Resin composition and optical film using same
A resin composition with cellulose resin, cinnamate ester copolymer, and antioxidant addresses the challenges of conventional optical compensation films by providing high stability and improved retardation and wavelength dispersion, suitable for liquid crystal displays and organic ELs.
Patent Information
- Application Number
- JP2019175041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-09-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-09-26
AI Technical Summary
Conventional optical compensation films made of cellulose resin and fumaric acid ester resin face challenges such as embrittlement, coloring, and difficulty in achieving desired retardation and wavelength dispersion characteristics, especially in high-temperature environments, and require multiple layers for achieving the desired three-dimensional refractive index.
A resin composition containing cellulose resin, a cinnamate ester copolymer, and an antioxidant with a molecular weight of 350 or more, which provides excellent retardation and wavelength dispersion characteristics, and enhances stability at high temperatures.
The resin composition achieves high stability, excellent retardation, and wavelength dispersion characteristics, allowing for thinner optical films with improved durability and reduced color shift, suitable for use in liquid crystal displays and organic ELs.
Smart Images

Figure 0007585604000001 
Figure 0007585604000002 
Figure 0007585604000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition and a film using the same, and more particularly to a resin composition suitable for optical films for liquid crystal displays and organic electroluminescence (EL) displays, which have excellent retardation characteristics, wavelength dispersion characteristics, and heat resistance, and an optical film using the same. [Background technology]
[0002] In recent years, the demand for display performance and durability in various displays has been increasing, and it has become an issue to improve response speed and compensate for a wider range of viewing angles, such as contrast and color balance when a displayed image is observed from an oblique direction. To solve these issues, display elements of the VA (Vertical Alignment) mode, OCB (Optical Compensated Bend) mode, and IPS (In-Plane Switching) mode have been developed, and optical compensation film materials with various retardation expression properties according to each liquid crystal mode are required.
[0003] Conventional optical compensation films include stretched films of cellulose resins, polycarbonates, cyclic polyolefins, etc. In particular, stretched films made of cellulose resins such as cellulose acylate are widely used as optical compensation films for liquid crystal displays because of their transparency, toughness, moisture permeability required for processing, and low wavelength dispersion.
[0004] However, optical compensation films made of cellulose-based resins have some problems. For example, cellulose-based resin films are processed into optical compensation films having retardation values suited to various displays by adjusting the stretching conditions, but the three-dimensional refractive index of the film obtained by uniaxial or biaxial stretching of the cellulose-based resin film is ny≧nx>nz. In order to manufacture an optical compensation film having a three-dimensional refractive index other than the above, for example, ny>nz>nx or ny=nz>nx, a special stretching method is required, such as bonding a heat-shrinkable film to one or both sides of the film, subjecting the laminate to a heat stretching treatment, and applying a shrinking force in the thickness direction of the polymer film, and it is also difficult to control the refractive index (retardation value) (for example, see Patent Documents 1 to 3). Here, nx represents the refractive index in the fast axis direction (the direction with the smallest refractive index) in the film plane, ny represents the refractive index in the slow axis direction (the direction with the largest refractive index) in the film plane, and nz represents the refractive index outside the film plane (thickness direction).
[0005] Cellulose-based resin films are generally manufactured by a solvent casting method, but because cellulose-based resin films formed by the casting method have an out-of-plane retardation (Rth) of about 40 nm in the film thickness direction, problems such as color shifts occur in IPS mode liquid crystal displays, etc. Here, the out-of-plane retardation (Rth) is the retardation value expressed by the following formula. Rth = [(nx + ny) / 2-nz] × d (In the formula, nx represents the refractive index in the fast axis direction in the film plane, ny represents the refractive index in the slow axis direction in the film plane, nz represents the refractive index outside the film plane, and d represents the film thickness.) Further, a retardation film (optical compensation film) made of a fumaric acid ester resin has been proposed (see, for example, Patent Document 4).
[0006] However, the three-dimensional refractive index of a stretched film made of a fumaric acid ester resin is nz>ny>nx, and in order to obtain an optical compensation film exhibiting the above three-dimensional refractive index, lamination with other optical compensation films, etc. is necessary.
[0007] In view of this, as an optical compensation film exhibiting the above three-dimensional refractive index, a resin composition and an optical compensation film using the same have been proposed (see, for example, Patent Documents 5 to 7). Although Patent Documents 5 to 7 have excellent performance as an optical compensation film, there is a demand for an optical compensation film that exhibits the target Re with a thinner film.
[0008] Here, optical compensation films are generally used as anti-reflection layers for reflective liquid crystal displays, touch panels, and organic EL displays, and in these applications, optical compensation films with larger retardation (hereinafter referred to as "reverse wavelength dispersion films") are required, particularly in the longer wavelength range. For example, when a reverse wavelength dispersion film is used as an optical compensation film for an organic EL circular polarizer, the phase difference is preferably about 1 / 4 of the measured wavelength λ, and the ratio Re(450) / Re(550) of the retardation at 450 nm to the retardation at 550 nm varies depending on the display configuration, but is generally preferably about 0.80 to 0.86. In addition, in consideration of the thinning of display devices, the reverse wavelength dispersion film used is also required to be thin. Various optical compensation films have been developed to meet the above-mentioned required characteristics.
[0009] As a retardation film (optical compensation film) that exhibits the above three-dimensional refractive index and is used as a reverse wavelength dispersion film, a retardation film containing a cellulose resin and a fumaric acid ester polymer has been proposed (see, for example, Patent Document 8 and Patent Document 9). However, the retardation films described in Patent Document 8 and Patent Document 9 have a problem in durability against high-temperature environments due to embrittlement and coloring caused by decomposition of ethyl cellulose, coloring of ester resins that exhibit negative birefringence and have many aromatic groups or polycyclic aromatic groups, and the like, and an optical compensation film with higher stability at high temperatures is required. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent No. 2818983 [Patent Document 2] Japanese Patent Application Publication No. 5-297223 [Patent Document 3] Japanese Patent Application Publication No. 5-323120 [Patent Document 4] JP 2008-64817 A [Patent Document 5] JP 2013-28741 A [Patent Document 6] JP 2014-125609 A [Patent Document 7] JP 2014-125610 A [Patent Document 8] JP 2015-157928 A [Patent Document 9] JP 2019-19303 A Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention has been made in consideration of the above problems, and its object is to provide an optical film that is made using a resin composition having excellent retardation properties and wavelength dispersion properties, and that has high stability at high temperatures. [Means for solving the problem]
[0012] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and found that a resin composition containing a specific antioxidant and an optical film using the same can solve the above problems, thereby completing the present invention.
[0013] That is, the present invention relates to a cellulose resin (A) represented by the following general formula (1) in an amount of 50% by weight or more and 98.99% by weight or less: A cinnamate ester copolymer (B) containing a cinnamate ester residue unit represented by the following general formula (2) and a residue unit represented by the following general formula (3) in an amount of 1% by weight or more and 49.99% by weight or less. The present invention relates to a resin composition containing 0.01% by weight or more and 5.0% by weight or less of an antioxidant (C) having a molecular weight of 350 or more.
[0014] [ka] (In the formula, R1, R2, and R3 each independently represent a hydrogen atom or a substituent having 1 to 12 carbon atoms.)
[0015] [ka] (In the formula, R4 represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. R5 to R9 represent a hydrogen atom, a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, a phenyl group, a thiol group, an amido group, an amino group, a hydroxyl group, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. Y represents a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, a thiol group, an amido group, or an ester group.)
[0016] [ka] (In the formula, R 10 represents a 5-membered or 6-membered heterocyclic residue containing one or more nitrogen or oxygen atoms as heteroatoms (the 5-membered and 6-membered heterocyclic residues may form a condensed ring structure with another ring structure).
[0017] The present invention will be described in detail below.
[0018] The resin composition of the present invention comprises 50% by weight or more and 98.99% by weight or less of a cellulose resin (A) represented by the general formula (1), A cinnamic acid ester copolymer (B) containing a cinnamic acid ester residue unit represented by the general formula (2) and a residue unit represented by the general formula (3) in an amount of 1% by weight or more and 49.99% by weight or less; The resin composition contains 0.01% by weight or more and 5.0% by weight or less of an antioxidant (C) having a molecular weight of 350 or more.
[0019] The cellulose resin (A) contained in the resin composition of the present invention is represented by the following general formula (1).
[0020] [ka] (In the formula, R1, R2, and R3 each independently represent a hydrogen atom or a substituent having 1 to 12 carbon atoms.)
[0021] Examples of the cellulose resin include cellulose and / or cellulose derivatives. Examples of the cellulose derivatives include cellulose ethers in which at least a portion of the hydroxyl groups in cellulose is etherified, and cellulose ether esters in which at least a portion of the hydroxyl groups in cellulose is esterified. The resin composition of the present invention may contain one or more of these cellulose resins.
[0022] In the present invention, the degree of substitution (hereinafter referred to as "DS") of the cellulose resin is preferably 1.5 to 2.95, more preferably 1.8 to 2.8. This makes the resin composition of the present invention more excellent in terms of its solubility, compatibility, and stretching processability. Here, DS can be defined as the ratio of hydroxyl groups of cellulose in a cellulose derivative, and DS=3 when 100% is substituted. The method for measuring DS is as described in the 17th revised Japanese Pharmacopoeia, and can be calculated from the gas chromatography peak area after the elimination of the substituents after the reaction of cellulose to a derivative. When there are two or more types of substituents, the substitution degrees are expressed separately for each type. When ethyl cellulose is used, DS is the substitution degree of the ethyl group.
[0023] Cellulose resin has excellent mechanical properties and excellent moldability during film formation. It is therefore recommended that the number average molecular weight (Mn) calculated based on standard polystyrene standards obtained from the elution curve measured by gel permeation chromatography (GPC) be 1×10 3 ~1×10 6 Preferably, 5×10 3 ~2×10 5 It is even more preferable that:
[0024] The cellulose resin is preferably a cellulose ether, which provides better compatibility with the cinnamic acid ester copolymer (B), and also provides the resulting composition with a larger in-plane retardation Re and excellent stretchability.
[0025] Cellulose ether is a polymer in which β-glucose units are polymerized in a linear chain, and some or all of the hydroxyl groups at the 2nd, 3rd, and 6th positions of the glucose units are etherified.
[0026] In the cellulose ether of formula (1), R1 to R3 each independently represent a hydrogen atom or a substituent having 1 to 12 carbon atoms. From the viewpoint of solubility and compatibility, R1 to R3 are preferably a substituent having 1 to 12 carbon atoms. Examples of the substituent having 1 to 12 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a decanyl group, a dodecanyl group, an isobutyl group, a t-butyl group, a cyclohexyl group, a phenonyl group, a benzyl group, and a naphthyl group. Among these, from the viewpoint of solubility and compatibility, an alkyl group having 1 to 5 carbon atoms, that is, a methyl group, an ethyl group, a propyl group, a butyl group, and a pentyl group, are preferred.
[0027] The hydroxyl group of the cellulose ether used in the present invention may be substituted with one kind of ether group, or may be substituted with two or more kinds of ether groups, such as ethyl methyl cellulose, etc. Also, it may be substituted with an ester group in addition to the ether group.
[0028] Examples of cellulose ethers include alkyl celluloses such as methyl cellulose, ethyl cellulose, and propyl cellulose; hydroxyalkyl celluloses such as hydroxyethyl cellulose and hydroxypropyl cellulose; aralkyl celluloses such as benzyl cellulose and trityl cellulose; cyanoalkyl celluloses such as cyanoethyl cellulose; carboxyalkyl celluloses such as carboxymethyl cellulose and carboxyethyl cellulose; carboxyalkyl alkyl celluloses such as carboxymethyl methyl cellulose and carboxymethyl ethyl cellulose; and aminoalkyl celluloses such as aminoethyl cellulose. The cellulose ether is preferably at least one of the group consisting of methyl cellulose, ethyl cellulose, and propyl cellulose. This provides better compatibility with the cinnamic acid ester copolymer.
[0029] Cellulose ethers are generally synthesized by alkaline decomposition of cellulose pulp obtained from wood or cotton, and etherification of the alkaline decomposed cellulose pulp. Examples of the alkali that can be used include hydroxides of alkali metals such as lithium, potassium, and sodium, and ammonia. The alkali is generally used as an aqueous solution. The alkaline decomposed cellulose pulp is then etherified by contacting it with an etherification agent. Examples of the etherification agent include alkyl halides such as methyl chloride and ethyl chloride; aralkyl halides such as benzyl chloride and trityl chloride; halocarboxylic acids such as monochloroacetic acid and monochloropropionic acid; and alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide. A desired etherification agent may be used depending on the type of the desired cellulose derivative, and the etherification agents may be used alone or in combination of two or more.
[0030] For example, when etherifying a cellulose resin, a method in which an etherification reaction is carried out with a chloride or the like after alkali treatment can be exemplified.
[0031] If necessary, after the etherification, the copolymer may be subjected to a depolymerization treatment with hydrogen chloride, hydrogen bromide, hydrochloric acid, sulfuric acid, or the like in order to adjust the viscosity.
[0032] The resin composition of the present invention contains a cinnamate ester copolymer (B) containing a cinnamate ester residue unit represented by the following general formula (2) and a residue unit represented by the following general formula (3).
[0033] [ka] (In the formula, R4 represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. R5 to R9 represent a hydrogen atom, a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, a phenyl group, a thiol group, an amido group, an amino group, a hydroxyl group, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. Y represents a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, or a thiol group.)
[0034] [ka] (In the formula, R 10 represents a 5-membered or 6-membered heterocyclic residue containing one or more nitrogen or oxygen atoms as heteroatoms (the 5-membered and 6-membered heterocyclic residues may form a condensed ring structure with another ring structure).
[0035] The cinnamate ester copolymer (B) exhibits negative birefringence, which is due to the inclusion of the residue units represented by the general formula (2) and the general formula (3).
[0036] Here, the positive and negative birefringence are defined as follows. Negative birefringence is when the stretching direction is the fast axis direction, and positive birefringence is when the direction perpendicular to the stretching direction is the fast axis direction. In other words, a resin that exhibits positive birefringence when uniaxially stretched has a small refractive index in the direction perpendicular to the stretching axis (fast axis: perpendicular to the stretching direction), and a resin that exhibits negative birefringence when uniaxially stretched has a small refractive index in the direction of the stretching axis (fast axis: stretching direction). The high expression of negative birefringence in the cinnamate ester copolymer (B) allows the optical compensation film to be made thinner.
[0037] R4 in the general formula (2) represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. Examples of the alkyl group having 1 to 12 carbon atoms include a methyl group, an ethyl group, an isopropyl group, an n-propyl group, an n-butyl group, an s-butyl group, a t-butyl group, and an ethylhexyl group. R5 to R9 in general formula (2) represent a hydrogen atom, a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, a phenyl group, a thiol group, an amino group, a hydroxyl group, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. Y in the general formula (2) represents a nitro group, a bromo group, an iodo group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, or a thiol group.
[0038] Specific examples of the residue unit represented by the general formula (2) include α-cyano-hydroxycinnamic acid ester residue units such as α-cyano-4-hydroxycinnamic acid methyl residue unit, α-cyano-2-hydroxycinnamic acid ethyl residue unit, α-cyano-3-hydroxycinnamic acid ethyl residue unit, α-cyano-4-hydroxycinnamic acid ethyl residue unit, and α-cyano-2,4-dihydroxycinnamic acid methyl residue unit; α-cyano-4-carboxycinnamic acid ester residue units such as α-cyano-4-carboxycinnamic acid methyl residue unit, α-cyano-4-carboxycinnamic acid ethyl residue unit, α-cyano-2,3-dicarboxycinnamic acid methyl residue unit, and α-cyano-2,3-dicarboxycinnamic acid ethyl residue unit; α-cyano-2-carboxy-3-hydroxycinnamic acid methyl residue unit, and α-cyano-2-carboxy-3-hydroxycinnamic acid ethyl residue unit; acid ester residue unit; hydroxybenzylidene malonate diester residue unit such as dimethyl hydroxybenzylidene malonate residue unit, diethyl hydroxybenzylidene malonate residue unit, di-n-propyl hydroxybenzylidene malonate residue unit, diisopropyl hydroxybenzylidene malonate residue unit; carboxybenzylidene malonate diester residue unit such as dimethyl carboxybenzylidene malonate residue unit, diethyl carboxybenzylidene malonate residue unit, di-n-propyl carboxybenzylidene malonate residue unit, diisopropyl carboxybenzylidene malonate residue unit; and more preferably α-cyano-hydroxycinnamic acid ester residue unit; α-cyano-carboxycinnamic acid ester residue unit; carboxybenzal malononitrile residue unit, hydroxybenzylidene malonate diester residue unit, carboxybenzylidene malonate diester residue unit.
[0039] In the cinnamic acid ester copolymer (B), the residue unit represented by the general formula (2) may contain one type of the residue units exemplified above, or may contain two or more types.
[0040] R in general formula (3) 10represents a 5-membered or 6-membered heterocyclic residue containing one or more nitrogen or oxygen atoms as heteroatoms (the 5-membered and 6-membered heterocyclic residues may form a condensed ring structure with another ring structure).
[0041] Specific examples of the residue unit represented by general formula (3) include 1-vinylpyrrole residue unit, 2-vinylpyrrole residue unit, 1-vinylindole residue unit, 9-vinylcarbazole residue unit, 2-vinylquinoline residue unit, 4-vinylquinoline residue unit, N-vinylphthalimide residue unit, N-vinylsuccinimide residue unit, 2-vinylfuran residue unit, 2-vinylbenzofuran residue unit, styrene residue unit, and 2-vinylnaphthalene residue unit, and more preferably 9-vinylcarbazole residue unit and N-vinylphthalimide residue unit.
[0042] In the cinnamate ester copolymer (B), the monomer component relating to the cinnamate ester residue unit of the general formula (2) preferably accounts for 21 mol % to 50 mol % relative to 100 mol % of the total monomer components.
[0043] The cinnamic acid ester copolymer (B) preferably has a residue unit represented by the following formula (4) in addition to the general formulas (2) and (3).
[0044] [ka] (where R 11 , R 12 each independently represents a hydrogen atom, a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms.
[0045] R in the residue unit represented by formula (4) 11 , R 12 each independently represents a hydrogen atom, a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms.
[0046] R 11 , R 12 Examples of the linear alkyl group having 1 to 12 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, and an n-hexyl group. R 11 , R 12 Examples of the branched alkyl group having 1 to 12 carbon atoms include an isopropyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. R 11 , R 12 Examples of the cyclic alkyl group having 3 to 6 carbon atoms include a cyclopropyl group, a cyclobutyl group, and a cyclohexyl group.
[0047] R in general formula (4) 11 , R 12 As the alkyl group, a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a sec-pentyl group, a 3-pentyl group, a neopentyl group, a hexyl group, an isohexyl group, and a neohexyl group are preferred, since they provide a good ratio Re(450) / Re(550), of the in-plane retardation (Re) at a light wavelength of 450 nm to the in-plane retardation (Re) at a light wavelength of 550 nm, and a hydrogen atom, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a isobutyl group, a sec-butyl group, and an isobutyl group are more preferred.
[0048] The residue unit represented by the general formula (4) is preferably an acrylic resin residue unit. Specific examples of the acrylic resin residue unit represented by the general formula (4) include an acrylic acid residue unit, a methacrylic acid residue unit, a 2-ethyl acrylic acid residue unit, a 2-propyl acrylic acid residue unit, a 2-isopropyl acrylic acid residue unit, a 2-pentyl acrylic acid residue unit, a 2-hexyl acrylic acid residue unit, a methyl acrylate residue unit, an ethyl acrylate residue unit, an n-propyl acrylate residue unit, an isopropyl acrylate residue unit, an n-butyl acrylate residue unit, an isobutyl acrylate residue unit, a sec-butyl acrylate residue unit, an n-pentyl acrylate residue unit, an isopentyl acrylate residue unit, a sec-pentyl acrylate residue unit, a 3-pentyl acrylate residue unit, a neopentyl acrylate residue unit, an n-hexyl acrylate residue unit, an isohexyl acrylate residue unit, a neohexyl acrylate residue unit, a methyl methacrylate residue unit, Examples of the methacrylate residue unit include ethyl methacrylate residue unit, n-propyl methacrylate residue unit, isopropyl methacrylate residue unit, n-butyl methacrylate residue unit, isobutyl methacrylate residue unit, sec-butyl methacrylate residue unit, n-pentyl methacrylate residue unit, isopentyl methacrylate residue unit, sec-pentyl methacrylate residue unit, 3-pentyl methacrylate residue unit, neopentyl methacrylate residue unit, n-hexyl methacrylate residue unit, isohexyl methacrylate residue unit, neohexyl methacrylate residue unit, methyl 2-ethylacrylate residue unit, ethyl 2-ethylacrylate residue unit, n-propyl 2-ethylacrylate residue unit, isopropyl 2-ethylacrylate residue unit, n-butyl 2-ethylacrylate residue unit, isobutyl 2-ethylacrylate residue unit, and sec-butyl 2-ethylacrylate residue unit.
[0049] Among these, since the ratio Re(450) / Re(550), which is the in-plane retardation (Re) at a light wavelength of 450 nm and the in-plane retardation (Re) at a light wavelength of 550 nm, is good, methyl acrylate residue unit, ethyl acrylate residue unit, n-propyl acrylate residue unit, isopropyl acrylate residue unit, n-butyl acrylate residue unit, isobutyl acrylate residue unit, sec-butyl acrylate residue unit, methyl methacrylate residue unit, ethyl methacrylate residue unit, n-propyl methacrylate residue unit, isopropyl methacrylate residue unit, n-butyl methacrylate residue unit, methacrylate isobutyl methacrylate residue unit, sec-butyl methacrylate residue unit, methyl methacrylate residue unit, ethyl methacrylate residue unit, n-propyl methacrylate residue unit, isopropyl methacrylate residue unit, n-butyl methacrylate residue unit, isobutyl methacrylate residue unit, and sec-butyl methacrylate residue unit are preferred, and methyl methacrylate residue unit, ethyl methacrylate residue unit, n-propyl methacrylate residue unit, isopropyl methacrylate residue unit, n-butyl methacrylate residue unit, isobutyl methacrylate residue unit, and sec-butyl methacrylate residue unit are more preferred.
[0050] The cinnamate ester copolymer (B) preferably contains a cinnamate ester residue unit represented by general formula (2), a residue unit represented by general formula (3) and a residue unit represented by general formula (4). The cinnamic acid ester copolymer (B) exhibits good compatibility and is more suitable for facilitating the formation of a composite with a different polymer. For this reason, the following copolymers are available: α-cyano-2-hydroxycinnamic acid ester-styrene-acrylic acid ester copolymer, α-cyano-2-hydroxycinnamic acid ester-2-vinylnaphthalene-acrylic acid ester copolymer, α-cyano-2-hydroxycinnamic acid ester-1-vinylindole-acrylic acid ester copolymer, α-cyano-2-hydroxycinnamic acid ester-9-vinylcarbazole-acrylic acid ester copolymer, α-cyano-3-hydroxycinnamic acid ester-styrene-acrylic acid ester copolymer, α-cyano-3-hydroxycinnamic acid ester-2-vinylnaphthalene-acrylic acid ester copolymer, α-cyano-3-hydroxycinnamic acid ester-1-vinylindole-acrylic acid ester copolymer, α-cyano-3-hydroxycinnamic acid ester-9-vinylcarbazole-acrylic acid ester copolymer, 4-hydroxy-α-cyanocinnamic acid acid ester-styrene-acrylate copolymer, α-cyano-4-hydroxycinnamate-2-vinylnaphthalene-acrylate copolymer, α-cyano-4-hydroxycinnamate-1-vinylindole-acrylate copolymer, α-cyano-4-hydroxycinnamate-9-vinylcarbazole-acrylate copolymer, 2-hydroxy-α-cyanocinnamate-styrene-methacrylate copolymer, 2-hydroxy-α-cyanocinnamate-2-vinylnaphthalene-methacrylate copolymer, α-cyano-2-hydroxycinnamate-1-vinylindole-methacrylate copolymer, α-cyano-2-hydroxycinnamate-9-vinylcarbazole-methacrylate copolymer, α-cyano-3-hydroxycinnamate-styrene-methacrylate copolymer, α-cyano-3-hydroxycinnamate-2-vinylnaphthalene-methacrylate copolymer,Preferred are α-cyano-3-hydroxycinnamic acid ester-1-vinyl indole-methacrylic acid ester copolymer, α-cyano-3-hydroxycinnamic acid ester-9-vinyl carbazole-methacrylic acid ester copolymer, α-cyano-4-hydroxycinnamic acid ester-styrene-methacrylic acid ester copolymer, α-cyano-4-hydroxycinnamic acid ester-2-vinyl naphthalene-methacrylic acid ester copolymer, α-cyano-4-hydroxycinnamic acid ester-1-vinyl indole-methacrylic acid ester copolymer, and α-cyano-4-hydroxycinnamic acid ester-9-vinyl carbazole-methacrylic acid ester copolymer.
[0051] The cinnamate ester copolymer (B) is characterized by containing a residue unit represented by general formula (2), a residue unit represented by general formula (3), and a residue unit represented by general formula (4), and thereby exhibiting a high retardation even in a thinner film.
[0052] In the cinnamate ester copolymer (B), the monomer component related to the cinnamate ester residue unit of the general formula (2) preferably accounts for 21 mol% to 50 mol% based on 100 mol% of all monomer components.The residue unit represented by the general formula (3) preferably accounts for 21 mol% to 65 mol% based on 100 mol% of all monomer components.
[0053] When the cinnamate ester copolymer (B) contains residue units of the formula (2) and the formula (3), the monomer component according to the formula (2) is preferably contained in an amount of 21 mol% or more and 70 mol% or less, and more preferably 35 mol% or more and 60 mol% or less, relative to the total of the formulas (2) and (3) (100 mol%).
[0054] When the cinnamic acid ester copolymer (B) contains residue units of the formula (2), the formula (3), and the formula (4), the content of each residue unit component is Formula (2) 21 mol% or more and 49 mol% or less Formula (3) 35 mol% or more and 60 mol% or less Formula (4) 1 mol% or more and 30 mol% or less This provides superior retardation properties when the resin composition of the present invention is used as a film.
[0055] Here, the composition ratio of the copolymer (B) is 1 It can be measured by H-NMR.
[0056] The cinnamic acid ester copolymer (B) may contain a monomer residue unit other than those of the general formulae (2) to (4). Examples of such monomer residue units include one or more of styrene residues such as styrene residues and α-methylstyrene residues, acrylic acid residues, acrylic acid ester residues, methacrylic acid residues, methacrylic acid ester residues, vinyl ester residues such as vinyl acetate residues and vinyl propionate residues, vinyl ether residues such as methyl vinyl ether residues, ethyl vinyl ether residues, and butyl vinyl ether residues, N-substituted maleimide residues such as N-methylmaleimide residues, N-cyclohexylmaleimide residues, and N-phenylmaleimide residues, acrylonitrile residues, methacrylonitrile residues, cinnamic acid residues, fumaric acid ester residues, fumaric acid residues, and olefin residues such as ethylene residues and propylene residues.
[0057] The cinnamate ester copolymer (B) has excellent mechanical properties and excellent processability during film formation. Its number average molecular weight (Mn) calculated as standard polystyrene from the elution curve measured by gel permeation chromatography (GPC) is 1×10 3 ~5×10 6 Preferably, it is 5×10 3 ~3×10 5 It is even more preferable that:
[0058] The cinnamic acid ester copolymer (B) may be produced by any method as long as the copolymer can be obtained, and can be produced by radical polymerization.
[0059] As the radical polymerization method, for example, any of bulk polymerization method, solution polymerization method, suspension polymerization method, precipitation polymerization method, emulsion polymerization method, and the like can be used.
[0060] The antioxidant (C) contained in the resin composition of the present invention has a molecular weight of 350 or more. Preferably, the antioxidant has a molecular weight of 500 or more.
[0061] Here, whether the resin composition of the present invention contains an antioxidant can be determined, for example, by measuring the UV-visible absorption spectrum of the resin composition.
[0062] The antioxidant (C) functions as a radical scavenger, a peroxide decomposer, and a radical chain initiation inhibitor. These may be used alone or in a mixture of two or more. Examples of radical scavengers include phenol-based antioxidants, amine-based antioxidants, and hindered amine-based stabilizers. Examples of peroxide decomposers include phosphorus-based antioxidants and sulfur-based antioxidants. Examples of radical chain initiation inhibitors include metal deactivators, ultraviolet absorbers, and quenchers. Among these, phenol-based antioxidants and combinations of phenol-based antioxidants with phosphate esters are particularly preferred because they are less coloring and have a large antioxidant effect even in small amounts.
[0063] In the present invention, the phenol-based antioxidant is a compound having a phenol group and a molecular weight of 350 or more, and examples thereof include hindered phenol-based antioxidants, semi-hindered antioxidants, and less hindered antioxidants. Examples of the hindered phenol-based antioxidants include octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 1,3,5-tris[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, etc., which are commercially available. Semi-hindered antioxidants include bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, etc. Less hindered phenols include 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, etc. Among these, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) are preferred because they are less discoloring and have a large antioxidant effect even in small amounts.
[0064] In the present invention, the phosphorus-based antioxidant is not particularly limited as long as it is a compound having a phosphite group and a molecular weight of 350 or more, and examples thereof include tris(2,4-di-tert-butylphenyl)phosphite, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 2,2'-methylenebis(4,6-di-tert-butyl-phenyl)-2-ethylhexyl phosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphonite. Among these, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, tris(2,4-di-tert-butylphenyl) phosphite, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphonite, which are relatively less hydrolyzed, are preferred.
[0065] In the present invention, the hindered amine stabilizer is not particularly limited as long as it is a compound having a 2,2,6,6-tetramethylpiperidine structure and a molecular weight of 350 or more, and examples thereof include bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, 1-methyl 10-(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, dimethyl succinate·1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethyl-4-piperidine polymer, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate, [6-[(1,1,3,3-tetramethylbutoxy)phenyl] ... [(2,2,6,6-tetramethyl-4-piperidinyl)amino]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imino]-1,6-hexanediyl(2,2,6,6-tetramethyl-4-piperidinyl)imino] polymer, bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, 1,2,3,4-butanetetracarboxylic acid tetrakis(1,2,2,6,6-pentamethylpiperidin-4-yl), 1,2,3,4-butanetetracarboxylic acid tetrakis(2,2,6,6-tetramethylpiperidin-4-yl), and the like. Among the hindered amine stabilizers, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate and bis(1-undecanoxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate are preferred due to their low compatibility and coloring.
[0066] In the present invention, the sulfur-based antioxidant is not particularly limited as long as it is a compound having a thioether group and a molecular weight of 350 or more, and examples thereof include 2,2-bis[[3-(dodecylthio)propionic acid]-1,3-propanediyl, 3,3'-thiobispropionic acid, ditridecyl, and distearyl thiodipropionate.
[0067] In the present invention, the amine-based antioxidant is not particularly limited as long as it is a compound having an aromatic amine or hydroxyamine structure and a molecular weight of 350 or more, and examples of the amine-based antioxidant include bis(octadecyl)hydroxylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, and di(4-octylphenyl)amine.
[0068] In the present invention, the ultraviolet absorber is not particularly limited as long as it is a compound having a molecular weight of 350 or more and has a benzotriazole structure, a triazine structure, a benzophenone structure, a cyanoacrylate structure, or a salicylate structure, and examples thereof include 2,2'-methylenebis[6-(benzotriazol-2-yl)-4-tert-octylphenol], 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-(hexyloxy)phenol, 2-bis{[(2-cyano-3,3-diphenylacryloyl)oxy]methyl}propane-1,3-diyl-bis(2-cyano-3,3-diphenylacrylate), and the like.
[0069] In the present invention, the metal deactivator is not particularly limited as long as it is a compound having a molecular weight of 350 or more that chelates metal ions and renders them harmless, such as oxalic acid derivatives, salicylic acid derivatives, and hydrazide derivatives.
[0070] In the present invention, the quencher is not particularly limited as long as it is a compound having a chelate structure of Ni or the like and a molecular weight of 350 or more.
[0071] The resin composition of the present invention contains 50% by weight or more and 98.99% by weight or less of cellulose resin (A) represented by general formula (1), 1% by weight or more and 49.99% by weight or less of cinnamic acid ester resin copolymer (B) containing cinnamic acid ester residue unit represented by general formula (2) and residue unit represented by general formula (3), and 0.01% by weight or more and 5.0% by weight or less of antioxidant (C) having a molecular weight of 350 or more. If the content of (C) is less than 0.01% by weight, the antioxidant effect is small, and if it is more than 5.0% by weight, it causes bleeding and blooming, and the stability of the optical properties of the film is reduced. More preferably, the composition contains 50% by weight or more and 98.98% by weight or less of (A), 1% by weight or more and 49.98% by weight or less of (B), and 0.04% by weight or more and 1.0% by weight or less of antioxidant (C) having a molecular weight of 350 or more. The composition ratios herein are based on the total amount of (A) to (C) being 100% by weight.
[0072] The resin composition of the present invention may contain additives other than (A) to (C). In that case, the weight ratio of the additive may be expressed as a value relative to the total amount of (A) to (C) being 100% by weight or 100 parts by weight.
[0073] The cellulose resin (A), the cinnamic acid ester copolymer (B) and the antioxidant (C) can be blended by melt blending, solution blending or the like. The melt blending method is a method of producing the film by melting the resin and the antioxidant by heating and kneading them. The solution blending method is a method of dissolving the resin and the antioxidant in a solvent and blending them. The solvent used for solution blending may be any solvent as long as it can dissolve the resin, the antioxidant and the like. However, the boiling point of the solvent is preferably 200°C or less, more preferably 170°C or less, so that the solvent is less likely to remain in the film formation process.
[0074] Examples of the solvent include halogenated hydrocarbons such as chloroform, dichloromethane, carbon tetrachloride, dichloroethane, tetrachloroethane, trichloroethylene, tetrachloroethylene, chlorobenzene, and dichlorobenzene; phenols such as phenol and chlorophenol; aromatic hydrocarbons such as benzene, toluene, xylene, methoxybenzene, mesitylene, and dimethoxybenzene; acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexane, and the like. Examples of suitable solvents include ketone-based solvents such as xanone, cyclopentanone, 2-pyrrolidone, and N-methyl-2-pyrrolidone; ester-based solvents such as ethyl acetate and butyl acetate; alcohol-based solvents such as t-butyl alcohol, glycerin, ethylene glycol, triethylene glycol, ethylene glycol monomethyl ether, diethylene glycol dimethyl ether, propylene glycol, dipropylene glycol, and 2-methyl-2,4-pentanediol; amide-based solvents such as dimethylformamide and dimethylacetamide; nitrile-based solvents such as acetonitrile and butyronitrile; ether-based solvents such as diethyl ether, dibutyl ether, and tetrahydrofuran; and carbon disulfide, ethyl cellosolve, butyl cellosolve, and the like, used alone or in mixture.
[0075] Any method may be used as a method for producing a film using the resin composition of the present invention, but it is preferable to produce it by a solution casting method. Here, the solution casting method is a method in which a resin solution (generally called a dope) is cast onto a support substrate, and then heated to evaporate the solvent to obtain a film. The coating method is not particularly limited, and a normal method can be adopted. For example, the T-die method, the doctor blade method, the bar coater method, the slot die method, the lip coater method, the reverse gravure coat method, the microgravure method, the spin coat method, the brush coating method, the roll coat method, the flexographic printing method, and the like can be mentioned. In addition, the support substrate to be used is not particularly limited, and examples thereof include polymer substrates made of polyester, polycarbonate, polystyrene, polyethylene, polypropylene, polyvinyl chloride, polyvinylidene chloride, triacetyl cellulose, polyvinyl alcohol, polyimide, polyarylate, polysulfone, polyethersulfone, epoxy resin, and the like, glass substrates such as glass plates and quartz substrates, metal substrates such as aluminum, stainless steel, and ferrotype, and inorganic substrates such as ceramic substrates, and the like can be mentioned. The substrate is preferably a polymer substrate or a metal substrate.
[0076] The film of the present invention has excellent transparency and can be suitably used as an optical film.
[0077] The viscosity of the resin solution when manufacturing an optical film using the resin composition of the present invention can be adjusted by the molecular weight and concentration of each component and the type of solvent. The viscosity of the resin solution is not particularly limited, but in order to make the film coatable more easily, it is preferably 100 to 30,000 cps, more preferably 300 to 20,000 cps, and particularly preferably 500 to 15,000 cps.
[0078] The drying method in the drying step of the coating solution is not particularly limited, and a common heating means can be used, such as a hot air blower, a heating roll, or a far infrared heater.
[0079] In a method for producing a film using the resin composition of the present invention, the drying temperature may be in only one stage, or in order to maintain the appearance and shorten the drying time, multi-stage drying may be used in which the first stage is dried at a low temperature and the second and subsequent stages are dried at a high temperature.
[0080] In the present invention, the concentrations of the cellulose resin (A), the cinnamic acid ester copolymer (B) and the antioxidant (C) in the dope are not particularly limited as long as they can be dissolved and film-formed. The method of dissolving the cellulose resin (A), the cinnamic acid ester copolymer (B) and the antioxidant (C) may be carried out so that the desired concentration is reached at the dissolving stage, or the cellulose resin (A), the cinnamic acid ester copolymer (B) and the antioxidant (C) may be prepared in advance as a low-concentration solution and then adjusted to a desired high-concentration solution in a concentration process. Furthermore, a high-concentration resin solution of the cellulose resin (A) and the cinnamic acid ester copolymer (B) may be prepared in advance, and then an antioxidant and various additives may be added to prepare a resin solution of a desired low concentration.
[0081] The optical film of the present invention has excellent retardation characteristics and can be suitably used as an optical compensation film.
[0082] The method for producing the optical compensation film using the resin composition of the present invention is not particularly limited as a method for expressing retardation. As a method for stretching the optical compensation film, a longitudinal uniaxial stretching method by roll stretching, a transverse uniaxial stretching method or an oblique stretching method by tenter stretching, an unbalanced sequential biaxial stretching method or an unbalanced simultaneous biaxial stretching method by combining these methods, etc. can be used.
[0083] The thickness of the unstretched film before stretching is preferably 5 to 200 μm, more preferably 5 to 150 μm, and particularly preferably 5 to 100 μm, from the viewpoints of ease of stretching treatment and suitability for thin optical members.
[0084] Further, the thickness of the optical compensation film after stretching is preferably from 5 to 100 μm, more preferably from 5 to 60 μm, in order to reduce the thickness of the image display device.
[0085] The stretching temperature is not particularly limited, but is preferably 50 to 200° C., more preferably 100 to 200° C., in order to obtain good retardation characteristics. The stretching ratio is not particularly limited, but is preferably 1.05 to 4.0 times, more preferably 1.1 to 3.5 times, in order to obtain good retardation characteristics. The retardation can be controlled by the stretching temperature and stretching ratio.
[0086] In the optical compensation film using the resin composition of the present invention, the retardation can be adjusted by the content of cellulose resin (A), the DS of the cellulose resin (A) contained, the substitution degree distribution at the 2nd, 3rd, and 6th positions of the substituent, and the stretching ratio.
[0087] A film using the resin composition of the present invention is suitable for use as an optical compensation film, and the optical compensation film is characterized by having excellent retardation properties and excellent wavelength dispersion properties.
[0088] The retardation property of the optical compensation film using the resin composition of the present invention varies depending on the intended optical compensation film, and examples thereof include those in which the retardation (Re) represented by the following formula (5) is preferably 50 to 300 nm, more preferably 100 to 300 nm, and particularly preferably 120 to 280 nm, and the Nz coefficient represented by the following formula (6) is preferably 0.3 to 1.0, and more preferably 0.4 to 0.8. The retardation property is measured using an automatic birefringence meter (manufactured by Oji Scientific Instruments Co., Ltd., product name KOBRA-21ADH) at a measurement wavelength of 589 nm.
[0089] These films have retardation properties that are difficult to achieve with conventional optical compensation films made of cellulose-based resins. Re = (ny-nx) × d (5) Nz=(ny-nz) / (ny-nx) (6) Rth = [(nx + ny) / 2 - nz] × d (7) (In the formula, nx represents the refractive index in the advancing axis direction in the film plane, ny represents the refractive index in the retarding axis direction in the film plane, nz represents the refractive index outside the film plane, and d represents the film thickness.)
[0090] As the retardation characteristics of the optical film of the present invention, since it is suitable for a retardation film for a circular polarizing plate and a retardation film for an IPS liquid crystal, the retardation (Re) at a measurement wavelength of 589 nm is preferably 30 nm or more and 300 nm or less, more preferably 65 nm or more and 300 nm or less, and still more preferably 130 nm or more and 300 nm or less.
[0091] As the retardation characteristics of the optical film of the present invention, since it is suitable for a retardation film for a circular polarizing plate and a retardation film for an IPS liquid crystal, the Nz coefficient at a measurement wavelength of 589 nm is preferably 0.3 or more and 1.5 or less, and more preferably 0.4 or more and 1.1 or less.
[0092] As the wavelength dispersion characteristics of the optical film of the present invention, in order to suppress color shift, preferably 0.60 < Re(450) / Re(550) < 1.05, more preferably 0.70 < Re(450) / Re(550) < 1.02, and particularly preferably 0.75 < Re(450) / Re(550) < 1.00.
[0093] When the cellulose-based resin of the present invention is used alone, an optical film with low wavelength dispersion can be provided. A resin composition in which an ester-based resin showing negative birefringence with respect to the stretching direction is blended with this film can generally provide an optical film showing inverse wavelength dispersion characteristics.
[0094] Satisfying these retardation characteristics and wavelength dispersion characteristics simultaneously is generally difficult to achieve in an optical compensation film using a cellulose-based resin, but the optical compensation film according to the present invention satisfies these characteristics simultaneously.
[0095] From the viewpoints of handling the film and suitability for thinning optical components, the optical compensation film using the resin composition of the present invention preferably has a thickness of 5 to 200 μm, more preferably 10 to 100 μm, particularly preferably 20 to 80 μm, and most preferably 10 to 60 μm.
[0096] In order to avoid a change in color tone when used in an image display device, the optical compensation film using the resin composition of the present invention has a YI of preferably 1.7 or less, more preferably 1.5 or less, and even more preferably 1.0 or less when made into a film. Here, the YI is measured in accordance with JIS-K 7373 using a halogen lamp of C light source as a light source and with a field of view of 2°. The thickness of the film made of the resin composition was measured at 30 μm.
[0097] In order to avoid color tone changes in a screen display device in a high-temperature environment and to maintain the color tone, it is more preferable that the optical compensation film using the resin composition of the present invention has a YI of 1.5 or less after 500 hours in an 85° C. environment.
[0098] In order to prevent the light quantity of the image display device from decreasing, the optical compensation film using the resin composition of the present invention has a transmittance of preferably 85% or more, more preferably 90% or more when made into a film. The light transmittance here represents the total light transmittance, and is measured in accordance with JIS K 7361-1 (1997 edition) using a white light source at wavelengths of 380 nm to 780 nm. The thickness of the film made of the resin composition was measured at 30 μm.
[0099] The optical compensation film using the resin composition of the present invention preferably has a haze of 3.0% or less, more preferably 1.5% or less. By controlling the haze within the above range, a high-contrast image can be obtained when the film is incorporated into a display device as a retardation film. Here, the haze is measured using a white light source at wavelengths of 380 nm to 780 nm in accordance with JIS-K 7136 (2000 edition). The thickness of the film made of the resin composition was measured at 30 μm.
[0100] In order to avoid a decrease in the amount of light of a screen display device in a high-temperature environment and to maintain a high-contrast image, the optical compensation film using the resin composition of the present invention preferably has a haze of 3% or less after 500 hours in an 85°C environment and a transmittance of 85% or more, and more preferably 90%.
[0101] The optical compensation film using the resin composition of the present invention preferably has a change in yellowness index YI of less than 1.0 after high-temperature treatment for 500 hours in an environment at 85° C. Here, the change in yellowness index YI can be expressed as (YI after high-temperature treatment)−(YI before high-temperature treatment).
[0102] The optical compensation film using the resin composition of the present invention preferably has a haze change of less than 2.0% after high-temperature treatment for 500 hours in an environment of 85° C. Here, the haze change can be expressed as (haze after high-temperature treatment)−(haze before high-temperature treatment).
[0103] The optical compensation film using the resin composition of the present invention can be laminated with a film containing other resins as necessary. Examples of other resins include polyethersulfone, polyarylate, polyethylene terephthalate, polynaphthalene terephthalate, polycarbonate, cyclic polyolefin, maleimide resin, fluorine resin, polyimide, etc. In addition, it is also possible to laminate a liquid crystal layer, a hard coat layer, a gas barrier layer, and a layer with a controlled refractive index (low reflection layer).
[0104] The optical compensation film using the resin composition of the present invention is suitably used in a polarizing plate used for applications such as liquid crystal displays, organic EL displays, etc. The polarizing plate is also suitably used as an image display device. Effect of the Invention
[0105] The resin composition of the present invention and a film using the same have excellent retardation properties and wavelength dispersion, and therefore can be suitably used in polarizing plates, liquid crystal displays, organic EL displays, etc., and can exhibit excellent display performance and high stability under high temperature and high humidity conditions. EXAMPLES
[0106] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0107] The physical properties shown in the examples were measured by the following methods. <Measurement of phase difference characteristics> Fully automatic birefringence meter (Oji Scientific Instruments, product name KOBRA-21ADH) The retardation characteristics of the retardation film using light with a wavelength of 589 nm (Re and Nz coefficients) was measured. <Measurement of total light transmittance and haze> The total light transmittance and haze of the prepared films were measured using a haze meter (manufactured by Nippon Denshoku Industries, product name: NDH5000, light source: white LED (5V3W, wavelength range 380nm to 780nm, total light transmittance and haze values are the sum of this range)) in accordance with JIS K 7361-1 (1997 edition) for the total light transmittance and JIS-K 7136 (2000 edition) for the haze. <Yellowness Index (YI) Measurement> The yellowness index YI of the prepared film was measured in accordance with JIS-K 7373 using a spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., product name: SD-5000, light source: C light source halogen lamp (12V50W), field of view: 2°). <Heat resistance test> A gear oven (manufactured by Toyo Seiki Seisakusho, product name: STD60P) (replacement rate 3 times / min) was used to create a high-temperature environment of 85°C. The haze and Total light transmittance and Heat resistance was measured by examining the YI and molecular weight change. The change in molecular weight was measured by gel permeation chromatography (GPC) on the film before and after exposure to a high-temperature environment, and the molecular weight was calculated based on the standard polystyrene equivalent. weight average The difference in molecular weight was taken as the rate of change. weight average The molecular weight was determined by GPC measurement of the composition itself, rather than of the individual components contained in the film, and the obtained measurement data was used. <Phase difference and wavelength dispersion> The retardation and wavelength dispersion were measured for the stretched optical compensation film using a fully automatic birefringence meter (manufactured by Oji Scientific Instruments, product name KOBRA-21ADH, light source: halogen lamp (12V100W)) at a measurement wavelength of R450 / R550 at 550nm and 450nm was measured.
[0108] Synthesis Example 1 (Cinnamic acid ester copolymer (B-1) (9-vinylcarbazole / 4-Hydroxy- Synthesis of α-isobutyl cyanocinnamate / isobutyl acrylate Add 5.0 g (5.0 g) of 9-vinylcarbazole to a 50 mL glass ampoule. 0.026 moles ), 3.2g (0.013 mol) of isobutyl 4-hydroxy-α-cyanocinnamate, 1.7g (0.013 mol) of isobutyl acrylate, 0.093g (0.00022 mol) of polymerization initiator 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane and 24.6g of ethyl cellosolve were added, and the ampoule was repeatedly replaced with nitrogen and depressurized, and then sealed under reduced pressure. The ampoule was placed in a thermostatic chamber at 47°C and held for 24 hours to carry out radical polymerization. After the polymerization reaction was completed, the polymer was removed from the ampoule, 41g of tetrahydrofuran was added, and the polymer solution was dropped into 330g of a methanol / water mixed solvent (weight ratio 80 / 20) to precipitate, filtered, and the filtrate was washed five times with 45g of a methanol / water mixed solvent (weight ratio 90 / 10) and filtered. The resin thus obtained was vacuum-dried at 80°C for 10 hours to obtain 9.2 g of a cinnamate ester copolymer (B-1) exhibiting negative birefringence (yield: 94%). The number average molecular weight of the obtained B-1 was 77,000, and the ratio of the residue units was 50 mol% 9-vinylcarbazole residue units, 25 mol% 4-hydroxy-α-cyanocinnamate isobutyl residue units, and 25 mol% isobutyl acrylate residue units.
[0109] Synthesis Example 2 (Cinnamic acid ester copolymer (B-2) (Synthesis of 4-hydroxy-α-ethyl cyanocinnamate / 9-vinylcarbazole copolymer) A 50mL glass ampoule was charged with 5.0g of ethyl 4-hydroxy-α-cyanocinnamate, 4.4g of 9-vinylcarbazole, 0.17g of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane as a polymerization initiator, and 8.5g of tetrahydrofuran. After repeated nitrogen replacement and depressurization, the ampoule was sealed under reduced pressure. The ampoule was placed in a thermostatic chamber at 62°C and held for 48 hours to carry out radical polymerization. After the polymerization reaction was completed, the polymer was removed from the ampoule and dissolved in 25g of tetrahydrofuran. The polymer solution was dropped into 500mL of methanol to precipitate, and then vacuum dried at 60°C for 10 hours to obtain 7.7g of cinnamate ester copolymer (B-2) exhibiting negative birefringence (yield: 82%). The number average molecular weight of the obtained B-2 was 22,000, and the ratio of the residue units was 58 mol % of 9-vinylcarbazole residue units and 42 mol % of ethyl 4-hydroxy-α-cyanocinnamate residue units.
[0110] Example 1 As the cellulose resin (A), 31.15 g of ethyl cellulose (ETHOCEL standard 100 manufactured by Dow Chemical Company, number average molecular weight Mn = 58,000, weight average molecular weight Mw = 180,000, Mw / Mn = 3.2, total substitution degree DS = 2.51), 8.75 g of the cinnamic acid ester resin (B-1) obtained in Synthesis Example 1, and 0.10 g of a semi-hindered phenol-based antioxidant Irganox 245 (manufactured by BASF, compound name: bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], Fw: 587) were dissolved in a toluene / ethyl acetate = 8 / 2 (weight ratio) solution to prepare a 15 wt % resin solution. The solution was cast onto a polyethylene terephthalate film using a coater, and then dried in two stages at 40°C for 6 minutes and 155°C for 5 minutes, to obtain a film (resin composition) with a width of 150 mm and a thickness of 39 μm (cellulose resin: 77.87% by weight, cinnamic acid ester copolymer (B-1): 21.88% by weight, semi-hindered phenol-based antioxidant: 0.25% by weight). The obtained film was cut into a 50 mm square, and then uniaxially stretched 2.0 times at 155°C (thickness after stretching: 30 μm) to obtain an optical compensation film. The obtained film had a total light transmittance of 93%, a haze of 0.4%, and a YI of 0.5, and after a heat resistance test, the total light transmittance was 93%, the haze was 0.5%, and the YI was 0.9. The total light transmittance, haze, retardation characteristics, wavelength dispersion characteristics, and heat resistance of the obtained optical compensation film were measured. The results are shown in Table 1.
[0111] [Table 1]
[0112] The optical compensation film thus obtained had high total light transmittance, low haze and YI, and high heat resistance.
[0113] Example 2 31.15 g of the ethyl cellulose used in Example 1, 8.75 g of the cinnamic acid ester copolymer (B-2) exhibiting negative birefringence obtained in Synthesis Example 2, 0.05 g of a semi-hindered phenol-based antioxidant Irganox 245 (manufactured by BASF, Fw: 587), and Subphosphorus Two types of antioxidants, 0.05 g of acid ester-based antioxidant Adeka STAB PEP-36 (manufactured by ADEKA, compound name: 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, Fw: 633), were dissolved in a toluene / ethyl acetate = 8 / 2 (weight ratio) solution to obtain a 15 wt% resin solution. The solution was cast onto a polyethylene terephthalate film using a coater, and dried in two stages at 40°C for 6 minutes and then 155°C for 5 minutes, to obtain a film (resin composition) with a width of 150 mm and a thickness of 39 μm (cellulose-based resin : 77.88% by weight, cinnamic acid ester copolymer (B-2): 21.88% by weight, semi-hindered phenol-based antioxidant: 0.12% by weight, Subphosphorus Acid ester antioxidant: 0.12% by weight. The obtained film was cut into 50 mm squares and then uniaxially stretched 2.0 times at 157°C (thickness after stretching: 30 μm) to obtain an optical compensation film. The obtained film had a total light transmittance of 92%, a haze of 0.6%, and a YI of 0.5, and after a heat resistance test, the total light transmittance was 92%, the haze was 0.6%, and the YI was 0.9. The total light transmittance, haze, retardation characteristics, wavelength dispersion characteristics, and heat resistance of the obtained optical compensation film were measured. The results are shown in Table 1. The optical compensation film thus obtained had high total light transmittance, low haze and YI, and high heat resistance.
[0114] Example 3 31.10 g of the ethyl cellulose used in Example 1, 8.70 g of the cinnamic acid ester copolymer (B-1) used in Example 1, and 0.20 g of the semi-hindered phenol-based antioxidant Irganox245 (manufactured by BASF, Fw:587) were dissolved in a toluene / ethyl acetate = 8 / 2 (weight ratio) solution to obtain a 15 wt% resin solution. The solution was cast onto a polyethylene terephthalate film by a coater, and dried in two stages at a drying temperature of 40 ° C. for 6 minutes and then at 155 ° C. for 5 minutes, to obtain a film (resin composition) with a width of 150 mm and a thickness of 39 μm (cellulose resin: 77.75 wt%, cinnamic acid ester copolymer (B-1): 21.75 wt%, semi-hindered phenol-based antioxidant: 0.50 wt%). The obtained film was cut into a 50 mm square, and then uniaxially stretched 2.0 times at 152° C. (thickness after stretching: 30 μm) to obtain an optical compensation film. The obtained film had a total light transmittance of 93%, a haze of 0.4%, and a YI of 0.5, and after a heat resistance test, the total light transmittance was 93%, the haze was 0.5%, and the YI was 0.8. The total light transmittance, haze, retardation characteristics, wavelength dispersion characteristics, and heat resistance of the obtained optical compensation film were measured. The results are shown in Table 1. The optical compensation film thus obtained had high total light transmittance, low haze and YI, and high heat resistance.
[0115] Example 4 31.18g of the ethyl cellulose used in Example 1, 8.78g of the cinnamic acid ester copolymer (B-1) used in Example 1, and 0.04g of the semi-hindered phenol-based antioxidant Irganox245 (manufactured by BASF, Fw:587) were dissolved in a toluene / ethyl acetate = 8 / 2 (weight ratio) solution to obtain a 15 wt% resin solution. The solution was cast onto a polyethylene terephthalate film by a coater, and dried in two stages at a drying temperature of 40 ° C. for 6 minutes and then at 155 ° C. for 5 minutes, to obtain a film (resin composition) with a width of 150 mm and a thickness of 39 μm (cellulose resin: 77.95 wt%, cinnamic acid ester copolymer (B-1): 21.95 wt%, semi-hindered phenol-based antioxidant: 0.10 wt%). The obtained film was cut into a 50 mm square, and then uniaxially stretched 2.0 times at 155° C. (thickness after stretching: 30 μm) to obtain an optical compensation film. The obtained film had a total light transmittance of 93%, a haze of 0.4%, and a YI of 0.5, and after a heat resistance test, the total light transmittance was 93%, the haze was 0.5%, and the YI was 0.9. The total light transmittance, haze, retardation characteristics, wavelength dispersion characteristics, and heat resistance of the obtained optical compensation film were measured. The results are shown in Table 1. The optical compensation film thus obtained had high total light transmittance, low haze and YI, and high heat resistance.
[0116] Example 5 Ethyl cellulose used in Example 1 31.18 g and the cinnamic acid ester copolymer (B-1) used in Example 1 8.78 g and sulfur-based antioxidant Adeka STAB AO-412S (ADEKA, chemical name: bis[3-(dodecylthio)propionic acid]2,2-bis[[3-(dodecylthio)-1-oxopropyloxy]methyl]-1,3-propanediyl, Fw: 1162) 0.04g was dissolved in a toluene / ethyl acetate = 8 / 2 (weight ratio) solution to obtain a 15 wt% resin solution. The solution was cast onto a polyethylene terephthalate film by a coater, and dried in two stages at 40 ° C. for 5 minutes and then 155 ° C. for 6 minutes, to obtain a film (resin composition) with a width of 150 mm and a thickness of 39 μm (cellulose resin: 77.95 wt%, cinnamic acid ester copolymer (B-1): 21.95 wt%, sulfur-based antioxidant: 0.10 wt%). The obtained film was cut into 50 mm squares, and then uniaxially stretched 2.0 times at 155 ° C. (thickness after stretching: 30 μm) to obtain an optical compensation film. The obtained film had a total light transmittance of 93%, a haze of 0.4%, and a YI of 0.5, and after a heat resistance test, the total light transmittance was 93%, the haze was 0.5%, and the YI was 1.2. The total light transmittance, haze, retardation characteristics, wavelength dispersion characteristics, and heat resistance of the obtained optical compensation film were measured. The results are shown in Table 1. The optical compensation film thus obtained had high total light transmittance, low haze and YI, and high heat resistance.
[0117] Comparative Example 1 An optical compensation film was obtained under the same conditions as in Example 1, except that no antioxidant was used. The obtained film had a total light transmittance of 93%, a haze of 0.4%, and a YI of 0.5. After the heat resistance test, the total light transmittance was 93%, the haze was 0.4%, and the YI was 1.8. The results are shown in Table 2. The obtained optical compensation film had a high YI and low heat resistance.
[0118] [Table 2]
[0119] Comparative Example 2 An optical compensation film was obtained under the same conditions as in Example 1, except that the film contained 10% by weight of the semi-hindered phenol antioxidant Irganox245. The film obtained had a total light transmittance of 91%, a haze of 1.3%, and a YI of 0.6%, and after the heat resistance test, the total light transmittance was 89% and the haze was 3.5%. The results are shown in Table 2. The obtained optical compensation film had high haze and low heat resistance.
[0120] Comparative Example 3 An optical compensation film was obtained under the same conditions as in Example 1, except that a low molecular weight semi-hindered phenol-based antioxidant Sumilizer MDP-S (Sumitomo Chemical, chemical name: 2,2'-methylenebis(6-tert-butyl-p-cresol), Fw: 341) was used instead of the semi-hindered phenol-based antioxidant Irganox245 (BASF, Fw: 587). The obtained film had a total light transmittance of 92%, a haze of 0.5%, and a YI of 0.5, and after the heat resistance test, the total light transmittance was 92%, the haze was 0.8%, and the YI was 1.6. The results are shown in Table 2. The obtained optical compensation film had a high YI and low heat resistance.
Claims
1. A cellulose resin (A) having a cellulose residue unit represented by the following general formula (1) of 50% by weight or more and 98.98% by weight or less, A resin composition comprising: 1% by weight or more and 49.98% by weight or less of a cinnamic acid ester copolymer (B) containing a cinnamic acid ester residue unit represented by the following general formula (2) and a residue unit represented by the following general formula (3); and 0.01% by weight or more and 1.0% by weight or less of an antioxidant (C) having a molecular weight of 350 or more and being at least one member selected from the group consisting of phenol-based antioxidants and sulfur-based antioxidants. [Formula 1] (In the formula, R 1 , R 2 , R 3 each independently represents a hydrogen atom or a substituent having 1 to 12 carbon atoms. [chemical 2] (In the formula, R 4 represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms. 5 ~R 9 represents a hydrogen atom, a nitro group, a bromo group, an iodine group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, a phenyl group, a thiol group, an amido group, an amino group, a hydroxyl group, an alkoxy group having 1 to 12 carbon atoms, or an alkyl group having 1 to 12 carbon atoms. Y represents a nitro group, a bromo group, an iodine group, a cyano group, a chloro group, a sulfonic acid group, a carboxylic acid group, a fluoro group, or a thiol group. [C3] (In the formula, R 10 represents a 5-membered heterocyclic residue containing one or more nitrogen atoms or oxygen atoms as heteroatoms, or a 6-membered heterocyclic residue containing one or more nitrogen atoms or oxygen atoms as heteroatoms (the 5-membered heterocyclic residue and the 6-membered heterocyclic residue may form a condensed ring structure with another ring structure).
2. The resin composition according to claim 1, wherein the cinnamic acid ester copolymer (B) contains a residue unit represented by the general formula (2) and a residue unit represented by the general formula (3), and further contains a residue unit represented by the following general formula (4). [C4] (Here, R 11 , R 12 each independently represents a hydrogen atom, a linear alkyl group having 1 to 12 carbon atoms, a branched alkyl group having 3 to 12 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms.
3. 3. The resin composition according to claim 1 or 2, wherein in the cinnamate ester copolymer (B), the ratio of the monomer component relating to the cinnamate ester residue unit of the general formula (2) is 21 mol% or more and 50 mol% or less with respect to the total of all monomer components (100 mol%).
4. A film comprising the resin composition according to claim 1 .
5. The film according to claim 4, wherein the retardation (Re) represented by the following formula (5) is 30 nm or more and 300 nm or less, the Nz coefficient represented by the following formula (6) is 0.3 or more and 1.5 or less, and the ratio Re(450) / Re(550) of the retardation at 450 nm (Re(450)) to the retardation at 550 nm (Re(550)) is more than 0.60 and less than 1.
05. Re=(ny-nx)×d (5) Nz=(ny-nz) / (ny-nx) (6) (In the formula, nx represents the refractive index in the fast axis direction in the film plane, ny represents the refractive index in the slow axis direction in the film plane, nz represents the refractive index outside the film plane, and d represents the film thickness.)
6. 6. The film according to claim 4, which has a thickness of 30 μm and a total light transmittance of 85% or more at measurement wavelengths of 500 nm to 650 nm.
7. 7. The film according to claim 4, having a yellowness index YI of 1.7 or less.
8. 8. The film according to claim 4, which has a haze of 3.0% or less at a thickness of 30 μm and a measurement wavelength of 500 nm to 650 nm.
9. The film according to claim 4 , which has a YI of 1.7 or less after 500 hours in an 85° C. environment.
10. 10. The film according to claim 4, which has a change in yellowness index (YI) of less than 1.0 after high-temperature treatment in an 85°C environment for 500 hours.
11. The film according to claim 4 , which has a haze change of less than 2.0% after high-temperature treatment in an 85° C. environment for 500 hours.
12. A polarizing plate using the film according to claim 4 .
Citation Information
Patent Citations
Manufacturing method of birefringent film, retardation plate and liquid crystal display device using the same
JP1993297223A
Production of double refraction film, phase shifter and liquid crystal display device
JP1993323120A
Retardation film
JP2008064817A
Ethyl cellulose resin composition, molding, and chassis for electrical and electronic equipment