Terminal film for power storage devices

A terminal film for all-solid-state batteries, using a combination of modified polyolefin and other resins, addresses the issue of heat-sealing strength in varying temperatures and hydrogen sulfide exposure, ensuring robust sealing performance across different conditions.

JP7585617B2Active Publication Date: 2024-11-19TOPPAN HOLDINGS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020054033
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-25
Publication Date
2024-11-19
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

The sealing performance of all-solid-state batteries is compromised due to the insufficient heat resistance of conventional terminal films, and using highly heat-resistant resins for improved heat sealing leads to decreased heat-sealing strength at room temperature.

Method used

A terminal film composed of a combination of a first resin, such as modified polyolefin with a polar group, and a second resin, such as polyester or polyamide, ensures excellent heat-sealing strength in both high-temperature and room-temperature environments by enhancing compatibility and dispersibility.

Benefits of technology

The combined resin composition maintains high heat seal strength in high-temperature environments while preserving initial seal strength at room temperature, even after exposure to hydrogen sulfide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585617000002
    Figure 0007585617000002
  • Figure 0007585617000003
    Figure 0007585617000003
  • Figure 0007585617000004
    Figure 0007585617000004
Patent Text Reader

Abstract

To provide a terminal film for power storage devices, capable of achieving, at a sufficiently high level, both seal strength under high temperatures and initial seal strength under a room temperature environment.SOLUTION: A terminal film 40 for power storage devices is disposed to cover a part of the outer peripheral surface of a metal terminal 30 that is electrically connected to a power storage device body 10 constituting a power storage device 100. The terminal film is composed of a resin composition including polyolefin, as a first resin, and at least one resin selected from among polyester, polyamide, polycarbonate and polyphenylene ether, as a second resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a terminal film for an electricity storage device that is arranged so as to cover a portion of the outer peripheral surface of a metal terminal that is electrically connected to a main body of an electricity storage device. [Background technology]

[0002] Known examples of power storage devices include secondary batteries such as lithium ion batteries, nickel metal hydride batteries, and lead storage batteries, as well as electrochemical capacitors such as electric double layer capacitors. Due to the miniaturization of portable devices or the limitations of installation space, there is a demand for further miniaturization of power storage devices, and lithium ion batteries with high energy density have attracted attention. Metal cans have traditionally been used as exterior materials for lithium ion batteries, but multilayer films that are lightweight, have high heat dissipation properties, and can be produced at low cost have come to be used.

[0003] A lithium ion battery using the above multilayer film as an exterior material is called a laminated lithium ion battery. The exterior material covers the battery contents (positive electrode, separator, negative electrode, electrolyte, etc.) and prevents moisture from penetrating into the battery. A laminated lithium ion battery is manufactured, for example, by forming a recess in a part of the exterior material by cold forming, accommodating the battery contents in the recess, folding back the remaining part of the exterior material, and heat sealing the edges (see, for example, Patent Document 1).

[0004] Laminated lithium-ion batteries include a current extraction terminal (sometimes called a "tab lead"). In order to improve the adhesion between the current extraction terminal and the exterior material, a terminal film (sometimes called a "tab sealant") may be disposed so as to cover part of the outer periphery of the current extraction terminal (see, for example, Patent Documents 2 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-101765 A [Patent Document 2] JP 2008-4316 A [Patent Document 3] JP 2010-218766 A [Patent Document 4] JP 2009-259739 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, research and development is being conducted on a power storage device called an all-solid-state battery as a next-generation battery of lithium-ion batteries. An all-solid-state battery is characterized by using a solid electrolyte as the electrolyte, rather than an organic electrolyte. While a lithium-ion battery cannot be used at temperatures higher than the boiling point of the electrolyte (about 80°C), an all-solid-state battery can be used at temperatures exceeding 100°C, and the conductivity of lithium ions can be increased by operating it under high temperature conditions (for example, 100 to 150°C).

[0007] However, when a laminate-type all-solid-state battery is manufactured using the above-mentioned laminate as an exterior material, the heat resistance of the terminal film is insufficient, which may result in insufficient sealing of the package of the all-solid-state battery. On the other hand, the present inventors have found that, from the viewpoint of ensuring heat seal strength in a high-temperature environment, if a highly heat-resistant resin is used for the terminal film to be fused by heat sealing, a problem occurs in that the heat seal strength in a room-temperature environment decreases when the battery is returned to room temperature after being operated in a high-temperature environment.

[0008] Therefore, the present disclosure provides a terminal film for an electricity storage device that can ensure excellent heat seal strength in a high-temperature environment and can also ensure excellent heat seal strength in a room temperature environment after being exposed to a high-temperature environment. [Means for solving the problem]

[0009] A terminal film for an electricity storage device (hereinafter also simply referred to as "terminal film") according to one aspect of the present disclosure is a terminal film for an electricity storage device arranged to cover a portion of the outer peripheral surface of a metal terminal that is electrically connected to an electricity storage device main body that constitutes an electricity storage device, and the terminal film is made of a resin composition that includes a polyolefin as a first resin and at least one resin selected from polyester, polyamide, polycarbonate, and polyphenylene ether as a second resin.

[0010] By using the second resin, the heat seal strength of the terminal film in a high-temperature environment can be improved. However, the present inventors have found that when the second resin is used alone, the heat seal strength in a room temperature environment decreases, making it difficult to ensure excellent heat seal strength in both environments. The second resin is a highly heat-resistant resin, and although its performance when used in a high-temperature environment has been studied, there has been no sufficient study so far on the change in heat seal strength in a room temperature environment before and after exposure to a high-temperature environment. Since an all-solid-state battery is repeatedly placed in a high-temperature environment when in use and in a room temperature environment when not in use, it is necessary that the heat seal strength of the terminal film does not deteriorate in both usage environments. Therefore, the present inventors have conducted extensive research and found that by using the first resin in combination with the second resin, the decrease in heat seal strength can be suppressed both in a high-temperature environment and in a room temperature environment. In other words, according to the above-mentioned terminal film for an electricity storage device, by using a combination of a specific first resin and a specific second resin as the material for the terminal film, it is possible to ensure excellent heat seal strength in a high temperature environment, and also to ensure excellent heat seal strength in a room temperature environment.

[0011] The terminal film for an electricity storage device preferably contains a modified polyolefin in which a polar group capable of reacting with polyester, polyamide, polycarbonate, or polyphenylene ether is modified. In the terminal film for an electricity storage device, the modified polyolefin is preferably modified with maleic anhydride. The compatibility between the first resin and the second resin is not necessarily good, and the dispersibility is insufficient, so that the above-mentioned combined effect may not be obtained sufficiently. On the other hand, the first resin contains a modified polyolefin having a polar group capable of reacting with the second resin, so that the compatibility between the first resin and the second resin can be increased and the dispersibility can be improved. As a result, the synergistic effect of the combined use of the first resin and the second resin can be obtained more sufficiently, and a better heat seal strength can be secured in a high temperature environment, and a better heat seal strength can be secured in a room temperature environment. In addition, when the modified polyolefin is a polyolefin modified with maleic anhydride, the above-mentioned effect can be obtained more sufficiently.

[0012] Here, the first resin may contain the above-mentioned modified polyolefin and a polyolefin (unmodified polyolefin) that does not have a polar group that can react with the second resin. Since the melting point and molecular weight of modified polyolefins tend to decrease due to modification, the use of a normal polyolefin (unmodified polyolefin) in combination can suppress the decrease in heat seal strength in a high temperature environment. When modified polyolefins and unmodified polyolefins are used in combination, the modified polyolefin plays a role as a compatibilizer, and can improve the dispersibility of the unmodified polyolefin and the second resin.

[0013] In the terminal film for an electricity storage device, the polyester or polyamide contained in the terminal film preferably has a crystallinity of 10% or more and less than 70% when heat-sealed under conditions of 260°C, 0.5 MPa, and 3 seconds and then cooled to room temperature. When the crystallinity of the polyester and / or polyamide measured by the above method is within the above range, the heat seal strength in a high-temperature environment can be further improved, and the flexibility of the terminal film can be further improved.

[0014] The terminal film for the power storage device preferably contains a hydrogen sulfide adsorbent in the terminal film. The hydrogen sulfide adsorbent may be contained in the terminal film, or in the case where the terminal film has a multi-layer structure, it may be contained in another layer. In the all-solid-state battery, for example, a sulfide-based electrolyte, an oxide-based electrolyte, or an organic polymer electrolyte is used as the electrolyte. When a sulfide-based electrolyte is used, hydrogen sulfide is generated when moisture is mixed into the cell, and there is a concern that the adhesion between the outer surface of the terminal and the terminal film may decrease. By containing a hydrogen sulfide adsorbent in the terminal film, it is possible to maintain excellent seal strength at room temperature and high temperature even after exposure to hydrogen sulfide. Effect of the Invention

[0015] According to the present disclosure, there is provided a terminal film for an electricity storage device that can achieve sufficiently high levels of both seal strength at high temperatures and initial seal strength at room temperature. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a perspective view illustrating an example of an all-solid-state battery. [Diagram 2] FIG. 1 is a cross-sectional view that illustrates an example of an exterior material for a power storage device. [Diagram 3] FIG. 2 is a cross-sectional view that illustrates a schematic configuration of a sealant layer included in an exterior material for an energy storage device. [Figure 4] FIG. 2 is a cross-sectional view taken along line IV-IV in FIG. 1, and is a cross-sectional view illustrating a schematic configuration of a tab (terminal film and metal terminal) of the all-solid-state battery. [Diagram 5] 1 is a cross-sectional view showing a schematic example of the configuration of a terminal film. FIG. [Figure 6] FIG. 2 is a plan view illustrating the evaluation samples prepared in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to the embodiments described below. In addition, in the embodiments shown below, technically preferable limitations are imposed for carrying out the invention, but these limitations are not essential requirements for the present invention.

[0018] <Electricity storage device> Fig. 1 is a perspective view showing a schematic configuration of a power storage device according to the present embodiment. In Fig. 1, an all-solid-state battery is illustrated as an example of a power storage device 100, and the following description will be given. Note that the power storage device having the configuration shown in Fig. 1 may be called a battery pack or a battery cell.

[0019] The energy storage device 100 is an all-solid-state battery, and includes an energy storage device body 50, an exterior material 10, a pair of metal terminals 30, and a terminal film (tab sealant) 40. The energy storage device body 50 is a battery body that performs charging and discharging. The exterior material 10 covers the surface of the energy storage device body 50 and is disposed so as to be in contact with a portion of the terminal film 40.

[0020] [Exterior material] 2 is a cross-sectional view showing an example of a cut surface of the exterior material 10. The exterior material 10 has a multilayer structure including, from the outside to the inside (the electricity storage device main body 50 side), a base material layer 11, a first adhesive layer 12, a barrier layer 13, a corrosion prevention treatment layer 14, a second adhesive layer 17, and a sealant layer 16, in this order.

[0021] (Sealant layer) The sealant layer 16 is a layer that imparts heat-sealing sealability to the exterior material 10, and is a layer that is placed on the inside and heat-sealed (thermally fused) when the electricity storage device is assembled.

[0022] For example, thermoplastic resins such as polyolefin, polyamide, polyester, polycarbonate, polyphenylene ether, polyacetal, polystyrene, polyvinyl chloride, and polyvinyl acetate can be used for the sealant layer 16, and polyolefin, polyamide, and polyester are preferred from the viewpoint of heat resistance and sealing suitability. When directly laminating to the barrier layer without using an adhesive, it is preferred to use a material in which at least one layer in contact with the barrier layer is modified with an acid, glycidyl, or the like.

[0023] Examples of polyolefin resins include low-, medium- and high-density polyethylenes, ethylene-α-olefin copolymers, polypropylene, and propylene-α-olefin copolymers. When the polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer.

[0024] Examples of polyester resins include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT). These polyester resins may be used alone or in combination of two or more. In addition, copolymers of any acid and glycol may be used.

[0025] Furthermore, similar to the terminal film described later, a resin composition containing a polyolefin as a first resin and at least one resin selected from polyester, polyamide, polycarbonate, and polyphenylene ether as a second resin may be used.

[0026] In order to impart sealing properties, heat resistance and other functionalities, for example, antioxidants, slip agents, flame retardants, antiblocking agents, light stabilizers, dehydrating agents, tackifiers, crystal nucleating agents, plasticizers and the like may be added.

[0027] The peak melting temperature of the sealant layer 16 varies depending on the application, but in the case of an exterior material for an all-solid-state battery, it is preferably 160 to 280° C. because this improves heat resistance.

[0028] The temperature at which the minor dispersion peak γ and the major dispersion peak α of the sealant layer 16 appear can be controlled, for example, by the structure of the base resin material contained in the sealant layer 16, the stretching ratio of the sealant layer 16, or the amount of additives (e.g., plasticizers) blended. The sealant layer 16 contains additives as necessary. Examples of additives include plasticizers, antioxidants, slip agents, flame retardants, AB agents, light stabilizers, dehydrating agents, and tackifiers.

[0029] Examples of the base resin material contained in the sealant layer 16 include polyester-based, polyolefin-based, and polyamide-based resins.

[0030] The polyester resin can be obtained by copolymerizing an acid component and a glycol component. Examples of the acid component include phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, cyclohexanedicarboxylic acid, adipic acid, and sebacic acid. Examples of the glycol component include ethylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, cyclohexanedimethanol, and propanediol. According to the study by the present inventors, the temperature at which the secondary dispersion peak γ exists in the general PET (copolymer of terephthalic acid and ethylene glycol) is outside the range of −130° C. to −50° C., and the seal strength at room temperature is insufficient. When a plasticizer is not blended in the sealant layer 16, it is preferable that the sealant layer 16 contains a polyester resin in which one acid component and two or more glycol components are copolymerized.

[0031] Examples of polyolefin resins include polyethylene and polypropylene resins. Generally used polyolefin resins have poor heat resistance, so it is preferable to use polyethylene or polypropylene modified with amide or the like.

[0032] Examples of polyamide resins include nylon 6 and nylon 6,6.

[0033] From the viewpoint of adjusting the temperature at which the minor dispersion peak γ and the major dispersion peak α of the sealant layer 16 appear, the sealant layer 16 preferably contains a plasticizer. As the plasticizer, for example, an ester-based compound can be used. Specific examples include glycol diesters, adipic acid esters, phthalic acid esters, diacetyl monoacyl glycerol derivatives, and esters having an ether skeleton. Although it depends on the base resin material of the sealant layer 16, the content of the plasticizer in the sealant layer 16 is preferably 30 mass% or less based on the mass of the sealant layer 16. When an excessive amount of plasticizer is blended in the sealant layer 16, the temperature at which the minor dispersion peak γ and the major dispersion peak α appear is excessively lowered, and the cohesive force tends to decrease.

[0034] The sealant layer 16 may have a single layer structure or a multi-layer structure of two or more layers (see Figs. 3(a) to 3(c)). When the sealant layer has a single layer structure, its thickness is preferably 10 to 300 µm, and more preferably 20 to 100 µm. When the thickness of the sealant layer 16 is 10 µm or more, it is easy to ensure sealing properties and insulation properties, while when the thickness is 300 µm or less, it is possible to ensure the cell volume.

[0035] FIG. 3(b) is a cross-sectional view that shows a two-layer structure of the sealant layer 16. The sealant layer 16 shown in the figure has a first resin layer 16a and a second resin layer 16b formed on the inner surface of the first resin layer 16a. The first resin layer 16a may be made of a different material from the second resin layer 16b, for example, and may have a different thickness from the second resin layer 16b. The thicknesses of the first resin layer 16a and the second resin layer 16b are, for example, 5 to 300 μm, and may be 20 to 200 μm. As shown in FIG. 3(c), the sealant layer 16 may have a three-layer structure and further include a third resin layer 16c.

[0036] When the electrolyte of the all-solid-state battery is a sulfide-based electrolyte, the sealant layer 16 preferably contains a hydrogen sulfide adsorbent. By containing the hydrogen sulfide adsorbent, the sealant layer 16 can maintain excellent seal strength at room temperature and at high temperatures even after exposure to hydrogen sulfide. As the hydrogen sulfide adsorbent, a material having the ability to absorb or adsorb hydrogen sulfide can be used. Specific examples thereof include zinc oxide, amorphous metal silicate, hydroxide of zirconium and lanthanoid elements, tetravalent metal phosphate, potassium permanganate, sodium permanganate, aluminum oxide, iron hydroxide, silver sulfate, silver acetate, isocyanate compounds, aluminum silicate, potassium aluminum sulfate, zeolite, activated carbon, amine compounds, and ionomers.

[0037] The content of the hydrogen sulfide adsorption substance in the sealant layer 16 is preferably 1 to 50 mass %, more preferably 2 to 25 mass %, and even more preferably 5 to 15 mass %, based on the mass of the sealant layer 16. When the content of the hydrogen sulfide adsorption substance in the sealant layer 16 is 1 mass % or more, the hydrogen sulfide adsorption effect is exhibited, while when the content is 50 mass % or less, the sealant layer 16 can achieve both adhesion and sealant suitability. When the sealant layer 16 has a multi-layer structure, all or some of the layers may contain the hydrogen sulfide adsorption substance. A layer other than the sealant layer 16 (e.g., the second adhesive layer 17) may contain a sulfide-based electrolyte, but from the viewpoint of the content of the hydrogen sulfide adsorbing substance, it is preferable that at least the sealant layer 16 contains the hydrogen sulfide adsorbing substance.

[0038] (base material layer) The base layer 11 provides heat resistance in the sealing process when manufacturing the electricity storage device and plays a role in suppressing the occurrence of pinholes that may occur during molding and distribution. In particular, in the case of an exterior material for a large-scale electricity storage device, the base layer 11 can also provide scratch resistance, chemical resistance, insulation, and the like.

[0039] The base layer 11 is preferably a layer made of a resin film formed of an insulating resin. Examples of the resin film include stretched or unstretched films such as polyester film, polyamide film, polypropylene film, and polyphenylene sulfide film. The base layer 11 may be a single layer film made of any of these resin films, or a laminate film made of two or more of these resin films.

[0040] Among these, polyester film and polyamide film are preferable as the base layer 11 because of their excellent moldability, and polyamide film is more preferable. These films are preferably biaxially stretched films. Examples of polyester resins constituting the polyester film include polyethylene terephthalate. Examples of polyamide resins constituting the polyamide film include nylon 6, nylon 6,6, a copolymer of nylon 6 and nylon 6,6, nylon 6,10, polymetaxylylene adipamide (MXD6), nylon 11, nylon 12, etc. Among these, nylon 6 (ONy) is preferable because of its excellent heat resistance, puncture strength, and impact strength.

[0041] Examples of the stretching method for the biaxially stretched film include a sequential biaxial stretching method, a tubular biaxial stretching method, a simultaneous biaxial stretching method, etc. From the viewpoint of obtaining better deep draw formability, the biaxially stretched film is preferably one stretched by a tubular biaxial stretching method.

[0042] The thickness of the substrate layer 11 is preferably 6 to 40 μm, and more preferably 10 to 30 μm. When the thickness of the substrate layer 11 is 6 μm or more, the pinhole resistance and insulating properties of the packaging material 10 tend to be improved. When the thickness of the substrate layer 11 exceeds 40 μm, the total thickness of the packaging material 10 tends to be large.

[0043] (First adhesive layer) The first adhesive layer 12 is a layer that bonds the base layer 11 and the barrier layer 13. Specific examples of materials constituting the first adhesive layer 12 include polyurethane resins in which a bifunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol. The above-mentioned various polyols can be used alone or in combination of two or more types depending on the functions and performance required for the exterior material. In addition, the above-mentioned polyurethane resins may be mixed with various other additives and stabilizers depending on the performance required for the adhesive.

[0044] The thickness of the first adhesive layer 12 is not particularly limited, but from the viewpoint of obtaining desired adhesive strength, conformability, processability, and the like, the thickness is, for example, preferably 1 to 10 μm, and more preferably 3 to 7 μm.

[0045] (Barrier layer) The barrier layer 13 has a water vapor barrier property that prevents moisture from penetrating into the inside of the electricity storage device. The barrier layer 13 also has extensibility for deep drawing. As the barrier layer 13, various metal foils such as aluminum, stainless steel, copper, etc., metal vapor deposition films, inorganic oxide vapor deposition films, carbon-containing inorganic oxide vapor deposition films, films provided with these vapor deposition films, etc. can be used. From the standpoints of mass (specific gravity), moisture resistance, processability, and cost, metal foils are preferred, and aluminum foil is more preferred.

[0046] As the aluminum foil, a soft aluminum foil that has been annealed can be preferably used from the viewpoint of imparting desired ductility during molding, but it is more preferable to use an aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The content of iron in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, in 100 mass% of the aluminum foil. By having an iron content of 0.1 mass% or more, an exterior material 10 having better pinhole resistance and ductility can be obtained. By having an iron content of 9.0 mass% or less, an exterior material 10 having better flexibility can be obtained. Although untreated aluminum foil may be used, it is preferable to use an aluminum foil that has been degreased. When the aluminum foil is degreased, the degreased treatment may be performed on only one side of the aluminum foil, or on both sides.

[0047] The thickness of the barrier layer 13 is not particularly limited, but taking into consideration the barrier properties, pinhole resistance, and processability, it is preferably 9 to 200 μm, and more preferably 15 to 100 μm.

[0048] (Corrosion prevention treatment layer) The corrosion prevention treatment layer 14 is a layer provided to prevent corrosion of the barrier layer 13. The corrosion prevention treatment layer 14 is formed, for example, by degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.

[0049] Examples of the degreasing treatment include acid degreasing and alkaline degreasing. Examples of the acid degreasing include a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid alone or a mixture of these. In addition, by using an acid degreasing agent in which a fluorine-containing compound such as monosodium ammonium difluoride is dissolved in the inorganic acid as described above, not only can the aluminum be degreased, but also a passive aluminum fluoride can be formed, which is effective in terms of corrosion resistance, particularly when an aluminum foil is used for the barrier layer 13. Examples of the alkaline degreasing include a method using sodium hydroxide or the like.

[0050] An example of the hydrothermal modification treatment is boehmite treatment in which an aluminum foil is immersed in boiling water containing triethanolamine. An example of the anodization treatment is alumite treatment.

[0051] The chemical conversion treatment may be of the immersion type or the coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of a mixture of these. On the other hand, examples of the coating type chemical conversion treatment include a method in which a coating agent having corrosion prevention properties is applied onto the barrier layer 13.

[0052] When forming at least a part of the corrosion prevention layer by any of these corrosion prevention treatments, namely, hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment in advance. When using a degreased metal foil, such as a metal foil that has been subjected to an annealing process, as the barrier layer 13, there is no need to perform a degreasing treatment again in forming the corrosion prevention layer 14.

[0053] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.

[0054] Among the above treatments, particularly in hydrothermal conversion treatment and anodization treatment, the aluminum foil surface is dissolved by a treatment agent to form an aluminum compound (boehmite, alumite) with excellent corrosion resistance. Therefore, since a bicontinuous structure is formed from the barrier layer 13 using the aluminum foil to the corrosion prevention treatment layer 14, the above treatment is included in the definition of chemical conversion treatment. On the other hand, as described later, it is also possible to form the corrosion prevention treatment layer 14 by a pure coating method alone, which is not included in the definition of chemical conversion treatment. As an example of this method, a method using a sol of a rare earth element oxide such as cerium oxide with an average particle size of 100 nm or less can be mentioned, which has an aluminum corrosion prevention effect (inhibitor effect) and is also environmentally friendly. By using this method, it is possible to impart a corrosion prevention effect to metal foil such as aluminum foil even with a general coating method.

[0055] Examples of the rare earth oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, and ether-based solvents. Among these, water-based sols are preferred. In order to stabilize the dispersion of the rare earth oxide sol, inorganic acids such as nitric acid, hydrochloric acid, and phosphoric acid or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, and lactic acid are usually used as dispersion stabilizers. Among these dispersion stabilizers, phosphoric acid is particularly expected to (1) stabilize the dispersion of the sol, (2) improve adhesion to the barrier layer 13 by utilizing the aluminum chelating ability of phosphoric acid, and (3) improve the cohesive force of the corrosion prevention treatment layer 14 (oxide layer) by easily causing dehydration condensation of phosphoric acid even at low temperatures.

[0056] The corrosion prevention treatment layer 14 formed by the rare earth element oxide sol is an aggregate of inorganic particles, and therefore the layer itself may lose its cohesive strength even after the dry curing process. Therefore, in this case, the corrosion prevention treatment layer is preferably compounded with the following anionic polymer or cationic polymer to supplement the cohesive strength.

[0057] The corrosion prevention treatment layer is not limited to the above-mentioned layers. For example, it may be formed using a treatment agent in which phosphoric acid and a chromium compound are mixed with a resin binder (such as aminophenol), as in the case of coating-type chromate, which is a known technology. By using this treatment agent, a layer having both corrosion prevention function and adhesion can be obtained. In addition, although it is necessary to consider the stability of the coating liquid, a coating agent in which a rare earth element oxide sol and a polycationic polymer or a polyanionic polymer are previously mixed into a one-component solution can be used to obtain a layer having both corrosion prevention function and adhesion.

[0058] The mass per unit area of ​​the corrosion prevention treatment layer is 0.005 to 0.200 g / m2, whether it is a multi-layer structure or a single-layer structure. 2 is preferable, and 0.010 to 0.100 g / m 2 It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the barrier layer 13. 2 Even if the thickness exceeds 100 mm, the corrosion prevention function does not change much. On the other hand, when a rare earth oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention treatment layer 14 can be calculated from its specific gravity.

[0059] From the viewpoint of adhesion between the sealant layer and the barrier layer, the corrosion prevention treatment layer may be, for example, an embodiment that contains cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate relative to 100 parts by mass of the cerium oxide, and a cationic polymer, or an embodiment that is formed by subjecting the barrier layer 13 to a chemical conversion treatment, or an embodiment that is formed by subjecting the barrier layer to a chemical conversion treatment, An embodiment containing a cationic polymer may also be used.

[0060] (Second adhesive layer) The second adhesive layer 17 is a layer that bonds the barrier layer 13, on which the corrosion prevention treatment layer 14 is formed, to the sealant layer 16. For the second adhesive layer 17, a general adhesive for bonding the barrier layer 13 and the sealant layer 16 can be used.

[0061] When the corrosion prevention treatment layer 14 has a layer containing at least one type of polymer selected from the group consisting of the above-mentioned cationic polymers and anionic polymers, the second adhesive layer 17 is preferably a layer containing a compound (hereinafter also referred to as a "reactive compound") that is reactive with the above-mentioned polymer contained in the corrosion prevention treatment layer 14.

[0062] For example, when the corrosion prevention treatment layer 14 contains a cationic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer. When the corrosion prevention treatment layer 14 contains an anionic polymer, the second adhesive layer 17 contains a compound reactive with the anionic polymer. When the corrosion prevention treatment layer 14 contains a cationic polymer and an anionic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer and a compound reactive with the anionic polymer. However, the second adhesive layer 17 does not necessarily have to contain the above two types of compounds, and may contain a compound reactive with both the cationic polymer and the anionic polymer. Here, "reactive" means to form a covalent bond with the cationic polymer or the anionic polymer. The second adhesive layer 17 may further contain an acid-modified polyolefin resin.

[0063] The compound reactive with the cationic polymer may be at least one compound selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, and a compound having an oxazoline group.

[0064] Examples of the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group include the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group, which are exemplified above as crosslinking agents for forming a crosslinked structure from a cationic polymer. Among these, the polyfunctional isocyanate compound is preferred in terms of high reactivity with the cationic polymer and ease of forming a crosslinked structure.

[0065] The compound reactive with anionic polymers includes at least one compound selected from the group consisting of glycidyl compounds and compounds having oxazoline groups.These glycidyl compounds and compounds having oxazoline groups include the glycidyl compounds and compounds having oxazoline groups exemplified above as crosslinking agents for forming cationic polymers into crosslinked structures.Among these, glycidyl compounds are preferred because of their high reactivity with anionic polymers.

[0066] When the second adhesive layer 17 contains an acid-modified polyolefin resin, it is preferable that the reactive compound also has a reactivity with the acidic group in the acid-modified polyolefin resin (i.e., forms a covalent bond with the acidic group). This further enhances the adhesion to the corrosion prevention treatment layer 14. In addition, the acid-modified polyolefin resin has a crosslinked structure, further improving the solvent resistance of the exterior material 10.

[0067] The content of the reactive compound is preferably from 1 to 10 times the equivalent of the acid group in the acid-modified polyolefin resin. If it is 1 or more times the equivalent, the reactive compound reacts sufficiently with the acid group in the acid-modified polyolefin resin. On the other hand, if it exceeds 10 times the equivalent, the acid-modified polyolefin resin may react with the acid group in the acid-modified polyolefin resin. Since the crosslinking reaction with the resin has reached saturation, there is a concern that unreacted substances remain and various performances may be deteriorated. Therefore, for example, the content of the reactive compound is preferably 5 to 20 parts by mass (solid content ratio) per 100 parts by mass of the acid-modified polyolefin resin.

[0068] The acid-modified polyolefin resin is a polyolefin resin to which an acidic group has been introduced. Examples of the acidic group include a carboxyl group, a sulfonic acid group, and an acid anhydride group, and maleic anhydride groups and (meth)acrylic acid groups are particularly preferred. For example, the acid-modified polyolefin resin may be the same as the modified polyolefin resin used in the sealant layer 16.

[0069] The second adhesive layer 17 may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier.

[0070] Examples of adhesives that form the second adhesive layer 17 include polyurethane resins in which a difunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and epoxy resins in which an amine compound or the like is reacted with a base material having an epoxy group, and these are preferred from the standpoint of heat resistance.

[0071] The thickness of the second adhesive layer 17 is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, processability, and the like, it is preferably 1 to 10 μm, and more preferably 2 to 7 μm.

[0072] [Metal terminal] Fig. 4 is a cross-sectional view of the terminal film and the metal terminal shown in Fig. 1 in the direction of line IV-IV. Of the pair of metal terminals 30, 30, one metal terminal 30 is electrically connected to the positive electrode of the electricity storage device main body 50, and the other metal terminal 30 is electrically connected to the negative electrode of the electricity storage device main body 50. The pair of metal terminals 30, 30 extend from the electricity storage device main body 50 to the outside of the exterior material 10. The shape of the pair of metal terminals 30, 30 may be, for example, a flat plate shape.

[0073] Metals can be used as the material of the metal terminal 30. The metal to be used as the material of the metal terminal 30 may be determined in consideration of the structure of the power storage device main body 50 and the materials of its components. For example, when the power storage device 100 is an all-solid-state battery, aluminum is preferably used as the material of the metal terminal 30 connected to the positive electrode of the power storage device main body 50. Copper having a nickel plating layer formed on the surface, or nickel, is preferably used as the material of the metal terminal 30 connected to the negative electrode of the power storage device main body 50.

[0074] The thickness of the metal terminal 30 depends on the size and capacity of the all-solid-state battery. In the case of a small all-solid-state battery, the thickness of the metal terminal 30 may be, for example, 50 μm or more. In the case of a large all-solid-state battery for power storage, vehicle mounting, etc., the thickness of the metal terminal 30 may be appropriately set within the range of, for example, 100 to 500 μm.

[0075] [Terminal film] 4, the terminal film 40 is disposed so as to cover a portion of the outer circumferential surface of the metal terminal 30. By disposing the terminal film 40 between the metal terminal 30 and the exterior material 10, it is possible to achieve an even higher level of sealing and insulation properties for the electricity storage device 100. The terminal film 40 has heat resistance equal to or greater than that of the sealant layer 16 and the base material layer 11 described above.

[0076] The terminal film 40 is made of a polyolefin as a first resin and a polyester, polyamide, polycarbonate, or polyphenylene ether (hereinafter, referred to as polyester) as a second resin. and at least one resin selected from the group consisting of resins (hereinafter referred to as resins, etc.). The terminal film 40 has a single-layer structure or a multi-layer structure. When the terminal film 40 has a single-layer structure, the terminal film 40 is made of a resin layer 40a (see FIG. 5(a)). When the terminal film 40 has a multi-layer structure, it is sufficient that the terminal film 40 includes at least one resin layer (resin layer 40a) that satisfies the above conditions (see FIGS. 5(b) and 5(c)). When the terminal film 40 has a multi-layer structure, it is preferable that all layers are made of the same type of resin material from the viewpoint of adhesion between adjacent layers.

[0077] The terminal film 40 preferably contains a modified polyolefin in which a polar group capable of reacting with the second resin, such as polyester, has been modified. By providing the terminal film 40 with the resin layer 40a having the above-mentioned composition, the terminal film 40 can achieve a sufficiently high level of both the seal strength at high temperatures and the initial seal strength (seal strength at room temperature). Examples of resins constituting the terminal film 40 are shown below.

[0078] (Polyolefin resin) Examples of polyolefin resins that can be used include polyethylene (LDPE, LLDPE, HDPE), polypropylene (homo, block, random), polybutene, etc. From the viewpoint of heat resistance and flexibility, it is preferable to use polypropylene, and it is particularly preferable to use block polypropylene.

[0079] (polyester resin) The polyester resin can be obtained by copolymerizing an acid component and a glycol component. Examples of the acid component include phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, cyclohexanedicarboxylic acid, adipic acid, and sebacic acid. Examples of the glycol component include ethylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, cyclohexanedimethanol, and propanediol. However, after heat sealing at 260°C-0.5Mpa-3s, it is preferable that the crystallinity is 10% or more and less than 70%. This is because if the crystallinity of the polyester is too low, the high-temperature seal strength is not sufficiently exhibited, and if it is too high, the flexibility tends to be poor. From the above tendency, it is more preferable to use a polyester with a crystallinity of 15% or more and less than 50%. It is preferable to use a polyester resin obtained by copolymerizing these.

[0080] (Polyamide resin) As the polyamide resin, nylons such as nylon 6, nylon 11, nylon 12, and nylon 6,6 can be used. Aramids having aromatic groups may also be used. As with polyesters, the crystallinity after heat sealing is preferably 10% or more and less than 70%, and more preferably 15% or more and less than 50%.

[0081] Furthermore, since polycarbonate and polyphenylene ether are non-crystalline, there is no preferred range for the degree of crystallinity.

[0082] The above-listed polyesters, polyamides, and other resins may be at least one of them, and may contain a plurality of them. Each resin may be one type or a blend of multiple types (for example, polyolefin may be a mixture of block and random).

[0083] (Modified polyolefin) Examples of the functional group with which the second resin reacts include, but are not limited to, the following functional groups. Polyester: terminal hydroxyl group, terminal carboxyl group, ester bond Polyamide: terminal amino group, amide bond Polycarbonate: terminal hydroxyl group, ester bond Polyphenylene ether: Terminal hydroxyl groups

[0084] Examples of the modifying group that reacts with each of the above functional groups include the following. Polyester, polycarbonate: hydroxyl group, acid-modified (ester) group, aldehyde group, oxazoline group, glycidyl group, amide group, imino group Polyamide reaction: hydroxyl group, acid-modified (ester) group, aldehyde group, glycidyl group Polyphenylene ether reaction: acid-modified (ester) group, oxazoline group, glycidyl group, amide group, imino group Specific examples include: Hydroxyl group: Poval (Kuraray), Mersen H (Tosoh) Glycidyl group: MODIPER (NOF), LOTADER, BONDINE (Arkema) Amide group: APOLHYA (Arkema) Imino group...Admer IP (Mitsui Chemicals) Oxazoline group...Epocross (Nippon Shokubai) The following can be given as suitable examples.

[0085] As for the acid modification, examples of the acid-modified polyolefin include those modified with an unsaturated carboxylic acid, an acid anhydride of an unsaturated carboxylic acid, or an ester of an unsaturated carboxylic acid.

[0086] Specific examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, tetrahydrophthalic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.

[0087] Examples of the acid anhydrides of unsaturated carboxylic acids include acid anhydrides of unsaturated carboxylic acids such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.

[0088] Examples of the esters of unsaturated carboxylic acids include esters of unsaturated carboxylic acids such as methyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconate, dimethyl tetrahydrophthalate, and dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.

[0089] As specific products, for example, the following can be used, and it is preferable to use acid-modified maleic acid. Maleic anhydride: Admer (Mitsui Chemicals), Modic (Mitsubishi Chemical), Toyo Tack (Toyobo), Sunstack (Sanyo Chemical) Carboxyl group: Nucrel, Himilan (Mitsui DuPont Polychemicals) *Ionomer systems can also be used. Ester group: Evaflex (Mitsui DuPont Polychemicals), LOTADER, BONDINE, EVATANE (Arkema)

[0090] Regarding the ratio of each resin in the terminal film 40, the ratio of polyolefin is preferably 10 to 80 wt% from the viewpoint of the balance between high-temperature seal strength and room-temperature seal strength. If the total amount of polyolefin and polyester, etc. is 100 wt%, the ratio of polyester, etc. is also preferably 90 to 20 wt%. The ratio of modified polyolefin in the polyolefin is preferably 0.1 wt% to 100 wt%, more preferably 0.5 wt% to 40 wt%. If the amount added is too small, the reaction with polyester or polyamide will not proceed easily. Although there is no problem in terms of performance at 100 wt%, if the melting point of the modified polyolefin is low, there is a risk of a decrease in high-temperature seal strength, so it is more preferable that the ratio is within 40 wt%.

[0091] When the terminal film 40 has a multi-layer structure, the resin layer 40a may be disposed on the side in contact with the metal terminal 30, or on the side in contact with the exterior material 10. When the terminal film 40 is made up of three or more layers, the resin layer 40a may be disposed between the resin layer 40b and the resin layer 40c (see FIG. 5(c)).

[0092] From the viewpoints of embeddability and insulating properties, the thickness of the terminal film 40 is preferably 15 μm or more, more preferably 30 to 300 μm, and further preferably 50 to 200 μm.

[0093] Generally, sulfide-based electrolytes, oxide-based electrolytes, organic polymer-based electrolytes, etc. are used as electrolytes for all-solid-state batteries. When the electrolyte for the all-solid-state battery is a sulfide-based electrolyte, it is preferable that the terminal film 40 contains a hydrogen sulfide adsorbent. When a sulfide-based electrolyte is used, hydrogen sulfide is generated when moisture is mixed into the cell, and there is a concern that the adhesion between the metal terminal (tab lead) and the terminal film (tab sealant) will decrease. By adding a hydrogen sulfide adsorbent, it is possible to maintain the seal strength at room temperature and high temperatures even when exposed to hydrogen sulfide.

[0094] Examples of the hydrogen sulfide adsorbing material are not particularly limited, but include, for example, zinc oxide, amorphous metal silicate, hydroxide of zirconium and lanthanoid elements, tetravalent metal phosphate, potassium permanganate, sodium permanganate, aluminum oxide, iron hydroxide, silver sulfate, silver acetate, isocyanate compounds, aluminum silicate, tetravalent metal phosphate, potassium aluminum sulfate, zeolite, activated carbon, amine compounds, ionomers, etc. By including a hydrogen sulfide adsorbing material in the terminal film 40, excellent seal strength can be maintained at room temperature and high temperatures even after exposure to hydrogen sulfide.

[0095] The content of the hydrogen sulfide adsorbent in the terminal film 40 is preferably 1 to 50 mass %, more preferably 2 to 25 mass %, and even more preferably 5 to 15 mass %, based on the mass of the terminal film 40. When the content of the hydrogen sulfide adsorbent in the terminal film 40 is 1 mass % or more, the hydrogen sulfide absorption or adsorption effect is exhibited, while when the content is 50 mass % or less, the terminal film 40 can achieve both adhesion and sealant suitability. When the terminal film 40 has a multi-layer structure, from the viewpoint of adhesion to the metal terminal 30, it is preferable that the layer in contact with the metal terminal 30 does not contain a hydrogen sulfide adsorbent. That is, it is preferable that the layer in contact with the exterior material 10 (for example, the resin layer 40a in FIG. 5(b) or the resin layers 40a and 40c in FIG. 5(c)) contains a hydrogen sulfide adsorbent, and when the terminal film 40 is composed of three or more layers, it is preferable that an intermediate layer (for example, the resin layer 40a in FIG. 5(c)) contains a hydrogen sulfide adsorbent.

[0096] The resin layer 40a may contain additives as necessary, such as a plasticizer, an antioxidant, a slip agent, a flame retardant, an AB agent, a light stabilizer, a dehydrating agent, and a tackifier.

[0097] Although the embodiments of the present disclosure have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and variations are possible within the scope of the gist of the present disclosure as described in the claims.

[0098] For example, in the above embodiment, the corrosion prevention treatment layer 14 is provided only on one surface (the second adhesive layer 17 side) of the barrier layer 13, but the corrosion prevention treatment layer 14 may also be provided on the other surface (the first adhesive layer 12 side) of the barrier layer 13. Furthermore, for example, when the sealant layer 16 is attached to the barrier layer 13 by thermal lamination, the second adhesive layer 17 may be omitted. When the base layer 11 is provided by coating or painting, the first adhesive layer 12 may not be provided. In the above embodiment, an all-solid-state battery is exemplified as the power storage device to which the exterior material 10 is applied, but the exterior material 10 may be applied to other power storage devices (for example, a lithium ion battery). EXAMPLES

[0099] The present disclosure will be described more specifically below based on examples, but the present disclosure is not limited to the following examples.

[0100] [Materials used] In order to fabricate the terminal films according to the examples and comparative examples, the following materials were prepared.

[0101] [Resin material] Polyolefin (Block Polypropylene): Novatec PP, made by Nippon Polypropylene Polyester 1: A copolymer of terephthalic acid as the acid component and ethylene glycol as the glycol component. Polyester 2: A copolymer of terephthalic acid as the acid component and ethylene glycol as the glycol component (the amount of ethylene glycol is increased compared to polyester 1) Polyester 3: A copolymer of naphthalenedicarboxylic acid as the acid component and ethylene glycol as the glycol component. Polyester 4: A copolymer of terephthalic acid as the acid component and ethylene glycol, butanediol and 1,4-cyclohexanedimethanol as the glycol component. Polyester 5: A copolymer of naphthalenedicarboxylic acid as the acid component and ethylene glycol as the glycol component (less ethylene glycol than polyester 3) Polyamide (nylon 6 (Ny6)): Glamid, manufactured by Toyobo Polycarbonate: Iupilon, manufactured by Mitsubishi Chemical Polyphenylene ether: Zylon, manufactured by Asahi Kasei Modified polyolefin 1 (maleic anhydride): Toyo Tack (PP), Toyobo Modified polyolefin 2 (hydroxyl group): Mersen, manufactured by Tosoh Modified polyolefin 3 (carboxyl group): Nucrel, manufactured by Mitsui DuPont Polychemicals Modified polyolefin 4 (ester group): EVATANE, manufactured by Arkema Polyolefin (modified polyolefin) and polyester, etc. are melt blended in advance using a twin-screw compounding machine.

[0102] [Hydrogen sulfide absorber] Zinc oxide: 3 parts by weight was added to the terminal film.

[0103] [Evaluation method] (Sample preparation) As samples for each example using the above resin materials, a terminal film sample cut to 50mm (TD) x 100mm (MD) was prepared, and a chemically treated AL cut to 50mm x 50mm was folded in half, and one side was heat sealed with a 10mm wide seal bar at 165℃, 0.6MPa, and 10sec. The heat sealed portion was then cut to a width of 15mm. See Figure 6 for the outline of the sample shape.

[0104] (Initial heat seal strength) The seal strength of the prepared samples was measured at room temperature at a speed of 50 mm / min. The results were ranked as follows: A: Burst strength is 25N / 15mm or more B: Burst strength is 20N / 15mm or more and less than 25N / 15mm C: Burst strength is 15N / 15mm or more and less than 20N / 15mm D: Burst strength is less than 15N / 15mm

[0105] (Initial heat seal strength after exposure to hydrogen sulfide) The prepared sample was left to stand at room temperature for 72 hours in an environment with a hydrogen sulfide concentration of 20 ppm, and the seal strength was measured at a speed of 50 mm / min. The results were ranked as follows: A: Burst strength is 25N / 15mm or more B: Burst strength is 20N / 15mm or more and less than 25N / 15mm C: Burst strength is 15N / 15mm or more and less than 20N / 15mm D: Burst strength is less than 15N / 15mm

[0106] (High temperature heat seal strength) The prepared sample was allowed to stand for 5 minutes in a 150°C environment, and then the seal strength was measured in a 150°C environment at a speed of 50 mm / min. The results were ranked as follows: A: Burst strength is 15N / 15mm or more B: Burst strength is 10N / 15mm or more and less than 15N / 15mm C: Burst strength is 5N / 15mm or more and less than 10N / 15mm D: Burst strength is less than 5N / 15mm

[0107] (High temperature heat seal strength after exposure to hydrogen sulfide) The prepared sample was left standing at room temperature for 72 hours in an environment with a hydrogen sulfide concentration of 20 ppm, and then left standing for 5 minutes in an environment at 150°C. After that, the seal strength was measured in an environment at 150°C at a speed of 50 mm / min. The results were ranked as follows: A: Burst strength is 15N / 15mm or more B: Burst strength is 10N / 15mm or more and less than 15N / 15mm C: Burst strength is 5N / 15mm or more and less than 10N / 15mm D: Burst strength is less than 5N / 15mm

[0108] The resin compositions and evaluation results for Examples 1 to 28 and Comparative Examples 1 to 4, each of which uses samples with different resin compositions, are summarized in Table 1. In each evaluation, samples that do not receive a D rank rating are considered to have excellent overall quality.

[0109] [Table 1]

[0110] As can be seen from the results shown in Table 1, it was confirmed that each of the Examples of the present invention provided excellent quality under all four conditions, namely, initial heat seal strength, initial heat seal strength after exposure to hydrogen sulfide, high-temperature heat seal strength, and high-temperature heat seal strength after exposure to hydrogen sulfide. Meanwhile, in each of the Comparative Examples, for example, Comparative Examples 1 and 2, which consisted only of polyolefin resin, had poor high-temperature sealability, and Comparative Example 3, which consisted only of polyester resin, and Comparative Example 4, which consisted only of polyamide resin, had poor initial seal strength and were of insufficient quality. [Explanation of symbols]

[0111] 10...Exterior materials 11...Base material layer 12...Adhesive layer 13. Barrier layer 14. Corrosion prevention treatment layer 16. Sealant layer 16a First resin layer 16b Second resin layer 16c Third resin layer 17...Adhesive layer 30...Metal terminal 40 Terminal film 40a, 40b, 40c...Resin layer 50....Electricity storage device main body 100 Energy storage device

Claims

1. A terminal film for an electricity storage device that is arranged so as to cover an outer peripheral surface of a part of a metal terminal that is electrically connected to an electricity storage device main body that constitutes an electricity storage device, An unmodified polyolefin resin; a second resin which is at least one resin selected from polyester, polyamide, polycarbonate, and polyphenylene ether; a modified polyolefin resin modified with a polar group capable of reacting with the second resin; A terminal film for an electricity storage device, comprising a first resin layer made of a resin composition comprising:

2. A terminal film for an electricity storage device as described in claim 1, wherein the total content of the unmodified polyolefin resin and the modified polyolefin resin in the resin composition is 10 mass% to 80 mass% based on the total mass of the resin composition.

3. 3. The terminal film for an electricity storage device according to claim 1, wherein the modified polyolefin resin is a maleic anhydride-modified polyolefin resin.

4. A terminal film for an electricity storage device described in any one of claims 1 to 3, wherein the polyester or polyamide has a crystallinity of 10% or more and less than 70% when heat-sealed under conditions of 260°C, 0.5 MPa, and 3 seconds and then cooled to room temperature.

5. A terminal film for an electricity storage device described in any one of claims 1 to 4, which contains a hydrogen sulfide adsorption material.

6. A terminal film for an electricity storage device described in any one of claims 1 to 5, wherein when the total amount of the unmodified polyolefin resin, the second resin and the modified polyolefin resin in the resin composition is 100 parts by mass, the content of the second resin is 20 parts by mass to 90 parts by mass.

7. A terminal film for an electricity storage device described in any one of claims 1 to 6, wherein the content of the modified polyolefin resin is 0.5 parts by mass to 40 parts by mass when the total amount of the unmodified polyolefin resin and the modified polyolefin resin in the resin composition is 100 parts by mass.

8. A terminal film for an electricity storage device described in any one of claims 1 to 7, which has a single layer structure consisting of the first resin layer.

9. A terminal film for an electricity storage device described in any one of claims 1 to 7, which has a multilayer structure having at least the first resin layer.

10. A terminal film for an electricity storage device as described in claim 9, further comprising a second resin layer consisting of the resin composition.

11. A terminal film for an electricity storage device as described in claim 10, wherein one outermost surface is constituted by the first resin layer, the other outermost surface is constituted by the second resin layer, and further comprising an intermediate layer provided between the first resin layer and the second resin layer.

12. A terminal film for an electricity storage device as described in Claim 11, wherein the first resin layer and the second resin layer are made of a resin composition having the same composition.

Citation Information

Patent Citations

  • Manufacturing method of lead wire member with sealing film

    JP2008004316A

  • Electrical parts, nonaqueous electrolyte battery, and lead wire and sealing container used for them

    JP2009259739A

  • Gripping method for lead conductor, manufacturing method for lead member, and fixing jig used for manufacture

    JP2010218766A

  • External facing material for power storage device

    JP2013101765A

  • Laminated body for sulfide gas adsorption

    JP2015089644A