Can

A can body with controlled thickness variations and dimensions addresses the breakage issue in thinner can bodies, enhancing productivity and resource efficiency.

JP7584590B2Active Publication Date: 2024-11-15ALTEMIRA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023127190
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-03
Publication Date
2024-11-15
Estimated Expiration
2039-09-19

AI Technical Summary

Technical Problem

Thinner can bodies and lids are demanded to save resources and energy, but the large thickness difference between the flange and wall portions leads to body breakage during DI press molding, reducing productivity.

Method used

A can body design with controlled thickness variations and specific dimensions, including a wall thickness of 0.270 mm to 0.285 mm, a flange thickness variation of ±10 μm, and a step difference of 60 μm or less, made from aluminum alloy, to prevent breakage during molding.

Benefits of technology

The design suppresses body breakage, maintains productivity by reducing interruptions, and conserves resources and energy while ensuring pressure resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584590000003
    Figure 0007584590000003
  • Figure 0007584590000004
    Figure 0007584590000004
  • Figure 0007584590000005
    Figure 0007584590000005
Patent Text Reader

Abstract

To provide a can body that does not cause breakage even when the can body is thinned.SOLUTION: A cylindrical can body 1 with a bottom centered around a can axis C includes a can bottom part 3 and a can trunk part 2, an outer diameter of the can trunk part 2 is within a range of 55 mm to 60 mm in a diameter, a can height from a can bottom 5b of the can bottom part 3 to an upper end opening 2a of the can trunk part 2 is within the range of 150 mm to 190 mm, a thickness of the can bottom part 3 on the can axis C is within the range of 0.270 mm to 0.285 mm, the can trunk part 2 has a flange part 2c on an upper opening 2a side that is thicker than a wall part 2b on a can bottom part 3 side, a variation in a wall thickness t1, which is obtained by measuring the thickness of the wall part 2b at eight points equally spaced in a circumferential direction, is ±7 μm, the variation in a flange thickness t2, which is obtained by measuring the thickness of the flange part 2c at eight points equally spaced in the circumferential direction, is ±10 μm, and a can body step difference t2-t1, which is a difference between an average value of the flange thickness t2 and the average value of the wall thickness t1, is 60 μm or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a can body having a bottomed, cylindrical can body centered on a can shaft, which has a can bottom and a cylindrical can body portion centered on the can shaft extending from the outer periphery of the can bottom toward the upper end in the can axial direction. [Background technology]

[0002] As an example of such a can body and finished can, Patent Document 1 describes a can body (beverage can) that includes a cylindrical can body with a bottom and a can lid that is wrapped around the opening of the can body and has a planned drinking spout, in which the can body includes a cylindrical can body portion that extends along the can axis, a can bottom portion that is provided on the lower end side of the can body in the axial direction, and a necking portion that is connected to the upper end side of the can body in the axial direction and that gradually reduces in diameter as it extends upward in the axial direction.

[0003] In the can body and finished can described in Patent Document 1, the outside diameter of the can body is in the range of 55 mm to 60 mm, the axial height from the upper end of the seaming panel of the can lid to the lower end of the necking part is in the range of 9 mm to 20 mm, and the difference between the outside diameter of the can body and the minimum outside diameter of the necking part is in the range of 6 mm to 8 mm. Also, the axial height of the can body is in the range of 120 mm to 190 mm.

[0004] Such a can body is manufactured by first punching a metal plate into a disk shape in a cupping press process using a cupping press and forming a shallow cup-shaped blank by drawing the disk. Next, this cup-shaped blank is redrawn and ironed with a punch in a DI press process using a DI press to elongate it in the can axial direction, thereby forming the above-mentioned cylindrical can body with a bottom.

[0005] Also, in such a can body, the outside diameter (diameter) of the can body is constant, while the bottom side of the can body is a wall part that is a thin part with a reduced thickness, and the part on the upper end opening side opposite to the can bottom is a flange part that is thicker than the wall part. For example, Patent Document 2 describes a can body to be manufactured into a bottle-shaped can, in which the original thickness of the metal plate is 0.345 mm to 0.390 mm, but the difference in thickness between the flange part (flange thickness) and the wall part (wall thickness) is 0.110 mm or less.

[0006] Here, in order to form such wall and flange portions with different thicknesses in a can body, as described above, a recess of a depth taking into consideration the difference in thickness (step) between the wall and flange portions may be formed at a position corresponding to the flange portion on the outer surface of a punch that performs ironing between a plurality of ironing dies in a DI press. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2016-005967 A [Patent Document 2] JP 2018-131261 A Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, there has been a strong demand for further thinning of the can body and the lid in order to conserve resources of the metal materials forming such can bodies and product cans and to conserve energy during material production. For example, in the case of aluminum alloy can bodies, there is a demand for producing the can body by forming a cup-shaped blank by drawing an aluminum alloy plate having a plate thickness of about 0.230 mm to 0.300 mm.

[0009] However, particularly in such a thin-walled can body, the can bottom side of the can body is a wall portion that is a thin-walled portion with a reduced thickness, as described above, and the portion on the upper opening side opposite the can bottom is a flange portion that is thicker than the wall portion. If there is a large difference in thickness between the flange thickness and the wall thickness, a phenomenon known as "body breakage" is likely to occur, in which the can body breaks during ironing between the punch and the ironing die in the DI press molding machine.

[0010] Once such a can break occurs, the broken can body remains inside the DI press molding machine, and the molding operation with the DI press molding machine must be temporarily stopped to remove the broken can body, which inevitably leads to a significant drop in the productivity of the can body and, ultimately, the productivity of finished cans.

[0011] The present invention has been made against this background, and has an object to provide a can body that is capable of suppressing the occurrence of barrel breaks even when the wall is thinned. [Means for solving the problem]

[0012] In order to solve the above problems and achieve the above object, the can body of the present invention has a bottomed cylindrical can main body centered on a can axis, the can main body includes a can bottom and a cylindrical can body centered on the can axis extending from the outer periphery of the can bottom to the upper end side in the can axial direction, the outer diameter of the can body is within a range of 55 mm to 60 mm, and a can height from the bottom of the can bottom to an upper opening of the can body is within a range of 150 mm to 190 mm, and the thickness of the can bottom on the can axis is 0.27 The can body has a flange portion on the upper end opening side that is thicker than the wall portion on the can bottom side, the wall thickness measured at eight equally spaced points around the wall has a variation of ±7 μm, the flange thickness measured at eight equally spaced points around the flange has a variation of ±10 μm, and a can body step, which is the difference between the average flange thickness and the average wall thickness, is 60 μm or less.

[0013] In the above-mentioned can body, the can main body is made of an aluminum alloy material, and the material strength is any one of 27k, 26k, and 25k.

[0014] In the can body, the wall portion is formed within a range of 132.0 mm from the can bottom to the upper end in the can axial direction, and the flange portion is formed within a range of 15.4 mm from the upper end opening to the lower end in the can axial direction, and a can body step portion serving as the can body step is formed within a range of 10.0 mm between the wall portion and the flange portion. Effect of the Invention

[0015] As described above, according to the present invention, even in the case of a thin-walled can body, it is possible to prevent the occurrence of body breaks due to the step between the flange portion and the wall portion, and it is possible to prevent the molding operation by the DI press molding machine from being interrupted due to body breaks, thereby improving the productivity of the can body. [Brief description of the drawings]

[0016] [Figure 1] 1 is a cross-sectional view taken along a can shaft, showing one embodiment of a can body of the present invention. FIG. [Diagram 2] 5 is an enlarged partial cross-sectional view showing the can bottom (part A in FIG. 1) of the product can of the embodiment shown in FIG. 1 and the embodiment shown in FIG. 4. [Diagram 3] FIG. 2 is a partial cross-sectional view showing an outline of the can body of the embodiment shown in FIG. 1 (however, for the purpose of explanation, the thickness of the flange portion is exaggerated). [Figure 4] 2 is a cross-sectional view taken along a can shaft, showing a state in which a shoulder portion, a neck portion, and a seam portion have been formed on the flange portion of the embodiment shown in FIG. 1. FIG. [Diagram 5] 5 is a side view showing an embodiment of a product can of the present invention in which a lid body is attached to a seam portion of the can body shown in FIG. 4. FIG. [Figure 6] 6 is an enlarged cross-sectional view of a portion B in FIG. 5 showing the seaming portion of the embodiment shown in FIG. 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Figures 1 to 3 show one embodiment of a can body of the present invention (however, Figure 2 is also common to one embodiment of a finished can of the present invention), and Figure 4 shows a state in which a shoulder portion, a neck portion, and a seam portion have been formed in the flange portion of the can body of this embodiment. Also, Figures 5 and 6 show one embodiment of a finished can of the present invention in which a lid body is attached by seaming to the seam portion of the can body shown in Figure 4.

[0018] The can body of this embodiment includes a cylindrical can body 1 with a bottom, which is made of a metal material such as aluminum or an aluminum alloy and is centered on a can axis C as shown in Fig. 1. That is, this can body 1 is configured by integrally forming a roughly cylindrical can body 2 centered on the can axis C and a roughly disk-shaped can bottom 3 that closes the opening at the lower end side of the can body 2 (the lower side in Figs. 1 to 3).

[0019] Of these, a dome section 4 having a concave curved surface shape is formed in the center of the can bottom 3 of the can body 1, which is concave toward the upper end side in the direction of the can axis C (upper side in Figs. 1 to 3), and an annular protrusion 5 is formed continuously in the circumferential direction around the can axis C on the outer periphery of the dome section 4, which protrudes toward the lower end side in the direction of the can axis C and then faces the upper end side in the direction of the can axis C as it moves toward the outer periphery in the radial direction relative to the can axis C. Here, in this embodiment, the thickness t0 of the dome section 4 of the can bottom 3 of the can body 1 on the can axis C is within a range of 0.270 mm to 0.285 mm.

[0020] Furthermore, the inner wall portion of the annular protrusion 5 protruding from the dome portion 4 to the lower end side in the direction of the can axis C forms a counter portion 5a that extends linearly and inclined toward the upper end side in the direction of the can axis C as it approaches the inner periphery of the can body 1 in a cross section along the can axis C, as shown in Fig. 2. In this embodiment, the counter angle θ that this counter portion 5a makes with a line L parallel to the can axis C in the cross section along the can axis C is within a range of 4° to 7°.

[0021] On the other hand, the can body 2 has an outer diameter D that is a constant size within a range of 55 mm to 60 mm. Also, the can height H1 from the can bottom 5b of the annular protrusion 5 of the can bottom 3 (the position where the annular protrusion 5 protrudes most toward the lower end side in the can axis C direction) to the upper end opening 2a of the can body 2 in the can axis C direction is a constant size within a range of 150 mm to 190 mm, and is 157.4 mm in this embodiment.

[0022] Furthermore, the can body 2 has a wall portion 2b on the can bottom 3 side and a flange portion 2c on the upper end opening 2a side, and a flange thickness t2, which is the radial thickness of the flange portion 2c relative to the can axis C, is thicker than a wall thickness t1, which is the radial thickness of the wall portion 2b relative to the can axis C, and a can body step portion 2d, which is a step in the can body 1, is formed between the wall portion 2b and the flange portion 2c.

[0023] Here, the wall portion 2b is formed within a range of 132.0 mm from the can bottom 5b to the upper end in the direction of the can axis C (106.0 mm from the boundary between the can body 2 and the can bottom 3 to the upper end in the direction of the can axis C), and the flange portion 2c is formed within a range of 15.4 mm from the upper end opening 2a to the lower end in the direction of the can axis C, and the can body step portion 2d is formed within a range of 10.0 mm between the wall portion 2b and the flange portion 2c.

[0024] The can body step t2-t1 between the flange thickness t2 of the flange portion 2c and the wall thickness t1 of the wall portion 2b is set to 60 μm or less. It is preferable that the can body step t2-t1 between the flange thickness t2 of the flange portion 2c and the wall thickness t1 of the wall portion 2b is set to 50 μm or more.

[0025] In this embodiment, the thickness is measured at eight points at equal intervals in the circumferential direction at a position at a height h1 79 mm from the can bottom 5b toward the upper end in the can axis C direction, and the average value is the wall thickness t1. At this time, the variation in the wall thickness t1 is preferably ±7 μm. In this embodiment, the thickness is measured at eight points at equal intervals in the circumferential direction at a position at a height h2 from the can bottom 5b, which is 7 mm from the upper end opening 2a of the can body 2 toward the lower end in the can axis C direction, and the average value is the flange thickness t2. At this time, the variation in the flange thickness t2 is preferably ±10 μm.

[0026] The upper opening 2a of the can body formed in this manner is trimmed as necessary to adjust it to the specified can height H1, and then, as shown in Fig. 4, the flange portion 2c is reduced in diameter in the necking process, thereby reducing the diameter toward the upper opening 2a to form a shoulder portion 6, and a cylindrical neck portion 7 is formed that is connected to the upper end of the shoulder portion 6 and is centered on the can axis C. Furthermore, the upper opening 2a from the neck portion 7 is expanded in diameter in a curved shape in a cross section along the can axis C toward the upper end in the direction of the can axis C, forming a seaming portion 8 that is connected to the upper end of the neck portion 7.

[0027] The can body thus formed is filled with contents such as a beverage, and then a lid body 9 equipped with a pull tab (not shown) is attached by rolling the seaming portion 8 as shown in Figures 5 and 6, thereby producing an embodiment of a finished can (filled can) of the present invention. That is, this embodiment of the finished can also has a finished can body 10 having a bottom and a cylindrical shape centered on the can axis C, and the above-mentioned disk-shaped lid body 9 centered on the can axis C that is rolled and attached to the upper opening of the finished can body 10.

[0028] This finished can body 10 also has a can bottom 3 similar to that of the can body 1 of the above-mentioned can body, and a generally cylindrical can body 2 centered on the can axis C, excluding a shoulder 6, a neck 7, a seam 8, and a lid 9, which extend from the outer periphery of the can bottom 3 toward the upper end in the direction of the can axis C. Here, the outer diameter of the can body 2 is within a range of 55 mm to 60 mm, like the can body 1, and the can height H2 of the finished can from the can bottom 5b of the can bottom 3 to the upper end 9a of the lid 9 is within a range of 150 mm to 190 mm, and is 155.6 mm in this embodiment, which is slightly lower than the can height H1 of the can body.

[0029] Here, wall thickness t3 of wall portion 2b in product can body 10 of this product can is approximately equal to wall thickness t1 of can body 1. Meanwhile, as a result of flange portion 2c being reduced in diameter in the above-mentioned necking process to form shoulder portion 6 and neck portion 7, flange thickness t4 of flange portion 2e in shoulder portion 6 and neck portion 7 of product can body 10 of this product can becomes thicker than flange thickness t2 of flange portion 2c in can body 1 of the can body.

[0030] In this product can body 10, the product can step t4-t3 between the flange thickness t4 of the flange portion 2e and the wall thickness t3 of the wall portion 2b is 74 μm or less. Note that, in this product can body 10, the product can step t4-t3 between the flange thickness t4 of the flange portion 2e and the wall thickness t3 of the wall portion 2b is preferably 60 μm or more.

[0031] Here, in the product can of this embodiment, the wall thickness t3 of the wall portion 2b is determined by measuring the thickness of the can body 2 at eight equally spaced points in the circumferential direction at a position at a height h1 79 mm from the can bottom 5b toward the upper end in the direction of the can axis C, as in the case of the can body, and averaging the measurements. It is preferable that the variation in the wall thickness t3 be within ±7 μm.

[0032] In the finished can of this embodiment, the flange thickness t4 of the flange portion 2e is measured at eight equally spaced points in the circumferential direction at a height h3 that is 4 mm from the upper end 9a of the lid 9 toward the lower end in the direction of the can axis C, as shown in Fig. 6. The position of this height h3 corresponds approximately to the position of the neck portion 7. It is preferable that the variation in the flange thickness t4 be within ±10 µm.

[0033] Furthermore, in this finished can, the shape and dimensions of the can bottom 3 are almost the same as those of the can body. Therefore, in the finished can of this embodiment, the thickness t0 of the dome portion 4 of the can bottom 3 on the can axis C is also within a range of 0.270 mm to 0.285 mm, and the counter angle θ that the counter portion 5a makes with a line L parallel to the can axis C in a cross section along the can axis C is also within a range of 4° to 7°.

[0034] In the can body and product can configured in this manner, the can body step t2-t1, which is the difference between the flange thickness t2 and the wall thickness t1 of the can body 1, is set to 60 μm or less, and the product can step t4-t3, which is the difference between the flange thickness t4 and the wall thickness t3 of the product can body 10, is set to 74 μm or less. In both cases, the flange thicknesses t2, t4 are thicker than the wall thicknesses t1, t3, but the can body step t2-t1 and the product can step t4-t3 are set small.

[0035] This makes it possible to reduce the step of the recess on the outer surface of the punch that performs ironing between multiple ironing dies in the DI press machine, and therefore prevents the can body 1 from getting caught on the step and breaking, even when forming the can body 1 from a thin metal plate, causing the can body 1 to break. This makes it possible to prevent the forming operation by the DI press machine from being interrupted by a break, thereby improving the productivity of can bodies and ultimately improving the productivity of finished cans.

[0036] Here, when the can body step t2-t1, which is the difference between the flange thickness t2 and the wall thickness t1 of the can body 2 of the can body 1 in the can body, exceeds 60 μm, trunk breakage is likely to occur in the can body 1. In addition, in the finished can, as described above, the flange thickness t4 becomes thicker as a result of the flange portion 2c of the can body 1 of the can body being necked and the flange portion 2c being reduced in diameter, so that if the finished can step t4-t3 is 74 μm or less, which is larger than the can body step t2-t1, trunk breakage can be prevented in the DI press process by the DI press molding machine for the can body.

[0037] Meanwhile, in such can bodies and finished cans, the punch and ironing die of the DI press molding machine form a dome section 4 having a concave curved surface in the center of the can bottom 3 of the can body 1 and the finished can body 10, which is recessed toward the upper end in the direction of the can axis C, as described above, and an annular protrusion 5 is formed on the outer periphery of this dome section 4, which protrudes toward the lower end in the direction of the can axis C and then faces the upper end in the direction of the can axis C as it moves toward the outer periphery in the radial direction relative to the can axis C. Here, the shape and dimensions of this can bottom section 3 are substantially unchanged between the can body 1 and the finished can body 10, as described above.

[0038] In the can body and product can of this embodiment, the inner wall portion of the annular convex portion 5 protruding from the dome portion 4 in the can bottom 3 to the lower end side in the direction of the can axis C is formed as a counter portion 5a that extends in a linear manner and inclines toward the upper end side in the direction of the can axis C as it approaches the inner periphery of the can body 1 or the product can body 10 in a cross section along the can axis C, and the counter angle θ that this counter portion 5a makes with a straight line L parallel to the can axis C in the above cross section is within the range of 4° to 7°.

[0039] Therefore, according to this embodiment, it is possible to avoid the occurrence of cracks in the can bottom 3 during the DI press process, which would impair the productivity of the can body and the product can, while ensuring the pressure resistance of the can bottom 3. In other words, if the counter angle θ is greater than 7°, the counter portion 5a will be inclined at a large angle with respect to the can axis C, which may impair the pressure resistance of the can bottom 3.

[0040] On the other hand, if the counter angle θ is smaller than 4°, the counter portion 5a will be nearly parallel to the can axis C, and the portion of the punch and ironing die of the DI press molding machine that forms the counter portion 5a will be cut vertically into the bottom surface portion of the cup-shaped material, which may cause cracks to form in the can bottom portion 3.

[0041] In this embodiment, the thickness t0 of the dome portion 4 of the can bottom 3 on the can axis C is within a range of 0.270 mm to 0.285 mm, and the thickness t0 of the dome portion 4 on the can axis C is approximately equal to the thickness of the metal sheet formed into the can body, so that the can body and the product can can be formed from a thinner metal sheet. Therefore, according to this embodiment, it is possible to conserve resources of the metal material forming the can body and the product can, and to conserve energy when producing such materials.

[0042] If the thickness t0 of the dome portion 4 on the can axis C is so thin as to be less than 0.270 mm, it may be impossible to ensure the necessary pressure resistance for the can body 1, and the pressure resistance of the product can body 10 may also be insufficient. On the other hand, if the thickness t0 of the dome portion 4 on the can axis C is so thick as to exceed 0.285 mm, the thickness of the metal plate formed into the can body and the product can may also become too thick, making it impossible to achieve sufficient resource and energy conservation. EXAMPLES

[0043] Next, the effects of the present invention will be demonstrated by giving examples of the present invention. In this example, one million cans each of seven types of can bodies 1 were formed by a DI press molding machine from three types of metal plates made of aluminum alloy material with a plate thickness of 0.285 mm and material strengths of 27k material, 26k material, and 25k material. The flange thickness t2 and wall thickness t1 were measured by the above-mentioned measurement method, and the can body step t2-t1 was calculated. These are shown in Table 1 as Examples 1 to 7 together with the counter angle. Note that the counter angle is different between Examples 1 to 3, Examples 4 to 6, and Example 7.

[0044] Next, shoulder 6 and neck 7 were formed by necking these can bodies, seaming portion 8 was formed, and lid 9 was attached by seaming to produce product can bodies 10 of product cans. Similarly, flange thickness t4 and wall thickness t3 were measured by the same measurement method as above, and product can step t4-t3 was calculated. Furthermore, drop pressure resistance and column strength of these product cans were calculated by simulation, and actual measurements were also taken. The results are also shown in Table 1.

[0045] As a comparative example for Examples 1 to 7, one million cans each for three types of can bodies were formed by a DI press molding machine from three types of metal plates made of aluminum alloy material with a plate thickness of 0.285 mm and varying material strength in the same manner as in Examples 1 to 6. Similarly, the flange thickness t2 and wall thickness t1 were measured, and the can body step t2-t1 was calculated.

[0046] Furthermore, in these comparative examples, a lid 9 was attached to the molded can body to produce a product can body 10, and the flange thickness t4 and wall thickness t3 were measured to calculate the product can step t4-t3. Also in these comparative examples, the drop pressure resistance and column strength of the product can were calculated by simulation and the actual values ​​were measured. The results are also shown in Table 1 as Comparative Examples 1 to 3.

[0047] The percentages in the pressure resistance column are based on the result of Comparative Example 1, which is taken as 100%. In the examples and comparative examples, the flange thickness t4 and wall thickness t3 of the finished can are greater than the flange thickness t2 and wall thickness t1 of the can body, and this includes the thickness of the paint.

[0048] [Table 1]

[0049] In this case, in the can bodies of Examples 1 to 7, only 5 out of 1 million cans were torn when molded using a DI press molding machine. In contrast, in the can body of Comparative Example 1, 50 out of 1 million cans were torn, and in the can body of Comparative Example 2, more than 500 out of 1 million cans were torn, and in the can body of Comparative Example 3, more than 500 out of 1 million cans were torn. In addition, in the product cans manufactured from the molded can bodies, the pressure resistance strength and column strength of Comparative Example 3 were smaller than those of Examples 1 to 7 and Comparative Examples 1 and 2. In Examples 1 to 6 and Comparative Examples 1 to 3, no cracks were generated in the can bottom 3.

[0050] Next, four types of can bodies having the same flange thickness t2, wall thickness t1, and can body step t2-t1 as in Examples 3, 6, and 7, but different counter angles, were molded from metal plates made of aluminum alloy material with a material strength of 25k and a thickness of 0.285 mm, as in Examples 3, 6, and 7, in the same numbers as in Examples 3, 6, and 7.

[0051] Furthermore, the can body thus formed was subjected to necking to form a shoulder 6 and a neck 7, a seaming portion 8 was formed, and a lid 9 was attached by seaming to produce a product can body 10. For this product can body 10 as well, the flange thickness t4 and wall thickness t3 were measured and the product can step t4-t3 was calculated, and the drop pressure resistance and column strength of the product can were calculated by simulation and the actual values ​​were measured. The results are shown in Table 2 as Comparative Examples 11 to 14.

[0052] [Table 2]

[0053] Of these Comparative Examples 11 to 14, in Comparative Examples 11 and 12, the counter angle was greater than 7° and the counter portion 5a was inclined at a large angle with respect to the can axis C, so that the pressure resistance strength was small in the simulation. In Comparative Examples 13 and 14, the product cans manufactured from the molded can bodies were able to ensure pressure resistance strength and column strength, but because the counter angle was smaller than 4°, cracks occurred in the can bottom 3 in one can out of one million cans during molding of the can bodies by a DI press molding machine. A product can with a crack in the can bottom 3 is a defective product that is functionally defective, so even one can cannot be distributed on the market. [Explanation of symbols]

[0054] 1 can body 2 Can body 2a Upper end opening of can body 2 2b Can body and product can wall 2c Flange part of can body 2d Can body step part 2e Flange part of product can 3. Bottom of the can 4 Dome section 5 Annular protrusion 5a Counter section 5b Can bottom 6 Shoulder 7 Neck 8. Sealing section 9 Lid 9a Upper end of the lid 9 10 Product can body C Can holder D Outside diameter of can body 2 H1 Height of the can body H2 Product can height h1: A height of 79 mm from the can bottom 5b to the upper end of the can axis in the C direction in the can body and product can h2: A height of 150 mm from the can bottom 5b of the can body to the upper end in the direction of the can axis C h3: A height of 4 mm from the upper end 9a of the lid 9 to the lower end in the direction of the can axis C t0: Thickness of the can axis C at the dome portion 4 of the can bottom 3 t1 Wall thickness of the can body t2 Flange thickness in can body t3 Wall thickness of the product can t4 Flange thickness in product can L Straight line parallel to can axis C θ Counter angle

Claims

1. The can has a cylindrical body with a bottom, the can body being centered on the can axis. The can body includes a can bottom and a cylindrical can body extending from an outer periphery of the can bottom toward an upper end in the can axial direction and centered on the can axis, A can body, wherein the outer diameter of the can body is within a range of 55 mm to 60 mm in diameter, and the can height from the bottom of the can bottom to the upper end opening of the can body is within a range of 150 mm to 190 mm, The thickness of the can bottom on the can axis is within a range of 0.270 mm to 0.285 mm; The can body has a flange portion on the upper opening side that is thicker than a wall portion on the can bottom side, The wall thickness measured at eight equally spaced points in the circumferential direction of the wall portion has a variation of ±7 μm; The flange thickness measured at eight equally spaced points in the circumferential direction of the flange portion has a variation of ±10 μm. A can body characterized in that a can body step, which is a difference between the average flange thickness and the average wall thickness, is 60 μm or less.

2. 2. The can body according to claim 1, wherein the can body is made of an aluminum alloy material and has a material strength of 27K, 26K, or 25K.

3. the wall portion is formed within a range of 132.0 mm from the can bottom to an upper end in the can axial direction, the flange portion is formed within a range of 15.4 mm from the upper end opening toward a lower end in the can axial direction, 3. The can body according to claim 1, wherein a can body step portion serving as the can body step is formed within a range of 10.0 mm between the wall portion and the flange portion.

Citation Information

Patent Citations

  • Taiyohoshaenerugiikyushusochi

    JP1976002042A

  • Aluminum can

    JP1992087940A

  • Metallic can body and its manufacturing method

    JP2008132522A

  • Beverage can

    JP2016005967A

  • Bottle can

    JP2018104095A