Visible light responsive photocatalyst and its manufacturing method

A solid-phase reaction using AgCl and P2O5 produces silver phosphate photocatalysts efficiently and safely, addressing inefficiencies in existing photocatalysts by enhancing visible light utilization and pollutant degradation.

JP7584139B2Active Publication Date: 2024-11-15RYUKOKU UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021041576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-11-15
Estimated Expiration
2041-03-15

Smart Images

  • Figure 0007584139000001
    Figure 0007584139000001
  • Figure 0007584139000002
    Figure 0007584139000002
  • Figure 0007584139000003
    Figure 0007584139000003
Patent Text Reader

Abstract

To provide a production method that can safely and efficiently prepare silver phosphate Ag3 PO4 with high photocatalyst effect in visible light without using a powerful drug or other drugs that are difficult to store and handle.SOLUTION: This invention relates to a method for producing a visible light-responsive photocatalyst Ag3PO4, including the steps of mixing AgCl with P2O5 and subjecting the mixture to a solid phase reaction. This invention also relates to a visible light-responsive photocatalyst comprising silver phosphate represented by Ag3PO4, and AgCl.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a visible light responsive photocatalyst and a method for producing the same, and more particularly to a photocatalyst containing silver phosphate represented by Ag3PO4. [Background technology]

[0002] Photocatalysts absorb light energy and convert it into electrons (e - ) and holes (h + ) pair, but this hole (h + ) converts the moisture on the catalyst surface into hydroxyl radicals, which have strong oxidizing power, and these hydroxyl radicals decompose organic matter such as pollutants, dirt, and bacteria, thereby exerting their function. The effect is proportional to the amount of light energy absorbed and is related to the band gap energy of the photocatalyst. The lower the band gap energy Eg, the greater the light energy that can be absorbed, and is related to the maximum absorbable wavelength λ by the following formula. Eg = Planck constant × speed of light / λ = 1240 / λ

[0003] Titanium oxide TiO2, which is widely used as a photocatalyst, has a band gap energy of 3.2 eV and can utilize ultraviolet light with a wavelength of 388 nm or less, but can utilize only a little less than 3% of the total solar energy. Patent Document 1 discloses an efficient method for producing monoclinic bismuth vanadate BiVO4, which has an even lower band gap energy, and has a band gap energy of 2.4 eV and can utilize the energy of visible light and ultraviolet light with a wavelength of 517 nm or less, but can utilize only a little less than 19% of the total solar energy. On the other hand, Patent Documents 2 and 3 disclose silver phosphate Ag3PO4, which has a band gap energy of 2.2 eV lower than monoclinic bismuth vanadate, and can utilize the energy of visible light and ultraviolet light with a wavelength of 554 nm or less, and can utilize 24% of the total solar energy.

[0004] In the methods disclosed in Patent Documents 2 and 3, AgNO3, designated as a toxic substance under the Poisonous and Deleterious Substances Control Law, and H3PO4, which is highly acidic and has serious effects on the human body, are used as materials. In addition, in the manufacturing method using a solvent, in addition to the cost of the solvent, there is a problem of waste liquid treatment. Furthermore, although a solid-phase reaction method in which materials are mixed and fired to synthesize is also possible, the conditions for efficiently manufacturing Ag3PO4 are not shown. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-111476 A [Patent Document 2] Japanese Patent Application Publication No. 10-33990 [Patent Document 3] JP 2009-78211 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a method for safely and efficiently producing silver phosphate Ag3PO4, which has a high photocatalytic effect under visible light, without using any poisonous substances or chemicals that are difficult to store and handle. [Means for solving the problem]

[0007] The inventors conducted various investigations into the raw materials for silver phosphate Ag3PO4 and discovered that Ag3PO4 can be produced safely and efficiently by carrying out a solid-state reaction using AgCl and P2O5 as raw materials, thus completing the present invention.

[0008] That is, the present invention relates to a method for producing a visible light responsive photocatalyst Ag3PO4, which includes a step of mixing AgCl and P2O5, and a step of subjecting the mixture to a solid-state reaction.

[0009] The molar ratio of AgCl to P2O5 is preferably 2:1 to 10:1.

[0010] The temperature of the solid-state reaction is preferably 500° C. or higher.

[0011] The rate of temperature rise up to the solid-phase reaction temperature is preferably 13 to 40° C. / min.

[0012] The rate of temperature rise up to the solid-phase reaction temperature is preferably 16 to 27° C. / min.

[0013] The present invention also relates to a visible light responsive photocatalyst containing silver phosphate represented by Ag3PO4 and AgCl.

[0014] It is preferred that Ag3PO4 is present on the surface. Effect of the Invention

[0015] According to the manufacturing method of the visible light responsive photocatalyst of the present invention, since AgCl and P2O5 are used as raw materials, it is possible to safely and efficiently produce silver phosphate Ag3PO4, which has a high photocatalytic effect under visible light, without using toxic substances or chemicals that are difficult to store and handle. [Brief description of the drawings]

[0016] [Figure 1] 1 shows XRD charts of the visible light responsive photocatalysts prepared in Examples 1 to 9. [Diagram 2] FIG. 2 is a plot of transmittance versus wavelength for methylene blue solutions treated with the visible light responsive photocatalysts prepared in Examples 1 to 9. [Diagram 3] FIG. 1 is a plot of transmittance versus wavelength for a methylene blue solution treated with Ag3PO4 produced by solid-state reaction at 1100° C. for 3 hours (Example 9) or bismuth vanadate (Comparative Example). [Figure 4] 1 is an SEM photograph of a cross section of the visible light responsive photocatalyst prepared in Example 6. The bright areas indicate areas where AgCl is present, and the dark areas indicate areas where Ag3PO4 is present. [Diagram 5]Energy dispersive X-ray spectroscopy of the cross section of Figure 4. The bright areas indicate areas where Ag is present. [Figure 6] Energy dispersive X-ray spectroscopy of the cross section of Figure 4. The light areas indicate areas with Cl. The dark areas indicate the presence of AgCl. [Figure 7] Energy dispersive X-ray spectroscopy of the cross section of Figure 4. The light areas indicate areas with P. The dark areas indicate the presence of Ag3PO4. [Figure 8] Energy dispersive X-ray spectroscopy of the cross section of Figure 4. The light areas indicate the areas with O. The dark areas indicate the presence of Ag3PO4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The method for producing the visible light responsive photocatalyst Ag3PO4 of the present invention is characterized by including a step of mixing AgCl and P2O5, and a step of subjecting the mixture to a solid-state reaction. The solid-state reaction is theoretically represented by the following chemical formula: 12AgCl+2P2O5+3O2(Air)→4Ag3PO4+6Cl2(↑)

[0018] The method of mixing AgCl and P2O5 is not particularly limited, and examples include a mortar, a grinder, a bead mill, etc. The mixing molar ratio of AgCl and P2O5 is preferably 2:1 to 10:1, and more preferably 5:1 to 7:1. If the amount of AgCl is less than 2:1, the two materials may not mix, and if it exceeds 10:1, there is a tendency for a large amount of AgCl, especially as a single substance, to exist, which reduces the photocatalytic effect.

[0019] The temperature of the solid-phase reaction of the mixture is preferably 500° C. or higher, more preferably 800° C. or higher. If the temperature is lower than 500° C., the materials tend to be below their melting points and not be able to be mixed well. There is no upper limit, but a temperature of 1100° C. or lower is preferred.

[0020] The time for the solid-phase reaction of the mixture depends on the temperature, but is preferably 0.5 to 8.0 hours, more preferably 1 to 3 hours. If it is less than 0.3 hours, the two materials will not be mixed sufficiently, and if it exceeds 20 hours, the materials will tend to volatilize gradually.

[0021] The rate of temperature rise up to the temperature of the solid-phase reaction is not particularly limited, but is preferably 13 to 40°C / min, and more preferably 16 to 27°C / min. The melting point of AgCl is 455°C, the boiling point is 1547°C, and the melting point of P2O5 is 340°C, the boiling point is 360°C, and therefore P2O5 with a low boiling point is easily volatilized. If the rate of temperature rise is too fast, the time required to reach the temperature of the solid-phase reaction that reacts AgCl and P2O5 is short, and the volatilization of P2O5 occurs, which tends to reduce the yield of Ag3PO4.

[0022] The visible light responsive photocatalyst of the present invention is characterized by containing silver phosphate represented by Ag3PO4 and AgCl. It is desirable that a part of Ag3PO4 is present on the surface of the sample (in contact with the air).

[0023] The content of AgCl is not particularly limited, but is preferably 10 to 90 mass%, more preferably 30 to 80 mass%. If it is less than 10 mass%, the amount of AgCl supplied is small, so that the amount of Ag3PO4 produced is small. On the other hand, if it exceeds 90 mass%, there is an excess of AgCl (very little P2O5), and it tends not to be possible to produce a satisfactory photocatalyst material.

[0024] The visible light responsive photocatalyst of the present invention can be applied to systems to be purified by utilizing visible light, and is particularly suitable for photodecomposing endocrine disruptors such as nonylphenol, bisphenol A, and natural estrogens present in water systems to be purified. EXAMPLES

[0025] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0026] Example 1 AgCl and P2O5 were mixed in a mortar at room temperature in a molar ratio of 6:1. The resulting mixture was subjected to solid-phase reaction firing at 300 °C for 3 hours to obtain a powdery visible light-responsive photocatalyst.

[0027] Examples 2 to 9 In Example 1, except that the firing temperature was changed to 400 °C (Example 2), 500 °C (Example 3), 600 °C (Example 4), 700 °C (Example 5), 800 °C (Example 6), 900 °C (Example 7), 1000 °C (Example 8), 1100 °C (Example 9), the same procedure as in Example 1 was carried out to obtain a powdery visible light-responsive photocatalyst for each example.

[0028] Comparative Example Bismuth oxide (Bi2O3) and ammonium metavanadate (NH4VO3) were weighed in a molar ratio of 1:3. They were placed in a crucible and fired at 700 °C for 3 hours to prepare bismuth vanadate.

[0029] <X-ray Diffraction> Using the visible light-responsive photocatalyst prepared in the examples, X-ray diffraction was measured with an XRD measuring device (RINT2500V manufactured by Rigaku Corporation). Figure 1 shows the X-ray diffraction chart. Since diffraction peaks exist near 33.02°, 54.7°, 57.56°, and 85.54°, it can be seen that Ag3PO4 is formed. Also, since many diffraction peaks derived from AgCl exist, it can be seen that AgCl is present in the photocatalyst prepared in the examples. The content of AgCl in the visible light-responsive photocatalyst prepared in Example 6 was about 50% by mass.

[0030] <Photocatalytic Effect> The visible light responsive photocatalyst prepared in the examples and an aqueous solution containing 3000 μL (0.1 mM) of methylene blue were placed in a plastic container, and while stirring, the solution was irradiated with visible light (wavelength 100 to 1400 nm) for 60 minutes using a solar simulator device (XES-301S+EL-100, manufactured by Minaga Electric Manufacturing Co., Ltd.). After irradiation, the solution was centrifuged at a rotation speed of 13000 rpm and an operating time of 30 minutes. 300 μL of the resulting solution was placed in a quartz cell, and the transmittance was measured using a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd.). Figure 2 shows a plot of the transmittance as a function of wavelength. The disappearance of the absorption of methylene blue indicates that the photocatalytic action is exerted. It can be seen that the catalyst that underwent a solid-phase reaction at a temperature of 600°C or higher has a high photocatalytic effect.

[0031] The photocatalytic effect of Ag3PO4 produced by the solid-phase reaction method at a firing temperature of 500°C or less was low. The reason for this is that the melting point of AgCl is 450°C, and when AgCl exceeds 450°C, it becomes liquid and reacts with P2O5 to produce Ag3PO4. If the firing temperature is lower than 500°C, AgCl does not become liquid and does not react sufficiently, and Ag3PO4 cannot be produced efficiently. On the other hand, since the melting point and boiling point of P2O5 are 340°C and 360°C, respectively, firing for a long time (for example, about 4 hours) at a temperature between 340°C and 500°C is effective for mixing very well.

[0032] Figure 3 shows a plot of transmittance versus wavelength for Ag3PO4 prepared by solid-state reaction at 1100°C for 3 hours (Example 9) or methylene blue solution treated with bismuth vanadate. It was confirmed that Ag3PO4, which has a low band gap energy, exhibits a higher photocatalytic effect than bismuth vanadate.

[0033] FIG. 4 shows an SEM photograph of the cross section of the visible light responsive photocatalyst produced in Example 6. The bright areas show the areas where AgCl is present, and the dark areas show the areas where Ag3PO4 is present. FIGS. 5 to 8 show the diagrams obtained by energy dispersive X-ray spectroscopy of the visible light responsive photocatalyst produced in Example 6. The bright areas in FIG. 5 (almost all of the diagram) show the presence of Ag, and the brighter areas in FIG. 6 show the presence of a large amount of Cl, which indicates that AgCl with a high boiling point (sublimation point) of 1547°C remains. The brighter areas in FIG. 7 show the presence of a large amount of P, and the bright areas in FIG. 8 show the presence of a large amount of O, and the two almost overlap, indicating the presence of a large amount of Ag3PO4. It can be seen that Ag3PO4 is present at least on the surface of the sample. [Industrial Applicability]

[0034] According to the present invention, a visible light responsive Ag3PO4 fine powder photocatalyst can be safely and efficiently produced. The obtained photocatalyst can photodecompose endocrine disruptors such as nonylphenol, bisphenol A, and natural estrogens present in the system to be purified, especially the water system, by using visible light, and can contribute to purifying environmental pollutants that are a major problem in today's society.

Claims

1. AgCl and P 2 O 5 and A step of subjecting the mixture to a solid-state reaction. A visible light responsive photocatalyst AgCl having 3 P.O. 4 Manufacturing method.

2. AgCl and P 2 O 5 The visible light responsive photocatalyst Ag according to claim 1, wherein the molar ratio of 3 P.O. 4 Manufacturing method.

3. A process for producing a sintered body comprising the steps of: mixing AgCl and P2O5; and A step of subjecting the mixture to a solid-state reaction. A method for producing a visible light responsive photocatalyst Ag 3 PO 4 having the following structure: Visible light responsive photocatalyst Ag with solid-phase reaction temperature of 500°C or higher 3 P.O. 4 Manufacturing method.

4. The visible light responsive photocatalyst Ag according to any one of claims 1 to 3, wherein the heating rate up to the temperature of the solid-phase reaction is 13 to 40°C / min. 3 P.O. 4 Manufacturing method.

5. The visible light responsive photocatalyst Ag according to claim 4, wherein the heating rate up to the temperature of the solid-phase reaction is 16 to 27° C. / min. 3 P.O. 4 Manufacturing method.

Citation Information

Patent Citations

  • Silver chloride-silver phosphate composite photocatalyst and preparation method thereof

    CN102247874A

  • Loaded type silver phosphate / polyphosphoric silver / silver chloride compound water treatment photo-catalyst and preparation method thereof

    CN102600870A

  • Silver halide / silver phosphate heterojunction membrane visible photo-catalysis material and preparation method thereof

    CN102698780A

  • Method for preparing silver phosphate nanometer material by solid phase chemical reaction

    CN103466584A

  • Preparation method of copper silver phosphate with photodegradation function and photocatalytic application

    CN104607217A