Decorative film and decorative molded body

A decorative film with a block copolymer and terpene resin adhesive layer addresses adhesion issues with polypropylene resin, ensuring strong bonding during vacuum or reduced pressure heating, enhancing decorative molding efficiency.

JP7585618B2Active Publication Date: 2024-11-19OJI HLDG CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020062896
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-11-19
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Conventional decorative films fail to exhibit sufficient adhesion to polypropylene resin adherends during vacuum or reduced pressure heating conditions, leading to peeling issues.

Method used

A decorative film with an adhesive layer containing a block copolymer composed of an isopentane-derived structure and a terpene resin, which enhances adhesion to polypropylene resin under vacuum or reduced pressure heating conditions.

Benefits of technology

The decorative film achieves excellent adhesion to polypropylene resin adherends, improving interlayer bonding and design freedom for decorative molding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585618000008
    Figure 0007585618000008
  • Figure 0007585618000009
    Figure 0007585618000009
  • Figure 0007585618000001
    Figure 0007585618000001
Patent Text Reader

Abstract

To provide a decorative film which exhibits excellent adhesiveness to adherends including a polypropylene resin when a decoration molding is performed under vacuum-heating conditions or under reduced pressure-heating conditions.SOLUTION: This invention relates to a decorative film including a decorative layer and an adhesive layer, wherein the adhesive layer comprises: a block copolymer including a block formed from an isopentane-derived structure; and a terpene-based resin. The decorative film is used for decoration molding under vacuum-heating conditions or under reduced pressure-heating conditions. This invention further relates to a decorated molded object obtained by applying the decorative film to an adherend including a polypropylene resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative film and a decorated molded article. [Background technology]

[0002] Conventionally, when protecting or decorating the surfaces of automobile interior and exterior parts, home appliance parts, building material parts, etc., paint was applied to the surface of the molded body by spray painting or the like after processing the molded body by injection molding or vacuum molding, and then dried and heated to harden. However, this type of painting has problems such as the emission of volatile organic solvents that worsens the work environment, the need for separate work processes and production equipment for each molded part, and the need to apply multiple coats of paint, which results in poor paint yield and low productivity.

[0003] In recent years, resin molded bodies have been increasingly used as molded bodies for the purpose of reducing the weight of automobile interior and exterior parts, home appliance parts, building material parts, etc. Spray painting is often not suitable for decorating resin molded bodies, and various methods have been developed to decorate the surface of resin molded bodies. Among them, the method of obtaining a decorated molded body by decorating the outermost surface of a molded body with a decorative film has the advantage of having a higher degree of freedom in design and superior productivity compared to the method of applying or printing on the surface using paint or the like. In addition, the decoration method using a decorative film can decorate the surface of a molded body having three-dimensional unevenness, and is therefore used for various purposes.

[0004] For example, Patent Document 1 discloses a laminate for decorative molding having a base layer and an adhesive layer, the adhesive layer having a silicone-based adhesive layer and an acrylic-based adhesive layer. Patent Document 2 discloses a sheet for vacuum molding having an adhesive layer on the lower surface of a surface film. In this case, the adhesive layer is made of a thermoplastic saturated copolymer polyester resin mixed with 1.5 to 2.5 equivalents of polyisocyanate and cured. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-154410 A [Patent Document 2] JP 2010-120209 A Summary of the Invention [Problem to be solved by the invention]

[0006] In a decorative molding, it is naturally required that the adherend and the decorative film are sufficiently adhered to each other and do not easily peel off. However, when decorative molding is performed under vacuum heating conditions or reduced pressure heating conditions, and when a polypropylene resin material is used as the adherend, there is a problem that the adhesiveness of the decorative film to the adherend is not sufficiently exhibited when a conventional adhesive sheet for decorative molding (decorative film) is used.

[0007] In order to solve these problems of the conventional technology, the inventors have conducted research with the aim of providing a decorative film that exhibits excellent adhesion to an adherend containing a polypropylene resin when decorative molding is performed under vacuum heating conditions or reduced pressure heating conditions. [Means for solving the problem]

[0008] As a result of intensive research to solve the above problems, the inventors have discovered that in a decorative film having a decorative layer and an adhesive layer, by blending a block copolymer containing a block composed of an isopentane-derived structure and a terpene resin in the adhesive layer, a decorative film can be obtained that exhibits excellent adhesion to an adherend containing a polypropylene resin when decorative molding is performed under vacuum heating conditions or reduced pressure heating conditions. Specifically, the present invention has the following configuration.

[0009] [1] A decorative film having a decorative layer and an adhesive layer, The adhesive layer contains a block copolymer including a block composed of an isopentane-derived structure and a terpene resin, A decorative film for decorative molding under vacuum heating conditions or reduced pressure heating conditions. [2] Block copolymers are The decorative film according to [1], which is a block copolymer including a block composed of an isopentane-derived structure and a block composed of a styrene-based polymer. [3] The terpene resin is at least one selected from the group consisting of terpene resins, aromatic modified terpene resins, and terpene phenol resins; The softening point of the terpene resin is 60 to 130°C. The decorative film according to [1] or [2], wherein the terpene resin has a number average molecular weight of 300 to 1,500. [4] The decorative film according to any one of [1] to [3], wherein the content of the terpene resin is 40 to 200 parts by mass based on 100 parts by mass of the block copolymer. [5] The decorative film according to any one of [1] to [4], wherein the adhesive layer has a thickness of 0.5 to 20 μm. [6] A decorated molded article obtained by laminating the decorative film according to any one of [1] to [5] to an adherend containing a polypropylene resin. [7] The decorative molded article according to [6], which is for use as an automobile part, an electronic device, or a building material. Effect of the Invention

[0010] According to the present invention, when decorative molding is performed under vacuum heating conditions or reduced pressure heating conditions, a decorative film that exhibits excellent adhesion to an adherend containing a polypropylene resin can be obtained. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a decorative film. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of the configuration of the decorative molded body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits.

[0013] (Decorative film) The present invention relates to a decorative film having a decorative layer and an adhesive layer, which is for decorative molding under vacuum heating conditions or reduced pressure heating conditions. Here, the adhesive layer contains a block copolymer containing a block composed of an isopentane-derived structure and a terpene resin. Since the decorative film of the present invention has the above-mentioned configuration, when decorative molding is performed under vacuum heating conditions or reduced pressure heating conditions, it exhibits excellent adhesion to an adherend containing a polypropylene resin. Therefore, the decorative film of the present invention is preferably used for bonding to an adherend containing a polypropylene resin as a main component.

[0014] Conventionally, polycarbonate resins and ABS resins have been used as the adherends of decorative molded bodies. For this reason, the specific configuration of decorative films for decorating adherends containing polypropylene resin as the main component has not been fully studied. Therefore, the present inventors have conducted intensive studies on decorative molding of adherends containing polypropylene resin as the main component under vacuum heating conditions or reduced pressure heating conditions. As a result, the present inventors have succeeded in obtaining a decorative film that exhibits excellent adhesion to adherends containing polypropylene resin as the main component by providing an adhesive layer in the decorative film that contains a block copolymer containing a block composed of an isopentane-derived structure and a terpene resin.

[0015] Fig. 1 is a cross-sectional view illustrating an example of the configuration of the decorative film of the present invention. As shown in Fig. 1, the decorative film 30 has a decorative layer 21 and an adhesive layer 11. In the decorative film 30, another layer may be provided between the decorative layer 21 and the adhesive layer 11, but in this embodiment, it is preferable that the decorative layer 21 and the adhesive layer 11 are laminated so as to be in direct contact with each other.

[0016] The decorative layer 21 may be a single layer, or may be a colored film in which a pigment or dye is kneaded into a substrate. Although the decorative layer 21 is depicted as a single layer in FIG. 1, the decorative layer 21 may have a multilayer structure including at least a substrate and a decorative layer. When the decorative layer 21 includes a substrate and a decorative layer, the decorative layer in the decorative layer 21 is preferably provided on the surface in contact with the adhesive layer 11. The decorative layer may be provided on the outermost layer of the decorative film (the surface opposite to the surface in contact with the adhesive layer 11). In such a case, a functional layer such as a hard coat layer or an anti-reflection layer may be provided on the outermost surface side of the decorative layer in addition to the decorative layer.

[0017] The decorative film of the present invention is for decorative molding under vacuum heating conditions or reduced pressure heating conditions. In this specification, molding under vacuum heating conditions or reduced pressure heating conditions is so-called TOM molding. The TOM molding method includes a step of laminating the decorative film on an adherend under vacuum heating conditions or reduced pressure heating conditions, and a step of pressing the decorative film onto the adherend by an air pressure difference.

[0018] (adhesive layer) The decorative film has an adhesive layer. In the present invention, the adhesive layer may be provided on both sides of the decorative layer, but it is preferable that one adhesive layer is provided on either one side of the decorative layer.

[0019] In this embodiment, the adhesive layer preferably contains a block copolymer and a terpene resin. Here, the block copolymer contains a block composed of an isopentane-derived structure. The content of the terpene resin is preferably 40 parts by mass or more, more preferably 45 parts by mass or more, even more preferably 50 parts by mass or more, and particularly preferably 55 parts by mass or more, relative to 100 parts by mass of the block copolymer. The content of the terpene resin is preferably 200 parts by mass or less, more preferably 180 parts by mass or less, even more preferably 160 parts by mass or less, and particularly preferably 140 parts by mass or less, relative to 100 parts by mass of the block copolymer. By setting the content of the terpene resin within the above range, the interlayer adhesion between the adhesive layer and the polypropylene layer can be increased, and further, the interlayer adhesion between the adhesive layer and the decorative layer can also be increased.

[0020] The total content of the block copolymer and the terpene resin is preferably 50% by mass or more, more preferably 60% by mass or more, based on the total mass of the adhesive layer. The total content of the block copolymer and the terpene resin may be 100% by mass, based on the total mass of the adhesive layer. By setting the total content of the block copolymer and the terpene resin within the above range, the decorative film can exhibit excellent adhesion to an adherend containing a polypropylene resin, and further, the interlayer adhesion between the adhesive layer and the decorative layer can be improved.

[0021] The block copolymer contained in the adhesive layer preferably contains a block composed of an isopentane-derived structure and a block composed of a styrene-based polymer. In this specification, the isopentane-derived structure is the following structure. The block composed of the isopentane-derived structure is a block formed by polymerization of the isopentane-derived structure of the above structure. The isopentane-derived structure is preferably a propylene-ethylene copolymer. [ka]

[0022] The block composed of a styrene-based polymer is preferably a block composed of a styrene polymer or an α-methylstyrene polymer.

[0023] The block copolymer contained in the adhesive layer may contain a block composed of other polymers in addition to the block composed of an isopentane-derived structure and the block composed of a styrene-based polymer. Examples of the block composed of other polymers include a block composed of an ethylene-derived structure and a block composed of a (meth)acrylic acid ester-based polymer.

[0024] In the block copolymer contained in the adhesive layer, when the block composed of the isopentane-derived structure is designated as A and the block composed of the styrene-based polymer is designated as B, the block copolymer may be a diblock copolymer of AB structure, or a triblock copolymer of ABA structure or BAB structure. It may also be a block copolymer having a repeating structure of each block such as -ABAB- structure. Furthermore, as described above, it may be a block copolymer further including a block composed of another polymer.

[0025] The block copolymer contained in the adhesive layer may further have a substituent in its polymer chain. For example, a block copolymer having a substituent with an unsaturated bond as the substituent may be used.

[0026] The block copolymer may be prepared by polymerization using a known method, or a commercially available product may be used, such as Septon 1020, Septon 2002, Septon 4033, or Septon HG252 manufactured by Kuraray Co., Ltd.

[0027] The terpene resin contained in the adhesive layer is preferably at least one selected from the group consisting of terpene resins, aromatic modified terpene resins, and terpene phenol resins. More specifically, examples of the terpene resins include α-pinene polymers, β-pinene polymers, dipentene polymers, and phenol-modified, aromatic modified, hydrogenated, and hydrocarbon modified terpene resins.

[0028] The softening point of the terpene resin is preferably 60° C. or higher, more preferably 65° C. or higher, even more preferably 70° C. or higher, and particularly preferably 75° C. or higher. The softening point of the terpene resin may be 100° C. or higher. The softening point of the terpene resin is preferably 130° C. or lower, and more preferably 125° C. or lower. The softening point of the terpene resin is a value measured using an automatic softening point measuring device (FLEX SCIENTIFIC, EX-719PD4) according to the method described in JIS K2207.

[0029] The number average molecular weight of the terpene resin is preferably 300 or more, more preferably 350 or more, and even more preferably 400 or more. The number average molecular weight of the terpene resin is preferably 1500 or less, more preferably 1400 or less, and even more preferably 1300 or less. The number average molecular weight of the terpene resin is measured by gel permeation chromatography (GPC) and converted using a calibration curve prepared using standard polystyrene with a known molecular weight.

[0030] As the terpene resin, commercially available products may be used, such as YS Resin PX 1150, YS Resin PX 1250, YS Resin TO 125, YS Resin TO 105, YS Polystar T 125, YS Polystar T 80, and YS Polystar G 125, all of which are manufactured by Yasuhara Chemical Co., Ltd.

[0031] The adhesive layer may contain additives in addition to the block copolymer and resin described above, such as antioxidants (or antiaging agents), silane coupling agents, tackifiers other than terpene resins, oil components, softeners, crosslinking agents, pigments, hydrogen abstraction initiators, etc.

[0032] Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, lactone-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, etc. These antioxidants may be used alone or in combination of two or more kinds.

[0033] Examples of the silane coupling agent include mercapto-based silane coupling agents containing a mercapto group, epoxy-based silane coupling agents having an epoxy group, and vinyl-based silane coupling agents having a vinyl group. Among these, it is preferable to use a mercapto-based silane coupling agent in the application of the present invention. Examples of the mercapto-based silane coupling agent include mercaptotrimethoxysilane, mercaptomethyltrimethoxysilane, mercaptomethyltriethoxysilane, triethoxy(2-mercaptoethyl)silane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 4-mercaptobutyltrimethoxysilane, 10-mercaptodecyltriethoxysilane, 11-mercaptoundecyltrimethoxysilane, and 11-mercaptoundecyltriethoxysilane.

[0034] Examples of tackifiers other than terpene resins include petroleum resins such as styrene resins, rosin resins, C5 resins, C9 resins, and C5 / C9 resins.

[0035] As the oil component, paraffin-based or naphthene-based system oils are preferred, and paraffin-based system oils are more preferably used because they are less likely to cause rubber deterioration.

[0036] Examples of the hydrogen abstraction initiator include benzophenone compounds such as methyl benzoylformate and 4-methylbenzophenone.

[0037] The thickness of the adhesive layer is preferably 0.5 μm or more, more preferably 1 μm or more. The thickness of the adhesive layer is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. In this embodiment, it is possible to reduce the thickness of the adhesive layer in this way.

[0038] (Decorative layer) The decorative film has a decorative layer. Here, the decorative layer may be a single-layer colored film in which a pigment or a dye is kneaded into a substrate, or the decorative layer may be a multi-layer film including a substrate and a decorative layer.

[0039] When the decorative layer is a multilayer film including a substrate and a decorative layer, the decorative layer is preferably a layer provided on the surface of the decorative film that is in contact with the adhesive layer. The decorative layer may also be provided on the outermost layer of the decorative film (the surface opposite to the surface in contact with the adhesive layer), and in this case, a functional layer such as a hard coat layer or an anti-reflection layer may be provided on the outermost layer.

[0040] The decorative layer is preferably a printed layer. The printed layer is formed by printing one side of the film-like substrate using an ink mainly composed of, for example, a thermosetting resin or an ultraviolet-curing resin. For printing, known printing methods such as inkjet printing and screen printing can be adopted. Examples of the film-like substrate to be printed include ABS resin (a copolymer of acrylonitrile, butadiene, and styrene), AS resin (a copolymer of acrylonitrile and styrene), acrylic resin, polyethylene terephthalate, polybutylene terephthalate, nylon, polyacetal, polyphenylene oxide, phenolic resin, urea resin, melamine resin, liquid crystal polymer, polytetrafluoroethylene, polyvinylidene fluoride, polysulfone, polyethersulfone, polyacetal, polyetheretherketone, polyphenylene sulfide, polyetherimide, polyamideimide, polycarbonate, polyolefin resin (polyethylene, polypropylene, etc.), polystyrene, and urethane resin. These substrates are preferably ones that can be stretched in a manner that conforms to the adherend during the molding process. In addition, the film-like substrate is usually a transparent film, but a coloring agent such as carbon (graphite) may be blended therein to impart design properties, or the substrate may be a colored layer.

[0041] The decorative layer may further have a surface protective layer or a print protective layer to protect the printed layer. The surface protective layer is preferably a layer disposed on the most exposed surface side of the decorative layer and serves to enhance scratch resistance and weather resistance. For this reason, the surface protective layer is preferably a layer containing a curable resin layer, and more preferably a hard coat layer. Among them, the curable resin is preferably a photocurable resin, and more preferably an ultraviolet curable resin. In this case, the resin composition for forming the surface protective layer preferably contains, for example, a photopolymerization initiator in addition to the ultraviolet curable resin. In addition, when the decorative layer is formed by printing, since it is easily scratched depending on the ink used, a print protective layer such as a hard coat layer may be provided on the ink layer to prevent scratches.

[0042] The surface protective layer may further include fine particles. Examples of the fine particles include inorganic fine particles, and metal oxides are preferred. In addition, the surface protective layer may include a pigment or a dye, if necessary. In addition, the surface protective layer may include additives such as a pigment dispersant, a defoamer, an ultraviolet absorber, HAL, an antioxidant, an antistatic agent, an anti-abrasion agent, and an antiblocking agent, if necessary.

[0043] The decorative layer may further include a separator layer when a protective film or an adhesive layer is present on the outermost layer. The protective film or separator layer is provided to temporarily protect the surface protective layer. For example, it is provided to prevent the surface protective layer or the printed layer from being scratched before use. The protective film is preferably a self-adhesive film made of an ethylene-vinyl acetate copolymer, or a slightly adhesive film in which a urethane-based and / or acrylic-based adhesive layer having removability is laminated on a PET film or the like. The separator layer is preferably configured, for example, by providing a release layer such as silicone on the surface of the above-mentioned base layer. Such a separator layer is peeled off during the manufacturing process or use, and removed from the decorative film or the decorated molded body.

[0044] Examples of the configuration of the surface side layer include the following layer configurations: Note that, in order to bond each layer, an adhesive layer may be provided between each layer, if necessary. (1) Configuration consisting of only a base layer (2) A decorative layer and a surface protective layer are provided in this order. (3) A decorative layer and a base layer are provided in this order. (4) A structure in which a base layer and a decorative layer are provided in this order (5) A decorative layer, a base layer, and a surface protective layer are provided in this order. (6) A configuration in which a protective film is further provided on the outermost surface of the configurations (1) to (5) described above. (7) A configuration in which a pressure-sensitive adhesive layer and a separator layer are further provided on the outermost surface of the configurations (1) to (5) described above.

[0045] When a pressure-sensitive adhesive layer is provided to bond each layer, a known pressure-sensitive adhesive can be used as the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer. Examples of the pressure-sensitive adhesive include natural rubber-based pressure-sensitive adhesives, synthetic rubber-based pressure-sensitive adhesives, acrylic-based pressure-sensitive adhesives, urethane-based pressure-sensitive adhesives, and silicone-based pressure-sensitive adhesives. The pressure-sensitive adhesive may be any of a solvent-based, solventless, emulsion-based, and water-based type.

[0046] (Method of manufacturing decorative film) The method for producing a decorative film of the present invention includes a step of applying an adhesive composition onto a decorative layer, and drying or curing the composition to form an adhesive layer.

[0047] The adhesive composition can be applied by a conventional method. When an adhesive composition prepared by dissolving in a solvent is used, it can be applied by a knife coater or the like, and then the solvent can be dried in a drying oven to form a sheet. On the other hand, when a pressure-sensitive adhesive prepared by a kneading method using heat is used, it can be formed into a sheet by using a hot melt coder that can soften the adhesive composition by heating in advance.

[0048] (Decorative molding) The present invention also relates to a decorated molded body obtained by bonding a decorative film to an adherend containing a polypropylene resin. In the decorated molded body, the adherend and at least the decorative film (or the decorative layer in the case of in-mold molding) are integrated with each other via an adhesive layer, and at least a part of the surface of the adherend is covered with the decorative film (or the decorative layer).

[0049] Fig. 2 is a cross-sectional view illustrating an example of the configuration of a decorated molded body. As shown in Fig. 2, the decorated molded body 100 has a configuration in which a decorative film 30 is laminated on an adherend 50. As shown in Fig. 2, the decorative film 30 has a decorative layer 21 and an adhesive layer 11, and the adhesive layer 11 is directly attached to the adherend 50.

[0050] The adherend contains a polypropylene resin. Here, the adherend contains polypropylene resin as a main component. Specifically, the content of polypropylene resin in the adherend is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The content of polypropylene resin in the adherend may be 100% by mass, and the adherend may be made of polypropylene resin.

[0051] The shape of the polypropylene resin-containing adherend is not particularly limited, and may be a plate-like shape or may have a three-dimensional shape. In addition, the adherend may have an uneven structure on a part of its surface.

[0052] The decorative molded body is preferably for use in automobile parts, electronic devices, or building materials. The present invention may relate to automobile parts, electronic devices, or building materials that include the above-mentioned decorative molded body. Examples of automobile parts include parts such as bodies, bumpers, spoilers, mirrors, wheels, emblems, and interior materials. Examples of electronic devices include electronic devices such as home appliances and liquid crystal display devices such as personal computers. Examples of building materials include furniture and building materials. Furthermore, the adherend may be road materials (e.g., traffic signs, soundproof walls, etc.), tunnel materials (e.g., side wall panels, etc.), musical instruments, containers, office supplies, sporting goods, toys, etc.

[0053] (Method of manufacturing decorated molded body) The method for producing the decorative molded body preferably includes a step of attaching the decorative film to the adherend. The method for producing the decorative molded body preferably includes molding under vacuum heating conditions or reduced pressure heating conditions, and the above-mentioned decorative film is an adhesive sheet suitable for decorative molding under vacuum heating conditions or reduced pressure heating conditions.

[0054] In this specification, molding under vacuum heating conditions or reduced pressure heating conditions is so-called TOM molding. The TOM molding method includes a step of laminating a laminated adhesive sheet for decorative molding onto an adherend under vacuum heating conditions or reduced pressure heating conditions, and a step of pressing the laminated adhesive sheet for decorative molding onto the adherend by an air pressure difference. Furthermore, the TOM molding preferably includes a step of heating the surface of the laminated adhesive sheet for decorative molding to 100°C or more and 180°C or less before the step of pressing the laminated adhesive sheet for decorative molding onto the adherend. By heating to 100°C or more and 180°C or less, the decorative film softens and becomes easier to follow the shape of the adherend. In this case, it is preferable to use an infrared heater for heating.

[0055] In this specification, molding under vacuum heating conditions or reduced pressure heating conditions does not include a method of bonding a laminate and a molded body by using a molded body provided with vacuum holes. Specifically, molding under vacuum heating conditions or reduced pressure heating conditions can be performed by using a "vacuum molding device" described in Japanese Patent No. 3733564. EXAMPLES

[0056] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0057] <Production of Adhesive Composition> Adhesive composition (A-1) An adhesive composition (A-1) was obtained by dissolving 100 parts by mass of a block copolymer (Septon 1020, manufactured by Kuraray Co., Ltd.) having a structure represented by the following structural formula, 60 parts by mass of a terpene resin (YS Resin PX 1150, manufactured by Yasuhara Chemical Co., Ltd., softening point 115°C, number average molecular weight 1000) and 0.6 parts by mass of an antioxidant (IRGANOX1010, manufactured by BASF Co., Ltd.) in toluene to a solids concentration of 30% by mass. [ka]

[0058] Adhesive composition (A-2) An adhesive composition (A-2) having a solid content concentration of 30 mass% was obtained in the same manner as in the preparation of adhesive composition (A-1), except that a resin having a structure represented by the following structural formula (Septon 2002, manufactured by Kuraray Co., Ltd.) was used as the block copolymer. [ka]

[0059] Adhesive composition (A-3) An adhesive composition (A-3) having a solid content concentration of 30 mass% was obtained in the same manner as in the preparation of adhesive composition (A-1), except that a resin having a structure represented by the following structural formula (Septon 4033, manufactured by Kuraray Co., Ltd.) was used as the block copolymer. [ka]

[0060] Adhesive composition (A-4) An adhesive composition (A-4) with a solids concentration of 30 mass% was obtained in the same manner as in the preparation of adhesive composition (A-3), except that the terpene resin (manufactured by Yasuhara Chemical Co., Ltd., YS Resin PX 1150, softening point 115°C, number average molecular weight 1000) was changed to a terpene resin (manufactured by Yasuhara Chemical Co., Ltd., YS Resin PX 800, softening point 80°C, number average molecular weight 700) and the amount added was changed to 100 mass parts.

[0061] Adhesive composition (A-5) An adhesive composition (A-5) having a solid content concentration of 30 mass% was obtained in the same manner as in the preparation of adhesive composition (A-3), except that the terpene resin (Yasuhara Chemical Co., Ltd., YS Resin PX 1150, softening point 115°C, number average molecular weight 1000) was changed to an aromatic modified terpene resin (Yasuhara Chemical Co., Ltd., YS Resin TO 125, softening point 125°C, number average molecular weight 800).

[0062] Adhesive composition (A-6) An adhesive composition (A-6) having a solid content concentration of 30 mass% was obtained in the same manner as in the preparation of adhesive composition (A-3), except that the terpene resin (manufactured by Yasuhara Chemical Co., Ltd., YS Resin PX 1150, softening point 115°C, number average molecular weight 1000) was changed to a terpene phenol resin (manufactured by Yasuhara Chemical Co., Ltd., YS Polystar T 80, softening point 80°C, number average molecular weight 500).

[0063] Adhesive composition (B-1) An adhesive composition (B-1) having a solid content concentration of 30 mass % was obtained in the same manner as in the preparation of adhesive composition (A-1), except that a hydrogenated polybutadiene resin (manufactured by Kuraray Co., Ltd., Septon 8004) having no isopentane-derived structure and represented by the following structural formula was used instead of the block copolymer having an isopentane-derived structure. [ka]

[0064] Adhesive composition (B-2) An adhesive composition (B-2) having a solid content concentration of 30 mass% was obtained in the same manner as the adhesive composition (A-3), except that a styrene-based resin (Mitsui Chemicals, Inc., FTR8100, number average molecular weight 800) was used instead of the terpene resin.

[0065] Adhesive composition (C-1) In a reaction vessel equipped with a stirrer, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, n-butyl acrylate (BA) and 2-hydroxyethyl acrylate (2HEA) were mixed in a mass ratio of 80:20, and 2,2'-azobis(2,4-dimethylvaleronitrile) was dissolved in the solution as a radical polymerization initiator. The solution was heated to 60°C to randomly copolymerize the monomer components to obtain a copolymer solution. 0.11 parts by mass of a xylylene diisocyanate compound (Takenate D-110N, manufactured by Mitsui Chemicals, Inc.) was added as a crosslinking agent to 100 parts by mass of the solid content of the copolymer obtained above, and ethyl acetate was added so that the solid content concentration was 30% by mass to obtain an adhesive composition (C-1).

[0066] Adhesive composition (C-2) Terephthalic acid: isophthalic acid: adipic acid was mixed as an acid component in a mass ratio of 30:30:40, and 1,4-butanediol and 1,6-hexanediol were mixed as a glycol component in a mass ratio of 25:75, and heated in the presence of a catalyst (tetrabutyl titanate) to obtain a thermoplastic saturated copolymer polyester resin. The thermoplastic saturated copolymer polyester resin obtained above was dissolved in a solvent (methyl ethyl ketone) and diluted and stirred to obtain a solution with a solid content concentration of 30% by mass. Next, 2 parts by mass of polyisocyanate (manufactured by Nippon Polyurethane, "Coronate HX" (hexamethylene diisocyanate), solid content concentration 100% by mass) was added to the solution to obtain an adhesive composition (C-2) with respect to 100 parts by mass of the thermoplastic saturated copolymer polyester resin.

[0067] <Preparation of decorative film> Example 1 The adhesive composition (A-1) prepared above was applied to an acrylic film (Kuraray Co., Ltd., Parapure HI grade 75 μm) using a knife coater so that the adhesive layer after drying would be 5 μm thick, and then dried at 100° C. for 3 minutes to volatilize and dry the toluene solvent. Next, a glassine release paper (Oji Tack Co., Ltd., G6W 60 g / m 2 ) was attached to the adhesive layer side with a hand roller to obtain a decorative film with release paper.

[0068] Example 2 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (A-2).

[0069] Example 3 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (A-3).

[0070] Example 4 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (A-4).

[0071] Example 5 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (A-5).

[0072] Example 6 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (A-6).

[0073] Example 7 A decorative film was obtained in the same manner as in Example 3, except that the thickness of the adhesive layer after drying was changed to 1 μm.

[0074] Example 8 A decorative film was obtained in the same manner as in Example 3, except that the thickness of the adhesive layer after drying was changed to 20 μm.

[0075] Comparative Example 1 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (B-1).

[0076] Comparative Example 2 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (B-2).

[0077] Comparative Example 3 A decorative film was obtained in the same manner as in Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (C-1).

[0078] Comparative Example 4 A decorative film was obtained in the same manner as in Comparative Example 1, except that the adhesive composition (A-1) was changed to the adhesive composition (C-2).

[0079] (Adhesion evaluation) <Preparation of Decorative Molded Body> A decorated molded body was produced by the TOM method using the decorative film obtained in each Example and Comparative Example. First, the decorative film from which the release paper had been peeled off and a plate-shaped molded body made of polypropylene resin (Sumitomo Chemical Co., Ltd., Sumikasen (registered trademark)-L GA401) measuring 100 mm x 100 mm x 2.0 mm thick were set in a TOM molding machine (Fuse Vacuum Co., Ltd., NGF molding machine) so that the molded body and the adhesive layer of the decorative film faced each other. The decorative film was laminated on the molded body at 140 ° C. using the TOM molding machine to obtain a decorated molded body. <Evaluation> The decorative molded body prepared above was aged for 24 hours in an environment of 23°C and 50% relative humidity, and then the adhesion between the decorative film and the polypropylene resin adherend was evaluated in accordance with JIS K 5600-5-6. Specifically, an adhesion test was performed using the cross-cut method as follows. First, cut 100 1mm x 1mm grids from the decorative film side with a razor, then pressed cellophane tape (CT28, manufactured by Nichiban Co., Ltd.) from above with a finger to adhere it to the decorative film and then peel it off. If the decorative film was not peeled off in all of the 100 squares, it was scored as 100 / 100, and if the decorative film was peeled off in all squares, it was scored as 0 / 100. The number of squares where the decorative film was not peeled off was counted and the adhesion of the decorative film was evaluated according to the following evaluation criteria. A:80 / 100~100 / 100 B:50 / 100~79 / 100 C:0 / 100~49 / 100

[0080] [Table 1]

[0081] [Table 2]

[0082] The decorative films obtained in the Examples showed good adhesion to polypropylene resin adherends, whereas the decorative films obtained in the Comparative Examples showed poor adhesion to polypropylene resin adherends. [Explanation of symbols]

[0083] 21 Decorative layer 11 Adhesive layer 30 Decorative film 50 Adherent 100 Decorative molding

Claims

1. A decorative film having a decorative layer and an adhesive layer, The adhesive layer contains a block copolymer including a block composed of an isopentane-derived structure and a terpene resin as a tackifier, The terpene resin is a terpene resin or an aromatic modified terpene resin, The content of the tackifier is 40 to 100 parts by mass based on 100 parts by mass of the block copolymer, A decorative film for decorative molding under vacuum heating conditions or reduced pressure heating conditions.

2. The block copolymer is The decorative film according to claim 1 , which is a block copolymer comprising a block composed of an isopentane-derived structure and a block composed of a styrene-based polymer.

3. The softening point of the terpene resin is 60 to 130° C. The decorative film according to claim 1 or 2, wherein the terpene resin has a number average molecular weight of 300 to 1,500.

4. The decorative film according to any one of claims 1 to 3, wherein the adhesive layer has a thickness of 0.5 to 20 µm.

5. A decorated molded article obtained by laminating the decorative film according to any one of claims 1 to 4 to an adherend containing a polypropylene resin.

6. The decorated molded article according to claim 5 , which is used for an automobile part, an electronic device, or a building material.

Citation Information

Patent Citations

  • Easy-disassembly hot-melt composition

    JP2008127473A

  • Sheet for vacuum forming

    JP2010120209A

  • Manufacturing method of modified cellulose fiber, manufacturing method of rein composition and manufacturing method of rubber composition

    JP2017115023A

  • Laminated body for decoration, decorative molded body, and method for producing decorative molded body

    JP2017154410A

  • Multilayered film and molding

    JP2018150447A