Copolymer, injection molded body, and compressed member
A tetrafluoroethylene/perfluoro(propyl vinyl ether) copolymer with optimized monomer content and melt flow rate addresses mold corrosion and enhances sealing and electrolyte resistance in high-temperature applications, ensuring effective use in non-aqueous electrolyte batteries.
Patent Information
- Application Number
- JP2021161170
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing fluororesins used in high-temperature environments, such as non-aqueous electrolyte batteries, face challenges with corrosion of molds during molding, low glass transition temperatures, high water vapor and electrolyte permeability, and poor sealing properties, leading to potential electrolyte leakage and fluorine ion elution.
A tetrafluoroethylene/perfluoro(propyl vinyl ether) copolymer with specific monomer content (2.0-2.8% PPVE by mass) and melt flow rate (5-23 g/10 min) is developed, featuring a high glass transition temperature, low functional group count (≤50 per unit), and optimized for injection molding, reducing mold corrosion and enhancing sealing and electrolyte resistance.
The copolymer exhibits excellent heat resistance, low water vapor and electrolyte permeability, resistance to electrolyte leakage, and superior sealing properties at high temperatures, maintaining integrity in harsh environments.
Smart Images

Figure 0007584383000005 
Figure 0007584383000001 
Figure 0007584383000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a copolymer, an injection molded article, and a compressed member. [Background technology]
[0002] Tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA) is known as a fluororesin that has excellent mechanical, chemical and electrical properties and is also melt-processable.
[0003] For example, Patent Document 1 describes a sealing material made of a fluorine-containing polymer having polymerization units based on tetrafluoroethylene and polymerization units based on one or more types of perfluoro(alkyl vinyl ether), characterized in that the fluorine-containing polymer contains polymerization units based on perfluoro(alkyl vinyl ether) in an amount of 4.0 mass% or less relative to the total polymerization units and has a melt flow rate of 0.1 to 100 g / 10 min. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-177574 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present disclosure is to provide a copolymer from which a molded article can be obtained that has a high glass transition temperature, can be easily molded by injection molding, is resistant to corrosion of a mold used for molding, and has excellent electrical properties, and further has very low water vapor permeability, very low electrolyte permeability, is resistant to electrolyte leakage, has excellent crack resistance against compressive stress, heat deformation resistance, and abrasion resistance, has very high sealing properties at high temperatures, and is resistant to elution of fluorine ions into the electrolyte. [Means for solving the problem]
[0006] According to the present disclosure, a fluoropolymer containing tetrafluoroethylene units and perfluoro(propyl vinyl ether) units is provided, the content of the perfluoro(propyl vinyl ether) units being 2.0 to 2.8% by mass based on the total amount of monomer units, the melt flow rate at 372°C being 5 to 23 g / 10 min, and the number of functional groups being 10 carbon atoms in the main chain. 6 Copolymers are provided in which the number of units per unit is 50 or less.
[0007] The present disclosure also provides an injection-molded article containing the above-mentioned copolymer.
[0008] The present disclosure also provides a compressed member containing the above-mentioned copolymer.
[0009] The present disclosure also provides an extrudate containing the above copolymer.
[0010] The present disclosure also provides a covered electric wire including a covering layer containing the above-mentioned copolymer.
[0011] The present disclosure also provides a film containing the above copolymer. Effect of the Invention
[0012] According to the present disclosure, it is possible to provide a copolymer from which a molded article can be obtained that has a high glass transition temperature, can be easily molded by injection molding, is resistant to corrosion of a mold used for molding, and has excellent electrical properties; further, has very low water vapor permeability, has excellent low electrolyte permeability, is resistant to electrolyte leakage, has excellent crack resistance against compressive stress, heat deformation resistance, and abrasion resistance, has very excellent sealing properties at high temperatures, and is resistant to elution of fluorine ions into the electrolyte. [Brief description of the drawings]
[0013] [Figure 1]FIG. 1 is a schematic cross-sectional view of a test jig used in an electrolyte leakage test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Specific embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.
[0015] The copolymers of the present disclosure contain tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.
[0016] Patent Document 1 describes that in-vehicle secondary batteries are sometimes exposed to high temperatures of 85°C or higher during use, and in order to maintain airtightness and liquid-tightness inside the battery, it is important that the sealing material retains sufficient compression recovery even under such harsh use conditions and can maintain high adhesion between the battery can and the sealing body.
[0017] However, there is a demand for copolymers that can exhibit excellent sealing properties even in higher temperature environments, and in particular, there is a demand for copolymers that can exhibit excellent sealing properties even at temperatures above the glass transition temperature of the copolymer.
[0018] It has been found that by appropriately adjusting the content of PPVE units, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units, the glass transition temperature of the copolymer is sufficiently increased and the copolymer exhibits excellent heat resistance. It has also been found that such a copolymer can be easily molded by injection molding, is less likely to corrode the mold used for molding, and has excellent electrical properties. It has also been found that a molded body containing such a copolymer has very low water vapor permeability, low electrolyte permeability, is less likely to leak electrolyte, has excellent crack resistance against compressive stress, heat deformation resistance and abrasion resistance, has very good sealing properties at high temperatures, and is less likely to dissolve fluorine ions into the electrolyte.
[0019] The copolymers of the present disclosure are melt-processable fluoroplastics, meaning that the polymers can be melted and processed using conventional processing equipment such as extruders and injection molding machines.
[0020] The content of the PPVE unit in the copolymer is 2.0 to 2.8% by mass based on the total monomer units. The content of the PPVE unit in the copolymer is preferably 2.1% by mass or more, more preferably 2.2% by mass or more, even more preferably 2.3% by mass or more, particularly preferably 2.4% by mass or more, and preferably 2.7% by mass or less. By having the content of the PPVE unit in the copolymer within the above range, it is possible to obtain a copolymer having a higher glass transition temperature, which is very excellent in low water vapor permeability, excellent in low electrolyte permeability, is less likely to cause electrolyte leakage, and has excellent crack resistance against compressive stress, excellent heat distortion resistance, and wear resistance, and which can give a molded product with excellent sealability at high temperatures.
[0021] The content of TFE units in the copolymer is preferably 97.2 to 98.0% by mass, more preferably 97.8% by mass or less, even more preferably 97.7% by mass or less, still more preferably 97.7% by mass or less, particularly preferably 97.6% by mass or less, and preferably 97.3% by mass or more, based on the total monomer units. By having the content of TFE units in the copolymer within the above range, it is possible to obtain a copolymer having a higher glass transition temperature, and a copolymer that gives a molded product having excellent low water vapor permeability, excellent low electrolyte permeability, low electrolyte leakage resistance, excellent crack resistance against compressive stress, excellent heat distortion resistance, and wear resistance, and excellent sealability at high temperatures.
[0022] In the present disclosure, the content of each monomer unit in the copolymer is 19 Measured by F-NMR.
[0023] The copolymer may also contain monomer units derived from a monomer copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 4.0 mass%, more preferably 0.05 to 0.80 mass%, and further preferably 0.1 to 0.5 mass%, based on the total monomer units of the copolymer.
[0024] Monomers that can be copolymerized with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF2) n Z 4 (In the formula, Z 1 , Z 2 and Z 3 are the same or different and represent H or F; Z 4 represents H, F or Cl, and n represents an integer of 2 to 10. 1 (In the formula, Rf 1 represents a perfluoroalkyl group having 1 to 5 carbon atoms.) Among these, HFP is preferred.
[0025] The copolymer is preferably at least one selected from the group consisting of copolymers consisting of only TFE units and PPVE units, and TFE / HFP / PPVE copolymers, and more preferably a copolymer consisting of only TFE units and PPVE units.
[0026] The melt flow rate (MFR) of the copolymer is 5 to 23 g / 10 min. The MFR of the copolymer is preferably 6 g / 10 min or more, more preferably 7 g / 10 min or more, even more preferably 8 g / 10 min or more, preferably 21 g / 10 min or less, more preferably 20 g / 10 min or less, even more preferably 19 g / 10 min or less, particularly preferably 18 g / 10 min or less, and most preferably 16 g / 10 min or less. By having the MFR of the copolymer within the above range, it is possible to obtain a copolymer that can be easily molded by injection molding, has excellent low water vapor permeability, excellent low electrolyte permeability, is less likely to leak electrolyte, has excellent abrasion resistance and heat deformation resistance, and gives a molded product that is excellent in sealing property at high temperatures.
[0027] In this disclosure, the MFR is a value obtained in accordance with ASTM D1238 using a melt indexer, as the mass of polymer flowing out per 10 minutes from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm under a load of 5 kg at 372°C (g / 10 minutes).
[0028] The MFR can be adjusted by adjusting the type and amount of a polymerization initiator used when polymerizing the monomers, the type and amount of a chain transfer agent, and the like.
[0029] In the present disclosure, the copolymer has a main chain carbon number of 10 6 The number of functional groups per unit is 50 or less. The main chain carbon number of the copolymer is 10 6The number of functional groups per unit is preferably 40 or less, more preferably 30 or less, even more preferably 20 or less, even more preferably 15 or less, particularly preferably 10 or less, and most preferably less than 6. By the number of functional groups of the copolymer being within the above range, the mold used for molding is less likely to be corroded, and the electrical properties of the copolymer can be further improved. In addition, it is possible to obtain a copolymer that gives a molded product that is more excellent in low electrolyte permeability, is more unlikely to leak electrolyte, and is more unlikely to dissolve fluorine ions into electrolyte. Furthermore, by the number of functional groups of the copolymer being within the above range, it is possible to suppress molding defects such as foaming caused by the decomposition of the functional groups of the copolymer to generate gas.
[0030] The type of functional group and the number of functional groups can be identified by infrared spectroscopy.
[0031] Specifically, the number of functional groups is measured by the following method. First, the copolymer is molded by cold pressing to prepare a film having a thickness of 0.25 to 0.30 mm. This film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer, and a difference spectrum with a base spectrum that is completely fluorinated and has no functional groups is obtained. From the absorption peaks of specific functional groups that appear in this difference spectrum, the number of carbon atoms in the copolymer is calculated according to the following formula (A): 6 Calculate the number of functional groups per unit, N.
[0032] N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm)
[0033] For reference, the absorption frequencies, molar absorption coefficients, and correction coefficients for several functional groups are shown in Table 1. The molar absorption coefficients were determined from the FT-IR measurement data of low-molecular-weight model compounds. [Table 1]
[0034] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are shown in the table. The absorption frequencies of -CF2H, -COF, -COOH free, -COOH bonded, -COOCH3, and -CONH2 are several tens of Kaiser (cm -1 ) lower.
[0035] For example, the functional group number of -COF is the absorption frequency of 1883 cm due to -CF2COF. -1 The number of functional groups determined from the absorption peak of -CH2COF and the absorption frequency of 1840 cm -1 The number of functional groups is the sum of the number of functional groups determined from the absorption peaks of
[0036] The functional groups are those present at the ends of the main chain or side chains of the copolymer, and those present in the main chain or side chains. The number of functional groups may be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH.
[0037] The functional group is introduced into the copolymer by, for example, a chain transfer agent or a polymerization initiator used in producing the copolymer. For example, when an alcohol is used as a chain transfer agent or a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced into the main chain end of the copolymer. In addition, the functional group is introduced into the side chain end of the copolymer by polymerizing a monomer having a functional group.
[0038] By subjecting the copolymer having such a functional group to a fluorination treatment, a copolymer having a number of functional groups within the above range can be obtained. That is, the copolymer of the present disclosure is preferably a fluorination-treated copolymer. It is also preferable that the copolymer of the present disclosure has a -CF3 end group.
[0039] The melting point of the copolymer is preferably 305 to 317° C., and more preferably 305 to 315° C. When the melting point is within the above range, it is possible to obtain a copolymer that gives a molded article having even more excellent sealability, particularly at high temperatures.
[0040] In this disclosure, melting points can be measured using a differential scanning calorimeter (DSC).
[0041] The glass transition temperature (Tg) of the copolymer is preferably 95° C. or higher, more preferably 98° C. or higher, more preferably 99° C. or higher, and preferably 110° C. or lower, more preferably 105° C. or lower, and even more preferably 103° C. or lower. Since the copolymer of the present disclosure can have such a high glass transition temperature, it is possible to obtain a copolymer that exhibits excellent heat resistance and gives a molded article that is even more excellent in sealability, particularly at high temperatures.
[0042] In the present disclosure, the glass transition temperature can be measured by dynamic viscoelasticity measurement.
[0043] The water vapor permeability of the copolymer is preferably 8.5 g cm / m 2 or less, and more preferably 8.0 g cm / m 2 or less, and more preferably 7.9 g cm / m 2 and even more preferably 7.6 g cm / m 2 The copolymer of the present disclosure has an excellent low water vapor permeability because the content of the PPVE unit, the melt flow rate (MFR) and the number of functional groups of the copolymer containing the TFE unit and the PPVE unit are appropriately adjusted. Therefore, by using a molded body containing the copolymer of the present disclosure as, for example, a compressed member of a secondary battery, the permeation of moisture can be effectively prevented even under high temperature and high humidity conditions.
[0044] In the present disclosure, the water vapor permeability can be measured under conditions of a temperature of 95° C. for 30 days. The water vapor permeability can be specifically measured by the method described in the Examples.
[0045] The electrolyte permeability of the copolymer is preferably 7.5 g cm / m 2 More preferably, it is 7.3 g cm / m or less. 2 or less, and more preferably 7.1 g cm / m 2 The copolymer of the present disclosure has an excellent low electrolyte permeability because the content of the PPVE unit, the melt flow rate (MFR) and the number of functional groups of the copolymer containing the TFE unit and the PPVE unit are appropriately adjusted. Therefore, by using a molded body containing the copolymer of the present disclosure as, for example, a compressed member of a secondary battery, the permeation of the electrolyte contained in the secondary battery can be effectively prevented.
[0046] In the present disclosure, the electrolyte permeability can be specifically measured by the method described in the Examples.
[0047] The copolymer of the present disclosure has an amount of eluted fluorine ions detected in an electrolyte immersion test of preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and even more preferably 0.7 ppm or less, by mass. When the amount of eluted fluorine ions is within the above range, the generation of gases such as HF in the nonaqueous electrolyte battery can be further suppressed, and the deterioration of the battery performance and the shortening of the battery life of the nonaqueous electrolyte battery can be further suppressed.
[0048] In the present disclosure, the electrolyte immersion test can be performed by preparing a test piece having a weight equivalent to 10 pieces of molded bodies (15 mm × 15 mm × 0.2 mm) using the copolymer, placing the test piece and 2 g of dimethyl carbonate (DMC) in a glass sample bottle in a constant temperature bath at 80°C, and leaving it for 144 hours.
[0049] The copolymer of the present disclosure can provide a molded article having excellent sealability at high temperatures. The sealability at high temperatures can be evaluated by measuring the storage modulus (E') at 150°C, the recovery at 150°C, and the surface pressure at 150°C. A copolymer having a high storage modulus (E') at 150°C and a large recovery at 150°C can continue to exhibit sufficient resilience for a long period of time even at high temperatures. In addition, a copolymer having a high surface pressure at 150°C can provide a molded article having excellent sealability at high temperatures. The copolymer of the present disclosure can provide a molded article having excellent sealability even at high temperatures exceeding the glass transition temperature of the copolymer.
[0050] The storage modulus (E') of the copolymer at 150°C is preferably 140 MPa or more, more preferably 145 MPa or more, even more preferably 148 MPa or more, and preferably 1000 MPa or less, more preferably 500 MPa or less, and even more preferably 300 MPa or less. When the storage modulus (E') of the copolymer at 150°C is within the above range, it is possible to obtain a copolymer that can continue to exhibit sufficient rebound resilience even at high temperatures for a long period of time, and that can give a molded product with even more excellent sealability at high temperatures.
[0051] The storage modulus (E') can be measured by dynamic viscoelasticity measurement in the range of 30 to 250°C under conditions of a temperature increase rate of 2°C / min and a frequency of 10 Hz. The storage modulus (E') at 150°C can be increased by adjusting the PPVE unit content and melt flow rate (MFR) of the copolymer.
[0052] The surface pressure of the copolymer at 150° C. is preferably 1.60 MPa or more, more preferably 1.65 MPa or more, and even more preferably 1.70 MPa or more, and although there is no particular upper limit, it may be 3.00 MPa or less. The surface pressure at 150° C. can be increased by adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups of the copolymer.
[0053] The surface pressure can be calculated from the height of the test piece obtained from the copolymer after it has been deformed by 50% compression deformation rate, by leaving it at 150°C for 18 hours, releasing the compression state, and leaving it at room temperature for 30 minutes, and then measuring the height of the test piece (the height of the test piece after compression deformation). The surface pressure can be calculated from the height of the test piece after compression deformation and the storage modulus (MPa) at 150°C according to the following formula. 150℃ surface pressure (MPa) = (t2-t1) / t1×E' t1: original height of test piece before compressive deformation (mm) x 50% t2: Height of the test piece after compressive deformation (mm) E': Storage modulus at 150℃ (MPa)
[0054] The recovery of the copolymer at 150°C can be measured using the same method as the measurement of surface pressure. The recovery of the molded product at 150°C is the difference (t2-t1) between the height of the test piece after compressive deformation (t2) and the original height of the test piece before compressive deformation (t1) when the test piece is deformed at a compressive deformation rate of 50%. The recovery of the molded product at 150°C can be increased by adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups of the copolymer.
[0055] The copolymer of the present disclosure preferably has a dielectric loss tangent of 6.0×10 at 6 GHz. -4 More preferably, it is 5.0×10 or less. -4 More preferably, it is 4.0×10 -4 In recent years, with an increase in the amount of information to be transmitted, there is a tendency for radio waves in the higher frequency range to be used more and more. For example, microwaves of 3 to 30 GHz are used for high frequency wireless LAN, satellite communications, mobile phone base stations, etc. Materials having a low dielectric tangent (tan δ) are required as materials for use in communication devices using such high frequencies. When the dielectric tangent of the copolymer of the present disclosure is in the above range, the attenuation rate of high frequency signals is greatly reduced, which is preferable.
[0056] In the present disclosure, the dielectric loss tangent is a value obtained by measuring the change in resonance frequency and electric field strength in a temperature range of 20 to 25°C using a network analyzer and a cavity resonator manufactured by Agilent Technologies.
[0057] The copolymer of the present disclosure can be produced by a polymerization method such as suspension polymerization, solution polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization method, emulsion polymerization or suspension polymerization is preferable. In these polymerizations, each condition such as temperature and pressure, polymerization initiator and other additives can be appropriately set according to the composition and amount of the copolymer.
[0058] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.
[0059] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, for example: dialkyl peroxycarbonates such as di-normal propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, and di-2-ethoxyethyl peroxydicarbonate; Peroxyesters such as t-butyl peroxyisobutyrate and t-butyl peroxypivalate; Dialkyl peroxides such as di-t-butyl peroxide; Di[fluoro(or fluorochloro)acyl]peroxides; The following are some representative examples.
[0060] Di[fluoro(or fluorochloro)acyl]peroxides include diacyl peroxides represented by [(RfCOO)-]2 (Rf is a perfluoroalkyl group, a ω-hydroperfluoroalkyl group, or a fluorochloroalkyl group).
[0061] Examples of di[fluoro(or fluorochloro)acyl]peroxides include di(ω-hydro-dodecafluorohexanoyl)peroxide, di(ω-hydro-tetradecafluoroheptanoyl)peroxide, di(ω-hydro-hexadecafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoroparyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, and di(ω-chloro-decafluorohexa di(ω-chloro-tetradecafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexadecafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydrododecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutanoyl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecafluorooctanoyl) peroxide, di(pentachlorotetradecafluorodecanoyl) peroxide, di(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.
[0062] The water-soluble radical polymerization initiator may be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide, diglutaric acid peroxide, t-butyl permalate, t-butyl hydroperoxide, etc. A reducing agent such as a sulfite may be used in combination with the peroxide, and the amount used may be 0.1 to 20 times the amount of the peroxide.
[0063] In the polymerization, a surfactant, a chain transfer agent, and a solvent can be used, and conventionally known surfactants, chain transfer agents, and solvents can be used.
[0064] As the surfactant, a known surfactant can be used, for example, a nonionic surfactant, an anionic surfactant, a cationic surfactant, etc. Among them, a fluorine-containing anionic surfactant is preferable, and a linear or branched fluorine-containing anionic surfactant having 4 to 20 carbon atoms, which may contain ether-bonded oxygen (i.e., an oxygen atom may be inserted between carbon atoms), is more preferable. The amount of the surfactant added (relative to the polymerization water) is preferably 50 to 5000 ppm.
[0065] Examples of the chain transfer agent include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; and halogenated hydrocarbons such as carbon tetrachloride, chloroform, methylene chloride, and methyl chloride. The amount of the chain transfer agent to be added may vary depending on the magnitude of the chain transfer constant of the compound used, but is usually used in the range of 0.01 to 20% by mass based on the polymerization solvent.
[0066] The solvent may be water or a mixed solvent of water and alcohol.
[0067] In the suspension polymerization, in addition to water, a fluorine-based solvent may be used. Examples of the fluorine-based solvent include hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, and CF2ClCF2CFHCl; chlorofluoroalkanes such as CF2ClCFClCF2CF3 and CF3CFClCFClCF3; hydrofluoroalkanes such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, and CF3CF2CF2CF2CF2CF2CF2H; CH3OC2F5, CH3OC3F5 Examples of the fluorine-based solvent include hydrofluoroethers such as CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, and CF3CHFCF2OCH2CF3; and perfluoroalkanes such as perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, and CF3CF2CF2CF2CF2CF3, among which perfluoroalkanes are preferred. The amount of the fluorine-based solvent used is preferably 10 to 100% by mass relative to the aqueous medium from the standpoints of suspension and economy.
[0068] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure is appropriately determined depending on the type, amount, and vapor pressure of the solvent used, as well as other polymerization conditions such as polymerization temperature, and may usually be 0 to 9.8 MPaG.
[0069] When an aqueous dispersion containing the copolymer is obtained by the polymerization reaction, the copolymer contained in the aqueous dispersion is coagulated, washed, and dried to recover the copolymer. When a slurry is obtained by the polymerization reaction, the copolymer is recovered by removing the slurry from the reaction vessel, washing, and drying. By drying, the copolymer can be recovered in the form of a powder.
[0070] The copolymer obtained by polymerization may be molded into pellets. The molding method for molding into pellets is not particularly limited, and conventionally known methods can be used. For example, a method of melt-extruding the copolymer using a single-screw extruder, a twin-screw extruder, or a tandem extruder, cutting the copolymer to a predetermined length, and molding the copolymer into pellets can be mentioned. The extrusion temperature during melt extrusion needs to be changed depending on the melt viscosity of the copolymer and the manufacturing method, and is preferably from the melting point of the copolymer +20°C to the melting point of the copolymer +140°C. The method of cutting the copolymer is not particularly limited, and conventionally known methods such as a strand cut method, a hot cut method, an underwater cut method, and a sheet cut method can be adopted. The obtained pellets may be heated to remove volatiles in the pellets (degassing treatment). The obtained pellets may be treated by contacting them with hot water at 30 to 200°C, steam at 100 to 200°C, or hot air at 40 to 200°C.
[0071] The copolymer obtained by polymerization may be fluorinated. The fluorination treatment can be carried out by contacting the unfluorinated copolymer with a fluorine-containing compound. The fluorination treatment can convert thermally unstable functional groups of the copolymer, such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and relatively thermally stable functional groups, such as -CF2H, to extremely thermally stable -CF3. As a result, the total number (functional group number) of -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and -CF2H of the copolymer can be easily adjusted to the above-mentioned range.
[0072] The fluorine-containing compound is not particularly limited, but may be a fluorine radical source that generates fluorine radicals under fluorination treatment conditions, such as F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, halogen fluorides (e.g., IF5, ClF3), etc.
[0073] A fluorine radical source such as F2 gas may be of 100% concentration, but from the viewpoint of safety, it is preferable to mix it with an inert gas and dilute it to 5 to 50 mass%, more preferably to dilute it to 15 to 30 mass%. Examples of the inert gas include nitrogen gas, helium gas, and argon gas, and nitrogen gas is preferable from the viewpoint of economy.
[0074] The conditions for the fluorination treatment are not particularly limited, and the copolymer in a molten state may be contacted with a fluorine-containing compound, but the treatment is usually carried out at a temperature below the melting point of the copolymer, preferably 20 to 240°C, more preferably 100 to 220°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably 5 to 25 hours. The fluorination treatment is preferably carried out by contacting a non-fluorinated copolymer with fluorine gas (F2 gas).
[0075] A composition may be obtained by mixing the copolymer of the present disclosure with other components as necessary, such as fillers, plasticizers, processing aids, release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, UV absorbers, antioxidants, foaming agents, fragrances, oils, softeners, and dehydrofluorination agents.
[0076] Examples of the filler include silica, kaolin, clay, organo clay, talc, mica, alumina, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, and glass fibers. Examples of the conductive agent include carbon black. Examples of the plasticizer include dioctyl phthalate and pentaerythritol. Examples of the processing aid include carnauba wax, sulfone compounds, low molecular weight polyethylene, and fluorine-based aids. Examples of the dehydrofluorination agent include organic oniums and amidines.
[0077] As the other component, a polymer other than the above-mentioned copolymer may be used. Examples of the other polymer include a fluororesin, a fluororubber, and a non-fluorinated polymer other than the above-mentioned copolymer.
[0078] Examples of a method for producing the above composition include a method of dry mixing the copolymer and other components, and a method of previously mixing the copolymer and other components in a mixer and then melt-kneading them in a kneader, melt extruder, or the like.
[0079] The copolymer of the present disclosure or the above composition can be used as a processing aid, molding material, etc., but is preferably used as a molding material. Aqueous dispersions, solutions, suspensions, and copolymer / solvent systems of the copolymer of the present disclosure are also available, which can be applied as paints, or used for encapsulation, impregnation, and film casting. However, since the copolymer of the present disclosure has the above-mentioned properties, it is preferable to use it as the above-mentioned molding material.
[0080] The copolymer of the present disclosure or the above composition may be molded to obtain a molded body.
[0081] The method of molding the copolymer or the composition is not particularly limited, and examples thereof include injection molding, extrusion, compression, blow, transfer, roto-molding, and roto-lining. As the molding method, among others, extrusion, compression, injection, or transfer molding is preferred, and injection, extrusion, or transfer molding is more preferred, and injection molding is even more preferred, because the molded body can be produced with high productivity. That is, the molded body is preferably an extrusion molded body, a compression molded body, an injection molded body, or a transfer molded body, and more preferably an injection molded body, an extrusion molded body, or a transfer molded body, because the molded body can be produced with high productivity, and more preferably an injection molded body.
[0082] The shape of the molded article is not particularly limited, and may be, for example, a hose, a pipe, a tube, a wire coating, a sheet, a seal, a gasket, a packing, a film, a tank, a roller, a bottle, a container, or the like.
[0083] The copolymer of the present disclosure, the above-mentioned composition, or the above-mentioned molded article can be used, for example, in the following applications. Food packaging films, lining materials for fluid transfer lines used in food manufacturing processes, packings, sealing materials, sheets and other fluid transfer components for food manufacturing equipment; Chemical stoppers, packaging films, lining materials for fluid transfer lines used in pharmaceutical manufacturing processes, packings, sealing materials, sheets and other chemical transfer components; Inner lining materials for chemical tanks and pipes in chemical plants and semiconductor factories; O-rings, tubes, packing, valve core materials, hoses, seals, etc. used in automobile fuel systems and peripheral devices; hoses, seals, and other fuel transfer materials used in automobile automatic transmission devices; Carburetor flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in automobile engines and peripheral devices, automobile brake hoses, air conditioner hoses, radiator hoses, electric wire covering materials, and other automobile parts; Semiconductor manufacturing equipment O-rings, tubes, packing, valve core materials, hoses, seal materials, rolls, gaskets, diaphragms, joints, and other chemical liquid transfer components for semiconductor equipment; Paint rolls for painting equipment, hoses, tubes, ink containers and other paint and ink components; Food and beverage tubes and food and beverage hoses and other food and beverage transport components such as tubes, hoses, belts, packings, and joints, food packaging materials, and glass cooking equipment; Waste liquid transport components such as tubes and hoses for transporting waste liquid; Components for transporting high-temperature liquids, such as tubes and hoses for transporting high-temperature liquids; Steam piping components such as steam piping tubes and hoses; Anticorrosive tapes for piping, such as tapes wrapped around piping on ship decks, etc.; Various coating materials such as electric wire coating materials, optical fiber coating materials, transparent front coating materials and back coating materials to be applied to the light incident surface of photovoltaic elements of solar cells; Sliding parts such as diaphragms in diaphragm pumps and various packings; Agricultural films, weather-resistant covers for various roofing materials and side walls; Interior materials used in the construction industry, and glass covering materials such as non-flammable fire-resistant safety glass; Lining materials such as laminated steel sheets used in the home appliance sector, etc.;
[0084] Further examples of the fuel transfer members used in the fuel systems of the above-mentioned automobiles include fuel hoses, filler hoses, evaporative hoses, etc. The above-mentioned fuel transfer members can also be used as fuel transfer members for sour gasoline, alcohol-resistant fuels, and fuels containing gasoline additives such as methyl tertiary butyl ether and amine-resistant fuels.
[0085] The above-mentioned chemical stoppers and packaging films for chemicals have excellent chemical resistance against acids, etc. Another example of the above-mentioned chemical liquid transfer member is anticorrosive tape wrapped around piping in chemical plants.
[0086] Examples of the molded article include radiator tanks for automobiles, chemical tanks, bellows, spacers, rollers, gasoline tanks, containers for transporting waste liquids, containers for transporting high-temperature liquids, and fishery / fish farming tanks.
[0087] Further examples of the molded article include parts used for automobile bumpers, door trims, instrument panels, food processing equipment, cooking appliances, water- and oil-repellent glass, lighting-related equipment, display panels and housings for office automation equipment, illuminated signs, displays, liquid crystal displays, mobile phones, printed circuit boards, electric and electronic components, miscellaneous goods, trash cans, bathtubs, unit baths, ventilation fans, lighting frames, etc.
[0088] A molded article containing the copolymer of the present disclosure has excellent heat resistance, can be easily produced by injection molding without corroding the mold, has extremely low water vapor permeability, has excellent low electrolyte permeability, is less likely to leak electrolyte, has excellent crack resistance against compressive stress, heat deformation resistance and abrasion resistance, has excellent sealing properties at high temperatures, and is less likely to dissolve fluorine ions into the electrolyte, and therefore can be suitably used as a compressed member containing the copolymer.
[0089] The compressed member of the present disclosure exhibits high surface pressure even when deformed at a high compression deformation rate. The compressed member of the present disclosure can be used in a state compressed and deformed at a compression deformation rate of 10% or more, and can be used in a state compressed and deformed at a compression deformation rate of 20% or more or 25% or more. By using the compressed member of the present disclosure after being deformed at such a high compression deformation rate, a certain level of resilience can be maintained for a long period of time, and sealing and insulating properties can be maintained for a long period of time.
[0090] The compressed member of the present disclosure exhibits a high storage modulus, a high recovery amount, and a high surface pressure even when deformed at a high compression deformation rate at high temperatures. The compressed member of the present disclosure can be used in a state where it is compressed and deformed at 150°C or higher and a compression deformation rate of 10% or more, and can be used in a state where it is compressed and deformed at 150°C or higher and a compression deformation rate of 20% or more or 25% or more. By using the compressed member of the present disclosure after being deformed at such a high temperature and high compression deformation rate, a certain rebound resilience can be maintained for a long period of time even at high temperatures, and sealing properties and insulating properties at high temperatures can be maintained for a long period of time.
[0091] The above compression deformation ratio is the compression deformation ratio of the part with the largest compression deformation ratio when the compressed member is used in a compressed state. For example, when a flat compressed member is used in a state compressed in its thickness direction, it is the compression deformation ratio in the thickness direction. Also, for example, when the compressed member is used in a state where only a part of it is compressed, it is the compression deformation ratio of the part with the largest compression deformation ratio among the compressed parts.
[0092] The size and shape of the compressed member of the present disclosure may be appropriately set depending on the application, and are not particularly limited. The shape of the compressed member of the present disclosure may be, for example, annular. In addition, the compressed member of the present disclosure may have a shape such as a circle, an oval, or a rectangle with rounded corners in a plan view, and may have a through hole in the center.
[0093] The compressed member of the present disclosure is preferably used as a member for constituting a non-aqueous electrolyte battery. The compressed member of the present disclosure is particularly suitable as a member used in contact with the non-aqueous electrolyte in a non-aqueous electrolyte battery, since it has very excellent low water vapor permeability, excellent low electrolyte permeability, is unlikely to leak electrolyte, has excellent crack resistance against compressive stress, excellent thermal deformation resistance and abrasion resistance, has very excellent sealing properties at high temperatures, and is unlikely to dissolve fluorine ions into the electrolyte. That is, the compressed member of the present disclosure may have a surface in contact with the non-aqueous electrolyte in the non-aqueous electrolyte battery.
[0094] The compressed member of the present disclosure is unlikely to dissolve fluorine ions into the non-aqueous electrolyte. Therefore, by using the compressed member of the present disclosure, it is possible to suppress an increase in the fluorine ion concentration in the non-aqueous electrolyte. As a result, by using the compressed member of the present disclosure, it is possible to suppress the generation of gases such as HF in the non-aqueous electrolyte battery, and to suppress the deterioration of the battery performance and the shortening of the life of the non-aqueous electrolyte battery.
[0095] Since the compressed member of the present disclosure can further suppress the generation of gases such as HF in a nonaqueous electrolyte battery and can further suppress the deterioration of battery performance and shortening of life of the nonaqueous electrolyte battery, the amount of eluted fluorine ions detected in an electrolyte immersion test is preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and more preferably 0.7 ppm or less, based on mass. The electrolyte immersion test can be performed by preparing a test piece having a weight equivalent to 10 molded bodies (15 mm x 15 mm x 0.2 mm) using the compressed member, placing the test piece and 2 g of dimethyl carbonate (DMC) in a glass sample bottle in a thermostatic chamber at 80°C, and leaving it for 144 hours.
[0096] The compressed member of the present disclosure has excellent liquid-tightness and low electrolyte permeability, and is unlikely to leak or penetrate electrolyte. Therefore, by using the compressed member of the present disclosure, poor battery performance and shortened life of a non-aqueous electrolyte battery can be suppressed.
[0097] The electrolyte leakage amount of the compressed member of the present disclosure is preferably 0.0030 g / 1000 hrs or less, and more preferably 0.0025 g / 1000 hrs or less, because this can further suppress poor battery performance and shortened life of the nonaqueous electrolyte battery. The electrolyte leakage amount of the compressed member can be measured by the method described in the Examples.
[0098] The compressed member of the present disclosure is difficult to transmit water vapor. Therefore, by using the compressed member of the present disclosure, it is possible to suppress the transmission of water vapor from the outside to the secondary battery. As a result, by using the compressed member of the present disclosure, it is possible to suppress the deterioration of the battery performance and the shortening of the life of the nonaqueous electrolyte battery.
[0099] The water vapor permeability of the compressed member of the present disclosure is preferably 8.5 g cm / m because this can further suppress deterioration of the battery performance and shortening of the life of the nonaqueous electrolyte battery. 2 or less, and more preferably 8.0 g cm / m 2 or less, and more preferably 7.9 g cm / m 2 and even more preferably 7.6 g cm / m 2 The water vapor transmission rate of a compressed member can be measured at a temperature of 95°C for 30 days.
[0100] The nonaqueous electrolyte battery is not particularly limited as long as it is a battery containing a nonaqueous electrolyte, and examples thereof include a lithium ion secondary battery, a lithium ion capacitor, etc. Examples of members constituting the nonaqueous electrolyte battery include a sealing member, an insulating member, etc.
[0101] The non-aqueous electrolyte is not particularly limited, but one or more of known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate can be used. The non-aqueous electrolyte battery may further include an electrolyte. The electrolyte is not particularly limited, but LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, and the like can be used.
[0102] The compressed member of the present disclosure can be suitably used as, for example, a sealing member such as a sealing gasket or sealing packing, or an insulating member such as an insulating gasket or insulating packing. A sealing member is a member used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating member is a member used to insulate electricity. The compressed member of the present disclosure may be a member used for both sealing and insulating purposes.
[0103] The compressed member of the present disclosure has excellent heat resistance and heat deformation resistance, and is also very excellent in sealing properties at high temperatures, so it can be suitably used in high-temperature environments. For example, the compressed member of the present disclosure is suitably used in an environment where the maximum temperature is 40° C. or higher. For example, the compressed member of the present disclosure is suitably used in an environment where the maximum temperature is 150° C. or higher. Examples of cases in which the compressed member of the present disclosure may reach such high temperatures include a case in which the compressed member is attached to a battery in a compressed state, and then other battery components are attached to the battery by welding, and a case in which a nonaqueous electrolyte battery generates heat.
[0104] The compressed member of the present disclosure has excellent low water vapor permeability, excellent low electrolyte permeability, is difficult to leak electrolyte, has excellent crack resistance against compressive stress, excellent heat deformation resistance and abrasion resistance, is very excellent in sealing properties at high temperatures, and is difficult to dissolve fluorine ions into the electrolyte, so it can be suitably used as a sealing member for a nonaqueous electrolyte battery or an insulating member for a nonaqueous electrolyte battery. For example, when a battery such as a nonaqueous electrolyte secondary battery is charged, the temperature of the battery may temporarily reach 40°C or higher, particularly temporarily reach 150°C or higher. The compressed member of the present disclosure does not lose its high resilience even when it is used in a battery such as a nonaqueous electrolyte secondary battery after being deformed at a high compression deformation rate at high temperatures, and even when it comes into contact with a nonaqueous electrolyte at high temperatures. Therefore, when the compressed member of the present disclosure is used as a sealing member, it has excellent sealing properties and the sealing properties are maintained for a long period of time even at high temperatures. In addition, the compressed member of the present disclosure has excellent insulating properties because it contains the above-mentioned copolymer. Therefore, when the compressed member of the present disclosure is used as an insulating member, it adheres firmly to two or more conductive members, preventing short circuits for a long period of time.
[0105] The copolymer of the present disclosure has a low dielectric tangent at 6 GHz and can therefore be suitably used as a material for high-frequency signal transmission products.
[0106] The above-mentioned high-frequency signal transmission products are not particularly limited as long as they are products used for transmitting high-frequency signals, and examples thereof include (1) insulating plates for high-frequency circuits, insulators for connecting parts, molded plates such as printed wiring boards, (2) molded bodies such as bases for high-frequency vacuum tubes and antenna covers, and (3) coated electric wires such as coaxial cables and LAN cables. The above-mentioned high-frequency signal transmission products can be suitably used in devices that utilize microwaves, particularly microwaves of 3 to 30 GHz, such as satellite communication devices and mobile phone base stations.
[0107] In the above-mentioned high-frequency signal transmission product, the copolymer of the present disclosure can be suitably used as an insulator because of its low dielectric loss tangent.
[0108] The above (1) molded plate is preferably a printed wiring board in that it can obtain good electrical properties. The above printed wiring board is not particularly limited, but examples thereof include printed wiring boards for electronic circuits of mobile phones, various computers, communication devices, etc. The above (2) molded body is preferably an antenna cover in that it has low dielectric loss.
[0109] The above-mentioned (3) covered electric wire is preferably a covered electric wire having a covering layer containing the copolymer of the present disclosure. That is, a molded product containing the copolymer of the present disclosure can be suitably used as a covering layer containing the copolymer.
[0110] Commercially available tetrafluoroethylene / fluoro(alkyl vinyl ether) copolymers are known to have a continuous use temperature of 260° C. Continuous use temperature refers to the maximum operating temperature that the polymer can withstand continuously. Recently, there has been a need for copolymers that can be used in harsher working environments, i.e., have a continuous use temperature of greater than 260° C. In many real-world industrial applications in oil and gas fields, there is an emerging need to have melt-processable polymeric materials with a continuous use temperature of greater than 260° C. to withstand the extremely high operating temperatures encountered in construction and the like. For example, when deep drilling, data communication cables may be exposed to temperatures of 280° C. or more in downhole wells. A molded article containing the copolymer of the present disclosure can have a continuous use temperature of 280° C. The molded article containing the copolymer of the present disclosure does not melt even at an extremely high temperature of 280° C., and the coating layer made of the molded article maintains its coating without forming ruptures or cracks due to thermal load, allowing for continuous use. Therefore, the molded article containing the copolymer of the present disclosure is suitable for use as a coating layer of a coated electric wire used in an environment with a maximum temperature of 280° C. or higher.
[0111] The coated electric wire comprises a core wire and a coating layer that is provided around the core wire and contains the copolymer of the present disclosure. For example, the coating layer can be an extrusion molded body obtained by melt-extrusion molding the copolymer of the present disclosure onto the core wire. The coated electric wire is suitable for use as a high-frequency transmission cable, a flat cable, a heat-resistant cable, etc., particularly suitable for use as a high-frequency transmission cable, since the coating layer has excellent heat resistance and a low dielectric loss tangent.
[0112] The core wire may be made of a metal conductor material such as copper or aluminum. The core wire preferably has a diameter of 0.02 to 3 mm. The core wire preferably has a diameter of 0.04 mm or more, more preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire preferably has a diameter of 2 mm or less.
[0113] Specific examples of the core wire include AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 micrometers), AWG-26 (solid copper wire with a diameter of 404 micrometers), AWG-24 (solid copper wire with a diameter of 510 micrometers), and AWG-22 (solid copper wire with a diameter of 635 micrometers).
[0114] The thickness of the coating layer is preferably 0.1 to 3.0 mm. It is also preferable that the thickness of the coating layer is 2.0 mm or less.
[0115] An example of a high-frequency transmission cable is a coaxial cable. A coaxial cable generally has a structure in which an internal conductor, an insulating coating layer, an external conductor layer, and a protective coating layer are laminated in this order from the core to the outer periphery. A molded article containing the copolymer of the present disclosure can be suitably used as an insulating coating layer containing a copolymer. The thickness of each layer in the above structure is not particularly limited, but usually, the internal conductor has a diameter of about 0.1 to 3 mm, the insulating coating layer has a thickness of about 0.3 to 3 mm, the external conductor layer has a thickness of about 0.5 to 10 mm, and the protective coating layer has a thickness of about 0.5 to 2 mm.
[0116] The coating layer may contain air bubbles, and it is preferable that the air bubbles are uniformly distributed in the coating layer.
[0117] The average bubble diameter of the bubbles is not limited, but is preferably 60 μm or less, more preferably 45 μm or less, even more preferably 35 μm or less, even more preferably 30 μm or less, particularly preferably 25 μm or less, and even more preferably 23 μm or less. The average bubble diameter is preferably 0.1 μm or more, and more preferably 1 μm or more. The average bubble diameter can be determined by taking an electron microscope image of the cross section of the electric wire, calculating the diameter of each bubble by image processing, and averaging the results.
[0118] The coating layer may have an expansion rate of 20% or more. More preferably, it is 30% or more, even more preferably, it is 33% or more, and even more preferably, it is 35% or more. There is no particular upper limit, but it is, for example, 80%. The upper limit of the expansion rate may be 60%. The expansion rate is a value calculated by ((specific gravity of electric wire coating material-specific gravity of coating layer) / specific gravity of electric wire coating material)×100. The expansion rate can be appropriately adjusted according to the application, for example, by adjusting the amount of gas inserted in the extruder described later, or by selecting the type of gas to be dissolved.
[0119] The coated electric wire may have another layer between the core wire and the coating layer, or may have another layer (outer layer) around the coating layer. When the coating layer contains bubbles, the electric wire of the present disclosure may have a two-layer structure (skin-foam) in which a non-foamed layer is inserted between the core wire and the coating layer, a two-layer structure (foam-skin) in which the outer layer is coated with a non-foamed layer, or even a three-layer structure (skin-foam-skin) in which the outer layer of skin-foam is coated with a non-foamed layer. The non-foamed layer is not particularly limited, and may be a resin layer made of a resin such as a TFE / HFP copolymer, a TFE / PAVE copolymer, a TFE / ethylene copolymer, a vinylidene fluoride polymer, a polyolefin resin such as polyethylene (PE), or polyvinyl chloride (PVC).
[0120] The coated electric wire can be produced, for example, by using an extruder to heat the copolymer and extrude the copolymer in a molten state onto a core wire to form a coating layer.
[0121] When forming the coating layer, the copolymer is heated and in the molten state, a gas is introduced into the copolymer to form the coating layer containing bubbles. As the gas, for example, chlorodifluoromethane, nitrogen, carbon dioxide, or a mixture of the above gases can be used. The gas may be introduced into the heated copolymer as a pressurized gas, or may be generated by mixing a chemical foaming agent into the copolymer. The gas dissolves in the molten copolymer.
[0122] Since a molded article containing the copolymer of the present disclosure has excellent heat resistance, it can be suitably used as a film containing the copolymer.
[0123] Tetrafluoroethylene and fluoro(alkyl vinyl ether) copolymers have excellent chemical and heat resistance, and can be melt molded, making them useful as release films and surface materials for rolls used in office automation equipment. In recent years, the manufacturing of thin-film products has required high heat resistance to withstand thermal lamination, and in the office automation equipment field, the trend toward colorization and high speed has led to a demand for even higher heat resistance in the surface materials of rolls in the fixing section, creating a severe situation.
[0124] The copolymer of the present disclosure has a TFE unit and a PPVE unit, and the PPVE unit content and melt flow rate (MFR) of the copolymer are appropriately adjusted, so that the film formed from the copolymer has high heat resistance. In the above-mentioned thermal lamination process, it is required to be able to withstand a wide range of temperature conditions from about 100 to about 300 ° C., but since the copolymer of the present disclosure has the above-mentioned configuration, it can be suitably used even under severe temperature conditions. The film containing the copolymer of the present disclosure does not melt even at an extremely high temperature of 280 ° C., and can withstand softening up to about 100 ° C. due to its high glass transition temperature. Therefore, the film containing the copolymer of the present disclosure is suitable for use as a heat-resistant film used in an environment with a maximum temperature of 280 ° C. or more.
[0125] The release film can be produced by molding the copolymer of the present disclosure by melt extrusion molding, calendar molding, press molding, casting molding, etc. From the viewpoint of obtaining a uniform thin film, the release film can be produced by melt extrusion molding. The copolymer of the present disclosure can be molded into a required shape by extrusion molding, compression molding, press molding, or the like to form a sheet, film, or tube, and used as a surface material for OA equipment rolls, OA equipment belts, etc. In particular, thin-walled tubes and films can be produced by melt extrusion molding.
[0126] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES
[0127] Next, embodiments of the present disclosure will be described with reference to examples, but the present disclosure is not limited to these examples.
[0128] The values in the examples and comparative examples were measured by the following methods.
[0129] (Monomer unit content) The content of each monomer unit was measured by an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker Biospin).
[0130] (Melt Flow Rate (MFR)) According to ASTM D1238, the mass of polymer flowing out per 10 minutes (g / 10 minutes) from a nozzle with an inner diameter of 2.1 mm and a length of 8 mm under a load of 5 kg at 372°C was determined using a Melt Indexer G-01 (manufactured by Toyo Seiki Seisakusho).
[0131] (Number of functional groups) The copolymer pellets were molded by cold pressing to prepare a film with a thickness of 0.25 to 0.30 mm. This film was scanned 40 times using a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] to obtain an infrared absorption spectrum, and a difference spectrum was obtained from the base spectrum, which was completely fluorinated and had no functional groups. From the absorption peaks of specific functional groups that appeared in this difference spectrum, the ratio of carbon atoms in the sample to carbon atoms in the sample was calculated according to the following formula (A): 6 The number of functional groups per unit, N, was calculated. N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm) For reference, the absorption frequencies, molar extinction coefficients, and correction coefficients for the functional groups in this disclosure are shown in Table 2. The molar extinction coefficients were determined from FT-IR measurement data of low molecular weight model compounds.
[0132] [Table 2]
[0133] (Melting Point) Using a differential scanning calorimeter (product name: X-DSC7000, manufactured by Hitachi High-Tech Science Corporation), the sample was heated a first time from 200°C to 350°C at a heating rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and then heated a second time from 200°C to 350°C at a heating rate of 10°C / min. The melting point was determined from the melting curve peak occurring during the second heating process.
[0134] (Glass transition temperature (Tg)) The dynamic viscoelasticity was measured using a dynamic viscoelasticity device DVA-220 (manufactured by IT Measurement & Control Co., Ltd.) at a temperature rise rate of 2° C. / min and a frequency of 10 Hz, and the temperature at the peak of the tan δ value was determined as the glass transition temperature.
[0135] Example 1 53.8L of pure water was put into a 174L autoclave, and after sufficient nitrogen replacement, 41.7kg of perfluorocyclobutane, 0.44kg of perfluoro(propyl vinyl ether) (PPVE), and 0.61kg of methanol were charged, and the temperature in the system was kept at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was pumped in up to 0.5MPa, and then 0.224kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously fed to keep the pressure constant, and 0.022kg of PPVE was added for every 1kg of TFE fed, and polymerization was continued for 7 hours. After releasing TFE and returning the autoclave to atmospheric pressure, the reaction product obtained was washed with water and dried to obtain 30kg of powder.
[0136] The obtained powder was melt-extruded at 360°C using a screw extruder (product name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of a TFE / PPVE copolymer. The PPVE content of the obtained pellets was measured by the method described above. The results are shown in Table 3.
[0137] The obtained pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Okawara Manufacturing Co., Ltd.) and heated to 210°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced up to atmospheric pressure. 0.5 hours after the introduction of F2 gas, evacuation was performed once and F2 gas was introduced again. Another 0.5 hours later, evacuation was performed again and F2 gas was introduced again. Thereafter, the above-mentioned F2 gas introduction and evacuation operation was performed once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the inside of the reactor was sufficiently replaced with N2 gas to complete the fluorination reaction. Various physical properties were measured using the fluorinated pellets by the above-mentioned methods. The results are shown in Table 3.
[0138] Example 2 Fluorinated pellets were obtained in the same manner as in Example 1, except that the amounts of PPVE and methanol were changed to 0.49 kg and 0.96 kg, respectively, and 0.025 kg of PPVE was added for every 1 kg of TFE fed. The results are shown in Table 3.
[0139] Example 3 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 0.42 kg of methanol, 0.027 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 7.5 hours. The results are shown in Table 3.
[0140] Example 4 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 1.04 kg of methanol, 0.027 kg of PPVE was added for every 1 kg of TFE fed, the polymerization time was 7.5 hours, the temperature rise temperature of the vacuum vibrating reactor was 180° C., and the reaction was carried out at a temperature of 180° C. for 10 hours. The results are shown in Table 3.
[0141] Example 5 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 1.29 kg of methanol, 0.027 kg of PPVE was added for every 1 kg of TFE fed, the polymerization time was 7.5 hours, the temperature rise temperature of the vacuum vibrating reactor was 180° C., and the reaction was carried out at a temperature of 180° C. for 10 hours. The results are shown in Table 3.
[0142] Example 6 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.55 kg of PPVE, 0.71 kg of methanol, 0.028 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 7.5 hours. The results are shown in Table 3.
[0143] Example 7 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.55 kg of PPVE, 1.16 kg of methanol, 0.028 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 7.5 hours. The results are shown in Table 3.
[0144] Example 8 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.57 kg of PPVE, 0.77 kg of methanol, 0.029 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 7.5 hours. The results are shown in Table 3.
[0145] Example 9 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 1.55 kg of methanol, 0.112 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, 0.027 kg of PPVE was added for every 1 kg of TFE fed, and the polymerization time was changed to 10 hours. The results are shown in Table 3.
[0146] Example 10 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.51 kg of PPVE, 1.38 kg of methanol, 0.112 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, 0.026 kg of PPVE was added for every 1 kg of TFE fed, and the polymerization time was changed to 10 hours. The results are shown in Table 3.
[0147] Example 11 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.46 kg of PPVE, 1.21 kg of methanol, 0.112 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, 0.024 kg of PPVE was added for every 1 kg of TFE fed, and the polymerization time was changed to 9 hours. The results are shown in Table 3.
[0148] Comparative Example 1 The pure water was changed to 26.6 L, the perfluorocyclobutane to 30.4 kg, the PPVE to 0.77 kg, and the methanol to 3.30 kg, TFE was pressurized to 0.58 MPa, 0.011 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added, and 0.031 kg of PPVE was added for every 1 kg of TFE fed, the polymerization time was changed to 10 hours, and 15 kg of powder was obtained. The same procedure as in Example 1 was followed to obtain fluorinated pellets. The results are shown in Table 3.
[0149] Comparative Example 2 Pellets (non-fluorinated pellets) were obtained in the same manner as in Example 1, except that 0.25 kg of PPVE, 2.49 kg of methanol, 0.149 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, and 0.013 kg of PPVE were added for every 1 kg of TFE supplied. The results are shown in Table 3.
[0150] Comparative Example 3 Pellets (non-fluorinated pellets) were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 0.63 kg of methanol, 0.027 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 7.5 hours. The results are shown in Table 3.
[0151] Comparative Example 4 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.46 kg of PPVE was added, no methanol was added, 0.104 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added, 0.024 kg of PPVE was added for every 1 kg of TFE fed, and the polymerization time was changed to 8 hours. The results are shown in Table 3.
[0152] Comparative Example 5 Fluorinated pellets were obtained in the same manner as in Example 1, except that 0.53 kg of PPVE, 1.83 kg of methanol, 0.224 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, 0.027 kg of PPVE was added for every 1 kg of TFE fed, and the polymerization time was changed to 8 hours. The results are shown in Table 3.
[0153] [Table 3]
[0154] In Table 3, "<6" means that the number of functional groups is less than 6.
[0155] The pellets thus obtained were then evaluated for the following properties, the results of which are shown in Table 4.
[0156] (Water vapor permeability) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared. The test cup (permeation area 12.56 cm2) was 2 The sheet test piece was placed in a container containing 18 g of water, covered with a sheet test piece, and then clamped with a PTFE gasket to seal. The sheet test piece was placed in contact with the water and held at 95°C for 30 days, then removed and left at room temperature for 2 hours before measuring the amount of mass loss. The water vapor permeability (g cm / m 2 In Table 4, the term "crack" means that the test piece had poor crack resistance against compressive stress and a crack occurred in the test piece during the test. Water vapor permeability (g cm / m 2 ) = mass loss (g) × thickness of sheet specimen (cm) / permeation area (m 2 )
[0157] (Electrolyte leakage test) Using an injection molding machine (SE50EV-A manufactured by Sumitomo Heavy Industries, Ltd.), the copolymer was injection molded at a cylinder temperature of 350 to 385°C and a mold temperature of 150 to 200°C to obtain a gasket with an outer diameter of Φ17.7 mm, an inner diameter of Φ14.3 mm, and a thickness of 1.6 mmt.
[0158] As shown in FIG. 1, 2 g of electrolyte 2 was placed in an aluminum alloy cup 1. The electrolyte contained ethylene carbonate (EC) and diethyl carbonate (DEC), and the volume ratio of EC to DEC (EC / DEC) was 30 / 70 (volume%). A gasket 7 was assembled between the cup 1 and the gasket compression jig 3, and the lid 4 was fastened with a bolt 5 to compress the gasket 7. A spacer 6 was placed between the lid 4 and the cup 1, and the compression deformation rate of the gasket 7 was adjusted to 50%. The mass of the test jig 10 thus obtained was measured. The test jig 10 was placed in a thermostatic chamber heated to 60° C., and after leaving it for 1000 hours, it was taken out and left at room temperature for 2 hours, after which the mass was measured. The amount of electrolyte leakage was calculated using the following formula. This operation was repeated five times to calculate the average value of the amount of electrolyte leakage. The average values are shown in Table 4. Electrolyte leakage amount (g / 1000h) = (mass of test jig before heating) - (mass of test jig after heating)
[0159] (Restored amount) About 2 g of the above pellets were placed in a mold (inner diameter 13 mm, height 38 mm) and melted for 30 minutes at 370°C using a hot plate press, then water-cooled while applying a pressure of 0.2 MPa (resin pressure) to produce a molded body with a height of about 8 mm. The molded body was then cut to produce a test piece with an outer diameter of 13 mm and a height of 6 mm.
[0160] The prepared test specimen was compressed to a compression deformation rate of 50% at room temperature (i.e., a test specimen with a height of 6 mm was compressed to a height of 3 mm) using a compression device. The compressed test specimen was fixed to the compression device and placed in an electric furnace and left at 150°C for 18 hours. The compression device was removed from the electric furnace and cooled to room temperature, after which the test specimen was removed. The recovered test specimen was left at room temperature for 30 minutes, after which the height of the recovered test specimen was measured and the recovery amount was calculated using the following formula. Recovery amount (mm) = t2-t1 t1: Spacer height (mm) t2: Height of the test piece removed from the compression device (mm) In the above test, t1 = 3 mm. In Table 4, the entry "crack" means that the test piece had poor crack resistance against compressive stress and a crack occurred in the test piece during the test.
[0161] (Storage modulus (E')) Dynamic viscoelasticity was measured using a DVA-220 (manufactured by IT Measurement & Control Co., Ltd.) A heat press molded sheet measuring 25 mm in length, 5 mm in width, and 0.2 mm in thickness was used as a sample test piece, and measurements were performed in the range of 30°C to 250°C under conditions of a heating rate of 2°C / min and a frequency of 10 Hz, and the storage modulus (MPa) at 150°C was read.
[0162] (Surface pressure at 150℃) From the results of the compression test at 150°C and the results of the storage modulus measurement at 150°C, the 150°C surface pressure was calculated using the following formula. 150℃ surface pressure (MPa) = (t2-t1) / t1×E' t1: Spacer height (mm) t2: Height of the test piece removed from the compression device (mm) E': Storage modulus at 150℃ (MPa)
[0163] (Electrolyte immersion test) About 5 g of the above pellets were placed in a mold (inner diameter 120 mm, height 38 mm) and melted for 20 minutes at 370°C using a hot plate press, then water-cooled while being pressurized at 1 MPa (resin pressure) to produce a molded body with a thickness of about 0.2 mm. Then, a test piece with a size of 15 mm square was produced using the obtained molded body.
[0164] Ten of the obtained test pieces and 2 g of electrolyte (dimethyl carbonate (DMC)) were placed in a 20 mL glass sample bottle, and the lid of the sample bottle was closed. The sample bottle was placed in a thermostatic chamber at 80 ° C. and left for 144 hours, so that the test pieces were immersed in the electrolyte. The sample bottle was then removed from the thermostatic chamber and cooled to room temperature, and the test pieces were removed from the sample bottle. The electrolyte remaining after the test pieces were removed was air-dried in a room controlled at 25 ° C. for 24 hours while still in the sample bottle, and 2 g of ultrapure water was added. The obtained aqueous solution was transferred to a measurement cell of an ion chromatography system, and the amount of fluorine ions in this aqueous solution was measured by an ion chromatography system (Dionex ICS-2100 manufactured by Thermo Fisher Scientific).
[0165] (Mold corrosion test) 20 g of pellets were placed in a glass container (50 ml screw tube), and a metal pillar (5 mm square, 30 mm long) made of HPM38 (Cr plating) or HPM38 (Ni plating) was hung from the glass container so as not to touch the pellets. The glass container was then covered with aluminum foil. The glass container was placed in an oven in this state and heated at 380°C for 3 hours. The heated glass container was then removed from the oven and cooled to room temperature, and the degree of corrosion on the surface of the metal pillar was visually observed. The degree of corrosion was judged according to the following criteria. ○: No corrosion observed △: Slight corrosion observed ×: Corrosion is observed
[0166] (Dielectric tangent) The pellets were melt-molded to produce cylindrical test pieces with a diameter of 2 mm. The test pieces were set in a 6 GHz cavity resonator manufactured by Kanto Electronics Application Development Co., Ltd., and measured with a network analyzer manufactured by Agilent Technologies, Inc. The measurement results were analyzed with the analysis software "CPMA" manufactured by Kanto Electronics Application Development Co., Ltd. on a PC connected to the network analyzer, and the dielectric loss tangent (tan δ) at 20°C and 6 GHz was obtained.
[0167] (Wire coating properties) The pellets obtained in each Example were extrusion-coated on a copper conductor having a conductor diameter of 0.812 mm with a 30 mm diameter electric wire coating molding machine (manufactured by Tanabe Plastic Machinery Co., Ltd.) to the following coating thickness to obtain a coated electric wire. The electric wire coating extrusion molding conditions were as follows. a) Core conductor: soft steel wire conductor diameter 0.812mm (AWG20) b) Coating thickness: 0.9 mm c) Insulated wire diameter: 2.6 mm d) Wire withdrawal speed: 7m / min) e) Extrusion conditions: · Single-screw extruder with cylinder diameter = 30 mm, L / D = 22 Die (inner diameter) / chip (outer diameter) = 26.0mm / 8.0mm Extruder temperature settings: Barrel C-1 (330°C), Barrel C-2 (350°C), Barrel C-3 (370°C), Head H (380°C), Die D-1 (380°C), Die D-2 (380°C). Core wire preheating was set at 80°C.
[0168] The obtained coated electric wire was cut into 20 cm pieces, 10 pieces were bundled together, wrapped in aluminum foil, and left in an oven at 280°C for 24 hours. After the heat treatment, the coated electric wire was removed from the aluminum foil and observed to confirm that the coating layer was maintained without fusing, melting, or bursting. This is indicated by ○ in the table.
[0169] (Film heat resistance) Using the pellets obtained in each Example, a film was produced using a T-die in an extruder (manufactured by Imoto Manufacturing Co., Ltd.) with a diameter of 14 mm. The extrusion molding conditions were as follows. a) Winding speed: 1m / min b) Roll temperature: 120℃ c) Film width: 70mm d) Thickness: 0.10mm e) Extrusion conditions: Single-screw extruder with cylinder diameter of 14 mm and L / D of 20 Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (350°C), Barrel section C-3 (370°C), T-die section (380°C) The obtained film was cut into a length of 10 cm, 10 sheets were stacked, wrapped in aluminum foil, and left in an oven at 280°C for 24 hours. After the heat treatment, the film was removed from the aluminum foil and observed to confirm that the film was not fused. This is indicated by ○ in the table.
[0170] (Wear test) Using pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared, and a test piece of 10 cm x 10 cm was cut out. The prepared test piece was fixed on the test stand of a Taber abrasion tester (No. 101 special type Taber abrasion tester, manufactured by Yasuda Seiki Seisakusho Co., Ltd.), and an abrasion test was performed using the Taber abrasion tester under the conditions of a load of 500 g, an abrasion wheel CS-10 (polished 20 times with abrasive paper #240), and a rotation speed of 60 rpm. The weight of the test piece after 1000 rotations was measured, and the weight of the test piece was measured after another 10,000 rotations of the same test piece. The amount of wear was calculated using the following formula. Wear amount (mg)=M1-M2 M1: Test piece weight after 1000 rotations (mg) M2: Test piece weight after 10,000 rotations (mg)
[0171] (Electrolyte permeability) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared. The test cup (permeation area 12.56 cm2) was 2 10 g of dimethyl carbonate (DMC) was placed in a test piece, which was then covered with a sheet specimen and a PTFE gasket was placed between the test pieces and tightened to seal. The test piece was placed in contact with the DMC and held at 60°C for 30 days, then removed and left at room temperature for 1 hour before measuring the amount of mass loss. The DMC permeability (g cm / m 2 ) was sought. Electrolyte permeability (g cm / m 2 ) = mass loss (g) × thickness of sheet specimen (cm) / permeation area (m 2 ) In Table 4, the entry "crack" means that the test piece had poor crack resistance against compressive stress and a crack occurred in the test piece during the test.
[0172] (Injection moldability) The copolymer was injection molded using an injection molding machine (SE50EV-A, manufactured by Sumitomo Heavy Industries, Ltd.) with a cylinder temperature of 395°C, a mold temperature of 220°C, and an injection speed of 3mm / s. The mold used was a Cr-plated HPM38 mold (100mm x 100mm x 3mmt, film gate, flow length from the gate was 100mm). The obtained injection molded article was observed and evaluated according to the following criteria. The presence or absence of cloudiness was confirmed by visual inspection. The presence or absence of surface roughness was confirmed by touching the surface of the injection molded article. 3: The entire injection molded product is transparent and the entire surface is smooth. 2: White turbidity is observed within 1 cm of the mold gate, and the entire surface is smooth. 1: White turbidity is observed within 1 cm of where the mold gate was located, and surface roughness is confirmed within 1 cm of where the mold gate was located. 0: The copolymer is not filled entirely into the mold, and a molded product with the desired shape cannot be obtained.
[0173] (Bending crack test (thermal deformation resistance)) Using pellets and a heat press molding machine, a sheet of approximately 2 mm thickness was produced. The sheet was punched out using a 13.5 mm x 38 mm rectangular dumbbell to obtain three test pieces. A notch was made in the center of the long side of each of the obtained test pieces with a 19 mm x 0.45 mm blade in accordance with ASTM D1693. The three obtained notched test pieces were attached to a stress crack test jig in accordance with ASTM D1693 and heated in an electric furnace at 80 ° C for 2 hours, after which the notch and its surroundings were visually observed and the number of cracks was counted. A sheet without cracks has excellent heat deformation resistance. ○: The number of cracks is 0 ×: The number of cracks is 1 or more.
[0174] [Table 4] [Explanation of symbols]
[0175] 10 Test fixture 1 cup 2 Electrolyte 3 Gasket compression tool 4 Lid 5 Volts 6 Spacer 7 Gasket
Claims
[Claim 1] A copolymer consisting of only tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of tetrafluoroethylene units is 97.2 to 98.0% by mass, The content of perfluoro(propyl vinyl ether) units is 2.0 to 2.8 mass% based on the total monomer units; The melt flow rate at 372°C is 5.6 to 23 g / 10 min. The total number of functional groups, which is the total number of --CF.dbd.CF.sub.2, --CF.sub.2H, --COF, --COOH, --COOCH.sub.3, --CONH.sub.2 and --CH.sub.2OH, is 10 or more when the number of carbon atoms in the main chain is 10. 6 Each piece is 50 or less Copolymer.
Citation Information
Patent Citations
Non-aqueous electrolytic liquid
JP1997245832A
Lithium secondary battery
JP2001283907A
Sealing material
JP2013177574A