Lithium sulfide powder and its manufacturing method
Patent Information
- Application Number
- JP2023094626
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-11-17
- Filing Date
- 2023-06-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2038-11-16
AI Technical Summary
【0009】 本発明によれば、溶媒を含まず、高純度かつ高比表面積であり、優れた反応性と取扱容易性とを兼ね備える硫化リチウム粉体、及び該硫化リチウム粉体を効率的に製造し得る製造方法を提供することができる。
Smart Images

Figure 0007584572000001
Abstract
Description
[Technical field]
[0001] The present invention relates to lithium sulfide powder and a method for producing the same. [Background technology]
[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. Among these batteries, lithium batteries have attracted attention because of their high energy density. Currently available lithium batteries use electrolytes containing flammable organic solvents, and therefore require the installation of safety devices to suppress temperature rise during short circuits, and improvements in structure and materials to prevent short circuits. In contrast, lithium batteries that use a solid electrolyte layer to replace the electrolyte and make the battery all-solid, do not use flammable organic solvents in the battery, and therefore are thought to be superior in terms of manufacturing cost and productivity, with simplified safety devices. Furthermore, sulfide solid electrolytes are known as solid electrolytes used in such solid electrolyte layers.
[0003] Lithium sulfide is used as a raw material for the sulfide solid electrolyte. Known methods for producing this lithium sulfide include, for example, a method using lithium hydroxide, which uses a solvent or an aqueous solution (e.g., Patent Documents 1 and 2), and a method in which lithium hydroxide is reacted with hydrogen sulfide without using a solvent (e.g., Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2005 / 040039 Brochure [Patent Document 2] JP 2011-084438 A [Patent Document 3] Japanese Patent Application Publication No. 9-278423 Summary of the Invention [Problem to be solved by the invention]
[0005] When lithium sulfide is used as a raw material for a solid electrolyte, lithium sulfide is generally required to have high purity and a large specific surface area in order to efficiently obtain a solid electrolyte with better battery performance, and the required performance has become increasingly higher in recent years. In addition, if lithium sulfide contains a solvent, the battery performance may be reduced when a sulfide solid electrolyte is obtained from the lithium sulfide as a raw material, so the lithium sulfide is also required to be solvent-free. However, the methods described in Patent Documents 1 and 2 use a solvent or aqueous solution, which may result in a decrease in purity, or in the inability to completely remove the solvent or in the need for large-scale equipment to remove the solvent, and may not be able to satisfy the increasingly high performance requirements of recent years. The method described in Patent Document 3 does not use a solvent, so it can meet the requirements for high purity and can obtain a solvent-free product, but it may not be able to meet the requirements for a high specific surface area.
[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a lithium sulfide powder that does not contain a solvent, has high purity and a large specific surface area, and combines excellent reactivity and ease of handling, and a production method that can efficiently produce the lithium sulfide powder. [Means for solving the problem]
[0007] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by the invention having the following configuration.
[0008] 1. Solvent-free, specific surface area of 10m 2 / g or more and an average particle size of 0.1 mm or more and 1.5 mm or less. 2. The lithium sulfide powder according to 1 above, wherein the lithium hydroxide content is 0.3 mass % or less. 3. The lithium sulfide powder according to 1 or 2 above, having a lithium sulfide content of 98.0% by mass or more. 4. A method for producing a modified lithium sulfide powder, comprising contacting lithium sulfide powder with hydrogen sulfide in the absence of a solvent, and subjecting the product obtained by said contact to a dehydrosulfiding treatment. 5. A method for producing a modified lithium sulfide powder according to 4 above, comprising reacting lithium hydroxide with a substance containing at least elemental sulfur in the presence or absence of a solvent to obtain lithium sulfide powder, and using the lithium sulfide powder for contact with the hydrogen sulfide. 6. The method for producing a modified lithium sulfide powder according to 4 or 5 above, wherein the contact is carried out at least once under a temperature condition of 20°C or higher and 120°C or lower. 7. The method for producing a modified lithium sulfide powder according to any one of 4 to 6 above, wherein the contact is carried out two or more times under different temperature conditions. 8. The method for producing a modified lithium sulfide powder according to the above 7, wherein the contact is carried out at 140° C. or higher and then at 20° C. or higher and 120° C. or lower. 9. The method for producing a modified lithium sulfide powder according to any one of the above 4 to 8, wherein the dehydrosulfurization treatment of the product is carried out at 130° C. or higher in the presence of an inert gas. Effect of the Invention
[0009] According to the present invention, it is possible to provide lithium sulfide powder that does not contain a solvent, has high purity and a large specific surface area, and combines excellent reactivity and ease of handling, and a production method that can efficiently produce the lithium sulfide powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention (hereinafter, sometimes referred to as "the present embodiment") will be described. In this specification, the upper and lower limit values of "more than", "less than", and "to" in the description of a numerical range are values that can be arbitrarily combined, and the numerical values in the examples can be the upper and lower limits.
[0011] [Lithium sulfide powder] The lithium sulfide powder of this embodiment does not contain a solvent and has a specific surface area of 10 m 2 / g or more and an average particle size of 0.1 mm or more and 1.5 mm or less. Hereinafter, each property of the lithium sulfide powder of the present embodiment will be described.
[0012] (solvent free) The lithium sulfide powder of the present embodiment does not contain a solvent. Conventionally, various solvents have been used in the production of lithium sulfide, and even if a removal process such as drying or distillation is performed, the solvent may remain. When an attempt is made to obtain a sulfide solid electrolyte using this as a raw material, the battery performance of the sulfide solid electrolyte may be reduced due to the remaining solvent. The lithium sulfide powder of the present embodiment is obtained by dissolving in a solvent that can be used in the production of lithium sulfide, which is caused by such a production process, for example, a saturated hydrocarbon solvent such as hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane, tridecane, cyclohexane, etc.; an unsaturated hydrocarbon solvent such as hexene, cyclohexene, etc.; an aromatic hydrocarbon solvent such as benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, etc.; a ketone solvent such as acetone, methyl ethyl ketone, etc.; diethyl ether, dibutyl ether, dimethyl ether, methyl ethyl ether, dipropyl ether, dibutyl ether, cyclopentane, etc. The solvent does not include ether solvents such as ethyl methyl ether, anisole, tetrahydrofuran, methyl cellosolve, ethyl cellosolve, butyl cellosolve, diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether; alcohol solvents such as ethanol, butanol, hexanol, methylhexanol, and ethylhexanol; ester solvents such as ethyl acetate; halogenated hydrocarbon solvents such as dichloromethane and chlorobenzene; amide solvents such as dimethylformamide, dimethylacetamide, and methylpyrrolidone; and nitrile solvents such as acetonitrile, methoxyacetonitrile, propionitrile, methoxypropionitrile, isobutyronitrile, and benzonitrile. In this specification, "containing no solvent" means that the solvent is substantially not contained, and includes an embodiment in which the content of the solvent in lithium sulfide is 0% by mass, and an embodiment in which the solvent is contained within a range of 0.1% by mass or less, which is the measurement limit. The content of the solvent can be measured by dissolving lithium sulfide in methanol and quantifying the amount of the solvent by gas chromatography.
[0013] (specific surface area) The specific surface area of the lithium sulfide powder of this embodiment is 10 m 2 / g or more. Since the lithium sulfide powder of the present embodiment has such a high specific surface area, when used as a raw material for a solid electrolyte, it has excellent reactivity, and therefore a solid electrolyte can be efficiently obtained. From the same viewpoint, the specific surface area of the lithium sulfide powder is preferably 12 m 2 / g or more, more preferably 15m 2 / g or more, more preferably 20m 2 / g or more. There is no particular upper limit, but it is usually set at 50m 2 / g or less. In this specification, the specific surface area is a value measured by the BET method (gas adsorption method), and the gas may be nitrogen (nitrogen method) or krypton (krypton method), and is appropriately selected according to the size of the specific surface area. The specific surface area can be measured using a commercially available device such as a gas adsorption amount measuring device (e.g., AUTOSORB6 (manufactured by Sysmex Corporation)).
[0014] (Average particle size) The average particle size of the lithium sulfide powder of this embodiment is 0.1 mm or more and 1.5 mm or less. When used as a raw material for producing a solid electrolyte, the smaller the average particle size of the lithium sulfide powder, the better because the reactivity is improved, but on the other hand, the smaller the average particle size, the more likely it is to cause aggregation, adhesion, scattering, etc. due to static electricity, intermolecular forces, etc. during handling, making it difficult to handle. By having the average particle size of the lithium sulfide powder of this embodiment within the above range, it is possible to achieve both excellent reactivity and ease of handling. From the same viewpoint, the average particle size of the lithium sulfide powder is preferably 0.15 mm or more, more preferably 0.25 mm or more, and the upper limit is preferably 1.3 mm or less, more preferably 1.0 mm or less. In this specification, the average particle size refers to the particle size D50 when the cumulative volume percentage is 50% in the particle size distribution measured by the laser diffraction method. Specifically, it can be measured using a commercially available device such as a laser diffraction type particle size distribution measuring device (e.g., "SALD-1000 (trade name)" (manufactured by Shimadzu Corporation), "Mastersizer 2000 (trade name)" (manufactured by Malvern Instruments Ltd), "LA-950 (trade name)" (manufactured by Horiba, Ltd.), etc.).
[0015] (Other properties) The pore volume of the lithium sulfide powder of this embodiment is not particularly limited, but considering the case where it is used as a raw material for a solid electrolyte, it is preferably 0.005 ml / g or more, more preferably 0.01 ml / g or more, and the upper limit is usually 1.0 ml / g or less. The pore volume can be measured using the same device as that used to measure the specific surface area, and may be a value obtained by interpolating the measurement points where the relative pressure P / P0 is 0.99 or more to 0.99. The lower measurement limit of the device is 0.001 ml / g.
[0016] The lithium sulfide powder of this embodiment may contain lithium hydroxide. Lithium hydroxide is mainly derived from the raw material, and the content is preferably small, specifically, preferably 0.3 mass% or less, more preferably less than 0.3 mass%, further preferably 0.2 mass% or less, and particularly preferably 0.1 mass% or less (measurement limit or less). There is no particular limit to the lower limit, and it is, for example, about 0.01 mass% or more. If the content of lithium hydroxide in the lithium sulfide powder is within the above range, when it is used as a raw material for a solid electrolyte, the ion conductivity of the obtained solid electrolyte is higher, and a solid electrolyte with better battery performance is obtained. In this specification, the content of lithium hydroxide is a value measured by potentiometric titration.
[0017] The lithium sulfide content in the lithium sulfide powder of the present embodiment is preferably as high as possible, and is, for example, 98.0 mass% or more, preferably 98.3 mass% or more, more preferably 98.5 mass% or more, even more preferably 98.7 mass% or more, and particularly preferably 99.0 mass% or more. In this specification, the lithium sulfide content in the lithium sulfide powder is a value measured by potentiometric titration.
[0018] The lithium sulfide powder of this embodiment may contain moisture. The moisture content in the lithium sulfide powder is preferably as small as possible, and is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0.1% by mass or less. When the moisture content is within the above range, when the lithium sulfide powder is used as a raw material for a solid electrolyte, a decrease in ion conductivity due to water can be suppressed, and a solid electrolyte with better battery performance can be obtained. Thus, the lithium sulfide powder of this embodiment has a high lithium sulfide content, a low lithium hydroxide and water content, and is of high purity. In this specification, the moisture content in the lithium sulfide powder is a value measured by a vaporization method at 280° C. using a Karl Fischer moisture meter.
[0019] (Manufacturing method) The method for producing the lithium sulfide powder of the present embodiment is not particularly limited, and for example, the lithium sulfide powder can be produced by the method for producing the modified lithium sulfide powder of the present embodiment described later. That is, the lithium sulfide powder of the present embodiment is the same as the modified lithium sulfide powder obtained by the method for producing the modified lithium sulfide powder of the present embodiment.
[0020] (Application) The lithium sulfide powder of the present embodiment does not contain a solvent, has high purity and a large specific surface area, and has both excellent reactivity and ease of handling, and therefore can be suitably used as a raw material for solid electrolytes. The obtained solid electrolyte is suitably used in lithium ion secondary batteries, more specifically, in the solid electrolyte layer of an all-solid-state lithium ion secondary battery, and as a solid electrolyte to be mixed into a positive electrode or a negative electrode mixture. For example, a layer made of a solid electrolyte is provided between a positive electrode, a negative electrode, and between the positive electrode and the negative electrode to obtain an all-solid-state lithium ion secondary battery.
[0021] [Method for producing modified lithium sulfide powder] The method for producing the modified lithium sulfide powder of this embodiment includes contacting lithium sulfide powder with hydrogen sulfide in the absence of a solvent and subjecting the product obtained by the contact to a dehydrosulfiding treatment. In this specification, "modification" means improving at least one of the properties of the powder, such as the specific surface area and pore volume. Therefore, according to the production method of this embodiment, it can be said that the modified lithium sulfide powder can be obtained by improving at least one of the properties of the lithium sulfide powder used in the contact, such as the specific surface area and pore volume. The above-mentioned lithium sulfide powder of this embodiment can be produced by the production method of the modified lithium sulfide of this embodiment.
[0022] (Lithium sulfide powder) In the production method of the present embodiment, the lithium sulfide powder used in the contact can be used without any particular limitation. For example, a commercially available product may be used as is, or a product obtained by reacting lithium hydroxide, which will be described later, with a substance containing at least elemental sulfur may be used.
[0023] (Reacting) The lithium sulfide powder used in the contact can be a lithium sulfide powder obtained by reacting lithium hydroxide with a substance containing at least a sulfur element (hereinafter, the reaction between lithium hydroxide and a substance containing at least a sulfur element may be simply referred to as "reaction"). That is, the production method of this embodiment includes reacting lithium hydroxide with a substance containing at least a sulfur element to obtain lithium sulfide, and the lithium sulfide can be used in the contact. The method of reacting lithium hydroxide with a substance containing at least a sulfur element is not particularly limited, and can be carried out according to, for example, the following method that has been conventionally used. Note that, in this embodiment, the method of reacting lithium hydroxide with a substance containing at least a sulfur element is not limited to the following method.
[0024] a. A method in which lithium hydroxide and hydrogen sulfide are reacted in an aqueous solvent at a temperature below the boiling point of water (100°C or less). Specifically, hydrogen sulfide is introduced into an aqueous solution of lithium hydroxide and reacted at a temperature below the boiling point of water (100°C or less) (see JP 2011-084438 A). b. A method in which hydrogen sulfide gas is blown into a slurry consisting of lithium hydroxide and a hydrocarbon organic solvent (e.g., toluene), the lithium hydroxide is reacted with hydrogen sulfide, the reaction is continued while removing water produced by the reaction from the slurry, and after the water in the system has substantially disappeared, the blowing of hydrogen sulfide is stopped and an inert gas is blown in (see JP 2010-163356 A).
[0025] c. A method of reacting lithium hydroxide with a gaseous sulfur source (for example, hydrogen sulfide or hydrogen-containing sulfur vapor) at a temperature of 130 to 445° C. (see JP-A-9-278423 and JP-A-9-283156). d. A method in which, in the absence of a solvent, a predetermined amount of lithium hydroxide powder and hydrogen sulfide gas are added to a reaction vessel to be used and reacted with stirring (see WO 2016 / 098351).
[0026] In the production method of this embodiment, the substance containing at least elemental sulfur to be reacted with lithium hydroxide is not particularly limited as long as it contains at least elemental sulfur and is capable of producing lithium sulfide by reaction with lithium hydroxide. Examples of the substance include the hydrogen sulfide used in the above methods a and b, and the hydrogen-containing sulfur vapor used in the above methods c and d. Of these, hydrogen sulfide is preferred because it is easily available and a stable reaction can be easily achieved. As the hydrogen sulfide, for example, commercially available hydrogen sulfide can be used as it is. The hydrogen sulfide may or may not be dehydrated, but from the viewpoint of further reducing the influence on the reaction, it is preferable that the water content is small, and the water content may be, for example, about 50 ppm by mass or less.
[0027] The lithium hydroxide used in the production method of the present embodiment may be anhydrous lithium hydroxide or a hydrate such as lithium hydroxide monohydrate. If the modified lithium sulfide powder obtained by the production method of the present embodiment contains moisture, the battery performance may be deteriorated when the powder is used as a raw material for a solid electrolyte, and from the viewpoint of reducing the burden for removing moisture, it is preferable to use anhydrous lithium hydroxide. In the case of anhydrous lithium hydroxide, the water content is usually 5% by mass or less, 3% by mass or less, or 1.5% by mass or less. Here, the water content in lithium hydroxide can be measured using a Karl Fischer moisture meter in the same manner as in the measurement of the water content in the lithium sulfide powder.
[0028] The average particle size of the lithium hydroxide is preferably 0.01 mm or more, more preferably 0.05 mm or more, and even more preferably 0.1 mm or more, and the upper limit is preferably 3 mm or less, more preferably 2 mm or less, and even more preferably 1.5 mm or less. When the average particle size of the lithium hydroxide is within the above range, the lithium sulfide powder of the present embodiment having an average particle size of 0.1 mm or more and 1.5 mm or less is easily obtained, and the reaction with hydrogen sulfide is easily promoted.
[0029] In the production method of the present embodiment, the reaction between lithium hydroxide and a substance containing at least elemental sulfur can be carried out, for example, in the presence of a solvent as in the above methods a and b, or in the absence of a solvent as in the above methods c and d. Either method is acceptable, but from the viewpoint of efficiently obtaining solvent-free lithium sulfide, it is preferable to carry out the reaction in the absence of a solvent. In the production method of the present embodiment, when a solvent is used in the reaction between lithium hydroxide and a substance containing at least elemental sulfur, examples of the solvent that can be used include the solvents described in the above publication and those exemplified as solvents not included in the lithium sulfide powder of the present embodiment, that is, the above-mentioned saturated hydrocarbon solvents, unsaturated hydrocarbon solvents, aromatic hydrocarbon solvents, ketone solvents, ether solvents, alcohol solvents, ester solvents, halogenated hydrocarbon solvents, amide solvents, nitrile solvents, and the like.
[0030] In the production method of this embodiment, the reaction conditions between lithium hydroxide and a substance containing at least elemental sulfur may be in accordance with the conditions described in the above patent documents and are not particularly limited, but for example, in a method in which the reaction is carried out in the presence of a solvent, such as the above methods a and b, the temperature is usually 140° C. or higher and 230° C. or lower, and preferably 150° C. or higher and 220° C. or lower. If the reaction temperature is within the above range, not only can the reaction be promoted from a thermochemical perspective, but also the lithium hydroxide particles are less likely to aggregate, and the substance containing at least elemental sulfur is more likely to diffuse into the inside of the lithium hydroxide, so that the reaction can proceed further and a high-purity lithium sulfide powder in which the amount of unreacted lithium hydroxide is reduced can be easily obtained.
[0031] The reaction time can vary depending on the amount of lithium hydroxide and the substance containing at least a sulfur element used, the blending ratio, etc., and cannot be generally specified, but is usually about 1 hour to 60 hours, preferably 2 hours to 30 hours. Here, the reaction between lithium hydroxide and the substance containing at least a sulfur element is usually carried out by supplying the substance containing a sulfur element to a reaction vessel in which lithium hydroxide is present, and the reaction time is the time from the start of the supply of the substance containing at least a sulfur element (also referred to as the "start of the reaction") to the stop of the supply (also referred to as the "end of the reaction"). Note that water is generated in the reaction between lithium hydroxide and the substance containing at least a sulfur element, and the stop of the supply of the substance containing a sulfur element (end of the reaction) may be specifically the time when the generation of water stops or thereafter.
[0032] In the manufacturing method of this embodiment, after the reaction is completed, a post-treatment may be performed by further supplying hydrogen sulfide. By further supplying hydrogen sulfide, the reforming effect caused by contact between the lithium sulfide powder and hydrogen sulfide, which will be described later, is promoted. In this case, after the reaction is completed, the reaction may be continued in the reaction vessel in which the reaction was performed.
[0033] The method of supplying hydrogen sulfide is not particularly limited, and may be either a closed system (batch type) or a flow system, as long as it is performed according to the above-mentioned reaction format. In the case of a closed system, for example, hydrogen sulfide is supplied to a reaction vessel holding lithium sulfide powder so as to reach a predetermined pressure, and when the pressure in the reaction vessel decreases to the predetermined pressure due to the reduction caused by the reaction of hydrogen sulfide, hydrogen sulfide is supplied again. In addition, in the case of a flow system, the supply amount of hydrogen sulfide may be the same as or different from the supply amount when the above reaction is carried out in a flow system. The specific supply amount of hydrogen sulfide cannot be generally specified because it can vary depending on the amount of lithium sulfide, the capacity of the reaction vessel, etc., but from the viewpoint of more efficiently improving the reforming effect by contacting the lithium sulfide powder with hydrogen sulfide described later, it is preferably 5 N-mL / min or more, more preferably 50 N-mL / min or more, and even more preferably 100 N-mL / min or more, and the upper limit is preferably 1500 N-mL / min or less, more preferably 500 N-mL / min or less, and even more preferably 200 N-mL / min or less, relative to 100 g of lithium sulfide powder.
[0034] The temperature conditions during the post-treatment (the internal temperature of a reaction vessel or the like in which lithium sulfide is held) may be appropriately selected from the same temperature range as the reaction temperature described above, and is preferably 140° C. or higher, more preferably 160° C. or higher, even more preferably 180° C. or higher, and particularly preferably 190° C. or higher. There is no particular upper limit to the post-treatment temperature, but it may be set to, for example, about 230° C. or lower. By increasing the post-treatment temperature, hydrogen sulfide is more likely to diffuse into the inside of the powder, such as into the pores of lithium sulfide, and thus reforming due to contact between lithium sulfide and hydrogen sulfide, as described below, is promoted, and a more excellent reforming effect is obtained. The post-treatment time is not particularly limited and can be appropriately set depending on the amount of lithium sulfide to be post-treated, the supply amount of hydrogen sulfide, and the like, and cannot be generally specified; however, it is usually about 5 minutes to 10 hours, and from the viewpoint of performing the post-treatment more efficiently, it is preferably 10 minutes to 5 hours, and more preferably 15 minutes to 3 hours.
[0035] In addition, the lithium sulfide powder obtained by the above reaction may contain gases such as inert gases and hydrogen sulfide. In the production method of this embodiment, it is preferable to remove these gases under reduced pressure. That is, in the production method of this embodiment, it is preferable to contact the lithium sulfide powder with hydrogen sulfide, which will be described later, after removing the gases contained in the lithium sulfide powder obtained by the above reaction under reduced pressure. A modified lithium sulfide powder with higher purity and a larger specific surface area can be obtained.
[0036] The above reaction produces lithium sulfide powder, which may contain unreacted lithium hydroxide, etc. The lithium sulfide content in the lithium sulfide powder produced by the above reaction is usually about 97.5% by mass or more, and when unreacted lithium hydroxide is contained, the content is usually about 1.0% by mass. The moisture content in the lithium sulfide powder is about 1.5% by mass or less. The average particle size of the lithium sulfide powder obtained by the above reaction will vary depending on the average particle size of the lithium hydroxide used in the reaction, but will be approximately 0.1 mm or more and 1.5 mm or less.
[0037] (Contacting) The method for producing the modified lithium sulfide powder of this embodiment includes contacting the lithium sulfide powder with hydrogen sulfide in the absence of a solvent (hereinafter, sometimes simply referred to as "contact"). This contact causes the lithium sulfide powder to react with hydrogen sulfide, producing lithium hydrosulfide (LiSH) in at least a portion of the lithium sulfide powder, which is then desulfurized to lithium sulfide, thereby modifying the lithium sulfide powder. Although the mechanism of modification in this embodiment is unclear, it is believed that the portion of the lithium sulfide powder that produced lithium hydrosulfide by contact with hydrogen sulfide returns to lithium sulfide by desulfurization, resulting in a state different from that of the original lithium sulfide portion, resulting in a modified lithium sulfide powder with an improved specific surface area, etc. Therefore, in the manufacturing method of the present embodiment, in order to obtain a modified lithium sulfide powder having a higher purity and a larger specific surface area, it is essential to produce a larger amount of lithium hydrosulfide by carrying out contact. In addition, when the lithium sulfide powder contains unreacted lithium hydroxide, lithium sulfide is produced by the reaction between lithium hydroxide and hydrogen sulfide by carrying out contact, so that an effect of obtaining a lithium sulfide powder of higher purity is also obtained.
[0038] The contact needs to be carried out in the absence of a solvent. By carrying out the contact in the absence of a solvent, a modified lithium sulfide powder free of a solvent can be efficiently obtained. If the contact is carried out in the presence of a solvent, the resulting modified lithium sulfide powder will contain the solvent. Although the solvent can be removed by drying the modified lithium sulfide powder containing the solvent, there are cases where the solvent cannot be completely removed, and even if the solvent can be completely removed, a large-scale facility is required, making it impossible to efficiently obtain the modified lithium sulfide powder.
[0039] When using a commercially available lithium sulfide powder, it is sufficient to select one with a smaller solvent content, and if no solvent is used in the reaction between the lithium hydroxide and a substance containing at least elemental sulfur, the obtained lithium sulfide powder can be used as is. In addition, if a solvent is used in the reaction and the lithium sulfide powder is accompanied by a solvent, a drying process may be performed to remove the solvent before use in the contact. The drying process may be performed based on a known method, and various drying process conditions such as drying temperature and time may be appropriately set depending on the type of solvent to be removed.
[0040] The lithium sulfide powder is preferably contacted with hydrogen sulfide by a heat treatment in the presence of hydrogen sulfide. More specifically, the heat treatment may be performed under a hydrogen sulfide gas flow, specifically under the following temperature conditions: The contact is preferably carried out at least once under a temperature condition of 20° C. or more and 120° C. or less. By carrying out the contact at least once under the above temperature condition, lithium hydrosulfide can be produced more efficiently and in larger quantities. From the same viewpoint, the temperature condition is more preferably 30° C. or more and 110° C. or less, further preferably 40° C. or more and 110° C. or less, and particularly preferably 50° C. or more and 80° C. or less.
[0041] The contact is preferably carried out two or more times under different temperature conditions as necessary. For example, when a commercially available lithium sulfide is used, the contact is carried out two or more times under different temperature conditions to efficiently produce a larger amount of lithium hydrosulfide. In this case, the different temperature conditions to be combined with the above-mentioned temperature conditions of 20°C or more and 120°C or less are preferably 140°C or more, more preferably 160°C or more, even more preferably 180°C or more, particularly preferably 190°C or more, and although there is no particular limit as an upper limit, it may be about 230°C or less. In the production method of this embodiment, from the viewpoint of efficiently producing a larger amount of lithium hydrosulfide, it is preferable to carry out contact under higher temperature conditions and then carry out contact under lower temperature conditions, specifically, it is preferable to carry out contact at 140°C or more (hereinafter, the first contact may be referred to as "first contact", and the same applies to the second and subsequent contacts), and then carry out the second contact at 20°C or more and 120°C or less. By carrying out contact at such a temperature in the absence of a solvent, when the lithium sulfide powder is accompanied by a solvent, it is possible to further reduce the content of the solvent.
[0042] The temperature conditions for contact in this embodiment are not limited to those described in the specific examples above. For example, it is possible to perform contact (first contact) at 140° C. or higher, contact (second contact) at 20° C. or higher and 120° C. or lower, and then contact (third contact) at 140° C. or higher. In another embodiment, it is possible to perform contact (first contact) at 140° C. or higher, contact (second contact) at 150° C. (a temperature outside the range of 20° C. or higher and 120° C. or lower), and then contact (third contact) at 80° C. (a temperature in the range of 20° C. or higher and 120° C. or lower). It is also possible to perform contact (first contact) at 180° C. or higher, contact (second contact) at 60° C. (a temperature in the range of 20° C. or higher and 120° C. or lower), and then contact (third contact) at 80° C. (a temperature in the range of 20° C. or higher and 120° C. or lower).
[0043] In this embodiment, for example, when the contact is performed two or more times, the contact time under higher temperature conditions, preferably 140° C. or higher, may be about 5 minutes to 10 hours, and from the viewpoint of efficiently producing a larger amount of lithium hydrosulfide, is preferably 10 minutes to 5 hours, more preferably 15 minutes to 3 hours. From the same viewpoint, the contact time under lower temperature conditions, preferably 20° C. to 120° C., is about 1 hour to 20 hours, preferably 2 hours to 15 hours, more preferably 5 hours to 12 hours. In addition, the temperature in each contact may vary as long as it is within the above-mentioned predetermined temperature range, but from the viewpoint of obtaining a more stable reforming effect, it is preferable to maintain the same temperature for the above-mentioned contact time. In addition, the time required to shift from the first contact to the second contact (the time required to shift to the temperature condition of the next contact) is not considered as the contact time, and it is preferable to shift to the temperature condition of the next contact as soon as possible, and in consideration of making the shift easier, for example, the shift to 100°C may be performed within 30 minutes to 1.5 hours.
[0044] In this embodiment, when the lithium sulfide powder obtained by the above reaction is used and two or more contacts are performed under different temperature conditions, the post-treatment in the above reaction can be performed under a higher temperature condition than the first contact. In this case, for example, if the contact is performed at 20° C. or higher and 120° C. or lower after the post-treatment in the above reaction, two or more contacts are performed under substantially different temperature conditions.
[0045] The amount of hydrogen sulfide supplied in the above contact cannot be generally defined as it may vary depending on the amount of lithium sulfide, the capacity of the reaction vessel, etc., but from the viewpoint of efficiently producing a larger amount of lithium hydrosulfide, the amount is preferably 5 N-mL / min or more, more preferably 50 N-mL / min or more, and even more preferably 100 N-mL / min or more, per 100 g of lithium sulfide powder, with the upper limit being preferably 1500 N-mL / min or less, more preferably 500 N-mL / min or less, and even more preferably 200 N-mL / min or less.
[0046] The product obtained by the above contact is lithium sulfide powder, at least a part of which becomes lithium hydrosulfide due to the reaction between lithium sulfide powder and hydrogen sulfide. In the product, lithium hydrosulfide is unevenly distributed on the surface and its vicinity (including the inner wall surface of the lithium sulfide pores), which are parts of the lithium sulfide powder that are likely to come into contact with hydrogen sulfide. In other words, the product contains lithium hydrosulfide and can be said to be lithium sulfide powder having a layer of lithium hydrosulfide on at least a part of its surface. The content of lithium hydrosulfide in the product is usually 5% by mass or more and 100% by mass or less, further 20% by mass or more and 75% by mass or less, further 30% by mass or more and 50% by mass or less. In this way, the product obtained by the above contact may be substantially lithium hydrosulfide powder without any remaining lithium sulfide. In the production method of the present embodiment, by carrying out the above contact, the content of lithium hydrosulfide becomes higher, and an excellent modification effect is obtained.
[0047] (Desulfurization) The method for producing the modified lithium sulfide powder of the present embodiment includes subjecting the product obtained by the above contact to a desulfurization treatment. The product obtained by the above contact is lithium sulfide powder at least a part of which is lithium hydrosulfide, and by subjecting the product to a desulfurization treatment, the lithium hydrosulfide is converted to lithium sulfide, thereby obtaining the modified lithium sulfide powder.
[0048] The method of dehydrogensulfurization is not particularly limited, but may be, for example, a method of heat treatment in the presence of an inert gas. More specifically, heat treatment may be performed under a stream of an inert gas, and the heating temperature conditions are preferably 130° C. or higher and 230° C. or lower, more preferably 140° C. or higher and 220° C. or lower, and even more preferably 150° C. or higher and 210° C. or lower. With the above heating temperature conditions, dehydrogensulfurization can be performed more efficiently. Examples of the inert gas include rare gases such as helium, neon, and argon, nitrogen, and carbon dioxide. Of these, nitrogen is preferred from the viewpoints of being less expensive and more readily available.
[0049] The modified lithium sulfide powder obtained by the method for producing the modified lithium sulfide powder of the present embodiment does not contain a solvent and has a specific surface area of 10 m 2 / g or more and an average particle size of 0.1 mm or more and 1.5 mm or less, that is, the lithium sulfide powder of the present embodiment can be obtained by the method for producing the modified lithium sulfide powder of the present embodiment. The lithium sulfide powder obtained by the manufacturing method of this embodiment does not contain a solvent, has high purity and a large specific surface area, and has both excellent reactivity and ease of handling, and therefore can be suitably used as a raw material for solid electrolytes. The obtained solid electrolyte is suitably used in lithium ion secondary batteries, more specifically, in the solid electrolyte layer of an all-solid-state lithium ion secondary battery, and as a solid electrolyte to be mixed into a positive electrode or a negative electrode mixture. For example, an all-solid-state lithium ion secondary battery can be obtained by providing a layer of solid electrolyte between a positive electrode, a negative electrode, and between the positive electrode and the negative electrode.
[0050] (Lithium hydrosulfide-containing powder) The lithium hydrosulfide-containing powder of this embodiment does not contain a solvent, contains lithium hydrosulfide and lithium sulfide, and is characterized in that the content of the lithium hydrosulfide is 5 mass% or more and 100 mass% or less with respect to the total of the lithium hydrosulfide and lithium sulfide. The lithium hydrosulfide-containing powder of this embodiment is a lithium sulfide powder at least a part of which becomes lithium hydrosulfide by a reaction between lithium sulfide powder and hydrogen sulfide, which is a product obtained by contacting in the manufacturing method of the modified lithium sulfide powder of this embodiment. In addition, since the contacting in the manufacturing method of this embodiment is performed in the absence of a solvent, the lithium hydrosulfide-containing powder of this embodiment does not contain a solvent. EXAMPLES
[0051] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.
[0052] (Measurement of lithium sulfide content, lithium hydroxide content, and lithium hydrosulfide content) The lithium sulfide content, lithium hydroxide content, and lithium hydrosulfide content in the lithium sulfide powder were analyzed and measured by hydrochloric acid titration and silver nitrate titration. Specifically, the lithium sulfide powder obtained in the examples and comparative examples was weighed in a glove box (dew point: about -100°C, nitrogen atmosphere), dissolved in water, and measured and calculated using a potentiometric titrator ("COM-980 (model number)" manufactured by Hiranuma Sangyo Co., Ltd.). (Measurement of Solvent Content) The presence or absence of the solvent in the lithium sulfide powder and the content thereof were confirmed and quantified by dissolving the lithium sulfide powder in methanol and subjecting the resulting solution to gas chromatography. (Measurement of moisture content) The moisture content in the anhydrous lithium hydroxide and lithium sulfide powders was measured using a Karl Fischer moisture meter. (Measurement of average particle size) Using a laser diffraction particle size distribution analyzer ("LA-950 (product name)" (manufactured by Horiba, Ltd.), the particle diameter D50 at a cumulative volume percentage of 50% was measured and used as the average particle diameter. (Measurement of specific surface area) The specific surface area was measured using a gas adsorption measurement device.
[0053] (Production Example 1: Synthesis of lithium sulfide (based on method d above)) In a 500mL separable flask (equipped with an anchor stirring blade), 200g of lithium hydroxide anhydride (manufactured by Honjo Chemical Co., Ltd., particle size range: 0.1mm to 1.5mm, moisture content: 1% by mass or less) was added under nitrogen gas flow, and the temperature was raised to 200°C using an oil bath while stirring at 60 rpm, and the temperature was maintained at 200°C. In addition, the upper part of the separable flask was maintained at 100°C using a ribbon heater. The nitrogen was switched to hydrogen sulfide (manufactured by Tomoe Shokai Co., Ltd.), and the reaction between lithium hydroxide and hydrogen sulfide was carried out while supplying it at a flow rate of 500N-mL / min. The moisture generated by the progress of the reaction was condensed and collected by a condenser, and 144mL of water was collected after 6 hours of reaction, and no water was generated even after another 3 hours. Next, while maintaining the temperature at 200° C., the hydrogen sulfide was replaced with nitrogen, and nitrogen was passed through for 20 minutes to replace the hydrogen sulfide in the flask with nitrogen. The lithium sulfide thus obtained was measured by potentiometric titration, and the lithium sulfide content was found to be 98.5% by mass, and the lithium hydroxide content was 0.1% by mass or less (below the detection limit). The specific surface area and average particle size were also measured, and the specific surface area was 8 m 2 / g, and the average particle size was 350 μm (0.35 mm).
[0054] (Production Example 2: Synthesis of lithium sulfide (based on method b above)) To a 600 ml separable flask, 270 g of toluene (a reagent manufactured by Hiroshima Wako Co., Ltd.) was added under a nitrogen stream, followed by 30 g of anhydrous lithium hydroxide (manufactured by Honjo Chemical Co., Ltd., particle size range: 0.1 mm to 1.5 mm, moisture content: 1 mass % or less). The mixture was maintained at 95°C while stirring with a full zone stirring impeller at 300 rpm. The temperature was raised to 104°C while hydrogen sulfide (Tomoe Shokai Co., Ltd.) was blown into the slurry solution obtained by the above reaction at a supply rate of 300 ml / min. An azeotropic gas of water and toluene was continuously discharged from the separable flask. This azeotropic gas was dehydrated by condensing it in a condenser outside the system. During this time, toluene in an amount equal to the amount of toluene distilled was continuously supplied to keep the amount of the slurry solution constant. The amount of water in the condensate gradually decreased, and distillation of water was no longer observed 6 hours after the introduction of hydrogen sulfide (the total amount of water was 22 ml). During the reaction, the solid was dispersed in the toluene and stirred, and no water separated from the toluene. Thereafter, the hydrogen sulfide was replaced with nitrogen, which was passed at 300 N-ml / min for 1 hour. Next, the slurry solution was filtered, and after filtration, it was vacuum dried at 200° C. to obtain lithium sulfide powder. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was found to be 97.7% by mass, and the lithium hydroxide content was found to be 0.7% by mass. The specific surface area and average particle size were also measured, and the specific surface area was 15 m 2 / g, and the average particle size was 350 μm (0.35 mm).
[0055] Example 1 4.0 g of the lithium sulfide powder obtained in Production Example 1 was placed in a Schlenk flask equipped with an inert gas and hydrogen sulfide flowing equipment and capable of being sealed in a glove box, and was placed in an oil bath while flowing nitrogen (flow rate: 100 N-mL / min), and the temperature was raised to 200 ° C. When the temperature of the powder stabilized at 200 ° C., nitrogen was switched to hydrogen sulfide, and contact (first contact) between the lithium sulfide powder and hydrogen sulfide was performed for 30 minutes at a flow rate of 50 N-mL / min, and then the temperature was lowered from 200 ° C. to 60 ° C. over 1 hour, and the second contact (second contact) between the lithium sulfide powder and hydrogen sulfide was performed by holding at 60 ° C. for 8 hours at a flow rate of 50 N-mL / min. Thereafter, the hydrogen sulfide gas was stopped, and a portion was sampled. Here, when the powder obtained by sampling after the hydrogen sulfide gas was stopped (powder before dehydrosulfidation treatment) was analyzed, it was confirmed to contain lithium hydrosulfide, with the content being 34.1 mass%. Thereafter, the hydrogen sulfide was switched to nitrogen and circulated (flow rate: 100 N-mL / min) while the temperature was raised from 60°C to 160°C over 30 minutes and held at that temperature for 30 minutes to carry out dehydrosulfidation treatment. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was 98.6% by mass, the lithium hydroxide content was 0.2% by mass, and the solvent content was not detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 21 m 2 The average particle size was 437 μm (0.437 mm) and the results are shown in Table 1.
[0056] Example 2 Lithium sulfide powder was obtained in the same manner as in Example 1, except that the temperature of the second contact was changed from 60°C to 40°C. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was 99.0% by mass, the lithium hydroxide content was 0.1% by mass, and the solvent content was not detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 17 m 2 / g, and the average particle size was 386 μm (0.386 mm). The lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, and was found to be 20.4 mass%. These results are shown in Table 1.
[0057] Example 3 Lithium sulfide powder was obtained in the same manner as in Example 1, except that the temperature of the second contact was changed from 60°C to 25°C. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was 98.3% by mass, the lithium hydroxide content was 0.2% by mass, and the solvent content was not detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 13 m 2 / g, and the average particle size was 410 μm (0.410 mm). These results are shown in Table 1. Furthermore, when the lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, the content was 8.8 mass%.
[0058] Example 4 4.0 g of the lithium sulfide powder obtained in Production Example 1 was placed in a Schlenk flask equipped with equipment capable of flowing an inert gas and hydrogen sulfide and capable of being sealed. While flowing nitrogen (flow rate: 100 mL / min), when the temperature of the powder stabilized at room temperature (25° C.), the nitrogen was switched to hydrogen sulfide and the lithium sulfide powder was contacted with hydrogen sulfide at a flow rate of 50 mL / min for 16 hours. Thereafter, the hydrogen sulfide was switched to nitrogen and flowed (flow rate: 100 mL / min) while the temperature was raised from 60°C to 160°C over 1 hour and maintained at that temperature for 30 minutes to carry out dehydrosulfidation treatment. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was 99.0% by mass, the lithium hydroxide content was 0.1% by mass, and the solvent content was not detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 13 m 2 / g, and the average particle size was 393 μm (0.393 mm). The lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, and was found to be 11.3 mass%. These results are shown in Table 1.
[0059] Example 5 In a 500mL separable flask (equipped with an anchor stirring blade), 200g of lithium hydroxide anhydride (manufactured by Honjo Chemical Co., Ltd., particle size range: 0.1mm to 1.5mm, moisture content: 1% by mass or less) was added under nitrogen gas flow, and the temperature was raised to 200°C using an oil bath while stirring at 60 rpm, and the temperature was maintained at 200°C. The upper part of the separable flask was also maintained at 100°C using a ribbon heater. Nitrogen was switched to hydrogen sulfide (manufactured by Tomoe Shokai Co., Ltd.) and the reaction between lithium hydroxide and hydrogen sulfide was carried out while supplying it at a flow rate of 500N-mL / min. The moisture generated by the progress of the reaction was condensed and collected by a condenser, and 144mL of water was collected after 6 hours of reaction. Thereafter, the temperature was maintained at 200°C and hydrogen sulfide was continuously supplied for another 3 hours (corresponding to the first contact), but no water was generated. Next, the temperature was lowered from 200°C to 60°C over 1 hour while supplying hydrogen sulfide, and the temperature was maintained at 60°C for 8 hours with a flow rate of 100 N-mL / min to carry out contact between the reactant (lithium sulfide powder) and hydrogen sulfide (second contact). Thereafter, the hydrogen sulfide was replaced with nitrogen and, while flowing (flow rate: 100 N-mL / min), the temperature was raised from 60°C to 160°C over 1 hour and held at that temperature for 30 minutes to carry out dehydrosulfidation treatment. The lithium sulfide thus obtained was measured by potentiometric titration, and the lithium sulfide content was 98.6% by mass, the lithium hydroxide content was 0.2% by mass, and no solvent was detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 21 m2 / g, and the average particle size was 436 μm (0.436 mm). The lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, and was found to be 29.5 mass%. These results are shown in Table 1.
[0060] Example 6 Lithium sulfide powder was obtained in the same manner as in Example 1, except that the time for the second contact was changed from 8 hours to 16 hours. The lithium sulfide powder thus obtained was measured by potentiometric titration, and the lithium sulfide content was 99.0% by mass, the lithium hydroxide content was 0.1% by mass, and the solvent content was not detected (0.1% by mass or less). The specific surface area and average particle size were also measured, and the specific surface area was 24 m 2 / g, and the average particle size was 350 μm (0.350 mm). The lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, and was found to be 41.5 mass %. These results are shown in Table 1.
[0061] Comparative Example 1 6.0 g of lithium sulfide obtained in Production Example 2 was weighed into a Schlenk flask in a glove box. 120 ml of dehydrated toluene (manufactured by Wako Pure Chemical Industries, Ltd.) was added to this under a nitrogen atmosphere. While flowing hydrogen sulfide at 100 ml / min, stirring was performed with a Teflon (registered trademark) anchor blade for 2 hours under conditions of 50°C and normal pressure. Hydrogen sulfide was stopped, and a portion was sampled. Next, the oil bath temperature was raised to 110°C, and heat treatment was performed for 2 hours under conditions of 110°C and normal pressure. After the temperature was raised, nitrogen was passed through to recover the modified lithium sulfide. Vacuum drying was performed at 200°C to obtain lithium sulfide powder. The resulting modified lithium sulfide was measured by potentiometric titration, and the purity of the lithium sulfide was 97.8% by mass, the content of lithium hydroxide was 0.4% by mass, and the content of toluene was 0.2% by mass. The specific surface area and average particle size were also measured, and the specific surface area was 27 m 2 / g, and the average particle size was 394 μm (0.394 mm). The lithium hydrosulfide content of the powder before the dehydrosulfidation treatment was measured in the same manner as in Example 1, and was found to be 44.4 mass%. These results are shown in Table 1.
[0062] Comparative Example 2 6.0 g of lithium sulfide obtained in Production Example 2 was weighed into a Schlenk flask in a glove box. 120 ml of dehydrated ethanol (manufactured by Wako Pure Chemical Industries, Ltd.) was added to this under a nitrogen atmosphere. While flowing hydrogen sulfide at 100 ml / min, stirring was performed with a Teflon (registered trademark) anchor blade for 2 hours under conditions of 50°C and normal pressure. Hydrogen sulfide was stopped, and a portion was sampled. Next, the oil bath temperature was raised to 110°C, and heat treatment was performed for 2 hours under conditions of 110°C and normal pressure. After the temperature was raised, nitrogen was passed through to recover the modified lithium sulfide. Vacuum drying was performed at 200°C to obtain lithium sulfide powder. The resulting modified lithium sulfide was measured by potentiometric titration, and the purity of the lithium sulfide was 96.5% by mass, the content of lithium hydroxide was 0.7% by mass, the content of toluene was 0.4% by mass, and the content of ethanol was 0.8% by mass. The specific surface area and average particle size were also measured, and the specific surface area was 40 m 2 / g, and the average particle size was 10 μm (0.010 mm). Furthermore, when the content of lithium hydrosulfide was measured for the powder before the dehydrosulfidation treatment in the same manner as in Example 1, no lithium hydrosulfide was detected. These results are shown in Table 1.
[0063] [Table 1] *1. Content in powder before dehydrogenation treatment.
[0064] From the results of Examples 1 to 6, the lithium sulfide powder of this embodiment (lithium sulfide powder obtained by the production method of this embodiment) has a solvent content of 0.1 mass % or less (no solvent was detected), does not contain a solvent, and has a specific surface area of 13 to 24 m 2 / g and 10m 2 / g or more, and the average particle size was 350 to 437 μm (0.350 to 0.437 mm), which was 0.1 mm or more and 1.5 mm or less. The lithium hydroxide content was 0.1 to 0.2 mass%, both of which were 0.3 mass% or less, and the lithium sulfide content was 98.3 to 99.0 mass%, which was 98.0 mass% or more. Therefore, it was confirmed that the lithium sulfide powders of this embodiment in Examples 1 to 6 (lithium sulfide powders obtained by the manufacturing method of this embodiment) do not contain a solvent, have high purity and a large specific surface area, and are easy to handle.
[0065] From the results of Examples 1 to 3, it was found that the specific surface area tends to improve when the temperature of the second contact is increased. The lithium sulfide powder obtained in Example 5 was obtained by performing the first contact as a post-treatment of the lithium sulfide powder obtained by reaction, followed by the second contact at 60°C. As with the other Examples, it had high purity and a high specific surface area, and was easy to handle. From this, it was confirmed that the post-treatment after the reaction can be the first contact. In addition, from a comparison between Examples 1 and 6, it was confirmed that the reactivity can be improved by increasing the second contact time, since the specific surface area can be increased by about 14% and the average particle size can be reduced by about 20%. From the above results, it can be seen that the manufacturing method of this embodiment can be adapted by adjusting the contact temperature, contact time, etc. according to the desired specific surface area and average particle size.
[0066] On the other hand, the lithium sulfide powders obtained in Comparative Examples 1 and 2, in which a solvent was used during contact, had a large specific surface area but contained 0.2 and 1.2 mass% of the solvent. Although the solvent can be removed from the lithium sulfide powders obtained in these Comparative Examples by drying treatment or the like, this requires large-scale equipment and there is a possibility that the solvent cannot be completely removed, so it is difficult to say that the solvent can be obtained efficiently.
[0067] Moreover, from the results of Examples 1 to 6, it was confirmed that the content of lithium hydrosulfide in the lithium hydrosulfide-containing powder of the present embodiment was 8.8 to 41.5 mass %. [Industrial Applicability]
[0068] The lithium sulfide powder of the present embodiment does not contain a solvent, has high purity and a large specific surface area, and has both excellent reactivity and ease of handling, and therefore can be suitably used as a raw material for solid electrolytes. The obtained solid electrolyte is suitably used in lithium ion secondary batteries, more specifically, in the solid electrolyte layer of an all-solid-state lithium ion secondary battery, and as a solid electrolyte to be mixed into a positive electrode or a negative electrode mixture. For example, a layer made of a solid electrolyte is provided between a positive electrode, a negative electrode, and between the positive electrode and the negative electrode to obtain an all-solid-state lithium ion secondary battery.
Claims
1. The solvent content is 0.1% by mass or less, Specific surface area is 10m 2 / g or more and 50 m 2 / g or less, The content of lithium hydroxide is 0.01% by mass or more and 0.3% by mass or less, The lithium sulfide content is 98.0% by mass or more, The pore volume is 0.005 ml / g or more and 1.0 ml / g or less. Modified lithium sulfide powder.
2. The modified lithium sulfide powder according to claim 1, having an average particle size of 0.15 mm or more and 1.5 mm or less.
3. The modified lithium sulfide powder according to claim 1 or 2, having a moisture content of 0.5 mass% or less.
Citation Information
Patent Citations
Preparation method and device of high-purity lithium sulfide
CN105016310A
Production of lithium sulfide
JP1997278423A
Method for producing lithium sulfide
JP2010163356A
Lithium sulfide and method for producing the same
JP2011084438A
Method and device for producing lithium sulfide
JP2012140261A