Method for manufacturing chip configuration wafer

By irradiating the processed wafer from the opposite side and adjusting the beveling portion and depth of altered layer formation, the method ensures effective separation of SiC wafers with beveled edges, maintaining wafer area and efficiency.

JP7585714B2Active Publication Date: 2024-11-19DENSO CORP +3
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020180823
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-11-19
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

The challenge in separating SiC wafers with beveled portions using laser beams is that the laser beam scattering prevents proper formation of altered layers, making it difficult to separate chip-constituting wafers from processed wafers.

Method used

Irradiate the processed wafer from the opposite side to form an altered layer along the surface direction, ensuring the laser beam is focused near the outer edge by adjusting the beveling portion to have a larger area on one side than the other and setting the depth of the altered layer formation to avoid intersection with the beveling portion.

Benefits of technology

This method allows for easy and complete formation of altered layers up to the edge of the processed wafer, facilitating easy separation of chip-constituting wafers without reducing the usable area of the SiC wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585714000001
    Figure 0007585714000001
  • Figure 0007585714000002
    Figure 0007585714000002
  • Figure 0007585714000003
    Figure 0007585714000003
Patent Text Reader

Abstract

To easily separate a chip constitution wafer from a processing wafer in which a beveling part is formed.SOLUTION: A manufacturing method of a chip constitution wafer includes: forming an epitaxial film consisting of Sic on a first principal surface of an SiC wafer, and preparing a processing wafer 20 defining a surface at the side of the epitaxial film as one face 20a and defining a surface at the side of the SiC wafer as another face 20b; forming an altered layer by irradiating the inside of the processing wafer 20 with laser beams from the other face 20b of the processing wafer 20; separating the processing wafer 20 into a chip constitution wafer at the side of the one face 20a of the processing wafer 20 and a recycle wafer at the side of the other face 20b of the processing wafer 20 by separating the processing wafer 20 with the altered layer defined as a boundary; and utilizing the recycle wafer as an SiC wafer again. In preparing the processing wafer 20, a processing wafer in which a beveling part 21 where an area of the other face 20b is larger than that of the one face 20a is formed at an outer edge of the processing wafer 20 is prepared.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a processing wafer made of silicon carbide (hereinafter simply referred to as SiC). Ha The present invention relates to a method for manufacturing a chip configuration wafer. [Background technology]

[0002] A method has been proposed for irradiating a SiC ingot having a first main surface and a second main surface with a laser beam to separate the SiC ingot into SiC wafers (see, for example, Patent Document 1). Specifically, in this method, a laser beam is irradiated from the normal direction of the second main surface of the SiC ingot to form an altered layer in the SiC ingot, and the SiC wafers are separated from the SiC ingot at the altered layer as a boundary. In this case, the second main surface is composed of a C-plane. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-111143 A Summary of the Invention [Problem to be solved by the invention]

[0004] When a semiconductor chip is formed using the above-mentioned SiC wafer, the semiconductor chip is formed, for example, as follows. That is, first, an epitaxial film is formed on the SiC wafer to form a processed wafer, and semiconductor elements are formed on the processed wafer. After that, the processed wafer is thinned to a desired thickness to form a chip-configured wafer, and the chip-configured wafer is divided into chip units to form the semiconductor chip.

[0005] In this case, when thinning the processed wafer to form a chip-constituting wafer, it is possible to irradiate the processed wafer with laser light to form an altered layer and separate the portion to be thinned using the altered layer as a boundary, just as in separating the SiC wafer from the above-mentioned SiC ingot.

[0006] Incidentally, when forming a semiconductor chip, it is considered to form a beveled portion on the outer edge of the processed wafer in order to make it easier to form a semiconductor element or to make the processed wafer easier to handle. However, when attempting to form an altered layer by irradiating a laser beam onto a processed wafer on which a beveled portion has been formed, the laser beam is scattered at the beveled portion because the laser beam is not perpendicular to the beveled portion, and there is a possibility that an altered layer will not be formed properly inside. For this reason, in the case of a processed wafer on which a beveled portion has been formed, there is a possibility that it will be difficult to separate the chip-constituting wafer from the processed wafer.

[0007] In view of the above, the present invention is to facilitate separation of a chip-constituting wafer from a processed wafer on which a beveled portion is formed. Ruchi The present invention aims to provide a method for manufacturing a top configuration wafer. [Means for solving the problem]

[0008] In claim 1 for achieving the above object, there is provided a method for manufacturing a chip-configured wafer on which semiconductor elements are formed, comprising the steps of: preparing a SiC wafer (1) having a first main surface (1a) and a second main surface (1b) opposite to the first main surface and made of SiC; forming an epitaxial film (2) made of SiC on the first main surface of the SiC wafer; preparing a processed wafer (20) having a surface on the epitaxial film side as one surface (20a) and a surface on the SiC wafer side as the other surface (20b); and applying laser light to the inside of the processed wafer from the other surface of the processed wafer. By irradiating the processed wafer with laser light (L), an altered layer (23) is formed along the surface direction of the processed wafer, and the processed wafer is separated at the altered layer as a boundary to separate the processed wafer into a chip configuration wafer (50) on one side of the processed wafer and a recycled wafer (60) on the other side of the processed wafer, and the recycled wafer is reused as a SiC wafer. In preparing the processed wafer, a beveled portion (21) is formed on the outer edge of the processed wafer, the area of ​​which is larger on the other side than on the one side.

[0009] According to this, when forming an altered layer inside the processed wafer by irradiating the laser light, the laser light can be easily irradiated up to the very edge of the processed wafer, compared to when the area of ​​the other side of the processed wafer is equal to or smaller than the area of ​​the one side, so that the altered layer can be easily formed up to the edge of the processed wafer, and the chip configuration wafer can be easily separated from the processed wafer.

[0012] The reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]

[0013] [Figure 1A] 2A to 2C are cross-sectional views illustrating a manufacturing process of the semiconductor chip in the first embodiment. [Figure 1B] 1B is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1A. [Figure 1C] 1C is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1B. [Figure 1D] 1D is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1C. [Figure 1E] 1D; FIG. 1E is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. [Figure 1F] 1C is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1E. [Figure 1G] 1C is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1F. [Figure 1H] 1C is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1G. [Figure 1I] 1C is a cross-sectional view showing a manufacturing process of the semiconductor chip subsequent to FIG. 1H. [Figure 1J] 1I is a cross-sectional view showing a manufacturing process of the semiconductor chip following FIG. 1I. [Figure 1K] FIG. 1C is a cross-sectional view of a processed wafer obtained by forming an epitaxial film for thickness on a recycled wafer formed in the step of FIG. 1F. [Diagram 2] FIG. 1B is a plan view of the SiC wafer shown in FIG. 1A. [Diagram 3] 1D is a schematic cross-sectional view showing a beveled portion of the processed wafer shown in FIG. 1C. FIG. [Figure 4] 1F is a schematic diagram showing a path of laser light when irradiating the processed wafer of FIG. 1E. FIG. [Diagram 5] 1F is a schematic plan view showing an altered layer when the processed wafer of FIG. 1E is irradiated with laser light. FIG. [Figure 6] 1F is a schematic cross-sectional view showing an altered layer when the processed wafer of FIG. 1E is irradiated with laser light. FIG. [Figure 7] 1F is a schematic cross-sectional view showing the relationship between an altered layer and the shape of a beveled portion when the processed wafer of FIG. 1E is irradiated with laser light. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In the following embodiments, parts that are the same or equivalent to each other will be denoted by the same reference numerals.

[0015] (First embodiment) A method for manufacturing the semiconductor chip 100 in the first embodiment will be described with reference to the drawings.

[0016] 1A, a bulk-wafer-shaped SiC wafer 1 having a first main surface 1a and a second main surface 1b is prepared. The thickness of the SiC wafer 1 is arbitrary, but is set to, for example, about 325 to 525 μm.

[0017] The SiC wafer 1 of this embodiment is a 6-inch hexagonal single crystal wafer, and as shown in FIG. 1A and FIG. 2, the entirety is substantially disk-shaped. In the SiC wafer 1 of this embodiment, the area of ​​the second main surface 1b is larger than the area of ​​the first main surface 1a, and the side surface 1c connecting the first main surface 1a and the second main surface 1b is curved. In the SiC wafer 1, the Si surface is the first main surface 1a, and the C surface is the second main surface 1b. Since the laser light L is irradiated from the second main surface 1b side in the process of FIG. 1E described later, the second main surface 1b is made into a mirror surface by mirror processing or the like. The mirror processing is performed, for example, by polishing using a grinder or polishing such as CMP (short for Chemical Mechanical Polishing).

[0018] In addition, the SiC wafer 1 has a c-axis extending from the first main surface 1a to the second main surface 1b (i.e., <0001> The first main surface 1a has an off-axis direction ({0001} direction) 10 and a c-plane ({0001} plane) 11 perpendicular to the c-axis 10. In this embodiment, the c-axis 10 is inclined with respect to a perpendicular line 12 to the first main surface 1a, and the c-plane 11 and the first main surface 1a have a predetermined off-angle α. The off-angle is, for example, about 4°. However, the off-angle α is not limited to this and is appropriately set depending on the semiconductor element to be manufactured, for example, within a range of less than 10°.

[0019] Furthermore, an orientation flat 13 indicating a crystal orientation is formed on the SiC wafer 1. In this embodiment, the orientation flat 13 is formed so as to be parallel to the off-direction A, where the direction from the perpendicular line 12 toward the c-axis 10 is defined as the off-direction A.

[0020] The SiC wafer 1 can also be prepared by reusing a recycled wafer 60 formed in the process of Fig. 1F described later. For this reason, a protective film made of an oxide film or the like may be formed on the second main surface 1b or the like of the SiC wafer 1, as necessary.

[0021] 1B, an epitaxial film 2 is formed on the first main surface 1a of the SiC wafer 1 to prepare a processed wafer 20 having one surface 20a, another surface 20b opposite to the one surface 20a, and a side surface 20c connecting the one surface 20a and the other surface 20b. A chip formation region RA in which a semiconductor element, which will be described later, is formed is formed on the one surface 20a side of the processed wafer 20.

[0022] In this embodiment, the epitaxial film 2 is - The epitaxial layer is called n type. - The mold epitaxial layer is a portion where one-side element components 22 such as a diffusion layer described later are formed, and has a thickness of, for example, about 10 μm. In the following, the surface of the processed wafer 20 facing the epitaxial film 2 is referred to as one surface 20a of the processed wafer 20, the surface of the processed wafer 20 facing the SiC wafer 1 is referred to as the other surface 20b of the processed wafer 20, and the surface connecting the one surface 20a and the other surface 20b is referred to as the side surface 20c.

[0023] In addition, the processed wafer 20 is prepared with a beveled portion 21 formed on the side surface 20c, which is the outer edge portion. Specifically, as shown in Fig. 3, the beveled portion 21 is formed so that, when a plane passing through the center between the one surface 20a and the other surface 20b of the processed wafer 20 and along the surface direction of the processed wafer 20 is taken as a horizontal imaginary plane K, the part on the one surface 20a side and the part on the other surface 20b side are asymmetrical with respect to the horizontal imaginary plane K. More specifically, the beveled portion 21 is formed so that the area of ​​the other surface 20b of the processed wafer 20 is larger than the area of ​​the one surface 20a. In other words, the beveling portion 21 is formed so that, if a plane passing through the boundary between the one surface 20a and the beveling portion 21 and perpendicular to the horizontal virtual surface K is defined as a first orthogonal virtual surface K1, and a plane passing through the boundary between the other surface 20b and the beveling portion 21 and perpendicular to the horizontal virtual surface K is defined as a second orthogonal virtual surface K2, the second orthogonal virtual surface K2 is located closer to the outer edge of the processed wafer 20 than the first orthogonal virtual surface K1. In other words, the beveling portion 21 is formed so that the curvature of the portion on the other surface 20b side from the horizontal virtual surface K is larger than the curvature of the portion on the one surface 20a side from the horizontal virtual surface K. In this embodiment, for example, if the length between the intersection of the horizontal virtual surface K and the side surface 20c and the first orthogonal virtual surface K1 is defined as a length d, the beveling portion 21 is formed so that the length d is 100 μm or more.

[0024] Such a processed wafer 20 is prepared, for example, as follows. That is, for example, when preparing a SiC wafer 1, as described above, a wafer having a first main surface 1a with a larger area than the second main surface 1b and a curved side surface 1c is prepared. As a result, when the epitaxial film 2 is formed on the first main surface 1a of the SiC wafer 1, the shape of the epitaxial film 2 inherits the shape of the underlying SiC wafer 1, so that a processed wafer 20 is prepared in which the area of ​​the other surface 20b is larger than the area of ​​the one surface 20a. In addition, such a processed wafer 20 is prepared, for example, by forming the epitaxial film 2 on the first main surface 1a of the SiC wafer 1, and then performing a shape adjustment process such as etching as appropriate to form the beveling portion 21.

[0025] 1C, a general semiconductor manufacturing process is performed to form one-side element components 22 of the semiconductor element, such as gate electrodes 14, diffusion layers (not shown), surface electrodes, wiring patterns, and passivation films, in each chip formation region RA. Note that the semiconductor elements employed here may have various configurations, such as power devices. Thereafter, a surface protection film made of resist or the like is formed on one surface 20a of the processed wafer 20 as necessary.

[0026] Next, as shown in FIG. 1D, a holding member 30 is placed on one surface 20a of the processed wafer 20. For example, a dicing tape having a base material 31 and an adhesive 32 is used as the holding member 30. The base material 31 is made of a material that is not easily warped during the manufacturing process, such as glass, a silicon substrate, or ceramics. The adhesive 32 is made of a material that can change its adhesive strength, such as a material whose adhesive strength changes depending on temperature or light. In this case, the adhesive 32 is made of, for example, an ultraviolet curing resin, wax, or double-sided tape. However, the adhesive 32 is made of a material that maintains its adhesive strength even when forming the other surface side element component 25 of FIG. 1G, which will be described later.

[0027] Next, as shown in Fig. 1E, a laser beam L is irradiated from the normal direction to the other surface 20b of the processed wafer 20, and an altered layer 23 is formed along the surface direction of the processed wafer 20 at a position that is a predetermined depth H from the other surface 20b of the processed wafer 20. In this embodiment, the predetermined depth H when forming the altered layer 23 is set according to the ease of handling of the chip-configuration wafer 50 described later and the withstand pressure of the semiconductor chip 100 described later, and is set to about 200 to 370 µm, for example, so that the thickness of the chip-configuration wafer 50 is about 100 µm. Note that the depth here refers to the length in the direction from the other surface 20b along the one surface 20a, and the length along the depth direction that is the normal direction of the other surface 20b.

[0028] The process of forming the deteriorated layer 23 will be specifically described below. When forming the deteriorated layer 23, first, a laser device is prepared that has a laser light source that oscillates the laser light L, a mirror arranged to change the direction of the optical axis (i.e., optical path) of the laser light L, a focusing lens (i.e., focusing optical system) for focusing the laser light L, a displaceable stage, and the like. When forming the deteriorated layer 23, the processed wafer 20 is placed on the stage, and the laser light L is irradiated from the other surface 20b of the processed wafer 20 so that the focusing point of the laser light L is at a predetermined depth H, while the position of the stage, etc. is adjusted so that the focusing point of the laser light L is relatively scanned along the surface direction of the processed wafer 20.

[0029] More specifically, the modified layer 23 is formed as follows. That is, as shown in FIG. 4, if the off-direction A is the Y direction, and the surface direction perpendicular to the Y direction and parallel to one surface 20a of the processed wafer 20 is the X direction, the laser light L is scanned along the X direction, and then shifted in the Y direction and scanned again along the X direction. As a result, inside the processed wafer 20, as shown in FIG. 5 and FIG. 6, the laser light L is irradiated to separate SiC into amorphous Si and amorphous C, and the laser light L is efficiently absorbed by the separated amorphous C to form the modified layer 23a. In addition, a crack 23b propagating from the modified layer 23a along the c-plane 11 is formed. As a result, the modified layer 23 formed of the modified layer 23a and the crack 23b is formed inside the processed wafer 20.

[0030] 6 is a schematic cross-sectional view taken along line VI-VI in FIG. 5. The amount by which the laser light L is shifted in the Y direction (i.e., the index amount) is set based on the width of the crack 23b formed by propagation in the c-plane direction. For example, in this embodiment, when the width of the crack 23b formed on one side of the modified layer 23a is W1, and the index amount in the Y-axis direction is W, the crack is formed to satisfy W1≦W≦2×W1.

[0031] In this embodiment, for example, the laser output is 2.0 W, the feed rate is 785 mm / s, and the processing time is about 15 minutes when forming the affected layer 23. However, these conditions are only an example, and the inventors have confirmed that, for example, even when the laser output is higher or lower than 2.0 W, the affected layer 23 can be appropriately formed by adjusting each condition.

[0032] Here, the processed wafer 20 has a beveled portion 21. Therefore, when the laser light L is irradiated from the other surface 20b of the processed wafer 20 as described above, the laser light may be scattered in the beveled portion 21, and thus an altered layer 23 may not be appropriately formed inside the beveled portion 21.

[0033] For this reason, in this embodiment, as described above, the beveled portion 21 is formed so that the area of ​​the other side 20b of the processed wafer 20 is larger than the area of ​​the one side 20a. Therefore, compared to a case where the beveled portion 21 is formed so that the area of ​​the other side 20b of the processed wafer 20 is equal to or smaller than the area of ​​the one side 20a, it is easier to irradiate the laser light L up to the very edge of the processed wafer 20. Therefore, it is easier to form the altered layer 23 up to the outer edge of the processed wafer 20.

[0034] In this embodiment, the beveling portion 21 and the depth H are adjusted so that the deteriorated layer 23 does not intersect with the second orthogonal virtual plane K2, as shown in FIG. 7. In other words, the beveling portion 21 and the depth H are adjusted so that the depth h from the boundary between the other surface 20b and the beveling portion 21 to the side surface 20c is shorter than the depth H in the depth direction. In other words, the depth h from the boundary between the other surface 20b and the beveling portion 21 to the side surface 20c is the length of the portion located inside the processed wafer 20 in the second orthogonal virtual plane K2. As a result, the other surface 20b is located in a portion opposite to the portion where the deteriorated layer 23 is formed, so that the laser light L can be sufficiently focused on the portion where the deteriorated layer 23 is formed.

[0035] Next, as shown in FIG. 1F, an auxiliary member 40 is placed on the other surface 20b side of the processed wafer 20. The auxiliary member 40 is composed of a base material 41 and an adhesive 42 capable of changing adhesive strength, similar to the holding member 30. In this case, the base material in the auxiliary member 40 is composed of, for example, glass, a silicon substrate, ceramics, etc., and the adhesive 42 in the auxiliary member 40 is composed of, for example, ultraviolet curing resin, wax, double-sided tape, etc. Then, the holding member 30 and the auxiliary member 40 are gripped and a tensile force or the like is applied in the thickness direction of the processed wafer 20, and the chip configuration wafer 50 and the recycled wafer 60 are separated with the affected layer 23 as the boundary (i.e., the starting point of branching).

[0036] In the following description, the surface of the chip configuration wafer 50 on which the one-side element configuration portion 22 is formed is referred to as one surface 50a, the separated surface of the chip configuration wafer 50 is referred to as the other surface 50b, and the separated surface of the recycled wafer 60 is referred to as the one surface 60a. In addition, in each of the figures from FIG. 1F onwards, the affected layer 23 remaining on the other surface 50b of the chip configuration wafer 50 and the one surface 60a of the recycled wafer 60 are omitted as appropriate.

[0037] Thereafter, as shown in FIG. 1G, a typical semiconductor manufacturing process is performed to form other surface side element components 25 of the semiconductor element, such as metal film 24 constituting a back electrode, on the other surface 50b of chip configuration wafer 50.

[0038] Before the step of forming the other surface side element component 25, a step of planarizing the other surface 50b of the chip configuration wafer 50 by a CMP (short for chemical mechanical polishing) method or the like may be performed as necessary. FIG. 1G shows a diagram of the case where the other surface 50b of the chip configuration wafer 50 is planarized. After the step of forming the other surface side element component 25 is performed, a heat treatment such as laser annealing may be performed as necessary to make the metal film 24 and the other surface 50b of the chip configuration wafer 50 into ohmic contact.

[0039] 1H, a support member 70 is placed on the other surface 50b side of the chip configuration wafer 50, that is, on the metal film 24 side. The support member 70 is made of, for example, a dicing tape or the like, but may be made of a base material 71 and an adhesive 72 capable of changing the adhesive strength, similar to the holding member 30. When the holding member 70 is made of the base material 71 and the adhesive 72, the base material 71 is made of, for example, glass, a silicon substrate, ceramics, etc., and the adhesive 72 is made of, for example, an ultraviolet curing resin, wax, double-sided tape, etc.

[0040] 1I, the adhesive force of the adhesive 32 in the holding member 30 is weakened, and the holding member 30 attached to one surface 50a of the chip configuration wafer 50 is peeled off. For example, when the adhesive 32 is made of an ultraviolet curing resin, the holding member 30 is peeled off by irradiating it with ultraviolet light.

[0041] 1J, the chip configuration wafer 50 is diced into individual chip units by a dicing saw or laser dicing, to form each semiconductor chip 100. At this time, in this embodiment, the dicing depth is adjusted so that the base material 71 of the support member 70 remains connected without being cut while the chip configuration wafer 50 is divided into chip units.

[0042] Although the subsequent steps are not shown, the support member 70 is expanded to widen the gap between each semiconductor chip 100 at the diced cut portions. Thereafter, the adhesive strength of the adhesive 72 is weakened by heat treatment or light irradiation, and the semiconductor chip 100 is picked up. In this manner, the semiconductor chip 100 is manufactured.

[0043] 1F is used again as the SiC wafer 1 to carry out the steps in and after FIG. 1A. This allows the SiC wafer 1 to be used multiple times to form the semiconductor chip 100. In this case, it is preferable that the one surface 60a of the separated side of the recycled wafer 60 is flattened and the one surface 60a of the SiC wafer 1 is processed by a CMP method using a polishing device or dry etching so that the deteriorated layer 23 does not remain. In addition, when the thickness of the recycled wafer 60 (i.e., the SiC wafer 1) becomes thin, as shown in FIG. 1K, a thickness epitaxial film 3 for ensuring the thickness of the SiC wafer 1 may be formed to obtain the SiC wafer 1, and an epitaxial film 2 may be formed on the SiC wafer 1 to obtain the processed wafer 20. The thickness epitaxial film 3 may be, for example, n + The epitaxial layer for thickness determination is made up of a type epitaxial layer. When the epitaxial film for thickness determination 3 is formed, the shape adjustment process for forming the beveling portion 21 may be performed after the epitaxial film for thickness determination 3 is formed, or may be performed after the epitaxial film for thickness determination 3 is formed. When the shape adjustment process is performed after the epitaxial film for thickness determination 3 is formed, the epitaxial film 2 takes on the shape of the epitaxial film for thickness determination 3 when the epitaxial film 2 is formed, and thus the beveling portion 21 is formed.

[0044] According to the present embodiment described above, the beveling portion 21 is formed so that the area of ​​the other side 20b of the processed wafer 20 is larger than the area of ​​the one side 20a. Therefore, when the deteriorated layer 23 is formed inside the processed wafer 20 by irradiating the laser light L, the laser light L is more likely to be irradiated up to the immediate vicinity of the outer edge of the processed wafer 20 compared to a case in which the area of ​​the other side 20b of the processed wafer 20 is equal to or smaller than the area of ​​the one side 20a. Therefore, the deteriorated layer 23 can be easily formed up to the outer edge of the processed wafer 20, and the chip configuration wafer 50 can be easily separated from the processed wafer 20.

[0045] Incidentally, when the laser light L is irradiated to the outer edge of the processed wafer 20, it is also possible to perform edge trimming to remove the beveling portion 21 before irradiating the laser light L, so that the side surface 20c of the processed wafer 20 is perpendicular to the surface 20a. However, this method reduces the area of ​​the processed wafer 20. In particular, in this embodiment, the processed wafer 20 is separated into the chip-configuration wafer 50 and the recycled wafer 60 at the boundary of the altered layer 23, and the separated recycled wafer 60 is reused as the SiC wafer 1. For this reason, in the method of removing the beveling portion 21, the area of ​​the SiC wafer 1 is reduced each time the chip-configuration wafer 50 is formed, and the number of semiconductor chips 100 manufactured gradually decreases.

[0046] In contrast, in this embodiment, it is only necessary to adjust the shape of the beveling portion 21, and therefore it is possible to prevent the area of ​​the SiC wafer 1 from becoming smaller. Therefore, in this embodiment, it is possible to preferably separate the processed wafer 20 into the chip configuration wafer 50 and the recycled wafer 60 (i.e., the SiC wafer 1) while preventing the SiC wafer 1 from becoming smaller every time a semiconductor chip 100 is manufactured.

[0047] (1) In this embodiment, the beveling portion 21 is formed so that the curvature of the portion on the other surface 20b side of the horizontal imaginary plane K is larger than the curvature of the portion on the one surface 20a side of the horizontal imaginary plane K. This makes it possible to easily configure a processed wafer 20 in which the area of ​​the other surface 20b is larger than the area of ​​the one surface 20a.

[0048] (2) In this embodiment, the beveled portion 21 and the depth H are adjusted such that the depth h from the boundary between the other surface 20b and the beveled portion 21 to the side surface 20c in the depth direction is shorter than the depth H. As a result, the other surface 20b is located in a portion opposite to the portion where the deteriorated layer 23 is to be formed, so that the laser light L can be sufficiently focused on the portion where the deteriorated layer 23 is to be formed. This makes it possible to prevent the deteriorated layer 23 from not being formed on the side surface 20c of the processed wafer 20.

[0049] (Other embodiments) Although the present disclosure has been described based on the embodiment, it is understood that the present disclosure is not limited to the embodiment or structure. The present disclosure also encompasses various modifications and modifications within the equivalent range. In addition, various combinations and forms, as well as other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure.

[0050] 1B, an epitaxial film may also be formed on the second main surface 1b side of the SiC wafer 1. This makes it easier to leave a predetermined thickness or more as the recycled wafer 60, thereby increasing the number of times the wafer can be reused. [Explanation of symbols]

[0051] 1. SiC wafer 1a First main surface 1b Second main surface 2 Epitaxial film 20 Processed wafers 20a one side 20b Other side 21 Beveling Department 50 chip wafer 60 Recycled Wafers

Claims

1. A method for manufacturing a chip configuration wafer on which semiconductor devices are formed, comprising the steps of: Preparing a silicon carbide wafer (1) having a first main surface (1a) and a second main surface (1b) opposite to the first main surface and made of silicon carbide; An epitaxial film (2) made of silicon carbide is formed on a first main surface of the silicon carbide wafer, and a processed wafer (20) is prepared in which a surface on the epitaxial film side is one surface (20a) and a surface on the silicon carbide wafer side is another surface (20b); forming an altered layer (23) along a surface direction of the processed wafer by irradiating a laser beam (L) from the other surface of the processed wafer into the inside of the processed wafer; Separating the processed wafer at the deteriorated layer as a boundary, thereby separating the processed wafer into a chip configuration wafer (50) on one side of the processed wafer and a recycled wafer (60) on the other side of the processed wafer; and reusing the recycled wafer as the silicon carbide wafer. A method for manufacturing a chip configuration wafer, comprising the steps of: preparing the processed wafer, the processed wafer having a beveled portion (21) formed on the outer edge of the processed wafer, the other surface of which is larger in area than the one surface;

2. 2. The method for manufacturing a chip configuration wafer as described in claim 1, wherein the processed wafer is prepared such that, when a surface that passes through the center between the one surface and the other surface and is aligned along the surface direction of the processed wafer is defined as a virtual surface (K), the curvature of the portion located between the end of the virtual surface and the other surface is greater than the curvature of the portion located between the end of the virtual surface and the one surface.

3. 3. The method for manufacturing a chip configuration wafer as described in claim 1 or 2, wherein by preparing the processed wafer, when the direction from the other surface along the one surface is taken as the depth direction, the depth (h) from the boundary between the other surface and the beveling portion to the side surface (20c) connecting the one surface and the other surface is shorter than the depth (H) of the portion from the other surface that forms the altered layer.

Citation Information

Patent Citations

  • Generation method of wafer

    JP2016111143A

  • SiC EPITAXIAL WAFER AND MANUFACTURING METHOD THEREOF

    JP2019046859A

  • Method for guiding a crack in the peripheral region of a donor substrate

    US20180185957A1

  • Method and device for producing silicon carbide semiconductor element

    WO2011161906A1

  • Method for manufacturing semiconductor device

    WO2014188879A1