Semiconductor manufacturing equipment component and semiconductor manufacturing equipment using the same

Ceramics with yttrium zirconate and trace metals like manganese enhance plasma resistance and mechanical strength, addressing corrosion and peeling issues in semiconductor equipment, ensuring longevity and cleanliness.

JP7584248B2Active Publication Date: 2024-11-15KYOCERA CORP
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
JP2020126094
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-07-27
Publication Date
2024-11-15
Estimated Expiration
2040-07-27

AI Technical Summary

Technical Problem

Conventional semiconductor manufacturing equipment members face issues with corrosion resistance and mechanical integrity due to exposure to corrosive gases and plasma, leading to peeling and contamination from temperature fluctuations.

Method used

The use of ceramics with yttrium zirconate as a main component, combined with specific amounts of manganese, iron, cerium, or vanadium, enhances plasma resistance, mechanical strength, and thermal emissivity, reducing peeling and contamination.

Benefits of technology

The ceramic members maintain high plasma resistance, mechanical strength, and thermal emissivity, preventing peeling and color unevenness, thus extending product lifespan and reducing contamination in semiconductor manufacturing environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584248000002
    Figure 0007584248000002
  • Figure 0007584248000001
    Figure 0007584248000001
Patent Text Reader

Abstract

To provide a member for a semiconductor manufacturing device that includes ceramics having excellent plasma resistance and mechanical strength and has high thermal emissivity.SOLUTION: A member for a semiconductor manufacturing device includes ceramics that contains yttrium zirconate or a yttrium-aluminum complex oxide as a main component, includes at least one metal element selected from the group consisting of manganese, iron, cerium, and vanadium, and contains the metal element in a ratio of 40 mass ppm or more and 110 mass ppm or less in total.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a member for a semiconductor manufacturing apparatus and a semiconductor manufacturing apparatus using the same. [Background technology]

[0002] Conventionally, in the manufacture of semiconductors, liquid crystals, etc., plasma is used to treat objects in processes such as etching and film formation. In such processes, corrosive gases containing highly reactive halogen elements (e.g., fluorine, chlorine, etc.) are used. Therefore, high corrosion resistance is required for members that are used in manufacturing equipment for semiconductors, liquid crystals, etc. and that come into contact with corrosive gases and plasma. As such members, for example, Patent Document 1 describes a non-stoichiometric oxide composition that contains a substrate and at least one of yttrium oxide, hafnium oxide, zirconium oxide completely stabilized with yttria, and mixtures thereof on the surface of the substrate, and has a predetermined thermal emissivity, etc. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6312278 Summary of the Invention

[0004] The semiconductor manufacturing equipment member according to the present disclosure includes a ceramic having yttrium zirconate or yttrium aluminum composite oxide as a main component, containing at least one metal element selected from the group consisting of manganese, iron, cerium, and vanadium, with the metal elements contained in a total proportion of 40 ppm by mass or more and 110 ppm by mass or less.

[0005] Another semiconductor manufacturing equipment member according to the present disclosure includes a ceramic having a main crystal phase consisting of an yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide and a zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide, and containing at least one metal element selected from the group consisting of manganese, iron, cerium and vanadium, with the metal elements being contained in a total proportion of 40 ppm by mass or more and 110 ppm by mass or less.

[0006] Furthermore, a semiconductor manufacturing apparatus according to the present disclosure includes the above-mentioned semiconductor manufacturing apparatus member. [Brief description of the drawings]

[0007] [Figure 1] 1 is a graph showing an example of the total reflectance of a surface of a ceramic material included in a semiconductor manufacturing equipment member according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In a semiconductor manufacturing device, there is a space, such as a semiconductor chamber, that is exposed to repeated temperature increases and decreases. If a member, for example, whose base material is made of a metal such as aluminum and whose surface is covered with a topcoat layer, is used in such an atmosphere exposed to repeated temperature increases and decreases, there is a problem that peeling occurs due to the difference in linear expansion coefficient between the aluminum and the topcoat layer.

[0009] The semiconductor manufacturing equipment member according to the present disclosure includes a ceramic containing yttrium zirconate as a main component and manganese at a ratio of 40 mass ppm to 110 mass ppm. By using yttrium zirconate as a main component, the ceramic obtained has excellent plasma resistance and mechanical strength. Furthermore, by adding manganese at a ratio of 40 mass ppm to 110 mass ppm, the color tone of the ceramic can be developed into a dark color. As a result, the thermal emissivity of the ceramic obtained can be increased.

[0010] Therefore, the semiconductor manufacturing equipment member according to the present disclosure, which contains such ceramics, does not peel off even when exposed to temperature rises and falls, and has high thermal emissivity in addition to excellent plasma resistance and mechanical strength. Furthermore, since the ceramics of the semiconductor manufacturing equipment member according to the present disclosure have a dark color, color unevenness is unlikely to occur even when exposed to plasma, and the product value can be maintained for a long period of time.

[0011] A semiconductor manufacturing equipment member according to an embodiment of the present disclosure includes a ceramic containing yttrium zirconate as a main component and at least one metal element selected from the group consisting of manganese, iron, cerium, and vanadium, the metal element being contained in a total amount of 40 mass ppm to 110 mass ppm. In this specification, "containing yttrium zirconate as a main component" means that the ceramic contains at least 50 mass% of yttrium zirconate. In particular, the content of yttrium zirconate in a total of 100 mass% of the components constituting the ceramic is preferably 60 mass% or more. In this specification, "ceramic" refers to both polycrystalline and single crystalline bodies.

[0012] Ceramics containing yttrium zirconate as a main component can be obtained, for example, by firing a mixture of yttrium oxide and zirconium oxide. The mixing ratio of yttrium oxide and zirconium oxide is not limited. For example, yttrium oxide contributes to improving plasma resistance, and zirconium oxide contributes to improving mechanical strength. Therefore, when the ratio of yttrium oxide is increased, ceramics having better plasma resistance than mechanical strength can be obtained, and when the ratio of zirconium oxide is increased, ceramics having better mechanical strength than plasma resistance can be obtained.

[0013] In a semiconductor manufacturing equipment member according to an embodiment of the present disclosure, the ceramics mainly composed of yttrium zirconate contains at least one metal element selected from the group consisting of manganese, iron, cerium, and vanadium, and contains the metal element (hereinafter, these metal elements may be referred to as "coloring components") in a total ratio of 40 mass ppm to 110 mass ppm. By containing the coloring components in a total ratio of 40 mass ppm to 110 mass ppm, the ceramics mainly composed of yttrium zirconate can be imparted with a high thermal emissivity.

[0014] Each component of ceramics is identified by the JCPDS card based on the results of measurement using an X-ray diffraction device with CuKα radiation. Yttrium zirconate is, for example, YZrO3, Zr3Y4O 12 YAG, a type of yttrium aluminum oxide, is represented by the formula: Al5Y3O 12 YAM is expressed as Al2Y4O9, and YAP is expressed as AlYO3. Next, the content of each element is determined using an X-ray fluorescence analyzer (XRF) or an inductively coupled plasma optical emission spectrometer (ICP) and converted into the compound identified by the X-ray diffraction device. Here, the content of the coloring component is very small, so it can be determined, for example, using a glow discharge mass spectrometer (GDMS).

[0015] If the total content of the coloring components is less than 40 ppm by mass, color unevenness is likely to occur, and the commercial value is likely to be impaired.On the other hand, if the total content of the coloring components exceeds 110 ppm by mass, when the ceramic surface is exposed to plasma, the particles that make up the coloring components may fall off and become particles that float in the processing chamber of the semiconductor manufacturing equipment and become a source of contamination.

[0016] The reason why the inclusion of a coloring component in a specific ratio can impart high thermal emissivity to ceramics mainly composed of yttrium zirconate is that when a coloring component is added in a specific ratio to the ceramic powder, which is the primary raw material of such ceramics, the color tone of the ceramics can be made dark. Normally, ceramics mainly composed of yttrium zirconate have a white color, but by adding a coloring component in a specific ratio, the color tone can be made to be brown to dark brown.

[0017] The ceramics mainly composed of yttrium zirconate forming the semiconductor manufacturing equipment member according to the embodiment can be obtained, for example, by the following procedure. First, a powder of a compound constituting a coloring component is added to a mixture of yttrium oxide and zirconium oxide in a specific ratio, and additives generally contained in ceramics are added as necessary. The raw material thus obtained is fired to obtain ceramics.

[0018] Specifically, first, a powder mainly composed of yttrium oxide, a powder mainly composed of zirconium oxide (hereinafter, a mixture of the powder mainly composed of yttrium oxide and the powder mainly composed of zirconium oxide may be referred to as "ceramic powder"), a powder of a compound to be a coloring component, pure water, and a dispersant are added, and then pulverized and mixed in a bead mill to obtain a slurry. The ceramic powder is a mixture of a powder mainly composed of yttrium oxide and a powder mainly composed of zirconium oxide, with the powder mainly composed of yttrium oxide being mixed in a mass ratio of, for example, 2.5 to 3.1 to 1 part of the powder mainly composed of zirconium oxide. With this mass ratio, a ceramic exhibiting a good balance between plasma resistance and mechanical strength can be obtained.

[0019] When the coloring component is manganese, the manganese source is not limited as long as it is a compound containing manganese, and examples thereof include powders of manganese carbonate (MnCO3), manganese oxide (MnO2), manganese nitrate Mn(NO3)2, manganese oxalate (MnC2O4), and mixtures thereof. The powder of the compound serving as the manganese source is added so that the ratio of manganese contained in the ceramic is 40 mass ppm or more and 110 mass ppm or less. For example, the amount of manganese carbonate (MnCO3) added may be 84 mass ppm or more and 230 mass ppm or less, based on 100 mass% of the total ceramic powder.

[0020] When the coloring component is iron, the iron source may be iron oxide (Fe2O3) FE-Cr, Fe-Cr-Zn, Fe-Cr-Si, Fe-Cr-Zn-Si or Fe-Cr-Ni-Si composite oxide or iron oxide (Fe2O3) powder.When the coloring component is cerium, the cerium source may be cerium oxide (CeO2) powder.

[0021] An organic binder is added to the obtained slurry and stirred, and then the slurry is spray-dried and de-ironized to obtain granules. The granules are filled into a mold and then pressurized into a cylindrical shape using a molding method such as uniaxial pressing or cold isostatic pressing (CIP) to obtain a green body. This green body is then machined to obtain a precursor. This precursor is then degreased and fired to obtain a sintered ceramic body.

[0022] The firing atmosphere is air, the firing temperature is 1640°C to 1880°C, the holding time is 1.5 hours to 5 hours, and natural cooling is performed during the temperature drop process. To obtain ceramics having a main crystal phase of an yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide and a zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide, for example, an annealing treatment is performed during the temperature drop process, and the treatment temperature is set to 1300°C to 1500°C and held for 3 hours to 5 hours.

[0023] The relative density of the ceramic is preferably 98% or more. If the relative density of the ceramic is in this range, the open pores on the surface exposed to the plasma are reduced, and even if exposed to the plasma, the generation of particles can be suppressed. The relative density of the ceramic is calculated as a percentage of the apparent density of the ceramic calculated in accordance with JIS R 1634:1998 to the theoretical density of the ceramic.

[0024] The ceramics containing yttrium zirconate as a main component forming the semiconductor manufacturing equipment member according to one embodiment has a dark color tone ranging from brown to dark brown as described above. The color tone is expressed, for example, by the L*a*b* color system. The lightness index L* is expressed as a value ranging from 0 to 100, and the larger the value, the brighter the color tone. The chromaticness index a* indicates a more reddish color tone as the value increases, and a more negative value indicates a more greenish color tone. The chromaticness index b* indicates a more yellowish color tone as the value increases, and a more negative value indicates a more blueish color tone.

[0025] The ceramics mainly composed of yttrium zirconate forming the semiconductor manufacturing equipment member according to the embodiment is colored in such a way that, for example, in the L*a*b* color system, the lightness index L* is 0 to 70, the chromaticness index a* is -10 to 10, and the chromaticness index b* is -15 to 15. When these values ​​are shown, the color tone is brown to dark brown. In addition, the total reflectance at a wavelength of 360 nm is preferably 16% or less, and the total reflectance at a wavelength of 740 nm is preferably 25% to 50%.

[0026] The semiconductor manufacturing equipment member according to the embodiment is not limited to any particular member used in the semiconductor manufacturing equipment. Examples of such members include nozzles, clamp rings, lids, liners, bell jars, susceptors, focus rings, shower plates, and ion implantation equipment members. Among these, members used in an atmosphere exposed to repeated temperature rises and falls, such as in a semiconductor chamber, are preferred.

[0027] The ceramic forming the semiconductor manufacturing equipment member according to another embodiment of the present disclosure has a main crystal phase of an yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide, and a zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide, and contains coloring components in a total amount of 40 ppm by mass or more and 110 ppm by mass or less.

[0028] Yttrium oxide, whose composition formula is Y2O3, and zirconium oxide, whose composition formula is ZrO2, have similar crystal structures, so even if an X-ray diffraction apparatus is used, the main diffraction peaks overlap, making it difficult to identify each other. Therefore, when an X-ray diffraction apparatus is used to confirm a peak shift to a higher angle side from the diffraction peak caused only by Y2O3, which appears at a diffraction angle 2θ of 20.5°, it can be considered that an yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide is present. On the other hand, a zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide can be confirmed using a scanning electron microscope (SEM) and an energy dispersive spectrometer (EDS).

[0029] The yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide, and the zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide can be obtained, for example, by the following procedure. First, the above-mentioned ceramic powder, powder of a compound that is a coloring component, pure water, and a dispersant are added, and then pulverized and mixed in a bead mill to obtain a slurry. The ceramic powder is a mixture of a powder mainly composed of yttrium oxide and a powder mainly composed of zirconium oxide, with the powder mainly composed of yttrium oxide being mixed in a mass ratio of, for example, 2.5 to 3.1 to the powder mainly composed of zirconium oxide. With this mass ratio, a ceramic exhibiting a good balance between plasma resistance and mechanical strength can be obtained.

[0030] When the coloring component is manganese, the manganese source is not limited as long as it is a compound containing manganese, and examples thereof include powders of manganese carbonate (MnCO3), manganese oxide (MnO2), manganese nitrate Mn(NO3)2, manganese oxalate (MnC2O4), and mixtures thereof. The powder of the compound serving as the manganese source is added so that the ratio of manganese contained in the ceramic is 40 mass ppm or more and 110 mass ppm or less. For example, the amount of manganese carbonate (MnCO3) added may be 84 mass ppm or more and 230 mass ppm or less, based on the total of 100 mass% of the ceramic powder, as an external addition. When the coloring component is iron or cerium, the above-mentioned powder may be added.

[0031] An organic binder is added to the obtained slurry and stirred, and then the slurry is spray-dried and de-ironized to obtain granules. The granules are filled into a mold and then pressurized into a cylindrical shape using a molding method such as uniaxial pressing or cold isostatic pressing (CIP) to obtain a green body. This green body is then machined to obtain a precursor. This precursor is then degreased and fired to obtain a sintered ceramic body.

[0032] The firing atmosphere is air, the firing temperature is 1640°C to 1880°C, the holding time is 1.5 hours to 5 hours, and natural cooling is performed during the temperature drop process. As described above, if an annealing treatment is performed during the temperature drop process, it is possible to obtain ceramics having a main crystal phase of an yttrium oxide solid solution in which zirconium oxide is dissolved in yttrium oxide, and a zirconium oxide solid solution in which yttrium oxide is dissolved in zirconium oxide.

[0033] The ceramics having yttrium oxide solid solution and zirconium oxide solid solution as main crystal phases forming the semiconductor manufacturing equipment member according to another embodiment also exhibits a dark color tone ranging from brown to dark brown. Specifically, as described above, in the L*a*b* color system, the lightness index L* is 0 to 70, the chromaticness index a* is -10 to 10, and b* is -15 to 15. The total reflectance at a wavelength of 360 nm is preferably 16% or less, and the total reflectance at a wavelength of 740 nm is preferably 25% to 50%.

[0034] The ceramics forming the semiconductor manufacturing equipment member according to another embodiment of the present disclosure mainly comprises yttrium aluminum composite oxide and at least one of manganese, iron, cerium, and vanadium metal elements, the metal elements being contained in a total amount of 40 mass ppm to 110 mass ppm. In this specification, "mainly comprises yttrium aluminum composite oxide" means that the ceramic contains at least 90 mass% of yttrium aluminum composite oxide. In particular, the content of yttrium aluminum composite oxide in the total of 100 mass% of the components constituting the ceramic is preferably 99 mass% or more.

[0035] Ceramics containing yttrium-aluminum composite oxide as a main component can be obtained, for example, by firing or melting a mixture of yttrium oxide and aluminum oxide. The mixing ratio of yttrium oxide and aluminum oxide is not limited. For example, yttrium oxide contributes to improving plasma resistance, and aluminum oxide contributes to improving mechanical strength. Therefore, when the ratio of yttrium oxide is increased, ceramics having better plasma resistance than mechanical strength can be obtained, and when the ratio of aluminum oxide is increased, ceramics having better mechanical strength than plasma resistance can be obtained.

[0036] In a semiconductor manufacturing equipment member according to an embodiment of the present disclosure, the ceramics mainly composed of yttrium aluminum composite oxide contains coloring components in a total ratio of 40 ppm by mass or more and 110 ppm by mass or less. By containing the coloring components in a total ratio of 40 ppm by mass or more and 110 ppm by mass or less, the ceramics mainly composed of yttrium aluminum composite oxide can be imparted with high thermal emissivity.

[0037] YAG, a type of yttrium aluminum oxide, is Al5Y3O 12 , YAM is represented as Al2Y4O9, and YAP is represented as AlYO3. The identity and content of each component constituting the ceramics and the content of the coloring component may be determined by the above-mentioned method.

[0038] Ceramics (single crystals) mainly composed of yttrium aluminum composite oxide can be obtained, for example, by the following procedure: First, a powder mainly composed of yttrium oxide, a powder mainly composed of aluminum oxide, and a powder of a compound that will be a coloring component are heated and melted in a crucible made of molybdenum, and then crystallized by the EFG method, the Czochralski method, the chiroporus method, the TGT method, or the HEM method.

[0039] Here, the atmospheric gas during melting may be argon gas, the melting temperature may be 1550° C. to 1850° C., and the argon gas pressure may be 0.02 to 0.06 MPa. The powder of the compound that becomes the coloring component may be the powder described above.

[0040] The ceramics mainly composed of yttrium aluminum composite oxide forming the semiconductor manufacturing equipment member according to another embodiment also exhibits a dark color tone ranging from brown to dark brown. Specifically, as described above, in the L*a*b* color system, the lightness index L* is 0 to 70, the chromaticness index a* is -10 to 10, and b* is -15 to 15. The total reflectance at a wavelength of 360 nm is preferably 16% or less, and the total reflectance at a wavelength of 740 nm is preferably 25% to 50%.

[0041] Regardless of the main component, the ceramics of the present disclosure may have a surface in which the total reflectance in the wavelength range of 360 nm to 740 nm gradually increases according to a logarithmic approximation curve, a polynomial approximation curve, or a power approximation curve. A surface in which the total reflectance in the above wavelength range gradually increases according to any of the above approximation curves can absorb infrared rays more slowly than a surface in which the total reflectance increases linearly. Therefore, residual stress is less likely to accumulate, and the ceramics can be used in environments where high temperatures must be maintained (for example, in a semiconductor chamber). When setting the approximation function of the total reflectance, it is recommended to measure the wavelengths at intervals of 10 nm in the above wavelength range.

[0042] The approximation function showing the gradual increase in total reflectance is set using a graph tool provided in Excel (registered trademark, Microsoft Corporation), and then the correlation coefficient R is calculated. Then, using an r table (correlation coefficient test table), the correlation coefficient R is tested at a significance level of 5% (two-sided probability), and if it is significant, an approximation curve (logarithmic approximation curve, polynomial approximation curve, or power approximation curve) showing the gradual increase in total reflectance is determined.

[0043] 1 is a graph showing an example of the total reflectance of the surface of a ceramic included in a member for semiconductor manufacturing equipment of the present disclosure. This ceramic contains yttrium zirconate as a main component and manganese at a ratio of 100 mass ppm. The solid line in the graph shown in FIG. 1 represents the total reflectance of the surface of the ceramic in the wavelength range of 360 nm to 740 nm, and the dashed line represents a third-order polynomial approximation curve obtained from the total reflectance. This polynomial approximation curve is significant when the correlation coefficient R is tested at a significance level of 5% (two-sided probability), so it can be said that the total reflectance gradually increases according to the polynomial approximation curve.

[0044] The above-mentioned lightness index L*, chromaticness index a*, chromaticness index b* and total reflectance may be measured on a ground surface obtained by grinding a semiconductor manufacturing equipment member with a processing device such as a surface grinder, in accordance with JIS Z 8722: 2009, using a spectrophotometer (for example, CM-3700A or its successor model manufactured by Konica Minolta, Inc.) When measuring using this spectrophotometer, the measurement conditions, that is, the reference light source, viewing angle, measurement wavelength range, measured reflectance, measurement range and irradiation range, may be set as follows. <Measurement conditions> Measurement method: SCI (specular reflected light included) method Reference light source D65 Viewing angle 10° Measurement wavelength range: 360nm~740nm Measured reflectance Total reflectance Irradiation area 3mm×5mm Measurement area 3mm x 5mm

[0045] The semiconductor manufacturing equipment members according to the other embodiments include the above-mentioned members, and detailed description thereof will be omitted. EXAMPLES

[0046] Examples of the present embodiment will be specifically described below, but the present embodiment is not limited to these examples.

[0047] First, ceramic powder, manganese carbonate (MnCO3) powder, pure water and a dispersant were added, and then crushed and mixed in a bead mill to obtain a slurry. The ceramic powder used was a mixture of powder mainly composed of zirconium oxide and powder mainly composed of yttrium oxide in a mass ratio of 1:2.8. Manganese carbonate (MnCO3) powder was added (externally added) in the proportions shown in Table 1, relative to the total of 100 mass% of the ceramic powder.

[0048] Next, an organic binder was added to the slurry, which was then stirred. The slurry was then spray-dried and de-ironized to obtain granules. The granules were filled into a mold and then pressurized into a cylindrical shape using cold isostatic pressing (CIP) to obtain a green body. The precursor, which was machined into the green body, was then degreased and fired to obtain a sintered body. The firing atmosphere was air, the firing temperature was 1700°C, and the holding time was 3 hours.

[0049] Some of the sintered bodies were annealed during the cooling process. The annealing treatment was carried out by holding the body at 1400℃ for 4 hours. In the annealing treatment column of Table 1, samples that were annealed are marked with "Yes" and samples that were not annealed are marked with "No."

[0050] The sintered body was honed along the axial direction to form a flow path for supplying a gas for plasma generation. The end faces of the sintered body were polished to form gas nozzles, which were designated as samples No. 1 to 14. The main components of each sample were identified using an X-ray diffraction apparatus. Samples in which yttrium zirconate was not identified as the main component were further confirmed using a scanning electron microscope (SEM) and an energy dispersive spectrometer (EDS). The manganese content in each sample was measured using a glow discharge mass spectrometer (GDMS). The composition formula of the main component and the manganese content that were confirmed are shown in Table 1. The color unevenness of each sample was visually observed, and samples that could be visually confirmed were marked as "present," and samples that could not be visually confirmed were marked as "absent" in the color unevenness column of Table 1.

[0051] A hose for supplying pure water was connected to one of the supply ports of the flow path of each sample, and a container was connected to the outlet port communicating with the supply port. Next, pure water was supplied from the hose for 100 seconds at a flow rate of 5 mL / sec, and the number of particles contained in the pure water discharged into the container was measured using a liquid particle counter (LPC). The measured numbers are shown in Table 1. The particles to be measured were those with a diameter exceeding 0.2 μm. Furthermore, the containers used were ultrasonically cleaned before connection, and it was confirmed that the number of particles with a diameter exceeding 0.2 μm was 20 or less.

[0052] [Table 1]

[0053] As shown in Table 1, in samples No. 2 to 6 and 9 to 13, the manganese content was 40 ppm by mass or more and 110 ppm by mass, so no color unevenness was visible. On the other hand, in samples No. 1 and 8, which had a manganese content of 30 ppm by mass, color unevenness was visible, although the number of particles was small. Furthermore, among the samples in which color unevenness was not visible, samples No. 2 to 6 and 9 to 13 had an extremely small number of particles compared to samples No. 7 and 14, which had a manganese content of 120 ppm by mass.

Claims

1. A member for semiconductor manufacturing equipment comprising a ceramic containing yttrium zirconate or yttrium aluminum composite oxide as a main component, and containing elemental manganese in an amount of 40 ppm by mass or more and 110 ppm by mass or less.

2. A member for semiconductor manufacturing equipment comprising: a ceramic having a main crystal phase consisting of an yttrium oxide solid solution in which zirconium oxide is solid-dissolved in yttrium oxide; and a zirconium oxide solid solution in which yttrium oxide is solid-dissolved in zirconium oxide; and containing elemental manganese, the main crystal phase consisting of an yttrium oxide solid solution in which zirconium oxide is solid-dissolved in yttrium oxide, the main crystal phase containing elemental manganese in an amount of 40 ppm by mass or more and 110 ppm by mass or less.

3. 3. The semiconductor manufacturing equipment member according to claim 1, wherein the ceramic has a surface whose total reflectance in a wavelength range of 360 nm to 740 nm gradually increases according to a logarithmic approximation curve, a polynomial approximation curve, or a power approximation curve.

4. A semiconductor manufacturing apparatus comprising the member for semiconductor manufacturing apparatus according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Novel alcohol dehydrogenase complex and production thereof

    JP1988012278A

  • Member for apparatus for producing semiconductor or liquid crystal

    JP2000191369A

  • Aluminum nitride sintered compact and member for producing semiconductor

    JP2001163672A

  • Laminate, corrosion resistant member and halogen gas plasma resistant member

    JP2002001865A

  • Halogen gas plasma resistant member and production method therefor

    JP2002249864A