Super-junction semiconductor device and method for manufacturing the same

The method simplifies the formation of a superjunction semiconductor device by avoiding complex processes, reducing costs, and enhancing breakdown voltage through controlled impurity implantation and trench formation.

JP7585678B2Active Publication Date: 2024-11-19FUJI ELECTRIC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020157344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-13
Filing Date
2020-09-18
Publication Date
2024-11-19
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

Existing methods for manufacturing superjunction semiconductor devices, such as the multi-stage epitaxial and trench filling methods, face challenges including characteristic fluctuations, high manufacturing costs, and difficulties in maintaining breakdown voltage due to impurity concentration variations and complex processing steps.

Method used

A method for manufacturing a superjunction semiconductor device that involves forming a first semiconductor layer with a lower impurity concentration, creating trenches, and implanting impurities to form parallel pn structures without the need for a CMP process, allowing for easier formation of the SJ structure and reduced costs.

Benefits of technology

The method enables the easy formation of an SJ structure with improved breakdown voltage and reduced manufacturing costs by minimizing impurity concentration variations and simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585678000001
    Figure 0007585678000001
  • Figure 0007585678000002
    Figure 0007585678000002
  • Figure 0007585678000003
    Figure 0007585678000003
Patent Text Reader

Abstract

To provide a superjunction semiconductor device and a method of manufacturing the superjunction semiconductor device, enabling SJ structure to be easily formed and enabling cost reduction.SOLUTION: A method of manufacturing a semiconductor device comprising an active region 30 where current flows and a terminal end structure portion 40, includes first to eighth steps. In the first step, a first semiconductor layer 2 of a first conductivity type is formed on a front face of a semiconductor substrate 1 of the first conductivity type. In the second step, a first trench is formed. In the third step, a second semiconductor layer 27 of the first conductivity type that has an impurity concentration lower than that of the first semiconductor layer 2 is formed on a surface of the first semiconductor layer 2 and in the first trench. In the fourth step, parallel pn structure 20 is formed. In the fifth step, a second trench 18B is formed. In the sixth step, a second semiconductor region 5 of a second conductivity type is formed. In the seventh step, a gate insulating film 7 and a gate electrode 8 are formed. In the eighth step, a first semiconductor region 6 of the first conductivity type is formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a super-junction semiconductor device and a method for manufacturing a super-junction semiconductor device. [Background technology]

[0002] The electrification of automobiles, such as electric vehicles and hybrid vehicles, is becoming more and more common, and there is a strong demand for low loss (low on-resistance) power semiconductors to reduce power consumption. In order to reduce on-resistance in the low voltage class, trench gate MOSFETs (Metal Oxide Semiconductor Field Effect Transistors) are advantageous. Furthermore, a super junction (SJ) structure is effective in reducing the on-resistance of trench gate MOSFETs. The super junction structure consists of a parallel pn region in which n-type column regions and p-type column regions are alternately and repeatedly arranged in a direction parallel to the main surface of a semiconductor substrate. Multi-stage epitaxial growth and trench filling are well-known methods for forming this parallel pn region.

[0003] In the multi-stage epitaxial method, the parallel pn region is formed by the following process. First, an epitaxial layer is formed on the main surface of a semiconductor substrate. Next, impurities that form n-type and p-type regions in the epitaxial layer are ion-implanted. Thereafter, epitaxial layer formation and ion implantation are alternately repeated to obtain a parallel pn region of a predetermined thickness according to the breakdown voltage of the super-junction semiconductor device. Then, a heat treatment is performed to connect the n-type and p-type regions in the depth direction, thereby forming the parallel pn region. (For example, see Patent Document 1 below.)

[0004] In the trench filling method, the parallel pn region is formed by the following steps. First, an n-type epitaxial layer is formed on the main surface of a semiconductor substrate. Next, a trench is formed in this n-type epitaxial layer to form a p-type column region. The region where the trench is not formed becomes the n-type column region. The depth of the trench is set to a depth that provides a predetermined thickness of the parallel pn region according to the breakdown voltage of the super junction semiconductor device. The inside of the trench is then filled with a p-type epitaxial layer to form the parallel pn region (see, for example, Patent Documents 1 and 2 below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-21547 A [Patent Document 2] JP 2004-241768 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the multi-stage epitaxial method, the formation of masks using photolithography technology and ion implantation are repeated for each epitaxial growth, which increases the possibility of characteristic fluctuations due to dimensional and alignment variations. Furthermore, due to the thermal history for each epitaxial growth, mutual diffusion of the parallel pn regions may occur, resulting in concentration compensation in the adjacent n-type column region and p-type column region, which may increase the on-resistance. In addition, the number of processes increases, leading to long lead times and high manufacturing costs.

[0007] In addition, in the trench filling method, when filling the trench with a p-type epitaxial layer, the p-type epitaxial layer formed on the surface of the n-type epitaxial layer that becomes the n-type column region is removed by a CMP (Chemical Mechanical Polisher) process, and then an n-type epitaxial layer is formed on the surface. The reason for removing the p-type epitaxial layer is that if a p-type layer exists in the edge termination region, the breakdown voltage cannot be maintained. For this reason, the trench filling method requires a CMP device, and the characteristics may vary due to variations in the amount of polishing in the CMP process. In addition, the impurity concentration varies more in p-type epitaxial growth than in n-type epitaxial growth, and the impurity concentration must be controlled. Furthermore, due to the junction between the high-concentration p-type epitaxial layer and the n-type drift layer, the gradient of the impurity concentration is large, making it difficult for the depletion layer to spread, and there is a risk of a decrease in the breakdown voltage.

[0008] SUMMARY OF THE PRESENT DISCLOSURE In order to solve the above-mentioned problems associated with the conventional techniques, an object of the present invention is to provide a super junction semiconductor device in which an SJ structure can be easily formed and costs can be reduced, and a method for manufacturing the super junction semiconductor device. [Means for solving the problem]

[0009] In order to solve the above-mentioned problems and achieve the object of the present invention, a method for manufacturing a superjunction semiconductor device according to the present invention is a method for manufacturing a superjunction semiconductor device having an active region through which a current flows, and a termination structure disposed outside the active region and having a breakdown voltage structure surrounding the active region. First, a first step is performed in which a first semiconductor layer of a first conductivity type having a lower impurity concentration than the semiconductor substrate is formed on a front surface of a semiconductor substrate of a first conductivity type. Next, a second step is performed in which a first trench is formed from the surface of the first semiconductor layer. Next, a third step is performed in which a second semiconductor layer of a first conductivity type having a lower impurity concentration than the first semiconductor layer is formed on the surface of the first semiconductor layer and in the first trench. Next, a second conductivity type well region is formed inside the second semiconductor layer by injecting an impurity of a second conductivity type into the second semiconductor layer, and a fourth step is performed in which a parallel pn structure is formed in which a first column of a first conductivity type and a second column of a second conductivity type are repeatedly and alternately arranged in a direction parallel to the front surface, and the upper surface of the second column is in contact with the bottom surface of the well region. Next, a fifth step is performed to form a second trench that penetrates the second semiconductor layer and reaches the first column. Next, a sixth step is performed to form a second semiconductor region of a second conductivity type on the surface of the parallel pn structure in the active region. Next, a seventh step is performed to form a gate insulating film and a gate electrode inside the second trench. Next, an eighth step is performed to selectively form a first semiconductor region of a first conductivity type in the surface layer of the second semiconductor region in the active region.

[0010] In addition, in the method for manufacturing a super junction semiconductor device according to the present invention, in the above-mentioned invention, in the sixth step, the bottom surface of the second semiconductor region is formed to be shallower than the bottom surface of the well region.

[0011] In addition, in the method for manufacturing a super junction semiconductor device according to the present invention, in the above-mentioned invention, in the sixth step, the well region is formed so that its impurity concentration is lower than the impurity concentration of the second semiconductor region.

[0012] In addition, the manufacturing method of a super junction semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, in the fourth step, an impurity having the second conductivity type is implanted into the second semiconductor layer in the first trench.

[0013] In addition, the manufacturing method of a super junction semiconductor device according to the present invention is characterized in that, in the fourth step, an impurity having the second conductivity type is implanted into a surface layer of the second semiconductor layer on the surface of the first semiconductor layer.

[0014] In addition, in the method for manufacturing a super junction semiconductor device according to the present invention, in the above-mentioned invention, in the fourth step, the second columns are also formed in the termination structure portion.

[0015] In addition, in the method for manufacturing a super-junction semiconductor device according to the present invention, the sixth step is carried out before the fifth step.

[0016] In addition, the manufacturing method of a super junction semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, in the fourth step, an impurity having the second conductivity type is implanted only into the second semiconductor layer in the first trench.

[0017] In order to solve the above-mentioned problems and achieve the object of the present invention, the superjunction semiconductor device according to the present invention has the following features. The superjunction semiconductor device has an active region through which a current flows, and a termination structure disposed outside the active region and having a breakdown voltage structure surrounding the active region. A first semiconductor layer of a first conductivity type having a lower impurity concentration than the semiconductor substrate is provided on a front surface of a semiconductor substrate of a first conductivity type. A parallel pn structure is provided inside the first semiconductor layer, in which first columns of a first conductivity type and second columns of a second conductivity type are repeatedly and alternately arranged in a direction parallel to the front surface. A second semiconductor region of a second conductivity type is provided in a surface layer of the parallel pn structure in the active region. A first semiconductor region of a first conductivity type is selectively provided in a surface layer of the second semiconductor region in the active region. A second trench is provided penetrating the first semiconductor region and the second semiconductor region to reach the first column. A gate electrode is provided inside the second trench via a gate insulating film. A well region of a second conductivity type is provided inside the first semiconductor layer, the lower surface of the well region contacts the upper surface of the second column, the bottom surface of the well region is deeper than the bottom surface of the second semiconductor region, and the width of the upper surface of the well region is wider than the width of the second column. The termination structure includes a second semiconductor layer of a first conductivity type having an impurity concentration lower than that of the first semiconductor layer on a surface of the first semiconductor layer, and a resurf region of a second conductivity type having an impurity concentration lower than that of the well region on the surface of the first semiconductor layer of the termination structure, and the bottom surface of the resurf region is located deeper than the boundary between the first semiconductor layer and the second semiconductor layer.

[0018] In addition, in the super-junction semiconductor device according to the present invention, an impurity concentration of the well region is lower than an impurity concentration of the second semiconductor region.

[0019] In addition, in the super-junction semiconductor device according to the present invention, the parallel pn structure is also provided in the termination structure portion.

[0020] In addition, in the superjunction semiconductor device according to the present invention, in the above-mentioned invention, the repetition pitch of the parallel pn structure in the termination structure is narrower than the repetition pitch of the parallel pn structure in the active region.

[0022] In the super junction semiconductor device according to the present invention, in the above-mentioned invention, the well region and the second semiconductor region are in contact with a side wall of the second trench. The super junction semiconductor device according to the present invention is characterized in that, in the above-mentioned invention, the second semiconductor layer is also provided between the well region provided at the outermost part of the termination structure and the RESURF region. The super junction semiconductor device according to the present invention is characterized in that the impurity concentration of the well region is higher than the impurity concentration of the second column.

[0023] According to the above-mentioned invention, the edge termination region includes n - A first conductive type epitaxial layer (a second semiconductor layer of a first conductive type) is provided, - A field oxide film is provided on the surface of the n-type epitaxial layer. - The epitaxial layer provides - Type epitaxial layer and p -- The depletion layer extending from the pn junction with the type RESURF region is called n - By extending the epitaxial layer to the n-type epitaxial layer, the breakdown voltage of the SJ-MOSFET can be improved. - Since the p-type epitaxial layer has a low impurity concentration, it is easy to control the impurity concentration in the p-type base region by ion implantation, and the variation in the gate threshold voltage Vth can be suppressed.

[0024] In addition, a trench for a p-type column is formed in the region that will become the p-type column region, and an n-type drift layer having a lower impurity concentration than the n-type drift layer that will become the n-type column region is formed. - Deposit an n-type epitaxial layer. - The p-type column region 4 and the p-type well region are formed by ion implantation and diffusion of p-type impurities from the surface of the p-type epitaxial layer. This allows the p-type column region to be formed without depositing a p-type epitaxial layer, eliminating the need to remove the p-type epitaxial layer in the edge termination region. In addition, the surface portion in which the p-type column trenches are filled does not require a process of planarizing using a CMP device or the like. This makes it possible to easily form the SJ structure and reduce manufacturing costs. Effect of the Invention

[0025] According to the super junction semiconductor device and the method for manufacturing the super junction semiconductor device of the present invention, an SJ structure can be easily formed, and costs can be reduced. [Brief description of the drawings]

[0026] [Figure 1] 1 is a cross-sectional view showing a structure of an SJ-MOSFET according to an embodiment. [Figure 2A] FIG. 11 is a cross-sectional view showing another structure of the SJ-MOSFET according to the embodiment. [Figure 2B] FIG. 11 is a cross-sectional view showing another structure of the SJ-MOSFET according to the embodiment. [Figure 2C] FIG. 11 is a cross-sectional view showing another structure of the SJ-MOSFET according to the embodiment. [Figure 2D] FIG. 11 is a cross-sectional view showing another structure of the SJ-MOSFET according to the embodiment. [Diagram 3] FIG. 1 is a plan view showing a structure of an SJ-MOSFET according to an embodiment. [Figure 4] 1 is a cross-sectional view (part 1) showing a state during manufacture by a first manufacturing method of an SJ-MOSFET according to an embodiment. FIG. [Diagram 5] 4 is a cross-sectional view (part 2) illustrating a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Figure 6] 11 is a cross-sectional view (part 3) showing a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Figure 7] 4 is a cross-sectional view showing a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment (part 4). FIG. [Figure 8] 5 is a cross-sectional view showing a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment (part 5). FIG. [Figure 9A] 6 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment (part 6). FIG. [Figure 9B] FIG. 7 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 9C]FIG. 8 is a cross-sectional view showing a state during the manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 10A] FIG. 9 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 10B] 10 is a cross-sectional view showing a state during manufacture by a first manufacturing method of an SJ-MOSFET according to an embodiment; FIG. [Figure 10C] FIG. 11 is a cross-sectional view showing a state during manufacture by a first manufacturing method of an SJ-MOSFET according to an embodiment; [Figure 11] FIG. 12 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 12] FIG. 13 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 13] FIG. 14 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment (part 14). [Figure 14] FIG. 15 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 15] FIG. 16 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 16] FIG. 17 is a cross-sectional view showing a state during the manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 17] FIG. 18 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 18] FIG. 19 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 19] FIG. 20 is a cross-sectional view showing a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 20] FIG. 21 is a cross-sectional view showing a state during manufacture by a first manufacturing method of the SJ-MOSFET according to the embodiment. [Figure 21] FIG. 22 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 22] FIG. 23 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 23] FIG. 24 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment (part 24). [Figure 24] FIG. 25 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment (part 25). [Diagram 25] FIG. 26 is a cross-sectional view showing a state during manufacture by the first manufacturing method of the SJ-MOSFET according to the embodiment (part 26). [Figure 26] 1A to 1C are cross-sectional views showing a state during manufacture by a second manufacturing method of an SJ-MOSFET according to an embodiment of the present invention (part 1). [Figure 27] 11 is a cross-sectional view (part 2) showing a state during manufacture by a second manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Figure 28] 11 is a cross-sectional view (part 3) showing a state during manufacture by the second manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Figure 29] 11 is a cross-sectional view (part 4) showing a state during manufacture by a second manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Diagram 30] 5 is a cross-sectional view showing a state during manufacture by a second manufacturing method of the SJ-MOSFET according to the embodiment (part 5). FIG. [Diagram 31] 11 is a cross-sectional view (part 1) showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Diagram 32] 11 is a cross-sectional view (part 2) showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Diagram 33] 11 is a cross-sectional view (part 3) showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Diagram 34] 11 is a cross-sectional view (part 4) showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Diagram 35] 5 is a cross-sectional view showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment (part 5). FIG. [Diagram 36] 11 is a cross-sectional view (part 6) showing a state during manufacture by the third manufacturing method of the SJ-MOSFET according to the embodiment. FIG. [Figure 37] FIG. 7 is a cross-sectional view showing a state during manufacture by the third manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 38] FIG. 8 is a cross-sectional view showing a state during manufacture by the third manufacturing method of the SJ-MOSFET according to the embodiment; [Figure 39] FIG. 9 is a cross-sectional view showing a state during manufacture by a third manufacturing method of the SJ-MOSFET according to the embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] A preferred embodiment of the superjunction semiconductor device and the method of manufacturing the superjunction semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p, respectively. When the notations of n and p including + and - are the same, it indicates that the concentrations are close, but are not necessarily the same. In the following description of the embodiment and the accompanying drawings, the same symbols are attached to similar configurations, and duplicate explanations are omitted.

[0028] (Embodiment) The super-junction semiconductor device according to the present invention will be described by taking an SJ-MOSFET as an example. Fig. 1 is a cross-sectional view showing the structure of an SJ-MOSFET according to an embodiment.

[0029] The SJ-MOSFET (super junction semiconductor device) 50 shown in FIG. 1 is an SJ-MOSFET 50 having a MOS (Metal Oxide Semiconductor) gate on the front surface (the surface on the p-type base region 5 side, which will be described later) of a semiconductor substrate (silicon substrate: semiconductor chip) made of silicon (Si). This SJ-MOSFET 50 has an active region 30 and an edge termination region 40 surrounding the periphery of the active region 30. The active region 30 is a region through which current flows in the on-state. The edge termination region 40 includes a breakdown voltage holding region that relieves the electric field on the front surface side of the semiconductor substrate in the drift region and holds a breakdown voltage. Note that the boundary between the active region 30 and the edge termination region 40 has an n-type transistor, which will be described later, on only one side. + 1 shows only one unit cell (functional unit of an element) in the active region 30, and other unit cells adjacent thereto are omitted. A unit cell is shown from the center of a trench 18B to the center of an adjacent trench 18B.

[0030] n + The n-type semiconductor substrate (first conductivity type semiconductor substrate) 1 is a silicon single crystal substrate doped with, for example, arsenic (As) or phosphorus (P). + An n-type drift layer (first semiconductor layer of a first conductivity type) 2 is provided on a n-type semiconductor substrate 1. The n-type drift layer 2 is + The low-concentration n-type layer has a lower impurity concentration than the n-type semiconductor substrate 1 and is doped with, for example, phosphorus. + The n-type semiconductor substrate 1 and the n-type drift layer 2 together form a semiconductor base. +An n-type buffer layer (not shown) may be disposed between the n-type semiconductor substrate 1 and the n-type drift layer 2, with an impurity concentration lower than that of the n-type drift layer 2. The n-type buffer layer is, for example, a low-concentration n-type layer doped with phosphorus. A MOS gate structure (element structure) is formed on the front surface side of the semiconductor substrate. In addition, a back surface electrode 11 serving as a drain electrode is provided on the back surface of the semiconductor substrate.

[0031] The active region 30 of the SJ-MOSFET 50 is provided with a parallel pn region 20 in which n-type column regions 3 and p-type column regions 4 are alternately arranged in a repeated manner. The edge termination region 40 may also be provided with a parallel pn region 20B, which will be described later.

[0032] 1, the direction in which the n-type column regions 3 and p-type column regions 4 of the parallel pn region 20 are alternately and repeatedly arranged is the x-direction. A p-type well region 63 is provided on the p-type column region 4 of the active region 30. The bottom surface of the p-type well region 63 of the active region 30 is in contact with the top surface of the p-type column region 4. The p-type well region 63 and the p-type column region 4 of the active region 30 are connected to the n-type well region 63 provided on the top surface of the n-type drift layer 2. - From the surface of the epitaxial layer 27, + The p-type well region 63 is provided so as not to reach the surface of the n-type semiconductor substrate 1. The width of the upper surface of the p-type well region 63 is made wider than the width of the p-type column region 4. Here, the n-type well region 63 provided on the upper surface of the n-type drift layer 2 (above the first main surface of the semiconductor substrate) - The surface of the type epitaxial layer 27 is designated as an upper surface 100 .

[0033] The width of the top surface of the p-type well region 63 is wider than the width of the p-type column region 4, which has the effect of improving the reverse breakdown voltage (BVDSS: drain-source breakdown voltage). As will be described later, the planar shape of the n-type column region 3 and the p-type column region 4 in the active region 30 and the edge termination region 40 is, for example, a stripe shape. When the planar shape of the p-type column region 4 is a stripe shape, the planar shape of the p-type well region 63 is also a stripe shape.

[0034] The impurity concentration of the n-type column region 3 is n + The impurity concentration of the n-type semiconductor substrate 1 is lower than the impurity concentration of the n-type semiconductor substrate 1. The impurity concentration of the p-type column region 4 and the impurity concentration of the p-type well region 63 may be equal. Also, the impurity concentration of the n-type column region 3 and the impurity concentration of the p-type column region 4 may be equal.

[0035] A p-type base region (second semiconductor region of a second conductivity type) 5 is selectively provided on the upper surface 100 side of the active region 30 (above the first main surface of the semiconductor substrate). The p-type base region 5 is provided so as to overlap with the p-type well region 63. The bottom surface of the p-type well region 63 is provided at a deeper position than the bottom surface of the p-type base region 5 in the y direction (depth direction) in FIG. 1. The p-type base region 5 has a higher impurity concentration than the p-type well region 63. In addition, the p-type base region 5 has a higher impurity concentration than the p-type column region 4.

[0036] The surface side of the p-type base region 5 of the active region 30 is provided with n + A p-type source region (first semiconductor region of a first conductivity type) 6 is selectively provided on the surface side of the p-type base region 5 of the active region 30. + The p-type source region 6 ++ A mold contact region 14 may optionally be provided.

[0037] A trench structure is formed in the active region 30 and in the boundary between the active region 30 and the edge termination region 40. Specifically, a trench 18B (second trench) extends from the upper surface 100 to the p-type base region 5, the p-type base region 5A described later, and the n + The doped ...

[0038] The sidewall of the trench 18B provided in the active region 30 is provided with a p-type base region 5 and an n + The sidewall of trench 18B provided at the boundary between active region 30 and edge termination region 40 has p-type base region 5 and n-type source region 6 on the active region 30 side. +The p-type source region 6 is in contact with the edge termination region 40 side, and a p-type base region 5A, which will be described later, is in contact with the edge termination region 40 side. It should be noted that no trench 18B is provided in the edge termination region 40.

[0039] Trench 18B in active region 30 is provided between selectively provided p-type base region 5, and trench 18B at the boundary between active region 30 and edge termination region 40 is provided between p-type base region 5 and p-type base region 5A. Trench 18B has a planar shape that is, for example, a stripe shape extending in the depth direction (z direction) of FIG.

[0040] In the trench 18B, a gate insulating film 7 is formed along the inner wall of the trench 18B. A gate electrode 8 is provided inside the gate insulating film 7 in the trench 18B. The gate electrode 8 is insulated from the n-type column region 3 (n-type drift layer 2) and the p-type base region 5 by the gate insulating film 7. A gate wiring (not shown) may be provided as a part of the gate electrode 8, protruding from above the trench 18B (the side where the source electrode 10 described later is provided) toward the source electrode 10. The gate insulating film 7 is provided below the gate wiring. An interlayer insulating film 9 is provided above the gate wiring.

[0041] The interlayer insulating film 9 is provided on the upper surface 100 so as to cover the upper surface of the gate electrode 8 embedded in the trench 18B. An insulating film (not shown) is provided between the gate electrode 8 and the interlayer insulating film 9 (the boundary between the gate insulating film 7 formed along the inner wall of the trench 18B and the interlayer insulating film 9 covering the upper part of the gate electrode 8, and the boundary between the gate electrode 8 and the interlayer insulating film 9 are not shown). A contact hole 64A is provided between the adjacent trench 18B in the interlayer insulating film 9 covering the upper surface of the gate electrode 8 embedded in the trench 18B in the active region 30, and n + Type source region 6 and p ++ The n-type contact region 14 is exposed. Similarly, a contact hole 64A is provided in the interlayer insulating film 9 covering the upper surface of the gate electrode 8 embedded in the trench 18B of the adjacent active region 30 and the trench 18B provided at the boundary between the active region 30 and the edge termination region 40.+ Type source region 6 and p ++ The mold contact region 14 is exposed. Hereinafter, a description of the insulating film (not shown) provided between the gate electrode 8 and the interlayer insulating film 9 will be omitted.

[0042] The source electrode 10 is provided on the upper surface of the interlayer insulating film 9, and is connected to the n-type semiconductor layer 10 via a contact hole 64A formed in the interlayer insulating film 9 and an insulating film (not shown) provided on the lower surface of the interlayer insulating film 9. + Type source region 6 and p ++ The source electrode 10 is electrically connected to the contact region 14. Hereinafter, a description of an insulating film (not shown) provided on the lower surface of the interlayer insulating film 9 will be omitted. The source electrode 10 is electrically insulated from the gate electrode 8 by the interlayer insulating film 9. A barrier metal (not shown) for preventing diffusion of metal atoms from the source electrode 10 to the gate electrode 8 side may be provided between the source electrode 10 and the interlayer insulating film 9. A protective film (not shown) such as a passivation film made of polyimide is selectively provided on the source electrode 10. In an opening provided in the protective film such as a passivation film provided on the source electrode 10, a region where the source electrode 10 is exposed becomes a source pad region (not shown).

[0043] Furthermore, in the edge termination region 40 that maintains the breakdown voltage, a p-type column region 4A having the same width as the p-type column region 4 of the active region 30 is provided on the side closest to the active region 30. The p-type column region 4 and the p-type column region 4A may be at the same depth in the y direction (depth direction) in FIG. 1. A p-type well region 63A is provided on the p-type column region 4A. The top surface of the p-type column region 4A and the bottom surface of the p-type well region 63A are in contact with each other. Note that the p-type column region 4 and the p-type column region 4A may have the same impurity concentration, and the p-type well region 63 and the p-type well region 63A may also have the same impurity concentration.

[0044] The p-type base region 5A is provided so as to overlap the p-type well region 63A, and is in contact with the sidewall of the trench 18B provided at the boundary between the active region 30 and the edge termination region 40. The bottom surface of the p-type well region 63A is provided at a position deeper than the bottom surface of the p-type base region 5A in the y direction (depth direction) of FIG. 1. The p-type base region 5A may be formed at the same depth as the p-type base region 5 of the active region 30 in the y direction (depth direction) of FIG. 1. The p-type well region 63A may also be formed at the same depth as the p-type well region 63 of the active region 30 in the y direction (depth direction) of FIG.

[0045] The impurity concentration of the p-type base region 5A is the same as that of the p-type base region 5. The impurity concentration of the p-type base region 5A is higher than that of the p-type well region 63A. ++ A mold contact region 14A may be optionally provided.

[0046] A parallel pn region 20B is provided on the outer periphery side of the SJ-MOSFET 50 relative to the p-type columns 4A in the edge termination region 40. In the parallel pn region 20B, n-type column regions 3B and p-type column regions 4B are alternately arranged in a repeated manner. The direction in which the n-type column regions 3B and p-type column regions 4B are alternately arranged is the same as the direction in which the n-type columns 3 and p-type column regions 4 in the active region 30 are alternately arranged in a repeated manner.

[0047] In parallel pn region 20B of edge termination region 40, the sum of the widths of adjacent n-type columns and p-type columns is narrower than that of parallel pn region 20 in active region 30. Here, the sum of the widths of adjacent n-type columns and p-type columns is referred to as the repeat pitch. Thus, the widths of n-type column region 3B and p-type column region 4B in edge termination region 40 are narrower than the widths of n-type column region 3 and p-type column region 4 in active region 30. This makes it easier for the depletion layer to spread in edge termination region 40, and the breakdown voltage of edge termination region 40 can be made higher than the breakdown voltage of active region 30.

[0048] The edge termination region 40 includes p -- A resurf region 12 is provided. -- The type RESURF region 12 extends from the boundary between the active region 30 and the edge termination region 40 to below the field plate 29 and the field oxide film 13, which will be described later. -- The planar shape of the RESURF region 12 is annular.

[0049] p -- The p-type RESURF region 12 is provided deeper than the p-type base region 5A in the y direction (depth direction) in FIG. -- The impurity concentration of the p-type RESURF region 12 is lower than that of the p-type well region 63A. -- In the resurf region 12, a p-type well region 63A, a p-type base region 5A, and a p ++ A contact region 14A is provided. -- The RESURF region 12 is bordered by a trench 18B located at the boundary between the active region 30 and the edge termination region 40.

[0050] p -- The resurf region 12 can reduce the electric field concentration on the end of the p-type base region 5A on the outer periphery side of the SJ-MOSFET 50, thereby increasing the breakdown voltage of the edge termination region 40. In the parallel pn structure 20B of the edge termination region 40, the upper surfaces of some of the n-type column regions 3B and p-type column regions 4B on the active region 30 side are -- The silicon nitride layer 14 is in contact with the bottom surface of the resurf region 12 .

[0051] The top surface of the p-type column region 4B of the outermost parallel pn region 20B of the SJ-MOSFET 50 is in contact with the bottom surface of the outermost p-type well region 63B of the SJ-MOSFET 50. -- Between the resurf region 12 and the n-type resurf region 13, a - A type epitaxial layer 27 is provided.

[0052] In the edge termination region 40, n-type semiconductor layers are formed on the surface of the n-type drift layer 2 (semiconductor substrate).- A first conductive type epitaxial layer (a second semiconductor layer of a first conductive type) 27 is provided. - The n-type epitaxial layer 27 is formed on the entire surface of the n-type drift layer 2. - The surface layer of the epitaxial layer 27 includes p-type well regions 63, 63A, and 63B, p-type base regions 5 and 5A, and -- The upper portion of each of the resurf regions 12 and the n + Type source region 6 and p ++ Mold contact regions 14, 14A are provided.

[0053] Also, n - The impurity concentration of the p-type epitaxial layer 27 is lower than that of the n-type drift layer 2. Therefore, the p-type impurities implanted by ion implantation become more n-type impurities than the n-type drift layer 2 by the heat treatment after the ion implantation. - The ions are more likely to diffuse in the p-type epitaxial layer 27 and less likely to diffuse in the n-type drift layer 2. This makes it easier to control the diffusion of the p-type base region 5 due to the heat treatment after the ion implantation, thereby making it possible to suppress variations in the gate threshold voltage Vth.

[0054] In the x direction of FIG. 1, - The p-type epitaxial layer 27, the p-type well region 63B, and the p -- A field oxide film 13 is provided over the surface of the type RESURF region 12. The field oxide film 13 may be provided to a position deeper than the upper surface 100 in the y direction in FIG. 1. The field oxide film 13 is a p-type oxide film that is continuous from the end of the field oxide film 13 on the active region 30 side to a part of the lower surface. -- The field oxide film 13 is covered with a p-type resurf region 12. -- The p-type resurf region 12, the p-type well region 63B, and the n - A type epitaxial layer 27 is provided, which extends continuously from the other end of the field oxide film 13 to a part of the lower surface. - A type epitaxial layer 27 is provided.

[0055] p --An insulating film 66A connected to the end of the field oxide film 13 on the active region 30 side is provided on the upper surfaces of the resurf region 12, the p-type well region 63A, and the p-type base region 5A. - An insulating film 66B connected to the other end of the field oxide film 13 is provided on the upper surface of the type epitaxial layer 27. The insulating films 66A and 66B may be formed in the same process as the gate insulating film 7.

[0056] Field plate 29 is provided on the upper surface of field oxide film 13 and insulating film 66A that is connected to the end of field oxide film 13 on the active region 30 side. Field plate 29 is electrically connected to gate electrode 8 and also functions as a gate wiring.

[0057] The channel stopper 62 is provided on the upper surface of the field oxide film 13 and an insulating film 66B connected to the other end of the field oxide film 13. The field plate 29 and the channel stopper 62 are separated and provided at a distance on the field oxide film 13. The interlayer insulating film 9 is provided so as to cover the field oxide film 13, the field plate 29 and the channel stopper 62. An insulating film (not shown) is provided between the interlayer insulating film 9 and the field plate 29 and the channel stopper 62. Hereinafter, a description of the insulating film (not shown) provided between the interlayer insulating film 9 and the field plate 29 and the channel stopper 62 will be omitted.

[0058] A contact hole 64B is provided between the interlayer insulating film 9 provided so as to cover the upper surface of the gate electrode 8 embedded in the trench 18B provided at the boundary between the active region 30 and the edge termination region 40 and the interlayer insulating film 9 covering the field plate 29. ++ The mold contact area 14A is exposed.

[0059] A contact hole 64C is provided in the interlayer insulating film 9 covering the field oxide film 13, the field plate 29 and the channel stopper 62, and the field plate 29 is exposed.

[0060] The source electrode 10 provided on the upper surface of the interlayer insulating film 9 extends from the active region 30 to the upper surface of a part of the edge termination region 40, and is connected to the p ++ The n-type contact region 14A and the p-type base region 5A are electrically connected to the n-type contact region 14A and the p-type base region 5A.

[0061] The metal gate runner 61 is electrically connected to the field plate 29 via a contact hole 64C formed in the interlayer insulating film 9. -- The type RESURF region 12, the field oxide film 13, the field plate 29, the channel stopper 62 and the interlayer insulating film 9 of the edge termination region 40 may be provided in a ring shape on the outer periphery of the SJ-MOSFET 50. The metal gate runner 61 is electrically insulated from the source electrode 10.

[0062] 2A is a cross-sectional view showing another structure of the SJ-MOSFET 50 according to the embodiment. FIG. 2A differs from FIG. 1 in that the parallel pn region 20B located on the outer periphery side of the SJ-MOSFET 50 relative to the p-type column region 4A of the edge termination region 40 is not provided. When the parallel pn region 20B is not provided, the n - The n-type epitaxial layer 27 - The epitaxial layer 27 and p -- By expanding the depletion layer extending from the pn junction with the type RESURF region 12 to the outer periphery side of the SJ-MOSFET 50 of the n-type epitaxial layer 27, the breakdown voltage of the SJ-MOSFET 50 can be improved.

[0063] FIG. 2B is a cross-sectional view showing yet another structure of SJ-MOSFET 50 according to the embodiment. FIG. 2B differs from FIG. 2A in that p-type well region 63 in contact with the upper surface of p-type column region 4 of active region 30 and p-type well region 63A in contact with the upper surface of p-type column region 4A of edge termination region 40 are not provided. In FIG. 2B, p-type base region 5 is provided on the upper surface of p-type column region 4 of active region 30. The upper surface of p-type column region 4 of active region 30 is in contact with the bottom surface of p-type base region 5. Also, p-type base region 5A is provided on the upper surface of p-type column region 4A of edge termination region 40. The upper surface of p-type column region 4A of edge termination region 40 is in contact with the bottom surface of p-type base region 5A. The difference in cross-sectional shape between FIG. 2B and FIG. 2A is due to the difference in the position of the implantation region into which p-type impurities, which will be described later, are implanted to form p-type column region 4. SJ-MOSFET 50 shown in FIG. 2B has an implantation region 92 formed in section D2, as shown in FIG. 9C, which will be described later. In FIG. 2B, by not providing the p-type well regions 63, 63A, there is no region that locally narrows the current path formed in the n-type drift layer 2 (n-type column region 3). The on-voltage generated by flowing current causes a depletion layer to expand from the pn junction between the n-type column region 3 and the p-type column regions 4, 4A, and the current path narrows as the depletion layer expands. When the current path narrows (the depletion layer expands), the on-resistance increases. Therefore, by not providing the p-type well regions 63, 63A, the on-resistance (resistance in the operating state) can be made smaller than in FIG. 2A.

[0064] Fig. 2C is a cross-sectional view showing still another structure of the SJ-MOSFET 50 according to the embodiment. Fig. 2C differs from Fig. 2A in that contact holes 64D, 64E, and 64F formed in the interlayer insulating film 9 include recesses 67A, 67B, and 67C (grooves), and contact plugs 19 are embedded inside the recesses 67A, 67B, and 67C.

[0065] The interlayer insulating film 9 covering the upper surface of the gate electrode 8 embedded in the trench 18B of the active region 30 has a recess 67A between adjacent trenches 18B that is deeper than the upper surface 100 in the y direction. + Type source region 6 and p++ The bottom of the recess 67A is in contact with (exposed to) the p-type contact region. ++ The mold contact region 14 is in contact with (exposed to) the gate electrode 8. The recess 67A is a contact hole 64D. An insulating film (not shown) is provided between the gate electrode 8 and the interlayer insulating film 9. Hereinafter, a description of the insulating film (not shown) provided between the gate electrode 8 and the interlayer insulating film 9 will be omitted.

[0066] Similarly, a recess 67A deeper than the upper surface 100 in the y direction is provided in the interlayer insulating film 9 covering the upper surface of the gate electrode 8 embedded in the trench 18B of the adjacent active region 30 and the trench 18B provided at the boundary between the active region 30 and the edge termination region 40. + Type source region 6 and p ++ The recess 67A is in contact with (exposed to) the p-type contact region 14. ++ The mold contact region 14 is in contact with (exposed to) the recess 67A, which is the contact hole 64D.

[0067] A recess 67B that is deeper than the upper surface 100 in the y direction is provided between the interlayer insulating film 9 that is provided so as to cover the upper surface of the gate electrode 8 embedded in the trench 18B provided at the boundary between the active region 30 and the edge termination region 40 and the interlayer insulating film 9 that covers the field plate 29. The sidewalls and bottom of the recess 67B are provided with p ++ The mold contact region 14A is in contact with (exposed to) the recess 67B, which is the contact hole 64E.

[0068] A recess 67C is provided in the interlayer insulating film 9 covering the field oxide film 13, the field plate 29, and the channel stopper 62. The recess 67C penetrates the field plate 29 and exposes the surface of the field oxide film 13. The field plate 29 is in contact with (exposed to) the sidewall of the recess 67C. The recess 67C may also provide a recess (groove) in the surface of the field oxide film 13, and the field oxide film 13 may be in contact with (exposed to) the sidewall of the recess 67C. The field oxide film is in contact with (exposed to) the bottom of the recess 67C. This recess 67C is the contact hole 64F. An insulating film (not shown) is provided between the interlayer insulating film 9 and the field plate 29 and the channel stopper 62. Hereinafter, a description of the insulating film (not shown) provided between the interlayer insulating film 9 and the field plate 29 and the channel stopper 62 will be omitted.

[0069] The contact plug 19 is, for example, a metal film made of tungsten (W) which has high embedding properties. The contact plug 19 may be provided in the contact holes 64D, 64E, and 64F via a barrier metal. The source electrode 10 is connected to the n-type semiconductor layer 10 via the contact plug 19 in the contact hole 64D of the active region 30. + Type source region 6 and p ++ The source electrode 10 is electrically connected to the p-type contact region 14. The source electrode 10 also extends to a portion of the edge termination region 40 and is connected to the p-type contact region 14 via a contact plug 19 in a contact hole 64E of the edge termination region 40. ++ It is electrically connected to the contact region 14A.

[0070] The metal gate runner 61 is electrically connected to the field plate 29 via the contact plug 19 in the contact hole 64F. The source electrode 10 and the metal gate runner 61 are electrically insulated from each other.

[0071] Fig. 2C, like Fig. 2A, shows a case where parallel pn region 20B is not provided on the outer periphery side of SJ-MOSFET 50 relative to p-type column region 4A of edge termination region 40. Fig. 2C also shows a case where parallel pn region 20B is provided on the outer periphery side of SJ-MOSFET 50 relative to p-type column region 4A of edge termination region 40, as in Fig. 1.

[0072] 2D is a cross-sectional view showing another structure of SJ-MOSFET 50 according to an embodiment. FIG. 2D differs from FIG. 1 in that p-type well regions 63, 63A in contact with the top surfaces of p-type column regions 4, 4A are in contact with the sidewall of trench 18B. In FIG. 2D, p-type well region 63 of active region 30 extends in the x-direction of FIG. 2D and in contact with the sidewall of trench 18B, and p-type well region 63A of edge termination region 40 extends in the x-direction of FIG. 2D and in contact with trench 18B provided at the boundary with edge termination region 40.

[0073] As a result, the p-type well regions 63, 63A and the p-type base regions 5, 5A come into contact with the side walls of the trench 18B. This makes it easier to prevent defects due to channel defects such as defects in the p-type column regions 4, 4A and short channels. Furthermore, the two-stage concentration gradient of the p-type well regions 63, 63A and the p-type base regions 5, 5A eases the electric field near the channel junction, making it easier to ensure a sufficient channel length.

[0074] Fig. 3 is a plan view showing the structure of an SJ-MOSFET according to an embodiment, which is a plan view of the A-A' cross section of Fig. 1. As shown in Fig. 3, the repetition pitch P2 of the parallel pn regions 20B in the edge termination region 40 is narrower than the repetition pitch P1 of the parallel pn regions 20 in the active region 30.

[0075] 3. The repetition pitch P1 of the parallel pn region 20 indicates the sum of the width of the adjacent n-type column region 3 and the width of the p-type column region 4 in the x direction of FIG. 3. The repetition pitch P2 of the parallel pn region 20B indicates the sum of the width of the adjacent n-type column region 3B and the width of the p-type column region 4B in the x direction of FIG. 3. In order to ensure the avalanche resistance of the SJ-MOSFET 50 (super junction semiconductor device), it is necessary to make the withstand voltage of the edge termination region 40 higher than the withstand voltage of the active region 30. For this reason, it is preferable that the width of the n-type column region 3B and the width of the p-type column region 4B of the edge termination region 40 are narrower than the width of the n-type column region 3 and the width of the p-type column region 4 of the active region 30. This makes it easier for the depletion layer to spread in the edge termination region 40, and the withstand voltage of the edge termination region 40 can be made higher than the withstand voltage of the active region 30.

[0076] 3, the planar shape of n-type column region 3 and p-type column region 4 in active region 30 may be, for example, a stripe structure with a longitudinal direction parallel to the z direction. Furthermore, n-type column region 3B and p-type column region 4B in edge termination region 40 may also be a stripe structure with a longitudinal direction parallel to the z direction. Furthermore, p-type column region 4B in edge termination region 40 may also be a stripe structure with a longitudinal direction parallel to the z direction. Furthermore, although not shown, the planar shape of trench 18B may also be a stripe shape with a longitudinal direction parallel to the z direction.

[0077] (Method of Manufacturing Super-Junction Semiconductor Device According to the Embodiment) Next, a method for manufacturing the super-junction semiconductor device according to the embodiment will be described. Fig. 4 to Fig. 21 are cross-sectional views showing a state during the manufacturing process by a first manufacturing method of the SJ-MOSFET according to the embodiment. First, n + n-type drain layer + A type semiconductor substrate 1 is prepared.

[0078] Next, n + On the front surface of the n-type semiconductor substrate 1, +An n-type drift layer 2 having an impurity concentration lower than that of the n-type semiconductor substrate 1 is epitaxially grown. At this time, the impurity concentration of the n-type drift layer 2 is 1.0×10 16 / cm 3 Above 3.0×10 17 / cm 3 For example, when forming a super-junction semiconductor device with a breakdown voltage of 40 V, the impurity concentration of the n-type drift layer 2 may be set to 1.0×10 17 / cm 3 For example, when forming a super-junction semiconductor device with a breakdown voltage of 100 V, the impurity concentration of the n-type drift layer 2 may be set to 5.0×10 16 / cm 3 The impurity concentration of the n-type drift layer 2 is constant in the depth direction. Here, the depth direction is defined as the depth from the surface of the n-type drift layer 2 to the n + This is the direction toward the type semiconductor substrate 1. The state up to this point is shown in FIG.

[0079] Next, an oxide film 23 is formed on the surface of the n-type drift layer 2. Next, a resist mask 24 having openings at positions where the p-type column regions 4 are to be formed is formed on the surface of the oxide film 23 by photolithography. The state up to this point is shown in FIG.

[0080] Next, using the resist mask 24 as a mask, openings that expose the n-type drift layer 2 are formed in the oxide film 23 by dry etching. Next, the resist mask 24 is removed, and using the oxide film 23 with the openings as a mask, for example, anisotropic dry etching is performed to form p-type column trenches (first trenches) 25A in the n-type drift layer 2. The state up to this point is shown in FIG.

[0081] Next, isotropic etching and sacrificial oxidation are performed with the oxide film 23 still attached. This process removes damage to the p-type column trench 25A and rounds the bottom of the p-type column trench 25A. The order in which the isotropic etching and the sacrificial oxidation are performed does not matter. Also, it is possible to perform only one of the isotropic etching and the sacrificial oxidation.

[0082] Thereafter, the oxide film 23 is removed. The oxide film 23 may be removed simultaneously with a sacrificial oxide film (not shown). The width of the p-type column trench 25B formed after removing the oxide film 23 is set to W1. The state up to this point is illustrated in FIG. 7.

[0083] Next, a n-type impurity layer having an impurity concentration lower than that of the n-type drift layer 2 is formed so as to cover the surface of the n-type drift layer 2 and fill the inside of the p-type column trench 25B. - The n-type epitaxial layer 27 is epitaxially grown. - The impurity concentration of the epitaxial layer 27 is 1.0×10 15 / cm 3 Above 5.0×10 16 / cm 3 For example, when forming a super-junction semiconductor device with a breakdown voltage of 40 V, n-type impurities may be doped and epitaxially grown. - The impurity concentration of the epitaxial layer 27 is set to 2.0×10 16 / cm 3 In addition, when forming a super-junction semiconductor device with a breakdown voltage of 100 V, n - The impurity concentration of the epitaxial layer 27 is set to 1.0×10 16 / cm 3 It is also possible to use the following.

[0084] Impurity concentration of n-type drift layer 2 and n - The relationship between the impurity concentration of the n-type epitaxial layer 27 and the impurity concentration of the n-type drift layer 2 is as follows: 3 ]n - The impurity concentration of the type epitaxial layer 27 is b [ / cm 3 ], a>b. The impurity concentration a[ / cm 3 ] and n - Impurity concentration b[ / cm 3 ]The relationship 2≦a / b≦10 holds true.

[0085] n -The thickness of the flat portion of the n-type epitaxial layer 27 is defined as T1. - The flat portion of the epitaxial layer 27 is formed on the surface of the n-type drift layer 2 where the p-type column trenches 25B are not formed. - This is the portion where the n-type epitaxial layer 27 is formed. - The surface of the flat portion of the type epitaxial layer 27 is referred to as an upper surface 100 .

[0086] n - When forming the p-type epitaxial layer 27, the thickness T1 is set to a value larger than 1 / 2 the width W1 of the p-type column trench 25B (T1>W1 / 2). By setting the thickness T1 to be larger than 1 / 2 the width W1 of the p-type column trench 25B, - The upper surface 100 (surface) of the mold epitaxial layer 27 does not need to be planarized using a CMP device etc. The state up to this point is shown in FIG.

[0087] 9A to 9C are cross-sectional views of the state in which an ion implantation region is formed under different conditions by performing ion implantation 22 using an ion implantation mask 21. - An ion implantation mask 21 having a predetermined opening is formed on the surface (upper surface 100) of the p-type epitaxial layer 27 by photolithography, for example, using photoresist. The opening of the ion implantation mask 21 is formed above the p-type column trench 25B. Using the ion implantation mask 21 as a mask, ion implantation 22 of p-type impurities is performed. The p-type impurity is, for example, boron (B) or aluminum (Al). The ion implantation 22 may be performed once, or may be performed multiple times at different implantation depths. When the ion implantation 22 is performed multiple times at different depths, the order of the ion implantations 22 can be changed in various ways. Here, the depth is n - From the upper surface 100 (surface) of the type epitaxial layer 27 + The implantation depth is n - This is the depth (peak position of the impurity concentration distribution) at which the impurity is implanted from the upper surface 100 (surface) of the type epitaxial layer 27.

[0088] In addition, implantation regions 90, 91-1, 91-2, and 92, which will be described later and are formed by performing ion implantation 22, indicate regions (peak positions of the impurity concentration distribution) into which impurities are implanted from the upper surface 100. Therefore, the implantation depth is n - From the upper surface 100 (surface) of the type epitaxial layer 27 - 1, the depth to which implanted regions 90, 91-1, 91-2, and 92 are formed in type epitaxial layer 27 is shown.

[0089] Furthermore, n - Between the surface (upper surface 100) of the n-type epitaxial layer 27 and the surface of the n-type drift layer 2 ( - The section D1 is the thickness T1 of the flat portion of the n-type epitaxial layer 27, and the section from the surface of the n-type drift layer 2 (surface of the semiconductor substrate) to the bottom of the p-type column trench 25B is a section D2.

[0090] In FIG. 9A, ion implantation 22 is performed once to form implantation region 90. Implantation region 90 is formed in section D1. For example, when section D1 is 0.8 μm and section D2 is 1.0 μm, the implantation depth of implantation region 90 is 0.4 μm. Section D1 may be 0.5 μm or more and 1.0 μm or less. The implantation depth of implantation region 90 may be 0.2 μm or more and 1.0 μm or less. Section D2 may be 0.5 μm or more and 2.0 μm or less. Note that implantation region 90 may be formed at the boundary between section D1 and section D2.

[0091] In FIG. 9B, the ion implantation 22 is performed twice to form the implantation regions 91-1 and 91-2. The implantation region 91-1 is formed in the section D1, and the implantation region 91-2 is formed in the section D2. For example, when the section D1 is 0.8 μm and the section D2 is 1.0 μm, the implantation depth of the implantation region 91-1 is 0.4 μm, and the implantation depth of the implantation region 91-2 is 1.6 μm. The section D1 may be 0.5 μm or more and 1.5 μm or less. The implantation depths of the implantation regions 91-1 and 91-2 may be 0.2 μm or more and 2.0 μm or less. The section D2 may be 1.0 μm or more and 4.0 μm or less. Either the implantation region 91-1 or the implantation region 91-2 may be formed at the boundary between the section D1 and the section D2. The order in which the implantation regions 91-1 and 91-2 are formed may be any order.

[0092] In Fig. 9C, ion implantation 22 is performed once to form implantation region 92. Implantation region 92 is formed in section D2. For example, if section D1 is 0.8 µm and section D2 is 1.0 µm, the implantation depth of implantation region 92 is 1.2 µm. Section D1 may be 0.5 µm or more and 1.5 µm or less. The implantation depth of implantation region 92 may be 0.4 µm or more and 2.0 µm or less. Implantation region 92 may be formed at the boundary between section D1 and section D2.

[0093] 9A, 9B and 9C show typical examples of the implantation depth and number of implantations of p-type impurities in ion implantation 22, but the implantation depth of the implanted region, the number of implantations, etc. can be changed in various ways.

[0094] FIG. 10A is a cross-sectional view showing a state in which the ion implantation mask 21 is removed after the ion implantation 22 in FIG. 9A and the p-type impurities are diffused by heat treatment. - Since the p-type epitaxial layer 27 has a lower impurity concentration than the n-type drift layer 2, the p-type impurity is ion-implanted into the p-type epitaxial layer 27 through the p-type impurity ion implantation 22 and the subsequent heat treatment. - Therefore, the n-type drift layer 2 has a width W2 of the p-type column region 4 and a width W3 of the n-type epitaxial layer 27. - A p-type well region 63 having a wide width W3 is formed on the upper surface 100 of the p-type epitaxial layer 27.

[0095] The n-type column regions 3 are formed between adjacent p-type column regions 4, and parallel pn regions 20 are formed in the n-type drift layer 2. The p-type column regions 4A and p-type well regions 63A of the edge termination region 40 are also formed in the same manner in the same process.

[0096] The p-type impurity concentration in Fig. 10A is highest in the implantation region 90 shown in Fig. 9A, and the impurity concentration decreases in the depth direction as the distance from the implantation region 90 increases. - From the surface of the epitaxial layer 27, + 1 toward the semiconductor substrate 1.

[0097] FIG. 10B is a cross-sectional view in which the ion implantation mask 21 is removed after the ion implantation 22 in FIG. 9B, and the p-type impurities are diffused by heat treatment. - Since the p-type epitaxial layer 27 has a lower impurity concentration than the n-type drift layer 2, the p-type impurities are implanted into the implantation regions 91-1 and 91-2 by the ion implantation 22 of the p-type impurities and the subsequent heat treatment. - Therefore, the n-type drift layer 2 has a width W2 of the p-type column region 4 and a width W3 of the n-type epitaxial layer 27. - A p-type well region 63 having a wide width W3 is formed on the upper surface 100 of the p-type epitaxial layer 27.

[0098] The n-type column regions 3 are formed between adjacent p-type column regions 4, and parallel pn regions 20 are formed in the n-type drift layer 2. The p-type column regions 4A and p-type well regions 63A of the edge termination region 40 are also formed in the same manner in the same process.

[0099] The p-type impurity concentration in Fig. 10B is highest in implantation region 91-1 and implantation region 91-2 shown in Fig. 9B, and the impurity concentration decreases in the depth direction as the distance from implantation region 91-1 and implantation region 91-2 increases. Note that the p-type impurity increases in the portion where the p-type impurity diffusion of implantation region 91-1 and implantation region 91-2 overlaps, and the impurity concentration increases even if the portion is far from implantation region 91-1 and implantation region 91-2 in the depth direction. Here, the depth direction is n - From the surface of the epitaxial layer 27, + 1 toward the semiconductor substrate 1.

[0100] FIG. 10C is a cross-sectional view in which the ion implantation mask 21 is removed after the ion implantation 22 in FIG. 9C, and the p-type impurities are diffused by heat treatment. - Since the p-type epitaxial layer 27 has a lower impurity concentration than the n-type drift layer 2, the p-type impurity is transferred from the implantation region 92 to the n-type epitaxial layer 27 by the ion implantation 22 of the p-type impurity and the subsequent heat treatment. - This makes it easier for the impurities to spread into the type epitaxial layer 27 .

[0101] The implanted region 92 shown in FIG. - The p-type impurity in the implantation region 92 is formed in a section D2 that is separated from the upper surface 100 side of the n-type epitaxial layer 27. - The n-type epitaxial layer 27 is less likely to diffuse in a direction perpendicular to the depth direction (a direction parallel to the widths W2 and W3) on the upper surface 100 side of the p-type epitaxial layer 27. - The width W3 of the upper surface 100 of the type epitaxial layer 27 may be formed to be the same width.

[0102] The n-type column regions 3 are formed between adjacent p-type column regions 4, and parallel pn regions 20 are formed in the n-type drift layer 2. The p-type column regions 4A and p-type well regions 63A of the edge termination region 40 are also formed in the same process. The p-type impurity concentration in FIG. 10C is highest in the implantation region 92 shown in FIG. 9C, and the impurity concentration decreases with increasing distance from the implantation region 92. Here, the depth direction is n -From the surface of the epitaxial layer 27, + 1 toward the semiconductor substrate 1.

[0103] 10A and 10B have the same cross-sectional shape of the p-type well region, but FIG. 10C has a different cross-sectional shape from FIG. 10A and FIG. 10B. This is because the position of the implanted region formed by ion implantation 22 is different. The subsequent manufacturing steps will be explained based on the state of FIG. 10A. Here, the depth direction is n - From the surface (upper surface 100) of the type epitaxial layer 27 + The direction is toward the type semiconductor substrate 1. Moreover, "shallow" and "deep" refer to the depth in the depth direction.

[0104] Although the case where a photoresist is used as the ion implantation mask 21 has been described, for example, an oxide film may be used. When an oxide film is used, openings are formed in the oxide film using photolithography and etching techniques. When an oxide film is used as the ion implantation mask 21, it is also possible to perform a heat treatment for diffusing the implanted impurities with the oxide film still attached.

[0105] Next, n - On the surface (upper surface 100) of the type epitaxial layer 27, p -- An ion implantation mask 65 having an opening for forming the type RESURF region 12 is formed. The ion implantation mask 65 is made of, for example, a photoresist. Using the ion implantation mask 65 as a mask, ions of a p-type impurity are implanted. The p-type impurity is, for example, boron (B) or aluminum (Al). The state up to this point is shown in FIG. 11.

[0106] Next, after removing the ion implantation mask 65, a heat treatment is performed to diffuse the implanted p-type impurities, resulting in an n - The surface layer of the p-type epitaxial layer 27 -- A type RESURF region 12 is formed. -- Since the impurity concentration of the resurf region 12 is lower than that of the p-type well region 63A, the p-type well region 63A has p --The type RESURF region 12 is not formed. -- The bottom surface of the type RESURF region 12 is - The p-type epitaxial layer 27 is formed deeper than the boundary between the p-type drift layer 2. -- The bottom surface of the p-type RESURF region 12 may be formed shallower than the boundary (dotted line) between the p-type column region 4 A and the p-type well region 63 A. The state up to this point is shown in FIG.

[0107] Next, an oxide film 28 is formed on the upper surface 100. The oxide film 28 may be, for example, a LOCOS film. The thickness of the oxide film 28 in the active region 30 is formed to be thinner than the thicker portion of the oxide film 28 formed on the outer periphery of the edge termination region 40. The oxide film 28 is an n - A thick portion is formed on the upper surface of the type epitaxial layer 27, and the bottom surface of the thick portion of the oxide film 28 is formed to a position deeper than the upper surface 100. The end portion of the thick portion of the oxide film 28 on the active region 30 side is continuous from the end portion to a part of the lower surface, and is p -- The oxide film 28 is formed so as to be covered by the type RESURF region 12. The other end of the thick portion of the oxide film 28 is continuous with a part of the lower surface, and has an n-type - The semiconductor layer is then formed so as to be covered with a type epitaxial layer 27. The state up to this point is shown in FIG.

[0108] Next, a resist mask (not shown) having a predetermined opening is formed on the surface of the oxide film 28 by photolithography. Next, openings are formed in the oxide film 28 by dry etching using the resist mask. Next, the resist mask is removed, and the n-type SiO 2 film is removed by anisotropic dry etching using the oxide film 28 as a mask. - From the top surface 100 of the type epitaxial layer 27 - A trench 18A is then formed which penetrates the n-type epitaxial layer 27 and reaches the n-type drift layer 2. The state up to this point is shown in FIG.

[0109] Next, isotropic etching and sacrificial oxidation are performed with oxide film 28 still attached. This process removes damage to trench 18A and rounds the bottom of trench 18A. The order of isotropic etching and sacrificial oxidation may be either first. Also, only one of isotropic etching and sacrificial oxidation may be performed. After that, the oxide film 28 in the thin portion used as a mask for forming trench 18A is removed. At this time, the oxide film 28 in the thin portion and the sacrificial oxide film may be removed at the same time. The trench after removing oxide film 28 becomes trench 18B. Since oxide film 28 has a thin portion and a thick portion in edge termination region 40, a full surface etching is performed to remove the thin portion of oxide film 28, and the oxide film in the thick portion of edge termination region 40 is left. The sacrificial oxide film (not shown) may be removed together with the thin portion of oxide film 28. Also, oxide film 28 may be left in edge termination region 40 by removing oxide film 28 using photolithography and etching techniques. The oxide film remaining in edge termination region 40 (thicker portion of oxide film 28) becomes field oxide film 13. The state up to this point is shown in FIG.

[0110] Next, n - Type epitaxial layer 27, p -- A gate insulating film 7 is formed along the surfaces (upper surfaces 100) of the type RESURF region 12 and the p-type well regions 63, 63A and the inner walls of the trench 18B. This gate insulating film 7 may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen atmosphere. Alternatively, this gate insulating film 7 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).

[0111] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 7. This polycrystalline silicon layer is formed so as to fill the trench 18B. This polycrystalline silicon layer is patterned by photolithography and etching techniques to form a gate electrode 8 within the trench 18B via the gate insulating film 7.

[0112] Also, the polysilicon layer formed in edge termination region 40 may be selectively left to serve as field plate 29 and channel stopper 62 .

[0113] Field plate 29 is p -- The field plate 29 is formed continuously on the upper surface of the gate insulating film 7 (insulating film 66A) formed on the type RESURF region 12, the p-type well region 63A, and the p-type base region 5A (upper surface 100), and on the upper surface of the field oxide film 13 on the active region 30 side. The field plate 29 is electrically connected to the gate electrode 8, and also functions as a gate wiring.

[0114] The channel stopper 62 is in contact with the upper surface of the outer periphery of the field oxide film 13 and the n - The field plate 29 and the channel stopper 62 are formed continuously on the upper surface of the gate insulating film 7 (insulating film 66B) formed on the upper surface 100 of the type epitaxial layer 27. The field plate 29 and the channel stopper 62 are separated by the field oxide film 13.

[0115] Next, n - The upper surface 100 of the p-type epitaxial layer 27 (including the p-type well regions 63, 63A and - A p-type impurity ion implantation 22 is performed to form the p-type base regions 5, 5A from the surface of the n-type epitaxial layer 27. The p-type impurity is, for example, boron (B) or aluminum (Al). - In the edge termination region 40 on the n-type epitaxial layer 27, the field plate 29, the channel stopper 62, and the field oxide film 13 function as a mask. - The p-type epitaxial layer 27 is not doped with p-type impurities. The gate electrode 8 also functions as a mask. The state up to this point is shown in FIG. 16. Next, the gate insulating film 7 formed on the upper surface 100 is removed. Note that the gate insulating film 7 is removed when the thickness of the gate insulating film 7 becomes n-type as described later. + If the thickness does not interfere with the ion implantation for forming the type source region 6, for example, 500 Å or less, this need not be performed.

[0116] Next, the p-type impurities are diffused by heat treatment to form n - The p-type epitaxial layer 27, the p-type well regions 63, 63A, and the p -- P-type base regions 5, 5A are formed in the surface layer of type RESURF region 12. By this heat treatment, an insulating film 66C is formed so as to cover the upper surface of gate electrode 8 made of a polycrystalline silicon layer formed to fill trench 18B, field plate 29, and channel stopper 62.

[0117] The p-type base region 5 and the p-type well region 63 overlap, and the bottom surface of the p-type base region 5 is formed shallower than the bottom surface of the p-type well region 63. The p-type base region 5A and the p-type well region 63A overlap, and the bottom surface of the p-type base region 5A is formed shallower than the bottom surface of the p-type well region 63A.

[0118] The p-type base region 5 and the p-type base region 5A may have the same impurity concentration. The p-type well region 63 and the p-type well region 63A may have the same impurity concentration. The impurity concentration of the p-type base region 5 is higher than the impurity concentration of the p-type well region 63. The impurity concentration of the p-type base region 5A is higher than the impurity concentration of the p-type well region 63A. The p-type base regions 5, 5A are formed to contact the sidewall of the trench 18B.

[0119] In the edge termination region 40, the oxide film 28, the field plate 29, and the channel stopper 62 function as a mask, so that the n-type semiconductor layer 41 is covered with these. - The p-type epitaxial layer 27 and -- Boron (B) is not implanted into the p-type RESURF region 12. As a result, even if a heat treatment is performed to diffuse the p-type impurities that form the p-type base regions 5 and 5A, the n - The p-type epitaxial layer 27 and -- The p-type impurities forming the p-type base regions 5, 5A do not diffuse into the resurf region 12. - The p-type epitaxial layer 27 and -- A type RESURF region 12 remains.

[0120] In this manner, in the first manufacturing method, the p-type base region 5 in which the channel is to be formed is formed after the formation of the trench 18B. The state up to this point is illustrated in FIG.

[0121] Next, for example, a mask (not shown) having a desired opening is formed on the surface of the p-type base region 5 by photolithography using a resist. Using this resist mask as a mask, n-type impurities are ion-implanted. By this ion implantation, n-type impurities are implanted into the surface layer of the p-type base region 5. + An n-type impurity is implanted into a portion where a n-type source region 6 is to be formed. The n-type impurity to be implanted is arsenic (As), phosphorus (P), or the like.

[0122] Next, n + The ion implantation mask used for forming the p-type source region 6 is removed. Further, a mask having desired openings is formed on the surface of the p-type base region 5 by using, for example, a resist by photolithography technology, and n + The p-type source region 6 ++ A p-type impurity may be implanted to form the p-type contact region 14. The surface layer of the p-type base region 5A may also be implanted with p-type impurities. ++ In addition, the surface layer of the p-type base region 5A of the edge termination region 40 may be doped with n-type impurities to form the p-type contact region 14A. + The source region 6 is not formed.

[0123] Next, n + Type source region 6 and p ++In order to form the contact regions 14 and 14A, a heat treatment is performed to activate the implanted impurities. Here, the difference between the heat treatment for activation and the heat treatment after ion implantation (heat treatment for diffusing the implanted impurities) will be described. The semiconductor substrate into which ions have been implanted, for example, the n-type drift layer 2, is damaged by the ion implantation and defects are generated. The implanted impurities are in a state in which none of them function as charges due to the defects. The heat treatment for activation refers to a heat treatment for recovering the defects generated by the ion implantation and providing a charge amount (resistance) commensurate with the amount of implanted impurities. The heat treatment after ion implantation (heat treatment for diffusing the implanted impurities) refers to a heat treatment for recovering the defects generated by the ion implantation and providing a charge amount (resistance) commensurate with the amount of implanted impurities, and further diffusing the impurities to an arbitrary position in the semiconductor substrate, for example, the n-type drift layer 2. Therefore, the heat treatment for activation has a smaller thermal history than the heat treatment after ion implantation (heat treatment for diffusing the implanted impurities). A small thermal history means, for example, that the heat treatment temperature is low or the heat treatment time is short, or that the heat treatment temperature is low and the heat treatment time is short. + Type source region 6 and p ++ The order of ion implantation for forming the mold contact regions 14, 14A may be any. The state up to this point is shown in FIG.

[0124] Next, n - An interlayer insulating film 9 is formed on the entire upper surface (upper surface 100) of the n-type epitaxial layer 27. The interlayer insulating film 9 is formed on, for example, the gate insulating film 7, the gate electrode 8, the n-type epitaxial layer 27, and the n-type epitaxial layer 27 through an insulating film 66C. + Type source region 6, p ++ p-type contact region 14, p-type base region 5A, ++The interlayer insulating film 9 is formed so as to cover the upper portions of the contact region 14A, the field oxide film 13, the field plate 29, and the channel stopper 62. The interlayer insulating film 9 is formed of, for example, boron phosphorus silicate glass (BPSG), phosphorus silicate glass (PSG), or the like. The interlayer insulating film 9 may also be a laminated film formed by forming, for example, a high temperature oxide (HTO), non-doped silicate glass (NSG), or tetraethoxysilane (TEOS) film under the BPSG (between the BPSG and the gate electrode 8). The thickness of the interlayer insulating film 9 may be about 1 μm.

[0125] Next, the interlayer insulating film 9 and the insulating film 63C are patterned by photolithography and etching. + Type source region 6 and p ++ A contact hole 64A is formed exposing the surface of the contact region 14 (the boundary between the gate insulating film 7 formed along the inner wall of the trench 18B and the interlayer insulating film 9 covering the upper part of the gate electrode 8 is not shown). ++ A contact hole 64B is formed exposing the surface of the contact region 14A. Furthermore, a contact hole 64C is formed in the edge termination region 40 exposing the surface of the field plate 29. Thereafter, a heat treatment (reflow) is performed to flatten the interlayer insulating film 9. The state up to this point is shown in FIG.

[0126] Next, a metal film such as aluminum or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu) is formed by sputtering to fill the contact holes 64A, 64B, 64C and to continuously cover the upper surface of the interlayer insulating film 9. Before forming the metal film, a barrier metal (not shown) made of a titanium film (Ti), a titanium nitride film (TiN), or a laminated film of these (for example, Ti / TiN, etc.) may be formed by sputtering along the inner walls of the contact holes 64A, 64B, 64C and continuously on the upper surface of the interlayer insulating film 9. Thereafter, the metal film and the barrier metal (not shown) are patterned by photolithography and etching techniques to form the source electrode 10, the metal gate runner 61, and the gate electrode pad (not shown). The barrier metal may be formed only in the contact holes 64A, 64B, 64C.

[0127] The source electrode 10 is an n-type semiconductor layer having a surface exposed through a contact hole 64A in the active region 30. + Type source region 6 and p ++ The source electrode 10 is electrically connected to the p-type contact region 14 in the edge termination region 40, the surface of which is exposed through the contact hole 64B. ++ The metal gate runner 61 is electrically connected to the gate electrode 8 and field plate 29 whose surface is exposed through the contact hole 64C. A gate electrode pad (not shown) is electrically connected to the metal gate runner 61 and the gate electrode 8. Note that a tungsten plug or the like may be embedded in the contact holes 64A, 64B, 64C via a barrier metal.

[0128] Next, n +A back electrode 11 is formed on the back surface of the n-type semiconductor substrate 1 (the back surface of the semiconductor base). The back electrode 11 may be formed of a metal film of, for example, nickel (Ni), titanium (Ti), gold (Au), silver (Ag), aluminum (Al), or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu), etc. Alternatively, a laminate film of these (for example, Ti / Ni / Au, Al / Ti / Ni / Au, etc.) may be formed. After the back electrode 11 is formed, a heat treatment is performed to form an n-type electrode. + An ohmic junction is formed between the type semiconductor substrate 1 and the back surface electrode 11. This completes the SJ-MOSFET 50 shown in FIG.

[0129] In this way, the p-type column trenches 25B are formed in the regions that will become the p-type column regions 4 and 4A, and the n-type drift layer 2 has an impurity concentration lower than that of the n-type drift layer 2 that will become the n-type column region 3. - A p-type epitaxial layer 27 is formed so as to be embedded in the p-type column trench 25 .

[0130] Furthermore, n - The p-type column regions 4, 4A and the p-type well regions 63, 63A are formed by ion implantation of p-type impurities from the surface (upper surface 100) of the p-type epitaxial layer 27 and heat treatment to diffuse the implanted impurities. This allows the p-type column region 4 to be formed without depositing a p-type epitaxial layer, eliminating the need for a process to remove the p-type epitaxial layer in the edge termination region 40. In addition, the n-type impurity buried in the p-type column trench 25B is - The surface of the mold epitaxial layer 27 does not require a step of planarizing the surface using a CMP device, etc. Therefore, the number of manufacturing steps can be reduced, thereby reducing manufacturing costs.

[0131] Furthermore, compared to the multi-stage epitaxial method, the widths of the n-type column region 3 and the p-type column region 4 can be made finer, and for example, the on-resistance can be reduced in an SJ-MOSFET (super junction semiconductor device) 50 with a breakdown voltage of 100V or less. In addition, since the p-type column region 4 is formed by diffusion caused by ion implantation and heat treatment, interdiffusion occurs at the boundary between the p-type column region 4 and the n-type column region 3. Therefore, the conductivity type changes more gradually at the boundary between the p-type column region 4 and the n-type column region 3 than when the p-type column region and the n-type column region are formed by the conventional trench filling method. As a result, the depletion layer is more likely to spread, the electric field is relaxed, and the breakdown voltage can be improved.

[0132] The SJ-MOSFET 50 shown in Fig. 2C is manufactured as follows. First, like the SJ-MOSFET 50 shown in Fig. 2A, the same steps as those shown in Figs. 4 to 17 are performed to form up to the p-type base region 5. Contact plug 19 is formed in the steps shown in Figs. 20 and 21 instead of the steps shown in Figs. 18 and 19.

[0133] 17, a resist mask (not shown) having a desired opening is formed by photolithography on the upper part of the p-type base region 5 via the insulating film 66C. Ion implantation is performed using this resist mask to inject n-type impurities into the surface layer of the p-type base region 5 of the active region 30. + An n-type impurity is implanted to form a source region 6. The n-type impurity is, for example, arsenic (As) or phosphorus (P), etc. After that, the resist mask is removed.

[0134] Next, a resist mask (not shown) having a desired opening is formed by photolithography on the upper part of the p-type base region 5, 5A via the insulating film 66C. Ion implantation is performed using this resist mask to inject p-type impurities into the surface layer of the p-type base region 5, 5A. ++ The p-type impurities that form the p-type contact regions 14, 14A are implanted. ++ The p-type impurities forming the n-type contact regions 14 and 14A are +The n-type impurity forming the n-type source region 6 is implanted at a position deeper than the n-type impurity.

[0135] The surface layer of the p-type base region 5A of the edge termination region 40 is ++ p-type impurities are implanted to form the n-type contact region 14A, + The n-type impurity for forming the n-type source region 6 does not have to be implanted.

[0136] Next, n + Type source region 6 and p ++ A heat treatment is performed to activate the impurities implanted in the contact region 14. The heat treatment to activate the implanted impurities has a smaller thermal budget than the heat treatment to diffuse the implanted impurities. ++ The bottom surface of the contact region 14 is + The n-type source region 6 is formed deeper than the bottom surface of the n-type source region 6. + Type source region 6 and p ++ It is possible to change the order of ion implantation for forming the mold contact region 14. The state up to this point is shown in FIG.

[0137] Next, n - An interlayer insulating film 9 is formed on the entire upper surface (upper surface 100) of the n-type epitaxial layer 27. The interlayer insulating film 9 is formed on, for example, the gate insulating film 7, the gate electrode 8, the n-type epitaxial layer 27, and the n-type epitaxial layer 27 through an insulating film 66C. + Type source region 6, p ++ p-type contact region 14, p-type base region 5A, ++The interlayer insulating film 9 is formed so as to cover the upper portions of the contact region 14A, the field oxide film 13, the field plate 29, and the channel stopper 62. The interlayer insulating film 9 is formed of, for example, boron phosphorus silicate glass (BPSG), phosphorus silicate glass (PSG), or the like. The interlayer insulating film 9 may be a laminated film formed by forming, for example, a high temperature oxide (HTO), non-doped silicate glass (NSG), or tetraethoxysilane (TEOS) film under the BPSG (between the BPSG and the gate electrode 8). The thickness of the interlayer insulating film 9 may be about 1 μm.

[0138] Next, a resist mask (not shown) having an opening is formed on the surface of the interlayer insulating film 9 by, for example, photolithography. Next, an opening is formed in the interlayer insulating film 9 and the insulating film 66C by anisotropic dry etching using the resist mask (the boundary between the gate insulating film 7 formed along the inner wall of the trench 18B and the insulating film 66C covering the upper part of the gate electrode 8 is not shown). Next, recesses 67D, 67E, and 67F are formed by anisotropic dry etching. The recesses 67D, 67E, and 67F become the recesses 67A, 67B, and 67C in FIG. 2C when the SJ-MOSFET 50 is completed.

[0139] In the interlayer insulating film 9 and the insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B of the active region 30, a recess 67D deeper than the upper surface 100 is formed between the adjacent trenches 18B. + Type source region 6 and p ++ The p-type contact region 14 is in contact with (exposed to) the bottom of the recess 67D. ++ The mold contact region 14 is in contact with (exposed to) the recess 67D, which is the contact hole 64D.

[0140] Similarly, a recess 67D deeper than the upper surface 100 is formed between the interlayer insulating film 9 and insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B of the adjacent active region 30 and the interlayer insulating film 9 and insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B provided at the boundary between the active region 30 and the edge termination region 40. + Type source region 6 and p ++ The p-type contact region 14 is in contact with (exposed to) the bottom of the recess 67D. ++ The mold contact region 14 is in contact with (exposed to) the recess 67D, which is the contact hole 64D.

[0141] A recess 67E deeper than the upper surface 100 is formed between the interlayer insulating film 9 and insulating film 66C that are provided so as to cover the upper surface of the gate electrode 8 embedded in the trench 18B provided at the boundary between the active region 30 and the edge termination region 40, and the interlayer insulating film 9 that covers the field plate 29. ++ The mold contact region 14A is in contact with (exposed to) the recess 67E, which is the contact hole 64E.

[0142] A recess 67F is formed in the interlayer insulating film 9 and insulating film 66C covering the field plate 29 and the channel stopper 62. The surface of the field oxide film 13 is exposed at the bottom of the recess 67F, penetrating the field plate 29. The field plate 29 and the field oxide film 13 are in contact (exposed) at the sidewall of the recess 67F. The field oxide film 13 is in contact (exposed) at the bottom of the recess 67F. This recess 67F is a contact hole 64F. It is noted that the field oxide film 13 does not necessarily have to be in contact with the sidewall of the recess 67F.

[0143] After the dry etching for forming the contact holes 64D, 64E, and 64F is performed, the resist mask is removed, and the interlayer insulating film 9 is flattened by carrying out a heat treatment (reflow).

[0144] Next, a barrier metal (not shown) made of a titanium film (Ti), a titanium nitride film (TiN), or a laminated film thereof (e.g., Ti / TiN, etc.) is formed by sputtering from the surface of the interlayer insulating film 9 along the inner walls of the contact holes 64D, 64E, 64F. Next, for example, a tungsten film (W) is formed so as to be embedded in the contact holes 64D, 64E, 64F via the barrier metal.

[0145] Next, the tungsten film is etched back to form contact plugs 19 in the contact holes 64D, 64E, and 64F. The contact plug 19 formed in the contact hole 64D is connected to an n-type semiconductor layer via a barrier metal (not shown). + Type source region 6 and p ++ The contact plug 19 formed in the contact hole 64E is electrically connected to the p-type contact region 14 via a barrier metal (not shown). ++ The contact plug 19 formed in the contact hole 64F is electrically connected to the field plate 29 via a barrier metal (not shown). The state up to this point is shown in FIG.

[0146] Next, a metal film such as aluminum or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu) is formed by sputtering on the top surface of the SJ-MOSFET (super junction semiconductor device) shown in Fig. 21. Next, the metal film is patterned by photolithography and etching techniques to form the source electrode 10, the metal gate runner 61, and the gate electrode pad (not shown).

[0147] The source electrode 10 is p ++ The metal gate runner 61 is electrically connected to the contact plug 19 which is electrically connected to the type contact region 14. The metal gate runner 61 is also electrically connected to the field plate 29. The metal gate runner 61 is further electrically connected to the gate electrode 8, and a gate electrode pad (not shown) is electrically connected to the metal gate runner 61 and the gate electrode 8.

[0148] Next, n + A back electrode 11 is formed on the back surface of the n-type semiconductor substrate 1 (the back surface of the semiconductor base). The back electrode 11 may be formed of a metal film of, for example, nickel (Ni), titanium (Ti), gold (Au), silver (Ag), aluminum (Al), or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu), etc. Alternatively, a laminate film of these (for example, Ti / Ni / Au, Al / Ti / Ni / Au, etc.) may be formed. After the back electrode 11 is formed, a heat treatment is performed to form an n-type electrode. + An ohmic junction is formed between the type semiconductor substrate 1 and the back surface electrode 11. This completes the SJ-MOSFET 50 shown in FIG. 2C.

[0149] The SJ-MOSFET 50 shown in Fig. 2C can also be manufactured as follows. First, like the SJ-MOSFET 50 shown in Fig. 2A, the same steps as those shown in Figs. 4 to 17 are performed to form up to the p-type base region 5. Instead of the steps shown in Figs. 18 and 19, a contact plug 19 is formed in the steps shown in Figs. 22 to 25.

[0150] After the first manufacturing method of the SJ-MOSFET according to the embodiment is performed up to FIG. 17, a mask (not shown) having a desired opening is formed on the surface of the p-type base region 5 by photolithography using, for example, a resist. Using this resist mask as a mask, n-type impurities are ion-implanted. By this ion implantation, n-type impurities are implanted into the surface layer of the p-type base region 5. + An n-type impurity is implanted into the area where the p-type source region 6 is to be formed. The n-type impurity to be implanted is arsenic (As), phosphorus (P), or the like. Note that the surface layer of the p-type base region 5A of the edge termination region 40 is doped with n + The n-type impurity that forms the n-type source region 6 does not need to be implanted. + The ion implantation mask used to form the n-type source region 6 is then removed. + A heat treatment is performed to activate the implanted impurities to form the type source region 6. The state up to this point is shown in FIG.

[0151] Next, n- An interlayer insulating film 9 is formed on the entire upper surface (upper surface 100) of the n-type epitaxial layer 27. The interlayer insulating film 9 is formed on, for example, the gate insulating film 7, the gate electrode 8, the n-type epitaxial layer 27 through the insulating film 66C. + Type source region 6, p ++ p-type contact region 14, p-type base region 5A, ++ The interlayer insulating film 9 is formed so as to cover the upper part of the contact region 14A, the field oxide film 13, the field plate 29 and the channel stopper 62. The interlayer insulating film 9 is formed of, for example, BPSG (Boron Phosphorus Silicate Glass), PSG (Phosphorus Silicate Glass) or the like. The interlayer insulating film 9 may be a laminated film formed by forming, for example, an HTO (High Temperature Oxide), an NSG (None-doped Silicate Glass) or a TEOS (Tetraethoxysilane) film under the BPSG (between the BPSG and the gate electrode 8). The thickness of the interlayer insulating film 9 may be about 1 μm. The state up to this point is shown in FIG. 23.

[0152] Next, a resist mask (not shown) having an opening is formed on the surface of the interlayer insulating film 9 by, for example, photolithography. Next, an opening is formed in the interlayer insulating film 9 and the insulating film 66C by anisotropic dry etching using the resist mask (the boundary between the gate insulating film 7 formed along the inner wall of the trench 18B and the insulating film 66C covering the upper part of the gate electrode 8 is not shown). Next, recesses 67D, 67E, and 67F are formed by anisotropic dry etching. The recesses 67D, 67E, and 67F become the recesses 67A, 67B, and 67C in FIG. 2C when the SJ-MOSFET 50 is completed.

[0153] In the interlayer insulating film 9 and the insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B of the active region 30, a recess 67D deeper than the upper surface 100 is formed between the adjacent trenches 18B. +The p-type source region 6 is in contact with (exposed to) the p-type base region 5. The p-type base region 5 is in contact with (exposed to) the bottom of the recess 67D. This recess 67D is the contact hole 64D.

[0154] Similarly, a recess 67D deeper than the upper surface 100 is formed between the interlayer insulating film 9 and insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B of the adjacent active region 30 and the interlayer insulating film 9 and insulating film 66C covering the upper surface of the gate electrode 8 embedded in the trench 18B provided at the boundary between the active region 30 and the edge termination region 40. + The p-type source region 6 is in contact with (exposed to) the p-type base region 5. The p-type base region 5 is in contact with (exposed to) the bottom of the recess 67D. This recess 67D is the contact hole 64D.

[0155] A recess 67E deeper than upper surface 100 is formed between interlayer insulating film 9 and insulating film 66C provided so as to cover the upper surface of gate electrode 8 embedded in trench 18B provided at the boundary between active region 30 and edge termination region 40, and interlayer insulating film 9 covering field plate 29. P-type base region 5A is in contact with (exposed to) the sidewalls and bottom of recess 67E. This recess 67E is contact hole 64E.

[0156] A recess 67F is formed in the interlayer insulating film 9 and insulating film 66C covering the field plate 29 and the channel stopper 62. The surface of the field oxide film 13 is exposed at the bottom of the recess 67F, penetrating the field plate 29. The field plate 29 and the field oxide film 13 are in contact (exposed) with the sidewall of the recess 67F. The field oxide film 13 is in contact (exposed) with the bottom of the recess 67F. This recess 67F is a contact hole 64F. It is noted that the field oxide film 13 does not necessarily have to be in contact with the sidewall of the recess 67F.

[0157] Next, ion implantation 22 is performed using the interlayer insulating film 9 as a mask to inject p-type impurities into the bottom of the recess 67D and the side and bottom of the recess 67E. ++ The p-type impurities that form the p-type contact regions 14, 14A are implanted into the surface layer of the p-type base region 5A of the edge termination region 40. ++ p-type impurities are implanted to form the n-type contact region 14A, + It is not necessary to implant the n-type impurity that forms the n-type source region 6. The state up to this point is shown in FIG.

[0158] Next, a heat treatment (reflow) is performed to flatten the interlayer insulating film 9. At the same time as the flattening of the interlayer insulating film 9, the p ++ The p-type impurities forming the p-type contact regions 14, 14A may be activated.

[0159] Next, a barrier metal (not shown) made of a titanium film (Ti), a titanium nitride film (TiN), or a laminated film thereof (e.g., Ti / TiN, etc.) is formed by sputtering from the surface of the interlayer insulating film 9 along the inner walls of the contact holes 64D, 64E, 64F. Next, for example, a tungsten film (W) is formed so as to be embedded in the contact holes 64D, 64E, 64F via the barrier metal.

[0160] Next, the tungsten film is etched back to form contact plugs 19 in the contact holes 64D, 64E, and 64F. The contact plug 19 formed in the contact hole 64D is connected to an n-type semiconductor layer via a barrier metal (not shown). + Type source region 6 and p ++ The contact plug 19 formed in the contact hole 64E is electrically connected to the p-type contact region 14 via a barrier metal (not shown). ++ The contact plug 19 formed in the contact hole 64F is electrically connected to the field plate 29 via a barrier metal (not shown). The state up to this point is shown in FIG.

[0161] Next, a metal film such as aluminum or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu) is formed by sputtering on the top surface of the SJ-MOSFET (super junction semiconductor device) shown in Fig. 25. Next, the metal film is patterned by photolithography and etching techniques to form the source electrode 10, the metal gate runner 61, and the gate electrode pad (not shown).

[0162] The source electrode 10 is p ++ The metal gate runner 61 is electrically connected to the contact plug 19 which is electrically connected to the type contact region 14. The metal gate runner 61 is also electrically connected to the field plate 29. The metal gate runner 61 is further electrically connected to the gate electrode 8, and a gate electrode pad (not shown) is electrically connected to the metal gate runner 61 and the gate electrode 8.

[0163] Next, n + A back electrode 11 is formed on the back surface of the n-type semiconductor substrate 1 (the back surface of the semiconductor base). The back electrode 11 may be formed of a metal film of, for example, nickel (Ni), titanium (Ti), gold (Au), silver (Ag), aluminum (Al), or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu), etc. Alternatively, a laminate film of these (for example, Ti / Ni / Au, Al / Ti / Ni / Au, etc.) may be formed. After the back electrode 11 is formed, a heat treatment is performed to form an n-type electrode. + An ohmic junction is formed between the type semiconductor substrate 1 and the back surface electrode 11. This completes the SJ-MOSFET 50 shown in FIG. 2C.

[0164] Next, a second manufacturing method different from the first manufacturing method shown in Figs. 4 to 21 will be described. Figs. 26 to 30 are cross-sectional views showing a state during manufacturing by the second manufacturing method of the SJ-MOSFET according to the embodiment. The second manufacturing method is a method for manufacturing the SJ-MOSFET shown in Fig. 2D. Since the manufacturing method of the edge termination region 40 is the same as the first manufacturing method, Figs. 26 to 30 show cross-sectional views of the active region 30. In the second manufacturing method, the same steps as the first manufacturing method are performed up to the steps shown in Figs. 4 to 8, and n - A type epitaxial layer 27 is formed.

[0165] The second manufacturing method is different from the first manufacturing method in that - 9A. Specifically, in section D1, ion implantation 22 is performed on the entire surface of a predetermined region except for a part of edge termination region 40 to form implantation region 93. The predetermined region is on the active region 30 side of the opening of ion implantation mask 21 that forms p-type column region 4A shown in FIG.

[0166] Here, the depth is n - From the upper surface 100 (surface) of the type epitaxial layer 27 + The implantation depth is n - This is the depth (peak position of the impurity concentration distribution) at which the impurity is implanted from the upper surface 100 (surface) of the type epitaxial layer 27.

[0167] The implantation region 93 formed by the ion implantation 22 indicates a region where the impurity is implanted from the upper surface 100 (peak position of the impurity concentration distribution). - From the upper surface 100 (surface) of the type epitaxial layer 27 - 3 shows the depth to which implanted region 93 is formed in type epitaxial layer 27.

[0168] Furthermore, n - Between the surface (upper surface 100) of the n-type epitaxial layer 27 and the surface of the n-type drift layer 2 ( -The thickness T1 of the flat portion of the n-type epitaxial layer 27 is defined as section D1, and the section from the surface of the n-type drift layer 2 to the bottom of the p-type column trench 25B (the depth of the p-type column trench 25B) is defined as section D2.

[0169] The n shown in Figure 8 - After the step of forming the n-type epitaxial layer 27, - Ion implantation 22 of p-type impurities is performed on a predetermined region from the surface of the n-type epitaxial layer 27. The p-type impurity is, for example, boron (B) or aluminum (Al). - Ion implantation 22 is performed in a predetermined region of the p-type epitaxial layer 27, and it is not necessary to form a new ion implantation mask in the region on the outer periphery side from the opening of the ion implantation mask 21 that forms the p-type column region 4A of the edge termination region 40 where ion implantation 22 is not performed as shown in FIG. 9A. In the region on the outer periphery where ion implantation 22 is not performed, the oxide film 23 shown in FIG. 6 may be left as a mask to prevent p-type impurities from being implanted. In addition, in the region on the outer periphery, - Ion implantation 22 may be performed by forming an ion implantation mask 21 of resist or the like on the surface (upper surface 100) of the type epitaxial layer 27.

[0170] The implanted region 93 formed by the ion implantation 22 is formed in the section D1. When the section D1 is 0.8 μm and the section D2 is 1.0 μm, n - The depth from the surface of the type epitaxial layer 27 to the implantation region 93 is set to 0.4 μm. The section D1 (thickness T1) may be 0.5 μm or more and 1.0 μm or less. - The implantation depth from the surface (upper surface 100) of the type epitaxial layer 27 to the implantation region 93 may be 0.2 μm or more and 1.0 μm or less. Furthermore, the section D2 may be 0.5 μm or more and 2.0 μm or less. The implantation region 93 may be formed at the boundary between the sections D1 and D2. The state up to this point is shown in FIG. 26.

[0171] Next, the mask (not shown) used in the ion implantation 22, such as the oxide film 23 and the ion implantation mask 21 made of resist, is removed, and then heat treatment is performed to diffuse the p-type impurity, thereby forming the p-type column region 4 and the p-type well region 63.

[0172] where n - The p-type epitaxial layer 27 is formed with a lower impurity concentration than the n-type drift layer 2. The p-type impurity is ion-implanted into the implantation region 93 and then annealed to form the n-type - This makes it easier for the impurities to spread into the type epitaxial layer 27 .

[0173] The n-type column regions 3 are formed between adjacent p-type column regions 4, forming parallel pn regions 20. The p-type well region 63 is formed on the entire surface of a predetermined region where the ions 22 have been implanted.

[0174] The impurity concentration of the p-type well region 63 and the p-type column region 4 is highest in the implantation region 93, and decreases in the depth direction as the impurity concentration increases away from the implantation region 93. - From the surface of the epitaxial layer 27, + 1 toward the semiconductor substrate 1.

[0175] After the heat treatment for diffusing the p-type impurities after the ion implantation 22, the oxide film 28 is formed on the surface (upper surface 100) of the p-type well region 63. The oxide film 28 may be formed by the heat treatment for diffusing the p-type impurities after the ion implantation 22.

[0176] When the heat treatment is performed, the shape of the boundary between the p-type column region 4 and the p-type well region 63 (the corner between the p-type column trench 25B and the surface of the n-type drift layer 2) may be rounded by the diffusion of impurities. The state up to this point is shown in FIG.

[0177] In this way, in the second manufacturing method, before forming the trench 18A described later, ion implantation 22 is performed on the entire surface of a predetermined region except for a part of the edge termination region 40 to form an implantation region 93. After the ion implantation 22, a heat treatment is performed to form the p-type column region 4 and the p-type well region 63.

[0178] n - The n-type epitaxial layer 27 is formed to have a lower impurity concentration than the n-type drift layer 2. - Since the difference in impurity concentration between the p-type epitaxial layer 27 and the n-type drift layer 2 is large, the p-type impurity implanted by the ion implantation 22 is unlikely to diffuse into the n-type drift layer 2. - This facilitates diffusion in the type epitaxial layer 27.

[0179] The p-type well region 63 is formed over the entire surface of the predetermined region subjected to ion implantation 22 and contacts the sidewall of the trench 18B, and therefore has the same function as the p-type base region 5 formed in a later process. The p-type impurities implanted by ion implantation 22 are unlikely to diffuse into the n-type drift layer 2, and therefore it is possible to suppress the channel length from being expanded by heat treatment.

[0180] Next, a photoresist mask (not shown) having a predetermined opening is formed on the surface of the oxide film 28 by photolithography. Next, an opening is formed in the oxide film 28 by, for example, anisotropic dry etching using the photoresist mask. Next, the photoresist mask (not shown) is removed, and a trench 18A is formed by anisotropic dry etching using the oxide film 28 as a mask, penetrating the p-type well region 63 and reaching the n-type drift layer 2 (n-type column region 3). In the second manufacturing method, the p-type well region 63 contacts the side wall of the trench 18A. The state up to this point is shown in FIG. 28.

[0181] Next, isotropic etching and sacrificial oxidation are performed with the oxide film 28 remaining. This process removes damage to the trench 18A and rounds the bottom of the trench 18A. The order in which the isotropic etching and the sacrificial oxidation are performed does not matter. It is also possible to perform only one of the isotropic etching and the sacrificial oxidation. Thereafter, the oxide film 28 is removed. The sacrificial oxide film (not shown) may also be removed at the same time as the oxide film 28.

[0182] Next, the surface of the p-type well region 63 (n - A gate insulating film 7 is formed along the upper surface 100 of the type epitaxial layer 27 and the inner wall of the trench 18B. This gate insulating film 7 may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen atmosphere. Also, this gate insulating film 7 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).

[0183] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 7. This polycrystalline silicon layer is formed so as to fill the trench 18B. This polycrystalline silicon layer is patterned by photolithography and etching techniques to form a gate electrode 8 in the trench 18B via the gate insulating film 7. A p-type well region 63 contacts the sidewall of the trench 18B.

[0184] Next, the surface of the p-type well region 63 (n - Ion implantation 22 of p-type impurities, such as boron (B), is performed from the upper surface 100 of the p-type epitaxial layer 27 to form the p-type base region 5. In the active region 30, the gate electrode 8 functions as a mask. The state up to this point is shown in FIG.

[0185] Next, a heat treatment is performed to diffuse the p-type impurities implanted by ion implantation 22, thereby forming the p-type base region 5. The p-type base region 5 is formed in the surface layer of the p-type well region 63, and the impurity concentration of the p-type base region 5 is higher than the impurity concentration of the p-type well region 63. In the depth direction, the bottom surface of the p-type base region 5 is formed shallower than the bottom surface of the p-type well region 63. The p-type base region 5 and the p-type well region 63 are formed so as to contact the sidewall of the trench 18B.

[0186] Similarly, the sidewall of trench 18B (not shown) formed at the boundary between active region 30 and edge termination region 40 is in contact with p-type base region 5 and p-type well region 63 on the active region 30 side, and is in contact with p-type base region 5A and p-type well region 63A on the edge termination region 40.

[0187] When the trench 18B is formed after the p-type well region 63 is formed, the p-type impurities in the p-type well region 63 may diffuse and cause large variations in the gate threshold voltage due to a process in which heat is applied to the SJ-MOSFET (super junction semiconductor device) 50, such as the formation of the oxide film 28, the sacrificial oxide film, and the gate insulating film 7. Therefore, the gate threshold voltage can be stabilized by forming the p-type base region 5 after the formation of the trench 18B (after the formation of the gate electrode 8). The state up to this point is shown in FIG. 30.

[0188] In addition, if the ion implantation 22 of the p-type impurity for forming the p-type base region 5 is not performed, the number of ion implantations can be reduced, and the manufacturing cost can be reduced. + 2D is completed by performing the steps following the step of forming the p-type source region 6. In the second manufacturing method, the p-type well region 63 is different from that in the first manufacturing method in that the p-type well region 63 contacts the side wall of the trench 18B.

[0189] Next, a third manufacturing method different from the second manufacturing method shown in Figs. 26 to 30 will be described. Figs. 31 to 39 are cross-sectional views showing a state during manufacturing by the third manufacturing method of the SJ-MOSFET according to the embodiment. The third manufacturing method is a manufacturing method of the SJ-MOSFET shown in Fig. 2B. In the third manufacturing method, first, the same steps as the first manufacturing method are performed up to the steps shown in Figs. 4 to 8, 9C, and 10C, and the p-type impurity is diffused by heat treatment.

[0190] The third manufacturing method is different from the first manufacturing method in that the p-type column trench 25B is provided with n - The point is that the p-type column regions 4, 4A are formed by implanting ions of the second conductive type impurity only into the region in which the p-type epitaxial layer 27 is buried.

[0191] Next, n - On the surface (upper surface 100) of the type epitaxial layer 27, p -- An ion implantation mask 65 having an opening for forming the type RESURF region 12 is formed. The ion implantation mask 65 is made of, for example, a photoresist. Using the ion implantation mask 65 as a mask, ions of a p-type impurity are implanted. The p-type impurity is, for example, boron (B) or aluminum (Al). The state up to this point is shown in FIG.

[0192] Next, after removing the ion implantation mask 65, a heat treatment is performed to diffuse the implanted p-type impurities, resulting in an n - The surface layer of the p-type epitaxial layer 27 -- A type RESURF region 12 is formed. -- Since the impurity concentration of the resurf region 12 is lower than that of the p-type well region 63A, the p-type well region 63A has p -- The type RESURF region 12 is not formed. -- The bottom surface of the type RESURF region 12 is - The p-type epitaxial layer 27 is formed deeper than the boundary between the p-type drift layer 2. --The bottom surface of the p-type RESURF region 12 may be formed deeper or shallower than the boundary (dotted line) between the p-type column region 4 A and the p-type well region 63 A. The state up to this point is shown in FIG.

[0193] Next, an oxide film 28 is formed on the upper surface 100. The oxide film 28 may be, for example, a LOCOS film. The thickness of the oxide film 28 in the active region 30 is formed to be thinner than the thicker portion of the oxide film 28 formed on the outer periphery of the edge termination region 40. The oxide film 28 is an n - A thick portion is formed on the upper surface of the type epitaxial layer 27, and the bottom surface of the thick portion of the oxide film 28 is formed to a position deeper than the upper surface 100. The end portion of the thick portion of the oxide film 28 on the active region 30 side is continuous from the end portion to a part of the lower surface, and is p -- The oxide film 28 is formed so as to be covered by the type RESURF region 12. The other end of the thick portion of the oxide film 28 is continuous with a part of the lower surface, and has an n-type - The semiconductor layer is then formed so as to be covered with a type epitaxial layer 27. The state up to this point is shown in FIG.

[0194] Next, a resist mask (not shown) having a predetermined opening is formed on the surface of the oxide film 28 by photolithography. Next, openings are formed in the oxide film 28 by dry etching using the resist mask. Next, the resist mask is removed, and the n-type SiO 2 film is removed by anisotropic dry etching using the oxide film 28 as a mask. - From the top surface 100 of the type epitaxial layer 27 - Then, a trench 18A is formed which penetrates the n-type epitaxial layer 27 and reaches the n-type drift layer 2. The state up to this point is shown in FIG.

[0195] Next, isotropic etching and sacrificial oxidation are performed with oxide film 28 still attached. This process removes damage to trench 18A and rounds the bottom of trench 18A. The order of isotropic etching and sacrificial oxidation may be either first. Also, only one of isotropic etching and sacrificial oxidation may be performed. After that, the oxide film 28 in the thin portion used as a mask for forming trench 18A is removed. At this time, the oxide film 28 in the thin portion and the sacrificial oxide film may be removed at the same time. The trench after removing oxide film 28 becomes trench 18B. Since oxide film 28 has a thin portion and a thick portion in edge termination region 40, a full surface etching is performed to remove the thin portion of oxide film 28, and the oxide film in the thick portion of edge termination region 40 is left. The sacrificial oxide film (not shown) may be removed together with the thin portion of oxide film 28. Also, oxide film 28 may be left in edge termination region 40 by removing oxide film 28 using photolithography and etching techniques. The oxide film remaining in edge termination region 40 (thicker portion of oxide film 28) becomes field oxide film 13. The state up to this point is shown in FIG.

[0196] Next, n - Type epitaxial layer 27, p -- A gate insulating film 7 is formed along the surfaces (upper surfaces 100) of the type RESURF region 12 and the p-type well regions 63, 63A and the inner walls of the trench 18B. This gate insulating film 7 may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen atmosphere. Alternatively, this gate insulating film 7 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).

[0197] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 7. This polycrystalline silicon layer is formed so as to fill the trench 18B. This polycrystalline silicon layer is patterned by photolithography and etching techniques to form a gate electrode 8 within the trench 18B via the gate insulating film 7.

[0198] Also, the polysilicon layer formed in edge termination region 40 may be selectively left to serve as field plate 29 and channel stopper 62 .

[0199] Field plate 29 is p -- The field plate 29 is formed continuously on the upper surface of the gate insulating film 7 (insulating film 66A) formed on the type RESURF region 12, the p-type well region 63A, and the p-type base region 5A (upper surface 100), and on the upper surface of the field oxide film 13 on the active region 30 side. The field plate 29 is electrically connected to the gate electrode 8, and also functions as a gate wiring.

[0200] The channel stopper 62 is in contact with the upper surface of the outer periphery of the field oxide film 13 and the n - The field plate 29 and the channel stopper 62 are formed continuously on the upper surface of the gate insulating film 7 (insulating film 66B) formed on the upper surface 100 of the type epitaxial layer 27. The field plate 29 and the channel stopper 62 are separated by the field oxide film 13.

[0201] Next, n - The upper surface 100 of the p-type epitaxial layer 27 (including the p-type well regions 63, 63A and - A p-type impurity ion implantation 22 is performed to form the p-type base regions 5, 5A from the surface of the n-type epitaxial layer 27. The p-type impurity is, for example, boron (B) or aluminum (Al). - In the edge termination region 40 on the n-type epitaxial layer 27, the field plate 29, the channel stopper 62, and the field oxide film 13 function as a mask. - The p-type impurity is not implanted into the p-type epitaxial layer 27. The gate electrode 8 also functions as a mask. The state up to this point is shown in FIG.

[0202] Next, the gate insulating film 7 formed on the upper surface 100 is removed. Note that the gate insulating film 7 is removed when the thickness of the gate insulating film 7 is n + If the thickness does not interfere with the ion implantation for forming the type source region 6, for example, 500 Å or less, this need not be performed.

[0203] Next, the p-type impurities are diffused by heat treatment to form n - The p-type epitaxial layer 27, the p-type well regions 63, 63A, and the p -- P-type base regions 5, 5A are formed in the surface layer of type RESURF region 12. By this heat treatment, an insulating film 66C is formed so as to cover the upper surface of gate electrode 8 made of a polycrystalline silicon layer formed to fill trench 18B, field plate 29, and channel stopper 62.

[0204] The p-type base region 5 and the p-type well region 63 overlap, and the bottom surface of the p-type base region 5 is formed shallower than the bottom surface of the p-type well region 63. The p-type base region 5A and the p-type well region 63A overlap, and the bottom surface of the p-type base region 5A is formed shallower than the bottom surface of the p-type well region 63A.

[0205] The p-type base region 5 and the p-type base region 5A may have the same impurity concentration. The p-type well region 63 and the p-type well region 63A may have the same impurity concentration. The impurity concentration of the p-type base region 5 is higher than the impurity concentration of the p-type well region 63. The impurity concentration of the p-type base region 5A is higher than the impurity concentration of the p-type well region 63A. The p-type base regions 5, 5A are formed to contact the sidewall of the trench 18B.

[0206] In the edge termination region 40, the oxide film 28, the field plate 29, and the channel stopper 62 function as a mask, so that the n-type semiconductor layer 41 is covered with these. - The p-type epitaxial layer 27 and -- Boron (B) is not implanted into the p-type RESURF region 12. As a result, even if a heat treatment is performed to diffuse the p-type impurities that form the p-type base regions 5 and 5A, the n - The p-type epitaxial layer 27 and -- The p-type impurities forming the p-type base regions 5, 5A do not diffuse into the resurf region 12. - The p-type epitaxial layer 27 and -- A type RESURF region 12 remains.

[0207] In this way, in the third manufacturing method, the p-type base region 5 in which the channel is to be formed is formed after the formation of the trench 18B. The state up to this point is illustrated in FIG.

[0208] Next, for example, a mask (not shown) having a desired opening is formed on the surface of the p-type base region 5 by photolithography using a resist. Using this resist mask as a mask, n-type impurities are ion-implanted. By this ion implantation, n-type impurities are implanted into the surface layer of the p-type base region 5. + An n-type impurity is implanted into a portion where a n-type source region 6 is to be formed. The n-type impurity to be implanted is arsenic (As), phosphorus (P), or the like.

[0209] Next, n + The ion implantation mask used for forming the p-type source region 6 is removed. Further, a mask having desired openings is formed on the surface of the p-type base region 5 by using, for example, a resist by photolithography technology, and n + The p-type source region 6 ++ A p-type impurity may be implanted to form the p-type contact region 14. The surface layer of the p-type base region 5A may also be implanted with p-type impurities. ++ In addition, the surface layer of the p-type base region 5A of the edge termination region 40 may be doped with n-type impurities to form the p-type contact region 14A. + The source region 6 is not formed.

[0210] Next, n + Type source region 6 and p ++ A heat treatment is performed to activate the impurities implanted in the contact regions 14 and 14A. The heat treatment to activate the implanted impurities has a smaller thermal budget than the heat treatment to diffuse the implanted impurities. + Type source region 6 and p ++ The order of ion implantation for forming the mold contact regions 14, 14A may be any. The state up to this point is shown in FIG.

[0211] Next, n -An interlayer insulating film 9 is formed on the entire upper surface (upper surface 100) of the n-type epitaxial layer 27. The interlayer insulating film 9 is formed on, for example, the gate insulating film 7, the gate electrode 8, the n-type epitaxial layer 27, and the n-type epitaxial layer 27 through an insulating film 66C. + Type source region 6, p ++ p-type contact region 14, p-type base region 5A, ++ The interlayer insulating film 9 is formed so as to cover the type contact region 14A, the field oxide film 13, the field plate 29 and the channel stopper 62. The interlayer insulating film 9 is formed of, for example, BPSG, PSG or the like. The interlayer insulating film 9 may also be a laminated film formed by forming, for example, an HTO, NSG or TEOS film under the BPSG (between the BPSG and the gate electrode 8). The thickness of the interlayer insulating film 9 may be about 1 μm.

[0212] Next, the interlayer insulating film 9 and the insulating film 66C are patterned by photolithography and etching. + Type source region 6 and p ++ A contact hole 64A is formed exposing the surface of the contact region 14 (the boundary between the gate insulating film 7 formed along the inner wall of the trench 18B and the interlayer insulating film 9 covering the upper part of the gate electrode 8 is not shown). ++ A contact hole 64B is formed exposing the surface of the contact region 14A. Furthermore, a contact hole 64C is formed in the edge termination region 40 exposing the surface of the field plate 29. Thereafter, a heat treatment (reflow) is performed to flatten the interlayer insulating film 9. The state up to this point is shown in FIG.

[0213] Next, a metal film such as aluminum or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu) is formed by sputtering to fill the contact holes 64A, 64B, 64C and to continuously cover the upper surface of the interlayer insulating film 9. Before forming the metal film, a barrier metal (not shown) made of a titanium film (Ti), a titanium nitride film (TiN), or a laminated film of these (for example, Ti / TiN, etc.) may be formed by sputtering along the inner walls of the contact holes 64A, 64B, 64C and continuously on the upper surface of the interlayer insulating film 9. Thereafter, the metal film and the barrier metal (not shown) are patterned by photolithography and etching techniques to form the source electrode 10, the metal gate runner 61, and the gate electrode pad (not shown). The barrier metal may be formed only in the contact holes 64A, 64B, 64C.

[0214] The source electrode 10 is an n-type semiconductor layer having a surface exposed through a contact hole 64A in the active region 30. + Type source region 6 and p ++ The source electrode 10 is electrically connected to the p-type contact region 14 in the edge termination region 40, the surface of which is exposed through the contact hole 64B. ++ 21. The metal gate runner 61 is electrically connected to the gate electrode 8 and the field plate 29 whose surface is exposed in the contact hole 64C. A gate electrode pad (not shown) is electrically connected to the metal gate runner 61 and the gate electrode 8. A tungsten plug or the like may be embedded in the contact holes 64A, 64B, 64C via a barrier metal. The contact holes 64A, 64B, 64C may be contact holes having a recess as in the first manufacturing method shown in FIG.

[0215] Next, n +A back electrode 11 is formed on the back surface of the n-type semiconductor substrate 1 (the back surface of the semiconductor base). The back electrode 11 may be formed of a metal film of, for example, nickel (Ni), titanium (Ti), gold (Au), silver (Ag), aluminum (Al), or an alloy mainly composed of aluminum (Al-Si, Al-Cu, Al-Si-Cu), etc. Alternatively, a laminate film of these (for example, Ti / Ni / Au, Al / Ti / Ni / Au, etc.) may be formed. After the back electrode 11 is formed, a heat treatment is performed to form an n-type electrode. + An ohmic junction is formed between the type semiconductor substrate 1 and the back surface electrode 11. This completes the SJ-MOSFET 50 shown in FIG.

[0216] In this way, the p-type column trench 25B is - Since the second conductive type impurity is ion-implanted only into the region in which the p-type epitaxial layer 27 is buried, the p-type well regions 63 and 63A are not formed.

[0217] As described above, according to the embodiment, edge termination region 40 includes n - A type epitaxial layer is provided, - A field oxide film 13 is provided on the surface of the n-type epitaxial layer 27. - The n-type epitaxial layer 27 - The epitaxial layer 27 and p -- The depletion layer extending from the pn junction with the type RESURF region 12 is called n - By extending the doped epitaxial layer 27, the breakdown voltage of the SJ-MOSFET 50 can be improved.

[0218] In another embodiment, edge termination region 40 is provided with parallel pn structure 20B in which the widths of n-type column regions 3B and p-type column regions 4B are narrower than the widths of n-type column regions 3 and p-type column regions 4 in active region 30. This makes it easier for the depletion layer to spread in edge termination region 40, and enables the breakdown voltage of edge termination region 40 to be made higher than the breakdown voltage of active region 30.

[0219] Furthermore, n -Since the type epitaxial layer 27 has a low impurity concentration, it becomes easier to control the diffusion of the p-type well regions 63, 63A and the p-type base regions 5, 5A, and it is possible to suppress the variation in the gate threshold voltage Vth.

[0220] In addition, since the p-type column region 4 can be formed without depositing a p-type epitaxial layer as in the conventional trench filling method, it is not necessary to remove the p-type epitaxial layer on the surface using a CMP device or the like and then form an n-type epitaxial layer on the surface after the p-type epitaxial layer is removed. Furthermore, the surface portion in which the p-type column trenches 25B are filled does not require a process of planarizing using a CMP device or the like. Therefore, the SJ structure can be easily formed and the manufacturing cost can be reduced.

[0221] In the above, the present invention has been described with reference to an example in which a MOS gate structure is formed on the first main surface of a silicon substrate, but the present invention is not limited to this, and the type of semiconductor (e.g., silicon carbide (SiC) and the like), the surface orientation of the main surface of the substrate, and the like can be changed in various ways. In addition, in the embodiments of the present invention, a trench-type MOSFET has been described with reference to an example, but the present invention is not limited to this, and the present invention is applicable to semiconductor devices of various configurations, such as super-junction semiconductor devices such as planar-type MOSFETs and super-junction semiconductor devices such as IGBTs (Insulated Gate Bipolar Transistors). In addition, in each embodiment of the present invention, the first conductivity type is n-type and the second conductivity type is p-type, but the present invention is similarly valid even if the first conductivity type is p-type and the second conductivity type is n-type. [Industrial Applicability]

[0222] INDUSTRIAL APPLICABILITY As described above, the super junction semiconductor device and the method of manufacturing the super junction semiconductor device according to the present invention are useful for high voltage semiconductor devices used in power conversion devices and power supply devices for various industrial machines and the like. [Explanation of symbols]

[0223] 1n + Semiconductor Substrate 2 n-type drift layer 3,3B n-type column region 4,4A,4B p-type column region 5,5A p-type base region 6n + Type Source Area 7 Gate insulating film 8. Gate electrode 9 Interlayer insulating film 10 Source electrode 11 Back electrode 12 pages -- Type RESURF region 13 Field oxide 14,14A p ++ Mold Contact Area 18A, 18B Trench 19 Contact plug 20, 20B parallel pn area 21, 65 Ion implantation mask 22 Ion Implantation 23 Oxide film 24 Resist mask 25A, 25B Trench for p-type columns 27 n - Type epitaxial layer 28 Oxide Film 29 Field Plate 30 active area 40 Edge Termination Area 50 SJ-MOSFET 61 Metal Gate Runner 62 Channel Stopper 63, 63A, 63B p-type well region 64A, 64B, 64C, 64D, 64E, 64F Contact holes 66A, 66B, 66C Insulating film 67A, 67B, 67C, 67D, 67E, 67F Recess 90, 91-1,91-2,92,93 injection area 100 Top W1, W2, W3 width T1 Thickness D1,D2 section

Claims

1. 1. A method for manufacturing a super-junction semiconductor device having an active region through which a current flows, and a termination structure disposed outside the active region and having a breakdown voltage structure surrounding the active region, comprising: a first step of forming a first semiconductor layer of a first conductivity type on a front surface of a semiconductor substrate of a first conductivity type, the first semiconductor layer having an impurity concentration lower than that of the semiconductor substrate; a second step of forming a first trench from a surface of the first semiconductor layer; a third step of forming a second semiconductor layer of a first conductivity type having an impurity concentration lower than that of the first semiconductor layer on a surface of the first semiconductor layer and within the first trench; a fourth step of forming a well region of the second conductivity type in the second semiconductor layer by injecting an impurity of a second conductivity type into the second semiconductor layer, and forming a parallel pn structure in which first columns of the first conductivity type and second columns of the second conductivity type are repeatedly and alternately arranged in a direction parallel to the front surface, the parallel pn structure having an upper surface of the second columns contacting a bottom surface of the well region; a fifth step of forming a second trench penetrating the second semiconductor layer and reaching the first column; a sixth step of forming a second semiconductor region of a second conductivity type on a surface of the parallel pn structure of the active region; a seventh step of forming a gate insulating film and a gate electrode inside the second trench; an eighth step of selectively forming a first semiconductor region of a first conductivity type in a surface layer of the second semiconductor region in the active region; 2. A method for manufacturing a super-junction semiconductor device comprising:

2. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the sixth step, the bottom surface of the second semiconductor region is formed to be shallower than the bottom surface of the well region.

3. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the sixth step, the well region is formed so that the impurity concentration therein is lower than the impurity concentration of the second semiconductor region.

4. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the fourth step, an impurity that imparts the second conductivity type to the second semiconductor layer in the first trench is implanted.

5. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the fourth step, an impurity having the second conductivity type is implanted into a surface layer of the second semiconductor layer on a surface of the first semiconductor layer.

6. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the fourth step, the second column is also formed in the termination structure portion.

7. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein the sixth step is carried out before the fifth step.

8. 2. The method for manufacturing a super-junction semiconductor device according to claim 1, wherein in the fourth step, an impurity having the second conductivity type is implanted only into the second semiconductor layer in the first trench.

9. 1. A super-junction semiconductor device having an active region through which a current flows, and a termination structure disposed outside the active region and having a breakdown voltage structure surrounding the active region, a first semiconductor layer of a first conductivity type provided on a front surface of a semiconductor substrate of a first conductivity type and having a lower impurity concentration than the semiconductor substrate; a parallel pn structure in which first columns of a first conductivity type and second columns of a second conductivity type are repeatedly and alternately arranged in a direction parallel to the front surface, the parallel pn structure being provided within the first semiconductor layer; a second semiconductor region of a second conductivity type provided in a surface layer of the parallel pn structure of the active region; a first semiconductor region of a first conductivity type selectively provided in a surface layer of the second semiconductor region of the active region; a second trench passing through the first semiconductor region and the second semiconductor region and reaching the first column; a gate electrode provided in the second trench via a gate insulating film; a well region of a second conductivity type is provided within the first semiconductor layer, a lower surface of the well region is in contact with an upper surface of the second column, a bottom surface of the well region is deeper than a bottom surface of the second semiconductor region, and a width of the upper surface of the well region is wider than a width of the second column; a second semiconductor layer of a first conductivity type having an impurity concentration lower than that of the first semiconductor layer on a surface of the first semiconductor layer of the termination structure; a second conductivity type RESURF region having a lower impurity concentration than the well region on a surface of the first semiconductor layer of the termination structure, a bottom surface of said resurf region being located deeper than a boundary between said first semiconductor layer and said second semiconductor layer,

10. 10. The super-junction semiconductor device according to claim 9, wherein the impurity concentration of the well region is lower than the impurity concentration of the second semiconductor region.

11. 10. The super-junction semiconductor device according to claim 9, wherein the parallel pn structure is also provided in the termination structure portion.

12. 10. The superjunction semiconductor device according to claim 9, wherein a repeat pitch of the parallel pn structure in the termination structure is narrower than a repeat pitch of the parallel pn structure in the active region.

13. The superjunction semiconductor device of claim 9, wherein the well region and the second semiconductor region are in contact with a sidewall of the second trench.

14. The superjunction semiconductor device as described in Claim 9, characterized in that the second semiconductor layer is also provided between the well region and the resurf region, which are provided at the outermost part of the termination structure portion.

15. The superjunction semiconductor device according to claim 9, wherein the impurity concentration of the well region is higher than the impurity concentration of the second column.

Citation Information

Patent Citations

  • Semiconductor device

    JP2004241768A

  • Semiconductor device

    JP2007173418A

  • Semiconductor device, and its fabrication process

    JP2007300034A

  • Semiconductor device

    JP2009147234A

  • Semiconductor device manufacturing method

    JP2016021547A