Multilayer adhesive film, flexible metal-clad laminate and flexible printed circuit board

The multilayer adhesive film with a thermoplastic polyimide layer on a non-thermoplastic polyimide film addresses the temperature dependence of dielectric properties, ensuring stable high-speed signal transmission in flexible printed circuit boards for automotive applications.

JP7584274B2Active Publication Date: 2024-11-15KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020177532
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-22
Publication Date
2024-11-15
Estimated Expiration
2040-10-22

AI Technical Summary

Technical Problem

Existing polyimide films do not adequately address the temperature dependence of dielectric properties, particularly dielectric loss tangent, in harsh environments, limiting their use in high-speed signal transmission across wide temperature ranges.

Method used

A multilayer adhesive film with a thermoplastic polyimide adhesive layer on a non-thermoplastic polyimide film, using specific diamine and acid dianhydride components, maintains a low and constant dielectric loss tangent across a wide temperature range from -50°C to 150°C.

Benefits of technology

The film ensures stable high-speed signal transmission in flexible printed circuit boards under extreme temperature variations, suitable for automotive applications like camera modules and millimeter wave radar components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584274000002
    Figure 0007584274000002
  • Figure 0007584274000001
    Figure 0007584274000001
Patent Text Reader

Abstract

To provide an adhesive film which can exhibit an excellent dielectric property in a wide temperature range.SOLUTION: An adhesive layer containing thermoplastic polyimide is disposed at least on one surface of a non-thermoplastic polyimide film so as to form a multi-layered adhesive film. When a dielectric loss tangent of the multi-layered adhesive film at 10 GHz and at -50°C is represented by Df-50, that at 0°C is represented by Df0, that at 50°C is represented by Df5, that at 100°C is represented by Df100, and that at 150°C is represented by Df150, a difference between the maximum and minimum values of them is 0.0005 or less, and all of Df-50, Df0, Df5, Df100 and Df150 are 0.0020 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer adhesive film having an adhesive layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide film, more specifically to a multilayer adhesive film suitable for use in flexible printed circuit boards expected to be used under harsh conditions from low to high temperatures, and to a flexible metal-clad laminate and a flexible printed circuit board having a metal layer on at least one side of the multilayer adhesive film. [Background technology]

[0002] Polyimide film is widely used as an electronic circuit board material due to its excellent mechanical strength, heat resistance, electrical insulation, and chemical resistance. For example, flexible copper-clad laminates (hereinafter also referred to as FCCL) are manufactured by laminating copper foil on at least one side of polyimide film as a circuit board material, and flexible printed circuit boards (hereinafter also referred to as FPC) are manufactured by further creating circuits on the polyimide film, and are used in various electronic devices.

[0003] In recent years, the demand for low dielectric constant and low dielectric loss tangent for electronic circuit board materials has been increasing as the electric signals propagate through circuits at higher frequencies in response to the high-speed signal transmission of electronic devices. This is because lowering the dielectric constant and dielectric loss tangent is effective in suppressing the transmission loss of electric signals. In recent years, as we are in the dawn of the IoT society, the trend toward higher frequencies is progressing, and there is a demand for circuit board materials, FCCLs, and FPCs that can suppress transmission loss, even in the range of 10 GHz or more.

[0004] As a representative technology of IoT, autonomous driving technology for automobiles and drones is under development. Electronic devices such as camera modules and millimeter wave antenna modules used in these devices require large capacity and high speed transmission of acquired data. In particular, when used in automotive applications, it is expected that the devices will be exposed to high temperatures due to exhaust heat from the engine and drive unit, or will be used in cold regions, so in addition to high speed transmission characteristics, stable high speed transmission performance is required in a wide temperature range. In addition, if high speed transmission can be realized in a wide temperature range, it will be possible to increase the freedom of installation location of signal circuits in the automobile. Therefore, the development of board materials that can be used suitably for FPCs that are expected to be used under such harsh conditions is awaited.

[0005] Incidentally, liquid crystal polyester (LCP) is sometimes used as a substrate material other than polyimide. Although LCP generally has poor processability, it is a material with excellent low moisture absorption and low dielectric tangent due to its crystallinity. In order to realize an even lower dielectric tangent, a method is known in which a wholly aromatic liquid crystal polyester that satisfies certain conditions is heat-treated to improve the dielectric properties, and it is known that this can realize a low dielectric tangent in the range of 30°C to 100°C (Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO2020 / 003690 Summary of the Invention [Problem to be solved by the invention]

[0007] Attempts have been made to develop polyimide films with low dielectric constants and dielectric loss tangents, but little attention has been paid to the temperature dependence of the dielectric properties of polyimide films. However, in recent years, the locations and applications in which FPCs are used have become more diverse, and it is expected that FPCs will be exposed to high temperatures and will be used at extremely low temperatures, so a material that exhibits excellent dielectric properties in a wide range of temperatures from low to high is desired. Therefore, the object of the present invention is to provide a multilayer adhesive film that has an adhesive layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide film, which can exhibit excellent dielectric properties, particularly a low dielectric loss tangent, in a wide range of temperatures. [Means for solving the problem]

[0008] The present invention can solve the above problems by providing the following novel multilayer adhesive film, flexible metal-clad laminate, and flexible printed circuit board.

[0009] 1) A multilayer adhesive film having an adhesive layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide film, characterized in that when the dielectric tangents of the multilayer adhesive film at 10 GHz measured at every 50°C increase in temperature including -50°C in a temperature range of -50°C to 150°C are respectively defined as Df-50 at -50°C, Df0 at 0°C, Df5 ​​at 50°C, Df100 at 100°C, and Df150 at 150°C, the difference between the maximum and minimum of these values ​​is 0.0005 or less, and all of Df-50, Df0, Df5, Df100, and Df150 are 0.0020 or less.

[0010] 2) The multilayer adhesive film described in 1), characterized in that the differences between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 are 0.0004 or less.

[0011] 3) The polyimide film according to 1) or 2), wherein all of Df-50, Df0, Df5, Df100 and Df150 are in the range of 0.0013 to 0.0020.

[0012] 4) A multilayer adhesive film described in any one of 1) to 3), characterized in that the non-thermoplastic polyimide film is a film made from at least 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene diamine components and an acid dianhydride component as raw materials.

[0013] 5) The multilayer adhesive film according to 4), wherein the non-thermoplastic polyimide film further uses 3,3',4,4'-biphenyltetracarboxylic dianhydride as an acid dianhydride component.

[0014] 6) The multilayer adhesive film described in 5), characterized in that the non-thermoplastic polyimide film uses 4,4'-oxydiphthalic dianhydride in addition to 3,3',4,4'-biphenyltetracarboxylic dianhydride as an acid dianhydride component.

[0015] 7) A flexible metal-clad laminate comprising the multilayer adhesive film according to any one of 1) to 6) above and a metal layer on at least one surface thereof.

[0016] 8) A flexible printed circuit board obtained by forming a circuit on the metal layer of the flexible metal-clad laminate according to claim 7. Effect of the Invention

[0017] The multilayer adhesive film of the present invention is a multilayer adhesive film in which an adhesive layer containing a thermoplastic polyimide is provided on at least one side of a non-thermoplastic polyimide film, so that a flexible copper-clad laminate (FCCL) can be manufactured by forming a metal layer on the surface of the adhesive layer, and a flexible printed circuit board (FPC) can be manufactured by forming a circuit on the metal layer. The obtained FCCL and FPC have a low dielectric tangent in a wide temperature range from low to high temperatures, and the dielectric tangent is within a certain range in all temperature ranges, so that they can be suitably used for special applications under severe conditions, such as in-vehicle parts. Specifically, examples of the applications include camera modules, image processing ECUs, millimeter-wave radar parts, inverters, and motors in advanced driving assistance systems, and even when used for the above applications, stable high-speed transmission can be realized in a wide temperature range. [Brief description of the drawings]

[0018] [Figure 1] 1 is a plot of dielectric tangents at temperatures from -50°C to 150°C for the multilayer adhesive films of the examples and the films of the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The following describes an embodiment of the present invention, but the present invention is not limited thereto. All academic and patent documents described in this specification are incorporated herein by reference. Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)."

[0020] The multilayer film of the present invention is a multilayer adhesive film having an adhesive layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide film, and when the dielectric tangents of the multilayer adhesive film at 10 GHz measured every 50°C increase in temperature, including -50°C, in the temperature range of -50°C to 150°C are respectively the dielectric tangent Df-50 at -50°C, the dielectric tangent Df0 at 0°C, the dielectric tangent Df5 at 50°C, the dielectric tangent Df100 at 100°C, and the dielectric tangent Df150 at 150°C, the difference between the maximum and minimum of these values ​​is 0.0005 or less, and all of Df-50, Df0, Df5, Df100 and Df150 are 0.0020 or less.

[0021] Although the liquid crystal polyester (LCP) disclosed in Patent Document 1 exhibits a relatively low dielectric constant and dielectric loss tangent in the cold to room temperature range, the dielectric loss tangent tends to increase in a high temperature environment. This is presumably due to the low heat resistance of LCP and the large permanent dipole moment of the molecules constituting LCP. Therefore, LCP is disadvantageous for use in vehicles where severe temperature changes may occur. Furthermore, Patent Document 1 does not suggest whether the dielectric constant and dielectric loss tangent are low and within a constant range in a wider temperature range of -50°C to 150°C as in the present invention.

[0022] On the other hand, multilayer adhesive films in which an adhesive layer containing a thermoplastic polyimide is provided on at least one side of a non-thermoplastic polyimide film have been widely used for FPC applications in recent years, but no attention has been paid to the temperature dependence of their dielectric tangent.

[0023] In response to such conventional knowledge, the present inventors have focused on the temperature dependence of the dielectric loss tangent of a multilayer adhesive film in which an adhesive layer containing a thermoplastic polyimide is provided on at least one side of a non-thermoplastic polyimide film, and have found that by using a polyimide resin having a certain structure in the multilayer adhesive film, it is possible to keep the dielectric loss tangent of an electronic circuit board constant and low, which is generally thought to fluctuate under harsh temperature environments, especially in high temperature regions. FPCs manufactured using this multilayer adhesive film can be used even under harsh conditions.

[0024] Here, the dielectric loss tangent at 10 GHz measured every time the temperature rises by 50° C., including −50° C., in the temperature range of 50° C. to 150° C., refers to the dielectric loss tangent measured as follows.

[0025] <Equipment used> 1. Network analyzer N5290A (Keysight Technologies) 2. Split cylinder resonator 10GHz CR710 (EM Lab) 3. Split Cylinder Resonator Dielectric Constant Measurement Software CRMA (EM Lab) 4. Environmental test equipment SH662 (manufactured by Espec Corporation)

[0026] <Measurement method> The sample was set in a split cylinder resonator connected to a network analyzer and left to stand for 2 hours in an environmental tester maintained at a constant temperature. After standing, the dielectric constant and dielectric loss tangent were measured. The temperature measurements were performed in order from the highest to the lowest: 150°C, 100°C, 50°C, 0°C, and -50°C. The dielectric loss tangents thus obtained are designated as Df-50 at -50°C, Df0 at 0°C, Df5 ​​at 50°C, Df100 at 100°C, and Df150 at 150°C, respectively, and the maximum and minimum are calculated. The difference between the maximum and minimum is preferably 0.0005 or less, more preferably 0.0004 or less. Df-50, Df0, Df5, Df100, and Df150 are all preferably 0.0020 or less, and more preferably 0.0018 or less.

[0027] The multilayer adhesive film of the present invention is a multilayer polyimide film having at least one non-thermoplastic polyimide resin layer.

[0028] The total thickness of the multilayer adhesive film is preferably 7 μm or more, more preferably 10 μm to 100 μm, from the viewpoint of handling properties when the film is processed into FCCL or the like.

[0029] The thickness ratio of the non-thermoplastic polyimide film and the adhesive layer is preferably in the range of 75:25 to 60:40.

[0030] The following describes in the order of the non-thermoplastic polyimide film, the adhesive layer containing a thermoplastic polyimide, the production of the multilayer adhesive film, the flexible metal-clad laminate, and the flexible printed circuit board.

[0031] (Non-thermoplastic polyimide film) An example of a method for producing the non-thermoplastic polyimide film of the present invention will be described in detail. Polyamic acid (hereinafter, also referred to as polyamic acid), which is a precursor of polyimide used in the production of the non-thermoplastic polyimide film of the present invention, is obtained by mixing and reacting at least one diamine and at least one acid dianhydride in an organic solvent so that the mixture is substantially equimolar.

[0032] The diamine used in the polyamic acid of the non-thermoplastic polyimide film of the present invention is not particularly limited, and examples thereof include 2,2-bis{4-(4-aminophenoxy)phenyl}propane, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylpropane, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfide, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diamino-1,1'-biphenyl, 4,4'-diamino-3,3'-dimethylbiphenyl, 4,4'-diamino-3,3'-hydroxybiphenyl, 1,4-diaminobenzene, 1,3-diaminobenzene, 4,4'-diaminodiphenyl ether, and 1,3-bis(3-aminophenoxy)benzene.

[0033] The easiest way to obtain a multilayer film in which the difference between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 is 0.0005 and all of these are 0.0020 or less is to control these properties of the non-thermoplastic polyimide film. This is because the non-thermoplastic polyimide film is the main component of the multilayer adhesive film. From this viewpoint, it is preferable to use 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene in combination among the above. Furthermore, the amount of 1,4-diaminobenzene used is preferably 70 mol% or more relative to 100 mol% of the diamine component, more preferably in the range of 70 mol% to 95 mol%, and even more preferably in the range of 80 mol% to 90 mol%, and it is preferable to use 5 mol% or more of 1,3-bis(4-aminophenoxy)benzene relative to 100 mol% of the diamine component, more preferably in the range of 5 mol% to 30 mol%, and even more preferably in the range of 10 mol% to 20 mol%. If a non-thermoplastic polyimide film produced using 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene as raw materials within this range is used for a multilayer adhesive film, the differences between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 of the multilayer adhesive film will be small, and all of these values ​​will tend to be small.

[0034] The acid dianhydride is not particularly limited, and specific examples thereof include pyromellitic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propanoic dianhydride, p-phenylenebis(trimellitic monoester acid anhydride), 4,4'-oxydiphthalic dianhydride, and 3,4'-oxydiphthalic dianhydride.

[0035] Among the above, it is preferable to use 3,3',4,4'-biphenyltetracarboxylic dianhydride, from the viewpoint that the difference between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 of the multilayer adhesive film becomes small, and all of these values ​​can be made small. The amount of 3,3',4,4'-biphenyltetracarboxylic dianhydride used is preferably 40 mol% or more relative to 100 mol% of the acid dianhydride component, and more preferably in the range of 50 mol% to 70 mol%. Furthermore, it is preferable to use 4,4'-oxydiphthalic dianhydride in addition to the use of 3,3',4,4'-biphenyltetracarboxylic dianhydride. It is preferable to use 20 mol% or more of 4,4'-oxydiphthalic dianhydride relative to 100 mol% of the acid dianhydride component, and more preferably in the range of 30 mol% to 50 mol%.

[0036] In addition to the above-mentioned dianhydride monomers, other dianhydrides such as pyromellitic dianhydride may be added as long as the dielectric properties are not deteriorated. The amount of the other dianhydride added is preferably 10 mol % or less, more preferably 6 mol % or less, and even more preferably 3 mol % or less, based on 100 mol % of the dianhydride component.

[0037] From the above, when 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene are used as the diamine components and 3,3',4,4'-biphenyltetracarboxylic dianhydride is used as the acid dianhydride component, or when 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene are used as the amine components and 4,4'-oxydiphthalic dianhydride is used as the acid dianhydride component, it becomes easy to reduce the differences between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 of the final multilayer adhesive film and to reduce all of these values. In addition, when 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene are used as the diamine components and 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-oxydiphthalic dianhydride are used as the acid dianhydride components, it becomes easier to reduce the differences between the maximum and minimum values ​​of Df-50, Df0, Df5, Df100 and Df150 of the final multilayer adhesive film and to reduce all of these values.

[0038] Polyamic acid, which is a precursor of non-thermoplastic polyimide, is obtained by mixing and reacting the above diamine and acid dianhydride in an organic solvent so that the diamine and acid dianhydride are substantially equimolar. Any organic solvent that dissolves polyamic acid can be used, but amide solvents, i.e., N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, etc. are preferred, and N,N-dimethylformamide and N,N-dimethylacetamide are particularly preferred. The solid content concentration of polyamic acid is not particularly limited, and if it is within the range of 5% by weight to 35% by weight, a polyamic acid having sufficient mechanical strength when made into polyimide can be obtained.

[0039] The order of addition of the diamine and dianhydride raw materials is not particularly limited, but by controlling not only the chemical structure of the raw materials but also the order of addition, it is possible to control the dielectric tangent of the non-thermoplastic polyimide film, thereby reducing the difference between the maximum and minimum values ​​of Df-50, Df0, Df5, Df100 and Df150 of the final multilayer adhesive film, and reducing all of these values.

[0040] A filler can be added to the polyamic acid for the purpose of improving various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, loop stiffness, etc. Any filler can be used, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.

[0041] In addition, thermosetting resins such as epoxy resins and phenoxy resins, and thermoplastic resins such as polyether ketone and polyether ether ketone may be mixed within a range that does not impair the overall properties of the resulting non-thermoplastic polyimide film. As a method for adding these resins, if they are soluble in a solvent, they may be added to the polyamic acid. If the polyimide is also soluble, they may be added to the polyimide solution. If they are insoluble in a solvent, they may be first imidized and then composited by melt kneading. However, it is preferable to use a soluble resin to be mixed with the polyimide.

[0042] To obtain the non-thermoplastic polyimide film of the present invention, the following steps are preferably included. i) reacting an aromatic diamine with an aromatic tetracarboxylic dianhydride in an organic solvent to obtain a polyamic acid solution; ii) casting a membrane-forming dope containing the polyamic acid solution onto a support; iii) peeling the gel film from the support after heating on the support; iv) A step of further heating to imidize the remaining amic acid and drying.

[0043] ii) The steps after this are roughly divided into thermal imidization and chemical imidization. Thermal imidization is a method in which a polyamic acid solution is poured onto a support as a film-forming dope without using a dehydrating ring-closing agent, and imidization is promoted only by heating. On the other hand, chemical imidization is a method in which a polyamic acid solution to which at least one of a dehydrating ring-closing agent and a catalyst has been added as an imidization promoter is used as a film-forming dope to promote imidization. Either thermal imidization or chemical imidization may be used, but chemical imidization is more productive.

[0044] As the dehydrating ring-closing agent, an acid anhydride such as acetic anhydride can be preferably used. As the catalyst, a tertiary amine such as an aliphatic tertiary amine, an aromatic tertiary amine, or a heterocyclic tertiary amine can be preferably used.

[0045] In the steps ii) and thereafter, the support for casting the film-forming dope can be a glass plate, an aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. Heating conditions are set according to the thickness of the film to be finally obtained and the production speed, and the film is partially imidized and / or dried, and then peeled off from the support to obtain a polyamic acid film (hereinafter also referred to as a gel film or a gel membrane).

[0046] In the steps iv) and after, the ends of the gel film are fixed to avoid shrinkage during curing, and the film is dried to remove water, residual solvent, and imidization promoter remaining in the film, and the remaining amic acid is completely imidized to obtain a film containing polyimide. It is preferable that the ends of the gel film are not only fixed, but also stretched in the conveying direction or perpendicular to the conveying direction.

[0047] The polyimide film thus obtained has a small and constant dielectric loss tangent at -50°C, 0°C, 50°C, 100°C and 150°C, and can therefore be suitably used as a high-frequency compatible circuit board for in-vehicle applications.

[0048] (Adhesive layer containing thermoplastic polyimide) The diamine and dianhydride used in the thermoplastic polyimide used in the adhesive layer of the present invention can be the same as those used in the non-thermoplastic polyimide resin layer. The thickness of the adhesive layer is thinner than that of the non-thermoplastic polyimide film, so its influence is not as large as that of the non-thermoplastic polyimide film, but by using a preferable component as the thermoplastic polyimide contained in the adhesive layer, it is possible to control the maximum and minimum differences of Df-50, Df0, Df5, Df100 and Df150 of the multilayer adhesive film finally obtained, as well as these values. From this viewpoint, the diamine that can be preferably used is at least one selected from 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 2,2-bis(4-aminophenoxyphenyl)propane, and 2,2'-dimethyl-4,4'-diaminobiphenyl.

[0049] As an acid dianhydride that can be suitably combined with these diamines, it is preferable to use at least one selected from the group consisting of pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 4,4'-oxydiphthalic dianhydride.

[0050] The polyamic acid solution which is the precursor of the thermoplastic polyimide used in the adhesive layer of the present invention can be produced by any known method as long as the resulting polyamic acid is imidized to produce a thermoplastic polyimide which has the properties required for conventional flexible printed circuit board materials.

[0051] The resulting polyamic acid solution can be used to produce a multilayer film by the method for producing a multilayer film described below. The adhesive layer may contain, in addition to the thermoplastic polyimide, silica, calcium phosphate, etc., within the range that does not impair the smoothness of the adhesive layer.

[0052] (Manufacturing of multi-layer adhesive films) The multilayer adhesive film of the present invention is a multilayer adhesive film having two or more layers, including at least one non-thermoplastic polyimide resin layer as described above as a core film and an adhesive layer containing a thermoplastic polyimide.

[0053] In the present invention, an example of a method for producing a multilayer adhesive film is a method (coating method) in which a polyamic acid solution, which is a precursor of the thermoplastic polyimide, is applied to at least one side of the non-thermoplastic polyimide film obtained as described above, and then dried and imidized.

[0054] Alternatively, the process for obtaining a non-thermoplastic polyimide film exemplified in the above section (Non-thermoplastic polyimide film), i) reacting an aromatic diamine with an aromatic tetracarboxylic dianhydride in an organic solvent to obtain a polyamic acid solution; ii) casting a membrane-forming dope containing the polyamic acid solution onto a support; iii) peeling the gel film from the support after heating on the support; iv) further heating to imidize the remaining amic acid and drying; In step ii) of the above, a co-extrusion die having a plurality of flow paths may be used to simultaneously form multiple resin layers. That is, in order to obtain a multi-layer polyimide film having an adhesive layer containing a thermoplastic polyimide on at least one side of the above-mentioned non-thermoplastic polyimide film, a precursor solution of the non-thermoplastic polyimide and a precursor solution of the thermoplastic polyimide are cast onto a support using a co-extrusion die, and the steps from iii) onward are carried out to obtain the multi-layer polyimide film.

[0055] Since imidization requires a very high temperature, when a resin layer other than polyimide is provided, it is preferable to adopt a coating method in order to suppress thermal decomposition. When an adhesive layer containing a thermoplastic polyimide is provided by coating, a precursor of the thermoplastic polyimide may be applied and then imidized, or a thermoplastic polyimide solution may be applied and dried.

[0056] (Flexible metal-clad laminates and flexible printed circuit boards) The multi-layer polyimide film thus obtained can be made into a flexible metal-clad laminate by providing a metal layer on at least one side of the multi-layer polyimide film. a) After obtaining a multi-layer polyimide film as described above, a metal foil is laminated by heating and pressing to obtain a flexible metal-clad laminate. b) A method of casting an organic solvent solution containing polyamic acid on a metal foil, removing the solvent by heating, and performing imidization to obtain a flexible metal-clad laminate. Details of a) and b) are described below.

[0057] In the method of a), a metal foil is laminated to the obtained multilayer polyimide film by heating and pressing (lamination), to obtain the flexible metal foil laminate of the present invention. The method and conditions for laminating the metal foil may be appropriately selected from those conventionally known.

[0058] In the method of b), the method for casting an organic solvent solution containing polyamic acid (a solution containing a precursor of a thermoplastic polyimide or an amic acid solution which is a precursor of a non-thermoplastic polyimide) onto a metal foil is not particularly limited, and a conventionally known method such as a die coater, a comma coater (registered trademark), a reverse coater, a knife coater, etc. As for the heating method for removing the solvent and performing imidization, a conventionally known method can be used, for example, a hot air oven or a far-infrared oven.

[0059] In addition, when a chemical imidization method is adopted for forming a non-thermoplastic polyimide film or an adhesive layer by the method (b), an acid is generated from an acid anhydride, which is a dehydrating ring-closing agent, during the imidization process, and oxidation may progress depending on the type of metal foil. It is preferable to appropriately select the dehydrating ring-closing agent depending on the type of metal foil and the heating conditions.

[0060] When providing an adhesive layer containing a non-thermoplastic polyimide film and a thermoplastic polyimide, the above-mentioned casting and heating steps are repeated multiple times, or a multi-layer cast layer is formed by coextrusion or continuous casting and heated all at once.

[0061] In the method of b), the flexible metal foil laminate of the present invention is obtained at the same time as the imidization is completed. When metal foil layers are provided on both sides of the resin layer, the metal foil may be laminated to the opposite resin layer surface by heating and pressing.

[0062] The metal foil that can be used in the present invention is not particularly limited, but when the flexible metal-clad laminate of the present invention is used for electronic and electrical equipment applications, examples of the metal foil include foils made of copper or copper alloys, stainless steel or its alloys, nickel or nickel alloys (including 42 alloy), and aluminum or aluminum alloys. In general flexible laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, but they can also be preferably used in the present invention. The surfaces of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. The thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient function depending on the application.

[0063] The metal layer of the thus obtained flexible metal-clad laminate is etched by a known method to obtain a flexible printed circuit board. EXAMPLES

[0064] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The relative dielectric constant and dielectric loss tangent of the laminates in the synthesis examples, examples, and comparative examples were evaluated as follows.

[0065] (Measurement of dielectric tangent) A multilayer polyimide film cut to 50 mm x 70 mm was placed on a split cylinder resonator CR710 (10 GHz, EM Lab) connected to a network analyzer N5290A (Keysight Technologies), and left to stand for 2 hours in an environmental tester kept at a constant temperature. After standing, the dielectric constant and dielectric loss tangent were measured. The measurements were performed at successively higher temperatures, starting from 150°C, 100°C, 50°C, 0°C, and -50°C. In addition, each time the temperature inside the environmental tester was set to a specific temperature, the tester was left to stand for 2 hours.

[0066] As a comparative example, the dielectric loss tangent of an LCP film (FELIOS R-F705T, manufactured by Panasonic Corporation) was measured in the same manner as in the "Measurement of dielectric loss tangent" above.

[0067] (Synthesis Example 1) In a 2000ml glass flask, 656.66g of N,N-dimethylformamide (DMF), 12.12g of 1,3-bis(4-aminophenoxy)benzene (TPE-R), 25.44g of 1,4-diaminobenzene (PDA) were added, and 48.86g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) was added, followed by stirring under a nitrogen atmosphere. After confirming that BPDA had dissolved, 31.77g of 4,4'-oxydiphthalic dianhydride (ODPA) was added and stirred for 30 minutes. Finally, a solution was prepared by dissolving 1.8 g of pyromellitic dianhydride (hereinafter also referred to as PMDA) in DMF to a solids concentration of 7.2%, and this solution was gradually added to the above reaction solution while paying attention to the increase in viscosity. When the viscosity at 23°C reached 2000 poise, addition and stirring were stopped, and a polyamic acid solution was obtained.

[0068] (Preparation of non-thermoplastic polyimide film) An imidization promoter consisting of acetic anhydride / isoquinoline / DMF (weight ratio 2.1 / 1.1 / 0.8) was added to the polyamic acid solution of Synthesis Example 1 at a weight ratio of 40% relative to the polyamic acid solution, and the solution was continuously stirred with a mixer, extruded from a T-die, and cast onto a stainless steel endless belt. The resin film was heated at 100°C for 330 seconds, and then the self-supporting gel film was peeled off from the endless belt and fixed to a tenter clip, and dried and imidized in a hot air oven at 250°C for 41 seconds, a hot air oven at 350°C for 37 seconds, a hot air oven at 380°C for 32 seconds, and a far-infrared heater oven at 380°C for 97 seconds to obtain a non-thermoplastic polyimide film having a thickness of 33 μm.

[0069] (Synthesis Example 2) 642.12g of DMF, 53.02g of TPE-R, and 38.16g of BPDA were added to a 2000ml glass flask, and the mixture was stirred for 30 minutes under a nitrogen atmosphere. Next, 8.49g of PMDA was added, and the mixture was stirred for 30 minutes. Next, 16.52g of 2,2'-dimethyl-4,4'-diaminobiphenyl (hereinafter also referred to as m-TB) and 18.11g of PMDA were added, and the mixture was stirred for 30 minutes. Finally, a solution was prepared by dissolving 1.7g of PMDA in DMF to a solid content concentration of 7.2%, and this solution was gradually added to the above reaction solution while paying attention to the increase in viscosity. When the viscosity at 23°C reached 1000 poise, the mixture was added, and stirring was stopped, to obtain a polyamic acid solution.

[0070] Example 1 The polyamic acid solution, which is the precursor of the thermoplastic polyimide prepared in Synthesis Example 2, was diluted with DMF until the solid content concentration was 10% by weight, and then the polyamic acid was applied to one side of the non-thermoplastic polyimide film obtained in Synthesis Example 1 with a comma coater so that the final thickness on one side was 8.5 μm, and the film was heated in a drying oven set at 120 ° C for 4 minutes. The other side was also similarly coated with polyamic acid so that the final thickness was 8.5 μm, and the film was heated in a drying oven set at 120 ° C for 4 minutes. Subsequently, the film was heated for 15 seconds in a hot air oven at an atmospheric temperature of 380 ° C to obtain a multilayer adhesive film with a total thickness of 50 μm.

[0071] Comparative Example 1 An LCP film (FELIOS R-F705T, manufactured by Panasonic Corporation) having a thickness of 50 μm was prepared. The results of measuring the dielectric tangent for the examples and comparative examples are shown in Table 1 and FIG.

[0072] The multilayer adhesive film of the present invention has a difference between the maximum and minimum dielectric tangent values ​​at -50°C, 0°C, 50°C, 100°C, and 150°C of 0.0005 or less, and all of the dielectric tangent values ​​measured at the above temperatures are 0.0020 or less, indicating that the multilayer adhesive film of the present invention exhibits a low and constant dielectric tangent over a wide temperature range.

[0073] Therefore, it can be said to be an ideal substrate for FPC boards for in-vehicle applications that require operational reliability in temperatures ranging from below zero to over 100°C. Specific applications include camera modules in advanced driver assistance systems, image processing ECUs, millimeter wave radar parts, inverters, and motors. This allows for greater freedom in the installation location of FPCs with excellent high-speed transmission characteristics. [Table 1]

Claims

1. A multi-layer adhesive film having an adhesive layer containing a thermoplastic polyimide on at least one side of a non-thermoplastic polyimide film, the dielectric dissipation factor at 10 GHz of the multilayer adhesive film measured at every 50°C increase in temperature, including -50°C, in a temperature range of -50°C to 150°C is Df-50 at -50°C, Df0 at 0°C, Df5 ​​at 50°C, Df100 at 100°C, and Df150 at 150°C, respectively, the difference between the maximum and minimum of these values ​​is 0.0005 or less, and all of Df-50, Df0, Df5, Df100, and Df150 are 0.0020 or less; The non-thermoplastic polyimide film is a multi-layer adhesive film characterized in that it is a film using, as raw materials, at least diamine components of 1,4-diaminobenzene and 1,3-bis(4-aminophenoxy)benzene, and acid dianhydride components of 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-oxydiphthalic dianhydride.

2. The multilayer adhesive film according to claim 1, wherein the differences between the maximum and minimum of Df-50, Df0, Df5, Df100 and Df150 are 0.0004 or less.

3. 3. The multilayer adhesive film according to claim 1, wherein all of Df-50, Df0, Df5, Df100 and Df150 are in the range of 0.0013 to 0.0020.

4. The diamine used in the thermoplastic polyimide is one or more selected from 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenoxyphenyl)propane, and 2,2'-dimethyl-4,4'-diaminobiphenyl; The multilayer adhesive film according to any one of claims 1 to 3, characterized in that the acid dianhydride used in the thermoplastic polyimide is one or more selected from the group consisting of pyromellitic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 4,4'-oxydiphthalic dianhydride.

5. A flexible metal-clad laminate comprising the multi-layer adhesive film according to any one of claims 1 to 4 and a metal layer on at least one surface of the multi-layer adhesive film.

6. A flexible printed circuit board obtained by forming a circuit on the metal layer of the flexible metal-clad laminate according to claim 5.

Citation Information

Patent Citations

  • Metal-clad laminate and circuit board

    JP2015193117A

  • Method for producing multilayered polyimide film

    JP2018126887A

  • Polyimide, adhesive, film-like adhesive, adhesion layer, adhesive sheet, copper foil with resin, copper-clad laminate, printed wiring board, and multilayer wiring board and method for producing the same

    JP2020117631A

  • Metal laminated board and circuit board

    JP2021170603A

  • Molded resin product including wholly aromatic liquid crystal polyester resin capable of reducing dielectric loss tangent by heat treatment, and electric / electronic component

    WO2020003690A1