Resin solution, flexible electronic device and method for producing same

A resin solution with inorganic fillers enhances UV absorption in polyimide films, facilitating easy peeling from glass substrates and reducing laser energy needs, ensuring device integrity in flexible electronics.

JP7585637B2Active Publication Date: 2024-11-19TOYOBO CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020121444
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-15
Publication Date
2024-11-19
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

The challenge of peeling polyimide films from glass substrates in flexible electronic devices without damaging the devices due to increased transparency and reduced UV absorption, leading to excessive laser energy requirements or device malfunction.

Method used

A resin solution containing specific amounts of inorganic fillers like zinc oxide and zirconium oxide particles is used to create a polyimide film with high UV shielding properties, allowing for easy laser peeling by absorbing UV light at the interface without direct impact on the device.

Benefits of technology

The solution enables easy peeling of polyimide films from glass substrates with minimal device damage, maintaining high transparency and flexibility while reducing laser energy requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585637000001
    Figure 0007585637000001
  • Figure 0007585637000002
    Figure 0007585637000002
  • Figure 0007585637000003
    Figure 0007585637000003
Patent Text Reader

Abstract

To provide a resin solution which achieves a resin film having high colorless transparency and high ultraviolet absorptivity, a method for manufacturing a flexible electronic device using the same, and a flexible electronic device.SOLUTION: A resin solution is obtained by blending at least one resin selected from the group consisting of a polyimide resin, a polyamide imide resin and a polyamic acid resin, a solvent, zinc oxide particles and / or zinc sulfide particles, and zirconium oxide particles and / or zirconium silicate particles.EFFECT: A resin film obtained from the resin solution can suppress a total addition amount by energizing ultraviolet absorption capability of a zinc oxide with a light diffusion effect by a zirconium compound, and accordingly suppresses whitening of a film, maintains high transparency, and has UV laser absorption performance. Therefore, a product having process suitability can be obtained by using the film as a member of a flexible electronic device.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin solution for obtaining a colorless and highly transparent polyimide-based resin film, a flexible electronic device using the resin film as a member, and a method for producing the same. [Background technology]

[0002] Polyimide films have excellent heat resistance, good mechanical properties, and are widely used in the electrical and electronic fields as flexible materials. However, because ordinary polyimide films are colored yellowish brown, they cannot be used in areas that require light transmission, such as display devices. On the other hand, display devices are becoming thinner and lighter, and more flexible. For this reason, attempts are being made to change the substrate material from glass to flexible polymer film substrates, but colored polyimide films cannot be used as substrate materials for liquid crystal displays, which display by turning light transmission on and off, and can only be used in a few areas, such as peripheral circuits such as TAB and COF that are equipped with the display device's driver circuits, and the back side of reflective display or self-luminous display devices.

[0003] In light of this background, the development of colorless and transparent polyimide films is underway. Representative examples include attempts to develop colorless and transparent polyimide films using fluorinated polyimide resins, semi-alicyclic or fully alicyclic polyimide resins, etc. (Patent Documents 1 to 3). These films are less colored and have transparency. In addition, a method has been proposed in which these colorless polyimides are heat-treated while being sprayed with a gas having a specified oxygen content (Patent Document 4), which shows that coloring can be further suppressed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-106508 [Patent Document 2] JP 2002-146021 A [Patent Document 3] JP 2002-348374 A [Patent Document 4] WO2008 / 146637 publication Summary of the Invention [Problem to be solved by the invention]

[0005] Colored polyimides absorb light in the ultraviolet range, making them easy to process with a UV laser. However, colorless polyimides, as mentioned above, have low absorbance, so excessive energy is required to process them with a UV laser. In the manufacture of flexible electronic devices such as flexible displays, the mainstream process is to apply a resin solution to a glass substrate, dry it, and if necessary perform a chemical reaction to obtain a resin film on the glass substrate, then form an electronic device on the resin film, and peel the electronic device together with the resin film from the glass substrate to obtain a flexible electronic device. In this process, the final step of peeling the resin film from the glass substrate is a difficult one. That is, it is difficult to control the adhesion between the resin film and the glass substrate, and if the adhesive strength is too strong, the tension applied to the resin film during peeling becomes too large, which may cause the resin film to stretch or bend at the peeling point, resulting in damage to the electronic device. On the other hand, if the adhesive strength is too weak, the film may peel off during the vacuum process or wet process that follows during the electronic device fabrication process. For this reason, a laser peeling method is used in which a UV laser is focused on the bond between the resin film and the glass from the glass side before or during peeling, destroying the bond at the interface and then peeling off the resin film. However, in recent years, the performance of resin films used as components of these flexible electronic devices has improved, achieving high transparency and colorlessness. As a result, the ultraviolet transmittance of the resin films has increased, and as a result, light absorption at the interface between the glass and the resin film has become poor. For this reason, it has become necessary to either increase the output of the UV laser in the laser peeling process or slow down the scanning speed. Slowing the scanning speed means lowering production throughput. Increasing the output of the UV laser naturally increases power consumption, but even more than that, the increased transparency of the resin film layer means that the laser light is irradiated onto the electronic device with little attenuation, which creates a serious problem of adverse effects on the electronic device. [Means for solving the problem]

[0006] The inventors have conducted intensive research to solve these problems, and as a result have discovered that by incorporating a specific amount of a specific inorganic component into a resin solution, it is possible to obtain a resin film having high UV shielding properties while maintaining the colorlessness and transparency of the resulting resin film, that a laser peeling method can be suitably applied, and that the resulting electronic device has high flexibility. That is, the present invention has the following configuration. [1]) A resin solution having the following (1) to (4) as essential components: (1) at least one resin component selected from the group consisting of polyimide resins, polyamideimide resins, and polyamic acid resins; (2) Inorganic filler (a): zinc oxide particles with a content of 625 ppm or more and 20,000 ppm or less relative to the resin component, and / or zinc sulfide particles with a content of 750 ppm or more and 20,000 ppm or less (3) Inorganic filler (b): Zirconium oxide particles with a content of 680 ppm or more and 10,000 ppm or less relative to the resin component, and / or zirconium silicate particles with a content of 1,000 ppm or more and 10,000 ppm or less (4) Solvent [2] The resin solution according to [1], characterized in that the particle diameter of the inorganic filler is 1.5 μm or less. [3] A method for producing a flexible electronic device, comprising the steps of: A step A of applying the resin solution according to the above [1] or [2] to an inorganic substrate; A process B of removing the solvent from the resin solution to obtain a resin film laminate; A step C of forming an electronic device on the resin film; Process D: peeling the electronic device together with the resin film from the inorganic substrate to obtain a flexible electronic device [4] The method for producing a flexible electronic device according to [3], characterized in that when peeling the electronic device together with the resin film from the inorganic substrate, an ultraviolet laser is irradiated from the inorganic substrate side. [5] A flexible electronic device characterized by using a resin film as a member, the resin film comprising the following (1) to (3) as essential components, and having a total light transmittance of 85% or more, a haze value of 10 or less, and an ultraviolet ray transmittance of 50% or less at a wavelength of 350 nm: (1) at least one resin component selected from the group consisting of polyimide resins, polyamideimide resins, and polyamic acid resins; (2) Inorganic filler (a): zinc oxide particles with a content of 625 ppm or more and 20,000 ppm or less relative to the resin component, and / or zinc sulfide particles with a content of 750 ppm or more and 20,000 ppm or less (3) Inorganic filler (b): Zirconium oxide particles with a content of 680 ppm or more and 10,000 ppm or less relative to the resin component, and / or zirconium silicate particles with a content of 1,000 ppm or more and 10,000 ppm or less Effect of the Invention

[0007] The present invention provides a colorless and highly transparent polyimide-based film obtained by using a resin containing a predetermined amount of zinc oxide particles and / or zinc sulfide particles as inorganic fillers, and zirconium oxide particles and / or zirconium silicate particles. It is generally known that zinc oxide has an ultraviolet absorbing effect. Therefore, it is known that adding zinc oxide to a film can provide an ultraviolet shielding effect. However, in order to provide a sufficient ultraviolet shielding effect, a considerable amount of zinc oxide needs to be added. Since the refractive index of zinc oxide is higher than that of polyimide resin, if the amount added is increased, whitening of the film is unavoidable due to the light scattering effect, and the haze value of the film increases, resulting in a decrease in transparency. On the other hand, zirconium oxide (zirconia) has a higher refractive index than zinc oxide, and zirconium silicate (zircon) has a birefringence effect, even though it has a refractive index similar to that of zinc oxide. Therefore, either of them exhibits a light scattering effect with the addition of a small amount, and by combining the two, it is possible to obtain sufficient ultraviolet absorption ability with an addition amount that does not cause significant whitening of the film. Since the light scattering effect of fine particles depends on the particle size, the scattering effect of the target wavelength can be improved by matching the particle size to the wavelength of light to be scattered. Therefore, by matching the ultraviolet absorption range of zinc oxide with the particle size of zirconium oxide and / or zirconium silicate, which are responsible for the light scattering effect, it is possible to obtain even higher ultraviolet absorption ability. As a result, in the laser peeling method, laser light is absorbed at the interface between the glass substrate and the resin film, making peeling easy, and at the same time, the laser is absorbed while being moderately diffused within the film, so the energy of the laser light is softly absorbed by the entire film without directly hitting the back side of the electronic device, minimizing any adverse effects on the electronic device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] <Resin component> In the present invention, the resin component (hereinafter, simply referred to as resin) preferably used is a polyimide resin such as a polyimide resin, a polyamideimide resin, a polyetherimide resin, a polyimidebenzazole resin, or a polyamic acid resin. The polyamic acid resin is a precursor of the polyimide resin. Among them, at least one resin selected from the group consisting of a polyimide resin, a polyamideimide resin, and a polyamic acid resin is preferable.

[0009] <Polyimide resin> The polyimide resin of the present invention, when made into a film having a thickness of 25 μm, preferably has a yellow index of 10 or less. Since transparency is good, the yellow index is preferably 4 or less, more preferably 3.5 or less, and even more preferably 3 or less. Since a lower yellow index is better, the lower limit is not particularly limited, but from an industrial standpoint, it is sufficient that the yellow index is 0.1 or more, and even if the yellow index is 0.2 or more, there is no problem.

[0010] The polyimide resin of the present invention preferably has a total light transmittance of 85% or more when made into a film having a thickness of 25 μm. In order to obtain good transparency, the total light transmittance is preferably 87% or more, more preferably 88% or more, and even more preferably 89% or more. There is no particular upper limit, but from an industrial perspective, it is sufficient that the total light transmittance is 99% or less, and even 98% or less is acceptable.

[0011] The polyimide resin of the present invention, when made into a film having a thickness of 25 μm, preferably has a haze value of 2 or less. More preferably, it is 1.5 or less, even more preferably, it is 1 or less, and even more preferably, it is 0.8 or less. There is no particular lower limit for the haze value, but from an industrial standpoint, a haze value of 0.01 or more is sufficient, and a haze value of 0.05 or more is acceptable.

[0012] The polyimide resin of the present invention preferably has an ultraviolet ray transmittance of 50% or less when made into a film having a thickness of 25 μm. More preferably, it is 45% or less, further preferably, it is 40% or less, and even more preferably, it is 35% or less. There is no particular lower limit to the ultraviolet ray transmittance, but from an industrial standpoint, a transmittance of 1% or more is sufficient, and even 5% or more is acceptable.

[0013] <Chemical composition of polyimide resin> Polyimide is obtained by a condensation polymerization reaction between a tetracarboxylic acid anhydride and a diamine. In the present invention, a polyimide resin having the following composition is preferred. A polyimide resin having a chemical structure obtained by condensation polymerization of a tetracarboxylic acid anhydride containing 70% by mass or more of an alicyclic tetracarboxylic acid anhydride when the total acid components are taken as 100 mol %, and a diamine containing 70% by mass or more of a diamine having an amide bond in the molecule when the total amine components are taken as 100% by mass. A polyimide resin having a chemical structure obtained by condensation polymerization of a tetracarboxylic acid anhydride containing 70% by mass or more of an alicyclic tetracarboxylic acid anhydride and a diamine containing 70% by mass or more of a diamine having a trifluoromethyl group in the molecule, when the total acid component is taken as 100 mol %. A polyimide having a chemical structure obtained from a tetracarboxylic acid anhydride containing 70% by mass or more of an aromatic tetracarboxylic acid anhydride when the total acid components are taken as 100% by mass, and a diamine containing 70% by mass or more of a diamine having at least a sulfur atom in the molecule when the total amine components are taken as 100% by mass. A polyimide resin having a chemical structure obtained by condensation polymerization of a tetracarboxylic anhydride containing 30% by mass or more of a tetracarboxylic acid containing at least a trifluoromethyl group in the molecule, and a diamine containing 70% by mass or more of a diamine having at least a trifluoromethyl group in the molecule, when the total acid component is taken as 100 mol %.

[0014] Examples of the alicyclic tetracarboxylic anhydride in the present invention include 1,2,3,4-cyclobutane tetracarboxylic acid, 1,2,3,4-cyclopentane tetracarboxylic acid, 1,2,3,4-cyclohexane tetracarboxylic acid, 1,2,4,5-cyclohexane tetracarboxylic acid, 3,3',4,4'-bicyclohexyl tetracarboxylic acid, bicyclo[2,2,1]heptane-2,3,5,6-tetracarboxylic acid, bicyclo[2,2,2]octane-2,3,5,6-tetracarboxylic acid, bicyclo[2,2,2]oct-7-ene-2,3,5, 6-Tetracarboxylic acid, tetrahydroanthracene-2,3,6,7-tetracarboxylic acid, tetradecahydro-1,4:5,8:9,10-trimethanoanthracene-2,3,6,7-tetracarboxylic acid, decahydronaphthalene-2,3,6,7-tetracarboxylic acid, decahydro-1,4:5,8-dimethanonaphthalene-2,3,6,7-tetracarboxylic acid, decahydro-1,4-ethano-5,8-methanonaphthalene-2,3,6,7-tetracarboxylic acid, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-no Norbornane-5,5'',6,6''-tetracarboxylic acid (also known as "norbornane-2-spiro-2'-cyclopentanone-5'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid"), methylnorbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-(methylnorbornane)-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclohexanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid (also known as "norbornane-2 -spiro-2'-cyclohexanone-6'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid), methylnorbornane-2-spiro-α-cyclohexanone-α'-spiro-2''-(methylnorbornane)-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclopropanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclobutanone-α'-spiro-2''-norbornane-5,5'',6,6''-Tetracarboxylic acid, norbornane-2-spiro-α-cycloheptanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclooctanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclononanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclodecanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cycloundecanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclododecanone-α'-spiro-2''-norbornane-5,5'' ,6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclotridecanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclotetradecanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-cyclopentadecanone-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, norbornane-2-spiro-α-(methylcyclopentanone)-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, and norbornane-2-spiro-α-(methylcyclohexanone)-α'-spiro-2''-norbornane-5,5'',6,6''-tetracarboxylic acid, and the like tetracarboxylic acids and their acid anhydrides. Among these, dianhydrides having two acid anhydride structures are preferred, and in particular, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclohexanetetracarboxylic dianhydride, and 1,2,4,5-cyclohexanetetracarboxylic dianhydride are preferred, 1,2,3,4-cyclobutanetetracarboxylic dianhydride and 1,2,4,5-cyclohexanetetracarboxylic dianhydride are more preferred, and 1,2,3,4-cyclobutanetetracarboxylic dianhydride is even more preferred. These may be used alone or in combination of two or more.

[0015] Examples of the aromatic tetracarboxylic anhydride in the present invention include 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid, 4,4'-oxydiphthalic acid, bis(1,3-dioxo-1,3-dihydro-2-benzofuran-5-carboxylic acid)1,4-phenylene, bis(1,3-dioxo-1,3-dihydro-2-benzofuran-5-yl)benzene-1,4-dicarboxylate, 4,4'-[4,4'-(3-oxo-1,3-dihydro-2-benzofuran-1,1-diyl)bis(benzene-1,4-diyloxy)]dibenzene-1,2 -dicarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 4,4'-[(3-oxo-1,3-dihydro-2-benzofuran-1,1-diyl)bis(toluene-2,5-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[(3-oxo-1,3-dihydro-2-benzofuran-1,1-diyl)bis(1,4-xylene-2,5-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[4,4'-(3-oxo-1,3-dihydro-2-benzofuran-1,1-diyl)bis(4-isopropyl-toluene 4,4'-[4,4'-(3-oxo-1,3-dihydro-2-benzofuran-1,1-diyl)bis(naphthalene-1,4-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[4,4'-(3H-2,1-benzoxathiol-1,1-dioxide-3,3-diyl)bis(benzene-1,4-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-benzophenonetetracarboxylic acid, 4,4'-[(3H-2,1-benzoxathiol-1, 1-dioxide-3,3-diyl)bis(toluene-2,5-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[(3H-2,1-benzoxathiol-1,1-dioxide-3,3-diyl)bis(1,4-xylene-2,5-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[4,4'-(3H-2,1-benzoxathiol-1,1-dioxide-3,3-diyl)bis(4-isopropyl-toluene-2,5-diyloxy)]dibenzene-1,2-dicarboxylic acid, 4,4'-[4,4'-(3H-2,1-benzoxathiol-1,1-dioxide-3,3-diyl)bis(naphthalene-1,4-diyloxy)]dibenzene-1,2-dicarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, pyromellitic acid, 4,4'-[spiro(xanthene-9,9'-fluorene)-2,6-diylbis(oxycarbonyl)]diphthalic acid, 4,4'-[spiro(xanthene-9,9'-fluorene)-3,6-diylbis(oxycarbonyl)]diphthalic acid, and the like tetracarboxylic acids and their acid anhydrides. The aromatic tetracarboxylic acids may be used alone or in combination of two or more. ,

[0016] In the present invention, in addition to the tetracarboxylic acid anhydride, a tricarboxylic acid or a dicarboxylic acid may be used. Examples of tricarboxylic acids include aromatic tricarboxylic acids such as trimellitic acid, 1,2,5-naphthalene tricarboxylic acid, diphenyl ether-3,3',4'-tricarboxylic acid, and diphenyl sulfone-3,3',4'-tricarboxylic acid, or hydrogenated products of the aromatic tricarboxylic acids such as hexahydrotrimellitic acid, alkylene glycol bistrimellitates such as ethylene glycol bistrimellitate, propylene glycol bistrimellitate, 1,4-butanediol bistrimellitate, and polyethylene glycol bistrimellitate, and monoanhydrides and esterified products thereof. Among these, monoanhydrides having one acid anhydride structure are preferred, and trimellitic anhydride and hexahydrotrimellitic anhydride are particularly preferred. These may be used alone or in combination.

[0017] Examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, and 4,4'-oxydibenzenecarboxylic acid, or hydrogenated products of the aromatic dicarboxylic acids such as 1,6-cyclohexanedicarboxylic acid, oxalic acid, succinic acid, glutaric acid, adipic acid, heptanedioic acid, octanedioic acid, azelaic acid, sebacic acid, undecadioic acid, dodecanedioic acid, 2-methylsuccinic acid, and acid chlorides or esters thereof. Among these, aromatic dicarboxylic acids and hydrogenated products thereof are preferred, and terephthalic acid, 1,6-cyclohexanedicarboxylic acid, and 4,4'-oxydibenzenecarboxylic acid are particularly preferred. The dicarboxylic acids may be used alone or in combination.

[0018] As the diamine having an amide bond in the molecule in the present invention, aromatic diamines and alicyclic amines can be mainly used. Examples of aromatic diamines include 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,4-bis[2-(4-aminophenyl)-2-propyl]benzene, 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene, 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4 -(3-aminophenoxy)phenyl]sulfone, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, m-aminobenzylamine, p-aminobenzylamine, 4-amino-N-(4-aminophenyl)benzamide, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,2'-trifluoromethyl-4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4, 4'-Diaminobenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, bis[4-(4-aminophenoxy)phenyl]methane, 1,1-bis[4-(4-aminophenoxy)phenyl]ethane, 1,2-bis[4-(4-aminophenoxy)phenyl]ethane, 1,1-bis[4-(4-aminophenoxy)phenyl]propane, 1,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,1-bis[4-(4-aminophenoxy)phenyl]butane, 1,3-bis[4-(4-aminophenoxy)phenyl]butane, 1,4-bis[4-(4-aminophenoxy)phenyl]butane, 2,2-bis[4-(4-aminophenoxy)phenyl]butane, 2,3-bis[4-(4-aminophenoxy)phenyl]butane, 2-[4-(4-aminophenoxy)phenyl]-2-[4-(4-aminophenoxy)-3-methylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl] nophenoxy)-3-methylphenyl]propane, 2-[4-(4-aminophenoxy)phenyl]-2-[4-(4-aminophenoxy)-3,5-dimethylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)-3,5-dimethylphenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis( 4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfoxide, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,4- Bis[4-(3-aminophenoxy)benzoyl]benzene, 4,4'-bis[(3-aminophenoxy)benzoyl]benzene, 1,1-bis[4-(3-aminophenoxy)phenyl]propane, 1,3-bis[4-(3-aminophenoxy)phenyl]propane, 3,4'-diaminodiphenyl sulfide, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, bis[4-(3-aminophenoxy)phenyl]methane, 1,1-bis[4-(3-aminophenoxy)phenyl]ethane, 1,2-bis[4-(3-aminophenoxy)phenyl]ethane, bis[4-(3-aminophenoxy)phenyl]sulfoxide, 4,4'-bis[3-(4-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[3-(3-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, bis[4-{4-(4-aminophenoxy)pheno 1,4-bis[4-(4-aminophenoxy)phenoxy-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-aminophenoxy)phenoxy-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-trifluoromethylphenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-fluorophenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-amino-6-methylphenoxy)-α,α-dimethylbenzyl]benzene , 1,3-bis[4-(4-amino-6-cyanophenoxy)-α,α-dimethylbenzyl]benzene, 3,3'-diamino-4,4'-diphenoxybenzophenone, 4,4'-diamino-5,5'-diphenoxybenzophenone, 3,4'-diamino-4,5'-diphenoxybenzophenone, 3,3'-diamino-4-phenoxybenzophenone, 4,4'-diamino-5-phenoxybenzophenone, 3,4'-diamino-4-phenoxybenzophenone, 3,4'-diamino-5'-phenoxybenzophenone, 3,3'-diamino-4, 4'-Diamino-5,5'-diamino-diamino-4 ...3-bis(4-amino-5-phenoxybenzoyl)benzene, 1,4-bis(4-amino-5-phenoxybenzoyl)benzene, 1,3-bis(3-amino-4-biphenoxybenzoyl)benzene, 1,4-bis(3-amino-4-biphenoxybenzoyl)benzene, 1,3-bis(4-amino-5-biphenoxybenzoyl)benzene, 1,4-bis(4-amino-5-biphenoxybenzoyl)benzene, 2,6-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzonitrile, 4 ,4'-[9H-fluorene-9,9-diyl]bisaniline (also known as "9,9-bis(4-aminophenyl)fluorene"), spiro(xanthene-9,9'-fluorene)-2,6-diylbis(oxycarbonyl)]bisaniline, 4,4'-[spiro(xanthene-9,9'-fluorene)-2,6-diylbis(oxycarbonyl)]bisaniline, 4,4'-[spiro(xanthene-9,9'-fluorene)-3,6-diylbis(oxycarbonyl)]bisaniline, 5-amino-2-(p-aminophenyl)fluorene nyl)benzoxazole, 6-amino-2-(p-aminophenyl)benzoxazole, 5-amino-2-(m-aminophenyl)benzoxazole, 6-amino-2-(m-aminophenyl)benzoxazole, 2,2'-p-phenylenebis(5-aminobenzoxazole), 2,2'-p-phenylenebis(6-aminobenzoxazole), 1-(5-aminobenzoxazolo)-4-(6-aminobenzoxazolo)benzene, 2,6-(4,4'-diaminodiphenyl)benzo[1,2-d: 5,4-d']bisoxazole, 2,6-(4,4'-diaminodiphenyl)benzo[1,2-d:4,5-d']bisoxazole, 2,6-(3,4'-diaminodiphenyl)benzo[1,2-d:5,4-d']bisoxazole, 2,6-(3,4'-diaminodiphenyl)benzo[1,2-d:4,5-d']bisoxazole, 2,6-(3,3'-diaminodiphenyl)benzo[1,2-d:5,4-d']bisoxazole, 2,6-(3,3'-diaminodiphenyl)benzo[1,2-d:4,5-d']bisoxazole and the like. In addition, some or all of the hydrogen atoms on the aromatic ring of the aromatic diamine may be substituted with halogen atoms, alkyl or alkoxy groups having 1 to 3 carbon atoms, or cyano groups, and further, some or all of the hydrogen atoms of the alkyl or alkoxy groups having 1 to 3 carbon atoms may be substituted with halogen atoms.

[0019] Examples of alicyclic diamines include 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 4,4'-methylenebis(2,6-dimethylcyclohexylamine), 9,10-bis(4-aminophenyl)adenine, and dimethyl 2,4-bis(4-aminophenyl)cyclobutane-1,3-dicarboxylate.

[0020] As the diamine having an amide bond in the molecule, 4-amino-N-(4-aminophenyl)benzamide is preferable. The diamine having an amide bond is preferably used in an amount of 70 mass % or more, more preferably 80 mass % or more, and further preferably 90 mass % or more of the total diamines. As the diamine having a trifluoromethyl group, 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl, 1,4-bis(4-amino-2-trifluoromethylphenoxy)benzene, and 2,2'-trifluoromethyl-4,4'-diaminodiphenyl ether are preferred. When using these diamine compounds having a fluorine atom in the molecule, particularly diamines having a trifluoromethyl group in the molecule, the amount used is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more of the total diamines.

[0021] <Solvent> The solvent used in the present invention is not limited as long as it dissolves the polyimide resin, and more preferably dissolves both the monomers that are the raw materials for the polyimide resin and the polyamic acid that is produced.Although not particularly limited, polar organic solvents are preferred, such as N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphoric amide, ethyl cellosolve acetate, diethylene glycol dimethyl ether, sulfolane, halogenated phenols, etc. In addition, in the case of polyimide resins with good solubility, general-purpose solvents such as methyl ethyl ketone, methyl butyl ketone, toluene, xylene, ethyl acetate, butyl acetate, alcohols, etc. can be used. These solvents can be used alone or in combination. The amount of the solvent used may be an amount sufficient to dissolve the target substance (resin component), and a specific amount used is such that the mass of the resin component in the solution in which the resin component is dissolved is usually 5 to 40 mass%, preferably 10 to 30 mass%.

[0022] <Inorganic filler> The zinc oxide used as the inorganic filler (a) in the present invention is an oxide of zinc represented by the chemical formula ZnO, and is also called zinc white or zinc oxide. The zinc oxide is contained in the polyimide film in a particulate state. The content is 625 ppm or more, preferably 800 ppm or more, more preferably 1200 ppm or more, and 20000 ppm or less, preferably 12000 ppm or less, and even more preferably 6000 ppm or less, based on the mass of the polyimide resin. Here, the unit ppm of the zinc oxide content is a unit of mass conversion (mg / kg). Specific examples of commercially available zinc oxide particles include ZnO-350, ZnO-510, ZnO-610, and ZnO-650 (manufactured by Sumitomo Osaka Cement Co., Ltd.), MZ-300, MZY-303S, MZ-306X, MZ-500, MZY-505S, MZY-510M3S, MZ-506X, and MZ-510HPSX (manufactured by Teika Co., Ltd.), XZ-F series, XZ-100P, FINEX-30, and FINEX-30S-L. Examples include P2, FINEX-30S-LPT, FINEX-30W-LP2, FINEX-30W-LPT, FINEX-50, FINEX-50S-LP2, FINEX-50W-LP2, FINEX-50S-LPT, FINEX-50W-LPT, ZINCA-20, fine zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd.), F-1, F-2 (manufactured by Hakusui Tech Co., Ltd.), FZO-50 (manufactured by Ishihara Sangyo Kaisha, Ltd.), etc. These zinc oxides may be used alone or in combination of two or more.

[0023] The zinc sulfide used as the inorganic filler (a) in the present invention is a zinc sulfide represented by the chemical formula ZnS. The content of the zinc sulfide particles is 750 ppm or more, preferably 900 ppm or more, more preferably 1200 ppm or more, and 20000 ppm or less, preferably 12000 ppm or less, and more preferably 6000 ppm or less, based on the mass of the polyimide resin. Here, the unit ppm of the zinc sulfide content is a unit of mass conversion (mg / kg). In the present invention, it is essential that either zinc oxide particles or zinc sulfide particles, or both, are contained in the polyimide film. When both zinc oxide particles and zinc sulfide particles are used, it is preferable to adjust the total of both to be in the range of 750 ppm or more and 20,000 ppm or less. If the amount of zinc oxide particles or zinc sulfide particles exceeds this range, the whitening of the film becomes unnecessarily large and the haze value may increase, and if it does not meet this range, the ultraviolet ray absorption effect may be insufficient. The above-mentioned predetermined range is a range in which sufficient ultraviolet ray absorption ability (ultraviolet ray shielding ability) and high visible light transmittance (colorlessness, transparency) can be achieved at the same time by using the zinc oxide particles or zinc sulfide particles in combination with the zirconium oxide or zirconium silicate described later.

[0024] The zirconium oxide used as the inorganic filler (b) in the present invention has the chemical formula ZrO 2 Zirconium oxide is an oxide of zirconium represented by the formula (1) and is also called zirconia. Zirconium oxide is contained in the polyimide film in a particulate state. The content is 680 ppm or more, preferably 900 ppm or more, more preferably 1200 ppm or more, and 10000 ppm or less, preferably 12000 ppm or less, and further preferably 6000 ppm or less, based on the mass of the polyimide resin. Here, the unit ppm of the zirconium oxide content is a unit of mass conversion (mg / kg). The zirconium silicate used as the inorganic filler (b) in the present invention has the chemical formula ZrSiO 4 , or ZrO 2 SiO 2 It is a silicate of zirconium represented by the formula (1) and is also called zircon. The content of zirconium silicate is 1000 ppm or more, preferably 1200 ppm or more, more preferably 2000 ppm or more, and 10000 ppm or less, preferably 12000 ppm or less, and more preferably 6000 ppm or less, based on the mass of the polyimide resin. Here, the unit ppm of the zirconium silicate content is a unit of mass conversion (mg / kg). In the present invention, it is essential that either or both of zirconium oxide particles and zirconium silicate particles are contained in the polyimide film. When both zirconium oxide particles and zirconium silicate particles are used, it is preferable to adjust the total of both to be in the range of 1000 ppm or more and 20000 ppm or less. If the blending amount of zirconium oxide particles and zirconium silicate particles exceeds this range, the whitening of the film becomes unnecessarily negligible and the haze value may increase, and if it does not meet this range, the ultraviolet absorbing ability of zinc oxide or zinc sulfide may not be fully supported. Such a predetermined range is a range that can achieve both sufficient ultraviolet absorbing ability (ultraviolet ray shielding ability) and high transmittance of visible light (colorlessness, transparency). It is known that zirconium contains hafnium, which is also a Group 4 element, as an impurity. The two are difficult to separate because of their very similar chemical properties, so products sold as zirconium compounds generally contain hafnium compounds. In the present invention, if the hafnium content is 5 mass% or less of the total of zirconium and hafnium, the total amount including hafnium will be treated as zirconium.

[0025] The particle size of the inorganic filler is preferably 1.5 μm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. Also, it is preferably 10 nm or more, and more preferably 20 nm or more. By keeping it within the above range, the scattering effect can be improved.

[0026] In addition to zinc oxide, zinc sulfide, zirconium oxide, and zirconium silicate, the resin solution of the present invention may be added with the following fillers to modify the viscoelasticity of the solution and the properties of the resulting resin coating. Fillers that can be used for this purpose include fine particles having an average particle size of about 0.03 μm to 3 μm, and specific examples include titanium oxide, alumina, silica, calcium carbonate, calcium phosphate, calcium hydrogen phosphate, calcium pyrophosphate, magnesium oxide, calcium oxide, and clay minerals.

[0027] <Production method of polyimide resin film and laminate> Generally, polyimide resin films are prepared by reacting tetracarboxylic anhydride with diamine in a solvent to obtain a solution of polyamic acid, which is a polyimide precursor, and then coating the polyamic acid solution on a temporary support, drying, and then chemically converting the amic acid bond to an imide bond to obtain a polyimide resin film. In some cases, polyamic acid is converted to polyimide in a solution to obtain a polyimide solution, which is then coated on a temporary support and dried to obtain a polyimide film. In some cases, the polymer is separated from the polyamic acid solution or polyimide solution by a reprecipitation operation or the like, and redissolved in another solvent to obtain a film using the obtained solution. Polyetherimide resins and polyamideimide resins are easily applicable to this reprecipitation-redissolution process.

[0028] The inorganic filler can be added by adding the inorganic filler in a state where it is dispersed in the solvent before the reaction of the tetracarboxylic anhydride and the diamine in the solvent, or by adding the filler to the polyimide or polyamic acid solution after polymerization. Another example is a method in which a precursor of inorganic particles (a compound that generates predetermined inorganic particles through a process such as decomposition by heating) is added to the solution in advance, and inorganic particles are generated and contained in the film during the process of drying or chemical reaction from amide acid bonds to imide bonds.

[0029] In the present invention, a flexible electronic device can be manufactured by including the following steps. Specifically, a flexible electronic device can be obtained by carrying out the following steps: step A of applying the resin solution of the present invention to a substrate (inorganic substrate) preferably made of an inorganic material; step B of removing the solvent from the resin solution (drying) and, if necessary, performing a conversion reaction from polyamic acid to polyimide to obtain a laminate (resin film laminate) made of a resin film and an inorganic substrate; step C of forming (processing) an electronic device on the resin film of the laminate; and step D of peeling off the electronic device together with the resin film from the inorganic substrate. That is, the resin film obtained from the resin solution of the present invention can be used as a member of a flexible electronic device.

[0030] In the step D, the electronic device may be peeled off from the inorganic substrate together with the resin film, for example, in the following modes (1) and (2). (1) A method in which a laser is irradiated from the inorganic substrate side of the laminate to ablate the interface between the support and the polyimide resin film, thereby peeling off the polyimide resin film. The type of laser used here includes solid (YAG) laser, gas (ultraviolet (UV) excimer) laser, etc., and it is particularly preferable to use a spectrum with a wavelength of 308 nm, etc. (2) A method in which a release layer is formed on the surface of the inorganic substrate before applying a resin solution to the inorganic substrate, and then the resin solution is applied to obtain a structure including a polyimide-based resin film / release layer / inorganic substrate, and the polyimide-based resin film is then peeled off. Examples of the release layer include Parylene (registered trademark, manufactured by Nippon Parylene LLC), a tungsten thin film, a molybdenum thin film, an amorphous silicon thin film, etc. A combination of the release layer formation and laser irradiation is also one of the preferred embodiments.

[0031] The inorganic substrate used in the present invention may be a glass substrate, a silicon wafer, or a metal plate. As the glass substrate, those commercially available for displays are preferred.

[0032] Alternatively, a method can be used in which the resin solution is applied to another substrate, preferably a flexible polymer film or metal foil, dried to a semi-dried film state, i.e., a film containing a solvent and a polymer, or a solvent and a polymer precursor, and then transferred and adhered to an inorganic substrate, followed by final drying or drying and chemical reaction to form a laminate of the polymer film and the inorganic substrate. According to this method, the polyimide resin film and the inorganic substrate are in direct contact with each other. EXAMPLES

[0033] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Note that the various physical properties in the production examples and examples were measured by the following methods.

[0034] <Particle size of filler> The central diameter D obtained from the Shimadzu Corporation laser diffraction type particle size distribution analyzer SALD-2300 50 was taken as the particle size of each filler.

[0035] <Film thickness measurement> The measurement was carried out using a micrometer (Militron 1245D, manufactured by Feinruf Co., Ltd.).

[0036] <Tensile modulus, tensile strength (breaking strength), and breaking elongation> The film was cut into strips of 100 mm x 10 mm in the machine direction (MD) and width direction (TD) during coating to prepare test pieces. Using a tensile tester (Shimadzu Corporation, Autograph (R), model name AG-5000A), the tensile modulus, tensile strength, and elongation at break were measured in both the MD and TD directions at a tensile speed of 50 mm / min and a chuck distance of 40 mm, and the average values ​​of the measured values ​​in the MD and TD directions were calculated.

[0037] <Coefficient of Linear Expansion (CTE)> The film was measured for each dimension in the machine direction (MD) and width direction (TD) at the time of coating under the following conditions, and the expansion / contraction rate / temperature was measured at intervals of 15°C, such as 30°C to 45°C and 45°C to 60°C. This measurement was repeated up to 300°C, and the average value of all measured values ​​was calculated as CTE. Furthermore, the average value of the measured values ​​in the MD and TD directions was calculated. Equipment name: MAC Science TMA4000S Sample length: 20mm Sample width: 2mm Heating start temperature: 25℃ End temperature: 300℃ Heating rate: 5℃ / min Atmosphere: Argon

[0038] <Haze> The haze of the film was measured using a HAZEMETER (NDH5000, manufactured by Nippon Denshoku Co., Ltd.). A D65 lamp was used as the light source. The same measurement was performed three times, and the arithmetic average value was used.

[0039] <Total light transmittance> The total light transmittance (TT) of the film was measured using a HAZEMETER (NDH5000, manufactured by Nippon Denshoku Co., Ltd.).

[0040] <UV transmittance> The transmittance at a wavelength of 350 nm was determined as the ultraviolet transmittance using a spectrophotometer.

[0041] <Yellow Index> Using a color meter (ZE6000, Nippon Denshoku) and a C2 light source, the tristimulus values ​​XYZ of the film were measured according to ASTM D1925, and the yellowness index (YI) was calculated according to the following formula. The same measurement was performed three times, and the arithmetic average value was used. YI=100×(1.28X-1.06Z) / Y

[0042] <Film warping> A film cut into a square measuring 100 mm x 100 mm was used as a test piece, and the test piece was placed on a flat surface at room temperature so that it was concave. The distances from the flat surface to the four corners (h1rt, h2rt, h3rt, h4rt: units in mm) were measured, and the average value was taken as the amount of warping (mm).

[0043] [Production Example 1: Production of Polyamic Acid Solution A (PAA Solution A)] After replacing the inside of a reaction vessel equipped with a nitrogen inlet tube, reflux tube, and stirring rod with nitrogen, 22.73 parts by mass of 4,4'-diaminobenzanilide (DABAN) was added to 201.1 parts by mass of N,N-dimethylacetamide (DMAc) and dissolved, and then 19.32 parts by mass of 1,2,3,4-cyclobutanetetracarboxylic acid dihydrate (CBDA) was added in portions as a solid, and the mixture was stirred at room temperature for 24 hours. After that, 173.1 parts by mass of DMAc was added to dilute the mixture, and a polyamic acid solution A with NV 10% and reduced viscosity 3.10 dl / g was obtained.

[0044] [Production Example 2: Production of Polyamic Acid Solution B (PAA Solution B)] After replacing the atmosphere in a reaction vessel equipped with a nitrogen inlet tube, a reflux tube, and a stirring rod with nitrogen, 32.02 parts by mass of 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl (TFMB) was dissolved in 279.9 parts by mass of N,N-dimethylacetamide (DMAc), and then 9.81 parts by mass of 1,2,3,4-cyclobutanetetracarboxylic acid dihydrate (CBDA) and 15.51 parts by mass of (ODPA) were added in portions as solids, and the mixture was stirred at room temperature for 24 hours. After that, a polyamic acid solution B with a solid content of 17% by mass and a reduced viscosity of 3.60 dl / g was obtained.

[0045] [Production Example 3: Production of Polyimide Solution C (PI Solution C)] In a reaction vessel equipped with a nitrogen inlet tube, a Dean-Stark tube, a reflux tube, a thermometer, and a stirrer, 32.02 parts by mass of 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl (TFMB) and 230 parts by mass of N,N-dimethylacetamide (DMAc) were added and completely dissolved while introducing nitrogen gas, and then 44.42 parts by mass of 4,4'-(2,2-hexafluoroisopropylidene)diphthalic dianhydride (6FDA) was added in portions as a solid, and the mixture was stirred at room temperature for 24 hours. After that, a polyamic acid solution Caa with a solid content of 25% by mass and a reduced end of 1.10 dl / g was obtained. Next, 204 parts by mass of DMAc was added to the obtained polyamic acid solution to dilute the polyamic acid concentration to 15% by mass, and then 1.3 parts by mass of isoquinoline was added as an imidization promoter. Next, while stirring the polyamic acid solution, 12.25 parts by mass of acetic anhydride was slowly dropped as an imidization agent. After that, the mixture was stirred for 24 hours to carry out a chemical imidization reaction, and a polyimide solution Cpi was obtained. Next, 100 parts by mass of the obtained polyimide solution was transferred to a reaction vessel equipped with a stirring device and a stirrer, and 150 parts by mass of methanol was slowly added dropwise while stirring, whereupon precipitation of a powdery solid was confirmed. Thereafter, the powder content of the reaction vessel was dehydrated and filtered, and further washed with methanol, and then vacuum dried at 50° C. for 24 hours, and then heated at 260° C. for an additional 5 hours to obtain polyimide powder Cpd. 20 parts by mass of the obtained polyimide powder was dissolved in 80 parts by mass of DMAc to obtain polyimide solution C.

[0046] [Production Example 4: Production of Polyimide Solution D (PI Solution D)] In a reaction vessel equipped with a nitrogen inlet tube, a Dean-Stark tube, a reflux tube, a thermometer, and a stirrer, 120.5 parts by mass of 4,4'-diaminodiphenylsulfone (4,4'-DDS), 51.6 parts by mass of 3,3'-diaminodiphenylsulfone (3,3'-DDS), and 500 parts by mass of gamma-butyrolactone (GBL) were added while introducing nitrogen gas. Then, 217.1 parts by mass of 4,4'-oxydiphthalic acid non-dihydrate (ODPA), 223 parts by mass of GBL, and 260 parts by mass of toluene were added at room temperature, and the internal temperature was raised to 160°C and heated to reflux at 160°C for 1 hour to perform imidization. After completion of imidization, the temperature was raised to 180°C, and the reaction was continued while removing toluene. After 12 hours of reaction, the oil bath was removed and the temperature was returned to room temperature, and GBL was added so that the solid content was 20% by mass, to obtain polyimide solution D.

[0047] [Production Example 5: Production of Polyamic Acid Solution E (PAA Solution E)] In a reaction vessel equipped with a nitrogen inlet tube, reflux tube, and stirring rod, 161 parts by mass of 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl (TFMB) and 1090 parts by mass of N-methyl-2-pyrrolidone were mixed and stirred under a nitrogen atmosphere to dissolve, and then 112 parts by mass of 1,2,4,5-cyclohexanetetracarboxylic dianhydride were added in portions as solids at room temperature and stirred at room temperature for 12 hours. Next, 400 parts by mass of xylene was added as an azeotropic solvent, and the mixture was heated to 180°C and reacted for 3 hours, and the azeotropic water was separated. After confirming that the outflow of water had ended, the xylene was removed by heating to 190°C over 1 hour to obtain polyamic acid solution E.

[0048] [Production Example 6: Production of Polyamic Acid Solution F (PAA Solution F)] After replacing the inside of a reaction vessel equipped with a nitrogen inlet tube, reflux tube, and stirring rod with nitrogen, 11.36 parts by mass of 4,4'-diaminobenzanilide (DABAN) and 16.01 parts by mass of 2,2'-ditrifluoromethyl-4,4'-diaminobiphenyl (TFMB) were added to 201.1 parts by mass of N,N-dimethylacetamide (DMAc) and completely dissolved. Next, 19.32 parts by mass of 1,2,3,4-cyclobutanetetracarboxylic acid dihydrate (CBDA) was added in portions as a solid, and then stirred at room temperature for 24 hours. Then, 173.1 parts by mass of DMAc was added to dilute the mixture, and a polyamic acid solution F with NV 10% and reduced viscosity 3.10 dl / g was obtained.

[0049] The polyimide solutions and polyamic acid solutions (polyimide precursor solutions) obtained in the Production Examples were formed into films by the following method, and the optical and mechanical properties were measured. The results are shown in Table 1. (Method to obtain a film for measuring physical properties alone) A polyimide solution or polyamic acid solution was applied to the center of a glass plate with sides of 30 cm, approximately 20 cm square, using a bar coater so that the final thickness was 25 ± 2 μm, and the plate was heated at 100 ° C for 30 minutes in an inert oven where dry nitrogen was gently flowing, and after confirming that the amount of residual solvent in the coating film was 40 mass % or less, the plate was heated at 300 ° C for 20 minutes in a muffle furnace substituted with dry nitrogen. The plate was then removed from the muffle furnace, and the edge of the dried coating film (film) was raised with a cutter knife and carefully peeled off from the glass to obtain a film.

[0050] [Table 1]

[0051] [Inorganic filler] The inorganic fillers shown in Table 2 were prepared and used in the Examples and Comparative Examples. The refractive indices listed for reference are typical values ​​listed in chemical handbooks, various physical property tables, and the like.

[0052] [Table 2]

[0053] Example 1 To the polyamic acid solution B obtained in the Production Example, ZnO-65 as an inorganic filler was added in an amount of 2000 ppm by mass relative to the resin component, and ZriO2-10 was added in an amount of 700 ppm by mass relative to the resin component, and the mixture was uniformly dispersed. In an atmosphere conditioned at 25°C and 45%RH, a roll-to-roll comma coater, a continuous drying oven, and a heat treatment oven were used to coat the polyamic acid solution with the inorganic filler dispersed therein on the non-slip surface of a polyethylene terephthalate film A4100 (manufactured by Toyobo Co., Ltd., hereinafter abbreviated as PET film) serving as a temporary support, so that the final film thickness was 18 μm, and then the film was dried in a continuous drying oven at 110°C for 15 minutes to obtain a self-supporting film with a residual solvent content of 23% by mass. The self-supporting film was peeled off from the A4100 film that had been used as the support, passed through a pin tenter having a pin sheet with pins arranged thereon, and the film end was held by inserting it into the pins, and the pin sheet interval was adjusted so that the film would not break and unnecessary slack would not occur, and the film was heated under the conditions of 200°C for 5 minutes, 250°C for 5 minutes, and 300°C for 10 minutes to remove the solvent and proceed with the imidization reaction. Thereafter, the film was cooled to room temperature in 3 minutes, and the poorly flat portions at both ends of the film were cut off with a slitter. The film was then wound up into a roll to obtain a roll of film (Example 1) 580 mm wide and 200 m long. The evaluation results of the obtained film (Example 1) are shown in Table 3.

[0054] (Examples 2 to 17) (Comparative Examples 1 to 7) Similarly, films were produced and evaluated in the same manner as in Example 1 by combining the polyamic acid solutions or polyimide solutions shown in Tables 3, 4, 5, and 6 with inorganic fillers. The results are shown in Tables 3, 4, 5, and 6. If the ultraviolet ray transmittance is 50% or less, the processability with a UV laser is good.

[0055] [Table 3]

[0056] [Table 4]

[0057] [Table 5]

[0058] [Table 6]

[0059] (Examples 18 to 21, Comparative Examples 8 and 9) In the polyimide solution D obtained in the manufacturing example, ZnO-300 and ZrSiO4-700 were uniformly dispersed as inorganic fillers according to Table 7. Next, the polyimide solution in which the fillers were dispersed was applied to a display glass (glass substrate of 370 mm x 470 mm and 0.7 mm thickness: Nippon Electric Glass Co., Ltd. OA10G) with a bar coater so that the final film thickness was 18 μm, and heated at 100 ° C for 20 minutes in an inert oven where dry nitrogen was gently flowed, and after confirming that the amount of residual solvent in the coating film was 40 mass % or less, it was heated at 300 ° C for 15 minutes in a muffle furnace substituted with dry nitrogen, and dried and a conversion reaction from polyamic acid to polyimide was performed, and a laminate consisting of a polyimide film and a glass substrate was obtained. The polyimide film was peeled off from the resulting laminate, and the optical properties were measured. The results are shown in Table 7. In Comparative Examples 8 and 9, the haze value was high and the transparency was low.

[0060] [Table 7]

[0061] (Application Example 1) First, the polyimide film (Example 1) obtained in Example 1 was cut into a rectangle of 360 mm x 460 mm. Next, the film surface was treated with UV / O 3 Using an irradiator (SKR1102N-03 manufactured by LAN Technical), UV / O was applied to the (a) layer side. 3 The UV / O irradiation was performed for 3 minutes. 3 The distance between the lamp and the film was 30 mm. A display glass (glass substrate of 370 mm × 470 mm and 0.7 mm thickness: Nippon Electric Glass Co., Ltd. OA10G) was coated with 3-aminopropyltrimethoxysilane (KBM-903, Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent using a spray coater. The glass substrate was washed with pure water, dried, and then irradiated with UV / O. 3 The specimen was irradiated with an irradiator (SKR1102N-03 manufactured by LAN Technical) for 1 minute and then dry-cleaned. Next, the glass substrate coated with the silane coupling agent was set on a roll laminator equipped with a silicone rubber roller, and first, 500 ml of pure water was dropped onto the silane coupling agent-coated surface using a dropper so that the water spread over the entire substrate, wetting the substrate. The surface-treated surface of the multi-layer polyimide film (Example 25) that had been subjected to the surface treatment was placed on the silane coupling agent-coated surface of the glass substrate, i.e., the surface wetted with pure water, and the glass substrate and the polyimide film were laminated by pressing the polyimide film and the glass substrate while pushing out the pure water between them with a rotating roll from one side of the glass substrate, to obtain a provisional laminate. The laminator used was a laminator manufactured by MCK Corporation with an effective roll width of 650 mm, and the lamination conditions were air source pressure: 0.5 MPa, lamination speed: 50 mm / sec, roll temperature: 22°C, environmental temperature 22°C, and humidity 55% RH. The obtained provisional laminate was heat-treated in a clean oven at 200° C. for 10 minutes to obtain a laminate LB-E01 consisting of a multilayer polyimide film and a glass substrate.

[0062] A tungsten film (75 nm thick) was formed on the polyimide film surface of the obtained laminate LB-E01 by the following process, and then a silicon oxide film (150 nm thick) was laminated as an insulating film without exposure to air. Next, a silicon oxynitride film (100 nm thick) was formed as a base insulating film by plasma CVD, and then an amorphous silicon film (54 nm thick) was laminated without exposure to air.

[0063] The amorphous silicon film thus obtained was used to fabricate TFT elements. First, the amorphous silicon thin film was patterned to form silicon regions of a specified shape, and then a gate insulating film was formed, a gate electrode was formed, source and drain regions were formed by doping the active region, an interlayer insulating film was formed, source and drain electrodes were formed, and an activation process was performed to fabricate a P-channel TFT array. The polyimide film was burned off along the inner side of the outer circumference of the TFT array by a UV-YAG laser, and then the glass substrate was irradiated with a 308 nm line beam of excimer laser at an energy of 85 mJ / cm2. The overlap rate of the line beam was 50%. Next, the cut edge was peeled off by scooping it up with a thin razor blade, and a flexible A3 size TFT array was obtained. Peeling was possible with very little force, and it was possible to peel off the TFT without damaging it. The cut surface by the UV-YAG laser was not disturbed, and no smears or other scattering were observed. The obtained flexible TFT array maintained good characteristics without any deterioration in performance even when wrapped around a 5 mmφ round rod.

[0064] (Application Example 2) Using the laminate LB-E21 obtained in Example 21, an amorphous silicon TFT was formed on the polyimide surface in the same manner as in Application Example 1, the periphery was similarly trimmed with a UV-YAG laser, and an excimer laser was irradiated from the glass substrate side under the same conditions as in Application Example 1, and then peeled off from the glass substrate in the same manner to obtain a flexible TFT array. The obtained flexible TFT array maintained good characteristics without any deterioration in performance even when wrapped around a 5 mmφ round rod.

[0065] (Application Comparison Example 1) The polyimide film ratio 3 obtained in Comparative Example 3 was laminated on a glass substrate in the same manner as in Application Example 1 to obtain a laminate LB-C03. The obtained laminate LB-C03 was used to form a TFT in the same manner, and the periphery was similarly trimmed with a UV-YAG laser, followed by peeling from the glass substrate to obtain a flexible TFT array. Jagged edges were observed on the cut surface by the UV-YAG laser, and about 20% of the TFTs were defective. A detailed analysis of the defective areas revealed fine peeled areas on the glass surface side of the insulating layer in the element. This is presumably due to the influence of the excimer laser light that had passed through the polyimide film. [Industrial Applicability]

[0066] As described above, the polyimide film of the present invention has appropriate UV shielding performance, and maintains high transparency and colorlessness. Furthermore, since it can be formed into a film with the minimum necessary amount of inorganic filler, the film has excellent mechanical properties. The polyimide film of the present invention can be widely used as a component of a flexible and lightweight display device, or as a switching element of a touch panel or the like that requires transparency, or as a pointing device, etc., via a laminate with an inorganic substrate such as a glass substrate.

Claims

1. A resin solution having the following (1) to (4) as essential components: (1) at least one resin component selected from the group consisting of polyimide resins, polyamideimide resins, and polyamic acid resins; (2) Inorganic filler (a): zinc oxide particles in an amount of 625 ppm or more and 20,000 ppm or less relative to the resin component, and / or zinc sulfide particles in an amount of 750 ppm or more and 20,000 ppm or less relative to the resin component. When both zinc oxide particles and zinc sulfide particles are used, the total amount of both is 750 ppm or more and 20,000 ppm or less based on the resin component. (3) Inorganic filler (b): zirconium oxide particles in an amount of 680 ppm to 10,000 ppm, and / or zirconium silicate particles in an amount of 1,000 ppm to 10,000 ppm, based on the resin component When both zirconium oxide particles and zirconium silicate particles are used, the total amount of the two is 1000 ppm or more and 20000 ppm or less based on the resin component. (4) Solvent

2. 2. The resin solution according to claim 1, wherein the particle size of the inorganic filler is 1.5 μm or less.

3. A method for producing a flexible electronic device, comprising the steps of: A step A of applying the resin solution according to claim 1 or 2 to an inorganic substrate; A process B of removing the solvent from the resin solution to obtain a resin film laminate; Step C of forming an electronic device on the resin film; A process D of peeling the electronic device together with the resin film from the inorganic substrate to obtain a flexible electronic device.

4. 4. The method for producing a flexible electronic device according to claim 3, wherein an ultraviolet laser is irradiated from the inorganic substrate side when the electronic device together with the resin film is peeled off from the inorganic substrate.

5. A flexible electronic device comprising, as a member, a resin film having the following essential components (1) to (3), a total light transmittance of 85% or more, a haze value of 10 or less, and an ultraviolet ray transmittance of 50% or less at a wavelength of 350 nm: (1) at least one resin component selected from the group consisting of polyimide resins, polyamideimide resins, and polyamic acid resins; (2) Inorganic filler (a): zinc oxide particles in an amount of 625 ppm or more and 20,000 ppm or less relative to the resin component, and / or zinc sulfide particles in an amount of 750 ppm or more and 20,000 ppm or less relative to the resin component. When both zinc oxide particles and zinc sulfide particles are used, the total amount of both is 750 ppm or more and 20,000 ppm or less based on the resin component. (3) Inorganic filler (b): zirconium oxide particles in an amount of 680 ppm to 10,000 ppm, and / or zirconium silicate particles in an amount of 1,000 ppm to 10,000 ppm, based on the resin component When both zirconium oxide particles and zirconium silicate particles are used, the total amount of both is 1000 ppm or more and 20000 ppm or less based on the resin component.

Citation Information

Patent Citations

  • Heat-resistant optical material having high refractive index and transparency

    JP1992013763A

  • Low refractive indexed, trasnparent polyimide copolymer and their precursor solution, and preparation thereof

    JP1999106508A

  • Soluble and transparent polyimide and method for producing the same

    JP2002146021A

  • Polyamic acid or polyimide and liquid crystalline orientating agent

    JP2002348374A

  • Manufacturing method for display device support substrate polyimide film

    JP2018132768A