Method for producing solid electrolyte

A novel manufacturing method for glass ceramic solid electrolytes using complex crystals formed from lithium, sulfur, and halogen atoms with a complexing agent addresses the conductivity limitations of conventional methods, achieving high ionic conductivity through improved dispersity and solvent removal.

JP7584354B2Active Publication Date: 2024-11-15IDEMITSU KOSAN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021089652
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-27
Filing Date
2021-05-27
Publication Date
2024-11-15
Estimated Expiration
2041-05-27

AI Technical Summary

Technical Problem

Conventional methods for manufacturing solid electrolytes, particularly those involving mechanical milling, struggle to achieve high ionic conductivity, and existing liquid phase methods face challenges in maintaining component dispersity and solvent removal, leading to reduced conductivity.

Method used

A novel manufacturing method involving the formation of a complex crystal by mixing raw materials containing lithium, sulfur, phosphorus, and halogen atoms with a complexing agent, followed by drying and complex decomposition to obtain a glass ceramic solid electrolyte with high ionic conductivity.

Benefits of technology

The method enables the production of a glass ceramic solid electrolyte with enhanced ionic conductivity by suppressing elution and aggregation of components, resulting in a more uniform and dispersed electrolyte structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584354000006
    Figure 0007584354000006
  • Figure 0007584354000007
    Figure 0007584354000007
  • Figure 0007584354000008
    Figure 0007584354000008
Patent Text Reader

Abstract

To provide a manufacturing method of a novel glass ceramic solid electrolyte which obtains a solid electrolyte having high ionic conductivity by using a liquid phase method.SOLUTION: A method of manufacturing a glass ceramic solid electrolyte comprises: mixing a raw material inclusion containing a lithium atom, a sulfur atom, a phosphorus atom and a halogen atom, and a complex agent to obtain a slurry of an electrolyte precursor containing complex crystal containing the complex agent, lithium atom, sulfur atom, phosphorous atom and halogen atom as constituent elements; drying the slurry of the electrolyte precursor; and performing complex decomposition of the electrolyte precursor obtained by drying to obtain an amorphous solid electrolyte having an intensity ratio Ic / Is of a diffraction peak intensity Ic and an intensity Is of a reference sample of LiX complex (in the formula, X represents a halogen) is 0.02 or smaller, or a GC solid electrolyte having an intensity ratio Ix / Igc of a diffraction peak intensity Ix of the LiX and a diffraction peak intensity Igc of the glass ceramic is 0.5 or smaller.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a solid electrolyte. [Background technology]

[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Conventionally, electrolytes containing flammable organic solvents have been used in batteries used for such purposes, but by making the battery fully solid-state, flammable organic solvents are not used in the battery, safety devices can be simplified, and manufacturing costs and productivity are excellent, so that batteries in which the electrolyte is replaced with a solid electrolyte layer are being developed.

[0003] The manufacturing methods of the solid electrolyte used in the solid electrolyte layer are roughly divided into a solid-phase method and a liquid-phase method. The liquid-phase method is further divided into a homogeneous method in which the solid electrolyte material is completely dissolved in a solvent, and a heterogeneous method in which the solid electrolyte material is not completely dissolved and goes through a solid-liquid coexistence suspension. For example, as a solid-phase method, a method is known in which raw materials such as lithium sulfide and diphosphorus pentasulfide are subjected to mechanical milling treatment using a device such as a ball mill or a bead mill, and then heated as necessary to produce an amorphous or crystalline solid electrolyte (see, for example, Patent Document 1). According to this method, a solid electrolyte is obtained by applying mechanical stress to raw materials such as lithium sulfide to promote the reaction between solids. On the other hand, as a homogeneous liquid phase method, a method in which a solid electrolyte is dissolved in a solvent and reprecipitated is known (see, for example, Patent Document 2), and as a heterogeneous method, a method in which a solid electrolyte raw material such as lithium sulfide is reacted in a solvent containing a polar aprotic solvent is known (see Patent Documents 3 and 4, and Non-Patent Document 1). For example, Patent Document 4 discloses a method for producing a solid electrolyte with a Li4PS4I structure, which includes a step of using dimethoxyethane (DME) and combining it with a Li3PS4 structure to obtain Li3PS4·DME. The ionic conductivity of the obtained solid electrolyte is 5.5×10 -5 S / cm (Calcium doped: 3.9 × 10-4 In recent years, the liquid phase method has been attracting attention as a method that can be easily and mass-produced in addition to its versatility and applicability in order to commercialize all-solid-state batteries. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 159667 Brochure [Patent Document 2] JP 2014-191899 A [Patent Document 3] International Publication No. 2014 / 192309 Brochure [Patent Document 4] International Publication No. 2018 / 054709 Brochure [Non-patent literature]

[0005] [Non-Patent Document 1] “CHEMISTRY OF MATERIALS”, 2017, No. 29, pp. 1830-1835 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the conventional solid-phase method involving mechanical milling and the like is centered on solid-phase reactions, and can easily obtain a solid electrolyte with high purity, thereby realizing high ionic conductivity, whereas the liquid-phase method has the problem that it is difficult to achieve high ionic conductivity compared to the solid-phase synthesis method. In addition, even if the above-mentioned complexation step is performed, the solid electrolyte is obtained as a crystal classified as a tetragonal crystal, as in Patent Document 4, so that the ionic conductivity is not sufficiently high for the required characteristics, and further improvement is required, and optimization of the manufacturing method is required.

[0007] The present invention has been made in view of the above circumstances, and has an object to provide a novel method for producing a glass-ceramic solid electrolyte having high ionic conductivity by using a liquid phase method. [Means for solving the problem]

[0008] As a result of intensive research into solving the above problems, the present inventors have found that the problems can be solved by the following invention.

[0009] 1. A homogeneous electrolyte precursor can be obtained by mixing a raw material containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms with a complexing agent to obtain a slurry of an electrolyte precursor containing a complex crystal containing the complexing agent, lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms as components, and a glass-ceramic solid electrolyte having high ionic conductivity can be obtained. 2. By drying the electrolyte precursor slurry, a powder of the electrolyte precursor is obtained, and a glass-ceramic solid electrolyte with high ionic conductivity can be obtained.

[0010] 3. The electrolyte precursor obtained by drying is decomposed to obtain an amorphous solid electrolyte in which the intensity ratio Ic / Is of the diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) to the intensity Is of a standard sample is 0.02 or less, or a GC solid electrolyte in which the intensity ratio Ix / Igc of the diffraction peak intensity Ix of LiX to the diffraction peak intensity Igc of a glass ceramic is 0.5 or less, thereby making it possible to obtain a glass ceramic solid electrolyte having high ionic conductivity.

[0011] That is, the present invention provides [1] to

[16] . [1] A method for producing a glass-ceramic solid electrolyte, comprising: mixing a raw material containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms with a complexing agent to obtain a slurry of an electrolyte precursor containing a complex crystal containing the complexing agent, lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms as constituent components; drying the electrolyte precursor slurry; and complexing the electrolyte precursor obtained by the drying to obtain an amorphous solid electrolyte in which an intensity ratio Ic / Is of a diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) to an intensity Is of a standard sample is 0.02 or less, or a solid electrolyte in which an intensity ratio Ix / Igc of a diffraction peak intensity Ix of LiX to a diffraction peak intensity Igc of a glass ceramic is 0.5 or less (hereinafter referred to as a GC solid electrolyte).

[0012] [2] The method for producing a glass-ceramic solid electrolyte according to [1], wherein the drying step includes removing the complexing agent, which is a liquid. [3] The method for producing a glass-ceramic solid electrolyte according to [1] or [2], wherein the decomplexation comprises removing the complexing agent, which is a component of the complex crystal. [4] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [3], further comprising heating.

[0013] [5] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [4], wherein after the complex decomposition, the amorphous solid electrolyte or the GC-modified solid electrolyte is subjected to at least one mechanical treatment selected from crushing and granulation. [6] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [5], wherein the amount of the complexing agent contained in the amorphous solid electrolyte or the GC solid electrolyte is adjusted to 15 mass % or less by the complexation. [7] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [6], wherein a vibration dryer is used in the complex decomposition.

[0014] [8] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [7], wherein the drying is fluidized drying using a medium. [9] A method for producing a glass-ceramic solid electrolyte according to any one of [1] to [8], comprising, as a raw material component, at least one selected from the group consisting of lithium sulfide, lithium halide, phosphorus sulfide, phosphorus halide, thiophosphoryl halide, and halogen molecules.

[10] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to [9], wherein the electrolyte precursor slurry further contains a solvent, and the solvent contains a solvent that does not dissolve the raw material inclusions, the complexing agent, and the electrolyte precursor.

[0015]

[11] The method for producing a glass-ceramic solid electrolyte according to

[10] , wherein 5 to 50 mL of the solvent is used per 1 g of the total mass of the raw material ingredients.

[12] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to

[11] , wherein the complexing agent contains a compound having a heteroatom.

[13] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to

[12] , wherein the complexing agent includes a compound having an amino group.

[0016]

[14] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to

[13] , wherein the complexing agent includes a compound having at least two tertiary amino groups in the molecule.

[15] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to

[14] , wherein the solid electrolyte contains a thiolicon region II type crystal structure.

[16] The method for producing a glass-ceramic solid electrolyte according to any one of [1] to

[15] , wherein the solid electrolyte does not have diffraction peaks at 2θ=17.5° and 26.1° corresponding to crystalline Li3PS4 in X-ray diffraction measurement using CuKα radiation. Effect of the Invention

[0017] According to the present invention, a glass-ceramic solid electrolyte having high ionic conductivity can be provided by using a liquid phase method. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a flow diagram illustrating an example of a preferred embodiment of the manufacturing method of the present embodiment. [Diagram 2] FIG. 2 is a conceptual diagram of a drying device. [Diagram 3] 1 shows X-ray diffraction spectra of an electrolyte precursor, an amorphous solid electrolyte, and a glass ceramic solid electrolyte obtained in Example 1. [Figure 4] 1 shows X-ray diffraction spectra of the amorphous solid electrolytes obtained in Examples 1 and 2 and Comparative Examples 1 to 3. [Diagram 5] 1 shows X-ray diffraction spectra of the glass ceramic solid electrolytes obtained in Examples 1 and 2 and Comparative Examples 1 and 2. [Figure 6] 1 shows X-ray diffraction spectra of raw materials used in the examples. [Figure 7] 1 is an X-ray diffraction spectrum of the solid electrolyte obtained in Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention (hereinafter, sometimes referred to as "the present embodiment") will be described. In this specification, the upper and lower limit values ​​of a numerical range expressed by "greater than or equal to", "less than or equal to", and "to" are values ​​that can be arbitrarily combined, and the numerical values ​​in the examples can also be used as the upper and lower limit values.

[0020] [Method for producing glass-ceramic solid electrolyte] The present embodiment is a method for producing a glass ceramic solid electrolyte, mixing a raw material containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms with a complexing agent to obtain a slurry of an electrolyte precursor containing a complex crystal containing the complexing agent, lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms as constituent components; drying the electrolyte precursor slurry; and complexing the electrolyte precursor obtained by the drying to obtain an amorphous solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms as constituent components, and having an intensity ratio Ic / Is of 0.02 or less between a diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) and an intensity Is of a standard sample, or a solid electrolyte having an intensity ratio Ix / Igc of 0.5 or less between a diffraction peak intensity Ix of LiX and a diffraction peak intensity Igc of a glass ceramic (hereinafter referred to as a GC solid electrolyte).

[0021] The inventors of the present invention found that the problem of ionic conductivity in the liquid phase method is due to the dispersibility and uniformity of the solid electrolyte components accompanying the dissolution and aggregation of the components, and thus came to the invention. For example, in the homogeneous method, the raw materials and solid electrolyte are completely dissolved once, so that the components can be uniformly dispersed in the liquid. However, in the subsequent precipitation process, precipitation proceeds according to the solubility specific to each component, so it is extremely difficult to precipitate the components while maintaining their dispersed state. As a result, each component separates and precipitates. In addition, in the homogeneous method, the affinity between the solvent and lithium becomes too strong, so that the solvent is difficult to remove even when dried after precipitation. For these reasons, the homogeneous method has a problem that the ionic conductivity of the solid electrolyte is significantly reduced.

[0022] In addition, in the heterogeneous solid-liquid coexistence method, it was found that, since a part of the solid electrolyte is dissolved, separation occurs due to the elution of specific components such as halogen atoms, and when the solvent becomes difficult to remove as in the homogeneous method, it is difficult to obtain a desired solid electrolyte. Furthermore, in the heterogeneous method, it was found that the elution or aggregation of specific components in the electrolyte precursor is likely to occur during the so-called complex decomposition, which is the removal of the complexing agent contained in the electrolyte precursor.

[0023] Furthermore, as disclosed in Patent Document 4, there is a production method in which a solid electrolyte having a crystalline structure is directly produced by complex decomposition, but the ionic conductivity of the solid electrolyte is not sufficiently high. In this embodiment, the raw material ingredients are mixed with a complex to obtain a slurry of an electrolyte precursor, the slurry of the electrolyte precursor is then dried, and the dried slurry of the electrolyte precursor is further decomposed. After the decomposition, an amorphous solid electrolyte is obtained in which the intensity ratio Ic / Is of the diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) to the intensity Is of a standard sample is 0.02 or less by XRD. This makes it possible to obtain a GC solid electrolyte in which the intensity ratio Ix / Igc of the diffraction peak intensity Ix of LiX to the diffraction peak intensity Igc of a glass ceramic is 0.5 or less, and a solid electrolyte exhibiting high ionic conductivity can be produced.

[0024] A flow diagram showing an outline of the manufacturing method of this embodiment is shown in Figure 1. The raw material ingredients and the complexing agent are mixed to obtain a slurry containing an electrolyte precursor, which is then dried to obtain a powdered electrolyte precursor, which is then heated (decomplexation) to obtain a decomposition product (amorphous solid electrolyte) or, depending on the heating conditions, a GC solid electrolyte in which part or all of the amorphous solid electrolyte is converted to glass ceramics. By mixing the raw material ingredients with a complexing agent to form an electrolyte precursor containing complex crystals, specific components such as halogen atoms are incorporated, and then complexed, which suppresses the elution and aggregation of the specific components. The intensity ratio Ic / Is between the diffraction peak intensity Ic of the LiX complex in the amorphous solid electrolyte and the intensity Is of the standard sample can be set to 0.02 or less, or the intensity ratio Ix / Igc between the diffraction peak intensity Ix of the LiX in the GC solid electrolyte and the diffraction peak intensity Igc of the glass ceramics can be set to 0.5 or less, so that a homogeneous complex decomposition product can be obtained, and a solid electrolyte with high ionic conductivity can be obtained. Moreover, by obtaining such an amorphous solid electrolyte, the content of residual halogen atoms, sulfur atoms, etc. can be reduced, and a solid electrolyte having high ionic conductivity can be obtained.

[0025] In this specification, the term "solid electrolyte" refers to an electrolyte that maintains a solid state under a nitrogen atmosphere at 25° C. The solid electrolyte in this embodiment is a solid electrolyte that contains lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms and has ionic conductivity due to the lithium atoms. As will be described in more detail later, the glass-ceramic solid electrolyte of the present application may be entirely crystalline, or may be partially crystalline and the remaining portion amorphous.

[0026] In this specification, the crystalline solid electrolyte is a solid electrolyte in which a peak derived from the solid electrolyte is observed in the X-ray diffraction pattern in the X-ray diffraction measurement, and it does not matter whether or not there is a peak derived from the raw material of the solid electrolyte. That is, the crystalline solid electrolyte includes a crystal structure derived from the solid electrolyte, and a part of the crystal structure may be derived from the solid electrolyte, or the whole of the crystal structure may be derived from the solid electrolyte. And, as long as the crystalline solid electrolyte has the above-mentioned X-ray diffraction pattern, it may include an amorphous solid electrolyte in a part of it. Therefore, the crystalline solid electrolyte includes so-called glass ceramics obtained by heating an amorphous solid electrolyte to a crystallization temperature or higher. However, the glass ceramic solid electrolyte is obtained via an amorphous solid electrolyte. For example, when the electrolyte precursor described later is heated, it crystallizes via an amorphous solid electrolyte, that is, it becomes a glass ceramic solid electrolyte, but when the electrolyte precursor is heated, it crystallizes without passing through an amorphous solid electrolyte, but it is not a glass ceramic solid electrolyte.

[0027] In this specification, the term "amorphous solid electrolyte" refers to an electrolyte that exhibits a halo pattern in which no peaks other than those derived from the material (including complexes derived from a complexing agent) are observed in an X-ray diffraction pattern in an X-ray diffraction measurement, and does not matter whether or not there are peaks derived from the raw materials of the solid electrolyte.

[0028] (Raw material content) In this embodiment, the raw material contains a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom. Examples of raw materials contained in the raw material content include compounds containing at least one of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms. More specifically, lithium sulfide; lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide (LiX, where X represents a halogen); phosphorus sulfides such as diphosphorus trisulfide (P2S3) and diphosphorus pentasulfide (P2S5); phosphorus halides such as various phosphorus fluorides (PF3, PF5), various phosphorus chlorides (PCl3, PCl5, P2Cl4), various phosphorus bromides (PBr3, PBr5), and various phosphorus iodides (PI3, P2I4); non-phosphorus halides obtained from lithium sulfide and phosphorus sulfide and having a PS4 structure as a molecular structure. Examples of the raw material include a solid electrolyte such as crystalline amorphous Li3PS4 or crystalline Li3PS4; a thiophosphoryl halide such as thiophosphoryl fluoride (PSF3), thiophosphoryl chloride (PSCl3), thiophosphoryl bromide (PSBr3), thiophosphoryl iodide (PSI3), thiophosphoryl fluoride dichloride (PSCl2F), and thiophosphoryl fluoride dibromide (PSBr2F); and a halogen element such as fluorine (F2), chlorine (Cl2), bromine (Br2), or iodine (I2), preferably chlorine (Cl2), bromine (Br2), or iodine (I2), and more preferably bromine (Br2) or iodine (I2).

[0029] The raw material further preferably contains at least one selected from lithium sulfide, lithium halide, phosphorus sulfide, phosphorus halide, and halogen molecules, and the compound containing a halogen atom further preferably contains lithium halide (LiX (wherein X represents a halogen)), and further preferably contains lithium sulfide, lithium halide, and phosphorus sulfide. In addition, the raw material content is preferably a compound consisting of two kinds of atoms such as lithium sulfide, lithium halide and phosphorus sulfide, rather than a solid electrolyte such as Li3PS4 produced by reacting lithium sulfide and phosphorus sulfide. For example, an electrolyte precursor obtained by mixing a solid electrolyte such as Li3PS4 and a lithium halide together with a complexing agent contains LiX and LiX complexes (wherein X represents a halogen) after complex decomposition described below, and contains halogen atoms not incorporated in the solid electrolyte, etc., and is preferably lithium sulfide, lithium halide and phosphorus sulfide from the viewpoint of improving the ionic conductivity of the resulting crystalline solid electrolyte.

[0030] Examples of the raw material containing substances other than those mentioned above include raw materials containing at least one atom selected from the above four types of atoms and containing atoms other than the four types of atoms, more specifically, lithium compounds such as lithium oxide, lithium hydroxide, and lithium carbonate; alkali metal sulfides such as sodium sulfide, potassium sulfide, rubidium sulfide, and cesium sulfide; metal sulfides such as silicon sulfide, germanium sulfide, boron sulfide, gallium sulfide, tin sulfide (SnS, SnS2), aluminum sulfide, and zinc sulfide; phosphate compounds such as sodium phosphate and lithium phosphate; halides of alkali metals other than lithium, such as sodium iodide, sodium fluoride, sodium chloride, and sodium bromide; metal halides such as aluminum halides, silicon halides, germanium halides, arsenic halides, selenium halides, tin halides, antimony halides, tellurium halides, and bismuth halides; and phosphorus oxyhalides such as phosphorus oxychloride (POCl3) and phosphorus oxybromide (POBr3).

[0031] The lithium sulfide used in this embodiment is preferably in the form of particles. The average particle size of lithium sulfide particles (D 50 In this specification, the average particle size (D 50) is the particle size at which the particle size distribution cumulative curve is accumulated from the smallest particle size to 50% of the total, and the volume distribution is the average particle size that can be measured using, for example, a laser diffraction / scattering particle size distribution measuring device. Among the above-mentioned examples of raw materials, the solid raw materials preferably have an average particle size similar to that of the lithium sulfide particles, that is, within the same range as the average particle size of the lithium sulfide particles.

[0032] When lithium sulfide, diphosphorus pentasulfide, and lithium halide are used as the raw material ingredients, the ratio of lithium sulfide to the total of lithium sulfide and diphosphorus pentasulfide is preferably 70 to 80 mol%, more preferably 72 to 78 mol%, and even more preferably 74 to 76 mol%, from the viewpoint of obtaining higher chemical stability and higher ionic conductivity. When lithium sulfide, diphosphorus pentasulfide, lithium halide, and other raw materials used as necessary are used, the content of lithium sulfide and diphosphorus pentasulfide relative to the total of these is preferably 60 to 100 mol%, more preferably 65 to 90 mol%, and even more preferably 70 to 80 mol%. Furthermore, when lithium bromide and lithium iodide are used in combination as the lithium halide, from the viewpoint of improving ion conductivity, the ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 to 99 mol%, more preferably 20 to 90 mol%, even more preferably 40 to 80 mol%, and particularly preferably 50 to 70 mol%.

[0033] In the case where a halogen element is used as a raw material content, lithium sulfide and diphosphorus pentasulfide are used, the ratio of the number of moles of lithium sulfide excluding the same number of moles of lithium sulfide as the halogen element to the total number of moles of lithium sulfide and diphosphorus pentasulfide excluding the same number of moles of lithium sulfide as the halogen element is preferably within the range of 60 to 90%, more preferably within the range of 65 to 85%, even more preferably within the range of 68 to 82%, even more preferably within the range of 72 to 78%, and particularly preferably within the range of 73 to 77%. This is because higher ion conductivity can be obtained at these ratios. From the same viewpoint, when lithium sulfide, diphosphorus pentasulfide, and a halogen element are used, the content of the halogen element relative to the total amount of lithium sulfide, diphosphorus pentasulfide, and a halogen element is preferably 1 to 50 mol%, more preferably 2 to 40 mol%, even more preferably 3 to 25 mol%, and even more preferably 3 to 15 mol%.

[0034] When lithium sulfide, diphosphorus pentasulfide, a halogen element, and a lithium halide are used, the content of the halogen element (α mol %) and the content of the lithium halide (β mol %) relative to the total amount thereof preferably satisfy the following formula (2), more preferably satisfy the following formula (3), even more preferably satisfy the following formula (4), and even more preferably satisfy the following formula (5). 2≦2α+β≦100…(2) 4≦2α+β≦80 …(3) 6≦2α+β≦50 …(4) 6≦2α+β≦30 …(5)

[0035] When two types of halogens are used as simple substances, the molar number of one halogen atom in the substance is A1 and the molar number of the other halogen atom in the substance is A2, and A1:A2 is preferably 1 to 99:99 to 1, more preferably 10:90 to 90:10, even more preferably 20:80 to 80:20, and even more preferably 30:70 to 70:30.

[0036] Furthermore, when the two types of halogen elements are bromine and iodine, the molar number of bromine is B1 and the molar number of iodine is B2, then B1:B2 is preferably 1 to 99:99 to 1, more preferably 15:85 to 90:10, even more preferably 20:80 to 80:20, even more preferably 30:70 to 75:25, and particularly preferably 35:65 to 75:25.

[0037] (Complexing Agent) In this embodiment, a complexing agent is used. In this specification, the complexing agent means a substance capable of forming a complex with lithium atoms, and has a property of promoting the formation of an electrolyte precursor containing a complex crystal by reacting with sulfides, halides, etc. containing lithium atoms contained in the raw material. By using a complexing agent to form an electrolyte precursor containing complex crystals, it is possible to suppress the elution of specific components such as halogen molecules, which was a cause of reduced conductivity in conventional technologies, and to obtain a glass-ceramic solid electrolyte with high ionic conductivity.

[0038] The complexing agent can be used without any particular limitation as long as it has the above-mentioned properties, and it is preferable to include a compound having an atom having a high affinity with a lithium atom, such as a nitrogen atom, an oxygen atom, a chlorine atom, or the like, and more preferable to include a compound having a group containing such a heteroatom, because such a heteroatom or group containing such a heteroatom can be coordinated (bonded) with lithium. The complexing agent is considered to have a property that the heteroatom in its molecule has a high affinity with lithium atoms, and is likely to form an aggregate by bonding with a lithium-containing structure such as Li3PS4, which typically contains a PS4 structure, and a raw material containing lithium such as lithium halide, which exists as the main structure in the solid electrolyte obtained by the manufacturing method of this embodiment. Therefore, by mixing the above-mentioned raw material content with the complexing agent, a lithium-containing structure such as the PS4 structure or an aggregate via the complexing agent, a raw material containing lithium such as lithium halide or an aggregate via the complexing agent will be evenly present, and an electrolyte precursor in which specific components such as halogen atoms are more dispersed and fixed will be obtained, and as a result, it is considered that a glass ceramic solid electrolyte with high ionic conductivity will be obtained.

[0039] Therefore, it is preferable to have at least two heteroatoms capable of coordinating (bonding) in the molecule, and more preferable to have a group containing at least two heteroatoms in the molecule. By having a group containing at least two heteroatoms in the molecule, a lithium-containing structure such as Li3PS4 containing a PS4 structure and a lithium-containing raw material such as lithium halide can be bonded through at least two heteroatoms in the molecule, so that the halogen atoms are more dispersed and fixed in the electrolyte precursor, resulting in a glass ceramic solid electrolyte with high ionic conductivity and suppressed generation of hydrogen sulfide. In addition, among heteroatoms, nitrogen atoms are preferable, and as a group containing a nitrogen atom, an amino group is preferable, that is, the complexing agent preferably contains a compound having an amino group.

[0040] There are no particular limitations on the amine compound having an amino group in the molecule, as long as it can promote the formation of the electrolyte precursor, but it is preferable that the complexing agent contains a compound having at least two tertiary amino groups in the molecule. By having such a structure, when the raw material contents are mixed with a complexing agent, the lithium-containing structure such as Li3PS4 having a PS4 structure and the lithium-containing raw material such as lithium halide can be bonded via at least two nitrogen atoms in the molecule, so that the halogen atoms are more dispersed and fixed in the electrolyte precursor, resulting in a glass ceramic solid electrolyte with high ionic conductivity.

[0041] Examples of such amine compounds include aliphatic amines, alicyclic amines, heterocyclic amines, and aromatic amines, and these can be used alone or in combination of two or more kinds.

[0042] More specifically, representative and preferred examples of the aliphatic amine include aliphatic primary diamines such as ethylenediamine, diaminopropane, and diaminobutane; aliphatic secondary diamines such as N,N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyldiaminopropane, and N,N'-diethyldiaminopropane; and aliphatic tertiary diamines such as N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N',N'-tetramethyldiaminopropane, N,N,N',N'-tetraethyldiaminopropane, N,N,N',N'-tetramethyldiaminobutane, N,N,N',N'-tetramethyldiaminopentane, and N,N,N',N'-tetramethyldiaminohexane. In the examples given in this specification, for example, in the case of diaminobutane, unless otherwise specified, all isomers are included, such as isomers relating to the position of the amino group, such as 1,2-diaminobutane, 1,3-diaminobutane, and 1,4-diaminobutane, as well as linear and branched isomers for butane. The number of carbon atoms in the aliphatic amine is preferably 2 or more, more preferably 4 or more, and even more preferably 6 or more, with the upper limit being preferably 10 or less, more preferably 8 or less, and even more preferably 7 or less. The number of carbon atoms in the hydrocarbon group of the aliphatic hydrocarbon group in the aliphatic amine is preferably 2 or more, and the upper limit being preferably 6 or less, more preferably 4 or less, and even more preferably 3 or less.

[0043] Representative and preferred examples of the alicyclic amine include alicyclic primary diamines such as cyclopropanediamine and cyclohexanediamine; alicyclic secondary diamines such as bisaminomethylcyclohexane; and alicyclic tertiary diamines such as N,N,N',N'-tetramethyl-cyclohexanediamine and bis(ethylmethylamino)cyclohexane. Representative and preferred examples of the heterocyclic amine include heterocyclic primary diamines such as isophoronediamine; heterocyclic secondary diamines such as piperazine and dipiperidylpropane; and heterocyclic tertiary diamines such as N,N-dimethylpiperazine and bismethylpiperidylpropane. The number of carbon atoms in the alicyclic amine and heterocyclic amine is preferably 3 or more, more preferably 4 or more, and the upper limit is preferably 16 or less, more preferably 14 or less.

[0044] Representative and preferred examples of the aromatic amine include aromatic primary diamines such as phenyldiamine, tolylenediamine, and naphthalenediamine; aromatic secondary diamines such as N-methylphenylenediamine, N,N'-dimethylphenylenediamine, N,N'-bismethylphenylphenylenediamine, N,N'-dimethylnaphthalenediamine, and N-naphthylethylenediamine; and aromatic tertiary diamines such as N,N-dimethylphenylenediamine, N,N,N',N'-tetramethylphenylenediamine, N,N,N',N'-tetramethyldiaminodiphenylmethane, and N,N,N',N'-tetramethylnaphthalenediamine. The aromatic amine has preferably 6 or more, more preferably 7 or more, and even more preferably 8 or more, and the upper limit is preferably 16 or less, more preferably 14 or less, and even more preferably 12 or less.

[0045] The amine compound used in the present embodiment may be substituted with a substituent such as an alkyl group, an alkenyl group, an alkoxyl group, a hydroxyl group, or a cyano group, or with a halogen atom. Although diamines have been given as specific examples, it goes without saying that the amine compounds that can be used in this embodiment are not limited to diamines, and include, for example, aliphatic monoamines corresponding to various diamines such as trimethylamine, triethylamine, ethyldimethylamine, and the above-mentioned aliphatic diamines; piperidine compounds such as piperidine, methylpiperidine, and tetramethylpiperidine; pyridine compounds such as pyridine and picoline; morpholine compounds such as morpholine, methylmorpholine, and thiomorpholine; imidazole compounds such as imidazole and methylimidazole; and the above-mentioned alicyclic diamines. In addition to monoamines such as alicyclic monoamines such as the corresponding monoamines; heterocyclic monoamines corresponding to the above heterocyclic diamines; and aromatic monoamines corresponding to the above aromatic diamines, polyamines having three or more amino groups, such as diethylenetriamine, N,N',N''-trimethyldiethylenetriamine, N,N,N',N'',N''-pentamethyldiethylenetriamine, triethylenetetramine, N,N'-bis[(dimethylamino)ethyl]-N,N'-dimethylethylenediamine, hexamethylenetetramine, and tetraethylenepentamine, can also be used.

[0046] Among the above, from the viewpoint of obtaining higher ion conductivity, a tertiary amine having a tertiary amino group as an amino group is preferable, a tertiary diamine having two tertiary amino groups is more preferable, a tertiary diamine having two tertiary amino groups at both ends is even more preferable, and an aliphatic tertiary diamine having a tertiary amino group at both ends is even more preferable. In the above amine compounds, the aliphatic tertiary diamine having a tertiary amino group at both ends is preferably tetramethylethylenediamine, tetraethylethylenediamine, tetramethyldiaminopropane, or tetraethyldiaminopropane, and considering the ease of availability, etc., tetramethylethylenediamine or tetramethyldiaminopropane is preferable.

[0047] As a complexing agent other than the amine compounds, for example, a compound having a group containing a heteroatom such as an oxygen atom or a halogen atom such as a chlorine atom has a high affinity with lithium atoms and can be mentioned as a complexing agent other than the above amine compounds. In addition, a compound having a group other than an amino group, such as a nitro group or an amide group, containing a nitrogen atom as a heteroatom can also provide the same effect.

[0048] Examples of the other complexing agents include alcohol solvents such as ethanol and butanol; ester solvents such as ethyl acetate and butyl acetate; aldehyde solvents such as formaldehyde, acetaldehyde and dimethylformamide; ketone solvents such as acetone, methyl ethyl ketone and cyclohexanone; ether solvents such as diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, diethoxyethane, cyclopentyl methyl ether, tert-butyl methyl ether and anisole; 2-methoxyethyl acetate, 2-ethoxyethyl acetate (ethylene glycol acetate), 2-methoxy-1-methylethyl acetate, and the like. Examples of suitable solvents include glycol ester solvents such as ethyl ether, 2-ethoxy-methylethyl acetate, 2-(2-ethoxyethoxy)ethyl acetate, (2-acetoxyethoxy)methyl acetate, 1-methyl-2-ethoxyethyl acetate (propylene glycol monoethyl ether acetate), ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, and 2-methoxyethyl 3-(2-methoxyethoxy)propionate; halogen atom-containing aromatic hydrocarbon solvents such as trifluoromethylbenzene, nitrobenzene, chlorobenzene, chlorotoluene, and bromobenzene; and solvents containing carbon atoms and hetero atoms such as acetonitrile, dimethyl sulfoxide, and carbon disulfide. Among these, ether solvents and glycol ester solvents are preferred, and glycol ester solvents are more preferred. Among the ether solvents, diethyl ether, diisopropyl ether, dibutyl ether, and tetrahydrofuran are more preferable, and diethyl ether, diisopropyl ether, and dibutyl ether are even more preferable. Among the glycol ester solvents, acetate is more preferable, and 2-methoxy-1-methylethyl acetate and 2-ethoxy-methylethyl acetate are even more preferable.

[0049] The amount of the complexing agent used per 1 g of the total mass of the raw materials is preferably 0.1 to 30 mL, more preferably 0.5 to 20 mL, and even more preferably 1.0 to 10 mL, from the viewpoint of efficiently obtaining the effect of using the complexing agent, that is, forming an electrolyte precursor in which halogen atoms are more dispersed and fixed, and obtaining a glass-ceramic solid electrolyte with high ionic conductivity.

[0050] (solvent) In this embodiment, it is preferable to add a solvent to the raw material content and the complexing agent. By mixing the raw material content and the complexing agent using a solvent, the effect of using the above-mentioned complexing agent is promoted, that is, the formation of the electrolyte precursor acting with lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms is promoted, and it becomes easy to make the lithium-containing structure such as PS4 structure or the aggregate via the complexing agent, the raw material containing lithium such as lithium halide or the aggregate via the complexing agent exist evenly, and the halogen atoms are more dispersed and fixed to obtain the electrolyte precursor, so that the effect of obtaining high ion conductivity is easily exhibited.

[0051] This embodiment is a so-called heterogeneous method, and it is preferable that the electrolyte precursor does not completely dissolve in the solvent or liquid complexing agent, but precipitates. In this embodiment, the solubility of the electrolyte precursor can be adjusted by adding a solvent. In particular, halogen atoms are easily eluted from the electrolyte precursor, so that the desired electrolyte precursor can be obtained by suppressing the elution of halogen atoms by adding a solvent. As a result, a glass ceramic solid electrolyte having high ionic conductivity can be obtained through an electrolyte precursor in which specific components such as halogens are dispersed. Further, a solvent can be further added to the electrolyte precursor slurry after mixing.

[0052] Preferred examples of solvents having such properties include solvents having a solubility parameter of 10 or less. In this specification, the solubility parameter is a value δ ((cal / cm) calculated by the following formula (1) as described in various documents, such as "Chemical Handbook" (published in 2004, revised 5th edition, Maruzen Co., Ltd.). 3 ) 1 / 2 ) and is also called the Hildebrand parameter or SP value.

[0053]

number

[0054] By using a solvent with a solubility parameter of 10 or less, the solvent has a property of being relatively difficult to dissolve halogen atoms, raw materials containing halogen atoms such as lithium halide, and further components containing halogen atoms constituting the complex crystal contained in the electrolyte precursor (for example, an aggregate in which lithium halide and a complexing agent are bonded), etc., compared to the above complexing agent, and the halogen atoms are easily fixed in the electrolyte precursor, and the halogen atoms are present in a well-dispersed state in the obtained electrolyte precursor and further in the solid electrolyte, making it easier to obtain a glass ceramic solid electrolyte having high ion conductivity. That is, the solvent used in this embodiment is preferably one that does not dissolve the electrolyte precursor or one that does not easily dissolve it, and more preferably a solvent containing a solvent that does not dissolve the raw material contents, the complexing agent, and the electrolyte precursor. From the same viewpoint, the solubility parameter of the solvent is preferably 9.5 or less, more preferably 9.0 or less, and further preferably 8.5 or less.

[0055] More specifically, the solvent used in the present embodiment can be a wide variety of solvents that have been conventionally used in the production of solid electrolytes. Examples of the solvent include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents; solvents containing carbon atoms such as alcohol-based solvents, ester-based solvents, aldehyde-based solvents, ketone-based solvents, ether-based solvents, and solvents containing carbon atoms and heteroatoms; and the like. Among these, a solvent having a solubility parameter in the above-mentioned range may be appropriately selected and used.

[0056] More specifically, examples of the solvent include aliphatic hydrocarbon solvents such as hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane, and tridecane; alicyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, chlorobenzene, chlorotoluene, and bromobenzene; alcohol-based solvents such as ethanol and butanol; ester-based solvents such as ethyl acetate and butyl acetate; aldehyde-based solvents such as formaldehyde, acetaldehyde, and dimethylformamide; ketone-based solvents such as acetone and methyl ethyl ketone; ether-based solvents such as diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, dimethoxyethane, cyclopentyl methyl ether, tert-butyl methyl ether, and anisole; and solvents containing carbon atoms and hetero atoms such as acetonitrile, dimethyl sulfoxide, and carbon disulfide.

[0057] Among these solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, and ether solvents are preferred, and from the viewpoint of obtaining a more stable and high ion conductivity, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents are preferred, and heptane, cyclohexane, methylcyclohexane, ethylcyclohexane, dimethylcyclohexane, toluene, and ethylbenzene are more preferred, and heptane, cyclohexane, methylcyclohexane, and ethylcyclohexane are even more preferred. The solvent used in this embodiment is preferably the organic solvent exemplified above, and is an organic solvent different from the complexing agent. In this embodiment, these solvents may be used alone or in combination.

[0058] The amount of the solvent used per gram of the total mass of the raw materials is preferably 5 to 50 mL, more preferably 5 to 30 mL, and even more preferably 5 to 20 mL, from the viewpoint of obtaining a solid electrolyte with high ionic conductivity.

[0059] (mixture) As shown in the flow diagram of Fig. 1, it is necessary to mix the raw material inclusion, the complexing agent, and the solvent. In this embodiment, the raw material inclusion, the complexing agent, and the solvent may be mixed in either a solid or liquid form, but since the raw material inclusion usually contains a solid and the complexing agent is liquid, they are usually mixed in a form (slurry) in which the solid raw material inclusion is present in the liquid complexing agent and the solvent.

[0060] The amount of the raw material ingredients is preferably 5 g or more, more preferably 10 g or more, even more preferably 20 g or more, and even more preferably 30 g or more, per 1 L of the total amount of the complexing agent and the solvent, and the upper limit is preferably 500 g or less, more preferably 400 g or less, even more preferably 300 g or less, and even more preferably 250 g or less. When the amount of the raw material ingredients is within the above range, the raw material ingredients are easily mixed, the dispersion state of the raw materials is improved, and the reaction between the raw materials is promoted, so that an electrolyte precursor and further a glass ceramic solid electrolyte can be efficiently obtained.

[0061] The method of mixing the raw material ingredients, the complexing agent, and the solvent is not particularly limited, and the raw material ingredients, the complexing agent, and the solvent may be mixed by feeding them into a device capable of mixing the raw material ingredients, the complexing agent, and the solvent. For example, the raw material ingredients are fed into a tank, and the complexing agent and the solvent are added, which is preferable from the viewpoint of work efficiency because it suppresses the splashing of the liquid caused by the addition of solids. In addition, when a halogen element is used as a raw material, the raw material may not be solid, specifically, fluorine and chlorine are gaseous, and bromine is liquid, at room temperature and pressure. For example, when the raw material is liquid, it may be supplied into the tank together with a complexing agent or a solvent separately from other solid raw materials, and when the raw material is gas, it may be supplied by blowing it into the complexing agent, the solvent, and the solid raw materials.

[0062] This embodiment is characterized by including mixing the raw material ingredients, the complexing agent, and, if necessary, a solvent, and can also be produced by a method that does not use equipment generally called a grinder, such as a media-type grinder such as a ball mill or a bead mill, which is used for the purpose of grinding solid raw materials. When a media-type mill is used, a wet bead mill, a wet ball mill, a wet vibration mill, etc., described later in the section on grinding the electrolyte precursor, can be used. In particular, it is preferable to use a bead mill capable of circulating operation. In this embodiment, the raw material inclusions, the complexing agent, and the solvent are simply mixed together to mix the raw materials and the complexing agent contained in the inclusions to form an electrolyte precursor. The mixture of the raw material inclusions, the complexing agent, and the solvent may be pulverized by a pulverizer, since this can shorten the mixing time required to obtain the electrolyte precursor and can also be pulverized.

[0063] The device for mixing the raw material content, the complexing agent and the solvent may be, for example, a mechanical stirring mixer equipped with a stirring blade in a tank. The mechanical stirring mixer may be a high-speed stirring mixer, a double-arm mixer, etc., and the high-speed stirring mixer is preferably used from the viewpoint of improving the uniformity of the raw material in the mixture of the raw material content and the complexing agent and obtaining a higher ion conductivity. In addition, the high-speed stirring mixer may be a vertical shaft rotating mixer, a horizontal shaft rotating mixer, etc., and either type of mixer may be used.

[0064] Examples of the shape of the stirring blade used in the mechanical stirring mixer include blade type, arm type, anchor type, paddle type, full zone type, ribbon type, multi-stage blade type, double arm type, shovel type, double-shaft blade type, flat blade type, C-type blade type, anchor type, paddle type, full zone type, etc., and from the viewpoint of increasing the uniformity of the raw material in the raw material content and obtaining higher ionic conductivity, the shovel type, flat blade type, C-type blade type, etc. are preferred. Furthermore, if a small amount of production is required, stirring using a stirrer may be used.

[0065] The temperature conditions when mixing the raw material ingredients, the complexing agent, and if necessary, the solvent are not particularly limited, and are, for example, −30 to 100° C., preferably −10 to 50° C., and more preferably about room temperature (23° C.) (for example, about room temperature ±5° C.) The mixing time is about 0.1 to 150 hours, and from the viewpoint of more uniform mixing and obtaining higher ion conductivity, is preferably 0.2 to 120 hours, more preferably 0.3 to 100 hours, and even more preferably 0.5 to 80 hours.

[0066] By mixing the raw material inclusion, the complexing agent, and the solvent, the lithium atom, sulfur atom, phosphorus atom, and halogen atom contained in the raw material inclusion and the complexing agent act to obtain an electrolyte precursor in which these atoms are directly bonded to each other with and / or without the complexing agent. That is, in this embodiment, the electrolyte precursor obtained by mixing the raw material inclusion and the complexing agent contains a complex crystal composed of the complexing agent, lithium atom, sulfur atom, phosphorus atom, and halogen atom, and by mixing the raw material inclusion and the complexing agent, a material containing an electrolyte precursor (hereinafter, sometimes referred to as "electrolyte precursor containing material") is obtained. In this embodiment, the obtained electrolyte precursor is not completely dissolved in the complexing agent, which is a liquid, and a suspension containing the electrolyte precursor, which is usually a solid, is obtained. Therefore, this embodiment corresponds to a heterogeneous system in the so-called liquid phase method.

[0067] (Crushing of electrolyte precursor) This embodiment preferably further includes pulverizing the electrolyte precursor. By pulverizing the electrolyte precursor, a solid electrolyte having a small particle size can be obtained while suppressing a decrease in ion conductivity. The grinding of the electrolyte precursor in this embodiment is different from the mechanical milling of the so-called solid phase method, and does not obtain an amorphous or crystalline solid electrolyte by mechanical stress. As described above, the electrolyte precursor contains a complexing agent, and a lithium-containing structure such as a PS4 structure and a lithium-containing raw material such as lithium halide are bonded (coordinated) through the complexing agent. It is considered that when the electrolyte precursor is ground, fine particles of the electrolyte precursor are obtained while maintaining the above-mentioned bond (coordination) and dispersion. When this electrolyte precursor is heat-treated, the complexing agent is removed and at the same time, the components that were bonded (coordinated) through the complexing agent are bonded, and the reaction to the crystalline solid electrolyte easily occurs. Therefore, large grain growth due to the aggregation of particles, as seen in the synthesis of a normal solid electrolyte, is unlikely to occur, and the electrolyte precursor can be easily finely granulated.

[0068] In addition, from the viewpoint of the performance and manufacturing of the all-solid-state battery, it is desirable that the particle size of the solid electrolyte is small, but it is not easy to atomize the solid electrolyte by pulverization using a bead mill or the like. Although it is possible to atomize the solid electrolyte to a certain degree by wet pulverization using a solvent, there is a problem that the solid electrolyte is easily deteriorated by the solvent and is easily aggregated during pulverization, so that an excessive load is applied to the pulverization. On the other hand, it is difficult to atomize to submicron size even if dry pulverization is performed without using a solvent. Under such circumstances, it can be a great advantage that the performance of the all-solid-state battery can be improved and the manufacturing efficiency can be improved by a simple process of pulverizing the electrolyte precursor.

[0069] Furthermore, the stirring and mixing associated with the milling makes it easier to uniformly distribute lithium-containing structures such as PS4 structures or aggregates formed via a complexing agent, and lithium-containing raw materials such as lithium halides or aggregates formed via a complexing agent, and an electrolyte precursor is obtained in which specific components such as halogen atoms are more dispersed and fixed.As a result, the effect of obtaining high ionic conductivity along with fine particle size is more easily achieved.

[0070] The pulverizer used for pulverizing the electrolyte precursor is not particularly limited as long as it can pulverize particles, and for example, a media-type pulverizer using a pulverizing medium can be used. Among the media-type pulverizers, a wet pulverizer capable of wet pulverization is preferable, considering that the electrolyte precursor is mainly in a liquid state accompanied by liquids such as a complexing agent and a solvent, or in a slurry state. Representative examples of wet grinding machines include wet bead mills, wet ball mills, and wet vibration mills, among which wet bead mills using beads as grinding media are preferred because they allow the grinding conditions to be freely adjusted and are easy to handle smaller particle sizes. Dry grinding machines such as dry media grinding machines such as dry bead mills, dry ball mills, and dry vibration mills, and dry non-media grinding machines such as jet mills can also be used.

[0071] In addition, the electrolyte precursor to be pulverized by the pulverizer is usually supplied as an electrolyte precursor-containing material obtained by mixing a raw material containing material and a complexing agent, and is mainly supplied in a liquid state or a slurry state, that is, the object to be pulverized by the pulverizer is mainly an electrolyte precursor-containing liquid or an electrolyte precursor slurry. Therefore, the pulverizer used in this embodiment is preferably a flow-type pulverizer that can perform a circulation operation to circulate the electrolyte precursor-containing liquid or the electrolyte precursor slurry as necessary. More specifically, it is preferable to use a pulverizer that circulates between a pulverizer (pulverizer mixer) that pulverizes the slurry and a temperature holding tank (reaction vessel) as described in JP 2010-140893 A.

[0072] The size of the beads used in the above-mentioned grinding machine may be appropriately selected depending on the desired particle size, processing amount, etc. For example, the diameter of the beads may be about 0.05 mmφ or more and 5.0 mmφ or less, preferably 0.1 mmφ or more and 3.0 mmφ or less, and more preferably 0.3 mmφ or more and 1.5 mmφ or less.

[0073] As a pulverizer used for pulverizing the electrolyte precursor, a machine capable of pulverizing an object by using ultrasonic waves, for example, a machine called an ultrasonic pulverizer, an ultrasonic homogenizer, a probe ultrasonic pulverizer, or the like, can be used. In this case, various conditions such as the frequency of the ultrasonic waves may be appropriately selected depending on the average particle size of the desired electrolyte precursor, and the frequency may be, for example, about 1 kHz or more and 100 kHz or less, and from the viewpoint of more efficiently pulverizing the electrolyte precursor, the frequency is preferably 3 kHz or more and 50 kHz or less, more preferably 5 kHz or more and 40 kHz or less, and even more preferably 10 kHz or more and 30 kHz or less. The output of the ultrasonic crusher may usually be about 500 to 16,000W, preferably 600 to 10,000W, more preferably 750 to 5,000W, and further preferably 900 to 1,500W.

[0074] The average particle size of the electrolyte precursor obtained by grinding (D 50 ) is appropriately determined according to the desire, but is usually 0.01 μm or more and 50 μm or less, preferably 0.03 μm or more and 5 μm or less, and more preferably 0.05 μm or more and 3 μm or less. By setting the average particle size in this range, it is possible to meet the demand for a solid electrolyte having a small particle size of 1 μm or less.

[0075] The grinding time is not particularly limited as long as it is a time that allows the electrolyte precursor to have a desired average particle size, and is usually from 0.1 hours to 100 hours. From the viewpoint of efficiently achieving a particle size of the desired size, the grinding time is preferably from 0.3 hours to 72 hours, more preferably from 0.5 hours to 48 hours, and even more preferably from 1 hour to 24 hours.

[0076] The pulverization may be carried out after drying an electrolyte precursor-containing material such as an electrolyte precursor-containing liquid or an electrolyte precursor slurry to convert the electrolyte precursor into powder. In this case, it is preferable to use any of the dry grinders among the grinders exemplified above as grinders that can be used in the present production method. Other matters related to grinding, such as grinding conditions, are the same as those for grinding the electrolyte precursor-containing liquid or the electrolyte precursor slurry, and the average particle size of the electrolyte precursor obtained by grinding is also the same as above.

[0077] (Dry) In this embodiment, the electrolyte precursor slurry containing the complex crystals is required to be dried. In particular, the drying preferably includes removing the liquid complexing agent (the complexing agent that is not incorporated in the electrolyte precursor). This removes the liquid component of the complexing agent to obtain a powder of the electrolyte precursor. By drying in advance, it is possible to suppress the release of halogen atoms from the electrolyte precursor and to perform the complex decomposition efficiently. The drying and the subsequent heating may be performed in the same step. The liquid component of the complexing agent means a complexing agent that is not incorporated into the electrolyte precursor and exists in the liquid portion of the electrolyte precursor slurry. The electrolyte precursor obtained by drying forms a complex structure and contains a complexing agent.

[0078] The electrolyte precursor slurry is preferably dried under reduced pressure, by heating, or by a combination thereof, and more preferably by fluidized drying using a medium. By subjecting the electrolyte precursor to heat drying under vacuum, it is possible to remove the complexing agent present in the liquid portion of the electrolyte precursor slurry. If necessary, the drying method can also be applied to drying an amorphous solid electrolyte and a solid electrolyte at least a part of which has turned into a glass ceramic.

[0079] Fluidized drying using a medium allows the slurry to flow, increasing the heat transfer area of ​​the slurry and promoting rapid and uniform heat conduction, making it possible to dry in a short time. Therefore, there is no need to dry at high temperatures for uniform drying, and even if drying is performed at high temperatures, it only takes a short time, so that it is possible to minimize the elution of halogen atoms due to the thermal history caused by high-temperature drying, and to suppress quality deterioration such as a decrease in ion conductivity. Furthermore, there is no need to select low-temperature drying to suppress the thermal history caused by high-temperature drying, and long drying times are not required, resulting in excellent productivity. In addition, since the slurry is fluidized using a medium, the drying can be uniformly performed almost without being affected by the viscosity of the slurry, and therefore, the method can be used with slurries of a wide range of viscosities.

[0080] When using media particles as the medium and performing fluidized drying while fluidizing the media particles in a dryer, the media is already heated and has a heat quantity in the dryer. The slurry to be dried has an increased heat transfer area due to the fluidized catalytic cracking catalyst of the media particles flowing, and is heated by the heat quantity of the media, which makes it possible to shorten the drying time. By carrying out such drying, it is possible to suppress agglomeration caused by a drying state with low uniformity in a conventional drying method, for example, a batch-type drying method such as vacuum drying, and to suppress deterioration of quality. Furthermore, since the fluidized drying using a medium can adopt a flow-through type, excellent productivity can be obtained. Thus, the manufacturing method of the present embodiment makes it possible to manufacture a solid electrolyte with excellent performance such as ion conductivity with high productivity by adopting fluidized drying using a medium.

[0081] As a dryer capable of performing fluidized drying using a medium (also referred to as a "media fluidized bed dryer"), any dryer can be used without particular restrictions as long as it can dry the slurry to be dried while flowing using media particles as the medium. It is also possible to use a commercially available fluidized bed dryer in which media particles are contained as a medium inside the dryer and the media particles are dried while flowing.

[0082] A preferred embodiment of a drying device capable of performing fluidized drying using a medium that can be used in this embodiment will be described with reference to Fig. 2. The drying device shown in Fig. 2 includes a medium fluidized dryer capable of performing fluidized drying by fluidizing media particles as a medium, and a bag filter for recovering a powdered solid electrolyte or the solid electrolyte from a fluid that contains gas and a powder obtained by drying, i.e., a solid electrolyte or an electrolyte precursor contained in a slurry, discharged by the dryer.

[0083] The media fluidized dryer shown in Figure 2 is a type that uses media particles as a medium, and the media particles inside the dryer are fluidized by gas, and a slurry is supplied into the fluidized bed of media particles and the slurry is dried. When a slurry is supplied into the fluidized bed of media particles, the slurry flows and the heat transfer area increases, making it possible to dry in a shorter time. The dryer has a partition plate preferably having a plurality of vents for supplying gas therein. By having the partition plate, the media particles serving as the medium do not remain at the bottom, but form a fluidized bed by convection within the dryer due to the gas supplied into the dryer through the vents.

[0084] An outlet is provided above the medium fluidized dryer for discharging the gas supplied from below and the fluid containing the powder contained in the slurry, i.e., the solid electrolyte or the electrolyte precursor, and the fluid discharged from the outlet is supplied to a bag filter. The bag filter is provided with multiple filters, and the powder in the fluid is collected by the filters and recovered as the solid electrolyte or the electrolyte precursor, and the gas in the fluid is exhausted from an outlet above the bag filter.

[0085] In a medium fluidized dryer, it is effective to use media particles as the medium, and the media particles are kept in a fluidized state by a gas, as shown in Fig. 2. As the gas, it is preferable to use an inert gas such as nitrogen or argon from the viewpoint of suppressing deterioration of the solid electrolyte and the electrolyte precursor due to oxidation, and it is more preferable to adopt nitrogen in consideration of the cost.

[0086] As the media particles, it is preferable to use ceramic balls in consideration of drying efficiency, fluidity, etc. The particle size of the media particles cannot be generally specified because it varies depending on the size of the fluidized dryer, but it is usually sufficient to use particles of about 0.5 mm to 5.0 mm, and in consideration of drying efficiency, fluidity, etc., it is preferably 1.0 mm to 3.0 mm. In addition, when the particle size of the media particles is within the above range, it is possible to suppress exhaust to the outside of the dryer along with the fluid containing the gas and the solid electrolyte and / or electrolyte precursor contained in the dried slurry, so that the amount of the particles captured by the bag filter can be reduced.

[0087] When a gas is used to fluidize the medium, it is preferable that the gas is heated. In the case of the medium fluidized dryer of the type shown in Fig. 2, the gas is used as a heat source for drying the slurry, so that the gas is heated. It is also preferable that the media particles are heated. In the case of a medium flow dryer of the type shown in Fig. 2, the media particles are in a state of being heated by a heated gas, and the slurry is heated by the gas and by the media particles heated by the gas, making it possible to dry the slurry in an extremely short time.

[0088] Furthermore, there are no particular limitations on the opening size of the ventilation hole in the partition plate, so long as it is smaller than the particle size of the media particles so as to prevent the media particles from falling to the bottom; for example, it may be approximately 0.1 mm or more and 3 mm or less. Considering the ease of supplying the medium (gas) from below, the opening size is preferably 0.3 mm or more and 2.5 mm or less, and more preferably 0.5 mm or more and 2.0 mm or less.

[0089] The drying temperature in the main drying can be set according to the type of complexing agent contained in the slurry (mainly the complexing agent not incorporated in the electrolyte precursor) and the type of solvent used as needed. For example, the drying can be performed at a temperature equal to or higher than the boiling point of the complexing agent and the solvent used as needed. As described above, the drying temperature varies depending on the boiling point of the polar solvent used, and therefore cannot be generally specified, but the drying temperature is usually about 50 to 150°C, preferably 55 to 130°C, more preferably 60 to 100°C, and even more preferably 65 to 80°C.

[0090] For example, when using a medium fluidized dryer of the type shown in Fig. 2, the gas supply temperature is usually about 60 to 200°C, and from the viewpoint of drying in a shorter time and suppressing thermal history to improve quality, it is preferably 70 to 180°C, more preferably 80 to 160°C, and even more preferably 90 to 150°C, and the gas supply rate is usually about 0.5 to 10.0 m / s based on the supply temperature, and from the viewpoint of maintaining good fluidity of the media particles, it is preferably 1.0 to 8.0 m / s, more preferably 1.5 to 5.0 m / s, and even more preferably 2.0 to 3.5 m / s. The gas supply rate is the linear velocity relative to the cross-sectional area of ​​the fluidized bed of the media particles as the medium in the direction perpendicular to the flow direction of the gas (which can also be said to be the cross-sectional area of ​​the container in which the media particles are stored in the dryer in the direction perpendicular to the flow direction of the gas).

[0091] The temperature of the fluid at the outlet of the fluidized dryer is usually about 50 to 120° C., and from the same viewpoint, it is preferably 55 to 100° C., more preferably 60 to 90° C., and further preferably 65 to 80° C. Within the above range, the drying temperature in the fluidized dryer can be easily set within the above preferred drying temperature range. The temperature of the fluid can be adjusted by the amount and temperature of the gas supplied, the amount of the slurry supplied, etc., and is easily adjusted by the amount of the slurry supplied.

[0092] In the production method of this embodiment, from the viewpoint of efficiently collecting the powder obtained by drying, that is, the solid electrolyte or electrolyte precursor, a bag filter is preferably used as shown in FIG.

[0093] The filter used in the bag filter can be any material, including polypropylene, nylon, acrylic, polyester, cotton, wool, heat-resistant nylon, polyamide / polyimide, PPS (polyphenylene sulfide), glass fiber, PTFE (polytetrafluoroethylene), etc., and functional filters such as electrostatic filters can also be used. Among these, filters made of heat-resistant nylon, polyamide / polyimide, PPS (polyphenylene sulfide), glass fiber, and PTFE (polytetrafluoroethylene) are preferred, filters made of heat-resistant nylon, PPS (polyphenylene sulfide), and PTFE (polytetrafluoroethylene) are more preferred, and filters made of PTFE (polytetrafluoroethylene) are particularly preferred.

[0094] The bag filter may also have a brushing means, for example, preferably a pulsating counter pressure type or a pulse jet type, with the pulse jet type being preferred.

[0095] An induced draft fan may be provided in the line from the exhaust port of the bag filter to forcibly exhaust the gas exhausted from the exhaust port. By exhausting the gas with an induced draft fan or the like, filtration in the bag filter proceeds smoothly and a stable fluidized layer of media particles is obtained in the fluidized dryer, so that the slurry can be dried in a shorter time.

[0096] When the drying in the present embodiment is carried out under reduced pressure, from the viewpoint of obtaining a glass-ceramic solid electrolyte having high ion conductivity, the pressure is preferably less than 1000.0 Pa, more preferably 500.0 Pa or less, and even more preferably 300.0 Pa or less, and from the viewpoint of the apparatus, the pressure is preferably 0.1 Pa or more, more preferably 1.0 Pa or more, and even more preferably 5.0 Pa or more. When drying under reduced pressure, heating may be performed to shorten the drying time. The temperature varies depending on the pressure and the like, but from the viewpoint of obtaining a solid electrolyte having high ionic conductivity, the temperature is usually preferably 120° C. or lower, more preferably 80° C. or lower, and even more preferably 50° C. or lower. There is no particular lower limit, but the temperature is preferably 0° C. or higher, more preferably 10° C. or higher, and even more preferably 15° C. or higher. It is even more preferable to dry the solid electrolyte without external heating or cooling.

[0097] (electrolyte precursor) The electrolyte precursor of the present embodiment is characterized in that it contains a complexing agent, a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom as its constituent components, and in that a peak different from the peak derived from the raw materials is observed in the X-ray diffraction pattern in an X-ray diffraction measurement, and is required to contain a complex crystal containing a complexing agent, a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom as its constituent components. When the raw material contents are merely mixed, only a peak derived from the raw material is observed, and when the raw material contents are mixed with a complexing agent, a peak different from the peak derived from the raw material is observed, so that the electrolyte precursor (or the complex crystal contained therein) has a structure that is clearly different from the raw material itself contained in the raw material contents. This has been specifically confirmed in the Examples. Examples of measurement of X-ray diffraction patterns of the electrolyte precursor (or the complex crystal contained therein) and each raw material such as lithium sulfide are shown in Figures 3 and 6, respectively. From the X-ray diffraction pattern, it can be seen that the electrolyte precursor (or the complex crystal contained therein) has a predetermined crystal structure. In addition, the diffraction pattern does not include the diffraction pattern of any raw material such as lithium sulfide shown in Figure 6, and it can be seen that the electrolyte precursor (or the complex crystal contained therein) has a crystal structure different from that of the raw material.

[0098] In addition, the electrolyte precursor (or the complex crystals contained therein) is characterized by having a structure different from that of the crystalline solid electrolyte. This has also been specifically confirmed in the Examples. FIG. 3 also shows the X-ray diffraction pattern of the crystalline solid electrolyte, which is different from the diffraction pattern of the electrolyte precursor (or the complex crystals contained therein). The electrolyte precursor (or the complex crystals contained therein) has a specific crystal structure, and is different from the amorphous solid electrolyte having a broad pattern shown in FIG. 3.

[0099] The complex crystal contains a complexing agent, a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom as components, and is typically presumed to form a complex structure in which a lithium atom is directly bonded to other atoms with and / or without the intervention of a complexing agent. Here, whether the complexing agent is a component of the complex crystal can be confirmed by, for example, gas chromatography analysis. Specifically, the powder of the electrolyte precursor is dissolved in methanol, and the resulting methanol solution is analyzed by gas chromatography to quantitatively determine the amount of the complexing agent contained in the complex crystal. The content of the complexing agent in the electrolyte precursor varies depending on the molecular weight of the complexing agent, but is usually about 10% by mass to 70% by mass, preferably 15% by mass to 65% by mass.

[0100] In this embodiment, it is preferable to form a complex crystal containing halogen atoms in terms of improving ion conductivity. By using a complexing agent, a lithium-containing structure such as a PS4 structure and a lithium-containing raw material such as lithium halide are bonded (coordinated) through the complexing agent, and it becomes easier to obtain a complex crystal in which halogen atoms are more dispersed and fixed, thereby improving ion conductivity.

[0101] The fact that the halogen atoms in the electrolyte precursor form a complex crystal can be confirmed by the fact that a predetermined amount of halogen atoms is contained in the electrolyte precursor even after solid-liquid separation of the electrolyte precursor-containing material. This is because halogen atoms that do not form a complex crystal are more easily dissolved than halogen atoms that form a complex crystal and are discharged into the liquid of solid-liquid separation. It can also be confirmed by the fact that the proportion of halogen atoms in the electrolyte precursor or solid electrolyte is not significantly reduced compared to the proportion of halogen atoms supplied from the raw material by composition analysis using ICP analysis (inductively coupled plasma atomic emission spectroscopy) of the electrolyte precursor or solid electrolyte. The amount of halogen atoms remaining in the electrolyte precursor is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on the charged composition. The upper limit of the amount of halogen atoms remaining in the electrolyte precursor is 100% by mass.

[0102] (complexolysis) This embodiment includes obtaining an amorphous solid electrolyte or a solid electrolyte in which at least a part of the amorphous solid electrolyte is converted into a glass ceramic by complexing the electrolyte precursor obtained by the drying. The decomplexation means removing the complexing agent from the electrolyte precursor (complex crystal), and any method capable of removing the complexing agent may be adopted. For example, it is preferable to use a heating method, or to heat the electrolyte precursor under a reduced pressure of less than 1000 Pa while applying vibration. By the decomposition, the complexing agent, which is a component of the complex crystal in the electrolyte precursor, is removed, and an amorphous solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms or a solid electrolyte at least part of which is glass-ceramicized is obtained. The electrolyte precursor to be decomposed may be a ground electrolyte precursor obtained by the above-mentioned grinding. In this decomposition, a part of which is glass-ceramicized may be used as a glass-ceramic solid electrolyte, and a glass-ceramic solid electrolyte may be obtained by further heating the glass-ceramic solid electrolyte. Here, the removal of the complexing agent in the electrolyte precursor is supported by the fact that it is clear from the results of X-ray diffraction patterns, gas chromatography analysis, etc. that the complexing agent constitutes a complex crystal of the electrolyte precursor, and in addition, the X-ray diffraction pattern of a solid electrolyte obtained by removing the complexing agent through decomplexation of the electrolyte precursor is the same as that of a solid electrolyte obtained by a conventional method without using a complexing agent.

[0103] In the manufacturing method of this embodiment, the amorphous solid electrolyte or glass ceramic solid electrolyte is obtained by removing the complexing agent in the electrolyte precursor by heating the electrolyte precursor, and the less the complexing agent in the amorphous solid electrolyte or glass ceramic solid electrolyte, the more preferable, but the complexing agent may be contained to an extent that does not impair the performance of the amorphous solid electrolyte or glass ceramic solid electrolyte. The content of the complexing agent contained in the amorphous solid electrolyte or glass ceramic solid electrolyte may be 15 mass % or less, preferably 5 mass % or less, more preferably 3 mass % or less, and even more preferably 1 mass % or less.

[0104] Conventionally, in order to obtain a crystalline solid electrolyte having high ionic conductivity, for example, a solid electrolyte having a thiolicon region II type crystal structure described later, it was necessary to prepare an amorphous solid electrolyte by mechanical pulverization such as mechanical milling, or other melt quenching treatments, and then heat the amorphous solid electrolyte to obtain it. However, the manufacturing method of the present embodiment is superior to the conventional manufacturing method using mechanical milling, etc., in that a crystalline solid electrolyte having a thiolicon region II type crystal structure can be obtained by a method that does not involve mechanical pulverization or other melt quenching treatments.

[0105] In this embodiment, when a crystalline solid electrolyte is obtained after an amorphous solid electrolyte is obtained, it is possible to adjust the crystal structure of the crystalline solid electrolyte by adjusting the heating temperature, heating time, and the like. When obtaining an amorphous solid electrolyte, the heating temperature of the electrolyte precursor may be determined according to the structure of the crystalline solid electrolyte obtained by heating the amorphous solid electrolyte. Specifically, the amorphous solid electrolyte is subjected to differential thermal analysis (DTA) at a temperature rise rate of 10°C / min using a differential thermal analyzer (DTA device), and the heating temperature is preferably set to 5°C or less, more preferably 10°C or less, and even more preferably 20°C or less, starting from the temperature of the top of the exothermic peak observed on the lowest temperature side. There is no particular limit to the lower limit, but the heating temperature may be set to about 40°C or more less than the temperature of the top of the exothermic peak observed on the lowest temperature side. By setting the temperature range, an amorphous solid electrolyte can be obtained more efficiently and reliably. The heating temperature for obtaining an amorphous solid electrolyte cannot be generally defined because it varies depending on the structure of the crystalline solid electrolyte to be obtained. However, it is usually preferably 300° C. or lower, more preferably 250° C. or lower, and even more preferably 230° C. or lower. There is no particular lower limit, but the heating temperature is preferably 100° C. or higher, more preferably 150° C. or higher, and even more preferably 100° C. or higher.

[0106] When a crystalline solid electrolyte is obtained by complex decomposition, the heating temperature of the electrolyte precursor is preferably the same as that of the crystallization described below.

[0107] The degree of vacuum during the complex decomposition is preferably less than 1000.0 Pa, more preferably 500.0 Pa or less, and even more preferably 300.0 Pa or less, from the viewpoint of obtaining a solid electrolyte having high ionic conductivity, and is preferably 0.1 Pa or more, more preferably 1.0 Pa or more, and even more preferably 5.0 Pa or more, from the viewpoint of the apparatus. Under high vacuum, the removal rate of the complexing agent is fast, and the content of the complexing agent can be reduced while maintaining the dispersion state of each component in the solid electrolyte. On the other hand, under low vacuum, the removal rate of the complexing agent is slow, and elution or aggregation of specific components in the electrolyte precursor occurs, making it impossible to sufficiently reduce the content of the complexing agent. If the crystallization step is carried out while still containing a large amount of complexing agent, a crystalline phase with low ionic conductivity is observed, and performance is reduced, so it is preferable to sufficiently reduce the content of the complexing agent.

[0108] The method of applying vibration is not particularly limited and may include heating and reducing pressure, but a vibration dryer, a drum dryer, a screw conveyor dryer, a rotary dryer with a heating tube, or a vibration transport dryer is preferred. As mentioned above, in order to prevent the elution or aggregation of specific components, it is preferable to apply heat uniformly to the powder. Although there are methods such as stirring to apply heat uniformly, stirring applies energy directly to the powder, and there is a risk of applying more heat than necessary. As a result, it is more preferable to use a vibration dryer.

[0109] In particular, it is preferable to carry out the complex decomposition in a short time from the viewpoint of preventing disproportionation of halogen atoms and obtaining a solid electrolyte having high ionic conductivity, and in order to achieve this, it is preferable to appropriately select and combine the temperature, degree of vacuum and vibration method.

[0110] The complex decomposition will now be described in more detail. The electrolyte precursor obtained by drying forms a complex crystal with the help of a complexing agent. The role of this complexing agent is to coordinate (disperse) specific components by forming them into a complex. In the decomplexation process, it is important to remove (decompose) the complexing agent without agglomerating the specific components dispersed by the complexing agent. Decomposition is the process of removing the complexing agent by breaking down the complex structure through the application of heat, but a high degree of vacuum is required to decompose the specific components without agglomerating them.

[0111] When heat is applied under low pressure, the heat is used to decompose the complexing agent from the complex, and the gas (decomposition gas) derived from the complexing agent generated by the decomposition passes through the powder surface and pores of the electrolyte precursor and escapes. On the other hand, when heat is applied under high pressure, the complexing agent is also difficult to decompose as the gas becomes difficult to escape from the electrolyte precursor, but heat continues to be applied during that time, so the energy used for decomposition until then affects the electrolyte precursor structure itself, such as the liberation of specific components (halogen atoms, etc.). The liberated specific components are attracted to the decomposition gas molecules (which have polarity) that are adsorbed on the particle surface without being able to escape as decomposition gas, and coagulate. For these reasons, in order to perform complex decomposition without coagulation, it is important to smoothly remove the decomposition gas that corresponds to the amount of heat applied, and a high vacuum is required for smooth removal of the decomposition gas.

[0112] The electrolyte precursor is a complex and a delicate substance, and therefore it is not preferable to apply heat or mechanical force to it. However, the complex cannot be decomposed without applying heat, and it cannot be heated uniformly without mechanical mixing. The advantage of the vibration dryer is that it does not directly apply mechanical energy using an agitator or the like, but rather creates convection in the dryer by devising a way to vibrate the can body, and the powder can be heated uniformly. Since complex decomposition only progresses when heat is applied, it is very important to apply heat uniformly to the powder. For this reason, it is highly preferable to use a vibration dryer for complex decomposition, since it is possible to obtain a glass-ceramic solid electrolyte with high ionic conductivity.

[0113] The electrolyte precursor obtained by the drying is decomposed to obtain an amorphous solid electrolyte containing lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms as constituent components, and in which the intensity ratio Ic / Is of the diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) to the intensity Is of a standard sample is 0.02 or less, or a GC solid electrolyte in which the intensity ratio Ix / Igc of the diffraction peak intensity Ix of LiX to the diffraction peak intensity Igc of a glass ceramic is 0.5 or less. In the amorphous solid electrolyte, when the intensity ratio Ic / Is between the diffraction peak intensity Ic of the LiX complex (wherein X represents a halogen) and the intensity Is of the standard sample is 0.02 or less, the LiX complex is not generated or the precipitation of the LiX complex is very small, so the halogen is taken into the amorphous and dispersed. On the other hand, when the intensity ratio Ic / Is is large, a large number of complex crystals are generated, and it is considered that the halogen is not taken into the amorphous and is unevenly distributed. In addition, the intensity ratio Ix / Igc between the diffraction peak intensity Ix of LiX in the GC solid electrolyte and the diffraction peak intensity Igc of the glass ceramic is 0.5 or less, which indicates that the precipitation of LiX is suppressed as a result of the halogen being taken into the amorphous, and the halogen is also taken into the crystal structure of the glass ceramic. Therefore, by making it into a complex decomposition product as in this embodiment, it is possible to reduce halogen atoms not taken into the crystal structure, and therefore it is preferable to increase the ion conductivity. The diffraction peak intensities of the LiX complex, LiX, and glass ceramics are the intensities of the maximum peaks. The intensity ratio Ic / Is is preferably 0.01 or less, more preferably 0.05 or less. The intensity ratio Ix / Igc is preferably 0.3 or less, more preferably 0.2 or less, and even more preferably 0.1 or less.

[0114] (Amorphous solid electrolyte) The amorphous solid electrolyte obtained by complex decomposition contains lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms. Representative examples include solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-LiI-LiBr, and solid electrolytes further containing other atoms such as oxygen atoms and silicon atoms, such as Li2S-P2S5-Li2O-LiI and Li2S-SiS2-P2S5-LiI. From the viewpoint of obtaining higher ionic conductivity, solid electrolytes composed of lithium sulfide, phosphorus sulfide and lithium halide, such as Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-LiI-LiBr, are preferred. The types of atoms constituting the amorphous solid electrolyte can be confirmed, for example, by an ICP emission spectroscopic analyzer.

[0115] When the amorphous solid electrolyte obtained by complex decomposition contains at least Li2S-P2S5, the molar ratio of Li2S to P2S5 is preferably 65-85:15-35, more preferably 70-80:20-30, and even more preferably 72-78:22-28, from the viewpoint of obtaining higher ionic conductivity. In the case where the amorphous solid electrolyte obtained in this embodiment is, for example, Li2S-P2S5-LiI-LiBr, the total content of lithium sulfide and diphosphorus pentasulfide is preferably 60 to 95 mol%, more preferably 65 to 90 mol%, and even more preferably 70 to 85 mol%. The ratio of lithium bromide to the total of lithium bromide and lithium iodide is preferably 1 to 99 mol%, more preferably 20 to 90 mol%, even more preferably 40 to 80 mol%, and particularly preferably 50 to 70 mol%.

[0116] In the amorphous solid electrolyte obtained by complex decomposition, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms is preferably 1.0-1.8:1.0-2.0:0.1-0.8:0.01-0.6, more preferably 1.1-1.7:1.2-1.8:0.2-0.6:0.05-0.5, and further preferably 1.2-1.6:1.3-1.7:0.25-0.5:0.08-0.4. In addition, when bromine and iodine are used in combination as halogen atoms, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, bromine, and iodine is preferably 1.0-1.8:1.0-2.0:0.1-0.8:0.01-0.3:0.01-0.3, more preferably 1.1-1.7:1.2-1.8:0.2-0.6:0.02-0.25:0.02-0.25, more preferably 1.2-1.6:1.3-1.7:0.25-0.5:0.03-0.2:0.03-0.2, and even more preferably 1.35-1.45:1.4-1.7:0.3-0.45:0.04-0.18:0.04-0.18. By setting the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms and halogen atoms within the above range, it becomes easier to obtain a glass ceramic solid electrolyte having a thiolithiregion II type crystal structure described later and with higher ion conductivity.

[0117] The shape of the amorphous solid electrolyte is not particularly limited, but may be, for example, particulate. The average particle diameter (D 50 ) can be, for example, in the range of 0.01 μm to 500 μm, or 0.1 to 200 μm.

[0118] (Glass-ceramic solid electrolyte) The glass ceramic solid electrolyte obtained by this embodiment may be obtained by simultaneously performing crystallization by complex decomposition to obtain a glass ceramic solid electrolyte, or may be obtained by obtaining an amorphous solid electrolyte by complex decomposition and then performing heating (crystallization) to obtain a glass ceramic solid electrolyte, or may be obtained by obtaining a solid electrolyte in which a part of the electrolyte is converted to glass ceramic by complex decomposition and then performing further crystallization by heating to obtain a glass ceramic solid electrolyte. In this embodiment, the solid electrolyte obtained as the final product is a glass ceramic solid electrolyte, and the solid electrolyte containing glass ceramics generated during the process of obtaining it is called a GC-type solid electrolyte. In addition, when a glass ceramic solid electrolyte is obtained as the final product without performing heating (crystallization) after complex decomposition, the glass ceramic solid electrolyte and the GC-type solid electrolyte are the same. The crystal structure of the glass ceramic solid electrolyte obtained in this embodiment is a Li3PS4 crystal structure, a Li4P2S6 crystal structure, a Li7PS6 crystal structure, a Li7P3S 11 Examples of such structures include a crystal structure having peaks at 2θ=approximately 20.2° and 23.6° (for example, JP 2013-16423 A).

[0119] Also, Li 4-x Ge 1-x P x S4 thio-LISICON Region II crystal structure (Kanno et al., Journal of The Electrochemical Society, 148(7)A742-746(2001)), Li 4-x Ge 1-x P x Examples of the crystal structure include a crystal structure similar to the S4-type thio-LISICON Region II type (see Solid State Ionics, 177 (2006), 2721-2725). The crystal structure of the glass ceramic solid electrolyte is preferably the thio-LISICON Region II type crystal structure among the above, since it can provide higher ionic conductivity. Here, the "thio-LISICON Region II type crystal structure" refers to a Li 4-x Ge1-x P x S4 thio-LISICON Region II crystal structure, Li 4-x Ge 1-x P x It indicates that the crystal structure is similar to S4-based thio-LISICON Region II type. The glass ceramic solid electrolyte may have the above-mentioned thio-LISICON Region II type crystal structure or may have it as the main crystal, but from the viewpoint of obtaining higher ionic conductivity, it is preferable that it has it as the main crystal. In this specification, "having it as the main crystal" means that the ratio of the target crystal structure among the crystal structures is 80% or more, preferably 90% or more, and more preferably 95% or more. In addition, from the viewpoint of obtaining higher ionic conductivity, it is preferable that the glass ceramic solid electrolyte does not contain crystalline Li3PS4 (β-Li3PS4).

[0120] In X-ray diffraction measurements using CuKα radiation, the diffraction peaks of the Li3PS4 crystal structure appear, for example, at 2θ = 17.5°, 18.3°, 26.1°, 27.3°, and 30.0°, the diffraction peaks of the Li4P2S6 crystal structure appear, for example, at 2θ = 16.9°, 27.1°, and 32.5°, the diffraction peaks of the Li7PS6 crystal structure appear, for example, at 2θ = 15.3°, 25.2°, 29.6°, and 31.0°, and the diffraction peaks of the Li7P3S 11 Diffraction peaks of the crystal structure appear, for example, at 2θ = 17.8°, 18.5°, 19.7°, 21.8°, 23.7°, 25.9°, 29.6°, and 30.0°. 4-x Ge 1-x P x The diffraction peaks of the S4 thio-LISICON Region II crystal structure appear, for example, at 2θ = 20.1°, 23.9°, and 29.5°, and Li 4-x Ge 1-x P xDiffraction peaks with a crystal structure similar to that of the S4 thio-LISICON Region II type appear, for example, around 2θ = 20.2 and 23.6°. Note that the peak positions may shift within a range of ±0.5°.

[0121] As described above, when a thio-LISICON Region II type crystal structure is obtained in this embodiment, it is preferably free of crystalline Li3PS4 (β-Li3PS4). Fig. 3 shows an example of X-ray diffraction measurement of the glass-ceramic solid electrolyte obtained by the manufacturing method of this embodiment. Fig. 4 shows an example of X-ray diffraction measurement of glass-ceramic Li3PS4 (β-Li3PS4). As can be understood from Fig. 3 and Fig. 4, the solid electrolyte of this embodiment does not have diffraction peaks at 2θ = 17.5° and 26.1° found in crystalline Li3PS4, or even if it has such peaks, the detected peaks are extremely small compared to the diffraction peaks of the thio-LISICON Region II type crystal structure.

[0122] The crystal structure represented by the composition formula Li having the above Li7PS6 structural skeleton and with a part of P substituted by Si 7-x P 1-y Si y S6 and Li 7+x P 1-y Si y S6 (where x is -0.6 to 0.6 and y is 0.1 to 0.6) is cubic or orthorhombic, preferably cubic, and in X-ray diffraction measurement using CuKα radiation, it mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°. The above composition formula Li 7-x-2y PS 6-x-y Cl x (where 0.8 ≤ x ≤ 1.7 and 0 < y ≤ -0.25x + 0.5) is preferably cubic, and in X-ray diffraction measurement using CuKα radiation, it mainly has peaks appearing at positions of 2θ = 15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°. Also, the above composition formula Li 7-x PS 6-x Hax The crystal structure represented by the formula (Ha is Cl or Br, and x is preferably 0.2 to 1.8) is preferably a cubic crystal, and in X-ray diffraction measurement using CuKα radiation, has peaks that appear mainly at 2θ=15.5°, 18.0°, 25.0°, 30.0°, 31.4°, 45.3°, 47.0°, and 52.0°. The positions of these peaks may vary within a range of ±0.5°.

[0123] The shape of the glass ceramic solid electrolyte is not particularly limited, but may be, for example, particulate. The average particle diameter (D 50 ) can be, for example, in the range of 0.01 μm to 500 μm, or 0.1 to 200 μm.

[0124] (Heating (crystallization)) This embodiment may further include heating the amorphous solid electrolyte obtained by complex decomposition to crystallize it. Even when a solid electrolyte partially converted into a glass ceramic is obtained by complex decomposition, it may be heated to further promote crystallization. This embodiment is not suitable for a crystalline solid electrolyte that does not pass through an amorphous solid electrolyte after complex decomposition as in Patent Document 4. The glass ceramic of this embodiment is in a metastable phase and requires heating at a predetermined crystallization temperature, whereas in the case of a crystalline solid electrolyte in a stable phase that does not pass through an amorphous solid electrolyte, even if a relatively large amount of LiX or LiX complex is produced, it can become uniform by heating and crystallizing, and since LiX cannot be incorporated into the amorphous solid electrolyte, it is difficult to reduce the diffraction peak intensity of LiX or the like to a predetermined value or less.

[0125] The heating temperature for obtaining a glass ceramic solid electrolyte cannot be generally defined because it varies depending on the structure of the glass ceramic solid electrolyte to be obtained. In general, however, the heating temperature is preferably 130° C. or higher, more preferably 135° C. or higher, and even more preferably 140° C. or higher. There is no particular upper limit, but the heating temperature is preferably 300° C. or lower, more preferably 280° C. or lower, and even more preferably 250° C. or lower.

[0126] The heating time is not particularly limited as long as the desired glass ceramic solid electrolyte can be obtained, but is preferably, for example, 1 minute or more, more preferably 10 minutes or more, even more preferably 30 minutes or more, and even more preferably 1 hour or more. The upper limit of the heating time is not particularly limited, but is preferably 24 hours or less, more preferably 10 hours or less, even more preferably 5 hours or less, and even more preferably 3 hours or less.

[0127] In addition, the heating is preferably performed in an inert gas atmosphere (e.g., nitrogen atmosphere, argon atmosphere) or reduced pressure atmosphere (particularly in vacuum). This is because deterioration (e.g., oxidation) of the glass ceramic solid electrolyte can be prevented. The heating method is not particularly limited, and examples thereof include a method using an agitator-type dryer, a hot plate, a vacuum heating device, an argon gas atmosphere furnace, and a firing furnace. In addition, industrially, a horizontal dryer having a heating means and a feeding mechanism, a horizontal vibration fluidized dryer, etc. can also be used, and may be selected according to the amount of processing to be heated, but an agitator-type dryer such as a PV mixer is preferred from the viewpoint of preventing granulation.

[0128] (Mechanical treatment of amorphous or glass-ceramic solid electrolytes) In this embodiment, it is also preferable to mechanically treat the amorphous or glass ceramic solid electrolyte obtained after the complex decomposition (hereinafter, in the explanation of this mechanical treatment, the amorphous or glass ceramic solid electrolyte (including a solid electrolyte in which at least a part of the amorphous solid electrolyte has been converted into glass ceramic) may be simply referred to as a solid electrolyte). The mechanical treatment is performed by subjecting the amorphous or glass ceramic solid electrolyte to a mechanical treatment of a volume-based average particle size of 3 μm or more measured by a laser diffraction particle size distribution measuring method and a specific surface area of ​​20 m2 measured by a BET method. 2 It is preferable that the solid electrolyte obtained in the present embodiment, which has a molecular weight of 0.1 to 1.0 kg / g or more, is subjected to at least one mechanical treatment selected from crushing and granulation. That is, the mechanical treatment of the solid electrolyte is characterized in that the solid electrolyte is subjected to at least one mechanical treatment selected from crushing and granulation. By mechanically treating the solid electrolyte of the present embodiment, it is possible to easily adjust the morphology to a desired one or to obtain a crystalline solid electrolyte having a desired morphology and high ionic conductivity. Moreover, the solid electrolyte of the present embodiment is different from primary particles in which highly active newly formed surfaces are exposed by crushing coarse particles, and therefore can be easily atomized by crushing without using a dispersant.

[0129] The method for mechanically treating the solid electrolyte is not particularly limited as long as it includes at least one treatment selected from crushing and granulation, and examples of the method include methods using equipment such as a grinder or a stirrer. The agitator may be, for example, a mechanical agitation mixer equipped with an agitating blade in a tank, as exemplified above as an apparatus that can be used in the method for producing a solid electrolyte. The mechanical agitation mixer may be a high-speed agitation mixer, a double-arm mixer, or the like, and any type may be used. However, from the viewpoint of more easily adjusting the desired morphology, a high-speed agitation mixer is preferred. More specifically, as described above, the high-speed agitation mixer may be a vertical shaft rotary mixer, a horizontal shaft rotary mixer, or the like, as well as various devices such as a high-speed swirling thin film agitator and a high-speed shear agitator. Among them, from the viewpoint of more easily adjusting the desired morphology, a high-speed swirling thin film agitator (also referred to as a "thin film swirling high-speed mixer") is preferred.

[0130] A pulverizer that can be used in the mechanical treatment of a solid electrolyte is one having a volume-based average particle size of at least 3 μm as measured by a laser diffraction particle size distribution measurement method, and a specific surface area of ​​at least 20 m as measured by the BET method. 2 An example of such a grinding machine is a grinding machine having a rotor capable of stirring a solid electrolyte having a molecular weight of 1.0 to 1.0 kg / g or more. In the mechanical treatment of solid electrolytes, the crushing (atomization) and granulation (particle growth) of the solid electrolyte can be adjusted by adjusting the peripheral speed of the rotor of the pulverizer. In other words, the average particle size can be reduced by crushing, and the average particle size can be increased by granulation, so that the crystallinity of the solid electrolyte and the morphology of the crystalline solid electrolyte resulting from this embodiment can be easily adjusted freely. More specifically, crushing can be achieved by rotating the rotor at a low peripheral speed, and granulation can be achieved by rotating the rotor at a high peripheral speed. In this way, the morphology of the solid electrolyte can be easily adjusted by simply adjusting the peripheral speed of the rotor.

[0131] Regarding the peripheral speed of the rotating body, low peripheral speed and high peripheral speed cannot be generally defined because they can vary depending on, for example, the particle size, material, and amount of the medium used in the grinding machine. For example, in the case of a device that does not use a grinding medium such as a ball or bead, such as a high-speed rotating thin film type agitator, even at a relatively high peripheral speed, mainly crushing occurs and granulation is difficult to occur. On the other hand, in the case of a device that uses a grinding medium such as a ball mill or a bead mill, as described above, crushing can be performed at a low peripheral speed and granulation can be performed at a high peripheral speed. Therefore, if the specified conditions of the grinding device, grinding medium, etc. are the same, the peripheral speed at which crushing is possible is smaller than the peripheral speed at which granulation is possible. Therefore, for example, in the condition where granulation is possible at a peripheral speed of 6 m / s, a low peripheral speed means less than 6 m / s, and a high peripheral speed means 6 m / s or more.

[0132] As a more specific example of a pulverizer, a media type pulverizer can be given. Media type pulverizers are roughly classified into a container drive type pulverizer and a media agitation type pulverizer. Examples of the container-driven grinding machine include a stirring tank, a grinding tank, or a combination of these, such as a ball mill or a bead mill. As the ball mill or bead mill, any of various types such as a rotary type, a rolling type, a vibrating type, or a planetary type can be used. Examples of media agitation type crushers include impact type crushers such as cutter mills, hammer mills, and pin mills; tower type crushers such as tower mills; agitation tank type crushers such as attritors, aquamizers, and sand grinders; flow tank type crushers such as Viscomill and Pearl Mill; flow pipe type crushers; annular type crushers such as Coball mills; and continuous dynamic type crushers.

[0133] In terms of more easily adjusting the desired morphology in the mechanical treatment of the solid electrolyte, a container-driven pulverizer is preferred, and among them, a bead mill and a ball mill are preferred. A container-driven pulverizer such as a bead mill and a ball mill is provided with a container such as a stirring tank or a grinding tank that contains the precursor for mechanical treatment as a rotating body that can stir the precursor for mechanical treatment. Therefore, as described above, the morphology of the solid electrolyte can be easily adjusted by adjusting the peripheral speed of the rotating body. Bead mills and ball mills can adjust the morphology by adjusting the particle size, material, amount of beads, balls, etc. used, making it possible to adjust the morphology more finely and also to adjust morphology that has not been seen before. For example, as a bead mill, a centrifugal separation type that can use so-called microbeads with extremely fine particles (φ0.015 to 1 mm or so) (e.g., Ultra Apex Mill (UAM)) can be used.

[0134] Regarding the adjustment of morphology, the smaller the energy applied to the solid electrolyte, i.e., the slower the circumferential speed of the rotor, or the smaller the particle size of the beads, balls, etc., the smaller the average particle size (crushing) and the larger the specific surface area tends to be, whereas the larger the energy is, i.e., the faster the circumferential speed of the rotor, or the larger the particle size of the beads, balls, etc., the larger the average particle size (granulation) and the smaller the specific surface area tends to be. Also, for example, the longer the time of mechanical treatment, the larger the average particle size tends to be (granulation).

[0135] The particle size of the media used in a bead mill, ball mill, etc. may be appropriately determined taking into consideration the desired morphology as well as the type and scale of the apparatus used, and is usually preferably 0.01 mm or more, more preferably 0.015 mm or more, even more preferably 0.02 mm or more, and still more preferably 0.04 mm or more, with the upper limit being preferably 3 mm or less, more preferably 2 mm or less, even more preferably 1 mm or less, and still more preferably 0.8 mm or less. Examples of the material of the medium include metals such as stainless steel, chrome steel, and tungsten carbide; ceramics such as zirconia and silicon nitride; and minerals such as agate.

[0136] The processing time for the mechanical treatment may be appropriately determined taking into consideration the desired morphology as well as the type and scale of the apparatus used, and is usually preferably 5 seconds or more, more preferably 30 seconds or more, even more preferably 3 minutes or more, and still more preferably 15 minutes or more, with the upper limit being preferably 5 hours or less, more preferably 3 hours or less, even more preferably 2 hours or less, and still more preferably 1.5 hours or less. The peripheral speed of the rotating body in the mechanical treatment (the rotation speed of an apparatus such as a bead mill or ball mill) may be appropriately determined taking into consideration the desired morphology as well as the type and scale of the apparatus used, and is usually preferably 0.5 m / s or more, more preferably 1 m / s or more, even more preferably 2 m / s or more, and even more preferably 3 m / s or more, with the upper limit being preferably 55 m / s or less, more preferably 40 m / s or less, even more preferably 25 m / s or less, and even more preferably 15 m / s or less. The peripheral speed may be the same or may be changed during the process.

[0137] The mechanical treatment can be carried out together with a solvent. The solvent can be appropriately selected from the solvents exemplified above, and from the viewpoint of obtaining a more stable and high ion conductivity together with a predetermined average particle size and specific surface area, an aliphatic hydrocarbon solvent, an alicyclic hydrocarbon solvent, an aromatic hydrocarbon solvent, and an ether-based solvent are preferred, and heptane, cyclohexane, toluene, ethylbenzene, diethyl ether, diisopropyl ether, dibutyl ether, dimethoxyethane, cyclopentyl methyl ether, tert-butyl methyl ether, and anisole are more preferred, heptane, toluene, and ethylbenzene are even more preferred, and heptane and toluene are even more preferred. In the mechanical treatment of the solid electrolyte, the solid electrolyte can be easily atomized by crushing without using a complexing agent. However, a dispersant may be used from the viewpoint of further increasing the dispersion and more efficiently atomizing the solid electrolyte. Of the above solvents, for example, an ether-based solvent can function as a dispersant. The amount of the solvent used may be such that the content of the solid electrolyte relative to the total amount of the solvent contained in the solid electrolyte slurry is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more, with the upper limit being preferably 30 mass % or less, more preferably 20 mass % or less, and even more preferably 15 mass % or less.

[0138] Mechanical treatment may be performed on the amorphous solid electrolyte before crystallization after complex decomposition, or on the glass ceramic solid electrolyte after heating. When mechanically treating an amorphous solid electrolyte, crystallization is required after that. On the other hand, when mechanically treating a glass ceramic solid electrolyte, heat treatment for crystallization is not required in principle after the mechanical treatment of the glass ceramic solid electrolyte. However, although the energy of the mechanical treatment is relatively small, some or all of the glass ceramic solid electrolyte may be vitrified (amorphized). In this case, crystallization (heating) may be performed again. That is, in this embodiment, heating may be included after the mechanical treatment of the solid electrolyte. Also, in this embodiment, heating may be performed not only after the mechanical treatment but also before the treatment. That is, in the treatment method of this embodiment, heating may be included after the mechanical treatment of the precursor for mechanical treatment. Also, in the treatment method of this embodiment, heating may be performed not only after the mechanical treatment but also before the treatment. The crystalline solid electrolyte of the present embodiment has a morphology consisting of a collection of chemically stable primary particles, unlike primary particles in which new surfaces are exposed by crushing coarse particles, and therefore granulation during crystallization is relatively suppressed, making it easier to adjust the morphology compared to conventional methods of finely granulating coarse particles.

[0139] According to this embodiment, a solid electrolyte having a desired morphology can be easily produced. The volume-based average particle size of the solid electrolyte obtained according to the present embodiment can be adjusted as desired, but is usually 0.05 μm or more, preferably 0.07 μm or more, more preferably 0.1 μm or more, and even more preferably 0.15 μm or more, and the upper limit is usually 50 μm or less, preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and even more preferably 10 μm or less. The specific surface area of ​​the solid electrolyte can also be adjusted as desired, but is usually set to 0.1 m 2 / g or more, preferably 0.3m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, with the upper limit usually being 70m 2 / g or less, preferably 50m 2 / g or less, more preferably 45m 2 / g or less, more preferably 40m 2 / g or less.

[0140] The glass ceramic solid electrolyte obtained by this embodiment has high ionic conductivity, excellent battery performance, and is less likely to generate hydrogen sulfide, so it is suitable for use in batteries. It is particularly suitable when lithium atoms are used as the conductive species. The solid electrolyte of this embodiment may be used in a positive electrode layer, a negative electrode layer, or an electrolyte layer. Each layer may be manufactured by a known method.

[0141] [Positive electrode mixture, negative electrode mixture] For example, when used in a positive electrode layer or a negative electrode layer, the positive electrode active material and the negative electrode active material are dispersed and mixed in a slurry of the electrolyte precursor, which is an electrolyte precursor-containing material, and then dried, so that the electrolyte precursor adheres to the surface of the active material. Furthermore, as in the above embodiment, the electrolyte precursor is heated to become an amorphous solid electrolyte or a crystalline solid electrolyte. At this time, by heating the electrolyte precursor together with the active material, a positive electrode composite or a negative electrode composite with the solid electrolyte adhered to the surface of the active material is obtained.

[0142] The positive electrode active material can be used without any particular limitation as long as it can promote the battery chemical reaction accompanied by the movement of lithium ions resulting from the lithium atoms preferably used as the atoms that exhibit ionic conductivity in this embodiment in relation to the negative electrode active material. Examples of such positive electrode active materials that can insert and remove lithium ions include oxide-based positive electrode active materials and sulfide-based positive electrode active materials.

[0143] Preferred examples of oxide-based positive electrode active materials include lithium-containing transition metal composite oxides such as LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminate), LNCO (lithium nickel cobalt oxide), and olivine-type compounds (LiMeNPO4, Me=Fe, Co, Ni, Mn). Examples of sulfide-based positive electrode active materials include titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), and nickel sulfide (Ni3S2). In addition to the above positive electrode active materials, niobium selenide (NbSe3) and the like can also be used. In this embodiment, the positive electrode active material may be used alone or in combination of two or more kinds.

[0144] As the negative electrode active material, any material that can promote a battery chemical reaction accompanied by the movement of lithium ions due to lithium atoms, such as an atom that is preferably used as an atom that exhibits ion conductivity in this embodiment, preferably a metal that can form an alloy with lithium atoms, an oxide thereof, an alloy of the metal and lithium atoms, etc., can be used without any particular limitation. As such a negative electrode active material capable of inserting and removing lithium ions, any material known as a negative electrode active material in the battery field can be used without any limitation. Examples of such negative electrode active materials include metallic lithium, metallic indium, metallic aluminum, metallic silicon, metallic tin, and other metallic lithium or metals capable of forming alloys with metallic lithium, oxides of these metals, and alloys of these metals with metallic lithium.

[0145] The electrode active material used in this embodiment may have a coating layer on its surface. The material for forming the coating layer may be an ion conductor such as a nitride, an oxide, or a composite of an atom, preferably a lithium atom, that exhibits ion conductivity in the glass ceramic solid electrolyte used in this embodiment. Specifically, lithium nitride (Li3N), Li4GeO4, or other ion conductors having a main structure, such as Li 4-2x Zinc x Conductors with a lithiated crystal structure such as GeO4, and conductors with a Li3PO4-type framework such as Li 4-x Ge 1-x P x Conductors with thiolicon-type crystal structures such as S4, La 2 / 3-x Li 3x Examples of such conductors include those having a perovskite crystal structure such as TiO3, and those having a NASICON crystal structure such as LiTi2(PO4)3. Also, Li y Ti 3-y O4(0 <y<3)、Li4Ti5O 12 Examples of conductors include lithium titanates such as (LTO), lithium metal oxides of metals belonging to Group 5 of the periodic table such as LiNbO3 and LiTaO3, and oxide-based conductors such as Li2O-B2O3-P2O5, Li2O-B2O3-ZnO, and Li2O-Al2O3-SiO2-P2O5-TiO2.

[0146] An electrode active material having a coating layer can be obtained, for example, by applying a solution containing various atoms constituting the material that forms the coating layer to the surface of an electrode active material, and then calcining the electrode active material after application at a temperature of preferably 200°C or higher and 400°C or lower. Here, the solution containing various atoms may be a solution containing alkoxides of various metals such as lithium ethoxide, titanium isopropoxide, niobium isopropoxide, tantalum isopropoxide, etc. In this case, the solvent may be an alcohol solvent such as ethanol or butanol, an aliphatic hydrocarbon solvent such as hexane, heptane, or octane, or an aromatic hydrocarbon solvent such as benzene, toluene, or xylene. The above attachment may be performed by immersion, spray coating, or the like.

[0147] From the viewpoint of improving production efficiency and battery performance, the firing temperature is preferably from 200°C to 400°C, more preferably from 250°C to 390°C, and the firing time is usually from about 1 minute to 10 hours, preferably from 10 minutes to 4 hours.

[0148] The coverage of the coating layer is preferably 90% or more, more preferably 95% or more, and even more preferably 100% based on the surface area of ​​the electrode active material, that is, the entire surface is preferably covered. The thickness of the coating layer is preferably 1 nm or more, more preferably 2 nm or more, and the upper limit is preferably 30 nm or less, more preferably 25 nm or less. The thickness of the coating layer can be measured by cross-sectional observation using a transmission electron microscope (TEM), and the coverage can be calculated from the thickness of the coating layer, atomic analysis value, and BET surface area.

[0149] In addition, the battery preferably uses a current collector in addition to the positive electrode layer, electrolyte layer, and negative electrode layer, and a known current collector can be used. For example, a layer of a material that reacts with the solid electrolyte, such as Au, Pt, Al, Ti, or Cu, coated with Au or the like can be used. EXAMPLES

[0150] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.

[0151] Example 1 In a 1L reactor equipped with an impeller, 13.19g of lithium sulfide, 21.26g of diphosphorus pentasulfide, 4.15g of lithium bromide, and 6.40g of lithium iodide were introduced under a nitrogen atmosphere. 100mL of tetramethylethylenediamine (TMEDA) as a complexing agent and 800mL of cyclohexane as a solvent were added, and the impeller was operated to mix by stirring. 456g of zirconia balls (diameter: 0.5mmφ) (bead filling rate in the grinding chamber: 80%) were charged into a bead mill capable of circulating operation ("Star Mill LMZ015 (model number)", manufactured by Ashizawa Finetech Co., Ltd.), and grinding was performed for 60 minutes while circulating between the reactor and the grinding chamber under the conditions of pump flow rate: 550mL / min, peripheral speed: 8m / s, and mill jacket temperature: 20℃, to obtain a slurry of an electrolyte precursor. Next, the obtained electrolyte precursor slurry was immediately dried at room temperature (23° C.) under reduced pressure (vacuum degree 300 Pa or less) to obtain a powdered electrolyte precursor.

[0152] 30 g of the obtained powder electrolyte precursor was filled into a can (volume: 150 ml) of a vibration dryer in a glove box. The vacuum was set to 100 Pa or less, and the temperature was gradually increased until the powder temperature reached 110°C. Heating (complex decomposition) was performed by circulating a heat medium heated to a predetermined temperature by a heat medium unit in the vibration dryer jacket. During the heat treatment, the amount of heat medium circulated was adjusted so that the vacuum did not exceed 100 Pa. The end of complex decomposition was determined by the elapse of one hour or more after the powder temperature exceeded 110°C and the vacuum degree returned to the value before the start of heating. The obtained amorphous solid electrolyte was heated (crystallized) at a heating temperature of 200°C under reduced pressure (vacuum degree 300 Pa or less) for 2 hours to obtain a glass ceramic solid electrolyte.

[0153] Example 2 30 g of the powdered electrolyte precursor obtained in Example 1 was filled into a can (volume: 150 ml) of a vibration dryer in a glove box. The vacuum was set to 300 Pa or less, and the temperature was gradually increased until the powder temperature reached 110°C. The vacuum of 300 Pa was maintained by adjusting the amount of N2 introduced into the suction port of the vacuum pump. Heating (complex decomposition) was performed by circulating a heat medium that had been heated to a predetermined temperature by a heat medium unit in the vibration dryer jacket. The end of the complex decomposition was determined to be when more than 2 hours had passed since the powder temperature exceeded 110°C. The obtained amorphous solid electrolyte was heated (crystallized) at a heating temperature of 200°C under reduced pressure (vacuum of 300 Pa or less) for 2 hours to obtain a glass ceramic solid electrolyte.

[0154] Comparative Example 1 20 g of the powder electrolyte precursor obtained in Example 1 was filled into a glass Schlenk flask (volume: 500 ml) in a glove box. The flask was evacuated to a vacuum of 300 Pa, and heated (complex decomposition) at 110° C. for 4 hours while the flask was left stationary without stirring. The obtained amorphous solid electrolyte was heated (crystallization) at a heating temperature of 200° C. under reduced pressure (vacuum of 300 Pa or less) for 2 hours to obtain a glass ceramic solid electrolyte.

[0155] Comparative Example 2 20 g of the powder electrolyte precursor obtained in Example 1 was filled into a glass Schlenk flask (volume: 500 ml) equipped with a stirrer in a glove box. This was heated (complexation) at 110°C for 4 hours with a vacuum of 1000 Pa and rotating the stirrer. The obtained amorphous solid electrolyte was heated (crystallization) at a heating temperature of 200°C under reduced pressure (vacuum of 300 Pa or less) for 2 hours to obtain a glass ceramic solid electrolyte.

[0156] Comparative Example 3 20 g of the powder electrolyte precursor obtained in Example 1 was filled into a glass Schlenk flask (volume: 500 ml) equipped with a stirrer in a glove box. The flask was heated (complex decomposition) at 110° C. for 20 hours while rotating the stirrer under a vacuum of 1000 Pa to obtain an amorphous solid electrolyte.

[0157] Comparative Example 4 In a 1L reactor equipped with an agitator, 15.3 g of lithium sulfide and 24.7 g of diphosphorus pentasulfide were added under a nitrogen atmosphere. After the agitator was operated, 400 mL of tetrahydrofuran, which had been cooled to -20°C in advance, was introduced into the vessel. After allowing the temperature to rise naturally to room temperature (23°C), stirring was continued for 72 hours, and the resulting reaction liquid slurry was poured into a glass filter (pore size: 40-100 μm) to obtain a solid content, which was then dried at 90°C to obtain 38 g of Li3PS4 (purity: 90% by mass) as a white powder. The XRD pattern of the obtained powder showed a halo pattern, and it was confirmed that the Li3PS4 was amorphous. The obtained Li3PS4 did not contain a complexing agent as a constituent.

[0158] A total of 2.0 g of the amorphous Li3PS4 and lithium iodide were weighed and introduced into a Schlenk flask (volume: 100 mL) with a stirring bar under a nitrogen atmosphere so that the molar ratio of Li3PS4:LiI was 1:1. After rotating the stirring bar, 20 mL of DME, a complexing agent, was added. After continuing for 3 days, the mixture was dried at 50°C (room temperature: 23°C) to obtain a powder. The obtained powder was then heated at 100°C under vacuum for 2 hours.

[0159] (Complexing agent content) The powdered electrolyte precursors and the crystalline solid electrolytes obtained in Examples 1 and 2, Comparative Examples 1 and 2, and a portion of the amorphous solid electrolyte obtained in Comparative Example 3 were dissolved in methanol, and the resulting methanol solutions were analyzed by gas chromatography to measure the content of tetramethylethylenediamine (complexing agent). The results are shown in Table 1.

[0160] [Table 1]

[0161] (Crystal structure) The electrolyte precursor, the amorphous solid electrolyte, and the glass ceramic solid electrolyte obtained in Example 1 were subjected to powder X-ray diffraction (XRD) measurement using an X-ray diffraction (XRD) device (D2 PHASER, manufactured by Bruker Corporation). The X-ray diffraction spectrum is shown in FIG. 3. It was confirmed that all of them contained a thiolicon region II type crystal structure.

[0162] In this embodiment, the X-ray diffraction (XRD) measurement was carried out as follows. The powder of the solid electrolyte in each example was cut into a groove of 20 mm diameter and 0.2 mm depth with glass to prepare a sample. This sample was measured with a Kapton film for XRD without exposing it to air. The above-mentioned powder X-ray diffraction measurement apparatus was used under the following conditions.

[0163] Tube voltage: 30kV Tube current: 10mA X-ray wavelength: Cu-Kα ray (1.5418Å) Optical system: Concentration method Slit configuration: Solar slit 4°, divergence slit 1mm, Kβ filter (Ni plate) Detector: Semiconductor detector Measurement range: 2θ=10-60deg Step width, scan speed: 0.05deg, 0.05deg / sec

[0164] The peak intensity was calculated by the following method. The half-width is calculated using the range of the maximum peak ±0.5°. If the ratio of the Lorentz function is A (0≦A≦1), the peak intensity corrected for the background is B, the 2θ maximum peak is C, the peak position in the range used for calculation (C±0.5°) is D, the half-width parameter is E, the background is F, and each peak intensity in the peak range used for calculation is G, calculate the following for each peak position when the variables are A, B, C, D, E, and F. H=G-{B×{A / (1+(DC)2 / E2)+(1-A)×exp(-1×(DC)2 / E2)}+F} The H values ​​were summed within the range of ±0.5° of the peak C to be calculated, and the sum was minimized with GRG nonlinearity using the solver function of the spreadsheet software Excel (Microsoft) to obtain the peak intensity. The peak of the standard sample was the 28.6° peak indicating the (111) surface of Si. The peak intensity Is was 353894.

[0165] In the X-ray diffraction spectrum of the electrolyte precursor (Fig. 1), peaks different from those derived from the raw materials used were observed, and the X-ray diffraction pattern was different from that of the amorphous solid electrolyte and the glass ceramic solid electrolyte (Figs. 4 and 5). In addition, powder X-ray diffraction (XRD) measurements were also performed on the raw materials used in each example (amorphous Li3PS4, lithium bromide, lithium iodide, lithium sulfide, diphosphorus pentasulfide, crystalline Li3PS4), and the resulting X-ray diffraction spectra are shown in Fig. 6. The X-ray diffraction spectrum of the electrolyte precursor showed an X-ray diffraction pattern different from that of the raw materials. It was confirmed that the X-ray diffraction spectrum of the amorphous solid electrolyte obtained in Example 1 had a broad pattern with no peaks other than those derived from the raw materials. In addition, in the X-ray diffraction spectrum of the glass-ceramic solid electrolyte, crystallization peaks were detected mainly at 2θ = 20.2° and 23.6°, and it had a thiolithiregion II type crystal structure. When the ionic conductivity was measured, it was 4.1 × 10 -3 (S / cm), confirming that it has high ionic conductivity.

[0166] In the X-ray diffraction spectrum of the amorphous solid electrolyte of Example 1, a peak of LiX complex is slightly observed at 2θ=12.4°. The intensity ratio Ic / Is between the peak intensity Ic of this peak and the peak intensity Is of the standard sample at 2θ=28.6° was calculated to be 0.0045. In addition, the intensity ratio Ix / Igc between the diffraction peak intensity Ix (2θ=28.3, LiBr) of LiX in the glass ceramic solid electrolyte after crystallization and the diffraction peak intensity Igc of the glass ceramic was calculated to be 0.08. Therefore, even if a GC-formed solid electrolyte similar to that after crystallization is obtained by complex decomposition, it is understood that no elution or aggregation of LiX occurs. Note that the peaks near 2θ=12°, 20°, and 23° in FIG. 4 are peaks of LiX complex, and are different from the peaks of 2θ=20.2° and 23.6° of the glass ceramic that appear after crystallization.

[0167] [Table 2]

[0168] [Table 3]

[0169] On the other hand, the intensity ratio Ic / Is in the X-ray diffraction spectrum of the amorphous solid electrolyte obtained in the comparative example was larger than that in the examples. This is considered to be due to the dissolution or aggregation of halogen during complex decomposition. Furthermore, in the crystalline solid electrolyte of Comparative Example 1, a peak derived from lithium bromide was clearly confirmed. Furthermore, in Comparative Example 2, peaks derived from crystalline Li3PS4 and Li7P2S8I1 were observed, and the ionic conductivity was low. In Comparative Example 3, although the complex decomposition time was extended, an amorphous solid electrolyte equivalent to that of Comparative Example 2 was obtained, so crystallization was not performed. In the above examples, a GC-containing solid electrolyte was not obtained by complex decomposition. However, if the GC-containing solid electrolyte obtained after complex decomposition was the glass ceramic solid electrolyte obtained in Comparative Examples 1 to 3, a glass ceramic solid electrolyte with high ionic conductivity would not be obtained even if the crystallization was promoted by heat treatment. This is because LiX aggregation occurs, as can be seen from the fact that the LiX peak is larger than the glass ceramic peak. For the solid electrolyte obtained in Comparative Example 4, peaks derived from lithium iodide were clearly observed at 2θ=26° and 29° (FIG. 7).

[0170] (Ionic Conductivity) The ionic conductivity of the solid electrolytes obtained in Examples 1 and 2 and Comparative Examples 1, 2, and 4 was measured as follows. From the obtained solid electrolyte, a 10 mm diameter (cross-sectional area S: 0.785 cm 2 ) and a height (L) of 0.1-0.3 cm were molded into a circular pellet to prepare a sample. Electrode terminals were attached to the top and bottom of the sample, and measurements were made at 25°C using an AC impedance method (frequency range: 5 MHz-0.5 Hz, amplitude: 10 mV) to obtain a Cole-Cole plot. The real part Z' (Ω) at the point where -Z'' (Ω) is minimum near the right end of the arc observed in the high frequency region was taken as the bulk resistance R (Ω) of the electrolyte, and the ionic conductivity σ (S / cm) was calculated according to the following formula: R=ρ(L / S) σ=1 / ρ The obtained ionic conductivity σ is shown in Table 2.

[0171] [Table 4]

[0172] In the examples, a glass ceramic solid electrolyte having high ionic conductivity was obtained. On the other hand, in Comparative Example 1 where no vibration was applied, and Comparative Example 2 where stirring was applied instead of vibration but the degree of vacuum was not set to less than 1000 Pa, the complex decomposition product specified in the present application was not obtained, and a solid electrolyte having high ionic conductivity like that of the examples was not obtained. In addition, as in Comparative Example 4, a solid electrolyte (amorphous Li3PS4) and lithium halide were mixed with a complexing agent, and the crystalline solid electrolyte obtained without passing through an amorphous or glass ceramic solid electrolyte contained lithium iodide, so that the ionic conductivity was lower than that of the solid electrolyte of the examples. [Industrial Applicability]

[0173] According to the present embodiment, it is possible to produce a glass ceramic solid electrolyte having high ionic conductivity, excellent battery performance, and suppressing the generation of hydrogen sulfide. The glass ceramic solid electrolyte obtained by the production method of the present embodiment is suitable for use in batteries, particularly batteries used in information-related devices and communication devices such as personal computers, video cameras, and mobile phones.

Claims

1. A method for producing a glass-ceramic solid electrolyte, comprising the steps of: mixing a raw material containing lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms with a complexing agent to obtain a slurry of an electrolyte precursor containing a complex crystal containing the complexing agent, lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms as constituent components; drying the electrolyte precursor slurry; and complexing the electrolyte precursor obtained by the drying to obtain an amorphous solid electrolyte in which an intensity ratio Ic / Is of a diffraction peak intensity Ic of a LiX complex (wherein X represents a halogen) to an intensity Is of a standard sample is 0.02 or less, or a GC solid electrolyte in which an intensity ratio Ix / Igc of a diffraction peak intensity Ix of LiX to a diffraction peak intensity Igc of a glass ceramic is 0.5 or less.

2. The method for producing a glass-ceramic solid electrolyte according to claim 1 , wherein the drying step includes removing the complexing agent that is a liquid.

3. 3. The method for producing a glass-ceramic solid electrolyte according to claim 1, wherein the decomplexation comprises removing the complexing agent which is a component of the complex crystal.

4. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 3, further comprising heating.

5. 5. The method for producing a glass-ceramic solid electrolyte according to claim 1, wherein after the complex decomposition, the amorphous solid electrolyte or the GC solid electrolyte is subjected to at least one mechanical treatment selected from crushing and granulation.

6. 6. The method for producing a glass-ceramic solid electrolyte according to claim 1, wherein the amount of the complexing agent contained in the amorphous solid electrolyte or the GC solid electrolyte is set to 15 mass % or less by the complex decomposition.

7. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 6, wherein a vibration dryer is used in the complex decomposition.

8. The method for producing a glass ceramic solid electrolyte according to any one of claims 1 to 7, wherein the drying is fluidized drying using a medium.

9. 9. The method for producing a glass-ceramic solid electrolyte according to claim 1, wherein the raw material contains at least one selected from the group consisting of lithium sulfide, lithium halide, phosphorus sulfide, phosphorus halide, thiophosphoryl halide, and halogen molecules.

10. 10. The method for producing a glass-ceramic solid electrolyte according to claim 1, wherein the electrolyte precursor slurry further contains a solvent, and the solvent contains a solvent that does not dissolve the raw material inclusions, the complexing agent, and the electrolyte precursor.

11. The method for producing a glass ceramic solid electrolyte according to claim 10, wherein 5 to 50 mL of the solvent is used per 1 g of the total mass of the raw material contents.

12. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 11, wherein the complexing agent contains a compound having a heteroatom.

13. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 12, wherein the complexing agent includes a compound having an amino group.

14. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 13, wherein the complexing agent contains a compound having at least two tertiary amino groups in the molecule.

15. The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 14, wherein the solid electrolyte contains a thiolicon region II type crystal structure.

16. The solid electrolyte is crystalline Li when measured by X-ray diffraction using CuKα radiation. 3 P.S. 4 The method for producing a glass-ceramic solid electrolyte according to any one of claims 1 to 15, wherein the glass-ceramic solid electrolyte does not have diffraction peaks at 2θ = 17.5° and 26.1° corresponding to

Citation Information

Patent Citations

  • Liquid solution for formation of a solid electrolyte-containing layer of all-solid type lithium secondary battery, all-solid type lithium secondary battery, and method for manufacturing the same

    JP2014191899A

  • Method for producing solid electrolyte

    JP2014225425A

  • Method of preparing sulfide-based solid electrolyte, and method of preparing all-solid secondary battery

    JP2019200856A

  • SOLID LITHIUM ION CONDUCTING MATERIAL AND METHOD FOR MANUFACTURING SOLID LITHIUM ION CONDUCTING MATERIAL - Patent application

    JP2021535582A

  • Production method of solid electrolyte

    WO2014192309A1