Laser processing device and method for manufacturing chips

The laser processing apparatus and method address the challenge of high pulse energy damage by using controlled aberration correction to form modified regions on sapphire substrates, enabling precise and high-yield chip production with reduced crack propagation and damage.

JP7584429B2Active Publication Date: 2024-11-15NICHIA CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021550394
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-08-07
Publication Date
2024-11-15
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Existing laser processing technologies face challenges in minimizing damage to workpieces due to high pulse energy, particularly when correcting spherical aberration during laser processing.

Method used

A laser processing apparatus and method that focuses laser beams on a sapphire substrate with controlled aberration correction, using a spatial light modulator and focusing optical system to form modified regions along specific cutting lines with adjusted aberration correction amounts, allowing for low pulse energy processing.

Benefits of technology

The method enables precise cutting of sapphire substrates with reduced crack propagation and damage, achieving high-yield chip production by optimizing aberration correction and pulse energy levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584429000001
    Figure 0007584429000001
  • Figure 0007584429000002
    Figure 0007584429000002
  • Figure 0007584429000003
    Figure 0007584429000003
Patent Text Reader

Abstract

This laser processing device for condensing laser light onto a processing target object which includes a sapphire substrate having the C-plane as the main surface, in order to form a modified region along a planned cutting line in the processing target object, is provided with a laser light source, a spatial optical modulator, and a condensing optical system. If a state in which aberration correction has been performed in such a way as to cancel out spherical aberration that occurs at the laser light condensing position is defined as an ideal condensing state, and the amount of aberration correction in the ideal condensing state is defined as an ideal aberration correction amount, then if the modified region is to be formed along a first planned cutting line in the a-axis direction of the sapphire substrate, the spatial optical modulator performs aberration correction using a first aberration correction amount that is smaller than the ideal aberration correction amount, and if the modified region is to be formed along a second planned cutting line in the m-axis direction of the sapphire substrate, the spatial optical modulator performs aberration correction using a second aberration correction amount that is smaller than the ideal aberration correction amount and that is different from the first aberration correction amount.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One aspect of the present invention relates to a laser processing apparatus and a method for manufacturing a chip. [Background technology]

[0002] 2. Description of the Related Art Known laser processing devices include devices that correct spherical aberration that occurs at a focusing position due to focusing of laser light on a workpiece, and focus the laser light on the workpiece (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-107334 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the above-mentioned techniques, when the pulse energy of the laser beam becomes large, damage is likely to occur to the workpiece. Therefore, in recent years, there has been a demand for laser processing with a small pulse energy of the laser beam.

[0005] An object of one aspect of the present invention is to provide a laser processing apparatus and a chip manufacturing method capable of realizing laser processing with small pulse energy of laser light. [Means for solving the problem]

[0006] A laser processing apparatus according to one aspect of the present invention is a laser processing apparatus that forms a modified region in a workpiece along a planned cutting line by focusing laser light on the workpiece, which includes a sapphire substrate having a C-plane as a main surface, and includes a laser light source that emits laser light, a spatial light modulator that modulates the laser light emitted by the laser light source, and a focusing optical system that focuses the laser light modulated by the spatial light modulator on the workpiece, wherein the spatial light modulator defines a state in which aberration correction is performed so as to cancel out spherical aberration occurring at the focusing position of the laser light as an ideal focusing state, and defines the aberration correction amount in the ideal focusing state as the ideal aberration correction amount, when a modified region is formed along a first planned cutting line along the a-axis direction of the sapphire substrate, aberration correction is performed with a first aberration correction amount smaller than the ideal aberration correction amount, and when a modified region is formed along a second planned cutting line along the m-axis direction of the sapphire substrate, aberration correction is performed with a second aberration correction amount smaller than the ideal aberration correction amount and different from the first aberration correction amount.

[0007] When forming a modified region along a first line to cut along the a-axis direction of the sapphire substrate, it is found that performing aberration correction with a first aberration correction amount smaller than the ideal aberration correction amount improves the extensibility of the crack in the thickness direction of the sapphire substrate, and the object to be processed can be cut along the first line to cut even with a small pulse energy, compared to when performing aberration correction with the ideal aberration correction amount. Also, when forming a modified region along a second line to cut along the m-axis direction of the sapphire substrate, performing aberration correction with a second aberration correction amount smaller than the ideal aberration correction amount and different from the first aberration correction amount improves the extensibility of the crack in the thickness direction of the sapphire substrate, and the object to be processed can be cut along the second line to cut even with a small pulse energy, compared to when performing aberration correction with the ideal aberration correction amount. Therefore, according to one aspect of the present invention, it is possible to realize laser processing with a small pulse energy of laser light.

[0008] In the laser processing apparatus according to one aspect of the present invention, the first aberration correction amount may be smaller than the second aberration correction amount, in which case the extendibility of the crack in the thickness direction of the sapphire substrate is further improved, and the object can be cut with even smaller pulse energy.

[0009] In the laser processing device according to one aspect of the present invention, the first line to cut may be perpendicular to an orientation flat of the workpiece when viewed in the thickness direction of the workpiece. This makes it possible to realize laser processing with small pulse energy of laser light based on the orientation flat of the workpiece.

[0010] In the laser processing device according to one aspect of the present invention, the second line to cut may be parallel to an orientation flat of the workpiece when viewed from the thickness direction of the workpiece. This makes it possible to realize laser processing with small pulse energy of the laser light based on the orientation flat of the workpiece.

[0011] In the laser processing apparatus according to one aspect of the present invention, a device layer may be provided on the front side of the workpiece, and the rear side of the workpiece may be the incident surface of the laser light. In this case, since laser processing with small pulse energy of the laser light can be realized as described above, it is possible to suppress damage to the device layer (so-called through light damage) caused by the laser light transmitted through the sapphire substrate from becoming large.

[0012] A chip manufacturing method according to one aspect of the present invention includes the steps of preparing an object to be processed including a sapphire substrate having a C-plane as a main surface, and modulating laser light emitted from a laser light source with a spatial light modulator and focusing the laser light modulated by the spatial light modulator on the sapphire substrate with a focusing optical system, thereby forming a modified region in the sapphire substrate. In modulating the laser light with the spatial light modulator, a state in which aberration correction is performed so as to cancel out spherical aberration occurring at the focusing position of the laser light is defined as an ideal focusing state, and the aberration correction amount in the ideal focusing state is defined as an ideal aberration correction amount. When a modified region is formed along a first planned cutting line along the a-axis direction of the sapphire substrate, aberration correction is performed with a first aberration correction amount smaller than the ideal aberration correction amount, and when a modified region is formed along a second planned cutting line along the m-axis direction of the sapphire substrate, aberration correction is performed with a second aberration correction amount smaller than the ideal aberration correction amount and different from the first aberration correction amount.

[0013] In the chip manufacturing method according to one aspect of the present invention, the first amount of aberration correction may be smaller than the second amount of aberration correction.

[0014] In the chip manufacturing method according to one aspect of the present invention, the first line to cut may be perpendicular to an orientation flat of the object when viewed in a thickness direction of the object.

[0015] In the chip manufacturing method according to one aspect of the present invention, the second line to cut may be parallel to an orientation flat of the object when viewed in a thickness direction of the object.

[0016] In a chip manufacturing method according to one aspect of the present invention, a device layer may be provided on a front surface side of an object to be processed, and a rear surface of the object may be an incident surface of laser light.

[0017] In the chip manufacturing method according to one aspect of the present invention, when forming a modified region along the first line to cut, the pulse energy of the laser light may be in the range of 9.0 μJ to 12.0 μJ, and the first aberration correction amount may be in the range of 25% to 75% of the ideal aberration correction amount. In this case, the chips can be manufactured with a good yield.

[0018] In the chip manufacturing method according to one aspect of the present invention, when forming a modified region along the first line to cut, the pulse energy of the laser light may be in the range of 8.5 μJ to 12.0 μJ, and the first aberration correction amount may be in the range of 50% to 62.5% of the ideal aberration correction amount. In this case, the chips can be manufactured with a good yield.

[0019] In the chip manufacturing method according to one aspect of the present invention, when forming a modified region along the second line to cut, the pulse energy of the laser light may be in the range of 8.0 μJ to 12.0 μJ, and the second aberration correction amount may be in the range of 75% to less than 100% of the ideal aberration correction amount. In this case, the chips can be manufactured with a good yield. Effect of the Invention

[0020] According to one aspect of the present invention, it is possible to provide a laser processing apparatus and a chip manufacturing method capable of realizing laser processing with small pulse energy of laser light. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a configuration diagram of a laser processing apparatus according to an embodiment. [Diagram 2] Fig. 2(a) is a plan view of the object to be processed, and Fig. 2(b) is a side sectional view of a part of the object to be processed. [Diagram 3] FIG. 3 is a graph showing evaluation results of laser processing along the first planned cutting line perpendicular to the orientation flat. [Figure 4]FIG. 4 is a graph showing evaluation results of laser processing along the second planned cutting line parallel to the orientation flat. [Diagram 5] FIG. 5 is a graph showing evaluation results of laser processing along the first planned cutting line perpendicular to the orientation flat. [Figure 6] Fig. 6(a) is a diagram for explaining a focusing state without aberration correction. Fig. 6(b) is a diagram for explaining a focusing state with weak correction because the amount of aberration correction is smaller than the ideal amount of aberration correction. Fig. 6(c) is a diagram for explaining an ideal focusing state. Fig. 6(d) is a diagram for explaining a focusing state with overcorrection because the amount of aberration correction is larger than the ideal amount of aberration correction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the embodiments will be described in detail with reference to the drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. [Laser processing equipment configuration]

[0023] 1, the laser processing apparatus 1 includes a stage 2, a laser light source 3, a spatial light modulator 4, a condensing lens (condensing optical system) 7, and a control unit 6. The laser processing apparatus 1 is an apparatus that forms a modified region 12 in the object 20 along a line to be cut by irradiating the object 20 with laser light L. Hereinafter, the first horizontal direction is referred to as the X direction, and the second horizontal direction perpendicular to the first horizontal direction is referred to as the Y direction. In addition, the vertical direction is referred to as the Z direction.

[0024] The stage 2 supports the workpiece 20, for example, by adsorbing a film attached to the workpiece 20. In this embodiment, the stage 2 is movable along each of the X direction and the Y direction. The stage 2 is also rotatable about an axis along the Z direction. The laser light source 3 emits laser light L that is transparent to the workpiece 20, for example, by a pulse oscillation method. The spatial light modulator 4 modulates the laser light L output by the laser light source 3. The spatial light modulator 4 is, for example, a reflective liquid crystal (LCOS: Liquid Crystal on Silicon) spatial light modulator (SLM: Spatial Light Modulator). The condenser lens 7 condenses the laser light L modulated by the spatial light modulator 4 onto the workpiece 20.

[0025] When the laser light L is focused inside the object 20 supported by the stage 2, the laser light L is particularly absorbed in a portion corresponding to the focusing point C of the laser light L, and a modified region 12 is formed inside the object 20. The modified region 12 is a region whose density, refractive index, mechanical strength, and other physical properties are different from those of the surrounding non-modified region. Examples of the modified region 12 include a melting treatment region, a crack region, a dielectric breakdown region, a refractive index change region, and the like.

[0026] As an example, when the stage 2 is moved along the X direction while irradiating the workpiece 20 with the laser light L and the focal point C is moved along the X direction relative to the workpiece 20, multiple modified spots 13 are formed so as to be lined up in a row along the X direction. One modified spot 13 is formed by irradiating one pulse of laser light L. One row of modified regions 12 is a collection of multiple modified spots 13 lined up in a row. Adjacent modified spots 13 may be connected to each other or separated from each other depending on the relative moving speed of the focal point C with respect to the workpiece 20 and the repetition frequency of the laser light L.

[0027] The control unit 6 controls the stage 2, the laser light source 3, the spatial light modulator 4, and the focusing lens 7. The control unit 6 is configured as a computer device including a processor, a memory, a storage, a communication device, etc. In the control unit 6, software (programs) loaded into the memory, etc. are executed by the processor, and the reading and writing of data in the memory and storage, as well as communication by the communication device, are controlled by the processor. In this way, the control unit 6 realizes various functions.

[0028] As shown in Figures 2(a) and 2(b), the workpiece 20 includes a sapphire substrate 11 having a C-plane as its main surface (front surface 11a and back surface 11b), and a plurality of functional elements 15 formed on the front surface 11a (one of the main surfaces) of the sapphire substrate 11. The workpiece 20 has a disk shape. An orientation flat 25 is formed on the workpiece 20. The orientation flat 25 is a flat surface formed on part of the outer circumferential surface of the workpiece 20. The orientation flat 25 constitutes part of the side surface of the workpiece 20.

[0029] The sapphire substrate 11 is a disk-shaped (plate-shaped) substrate made of sapphire, a hexagonal material. The C-plane is the (0001) plane. The functional elements 15 are light-receiving elements such as photodiodes, light-emitting elements such as laser diodes and light-emitting diodes, or circuit elements formed as circuits. The multiple functional elements 15 are arranged in a matrix on the surface 11a of the sapphire substrate 11. In this manner, the object 20 has a device layer 16 including multiple functional elements 15 provided on the surface 21 side. The shapes of the object 20 and the sapphire substrate 11 are not particularly limited.

[0030] The laser processing method performed by the laser processing device 1 is used as a chip manufacturing method for manufacturing a plurality of chips by cutting the object 20 for each functional element 15. Therefore, in the laser processing device 1, a plurality of lines to cut 5 are set in a lattice pattern on the object 20 so as to pass through the street region 17 between adjacent functional elements 15 (so as to pass through the width of the street region 17 when viewed from the thickness direction (Z direction) of the object 20). When cutting along the a-axis having cleavability, the laser may be irradiated by intentionally shifting (offsetting) the irradiation position of the laser light L in consideration of the amount of oblique cracking (cleavage amount). By offsetting, it is possible to prevent the cracks in the sapphire substrate 11 from protruding from the street region 17 and reaching the inside of the region that becomes the functional element 15. Then, the laser light L incident from the back surface 22 of the object 20, which is also the back surface 11b of the sapphire substrate 11, is condensed, and the modified region 12 is formed in the object 20 along each line to cut 5. The back surface 22 constitutes the incident surface of the laser light L. The cutting line 5 is a virtual line, but may be an actually drawn line. The cutting line 5 may be specified by coordinates.

[0031] The spatial light modulator 4 has a liquid crystal layer (display unit) into which the laser light L is incident. When forming the modified region 12, the spatial light modulator 4 performs aberration correction by displaying a predetermined modulation pattern on the liquid crystal layer and modulating the laser light L. The modulation pattern to be displayed is derived and stored in advance based on at least one of the depth position (position in the Z direction) where the modified region 12 is planned to be formed, the wavelength of the laser light L, the material of the workpiece 20, and the refractive indexes of the condenser lens 7 and the workpiece 20, for example. The operation of the spatial light modulator 4, such as displaying the modulation pattern, is controlled by the control unit 6.

[0032] The modulation pattern includes a spherical aberration correction pattern that reduces spherical aberration. Spherical aberration is a phenomenon in which each light beam constituting the laser light L does not converge to one point but scatters (becomes blurred). Spherical aberration causes the focusing area of ​​the laser light L (the area where each light beam constituting the laser light L is focused) to be elongated in the Z direction. In addition to the spherical aberration correction pattern, the modulation pattern may include at least one of a pattern for branching a processing point and an individual difference correction pattern for correcting individual differences occurring in the laser processing apparatus 1.

[0033] When forming the modified region 12 along the first line to cut 5a among the multiple lines to cut 5, the spatial light modulator 4 performs aberration correction with a first aberration correction amount smaller than the ideal aberration correction amount in an ideal light-concentration state. When forming the modified region 12 along the second line to cut 5b among the multiple lines to cut 5, the spatial light modulator 4 performs aberration correction with a second aberration correction amount smaller than the ideal aberration correction amount in an ideal light-concentration state and different from the first aberration correction amount.

[0034] The ideal focusing state is a state where aberration correction is performed to cancel out spherical aberration occurring at the focusing position of the laser light L, and is a focusing state in which the aberration is reduced to a level close to the focusing state when it is assumed that there is no medium. The ideal aberration correction amount is the aberration correction amount that results in an ideal focusing state in a medium. The focusing position of the laser light L can be specified by technical common sense. For example, the focusing position of the laser light L corresponds to the position of the focusing point C in Figure 1. For example, the focusing position of the laser light L corresponds to a position near the center of the focusing area of ​​the laser light L.

[0035] The first line to cut 5a is a line along the a-axis direction of the sapphire substrate 11. The first line to cut 5a is perpendicular to the orientation flat 25 of the object 20 when viewed from the Z direction. The second line to cut 5b is a line along the m-axis direction of the sapphire substrate 11. The second line to cut 5b is parallel to the orientation flat 25 of the object 20 when viewed from the Z direction. The first aberration correction amount is smaller than the second aberration correction amount. The m-axis is an axis perpendicular to the m-plane. The a-axis is an axis perpendicular to the a-plane.

[0036] FIG. 3 is a graph showing the evaluation results of laser processing along the first line to be cut 5a perpendicular to the orientation flat 25. The processing conditions were as follows: wavelength of the laser light L was 1030 nm, pulse width was 6 ps, pulse energy was 9.5 μJ, defocus was 40 μm, scan speed was 400 mm / s, and repetition frequency was 50 kHz. At this time, the pulse pitch calculated from the scan speed and repetition frequency was 8 μm. The incident surface of the laser light L was the back surface 22. The ideal aberration correction amount at this time was set to H0. The scan speed is the relative speed of the laser light L scanning along the line to be cut 5. Defocus is the distance between the objective lens and the incident surface of the medium to be processed, expressed as a distance of how close the focal point of the processing laser is to the incident surface of the medium to be processed when it is most focused (the same applies below).

[0037] The processing conditions for the first line to cut 5a along the a-axis direction may be a pulse width of 0.1 ps to 10 ps, ​​a pulse energy of 8.5 μJ to 12 μJ, and a defocus amount of 32 μm to 50 μm. The pulse pitch determined by the repetition frequency and the scanning speed may be 5 μm to 10 μm.

[0038] The horizontal axis is the amount of aberration correction. Here, the ideal amount of aberration correction H0 is set to 100%, and the amount of aberration correction when no aberration correction is performed is set to 0% (the same applies below). The expression (unit) of the amount of aberration correction is not particularly limited. If the amount of aberration correction is greater than the ideal amount of aberration correction H0, it is considered to be overcorrected. If the amount of aberration correction is smaller than the ideal amount of aberration correction H0, it is considered to be weakly corrected. The vertical axis includes the axis of the crack extension rate. For example, when laser processing is performed on a predetermined area (e.g., the entire area) of the processing object 20 as viewed from the Z direction, the "crack extension rate" is "area where it can be evaluated that the crack from the modified area 12 has sufficiently extended" / "predetermined area where laser processing has been performed" (see below). Evaluation of whether the crack from the modified area 12 has sufficiently extended can be performed by various evaluation methods. For example, when a crack propagating from the modified region 12 reaches both the front surface 11a and the back surface 11b of the sapphire substrate 11, it can be evaluated that the crack from the modified region 12 has propagated sufficiently. The closer the crack extension rate is to 100%, the better the crack has propagated in the Z direction from the modified region 12. The closer the crack extension rate is to 0%, the worse the crack has propagated in the Z direction from the modified region 12. The crack extension rate can also be confirmed visually. The broken line in the graph represents the crack extension rate. The vertical axis also includes the amount of cleavage. The amount of cleavage is the length along the m-axis direction of a crack that propagates from the modified region 12 formed by laser processing along the a-axis direction. Crack extension rate = Area in which a crack can be evaluated as having sufficiently extended from the modified area 12 as viewed in the Z direction / A predetermined area in which the workpiece 20 has been subjected to laser processing as viewed in the Z direction

[0039] FIG. 6(a) is a diagram for explaining a focusing state without aberration correction. FIG. 6(b) is a diagram for explaining a focusing state with weak correction because the amount of aberration correction is smaller than the ideal amount of aberration correction. FIG. 6(c) is a diagram for explaining an ideal focusing state. FIG. 6(d) is a diagram for explaining a focusing state with overcorrection because the amount of aberration correction is larger than the ideal amount of aberration correction. FIGS. 6(a) to 6(d) correspond to side cross-sectional views of a processing object 20 made of sapphire when the processing object 20 is irradiated with laser light L from air.

[0040] As shown in FIG. 6(a), in a focusing state without aberration correction, for example, the distance Z2 from the surface of the workpiece 20 to the focusing point of the outer ray of the laser light L is greater than the distance Z1 from the surface of the workpiece 20 to the focusing point of the inner ray of the laser light L. In this case, a difference ΔZ occurs between the distances Z1 and Z2. As shown in FIG. 6(b), in a focusing state with weak correction, for example, the distance Z2 is still greater than the distance Z1, and a difference ΔZ occurs between the distances Z1 and Z2. As shown in FIG. 6(c), in an ideal focusing state, for example, the distances Z1 and Z2 are equal, and no difference ΔZ occurs between the distances Z1 and Z2. As shown in FIG. 6(d), in a focusing state with overcorrection, for example, the distance Z2 is smaller than the distance Z1, and a difference ΔZ occurs between the distances Z1 and Z2.

[0041] As shown in FIG. 3, when the modified region 12 is formed along the first line to cut 5a, the following findings are found. That is, by making the amount of aberration correction smaller than the ideal amount of aberration correction (on the weak correction side), the crack extension rate can be increased. When the amount of aberration correction is in the range F1 of 37.5% or more and less than 75%, the crack extension rate tends to improve. In the range F1, the amount of cleavage was in the range of about 20 to about 30 μm. The range F1 is wider than the range F2 in FIG. 4. The range F1 is on the weak correction side compared to the range F2 in FIG. 4. When the amount of aberration correction is larger than the ideal amount of aberration correction (overcorrection), the crack extension rate deteriorates extremely. When the amount of aberration correction is larger than the ideal amount of aberration correction, the meandering of the crack and the amount of cleavage increase.

[0042] The range of pulse energy in laser processing of the first line to cut 5a along the a-axis direction may be set to a range in which the crack extension rate is 50% or more in order to improve the yield when cutting the workpiece 20 into chips. If the pulse energy is set too high, the functional element 15 may be damaged, leading to deterioration of the characteristics. In addition, if the pulse energy is set too high, the modified regions 12 may become large, and the modified regions 12 may affect each other, which may actually worsen the crack extension. Therefore, in processing the first line to cut 5a along the a-axis direction, the pulse energy may be set to the above-mentioned range of 8.5 μJ to 12.0 μJ. By setting the pulse energy to the above-mentioned range of 8.5 μJ to 12.0 μJ, it is possible to achieve good crack extension with a crack extension rate of 50% or more, and to suppress damage to the functional element 15.

[0043] FIG. 4 is a graph showing the evaluation results of laser processing along the second planned cutting line 5b parallel to the orientation flat 25. The processing conditions were as follows: the wavelength of the laser light L was 1030 nm, the pulse width was 6 ps, the pulse energy was 8.0 μJ, the scan speed was 400 m / s, and the defocus was 40 μm. The incident surface of the laser light L was the back surface 22. The ideal aberration correction amount at this time was H0. The horizontal axis is the aberration correction amount. The vertical axis includes an axis of the crack extension rate and an axis of the oblique cleavage amount. The broken line in the graph is the crack extension rate. The oblique cleavage amount is the length along the a-axis direction of the crack that extends from the modified region 12 formed by the laser processing along the m-axis direction. The oblique cleavage amount is likely to be a smaller value than the cleavage amount due to the characteristics of the sapphire substrate 11. Therefore, the crack along the m-axis direction is more likely to extend than the crack along the a-axis direction. The pulse energy of the laser processing along the m-axis direction may be set in a range in which the oblique cleavage amount is within 3.0 μm in order to make it easier to place the cutting position within the street region 17.

[0044] The processing conditions for the second line to cut 5b along the m-axis direction may be a pulse width of 0.1 ps to 10 ps, ​​a pulse energy of 8.0 μJ to 12 μJ, and a defocus amount of 30 μm to 50 μm. The pulse pitch determined by the repetition frequency and the scanning speed may be 5 μm to 10 μm.

[0045] The range of pulse energy in processing the second line to cut 5b along the m-axis direction may be set to a range in which the crack extension rate is 50% or more in order to improve the yield when cutting the workpiece 20 into chips. If the pulse energy is set too high, the functional element 15 may be damaged, leading to deterioration of the characteristics. If the pulse energy is set too high, the modified regions 12 may become large, and the modified regions 12 may affect each other, which may actually worsen the crack extension property. Therefore, in processing the second line to cut 5b along the m-axis direction, the pulse energy may be set in the above-mentioned range of 8.0 μJ to 12.0 μJ. By setting the pulse energy in the above-mentioned range of 8.0 μJ to 12.0 μJ, the crack can be extended well with a crack extension rate of 50% or more, and damage to the functional element 15 can be suppressed. Here, the crack in the m-axis direction is more likely to extend with a lower pulse energy than the crack in the a-axis direction. Therefore, the pulse energy in processing the second lines to cut 5b along the m-axis direction can be set to a range of 8.0 μJ to 12.0 μJ, which is wider than the range of pulse energy in laser processing along the a-axis direction (8.5 μJ to 12.0 μJ). Furthermore, when the pulse energy in processing the second lines to cut 5b along the m-axis direction is in the range of 8.0 μJ to 12.0 μJ, the oblique cleavage amount is within a range of 3.0 μm, so that the cutting position is likely to fall within the street region 17.

[0046] As shown in FIG. 4, when the modified region 12 is formed along the second line to cut 5b, the following findings are found. That is, by making the amount of aberration correction smaller than the ideal amount of aberration correction (on the weaker correction side), the crack extension rate can be increased. When the amount of aberration correction is in the range F2 of 75% or more and less than 100, the crack extension rate tends to improve. When the amount of aberration correction is 87.5%, the crack extension rate tends to have a maximum point. There is no problem with the amount of oblique cleavage even if the amount of aberration correction is smaller than the ideal amount of aberration correction.

[0047] 5 is a graph showing the evaluation results of laser processing along the first planned cutting line 5a perpendicular to the orientation flat 25. The processing conditions of the evaluation results of FIG. 5 are 9.0 μJ, 8.5 μJ, and 8.0 μJ, which are lower than the processing conditions of the evaluation results of FIG. 3, in which the pulse energy of the laser light L is reduced. The broken lines in the graph indicate the crack extension rate. O1 in the graph is the result of the crack extension rate when the pulse energy is 9.0 μJ, O2 in the graph is the result of the crack extension rate when the pulse energy is 8.5 μJ, and O3 in the graph is the result of the crack extension rate when the pulse energy is 8.0 μJ.

[0048] As shown in Fig. 5, when the modified region 12 is formed along the first line to cut 5a, the following findings are further found. That is, when the pulse energy of the laser light L is reduced, the maximum point of the crack extension rate becomes prominent. When the pulse energy of the laser light L is reduced, the crack extension rate has a maximum point in a range F3 where the aberration correction amount is 50% or more and less than 62.5%. The range F3 is a range on the weaker correction side than the range F2 in Fig. 4. The range F3 is narrower than the range F1 in Fig. 3.

[0049] The chip manufacturing method of this embodiment is a method for obtaining a chip by cutting the workpiece 20, and is performed using the above-mentioned laser processing apparatus 1. That is, the chip manufacturing method of this embodiment includes a step of preparing the workpiece 20, and a step of modulating the laser light L emitted from the laser light source 3 by the spatial light modulator 4, and concentrating the laser light L modulated by the spatial light modulator 4 on the sapphire substrate 11 by the condenser lens 7, thereby forming a modified region 12 on the sapphire substrate 11. In the modulation of the laser light L by the spatial light modulator 4, when the modified region 12 is formed along the first line to be cut 5a, aberration correction is performed with a first aberration correction amount smaller than the ideal aberration correction amount, while when the modified region 12 is formed along the second line to be cut 5b, aberration correction is performed with a second aberration correction amount smaller than the ideal aberration correction amount and different from the first aberration correction amount.

[0050] Here, based on the knowledge that the maximum point of the crack extension rate becomes prominent when the pulse energy of the laser light L is reduced, it is considered that the range of the first aberration correction amount in which the crack extension rate has a maximum value will be increased when the pulse energy of the laser light L is increased. Therefore, it is considered that the range of the first aberration correction amount in which the crack extension rate shows 50% or more will also be increased when the pulse energy of the laser light L is increased. In other words, the result shown in FIG. 5 that the range of the first aberration correction amount in which the crack extension rate shows 50% or more is at least 25% to 75% of the ideal aberration correction amount when the pulse energy of the laser light L is 9.0 μJ is considered to be applicable even when the pulse energy of the laser light L is 9.0 μJ or more. However, as described above, if the pulse energy is too high, it may have a negative effect on the crack extension property, so the upper limit of the pulse energy of the laser light L may be 12.0 μJ. In other words, when forming the modified region 12 along the first cutting line 5a along the a-axis direction, the pulse energy of the laser light L is in the range of 9.0 μJ or more and 12.0 μJ or less, and the first aberration correction amount is in the range of 25% or more and 75% or less of the ideal aberration correction amount, thereby achieving good crack extension with a crack extension rate of 50% or more.

[0051] 5, the result that the range of the first aberration correction amount showing the crack extension rate of 50% or more is 50% or more and 62.5% or less when the pulse energy of the laser light L is 8.5 μJ is considered to be applicable even when the pulse energy of the laser light L is 8.5 μJ or more. However, as described above, the upper limit of the pulse energy of the laser light L may be 12.0 μJ. In other words, when forming the modified region 12 along the first line to cut 5a along the a-axis direction, the pulse energy of the laser light L is in the range of 8.5 μJ or more and 12.0 μJ or less, and the first aberration correction amount is in the range of 50% or more and 62.5% or less of the ideal aberration correction amount, it is possible to achieve good crack extension with a crack extension rate of 50% or more.

[0052] 4, the result that the range of the second aberration correction amount showing a crack extension rate of 50% or more is 75% or more and 100% or less when the pulse energy of the laser light L is 8.0 μJ is considered to be applicable even when the pulse energy of the laser light L is 8.0 μJ or more. However, as described above, the upper limit of the pulse energy of the laser light L may be 12.0 μJ. In other words, when forming the modified region 12 along the second line to cut 5b along the m-axis direction, the pulse energy of the laser light L is in the range of 8.0 μJ or more and 12.0 μJ or less, and the second aberration correction amount is in the range of 75% or more and 100% or less of the ideal aberration correction amount, a good crack extension with a crack extension rate of 50% or more can be achieved.

[0053] As described above, in laser processing, as shown in FIG. 3, FIG. 4, and FIG. 5, when the modified region 12 is formed along the first line to cut 5a along the a-axis direction of the sapphire substrate 11, by performing aberration correction with a first aberration correction amount smaller than the ideal aberration correction amount, the extensibility of the crack in the Z direction is improved compared to the case where aberration correction is performed with the ideal aberration correction amount. In this case, it is found that the object 20 can be cut along the first line to cut even with small pulse energy. In addition, when the modified region 12 is formed along the second line to cut 5b along the m-axis direction of the sapphire substrate 11, by performing aberration correction with a second aberration correction amount smaller than the ideal aberration correction amount and different from the first aberration correction amount, the extensibility of the crack in the Z direction is improved compared to the case where aberration correction is performed with the ideal aberration correction amount. In this case, it is found that the object 20 can be cut along the second line to cut even with small pulse energy.

[0054] In this regard, in the laser processing device 1 and the chip manufacturing method, when the modified region 12 is formed along the first line to cut 5a, aberration correction is performed with the first aberration correction amount, and when the modified region 12 is formed along the second line to cut 5b, aberration correction is performed with the second aberration correction amount. Therefore, it is possible to improve the extensibility of the crack and realize laser processing with small pulse energy of the laser light L. As a result, damage to the object 20 can be suppressed. Even if the object 20 is thick, it is possible to precisely cut the object 20 while suppressing damage by suppressing an increase in pulse energy.

[0055] In the laser processing apparatus 1 and the chip manufacturing method, the first aberration correction amount is smaller than the second aberration correction amount. In this case, as found above, the crack extension is further improved, and the object 20 can be cut with even smaller pulse energy. When multiple rows of modified regions 12 are formed in the thickness direction of the sapphire substrate 11 along the first lines to cut 5a along the a-axis direction of the sapphire substrate 11 and the second lines to cut 5b along the m-axis direction of the sapphire substrate 11, all the first aberration correction amounts in the thickness direction of the sapphire substrate 11 may be smaller than all the second aberration correction amounts in the thickness direction of the sapphire substrate 11. In other words, all the first aberration correction amounts when multiple rows of modified regions 12 are formed along the first lines to cut 5a may be smaller than all the second aberration correction amounts when multiple rows of modified regions 12 are formed along the second lines to cut 5b.

[0056] In the laser processing apparatus 1 and the chip manufacturing method, the first line to cut 5a is perpendicular to the orientation flat 25 when viewed from the Z direction. This makes it possible to realize laser processing with small pulse energy based on the orientation flat 25.

[0057] In the laser processing apparatus 1 and the chip manufacturing method, the second line to cut 5b is parallel to the orientation flat 25 when viewed from the Z direction. This makes it possible to realize laser processing with small pulse energy based on the orientation flat 25.

[0058] In the laser processing apparatus 1 and the chip manufacturing method, a device layer 16 is provided on a front surface 21 side of an object 20 to be processed, and a back surface 22 of the object is an incident surface of the laser light L. In this case, since laser processing with small pulse energy of the laser light L can be realized as described above, it is possible to suppress damage to the device layer 16 caused by the laser light L transmitted through the sapphire substrate 11 (so-called through light damage) from becoming large.

[0059] In the chip manufacturing method, when the modified region 12 is formed along the first line to cut 5a, the pulse energy of the laser light L is in the range of 9.0 μJ to 12.0 μJ, and the first aberration correction amount is in the range of 25% to 75% of the ideal aberration correction amount. In this case, the crack extension rate is in the range of 50% or more, and the chip can be manufactured (cutting of the workpiece 20) with a good yield.

[0060] In the chip manufacturing method, when the modified region 12 is formed along the first line to cut 5a, the pulse energy of the laser light L may be in the range of 8.5 μJ to 12.0 μJ, and the first aberration correction amount may be in the range of 50% to 62.5% of the ideal aberration correction amount. In this case, the crack extension rate is in the range of 50% or more, and the chip can be manufactured with a good yield.

[0061] In the chip manufacturing method, when the modified region 12 is formed along the second line to cut 5b, the pulse energy of the laser light L may be in the range of 8.0 μJ to 12.0 μJ, and the second aberration correction amount may be in the range of 75% to less than 100% of the ideal aberration correction amount. In this case, the crack extension rate is set to a range of 50% or more, and the chip can be manufactured with a good yield. Also, the oblique cleavage amount can be set to a range of 3 μm or less.

[0062] Although the embodiments have been described above, one aspect of the present invention is not limited to the above-described embodiments.

[0063] In one embodiment of the present invention, the stage 2 is moved to move the laser light L relatively to the workpiece 20, but instead of or in addition to this, the condenser lens 7 may be moved to move the laser light L relatively to the workpiece 20. In one embodiment of the present invention, the rear surface 22 of the workpiece 20 is the incident surface of the laser light L, but the front surface 21 of the workpiece 20 may be the incident surface of the laser light L. In one embodiment of the present invention, the terms "along the a-axis direction and the m-axis direction", "parallel" and "perpendicular" may include an error, and may be substantially along the a-axis direction and the m-axis direction, may be substantially parallel, or may be substantially perpendicular.

[0064] One aspect of the present invention can be understood as a laser processing apparatus, a laser processing method, a semiconductor component manufacturing apparatus, or a semiconductor component manufacturing method. The configurations in the above-mentioned embodiments and modifications are not limited to the materials and shapes described above, and various materials and shapes can be applied. In addition, each configuration in the above-mentioned embodiments or modifications can be arbitrarily applied to each configuration in other embodiments or modifications. [Explanation of symbols]

[0065] 1...laser processing apparatus, 3...laser light source, 4...spatial light modulator, 5...planned cutting line, 5a...first planned cutting line, 5b...second planned cutting line, 7...collecting lens (collecting optical system), 11...sapphire substrate, 11a...front surface (main surface), 11b...back surface (main surface), 12...modified region, 16...device layer, 20...object to be processed, 22...back surface, 25...orientation flat, L...laser light.

Claims

1. A laser processing apparatus for forming a modified region in an object to be processed along a line to be cut by focusing laser light on the object to be processed, the modified region being included in the object, the modified region being included in the object to be processed along a line to be cut, a laser light source that emits the laser light; a spatial light modulator that modulates the laser light emitted by the laser light source; a focusing optical system that focuses the laser light modulated by the spatial light modulator on the object to be processed, The spatial light modulator comprises: When a state in which the aberration correction is performed so as to cancel out the spherical aberration occurring at the focusing position of the laser light is defined as an ideal focusing state, and an amount of aberration correction in the ideal focusing state is defined as an ideal aberration correction amount, When the modified region is formed along a first cutting line along an a-axis direction of the sapphire substrate, aberration correction is performed with a first aberration correction amount smaller than the ideal aberration correction amount; A laser processing apparatus that performs aberration correction with a second aberration correction amount that is smaller than the ideal aberration correction amount and different from the first aberration correction amount when forming the modified region along a second planned cutting line along the m-axis direction of the sapphire substrate.

2. The laser processing apparatus according to claim 1 , wherein the first aberration correction amount is smaller than the second aberration correction amount.

3. The laser processing apparatus according to claim 1 , wherein the first line to cut is perpendicular to an orientation flat of the object when viewed in a thickness direction of the object.

4. 4. The laser processing apparatus according to claim 1, wherein the second line to cut is parallel to an orientation flat of the object when viewed in a thickness direction of the object.

5. a device layer is provided on a front surface side of the object, 5. The laser processing apparatus according to claim 1, wherein a rear surface of the object is an incident surface of the laser light.

6. preparing an object to be processed including a sapphire substrate having a C-plane as a main surface; modulating a laser beam emitted from a laser source by a spatial light modulator, and focusing the laser beam modulated by the spatial light modulator on the sapphire substrate by a focusing optical system to form a modified region on the sapphire substrate; In the modulation of the laser light by the spatial light modulator, When a state in which the aberration correction is performed so as to cancel out the spherical aberration occurring at the focusing position of the laser light is defined as an ideal focusing state, and an amount of aberration correction in the ideal focusing state is defined as an ideal aberration correction amount, When the modified region is formed along a first cutting line along an a-axis direction of the sapphire substrate, aberration correction is performed with a first aberration correction amount smaller than the ideal aberration correction amount; A chip manufacturing method, in which when the modified region is formed along a second planned cutting line along the m-axis direction of the sapphire substrate, aberration correction is performed with a second aberration correction amount that is smaller than the ideal aberration correction amount and different from the first aberration correction amount.

7. The method for manufacturing a chip according to claim 6 , wherein the first amount of aberration correction is smaller than the second amount of aberration correction.

8. The method for manufacturing a chip according to claim 6 or 7, wherein the first line to cut is perpendicular to an orientation flat of the object when viewed in a thickness direction of the object.

9. 9. The method for manufacturing a chip according to claim 6, wherein the second line to cut is parallel to an orientation flat of the object when viewed in a thickness direction of the object.

10. a device layer is provided on a front surface side of the object, The method for manufacturing a chip according to any one of claims 6 to 9, wherein a rear surface of the object is an incident surface of the laser light.

11. A method for manufacturing a chip described in any one of claims 6 to 10, wherein when forming the modified region along the first planned cutting line, the pulse energy of the laser light is in the range of 9.0 μJ or more and 12.0 μJ or less, and the first aberration correction amount is in the range of 25% or more and 75% or less of the ideal aberration correction amount.

12. A method for manufacturing a chip described in any one of claims 6 to 10, wherein when forming the modified region along the first planned cutting line, the pulse energy of the laser light is in the range of 8.5 μJ or more and 12.0 μJ or less, and the first aberration correction amount is in the range of 50% or more and 62.5% or less of the ideal aberration correction amount.

13. A method for manufacturing a chip described in any one of claims 6 to 12, wherein when forming the modified region along the second planned cutting line, the pulse energy of the laser light is in the range of 8.0 μJ or more and 12.0 μJ or less, and the second aberration correction amount is in the range of 75% or more and less than 100% of the ideal aberration correction amount.

Citation Information

Patent Citations

  • Laser processing device and laser processing method

    JP2016107334A

  • Modified layer forming method and modified layer forming device for brittle material substrate

    JP2018052814A

  • Method for manufacturing light-emitting element

    JP2018120986A

  • Manufacturing method of light emitting element