] FIG. 2 is a vertical cross-sectional view of the wafer mounting table 210. [Figure 6] FIG. 4 is a vertical cross-sectional view of another embodiment of the wafer mounting table 10. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [First embodiment] The wafer mounting table 10 according to the first embodiment of the present invention will be described below with reference to the drawings. Fig. 1 is a vertical cross-sectional view of the wafer mounting table 10 installed in a chamber 94 (a cross-sectional view when cut along a plane including the central axis of the wafer mounting table 10), Fig. 2 is a plan view of the wafer mounting table 10, and Fig. 3 is a cross-sectional view of the wafer mounting table 10 cut along an upper surface of a grooved substrate 83 as viewed from above. In this specification, the symbol "to" indicating a numerical range is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0018] The wafer mounting table 10 is used for performing CVD, etching, and the like on a wafer W using plasma, and is fixed to a mounting plate 96 provided inside a semiconductor process chamber 94. The wafer mounting table 10 includes a ceramic base 20, a cooling base 30, and a metal bonding layer 40.
[0019] The ceramic base 20 has a central portion 22 having a circular wafer mounting surface 22a, and an outer peripheral portion 24 having an annular focus ring mounting surface 24a on the outer periphery of the central portion 22. Hereinafter, the focus ring may be abbreviated as "FR." A wafer W is mounted on the wafer mounting surface 22a, and a focus ring 78 is mounted on the FR mounting surface 24a. The ceramic base 20 is made of a ceramic material such as alumina or aluminum nitride. The FR mounting surface 24a is one step lower than the wafer mounting surface 22a.
[0020] The center portion 22 of the ceramic base material 20 incorporates a wafer adsorption electrode 26 on the side close to the wafer placement surface 22a. The wafer adsorption electrode 26 is formed of a material containing, for example, W, Mo, WC, MoC, etc. The wafer adsorption electrode 26 is a disk-shaped or mesh-shaped monopolar electrostatic electrode. The layer of the ceramic base material 20 above the wafer adsorption electrode 26 functions as a dielectric layer. A wafer adsorption DC power source 52 is connected to the wafer adsorption electrode 26 via a power supply terminal 54. The power supply terminal 54 is provided so as to pass through an insulating tube 55 disposed in a through hole that vertically penetrates the cooling base material 30 and the metal bonding layer 40, and reach the wafer adsorption electrode 26 from the lower surface of the ceramic base material 20. A low pass filter (LPF) 53 is provided between the wafer adsorption DC power source 52 and the wafer adsorption electrode 26.
[0021] The cooling substrate 30 is a disk member having a larger diameter than the ceramic substrate 20, and has an inner peripheral portion 32 where the ceramic substrate 20 is disposed, and an outer peripheral portion 34 that protrudes from the outer periphery of the ceramic substrate 20. The cooling substrate 30 includes a ceiling substrate 81, a grooved substrate 83, and a ceiling bonding layer 82. The cooling substrate 30 includes a refrigerant flow path 38 through which a refrigerant can circulate inside. The refrigerant flow path 38 is provided in a spiral shape from an inlet 38a to an outlet 38b so that the refrigerant can reach the entire area where the ceramic substrate 20 is disposed (FIG. 3). The inlet 38a and the outlet 38b of the refrigerant flow path 38 penetrate the grooved substrate 83 in the vertical direction and open to the bottom surface of the refrigerant flow path 38. The inlet 38a and the outlet 38b of the refrigerant flow path 38 are connected to a refrigerant cooling device (not shown), and the refrigerant discharged from the outlet 38b is temperature-adjusted by the refrigerant cooling device, and then returned to the inlet 38a and supplied into the refrigerant flow path 38.
[0022] The ceiling base material 81 is a disk member made of a metal matrix composite material (also called metal matrix composite (MMC)). The ceiling base material 81 constitutes the ceiling of the refrigerant passage 38. The MMC used for the ceiling base material 81 has a linear thermal expansion coefficient difference of 1.5×10 at 40 to 400°C from the ceramic material used for the ceramic base material 20. -6 / K or less, and 1.0×10 -6 / K or less is more preferable, and 0.5×10 -6 / K or less. Examples of MMC include materials containing Si, SiC, and Ti, and materials in which a porous SiC body is impregnated with Al and / or Si. A material containing Si, SiC, and Ti is called SiSiCTi, a material in which a porous SiC body is impregnated with Al is called AlSiC, and a material in which a porous SiC body is impregnated with Si is called SiSiC. When the ceramic base material 20 is an alumina base material, the MMC used for the ceiling base material 81 is preferably AlSiC or SiSiCTi. The linear thermal expansion coefficient at 40 to 400°C for alumina is 7.2×10 -6 / K, and AlSiC (SiC75%) is 7.8×10 -6 / K, and SiSiCTi is 7.3 × 10 -6 / K. When the ceramic base material 20 is an aluminum nitride base material, the MMC used for the ceiling base material 81 is preferably AlSiC or SiSiC. The linear thermal expansion coefficient of aluminum nitride at 40 to 400°C is 4.6×10 -6 / K, and AlSiC (SiC85%) is 5.6×10 -6 / K. The ceiling base material 81, together with the metal bonding layer 40 and the metal ceiling bonding layer 82, also functions as a radio frequency (RF) electrode for generating plasma. The power supply terminal 64 is provided so as to pass through a through hole 66 that passes through the grooved base material 83 and the ceiling bonding layer 82 in the vertical direction, and reach the underside of the ceiling base material 81. A high pass filter (HPF) 63 is disposed between the ceiling base material 81 and the RF power source 62.
[0023] The grooved substrate 83 is a disk member made of a ceramic material. As shown in FIG. 3, the upper surface of the grooved substrate 83 is provided with a flow channel groove 88 that constitutes the bottom and side walls of the refrigerant flow channel 38. The ceramic material used for the grooved substrate 83 has the same main component as the ceramic material used for the ceramic substrate 20. The main component refers to a component that occupies 50 mass% or more of the total components contained, preferably 70 mass% or more, and more preferably 90 mass% or more. The absolute value of the difference in linear thermal expansion coefficient is small between ceramic materials having the same main component. The ceramic material constituting the grooved substrate 83 may be a material having the same main component as the ceramic material constituting the ceramic substrate 20 but with a low purity. For example, the ceramic substrate 20 may be made of alumina with a high purity (e.g., alumina 99% or more) from the viewpoint of improving electrical properties as a dielectric layer, and the grooved substrate 83 may be made of alumina with a low purity (e.g., alumina 95%) from the viewpoint of improving mechanical properties such as toughness and reducing costs. The low purity material may contain more glass such as SiO2 than the high purity material. The ceramic material used for the grooved substrate 83 has an absolute difference in linear thermal expansion coefficient between the ceramic material used for the ceramic substrate 20 and the substrate 83 at 40 to 400°C of 1.5×10 -6 / K or less, and 1.0×10 -6 / K or less is more preferable, and 0.5×10 -6The ceramic material used for the grooved substrate 83 has an absolute value of 1.5×10 / K or less of linear thermal expansion coefficient difference at 40 to 400° C. from the MMC used for the ceiling substrate 81. -6 / K or less, and 1.0×10 -6 / K or less is more preferable, and 0.5×10 -6 It is more preferable that the value is equal to or less than 1 / K.
[0024] The ceiling bonding layer 82 is a metal bonding layer that bonds the lower surface of the ceiling base material 81 and the upper surface of the grooved base material 83. The ceiling bonding layer 82 may be, for example, a layer formed of solder or metal brazing material. The ceiling bonding layer 82 is formed, for example, by TCB (thermal compression bonding). TCB refers to a known method in which a metal bonding material is sandwiched between two members to be bonded, and the two members are pressurized and bonded while being heated to a temperature below the solidus temperature of the metal bonding material. The material of the ceiling bonding layer 82 may be the same as the material of the metal bonding layer 40.
[0025] The metal bonding layer 40 bonds the lower surface of the ceramic base material 20 and the upper surface of the cooling base material 30. The metal bonding layer 40 may be, for example, a layer formed of solder or a metal brazing material. The metal bonding layer 40 is formed, for example, of TCB.
[0026] The side surface of the outer periphery 24 of the ceramic substrate 20, the outer periphery of the metal bonding layer 40, and the side surface of the cooling substrate 30 are covered with an insulating film 42. The insulating film 42 may be, for example, a thermally sprayed film of alumina, yttria, or the like.
[0027] The wafer mounting table 10 is attached to a mounting plate 96 provided inside a chamber 94 by using a clamp member 70. The clamp member 70 is an annular member having a cross section in a substantially inverted L-shape, and has an inner peripheral step surface 70a. The wafer mounting table 10 and the mounting plate 96 are integrated by the clamp member 70. With the inner peripheral step surface 70a of the clamp member 70 placed on the outer periphery 34 of the cooling substrate 30 of the wafer mounting table 10, a bolt 72 is inserted from the upper surface of the clamp member 70 and screwed into a screw hole provided on the upper surface of the mounting plate 96. The bolt 72 is attached to a plurality of locations (e.g., 8 locations or 12 locations) that are provided at equal intervals along the circumferential direction of the clamp member 70. The clamp member 70 and the bolt 72 may be made of an insulating material or a conductive material (metal, etc.).
[0028] Next, a manufacturing example of the wafer mounting table 10 will be described with reference to Fig. 4. Fig. 4 is a manufacturing process diagram of the wafer mounting table 10. First, a disk-shaped ceramic sintered body 120, which is the base of the ceramic substrate 20, is produced by hot-pressing and firing a ceramic powder compact (Fig. 4A). The ceramic sintered body 120 has a built-in wafer adsorption electrode 26. Next, a hole 27 is made from the bottom surface of the ceramic sintered body 120 to the wafer adsorption electrode 26 (Fig. 4B), and a power supply terminal 54 is inserted into the hole 27 to join the power supply terminal 54 and the wafer adsorption electrode 26 (Fig. 4C).
[0029] In parallel with this, the MMC disk member 181 and the grooved disk member 183 made of a ceramic material and having a flow channel 88 formed on the upper surface are fabricated (FIG. 4D). Next, the through hole 131 penetrating in the vertical direction is formed in the MMC disk member 181, and the through holes 132 and 66 penetrating in the vertical direction and the inlet 38a and the outlet 38b penetrating in the vertical direction and opening on the bottom surface of the flow channel 88 are formed in the grooved disk member 183, and the power supply terminal 64 is joined to the lower surface of the MMC disk member 181 at a position facing the through hole 66 (FIG. 4E). When the ceramic sintered body 120 is made of alumina, it is preferable that the MMC disk member 181 is made of SiSiCTi or AlSiC. This is because the thermal expansion coefficient of alumina is approximately the same as that of SiSiCTi or AlSiC. Furthermore, when the ceramic sintered body 120 is made of alumina, the grooved disk member 183 is preferably made of alumina having a lower purity than the ceramic sintered body 120. The grooved disk member 183 can be manufactured by, for example, near net shape technology.
[0030] The SiSiCTi disk member can be manufactured, for example, as follows. First, silicon carbide, metal Si, and metal Ti are mixed to produce a powder mixture. Next, the obtained powder mixture is uniaxially pressed to produce a disk-shaped compact, which is then hot-press sintered in an inert atmosphere to obtain the SiSiCTi disk member.
[0031] When the grooved disk member 183 is produced using the near net shape technology, it can be produced, for example, as follows. That is, a molded body having a predetermined shape that will become the shape of the grooved substrate 83 after firing is produced by stacking a plurality of ceramic green sheets, and the molded body is fired at normal pressure to obtain the grooved substrate 83. The molded body may be produced by mold casting, or may be produced by a 3D printer using optical shaping or the like. The molded body may also be produced by producing a disk molded body without grooves, and then forming grooves corresponding to the flow channel grooves 88 by cutting or the like.
[0032] Next, metal bonding materials are placed on the upper surface of the MMC disk member 181 and the upper surface of the grooved disk member 183. Necessary through holes are provided in each metal bonding material. Then, the power supply terminal 64 of the MMC disk member 181 is inserted into the through hole 66 of the grooved disk member 183, and the MMC disk member 181 is placed on the metal bonding material placed on the upper surface of the grooved disk member 183. Furthermore, the power supply terminal 54 of the ceramic sintered body 120 is inserted into the through hole 131 of the MMC disk member 181 and the through hole 132 of the grooved disk member 183, and the ceramic sintered body 120 is placed on the metal bonding material placed on the upper surface of the MMC disk member 181. As a result, a laminate is obtained in which the grooved disk member 183, the metal bonding material, the MMC disk member 181, the metal bonding material, and the ceramic sintered body 120 are laminated in this order from the bottom. The laminate is heated and pressurized (TCB) to obtain the bonded body 110 (FIG. 4F). The bonded body 110 is formed by bonding a ceramic sintered body 120 to the upper surface of an MMC / ceramic block 130, which is the base of the cooling base material 30, via a metal bonding layer 140. The MMC / ceramic block 130 is formed by bonding an MMC disk member 181 and a grooved disk member 183 via a metal ceiling bonding layer 182. The MMC / ceramic block 130 has a refrigerant flow path 38 inside.
[0033] For example, TCB is performed as follows. That is, the laminate is pressed and bonded at a temperature equal to or lower than the solidus temperature of the metal bonding material (for example, a temperature equal to or higher than the solidus temperature minus 20°C and equal to or lower than the solidus temperature), and then returned to room temperature. This causes the metal bonding material to become a metal bonding layer. As the metal bonding material, an Al-Mg based bonding material or an Al-Si-Mg based bonding material can be used. For example, when TCB is performed using an Al-Si-Mg based bonding material, the laminate is pressed in a heated state under a vacuum atmosphere. It is preferable to use a metal bonding material with a thickness of about 100 μm.
[0034] Next, the outer periphery of the ceramic sintered body 120 is cut to form a step, thereby forming the ceramic base material 20 having the central portion 22 and the outer periphery portion 24. The outer periphery of the metal bonding layer 140 and the MMC / ceramic block 130 is cut as necessary to form the metal bonding layer 40 and the cooling base material 30. At this time, the outer periphery portion 34 of the cooling base material 30 is made to protrude from the outer periphery of the ceramic base material 20. An insulating tube 55 through which the power supply terminal 54 is inserted is disposed in the through holes 131, 132, the hole in the metal bonding layer 40, and the hole in the ceiling bonding layer 82. Furthermore, the insulating film 42 is formed by spraying the side surface of the outer periphery portion 24 of the ceramic base material 20, the periphery of the metal bonding layer 40, and the side surface of the cooling base material 30 with ceramic powder (FIG. 4G). In this way, the wafer mounting table 10 is obtained.
[0035] Next, an example of use of the wafer stage 10 will be described with reference to Fig. 1. As described above, the wafer stage 10 is fixed to the mounting plate 96 of the chamber 94 by the clamp members 70. A shower head 98 is disposed on the ceiling surface of the chamber 94, which ejects process gas into the chamber 94 from a number of gas injection holes.
[0036] A focus ring 78 is placed on the FR mounting surface 24a of the wafer mounting table 10, and a disk-shaped wafer W is placed on the wafer mounting surface 22a. The focus ring 78 has a step along the inner circumference of the upper end so as not to interfere with the wafer W. In this state, a DC voltage from the wafer suction DC power supply 52 is applied to the wafer suction electrode 26 to suction the wafer W onto the wafer mounting surface 22a. Then, the interior of the chamber 94 is set to a predetermined vacuum atmosphere (or reduced pressure atmosphere), and an RF voltage from the RF power supply 62 is applied to the ceiling base material 81 while supplying a process gas from the shower head 98. Then, plasma is generated between the wafer W and the shower head 98. Then, the plasma is used to perform CVD film formation or etching on the wafer W. The focus ring 78 is also worn out as the wafer W is plasma-processed, but since the focus ring 78 is thicker than the wafer W, the focus ring 78 is replaced after processing a plurality of wafers W.
[0037] In the wafer mounting table 10 of the first embodiment described above, MMC is used for the ceiling base material 81 of the cooling base material 30, while a ceramic material that is relatively inexpensive and can form the flow channel grooves 88 at a relatively low cost by near net shape technology or the like is used for the grooved base material 83. This reduces the manufacturing cost of the wafer mounting table. In addition, as the bonding layer between the ceramic base material 20 and the ceiling base material 81 and between the ceiling base material 81 and the grooved base material 83, a metal bonding layer with high thermal conductivity is used instead of a resin layer with low thermal conductivity. This provides high heat extraction capability. Furthermore, since the main component of the ceramic material constituting the grooved base material 83 is the same as the main component of the ceramic material constituting the ceramic base material 20, the grooved base material 83 has a small absolute value of the difference in linear thermal expansion coefficient between the ceramic base material 20 and the ceramic base material 20. Therefore, the ceramic base material 20, the ceiling base material 81, and the grooved base material 83 have a small absolute value of the difference in linear thermal expansion coefficient between them, and even if the stress relaxation property of the bonding layer is low, problems are unlikely to occur.
[0038] Furthermore, the ceiling base material 81, which is arranged in a portion of the cooling base material 30 where thermal stress is likely to occur when processing the wafer W with high-power plasma (the portion above the refrigerant flow path 38), is made of MMC, which has higher toughness than ceramic materials. Therefore, even if thermal stress occurs, the wafer mounting table 10 is less likely to break.
[0039] Furthermore, since MMC is conductive, the ceiling base material 81 can be used as an RF electrode, eliminating the need to prepare a separate RF electrode. Also, since the metal bonding layer 40 and the ceiling bonding layer 82 are made of metal, they can also be used as RF electrodes.
[0040] In this wafer mounting table 10, the ceramic material constituting the ceramic substrate 20, the MMC constituting the ceiling substrate 81, and the ceramic material constituting the grooved substrate 83 all have absolute values of linear thermal expansion coefficient differences of 1.5×10 -6 If the stress relaxation property of the bonding layer is low, problems are less likely to occur if the stress relaxation property of the bonding layer is low.
[0041] Furthermore, if the absolute value of the difference in linear thermal expansion coefficient between the ceramic material constituting the ceramic substrate 20 and the ceramic material constituting the grooved substrate 83 is small, the influence of the difference in linear thermal expansion coefficient between the ceramic substrate 20 and the ceiling substrate 81 and the influence of the difference in linear thermal expansion coefficient between the ceiling substrate 81 and the grooved substrate 83 are canceled, thereby suppressing warping and damage to the wafer mounting table 10. This increases the degree of freedom in the material constituting the ceiling substrate 81.
[0042] [Second embodiment] A wafer mounting table 210 according to a second embodiment of the present invention will be described below with reference to the drawings. Fig. 5 is a vertical cross-sectional view of the wafer mounting table 210. In Fig. 5, the same components as those in the first embodiment described above are denoted by the same reference numerals.
[0043] The wafer mounting table 210 is used in the same manner as the wafer mounting table 10. The wafer mounting table 210 includes a ceramic base 20, a cooling base 230, and a metal bonding layer 40.
[0044] The cooling substrate 230 is a disk member having a larger diameter than the ceramic substrate 20. The cooling substrate 230 includes a ceiling substrate 81, a perforated substrate 283, a bottom substrate 285, a ceiling bonding layer 82, and a bottom bonding layer 284. The cooling substrate 230 includes a refrigerant flow path 38 through which a refrigerant can circulate inside. An inlet 38a and an outlet 38b of the refrigerant flow path 38 penetrate the bottom substrate 285 in the vertical direction and open to the bottom surface of the refrigerant flow path 38.
[0045] The perforated substrate 283 is a disk member made of a ceramic material. The perforated substrate 283 has passage holes 288 extending in the vertical direction and constituting the side walls of the refrigerant passages 38. The details of the ceramic material used for the perforated substrate 283 are similar to those of the ceramic material used for the grooved substrate 83. The perforated substrate 283 may be manufactured using a near net shape technique.
[0046] The bottom substrate 285 is a disk member made of MMC. The bottom substrate 285 constitutes the bottom of the refrigerant flow path 38. The details of the MMC used for the bottom substrate 285 are the same as those of the MMC used for the ceiling substrate 81. The MMC used for the bottom substrate 285 preferably has the same main component as that of the MMC used for the ceiling substrate 81, but the main component may be different. The MMC used for the bottom substrate 285 may be made of the same material as that of the MMC used for the ceiling substrate 81. The MMC used for the bottom substrate 285 has an absolute difference in linear thermal expansion coefficient at 40 to 400°C from the ceramic material used for the ceramic substrate 20 of 1.5×10 -6 / K or less, and 1.0×10 -6 / K or less is more preferable, and 0.5×10 -6 It is more preferable that the value is equal to or less than 1 / K.
[0047] The bottom bonding layer 284 is a metal bonding layer that bonds the lower surface of the perforated substrate 283 and the upper surface of the bottom substrate 285. The bottom bonding layer 284 may be, for example, a layer formed of solder or a metal brazing material. The bottom bonding layer 284 is, for example, formed of TCB. The material of the bottom bonding layer 284 may be the same as the material of at least one of the metal bonding layer 40 and the ceiling bonding layer 82.
[0048] Such a wafer mounting stage 210 can be manufactured, for example, according to the manufacturing example of the wafer mounting stage 10 in FIG. 4, as shown below. The steps in FIG. 4A to FIG. 4C are the same as those in the manufacturing example of the wafer mounting stage 10. In the step in FIG. 4D, instead of manufacturing the MMC disk member 181 and the grooved disk member 183, a ceiling MMC disk member, a holed disk member made of a ceramic material, and a bottom MMC disk member are manufactured. The two MMC disk members are manufactured according to the MMC disk member 181, and the holed disk member is manufactured according to the grooved disk member 183. Thereafter, through holes are formed in each of the two MMC disk members and the holed disk member according to the step in FIG. 4E. Next, a laminate is prepared by stacking the bottom MMC disk member, metal bonding material, holed disk member, metal bonding material, ceiling MMC disk member, metal bonding material, and ceramic sintered body in this order from the bottom, according to the process of Fig. 4F, and the laminate is joined by TCB to prepare a joined body. Finally, cutting is performed according to the process of Fig. 4G, insulating tube 55 is placed, and insulating film 42 is formed. This results in wafer stage 210.
[0049] In the wafer placement table 210 of the second embodiment described above, MMC is used for the ceiling base material 81 of the cooling base material 230, while a ceramic material that is relatively inexpensive and can form the flow passage hole 288 at a relatively low cost by near net shape technology or the like is used for the perforated base material 283. This reduces the manufacturing cost of the wafer placement table. In addition, as the bonding layer between the ceramic base material 20 and the ceiling base material 81 and between the ceiling base material 81 and the perforated base material 283, a metal bonding layer with high thermal conductivity is used instead of a resin layer with low thermal conductivity. This provides high heat extraction capability. Furthermore, since the main component of the ceramic material constituting the perforated base material 283 is the same as the main component of the ceramic material constituting the ceramic base material 20, the perforated base material 283 has a small absolute value of the linear thermal expansion coefficient difference with the ceramic base material 20. Therefore, the ceramic base material 20, the ceiling base material 81, and the perforated base material 283 have a small absolute value of the linear thermal expansion coefficient difference between them, and even if the stress relaxation property of the bonding layer is low, problems are unlikely to occur.
[0050] Furthermore, the ceiling base material 81, which is arranged in a portion of the cooling base material 230 where thermal stress is likely to occur when the wafer W is processed with high-power plasma, is made of MMC, which has higher toughness than ceramic materials, so that the wafer mounting table 210 is less likely to break even if thermal stress occurs.
[0051] Furthermore, since MMC is conductive, the ceiling base material 81 can also be used as an RF electrode, and there is no need to prepare a separate RF electrode. Also, since the metal bonding layer 40, the ceiling bonding layer 82, and the bottom bonding layer 84 are made of metal, they can also be used as RF electrodes. Note that the bottom base material 285 made of MMC can also be used as an RF electrode.
[0052] Furthermore, since the bottom base material 285 is made of MMC and has a small absolute value of the difference in linear thermal expansion coefficient with the ceramic material constituting the ceramic base material 20, the influence of the difference in linear thermal expansion coefficient between the ceramic base material 20 and the ceiling base material 81 or the perforated base material 283, and the influence of the difference in linear thermal expansion coefficient between the ceiling base material 81 or the perforated base material 283 and the bottom base material 285 are canceled, thereby suppressing warping and damage of the wafer mounting table 210. This increases the degree of freedom in the materials constituting the ceiling base material 81 and the perforated base material 283.
[0053] Furthermore, since the perforated substrate 283 and the bottom substrate 285 are bonded with a metallic bottom bonding layer 284, bonding of the perforated substrate 283 and the bottom substrate 285 can be performed simultaneously with bonding of the ceramic substrate 20 and the ceiling substrate 81, and bonding of the ceiling substrate 81 and the perforated substrate 283, and the wafer mounting table 210 can be manufactured efficiently.
[0054] In addition, the bottom base material 285 may be bonded with a resin layer or the like since it has little effect on the heat extraction capacity. Therefore, the bottom base material 285 does not have to be made of MMC, and may be made of, for example, a high thermal expansion metal (for example, aluminum) having a relatively large linear thermal expansion coefficient, or may be made of ceramic or resin. In addition, the bottom bonding layer 284 does not have to be made of metal, and may be made of, for example, resin.
[0055] In this wafer mounting table 210, the ceramic material constituting the ceramic base 20, the MMC constituting the ceiling base 81, and the ceramic material constituting the perforated base 283 all have absolute values of linear thermal expansion coefficient differences of 1.5×10 -6 / K or less, even if the stress relaxation property of the bonding layer is low, problems are less likely to occur. Furthermore, the MMC constituting the base substrate 285 is such that the absolute values of the linear thermal expansion coefficient differences between each of these are all 1.5×10 -6 / K or less, problems are less likely to occur even if the stress relaxation property of the bonding layer is low.
[0056] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention.
[0057] For example, the wafer mounting table 10 of the first embodiment may have holes penetrating the wafer mounting table 10 from the lower surface of the cooling substrate 30 to the wafer mounting surface 22a. Examples of such holes include gas supply holes for supplying a thermally conductive gas (e.g., He gas) to the rear surface of the wafer W, and lift pin holes for inserting lift pins for moving the wafer W up and down relative to the wafer mounting surface 22a. The thermally conductive gas is supplied to a space formed by the wafer W and a large number of small protrusions (not shown) provided on the wafer mounting surface 22a. When the wafer W is supported by three lift pins, for example, the lift pin holes are provided in three places. The wafer mounting table 210 of the second embodiment may also have gas supply holes, lift pin holes, and the like.
[0058] In the wafer mounting table 10 of the first embodiment described above, the cooling substrate 30 is a circular plate member without a step, but as shown in Fig. 6, the upper surface of the outer circumferential portion 34 may be one step lower than the upper surface of the inner circumferential portion 32 to form a circular plate member with a step. In Fig. 6, a step is provided on the outer periphery of the grooved substrate 83, but the position of the step is not particularly limited, and a step may be provided on the outer periphery of the ceiling substrate 81. The same is true for the wafer mounting table 210 of the second embodiment, and a step may be provided on the outer periphery of one or more of the ceiling substrate 81, the perforated substrate 283, and the bottom substrate 285.
[0059] In the wafer mounting table 10 of the first embodiment described above, the ceiling base material 81 is made of MMC, but it may be made of a low thermal expansion metal material. In this case, the low thermal expansion metal material is preferably one that has high toughness and electrical conductivity, similar to MMC. In addition, the absolute value of the difference in linear thermal expansion coefficient between the low thermal expansion metal material and the ceramic material used for the ceramic base 20 at 40 to 400°C is 1.5×10 -6 / K or less. Examples of low thermal expansion metal materials include molybdenum and tungsten. For example, when the ceramic substrate 20 is an aluminum nitride substrate, the ceiling substrate made of a low thermal expansion metal material may be a molybdenum substrate. The linear thermal expansion coefficient of aluminum nitride at 40 to 400°C is 4.6×10 -6 / K, and molybdenum is 5.6×10 -6 / K. The same is true for the wafer mounting table 210 of the second embodiment, and the ceiling base material 81 may be made of a low thermal expansion metal material. In that case, the bottom base material 285 may also be made of a low thermal expansion metal material. In the wafer mounting table 210 of the second embodiment, one of the ceiling base material 81 and the bottom base material 285 may be made of MMC, and the other may be made of a low thermal expansion metal material.
[0060] In the first and second embodiments described above, the wafer adsorption electrode 26 is built into the center portion 22 of the ceramic substrate 20. Instead of or in addition to this, an RF electrode for generating plasma may be built into the ceramic substrate 20. In this case, a high-frequency power source is connected to the RF electrode, not to the ceiling substrate 81. Also, a focus ring (FR) adsorption electrode may be built into the outer circumferential portion 24 of the ceramic substrate 20. In this case, a DC power source is connected to the FR adsorption electrode. Also, the ceramic substrate 20 may have a heater electrode (resistance heating element) built into it. In this case, a heater power source is connected to the heater electrode. In this way, the ceramic substrate 20 may have one layer of electrodes built into it, or two or more layers of electrodes built into it.
[0061] In the above-mentioned first and second embodiments, the refrigerant flow path 38 is provided in a spiral shape from the inlet 38a to the outlet 38b, but the planar shape of the refrigerant flow path 38 is not particularly limited. Furthermore, a plurality of refrigerant flow paths 38 may be provided. Furthermore, the cross section of the refrigerant flow path 38 is rectangular, but the cross-sectional shape of the refrigerant flow path 38 is not particularly limited. For example, the upper corner of the cross section of the refrigerant flow path 38 may be a rounded surface. In this way, it is possible to prevent cracks from occurring starting from the upper corner of the cross section of the refrigerant flow path. In this case, the rounded surface may be provided on the ceiling base material 81.
[0062] In the first embodiment described above, the ceramic sintered body 120 in Fig. 4A was produced by hot-pressing and sintering a ceramic powder compact, but the compact may be produced by stacking a plurality of tape compacts, by a mold casting method, or by compressing ceramic powder. The same applies to the second embodiment.
[0063] In the above-described first embodiment, the grooved disk member 183 having the flow passage groove 88 formed therein is manufactured, and then the through holes 132, 66, the inlet 38a, and the outlet 38b are formed, but the grooved disk member 183 having the through holes 132, 66, the inlet 38a, and the outlet 38b may be manufactured using a near net shape technique. The same applies to the second embodiment. [Explanation of symbols]
[0064] 10 wafer mounting table, 20 ceramic substrate, 22 center, 22a wafer mounting surface, 24 outer periphery, 24a focus ring mounting surface, 26 wafer suction electrode, 27 hole, 30 cooling substrate, 32 inner periphery, 34 outer periphery, 38 coolant flow path, 38a inlet, 38b outlet, 40 metal bonding layer, 42 insulating film, 52 wafer suction DC power source, 53 low pass filter, 54 power supply terminal, 55 insulating tube, 62 RF power source, 63 high pass filter, 64 power supply terminal, 66 through hole, 70 clamp member, 70a inner peripheral step surface, 72 bolt, 78 focus ring, 81 ceiling substrate, 82 ceiling bonding layer, 83 grooved substrate, 88 flow path groove, 94 chamber, 96 installation plate, 98 shower head, 110 bonded body, 120 Ceramic sintered body, 130 MMC / ceramic block, 131, 132 through hole, 140 metal bonding layer, 181 MMC disk member, 182 ceiling bonding layer, 183 grooved disk member, 210 wafer mounting base, 230 cooling substrate, 283 perforated substrate, 284 bottom bonding layer, 285 bottom substrate, 288 flow path hole.
Claims
1. a ceramic substrate having a wafer mounting surface on an upper surface thereof and incorporating an electrode; A cooling substrate having a refrigerant flow path formed therein; a metal bonding layer bonding the lower surface of the ceramic substrate and the upper surface of the cooling substrate; Equipped with The cooling substrate includes a ceiling substrate made of a metal matrix composite material or a low thermal expansion metal material that constitutes the ceiling of the refrigerant flow path, a grooved substrate made of a ceramic material having the same main component as the ceramic substrate and having a flow groove on its upper surface that constitutes the bottom and side walls of the refrigerant flow path, and a metal ceiling joining layer that joins the lower surface of the ceiling substrate and the upper surface of the grooved substrate. Wafer placement stage.
2. The metal matrix composite material or low thermal expansion metal material constituting the ceiling base material and the ceramic material constituting the grooved base material have an absolute value of linear thermal expansion coefficient difference of 1.5×10 at 40 to 400° C. with the ceramic material constituting the ceramic base material. -6 / K or less, The wafer stage according to claim 1 .
3. 3. The wafer mounting table according to claim 1, wherein the ceramic material constituting the ceramic base is alumina, and the ceramic material constituting the grooved base is alumina having a purity lower than that of the alumina constituting the ceramic base.
4. a ceramic substrate having a wafer mounting surface on an upper surface thereof and incorporating an electrode; A cooling substrate having a refrigerant flow path formed therein; a metal bonding layer bonding the lower surface of the ceramic substrate and the upper surface of the cooling substrate; Equipped with The cooling substrate includes a ceiling substrate made of a metal matrix composite material or a low thermal expansion metal material that constitutes the ceiling of the refrigerant flow path, a perforated substrate made of a ceramic material having the same main component as the ceramic substrate and having a flow path hole that constitutes the side wall of the refrigerant flow path penetrating in the vertical direction, a bottom substrate that constitutes the bottom of the refrigerant flow path, a metal ceiling bonding layer that bonds the lower surface of the ceiling substrate and the upper surface of the perforated substrate, and a bottom bonding layer that bonds the lower surface of the perforated substrate and the upper surface of the bottom substrate. Wafer placement stage.
5. 5. The wafer support of claim 4, wherein the bottom substrate is made of a metal matrix composite material or a low thermal expansion metal material, and the bottom bonding layer is made of metal.
6. The metal matrix composite material or low thermal expansion metal material constituting the ceiling base material and the ceramic material constituting the perforated base material have an absolute value of 1.5×10 linear thermal expansion coefficient difference at 40 to 400° C. with the ceramic material constituting the ceramic base material. -6 / K or less, The wafer stage according to claim 4 or 5.
7. The wafer support according to any one of claims 4 to 6, wherein the ceramic material constituting the ceramic substrate is alumina, and the ceramic material constituting the perforated substrate is alumina having a lower purity than the alumina constituting the ceramic substrate.
Citation Information
Patent Citations
Measuring method of biological activity and its device
JP1981066748A
Measuring method of activity of animal*botanical tissue
JP1981066749A
Bonding structure of electrostatic chuck
JP1992287344A
Electrostatic chuck device
JP2012142413A
Holding device
JP2017126641A
Cited By
Holding device
JP7818732B1