Wiper rubber

By using a rubber composition of natural rubber and carbon black, vulcanized with sulfur and an organic peroxide, the wiper rubber achieves enhanced processability and durability, addressing the challenges of existing wiper rubber technologies.

JP7584304B2Active Publication Date: 2024-11-15BANDO CHEM IND LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021001940
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-08
Publication Date
2024-11-15
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Existing wiper rubber technologies face challenges in achieving optimal properties such as wipeability, maintenance, and processability during manufacturing, which are influenced by the method of vulcanization.

Method used

The wiper rubber is composed of a rubber composition containing natural rubber and carbon black, vulcanized using a combination of sulfur, a vulcanization accelerator, and an organic peroxide, with specific ratios and surface treatments to enhance properties.

Benefits of technology

The combination of sulfur, a vulcanization accelerator, and an organic peroxide improves the wiper rubber's processability, moldability, and resistance to permanent deformation and thermal changes, ensuring improved wiping performance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584304000002
    Figure 0007584304000002
  • Figure 0007584304000001
    Figure 0007584304000001
Patent Text Reader

Abstract

To provide a wiper rubber that suppresses both permanent deformation and a physical property change caused by a thermal history.SOLUTION: A wiper rubber 10 is made of a rubber composition including natural rubber and carbon black. The rubber composition is vulcanized by combining sulfur and a vulcanization accelerator with an organic peroxide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a wiper rubber for use in automobiles and the like. [Background technology]

[0002] 2. Description of the Related Art A wiper system including a wiper blade and a wiper arm that supports the wiper blade is used to wipe an object to be wiped, such as a windshield of an automobile. The wiper blade is usually provided with a wiper rubber made of vulcanized rubber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-64281 A Summary of the Invention [Problem to be solved by the invention]

[0004] There are various demands for wiper rubber, such as wiping ability and maintenance, processability during manufacturing, etc. These characteristics depend on various factors, one of which is the vulcanization method.

[0005] The objective of the present disclosure is to improve the properties of wiper rubber by the method of vulcanization. [Means for solving the problem]

[0006] In order to achieve the above object, the wiper rubber of the present disclosure is made of a rubber composition containing natural rubber and carbon black. The rubber composition is vulcanized by using sulfur, a vulcanization accelerator, and an organic peroxide in combination. Effect of the Invention

[0007] The wiper rubber of the present disclosure has improved properties due to being vulcanized using sulfur, a vulcanization accelerator, and an organic peroxide in combination. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram showing a cross-sectional shape of an exemplary wiper rubber according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an exemplary wiper rubber of the present disclosure will be described with reference to the drawings. FIG. 1 is a diagram showing a cross-sectional shape of an exemplary wiper rubber 10. The wiper rubber 10 includes a holding portion 11 held by a vertebra and a lip portion 13 for wiping an object to be wiped, such as a windshield of an automobile, and the holding portion 11 side and the lip portion 13 side are connected by a narrow neck portion 12. The corner portion of the tip of the lip portion 13 is an edge portion 14 that contacts the object to be wiped. In the wiper rubber 10 of FIG. 1, the tip of the lip portion 13 has a square cross section, and there are two edge portions 14. The two edge portions 14 contact the object to be wiped when the wiper moves from the initial position to the terminal position and when the wiper moves from the terminal position to the initial position, respectively, when the wiper moves back and forth to wipe.

[0010] The wiper rubber 10 is made of a rubber composition containing a rubber component and carbon black. As the rubber component, natural rubber is preferable, and it is more preferable to use only natural rubber.

[0011] The carbon black preferably has an iodine adsorption amount of 24 g / kg or more and 60 g / kg or less.

[0012] The reason for this is that by using carbon black with an iodine adsorption of 24 g / kg or more, the wear resistance of the rubber is improved, making it difficult to wear and suppressing deterioration of wiping performance. Also, by using carbon black with an iodine adsorption of 60 g / kg or less, sufficient dispersibility of the carbon black in the rubber can be obtained. As a result, the appearance of agglomerates on the edge portion 14 of the wiper rubber 10 can be suppressed, and deterioration of wiping performance due to the agglomerates can be suppressed.

[0013] The rubber composition forming the wiper rubber 10 is vulcanized using sulfur, a vulcanization accelerator, and an organic peroxide in combination.

[0014] Generally, in order to vulcanize rubber, sulfur and a vulcanization accelerator are blended as vulcanizing agents into the rubber composition, or an organic peroxide is blended into the rubber composition.

[0015] When sulfur and a vulcanization accelerator are used as vulcanizing agents, the phenomenon that vulcanization starts during the kneading and rolling process of the rubber composition (a phenomenon called "burning") tends to occur. Therefore, after the rolling process, it is necessary to proceed immediately to the wiper molding process using a vulcanization press. This is expressed as the wiper rubber material having poor processability.

[0016] On the other hand, when an organic peroxide is used as a vulcanizing agent, the kneading and rolling processability is good, but the molding time by vulcanization press tends to be long, which is expressed as poor moldability.

[0017] In contrast, the wiper rubber of the present disclosure is excellent in both processability and moldability by using sulfur and a vulcanization accelerator in combination with an organic peroxide. In other words, vulcanization acceleration in the kneading and rolling stages is suppressed, and the molding time by the vulcanization press is shortened.

[0018] In addition, the wiper rubber is constantly under pressure from the wiper arm and is in a deformed state. If the wiper rubber is subjected to a large permanent deformation, the wiping performance deteriorates, so it is necessary to reduce the permanent deformation. In the case of wipers for automobiles, they are used on the front and rear windows and are exposed to stimuli such as heat and ozone, which is an environment in which the physical properties are easily changed due to thermal history. In order to maintain the wiping performance of wiper rubber, it is desirable to suppress the change in physical properties, particularly the change in modulus.

[0019] In contrast, in the wiper rubber of the present disclosure, sulfur and a vulcanization accelerator are used in combination with an organic peroxide, thereby suppressing both permanent deformation and changes in physical properties due to thermal history.

[0020] Examples of organic peroxides include dicumyl peroxide, 1,3-bis(t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane. The organic peroxide may be one of the above or two or more of them. The content of the organic peroxide in the uncrosslinked rubber composition for forming the wiper rubber 10 is preferably 0.2% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.7% by mass or more, and is preferably 6.5% by mass or less, more preferably 5.5% by mass or less, and even more preferably 5.0% by mass or less.

[0021] The sulfur content in the uncrosslinked rubber composition is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.4 mass% or more, and is preferably 1.7 mass% or less, more preferably 1.5 mass% or less, even more preferably 1.2 mass% or less.

[0022] Furthermore, the ratio of the sulfur content to the organic peroxide content in the uncrosslinked rubber composition (sulfur content / organic peroxide content) is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.25 or more, and is preferably 2.0 or less, more preferably 1.5 or less, even more preferably 1.3 or less. The sulfur content in the uncrosslinked rubber composition is preferably higher than the organic peroxide content.

[0023] Next, a vulcanization accelerator is blended into the rubber composition forming the wiper rubber 10. As the vulcanization accelerator, a vulcanization accelerator having a thiocarbonyl group is more preferable.

[0024] Examples of vulcanization accelerators having a thiocarbonyl group include thiourea-based vulcanization accelerators such as N,N'-diphenylthiourea, trimethylthiourea (TMU), and N,N'-diethylthiourea (DEU); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), tetrabutylthiuram disulfide (TBTD), tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide (TMTM), and dipentamethylenethiuram tetrasulfide (DPTT); piperidinium pentamethylene dithiocarbamate (PPDC), dimethyldithiocarbamate, and the like. Examples of suitable vulcanization accelerators include dithiocarbamate-based vulcanization accelerators such as zinc diethyldithiocarbamate (ZnMDC), zinc diethyldithiocarbamate (ZnEDC), zinc dibutyldithiocarbamate (ZnBDC), zinc ethylphenyldithiocarbamate (ZnEPDC), zinc N-pentamethylenedithiocarbamate (ZnPDC), zinc dibenzyldithiocarbamate, sodium dibutyldithiocarbamate (NaBDC), copper dimethyldithiocarbamate (CuMDC), ferric dimethyldithiocarbamate (FeMDC), and tellurium diethyldithiocarbamate (TeEDC); and xanthate-based vulcanization accelerators such as zinc isopropylxanthate. Among these, thiuram-based vulcanization accelerators and dithiocarbamate-based vulcanization accelerators are preferred, and thiuram-based vulcanization accelerators are more preferred. The vulcanization accelerator having a thiocarbonyl group may be one of the above-mentioned vulcanization accelerators, or two or more of them may be blended.

[0025] The amount of the vulcanization accelerator having a thiocarbonyl group blended relative to 100 parts by mass of the rubber component is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, even more preferably 0.8 parts by mass or more, and is preferably 3.0 parts by mass or less, more preferably 2.5 parts by mass or less, and even more preferably 2.0 parts by mass or less. The content of the vulcanization accelerator having a thiocarbonyl group in the uncrosslinked rubber composition for forming the wiper rubber 10 is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.3% by mass or more, and is preferably 2.2% by mass or less, more preferably 1.9% by mass or less, and even more preferably 1.7% by mass or less. The ratio of the content of the vulcanization accelerator having a thiocarbonyl group to the content of the organic peroxide in the uncrosslinked rubber composition for forming the wiper rubber 10 (content of the vulcanization accelerator having a thiocarbonyl group / content of the organic peroxide) is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, and also preferably 1.0 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. The content of the vulcanization accelerator having a thiocarbonyl group in the uncrosslinked rubber composition is preferably less than the content of the organic peroxide. When sulfur is blended as a crosslinking agent, the ratio of the content of the vulcanization accelerator having a thiocarbonyl group to the content of sulfur in the uncrosslinked rubber composition (content of the vulcanization accelerator having a thiocarbonyl group / content of sulfur) is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, and also preferably 6.0 or less, more preferably 3.0 or less, and even more preferably 2.0 or less. The content of the vulcanization accelerator having a thiocarbonyl group in the uncrosslinked rubber composition is preferably the same as or less than the content of sulfur.

[0026] The uncrosslinked rubber composition for forming the wiper rubber 10 may contain only a vulcanization accelerator having a thiocarbonyl group, or may contain a vulcanization accelerator other than the vulcanization accelerator having a thiocarbonyl group in combination. Examples of vulcanization accelerators other than the vulcanization accelerator having a thiocarbonyl group include aldehyde-ammonia-based vulcanization accelerators, aldehyde-amine-based vulcanization accelerators, thiourea-based vulcanization accelerators, guanidine-based vulcanization accelerators, thiazole-based vulcanization accelerators, and sulfenamide-based vulcanization accelerators.

[0027] Next, it is preferable that the wiper rubber 10 is subjected to a surface treatment for reducing friction. Examples of the surface treatment include a chemical surface treatment and a coating treatment, and either one of the treatments or a combination of the two may be used.

[0028] As the chemical surface treatment, for example, halogen treatment is preferable. The halogen treatment may be applied to the entire wiper rubber 10, or may be applied mainly to the parts that come into contact with the object to be wiped, i.e., the lip portion 13 and the edge portion 14.

[0029] When the coating process is performed, the coating agent may contain a solid lubricant and an addition polymerization type silicone rubber. The solid lubricant may be graphite, molybdenum disulfide, fluororesin, spherical silica, porous spherical silica, calcium carbonate, diatomaceous earth, boron nitride, etc. As with the chemical surface treatment, the coating process may be performed on the entire wiper rubber 10, or may be performed mainly on the part that comes into contact with the object to be wiped. EXAMPLES

[0030] Examples of the wiper rubber of the present disclosure will be described below. Wiper rubbers of Examples 1 to 5 and Comparative Examples 1 to 3 were produced as follows. Each wiper rubber is also shown in Table 1 (the unit of composition is phr: per hundred rubber, that is, parts by mass relative to 100 parts by mass of the rubber component).

[0031] The rubber compounds for each are also shown in Table 1.

[0032] Example 1 The rubber composition for preparing the wiper rubber of Example 1 used natural rubber as a rubber component. In addition, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 50 parts by mass of carbon black, 4 parts by mass of process oil, and 5 parts by mass of antioxidant were used relative to 100 parts by mass of the natural rubber. Furthermore, 0.5 parts by mass of sulfur, 3 parts by mass of vulcanization accelerator, and 2.2 parts by mass of organic peroxide were used. More specifically, as the vulcanization accelerator, 0.5 parts by mass of dicarbamic acid vulcanization accelerator and 2.5 parts by mass of other vulcanization accelerator (vulcanization accelerator not containing a thiocarbonyl group) were used. For the rubber composition containing these, the sulfur was 0.29% by mass and the organic peroxide was 1.29% by mass.

[0033] The carbon black used was Sterling NS, a product name of Cabot Corporation. The iodine adsorption capacity of this carbon black is 29 g / kg, and the DBP (dibutyl phthalate) adsorption capacity is 70 ml / 100 g.

[0034] The rubber composition having the above-mentioned composition was formed into a wiper rubber having a cross-sectional shape shown in Fig. 1 and a length of 350 mm. The forming method was a vulcanization press machine, and the rubber was vulcanized at 165°C for 10 minutes.

[0035] Next, the formed wiper rubber was subjected to a chlorine treatment as a surface treatment. Specifically, the wiper rubber was immersed in chlorine water, and then washed with water, washed with hot water, and dried in that order.

[0036] Example 2 Except for the vulcanization accelerator, the wiper rubber of Example 2 was produced in the same manner as Example 1. Specifically, as the vulcanization accelerator, 0.5 parts by mass of a thiuram vulcanization accelerator (based on 100 parts by mass of the rubber component; the same applies below) and 2.5 parts by mass of other vulcanization accelerators (total of vulcanization accelerators: 3 parts by mass) were used.

[0037] Example 3 A wiper rubber of Example 3 was produced in the same manner as Example 1, except for the compounding amounts of the vulcanization accelerator and the organic peroxide. Specifically, the organic peroxide was 1.7 parts by mass. In addition, 0.5 parts by mass of a dicarbamic acid vulcanization accelerator and 2.5 parts by mass of other vulcanization accelerators were used as vulcanization accelerators. In Example 3, the sulfur was 0.29% by mass and the organic peroxide was 1.00% by mass relative to the rubber composition.

[0038] Example 4 A wiper rubber of Example 3 was produced in the same manner as Example 1 except for the amount of the organic peroxide. Specifically, the amount of the organic peroxide was 1.1 parts by mass. In Example 4, the amount of sulfur was 0.29% by mass and the amount of the organic peroxide was 0.65% by mass relative to the rubber composition.

[0039] Example 5 In Example 5, sulfur, a vulcanization accelerator, and an organic peroxide are used, but a substance containing a thiocarbonyl group (here, a thiuram-based or dithiocarbamic acid-based substance) is not used as the vulcanization accelerator, and only 3.0 parts by mass of other vulcanization accelerators are used. The wiper rubber of Example 5 was produced using a wiper rubber having the same compounding amount as that of Example 1 in other respects. In Example 5, the sulfur is 0.29% by mass and the organic peroxide is 1.29% by mass with respect to the rubber composition.

[0040] Comparative Example 1 Comparative Example 1 is an example in which sulfur and a vulcanization accelerator are used, but no organic peroxide is used. Specifically, 1 part by mass of a thiuram vulcanization accelerator and 2 parts by mass of another vulcanization accelerator are used as the vulcanization accelerator (total of vulcanization accelerators is 3 parts by mass). No organic peroxide is used. A wiper rubber of Comparative Example 1 was produced using a wiper rubber with the same compounding amounts as in Example 1 in other respects. In Comparative Example 1, the sulfur content is 0.30% by mass and the organic peroxide content is 0% by mass with respect to the rubber composition.

[0041] Comparative Example 2 Comparative Example 2 is also an example in which sulfur and a vulcanization accelerator are used, but no organic peroxide is used. Specifically, 1 part by mass of a thiuram-based vulcanization accelerator and 1 part by mass of a dithiocarbamic acid-based vulcanization accelerator are used as the vulcanization accelerators (total of vulcanization accelerators is 2 parts by mass). No organic peroxide is used. A wiper rubber of Comparative Example 2 was produced using a wiper rubber with the same compounding amounts as in Example 1 in other respects. In Comparative Example 2, the sulfur content is 0.30% by mass and the organic peroxide content is 0% by mass with respect to the rubber composition.

[0042] Comparative Example 3 Comparative Example 3 is an example in which an organic peroxide is used, but sulfur and a vulcanization accelerator are not used. Specifically, 2.2 parts by mass of organic peroxide are used. A wiper rubber of Comparative Example 3 was produced using a wiper rubber having the same compounding amount as Example 1 in other respects. In Comparative Example 3, the sulfur content is 0% and the organic peroxide content is 1.32% by mass with respect to the rubber composition.

[0043] [Table 1]

[0044] --Test evaluation-- The processability, permanent deformation and modulus change rate were evaluated for the wiper rubbers thus prepared in Examples 1 to 5 and Comparative Examples 1 to 3. The measurement results are shown in Table 1.

[0045] (About workability) The processability of the wiper rubber material is evaluated by the presence or absence of the phenomenon in which vulcanization begins during the mixing and rolling process of the rubber composition. If the phenomenon occurs, it is rated as poor (indicated by x), and if it is suppressed, it is rated as good (indicated by a single circle ○).

[0046] Mold moldability is an evaluation of the time required for molding using a vulcanizing press after kneading and rolling, and a shorter time is preferable. If molding is completed sufficiently after 10 minutes of treatment at 165°C, it is rated as good (○), and if molding is not completed sufficiently under these conditions, it is rated as poor (×).

[0047] The overall processability is indicated by a circle when both the wiper rubber material processability and the mold molding processability are good, and an x ​​when either one is poor.

[0048] (Characteristics of the manufactured wiper rubber) For permanent deformation, a tensile force was applied to the test piece, stretching it 100%, and then the test piece was kept in an 80°C environment for 72 hours. The tensile force was then released and the change in length from before the test was measured. The evaluation was based on the following criteria: less than 13% is especially desirable (shown as a double circle ◎), 13% to less than 15% is desirable (shown as a single circle ○), and 15% or more is undesirable (shown as an x).

[0049] The test piece used for evaluating the permanent deformation was prepared by cutting the rear rubber (holding portion 11) of the wiper rubber 10 below it (see FIG. 1) to have a length of 100 mm.

[0050] The rate of change in modulus was measured by measuring the rate of change in 60% modulus before and after a test in which the material was held in an environment of 80° C. for 72 hours. The evaluation was based on the following criteria: greater than -7% and less than 7% was particularly desirable (shown as double circle ◎), 7% or more and less than 10%, and greater than -10% and less than -7% were desirable (shown as single circle ○), and 10% or more and -10% or less were undesirable (shown as x).

[0051] The test specimen used for evaluating the modulus change rate was prepared by cutting out the back rubber of the wiper rubber 10 in the same manner as the test specimen for evaluating the permanent deformation, and further removing the protrusions remaining on the cut side by polishing. The test specimen was 100 mm long.

[0052] (evaluation) In Examples 1 to 5, in which sulfur and a vulcanization accelerator are used in combination with an organic peroxide, both the wiper rubber material processability and the mold molding processability are excellent. In contrast, in Comparative Examples 1 and 2, in which only sulfur and a vulcanization accelerator are used, the mold molding processability is excellent but the wiper rubber material processability is poor. In Comparative Example 3, in which only an organic peroxide is used, the wiper rubber material processability is excellent but the mold molding processability is poor.

[0053] Next, in the case of Examples 1 to 5, the permanent deformation and the rate of change in modulus are all desirable (◯) or particularly desirable (◎) values. In contrast, in the case of Comparative Examples 1 to 3, the rate of change in modulus is all undesirable (×) values. As for the permanent deformation, Comparative Example 2 is a particularly desirable (◎) value, but Comparative Examples 1 and 3 are undesirable (×) values.

[0054] In Comparative Examples 1 and 2, only sulfur and a vulcanization accelerator were used, and no organic peroxide was used. In Comparative Example 3, on the other hand, only an organic peroxide was used, and no sulfur or vulcanization accelerator was used.

[0055] In Example 5, both an organic peroxide and sulfur and a vulcanization accelerator are used, but the vulcanization accelerator used is one that does not have a thiocarbonyl group.

[0056] From the above comparison, it is found that by using both sulfur and a vulcanization accelerator, and an organic peroxide for vulcanization, a wiper rubber having excellent processability can be obtained.

[0057] Furthermore, it is preferable to use a substance having a thiocarbonyl group (e.g., thiuram-based or dithiocarbamic acid-based) as a vulcanization accelerator. This makes it possible to realize particularly desirable values ​​for both the permanent deformation and the rate of change in modulus due to thermal history. Such a wiper rubber has, for example, improved reversibility during use and exhibits excellent wiping performance.

[0058] In addition, by using carbon black with an iodine adsorption of 25 g / kg or more, the ozone resistance can be improved in addition to the above-mentioned improvement in abrasion resistance. Since wipers are often used outdoors, ozone resistance is an important characteristic. In addition, by using carbon black with an iodine adsorption of 60 g / kg or less, in addition to the above-mentioned dispersibility, the loss coefficient at around room temperature is reduced, which has a good effect on the reversibility of the wiper rubber. For the above reasons, it is desirable for the iodine adsorption to be 24 g / kg or more and 60 g / kg or less.

[0059] The effect of the present disclosure is remarkable in rubbers to which either vulcanization with sulfur and a vulcanization accelerator or vulcanization with an organic peroxide can be applied alone. For example, in the case of a mixture of natural rubber and chloroprene rubber, which is generally used as a wiper rubber, no improvement in modulus change rate was observed. [Industrial Applicability]

[0060] According to the technology of the present disclosure, since the permanent deformation and the modulus change rate are improved, the material is useful as a wiper rubber for use in automobiles, etc. [Explanation of symbols]

[0061] 10 Wiper rubber 11 Holding part 12 Neck 13 Lip 14 Edge section

Claims

1. A wiper rubber comprising a rubber composition containing a rubber component and carbon black, The rubber component is made of only natural rubber, The rubber composition is vulcanized by using sulfur, a vulcanization accelerator, and an organic peroxide in combination, A wiper rubber, characterized in that a ratio of the content of the sulfur to the content of the organic peroxide in the rubber composition is 0.1 or more and 2.0 or less.

2. In the wiper rubber of claim 1, The wiper rubber is characterized in that the vulcanization accelerator has a thiocarbonyl group.

3. The wiper rubber according to claim 1 or 2, The carbon black has an iodine adsorption amount of 24 g / kg or more and 60 g / kg or less.

4. In any one of claims 1 to 3, A wiper rubber, characterized in that a wiping portion of the wiper rubber for wiping an object to be wiped is subjected to a surface treatment for reducing a coefficient of friction.

5. In the wiper rubber of claim 1, The content of the organic peroxide in the rubber composition is 0.2 mass% or more and 6.5 mass% or less, The wiper rubber is characterized in that the content of the sulfur in the rubber composition is 0.1 mass % or more and 1.7 mass % or less.

Citation Information

Patent Citations

  • Rubber composition

    JP1986293240A

  • Wiper blade rubber

    JP1996319375A

  • Rubber composition, molded article of the same and wiper blade by using the same

    JP2009007395A

  • Wiper blade rubber

    JP2019064281A

  • Coating agent for wiper rubber and wiper rubber

    JP2020163981A