Preparation method of lithium sulfide

By reacting lithium sulfate powder with carbon monoxide and combining the crushing and heat treatment steps, the problems of high cost of lithium sulfide preparation and poor reactivity are solved, and the preparation of high-purity lithium sulfide fine powder is realized, and the performance of solid electrolyte is improved.

CN119053545APending Publication Date: 2024-11-29SOLID IONICS CO LTD

Patent Information

Application Number
CN202280094992.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-05-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the existing lithium sulfide preparation methods, it is difficult to crush lithium hydroxide or lithium carbonate, resulting in low reaction efficiency and high cost. The lithium sulfide powder has a large size and a reduced reactivity, making it difficult to prepare high-purity lithium sulfide.

Method used

The lithium sulfate powder is reacted with carbon monoxide reaction gas, and the lithium sulfate powder is refined through the pulverization and preheating steps, and the lithium sulfide powder is heat treated at high temperature to prepare micropowder lithium sulfide.

Benefits of technology

The preparation cost of lithium sulfide is reduced, the purity and reactivity of lithium sulfide powder are improved, and the reaction performance of solid electrolytes is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053545A_ABST
    Figure CN119053545A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing lithium sulfide, comprising: a lithium sulfide synthesis step for synthesizing a lithium sulfide powder by reacting a lithium sulfate powder with a reaction gas containing carbon monoxide, the method further comprising, before the lithium sulfide synthesis step, a lithium sulfate pulverization step for pulverizing the lithium sulfate powder; the lithium sulfate powder is pulverized to a predetermined size.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a lithium sulfide (Li 2 S) preparation method. Background Art

[0002] In recent years, the demand for lithium sulfide as a solid electrolyte raw material for all-solid-state lithium secondary batteries has been increasing. All-solid-state lithium secondary batteries are types that replace the organic liquid electrolyte and separator in currently commercialized lithium secondary batteries with solid electrolytes. Solid electrolytes are safer than liquid electrolytes because they are non-flammable or flame-retardant. Solid electrolytes are divided into oxide-based and sulfide-based. Sulfide-based solid electrolytes are mainly used as solid electrolytes because they have higher lithium ion conductivity and stability over a wide voltage range compared to oxide-based solid electrolytes.

[0003] Since lithium sulfide does not exist in natural mineral form, it is synthesized from other lithium compounds. Generally, lithium sulfide can be prepared by a synthesis process using lithium hydroxide or lithium carbonate as a lithium source. For example, the preparation method of lithium sulfide can be achieved by mixing a solid lithium source (e.g., lithium hydroxide or lithium carbonate) with a gaseous sulfur source (S or C S). 2(g) ) reaction to prepare lithium sulfide. However, it is difficult to crush lithium hydroxide or lithium carbonate into fine powder, and the reaction efficiency with the gas as a sulfur source is reduced, so it may be difficult to prepare high-purity lithium sulfide. In addition, since the size of lithium sulfide increases during the synthesis process, the reactivity may decrease during the synthesis process of the solid electrolyte. In addition, lithium hydroxide and lithium carbonate used as lithium sources are expensive, which may increase the preparation cost of lithium sulfide. Summary of the invention

[0004] Technical issues

[0005] The object of the present invention is to provide a method for preparing lithium sulfide, which can reduce the preparation cost of lithium sulfide and improve the purity of lithium sulfide powder.

[0006] Furthermore, an object of the present invention is to provide a method for preparing lithium sulfide, which can improve the reactivity of the lithium sulfide powder by reducing the size of the lithium sulfide powder.

[0007] Technical Solution

[0008] The method for preparing lithium sulfide of the present invention is characterized by comprising: a lithium sulfide synthesis step of synthesizing lithium sulfide powder by reacting lithium sulfate powder with a reaction gas containing carbon monoxide.

[0009] Furthermore, before the lithium sulfide synthesis step, the lithium sulfide preparation method of the present invention may further include: a lithium sulfate crushing step of crushing the lithium sulfate powder to a predetermined size. Furthermore, in the lithium sulfate crushing step, the lithium sulfate powder may be crushed to a powder having a size of 0.01 to 10.0 μm.

[0010] Furthermore, after the lithium sulfate crushing step, the method for preparing lithium sulfide of the present invention may further include: a lithium sulfate preheating step, wherein the lithium sulfate powder is heated to remove the residual moisture in the lithium sulfate powder. In the lithium sulfate preheating step, the lithium sulfate hydrate may be heated to 100-400°C.

[0011] Furthermore, after the lithium sulfide synthesis step, the lithium sulfide preparation method of the present invention may further include: a lithium sulfide powder heat treatment step, in which the synthesized lithium sulfide powder is heat treated to increase the crystallinity of the lithium sulfide powder. The lithium sulfide powder heat treatment step may be performed at a heat treatment temperature higher than the synthesis temperature of the lithium sulfide synthesis step.

[0012] Furthermore, the synthesis temperature of the lithium sulfide synthesis step may be 650-840°C, and the heat treatment temperature of the lithium sulfide powder heat treatment step may be 850-930°C.

[0013] Furthermore, the reaction gas may further include hydrogen and a transport gas. Furthermore, based on the total volume of the reaction gas, the reaction gas may include 10 to 50 volume percent of the carbon monoxide, 50 to 90 volume percent of hydrogen and a transport gas, and the volume ratio of the transport gas to hydrogen may be 90:10 to 99:1. Furthermore, based on the total volume of the reaction gas, the reaction gas may include 10 to 50 volume percent of the carbon monoxide, 0.5 to 10 volume percent of the hydrogen, and 45 to 90 volume percent of the transport gas.

[0014] In addition, the reaction gas may further include hydrogen. Based on the total volume of the reaction gas, the reaction gas may include 90-99.5 volume percent of the carbon monoxide and 0.5-10 volume percent of the hydrogen.

[0015] Furthermore, the lithium sulfide powder can be used as a solid electrolyte for all-solid-state batteries.

[0016] Effects of the Invention

[0017] In the method for preparing lithium sulfide of the present invention, lithium sulfate or lithium sulfate hydrate is used as a lithium source, thereby having the effect of reducing the preparation cost.

[0018] Furthermore, in the method for preparing lithium sulfide of the present invention, since carbon is not used, no carbon will remain in the prepared lithium sulfide powder, thereby having the effect of improving the purity of the lithium sulfide powder.

[0019] Furthermore, in the method for producing lithium sulfide of the present invention, since lithium sulfate which can be crushed into a smaller size than other lithium sources is used, there is an effect of reducing the size of the produced lithium sulfide powder.

[0020] Furthermore, in the method for preparing lithium sulfide of the present invention, since lithium sulfate crushed into small sizes is used, the reactivity with gas is improved as the surface area increases, thereby increasing the crystallinity of the lithium sulfide powder.

[0021] Furthermore, in the method for preparing lithium sulfide of the present invention, since the lithium sulfide powder is prepared as a fine powder, it has the effect of improving the reactivity of the lithium sulfate powder with other powders during the solid electrolyte synthesis process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 FIG. 4 is a process diagram of a method for preparing lithium sulfide according to an embodiment of the present invention.

[0023] Figure 2 This is a SEM image of lithium sulfate powder used in a specific embodiment of the present invention before pulverization.

[0024] Figure 3 This is a SEM image of the pulverized lithium sulfate powder used in a specific embodiment of the present invention.

[0025] Figure 4 The XRD spectrum of lithium sulfide powder synthesized according to a specific embodiment of the present invention.

[0026] Figure 5 This is the XRD pattern of commercially available lithium sulfide powder.

[0027] Figure 6 For display use Figure 4 Curve diagram of the charge and discharge performance of half-cells prepared with synthesized lithium sulfide powder and commercially available lithium sulfide powder. DETAILED DESCRIPTION

[0028] Hereinafter, a method for preparing lithium sulfide according to an embodiment of the present invention will be described in detail.

[0029] First, a method for preparing lithium sulfide according to an embodiment of the present invention is described.

[0030] Figure 1 FIG. 4 is a process diagram of a method for preparing lithium sulfide according to an embodiment of the present invention.

[0031] Reference Figure 1 According to an embodiment of the present invention, the method for preparing lithium sulfide includes a lithium sulfate crushing step S10 and a lithium sulfide synthesis step S30. In addition, the method for preparing lithium sulfide may also include a lithium sulfate preheating step S20 and a lithium sulfide powder heat treatment step S40.

[0032] In the above-mentioned method for preparing lithium sulfide, lithium sulfate or lithium sulfate hydrate may be used as a lithium source. In addition, in the above-mentioned method for preparing lithium sulfide, a gas containing carbon monoxide (CO) may be used as a reaction gas. In addition, the above-mentioned reaction gas may also contain hydrogen. In addition, the above-mentioned reaction gas may also contain hydrogen and a transport gas. The above-mentioned transport gas may contain a gas selected from nitrogen (N 2 ) and at least one of argon (Ar).

[0033] In the above-mentioned method for preparing lithium sulfide, lithium sulfide can be prepared by reacting lithium sulfate with carbon monoxide by the reaction represented by the following reaction formula 1) or 2).

[0034] Li 2 SO 4 +4CO→Li 2 S+4CO 2 -------1)

[0035] Li 2 SO 4 +2CO+2H 2 →Li 2 S+2CO 2 +2H 2 O-------2)

[0036] In the above-mentioned method for preparing lithium sulfide, since lithium sulfate or lithium sulfate hydrate is used as a lithium source, the preparation cost can be reduced. In addition, in the above-mentioned method for preparing lithium sulfide, since carbon is not used, no carbon will remain in the prepared lithium sulfide powder, thereby improving the purity of the synthesized lithium sulfide powder. In addition, in the above-mentioned method for preparing lithium sulfide, since lithium sulfate that can be crushed into a smaller size compared to other lithium sources is used, the size of the prepared lithium sulfide powder can be reduced. In addition, in the above-mentioned method for preparing lithium sulfide, since lithium sulfate crushed into a small size is used, the reactivity with gas increases with the increase in surface area, thereby increasing the crystallinity of the lithium sulfide powder. In addition, in the above-mentioned method for preparing lithium sulfide, since the lithium sulfide powder is prepared as a micropowder, the reactivity of the lithium sulfate powder with other powders during the solid electrolyte synthesis process can be improved.

[0037] The lithium sulfate crushing step S10 is a step of crushing the lithium sulfate powder to a specified size. The lithium sulfate powder can be a coarser powder of various sizes and used as a raw material. For example, the lithium sulfate powder can be a lithium sulfate powder with an average particle size of about 200 μm. In order to make the lithium sulfate powder have certain characteristics, it is necessary to use a powder with a size within a specified range. Therefore, in the lithium sulfate crushing step S10, the lithium sulfate powder can be crushed to a powder with a specified size. Preferably, the lithium sulfate powder can be crushed to a powder with a diameter of 0.01 to 10.0 μm. In addition, the lithium sulfate powder can be crushed to a powder with an average particle size of 0.1 to 1.0 μm. The lithium sulfate crushing step S10 can be performed using a crushing device such as a ball mill.

[0038] The lithium sulfate preheating step S20 is a step of removing residual water in the lithium sulfate powder by preheating the lithium sulfate powder. When lithium sulfate hydrate is used as the lithium source, the lithium sulfate preheating step S20 can be optionally performed. The lithium sulfate hydrate powder can be Li 2 SO 4 ·nH 2 When lithium sulfate powder is used as the lithium source, the lithium sulfate preheating step S20 may also be performed to remove the residual moisture in the lithium sulfate powder.

[0039] The lithium sulfate preheating step S20 may be performed by heating lithium sulfate hydrate powder or lithium sulfate powder at a preheating temperature of 100 to 400° C. The lithium sulfate preheating step S20 may be performed by a reaction represented by the following formula 3).

[0040] Li 2 SO 4 ·H 2 O→Li 2 SO 4 +H 2 O-------3)

[0041] The lithium sulfide synthesis step S30 is a step of synthesizing lithium sulfide powder by reacting lithium sulfate powder with a reaction gas. The lithium sulfide powder can be synthesized by reacting lithium sulfate powder with a reaction gas represented by the above formula 1) or formula 2).

[0042] The lithium sulfide synthesis step S30 can be performed under the conditions of a synthesis temperature of 650 to 840° C. and a synthesis time of 0.5 to 5 hours. In the lithium sulfide synthesis step S30, the synthesis temperature can be set to a temperature lower than the melting point of lithium sulfate. The lithium sulfide synthesis step (S30) can be performed at a synthesis temperature lower than 845° C., the melting point of lithium sulfate. In addition, the lithium sulfide synthesis step S30 can be performed by heating lithium sulfate powder while supplying a reaction gas. In the lithium sulfide synthesis step S30, lithium sulfide can be synthesized while separating oxygen from lithium sulfate powder.

[0043] The reaction gas may include carbon monoxide (CO). Furthermore, the reaction gas may include carbon monoxide (CO) and a transport gas. Furthermore, the reaction gas may include carbon monoxide (CO) and hydrogen (H 2 In addition, the reaction gas may include carbon monoxide (CO) and hydrogen (H 2 ) and a transport gas. The transport gas may include nitrogen (N 2 ) and at least one of argon (Ar). When the above-mentioned reaction gas is a mixed gas of carbon monoxide and a transport gas, based on the total volume of the reaction gas, 10 to 50 volume percent of carbon monoxide and 50 to 90 volume percent of the transport gas can be mixed. And, preferably, based on the total volume of the reaction gas, 25 to 40 volume percent of the above-mentioned carbon monoxide and 50 to 90 volume percent of the transport gas can be mixed. And, when the above-mentioned reaction gas is a mixed gas of carbon monoxide and hydrogen, based on the total volume of the reaction gas, 90 to 99.5 volume percent of carbon monoxide and 0.5 to 10 volume percent of hydrogen can be mixed. And, when the above-mentioned reaction gas is a mixed gas of carbon monoxide, hydrogen and a transport gas, based on the total volume of the reaction gas, 10 to 50 volume percent of carbon monoxide, 50 to 90 volume percent of hydrogen and a transport gas can be mixed. At this time, the above-mentioned hydrogen can be mixed with carbon monoxide in a state mixed with the transport gas. Furthermore, the transport gas and hydrogen may be mixed in a volume ratio of 90:10 to 99:1. Furthermore, the hydrogen may be mixed with carbon monoxide independently of the transport gas. At this time, the reaction gas may contain 10 to 50 volume percent carbon monoxide, 0.5 to 10 volume percent hydrogen, and 45 to 90 volume percent transport gas.

[0044] The carbon monoxide can react with the oxygen in lithium sulfate to generate carbon dioxide, thereby synthesizing lithium sulfide. The hydrogen can react with the oxygen in lithium sulfate to generate water vapor (H 2 O) to synthesize lithium sulfide. In addition, the above-mentioned transport gas can remove the carbon dioxide and water vapor (H 2O) is separated from lithium sulfide and transported to the outside. Therefore, the above transport gas can effectively synthesize high-purity lithium sulfide powder.

[0045] The lithium sulfide powder heat treatment step S40 is a step of increasing the crystallinity of the lithium sulfide powder by heat treating the synthesized lithium sulfide powder. The lithium sulfide powder heat treatment step can be performed while supplying the reaction gas used in the lithium sulfide synthesis step. The lithium sulfide powder heat treatment step can be performed optionally and can be performed when it is necessary to increase the crystallinity of the lithium sulfide powder synthesized in the lithium sulfide synthesis step.

[0046] The above-mentioned lithium sulfide powder heat treatment step can be carried out under the conditions of a heat treatment temperature of 850 to 930°C and a heat treatment time of 0.5 to 5 hours. In the above-mentioned lithium sulfide powder heat treatment step, the heat treatment temperature can be set to a temperature lower than the melting point of lithium sulfide. In addition, the above-mentioned heat treatment temperature can be higher than the synthesis temperature. For example, the above-mentioned heat treatment temperature can be determined within a temperature range higher than the melting point of lithium sulfate, 845°C, and lower than the melting point of lithium sulfide, 938°C. If the above-mentioned heat treatment temperature is too high, the lithium sulfide powder may be partially melted and the crystallinity may be reduced. In addition, if the above-mentioned heat treatment temperature is too low, the increase in the crystallinity of the lithium sulfide powder may be small.

[0047] Next, the method for preparing lithium sulfide of the present invention is described by means of more specific examples.

[0048] Figure 2 This is a SEM image of lithium sulfate powder used in a specific embodiment of the present invention before pulverization. Figure 3 This is a SEM image of the pulverized lithium sulfate powder used in a specific embodiment of the present invention. Figure 4 The XRD spectrum of lithium sulfide powder synthesized according to a specific embodiment of the present invention. Figure 5 This is the XRD pattern of commercially available lithium sulfide powder. Figure 6 For display use Figure 4 Curve diagram of the charge and discharge performance of half-cells prepared with synthesized lithium sulfide powder and commercially available lithium sulfide powder.

[0049] In this embodiment, lithium sulfate monohydrate (Li 2 SO 4 ·H 2 O) as a lithium source. Figure 2 As shown in FIG. 1 , it can be confirmed that the size of the lithium sulfate monohydrate is about 200 μm. The lithium sulfate monohydrate is crushed using a ball mill. Figure 3As shown, the lithium sulfate monohydrate is crushed into a powder with a diameter of about 0.1 μm. The crushed lithium sulfate powder is placed in an alumina boat and heated in a tube furnace. The lithium sulfate powder is synthesized under the conditions of a synthesis temperature of 780° C. and a synthesis time of 5 hours. In this embodiment, the lithium sulfate preheating step is not performed. In addition, in this embodiment, the lithium sulfide powder heat treatment step is not performed.

[0050] In this example, the crystallinity of synthesized lithium sulfide powder was evaluated, a solid electrolyte was prepared, and various properties were evaluated. In addition, in this example, commercially available lithium sulfide powder was purchased and evaluated together as a reference example for comparative evaluation.

[0051] Crystal phase evaluation

[0052] like Figure 4 As shown in the XRD spectrum, only Li 2 S peak was observed, and no peaks of unreacted phase or second phase were observed. Therefore, it was confirmed that the synthesized powder was crystalline lithium sulfide powder.

[0053] like Figure 5 As shown in the XRD spectrum of the reference example, the commercial lithium sulfide powder is also Figure 4 Peaks were shown at the same positions. Therefore, it was confirmed that the synthesized powder had the same phase as the commercially available lithium sulfide powder.

[0054] Preparation of solid electrolyte powder

[0055] 4.28 g of the above-synthesized lithium sulfide powder and 4.141 g of commercially available P 2 S 5 The powder was mixed with 1.58 g of commercially available LiCl powder, placed in a 250 cc zirconia container together with 300 g of zirconia balls with a diameter of 3 mm and 40 g of a solvent, sealed, and ground at 600 rpm for 20 hours using a planetary grinder to prepare a mixed powder. At this time, since the synthesized lithium sulfide powder is susceptible to moisture, the mixing and sealing process of the powder was carried out in a glove box replaced with sufficiently dry argon.

[0056] The ground mixed powder was dried in a vacuum oven at 110°C for 15 hours and then heat treated in a quartz tube sealed with argon at 360°C for 5 hours to prepare a solid electrolyte powder. The heat-treated solid electrolyte powder was analyzed by X-ray diffraction to confirm that Li 6 PS 5 Cl peak.

[0057] Measurement of ionic conductivity

[0058] The prepared solid electrolyte powder was uniaxially pressed in a glove box at a pressure of 560 MPa to prepare particles, and the ionic conductivity was measured using an AC impedance method. According to the evaluation results, the ionic conductivity of the solid electrolyte powder mixed with the lithium sulfide powder of the embodiment was measured to be 2.09 mS / cm. On the other hand, the ionic conductivity of the solid electrolyte powder mixed with the lithium sulfide powder of the reference example was measured to be 2.10 mS / cm. Therefore, it can be confirmed that the solid electrolyte powder of the embodiment has good ionic conductivity.

[0059] Preparation of half-cell and evaluation of charge and discharge performance

[0060] Solid electrolyte particles were prepared by uniaxially pressing 150 mg of the solid electrolyte powder of the embodiment in a mold with a diameter of 12 mm under a pressure of 450 MPa. The molding process was carried out in a glove box filled with argon. The positive electrode material was placed on the upper surface of the solid electrolyte particles and uniaxially pressed under a pressure of 550 MPa. The positive electrode material consisted of 57.6 parts by mass of lithium composite oxide (LiNi 0.8 Co 0.1 Mn 0.1 O 2 ) powder, 38.4 parts by mass of solid electrolyte powder whose particle size was adjusted to an average particle size of 1 μm, and 4 parts by mass of conductive carbon black material were mixed. Further, a half-cell was prepared by applying a pressure of 217 MPa to indium (In) powder as a negative electrode material. The prepared half-cell was charged and discharged at 30°C and 0.05C, and the charge and discharge range was 0.6 to 3.6V.

[0061] And, half-cells were prepared in the same manner using solid electrolyte powder mixed with commercially available lithium sulfide powder.

[0062] like Figure 6 As shown, it can be confirmed that the half-cells of Example (a) and Reference Example (b) exhibit comparable charge and discharge performance. Therefore, it can be confirmed that the lithium sulfide powder according to the example has the same characteristics as commercially available lithium sulfide powder when used for solid electrolyte powder.

[0063] The evaluation results of the lithium sulfide powders of Examples and Reference Examples are shown in Table 1 below.

[0064] Table 1

[0065]

[0066] It can be confirmed from the above specific embodiments that the method for preparing lithium sulfide powder according to the embodiment of the present invention can be applied to the preparation of lithium sulfide powder for solid electrolyte powder. In the method for preparing lithium sulfide powder according to the embodiment of the present invention, relatively cheap lithium sulfate is used as a lithium source, and therefore, lithium sulfide powder can be easily prepared at low cost.

[0067] The above description is only one embodiment of the method for preparing lithium sulfide for implementing the present invention. The present invention is not limited to the above embodiment. As required by the appended claims, it can be said that the technical spirit of the present invention exists within the scope of various modifications that can be made by those skilled in the art without departing from the main purpose of the present invention.

Claims

1. A method for preparing lithium sulfide, It is characterized in that include: The lithium sulfide synthesis step synthesizes lithium sulfide powder by reacting lithium sulfate powder with a reaction gas containing carbon monoxide.

2. The method for preparing lithium sulfide according to claim 1, It is characterized in that Before the lithium sulfide synthesis step, the method further includes: a lithium sulfate crushing step of crushing the lithium sulfate powder into a specified size.

3. The method for preparing lithium sulfide according to claim 2, It is characterized in that In the lithium sulfate pulverizing step, the lithium sulfate powder is pulverized into powder with a diameter of 0.01 to 10.0 μm.

4. The method for preparing lithium sulfide according to claim 2, It is characterized in that After the lithium sulfate crushing step, the method further includes: a lithium sulfate preheating step of removing residual moisture in the lithium sulfate powder by heating the lithium sulfate powder.

5. The method for preparing lithium sulfide according to claim 4, It is characterized in that In the lithium sulfate preheating step, the lithium sulfate hydrate is heated to 100-400°C.

6. The method for preparing lithium sulfide according to claim 1, It is characterized in that After the lithium sulfide synthesis step, the method further includes: a lithium sulfide powder heat treatment step, in which the crystallinity of the lithium sulfide powder is increased by heat treating the synthesized lithium sulfide powder.

7. The method for preparing lithium sulfide according to claim 6, It is characterized in that The lithium sulfide powder heat treatment step is performed at a heat treatment temperature higher than the synthesis temperature of the lithium sulfide synthesis step.

8. The method for preparing lithium sulfide according to claim 7, It is characterized in that The synthesis temperature of the lithium sulfide synthesis step is 650-840°C. The heat treatment temperature of the lithium sulfide powder heat treatment step is 850-930°C.

9. The method for preparing lithium sulfide according to claim 1, It is characterized in that The reaction gas further includes hydrogen and a transport gas.

10. The method for preparing lithium sulfide according to claim 9, It is characterized in that Based on the total volume of the reaction gas, the reaction gas includes 10-50 volume percent of the carbon monoxide, 50-90 volume percent of hydrogen and a transport gas, and the volume ratio of the transport gas to hydrogen is 90:10-99:

1.

11. The method for preparing lithium sulfide according to claim 9, It is characterized in that Based on the total volume of the reaction gas, the reaction gas includes 10-50 volume percent of the carbon monoxide, 0.5-10 volume percent of the hydrogen, and 45-90 volume percent of the transport gas.

12. The method for preparing lithium sulfide according to claim 1, It is characterized in that The reaction gas further includes hydrogen. Based on the total volume of the reaction gas, the reaction gas includes 90-99.5 volume percent of the carbon monoxide and 0.5-10 volume percent of the hydrogen.

13. The method for preparing lithium sulfide according to claim 1, It is characterized in that The above-mentioned lithium sulfide powder is used as a solid electrolyte for all-solid-state batteries.

Citation Information

Patent Citations

  • Preparation method of lithium sulfide

    CN113401878A

  • Method for producing lithium sulfide

    JP2013227180A

  • Preparation of lithium sulfide

    KR1020110132311A

Cited By

  • Electronic-grade lithium sulfide and preparation method and application thereof

    CN120483052A

  • Method for preparing high-purity lithium sulfide at high temperature and low pressure

    CN121651282A