Groove depth adjustment method and semiconductor device manufacturing method

By employing masks with varying thicknesses to adjust depth ratios, the method addresses the challenge of simultaneously etching grooves with different widths in SiC semiconductor devices, reducing costs and improving manufacturing efficiency.

JP7585720B2Active Publication Date: 2024-11-19FUJI ELECTRIC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020184613
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-11-19
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Existing methods for manufacturing silicon carbide (SiC) semiconductor devices face challenges in simultaneously etching grooves with different widths to control depth differences, leading to increased manufacturing costs due to the need for separate etching processes and multiple masks.

Method used

A method involving the use of masks with different thicknesses to simultaneously etch trenches and mesa grooves with controlled depth ratios by adjusting mask thickness to achieve desired depth ratios, allowing for simultaneous etching of grooves with varying widths.

Benefits of technology

This approach reduces the number of exposure masks and photolithography steps, thereby lowering the manufacturing cost and ensuring precise control over groove depths in SiC semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585720000001
    Figure 0007585720000001
  • Figure 0007585720000002
    Figure 0007585720000002
  • Figure 0007585720000003
    Figure 0007585720000003
Patent Text Reader

Abstract

To provide a groove depth adjustment method and a semiconductor device manufacturing method that can simultaneously etch grooves of different widths to control the difference in depth.SOLUTION: A groove depth adjustment method includes the steps of providing masks having different thicknesses on the upper surfaces of a plurality of substrates made of silicon carbide, forming a first opening having a predetermined width and a second opening having a width wider than the first opening in each of the masks, simultaneously etching a first groove and a second groove on each of the plurality of substrates through the first opening and the second opening, obtaining the depth ratio between the first groove and the second groove on each of the plurality of substrates, and obtaining the mask thickness at which the depth ratio is a desired value from a relationship between the mask thickness and the depth ratio.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for adjusting the depth of a trench and a method for manufacturing a semiconductor device, and more particularly to a method for adjusting the depth of a trench in a silicon carbide (SiC) semiconductor device and a method for manufacturing a SiC semiconductor device. [Background technology]

[0002] Conventionally, silicon (Si) semiconductors have been used in power semiconductor devices that are primarily used in power conversion devices and the like. In recent years, SiC, a wide-gap semiconductor, has been expected to replace Si as a semiconductor material. Compared to conventional semiconductor elements that use Si as a material, SiC semiconductors have the advantages of being able to reduce the resistance of elements in the on-state to one-hundredth of that of conventional semiconductor elements that use Si as a material, and being usable in higher temperature environments (e.g., 200°C or higher). This is due to the characteristics of the material itself, namely, that the band gap of SiC is about three times larger than that of Si, and that the dielectric breakdown field strength is nearly one order of magnitude larger than that of Si.

[0003] To date, commercial SiC semiconductor devices include Schottky barrier diodes (SBDs), planar vertical MOS field effect transistors (FETs), and trench MOSFETs. Trench MOSFETs are three-dimensional semiconductor devices in which a groove (trench) is formed in a SiC semiconductor substrate and the sidewall of the groove is used as a channel. Therefore, when comparing elements with the same on-resistance, trench MOSFETs can overwhelmingly reduce the element area compared to planar vertical MOSFETs, and are considered to be a particularly promising semiconductor element structure.

[0004] Typically, a semiconductor substrate for manufacturing a SiC semiconductor device has a plurality of chip regions in which the semiconductor device is formed. In the case of a trench-type MOSFET, the chip region has an active portion in which a plurality of narrow trenches of 1 μm or less are formed, and an outer peripheral portion in which a wide mesa groove of 5 μm or more and 200 μm or less is formed so as to surround the active portion. If the trenches and mesa grooves are simultaneously etched and formed by a general dry etching method, the depths of the trenches and mesa grooves will differ due to a loading effect.

[0005] In the case of Si, trench etching has a wide process window, so the loading effect can be suppressed by adjusting process conditions, such as performing dry etching at low pressure. However, in the case of SiC, trench etching is more difficult than in the case of Si, and the dry etching conditions are narrower. For example, to obtain an ideal trench shape for a trench-type MOSFET, it is necessary to finely adjust the etching gas flow rate ratio, which is not a process condition that suppresses the loading effect. Thus, in SiC, it is extremely difficult to find process conditions that achieve both suppression of the loading effect and adjustment of the trench shape.

[0006] For the above reasons, Patent Document 1 describes that in the case of a SiC trench MOSFET, the etching process for the trench and the mesa groove are performed separately in order to adjust the depth of the trench and the mesa groove. Since the trench and the mesa groove are etched separately, the etching depth of each can be freely adjusted. However, the etching mask formation process, such as the oxide film formation process, the patterning process, and the peeling process, required for etching, is required twice, which increases the manufacturing cost of the semiconductor device.

[0007] Patent Document 2 also describes that a trench is formed in an active portion and a mesa groove wider than the trench is formed in an outer peripheral portion surrounding the active portion by reactive ion etching (RIE) using a silicon dioxide film with a thickness of 1.0 to 2.0 μm as a mask. Patent Document 2 describes that the depth of the trench and mesa groove is about 0.5 to 3.0 μm, but does not describe whether the depth of the trench and mesa groove is the same or different. Furthermore, there is no description about the loading effect, and no mention is made of the process conditions for RIE. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2019-4078 A [Patent Document 2] Patent No. 6099749 Summary of the Invention [Problem to be solved by the invention]

[0009] In view of the above problems, the present invention has an object to provide a groove depth adjustment method and a semiconductor device manufacturing method that are capable of simultaneously etching grooves of different widths and controlling the difference in depth. [Means for solving the problem]

[0010] In order to achieve the above object, one aspect of the present invention is a method for adjusting groove depth, comprising the steps of: (a) providing masks of different thicknesses on upper surfaces of multiple substrates made of silicon carbide; (b) forming in each of the masks a first opening of a predetermined width and a second opening having a width wider than the first opening; (c) simultaneously etching to form a first groove and a second groove in each of the multiple substrates through the first opening and the second opening; (d) obtaining a depth ratio between the first groove and the second groove in each of the multiple substrates; and (e) obtaining a mask thickness that provides a desired depth ratio from a relationship between the mask thickness and the depth ratio.

[0011] Another aspect of the present invention includes the steps of: (a) obtaining a first width of a trench forming an insulating gate structure disposed in an active section, and a second width of a mesa groove disposed so as to surround the active section in an outer periphery and being wider than the first width; (b) obtaining a mask thickness by a method for adjusting a groove depth according to one aspect of the present invention, which allows etching of the trench of the first width and the mesa groove of the second width to the same depth; (c) forming a base region of a second conductivity type on an upper surface side of a drift region of a first conductivity type of a target substrate made of silicon carbide; and (d) forming a base region of a second conductivity type on an upper surface of the drift region. The gist of the invention is that the method for manufacturing a semiconductor device includes the steps of: (a) selectively forming a source region of a first conductivity type with a higher impurity concentration than the source region; (b) depositing a target mask to a mask thickness on the upper surfaces of the source region and the base region; (c) forming a first opening of a first width and a second opening of a second width in the target mask; (d) etching the target substrate through the first opening and the second opening to simultaneously form a trench and a mesa groove in the target substrate; and (e) forming an insulated gate electrode structure on the inside of the trench. Effect of the Invention

[0012] According to the present invention, it is possible to provide a groove depth adjustment method and a semiconductor device manufacturing method that are capable of simultaneously etching grooves with different widths and controlling the difference in depth. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic plan view showing an example of a SiC semiconductor device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 2 is a schematic cross-sectional view for explaining an example of trench etching according to an embodiment of the present invention. [Figure 4] 10A and 10B are schematic cross-sectional views for explaining another example of trench etching according to an embodiment of the present invention. [Diagram 5] FIG. 13 is a diagram showing the relationship between the film thickness of a mask and the depth ratio of a trench and a mesa groove. [Figure 6] 4 is a flowchart showing an example of a groove depth adjustment method according to an embodiment of the present invention. [Figure 7] 1A to 1C are schematic cross-sectional views for explaining an example of a process of a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Figure 8] 8 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 7 in the method for manufacturing a semiconductor device according to the embodiment of the present invention. [Figure 9] 9 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 8 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. [Figure 10] 10 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 9 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. [Figure 11] 11 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 10 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 12] 12 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 11 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 13] 13 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 12 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 14] 14 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 13 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 15] 15 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 14 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 16] 16 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 15 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 17] 17 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 16 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. [Figure 18] 18 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 17 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. [Figure 19] 19 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 18 in the method for manufacturing the semiconductor device according to the embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted by the same or similar reference numerals, and duplicated explanations will be omitted. However, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thickness of each layer, etc. may differ from the actual ones. In addition, parts with different dimensional relationships and ratios may be included between the drawings. In addition, the embodiments shown below are examples of devices and methods for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the materials, shapes, structures, arrangements, etc. of the components as described below.

[0015] In this specification, the source region of a MOS transistor is "one main region (first main region)" that can be selected as the emitter region of an insulated gate bipolar transistor (IGBT). In addition, in a thyristor such as a MOS controlled static induction thyristor (SI thyristor), one main region can be selected as the cathode region. The drain region of a MOS transistor is "the other main region (second main region)" of a semiconductor device that can be selected as the collector region in an IGBT or as the anode region in a thyristor. In this specification, when the term "main region" is used simply, it means either the first main region or the second main region that is appropriate from the technical common sense of a person skilled in the art.

[0016] In addition, the definitions of directions such as up and down in the following description are merely for convenience of explanation and do not limit the technical idea of the present invention. For example, if the object is rotated by 90° and observed, up and down are read as left and right, and if it is rotated by 180° and observed, up and down are read in reverse. In the following description, the case where the first conductivity type is p-type and the second conductivity type, which is the opposite, is n-type will be exemplified. However, the conductivity types may be selected in the reverse relationship, with the first conductivity type being n-type and the second conductivity type being p-type. Also, + and - attached to n or p mean semiconductor regions with relatively higher or lower impurity concentrations, respectively, compared to semiconductor regions without + and - attached. However, even for semiconductor regions with the same n attached, it does not mean that the impurity concentrations of the respective semiconductor regions are exactly the same. In addition, in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and a negative index is represented by attaching "-" before the index.

[0017] <Structure of SiC Semiconductor Device> The SiC semiconductor substrate (substrate) 100 for manufacturing the SiC semiconductor device according to an embodiment of the present invention consists of a plurality of chip regions 101 and dicing lines 102, as shown in FIG. 1. For example, the chip region 101 has a rectangular planar shape and is arranged on the substrate 100 in a matrix. The dicing lines 102 are arranged in a grid so as to surround each of the chip regions 101. As shown in FIG. 2, the chip region 101 is provided with an active part 101a containing active elements and an outer peripheral part 101b having a breakdown voltage structure. In FIG. 2, a MOSFET with a trench gate structure provided on the upper part of a drift layer 2 of the first conductivity type (n - -type) is exemplified as a case including an electric field relaxation region 20 as a breakdown voltage structure.

[0018] As shown in Fig. 2, a base region 6 of a second conductivity type (p type) is disposed on the upper surface of the drift layer 2. The drift layer 2 and the base region 6 are each composed of an epitaxially grown layer (hereinafter abbreviated as "epitaxial layer") made of SiC. + An n-type base contact region 8 is selectively provided on the upper portion of the base region 6. The n-type base contact region 8 is in contact with the base contact region 8 and has a higher impurity concentration than the drift layer 2. + A first main region (source region) 7 of a type is optionally provided.

[0019] A trench (first trench) 9a having a width of 1 μm or less is provided from the upper surfaces of the source region 7 and base region 6 through the base region 6. In other words, the source region 7 and base region 6 are in contact with the side surfaces of the trench 9a. A gate insulating film 11 is provided on the bottom and side surfaces of the trench 9a. A gate electrode 12a is buried in the trench 9a via the gate insulating film 11, forming an insulated gate electrode structure (11, 12a). As the gate insulating film 11, in addition to a silicon dioxide film (SiO2 film), a silicon oxynitride (SiON) film, a strontium oxide (SrO) film, a silicon nitride (Si3N4) film, an aluminum oxide (Al2O3) film, a magnesium oxide (MgO) film, an yttrium oxide (Y2O3) film, a hafnium oxide (HfO2) film, a zirconium oxide (ZrO2) film, a tantalum oxide (Ta2O5) film, or a bismuth oxide (Bi2O3) film, or a composite film obtained by stacking a plurality of these films, can be used. As the material for the gate electrode 12a, for example, a polysilicon layer (doped polysilicon layer) to which impurities such as phosphorus (P) or boron (B) are added at a high impurity concentration can be used.

[0020] The upper part of the drift layer 2 is made of n-type semiconductor material having a higher impurity concentration than the drift layer 2. +A p-type current spreading layer (CSL) 3 is selectively provided. The bottom of the trench 9a reaches the current spreading layer 3. The current spreading layer 3 is not necessarily provided. If the current spreading layer 3 is not provided, the bottom of the trench 9a reaches the drift layer 2. Inside the current spreading layer 3, a p + A gate bottom protection region 4b of a shaped type is provided. Inside the current spreading layer 3, a first base bottom buried region 4a is provided below the base contact region 8 at the same depth as the gate bottom protection region 4b and spaced apart from the gate bottom protection region 4b. A second base bottom buried region 5a is provided above the current spreading layer 3 so as to contact an upper surface of the first base bottom buried region 4a and a lower surface of the base region 6. The second base bottom buried region 5a is also provided below the base contact region 8.

[0021] An interlayer insulating film 13 is disposed on the upper surface of the gate electrode 12a. A silicon oxide film (BPSG) doped with boron (B) and phosphorus (P) is used as the interlayer insulating film 13. However, the interlayer insulating film 13 may be a silicon oxide film (PSG) doped with phosphorus (P), a non-doped SiO2 film called "NSG" that does not contain phosphorus (P) or boron (B), a silicon oxide film (BSG) doped with boron (B), a Si3N4 film, or the like. A laminate film of these may also be used.

[0022] A source contact layer 14 is provided so as to be in physical contact with the source region 7 and the base contact region 8 exposed between the interlayer insulating film 13. A barrier metal layer 15a is provided so as to cover the interlayer insulating film 13 and the source contact layer 14. A first main electrode (source electrode) 16a is electrically connected to the source region 7 and the base contact region 8 via the barrier metal layer 15a and the source contact layer 14. For example, if the source contact layer 14 is made of nickel silicide (NiSi x The barrier metal layer 15a can be made of a titanium nitride (TiN) film or a titanium (Ti) film, and the source electrode 16a can be made of an aluminum (Al) film or an aluminum-silicon (Al-Si) film. The source electrode 16a is disposed separately from the gate surface electrode (not shown).

[0023] On the peripheral portion 101b side of the active portion 101a, a base contact region 8b is provided on the upper portion of the base region 6. A wiring layer 12b is disposed on the upper surface of the base contact region 8b via a field oxide film 10, and a gate electrode pad 16b is disposed on the upper surface of the wiring layer 12b via a barrier metal layer 15b. Although not shown, the gate electrode pad 16b is electrically connected to the gate electrode 12a via the wiring layer 12b. The interlayer insulating film 13 and the field oxide film 10 extend to the peripheral portion 101b side. In addition, on the peripheral portion 101b side of the active portion 101a, a second base bottom buried region 5b and a first base bottom buried region 4c are provided so as to contact the lower surface of the base region 6.

[0024] The bottom surface of the drift layer 2 is + A second main region (drain region) 1 of a type having a SiO2 content is disposed on the bottom surface of the drain region 1. The drain region 1 is made of a SiC semiconductor substrate (substrate). A second main electrode (drain electrode) 17 is disposed on the bottom surface of the drain region 1. As the drain electrode 17, for example, a single layer film made of gold (Au) or a metal film laminated in the order of Ti, nickel (Ni) and Au can be used, and further a metal film of molybdenum (Mo), tungsten (W) or the like may be laminated on the bottom layer. In addition, a drain contact layer may be provided between the drain region 1 and the drain electrode 17. The drain contact layer is, for example, nickel silicide (NiSi x ) membrane.

[0025] During operation of the semiconductor device according to the embodiment, when the source electrode 16a is set to earth potential, a positive voltage is applied to the drain electrode 17, and a positive voltage equal to or greater than a threshold is applied to the gate electrode 12a, an inversion layer (channel) is formed on the side of the trench 9a in the base region 6, resulting in an ON state. The inversion layer is formed on the surface of the base region 6 exposed on the side of the trench 9a, which is the interface between the base region 6 and the gate insulating film 11 sandwiched at a position where the base region 6 faces the gate electrode 12a. In the ON state, a current flows from the drain electrode 17 to the source electrode 16a via the drain region 1, the drift layer 2, the current diffusion layer 3, the inversion layer of the base region 6, and the source region 7. On the other hand, when the voltage applied to the gate electrode 12a is less than the threshold, an inversion layer is not formed in the base region 6, resulting in an OFF state, and no current flows from the drain electrode 17 to the source electrode 16a.

[0026] As shown in FIG. 2, the first base bottom buried region 4c extends from the left active portion 101a to the outer peripheral portion 101b. Furthermore, the second base bottom buried region 5b extends from the left active portion 101a to the outer peripheral portion 101b. The outer peripheral portion 101b is provided with a mesa groove (second groove) 9b that penetrates the base region 6 from the upper surface to the second base bottom buried region 5b. The width of the mesa groove 9b in one chip region 101 is, for example, in the range of 5 μm or more and 200 μm or less. The outer peripheral portion 101b is provided with a p-type electric field relaxation region 20 so as to be exposed to the bottom and side surfaces of the second groove 9b. In the electric field relaxation region 20, a spatial modulation portion 21b is provided at the outer end so that the average impurity concentration decreases toward the outside. An interlayer insulating film 13 is provided on the bottom and side surfaces of the mesa groove 9b via a field oxide film 10.

[0027] 2, a junction termination structure called a "junction termination extension (JTE)" is provided as the electric field relaxation region 20, extending from the base contact region 8 across the upper portion of the base region 6 to near the outer end of the upper portion of the drift layer 2. The electric field relaxation region 20 extends beyond the second base bottom buried region 5b.

[0028] The JTE structure of the electric field relaxation region 20 has a main body 21a extending from the base contact region 8 across the upper part of the base region 6 to the outside of the first base bottom buried region 4c, and a plurality of spatial modulation portions 21b provided outside the main body 21a. The plurality of spatial modulation portions 21b are provided in a concentric ring shape spaced apart from each other. For example, the plurality of spatial modulation portions 21b form a spatial modulation pattern in which the width becomes narrower and the intervals become wider toward the outside.

[0029] By providing the spatial modulation portion 21b of the JTE structure in the electric field relaxation region 20, the amount of p-type impurity added effectively decreases toward the outside, so that electric field concentration can be relaxed.

[0030] At the outer end of the outer periphery 101b, n + The channel stoppers 3c are arranged in a concentric ring shape. + Instead of the channel stopper 3c, + A molded channel stopper may be provided.

[0031] <How to adjust the groove depth> As shown in FIG. 2, the semiconductor device according to the embodiment includes trenches 9a and mesa grooves 9b with different widths. For example, the trenches 9a are narrow, 1 μm or less, whereas the mesa grooves 9b are wide, 5 μm or more and 200 μm or less. The outer periphery 101b faces the outer periphery 101b of another chip region 101 via a dicing line 102. Therefore, if the depth of the dicing line 102 is the same as that of the mesa groove 9b, the substantial groove width is the sum of the width of the two adjacent mesa grooves 9b and the width of the dicing line 102. Considering such a case, the groove width is in the range of 5 μm or more and 400 μm or less. If the trenches 9a and mesa grooves 9b are etched simultaneously by a general dry etching method, the etching depths of the trenches 9a and mesa grooves 9b will differ due to the loading effect. If the groove width is 5 μm or more, the loading effect due to dry etching will be small and the etching depth will be almost constant, independent of the groove width.

[0032] For example, if the trench 9a is too shallow to penetrate the base region 6 that becomes the channel of the MOSFET, the on-voltage Von will increase. On the other hand, if the trench 9a is too deep to penetrate the gate bottom protection region 4b, the breakdown voltage will decrease. Also, if the mesa groove 9b is too shallow to remove the base region 6, the base region 6 will remain at the bottom of the mesa groove 9b, resulting in leakage defects. On the other hand, if the mesa groove 9b is too deep to be deeper than the first base bottom buried region 4c, electric field concentration will occur at the corners of the mesa groove 9b, resulting in a decrease in breakdown voltage. In this way, both the trench 9a and the mesa groove 9b must be deeper than the bottom of the base region 6 and shallower than the bottom of the first base bottom buried region 4c. Therefore, it is desirable that the trench 9a and the mesa groove 9b have the same depth. The trench 9a and the mesa groove 9b having the same depth means, for example, that the ratio of the depth of the mesa groove 9b to the depth of the trench 9a is 1±0.05, and more preferably 1±0.02.

[0033] In FIG. 3, a SiO2 film is formed on the upper surface of a SiC substrate 30 by chemical vapor deposition (CVD) to a thickness t of about 0.7 μm. m An example of deposition is shown. An opening 34a having a width W1 of 1 μm or less, for example, about 0.7 μm, and an opening 34b having a width W2 of 5 μm or more, for example, about 100 μm are opened in the SiO2 film by photolithography or the like to form a mask 31a. A high-density plasma etching technique such as inductively coupled plasma (ICP)-RIE can be adopted as the SiC dry etching. The etching conditions are, for example, SF6 / SiF4 / O2 / Ar gas system, coil applied power: about 1000 W to 2000 W, bias power: about 100 W to 400 W, and chamber pressure: about 0.2 Pa to 2.0 Pa. Since the amount of Si, which is the raw material of the etching product, is greater on the wide opening 34b than on the opening 34a, etching is more likely to be hindered on the opening 34b than on the opening 34a. Therefore, as shown in FIG. 3, the groove depth d2 of the second groove 33a etched from the opening 34b of width W2 tends to be shallower than the groove depth d1 of the first groove 32a etched from the opening 34a of width W1.

[0034] In Fig. 4, the SiO2 film is approximately 1.5 μm thick. m 3, the etching product Si should be generated in large amounts on the opening 35b of width W2, but the portion of the opening 35a of narrow width W1 makes it difficult for radicals and ions contributing to etching to reach the surface of the substrate 30 exposed in the opening 35a. Therefore, as shown in FIG. 4, the groove depth d2 of the second groove 33b etched from the opening 35b of width W2 tends to be deeper than the groove depth d1 of the first groove 32b etched from the opening 35a of width W1.

[0035] FIG. 5 shows the relationship between the mask thickness and the depth ratio of the second groove to the first groove when the width of the first groove is about 0.7 μm. FIG. 5 also shows the relationship between the mask thickness and the depth ratio of the second groove to the first groove when the width of the first groove is about 0.4 μm. As shown in FIG. 5, whether the width of the first groove is 0.7 μm or 0.4 μm, the depth ratio of the first groove / second groove tends to decrease as the mask thickness increases. Therefore, in order to adjust the depth ratio of the first groove / second groove to about 1, when the first groove is 0.7 μm, the mask thickness should be about 0.9 μm, and when the first groove is 0.4 μm, the mask thickness should be about 0.8 μm. Note that the relationship shown in FIG. 5 is an example, and the SiO2 film thickness of the mask at which the depth ratio of the first groove / second groove is 1 will differ depending on the conditions such as the etching device used, the process conditions, and the mask aperture ratio. Even in this case, if two or more different SiO2 film thicknesses are prepared and the relationship between film thickness and depth ratio is obtained through experiments, it is possible to calculate the film thickness that makes the depth ratio of the first groove / second groove 1. Specifically, it is preferable to use multiple SiC semiconductor substrates provided with different SiO2 film thicknesses.

[0036] The groove depth adjustment method according to the embodiment of the present invention will be described with reference to the flow chart of Fig. 6, where the method is applied to a semiconductor device manufacturing method. Note that the groove depth adjustment method described below is only one example, and it goes without saying that various other manufacturing methods, including modifications thereof, can be implemented within the scope of the spirit described in the claims.

[0037] 6, the width of the trench as the first groove and the width of the mesa groove as the second groove are obtained from the specifications of the semiconductor device to be manufactured. When the dicing line 102 is to have the same depth as the mesa groove 9b, the width of the second groove is the sum of the widths of the two mesa grooves in the adjacent chip regions and the width of the dicing line 102. For example, the width of the first groove is 1.0 μm or less, and the width of the second groove is 5 μm or more and 400 μm or less.

[0038] In step S101, SiO2 films with different thicknesses are deposited on a plurality of SiC semiconductor substrates by CVD technology, etc. Then, a mask is formed by openings corresponding to the first groove width and the second groove width by photolithography technology, etc.

[0039] In step S102, a first groove and a second groove are simultaneously dug into each of a plurality of substrates through an opening using a mask by dry etching technology. In step S103, the depth ratio of the formed first groove to the formed second groove is evaluated. Then, a mask thickness is obtained that makes the depth ratio of the first groove / second groove about 1, for example, 1±0.05, more preferably 1±0.02. Thereafter, in step S105, a trench and a mesa groove are simultaneously formed using the obtained mask thickness by dry etching or the like during the manufacture of the semiconductor device. At this time, the mask material and the openings corresponding to the first groove width and the second groove width are the same as in step S102.

[0040] According to the groove depth adjustment method of the embodiment, the trench and mesa groove can be simultaneously etched in the manufacturing of a semiconductor device to form the same groove depth. Therefore, the number of exposure masks used in the photolithography process can be reduced by one. In addition, the number of steps in the photolithography and dry etching of the trench and mesa groove can be reduced, which makes it possible to reduce the cost of the semiconductor device.

[0041] <Method of Manufacturing Insulated Gate Semiconductor Device> Next, the manufacturing method of the SiC semiconductor device according to the embodiment will be described with reference to the process cross-sectional views of Figures 7 to 19, taking the case of a trench-gate MOSFET as an example. A SiO2 film is used as an etching mask for the trench (first groove) and the mesa groove (second groove), and inductively coupled plasma (ICP)-RIE can be adopted as dry etching. Note that the manufacturing method of the trench-gate MOSFET described below is an example, and it goes without saying that various other manufacturing methods, including modifications thereof, can be realized within the scope of the spirit described in the claims.

[0042] First, n-type impurities such as nitrogen (N) are added. + A type SiC semiconductor substrate (substrate) 1p is prepared. As shown in FIG. 7, an n - A type drift layer 2p is epitaxially grown. Next, a photoresist film is applied to the upper surface of the drift layer 2p, and the photoresist film is patterned using a photolithography technique or the like. Using the patterned photoresist film as an ion implantation mask, n-type impurity ions such as nitrogen (N) are selectively implanted in multiple stages into the end of the active portion 101a and the outer peripheral portion 101b of the drift layer 2 from the upper surface side of the drift layer 2p. In this manner, an n-type ion implantation layer 3p is formed in the active portion 101a of the drift layer 2p, and an n-type ion implantation layer 3q is formed in the end of the outer peripheral portion 101b.

[0043] An oxide film made of SiO2 is deposited on the upper surface of the n ion implantation layers 3p, 3q and the drift layer 2p by CVD technology or the like. A photoresist film is applied to the upper surface of the oxide film, and the oxide film is patterned by photolithography technology, dry etching technology or the like. Using the patterned oxide film 40 as a mask for ion implantation, p-type impurity ions such as aluminum (Al) are implanted in multiple stages into the n ion implantation layer 3p and the drift layer 2p. As a result, as shown in FIG. 8, a first base bottom buried region 4a is selectively formed on the upper part of the n ion implantation layer 3p, a first base bottom buried region 4c is selectively formed on the upper part of the gate bottom protection region 4b and the drift layer 2p, and a spatial modulation section 21b is selectively formed.

[0044] After removing the oxide film 40, the first base bottom buried regions 4a and 4c, the gate bottom protection region 4b, the spatial modulation portion 21b, the drift layer 2p, and the upper surface of the n ion implantation layer 3q are - A type epitaxial layer 55 is grown. A photoresist film is applied to the surface of the epitaxial layer 55, and the photoresist film is patterned using a photolithography technique or the like. Using the patterned photoresist film as a mask for ion implantation, n-type impurity ions such as nitrogen (N) are selectively implanted in multiple stages into the upper part of the epitaxial layer 55 from the upper surface side of the epitaxial layer 55. As a result, as shown in FIG. 9, n-ion implanted layers 5p, 5q are formed on the n-ion implanted layers 3p, 3q, the first base bottom buried region 4a, and the gate bottom protection region 4b.

[0045] Next, an oxide film made of SiO2 is deposited on the upper surfaces of the n ion-implanted layers 5p, 5q and the epitaxial layer 55 by CVD or the like. A photoresist film is applied to the upper surface of the oxide film, and the oxide film is patterned by photolithography, dry etching, or the like. Using the patterned oxide film 60 as a mask for ion implantation, p-type impurity ions such as aluminum (Al) are selectively implanted in multiple stages into the n ion-implanted layer 5p and the epitaxial layer 55. As a result, second base bottom-embedded regions 5a, 5b are selectively formed on the first base bottom-embedded regions 4a, 4c, respectively, as shown in FIG.

[0046] After removing the oxide film 60, a p-type base region 6p is epitaxially grown on the upper surface of the second base bottom buried region 5a, 5b, the n ion implantation layers 5p, 5q, and the epitaxial layer 55. An oxide film made of SiO2 is deposited on the surface of the base region 6p by CVD technology or the like. A photoresist film is applied to the upper surface of this oxide film, and the oxide film is patterned by photolithography technology, dry etching technology, or the like. Using the patterned oxide film as a mask for ion implantation, n-type impurity ions such as phosphorus (P) are selectively implanted into the base region 6p in multiple stages from the upper surface side of the base region 6p. As a result, as shown in FIG. 11, a source region 7p is formed on the upper surface of the base region 6p above the second base bottom buried region 5a and the n ion implantation layer 5p.

[0047] After removing the oxide film used as the ion implantation mask, an oxide film made of SiO2 is deposited on the upper surface of the source region 7p and the base region 6p by CVD technology or the like. A photoresist film is applied to the upper surface of this oxide film, and the oxide film is patterned by photolithography technology, dry etching technology or the like. Using the patterned oxide film 80 as a mask for ion implantation, p-type impurity ions such as aluminum (Al) are selectively implanted into the source region 7p and the base region 6p from the upper surface side of the source region 7p and the base region 6p in multiple stages. As a result, as shown in FIG. 12, a base contact region 8p is formed on the upper surface of the source region 7p above the second base bottom buried regions 5a, 5b and on the upper surface of the base region 6p.

[0048] After removing the oxide film 80 used as a mask for ion implantation, an oxide film made of SiO2 is deposited on the upper surfaces of the base contact region 8p, the source region 7p, and the base region 6p by CVD technology or the like. The thickness of this oxide film is obtained in advance according to the groove depth adjustment method described using the flowchart of FIG. 6. Also, the thickness of the oxide film actually formed can be considered to be the same thickness if it is within ±5% of the value obtained according to the groove depth adjustment method. A photoresist film is applied to the upper surface of the oxide film, and the oxide film is patterned using photolithography technology, dry etching technology, or the like. Using the patterned oxide film 90 as an etching mask, trenches 9a and mesa grooves 9b are selectively formed at the same depth at the same time by dry etching technology such as ICP-RIE. For example, in the case of ICP-RIE using a SF6 / SiF4 / O2 / Ar gas system, the following etching conditions can be adopted. The etching conditions are coil applied power: about 1000 W to 2000 W, bias power: about 100 W to 400 W, and pressure in the chamber: about 0.2 Pa to 2.0 Pa. As shown in Fig. 13, the trench 9a penetrates the source region 7p, the base region 6p, and the n ion implantation layer 5p to reach the gate bottom protection region 4b. The mesa groove 9b penetrates the base contact region 8p, the base region 6p, the second base bottom buried region 5b, the epitaxial layer 55, and the n ion implantation layer 5q to reach the first base bottom buried region 4c, the spatial modulation section 21b, the drift layer 2p, and the n ion implantation layer 3q.

[0049] After removing the oxide film 90, a carbon (C) film is formed on the upper surfaces of the trench 9a and mesa groove 9b by carbon sputtering or the like. Then, a heat treatment is performed to simultaneously activate the implanted n-type impurity ions and p-type impurity ions. As a result, as shown in FIG. 14, an n-type ion implanted layer 3p and an n-type ion implanted layer 5p are formed. + A p-type current spreading layer 3 is formed on the upper surface of the drift layer 2. + The first base bottom buried region 4a of the p type is sandwiched between the first base bottom buried region 4a and the base region 6. + The bottom of the second base bottom buried region 5a and the bottom of the trench 9a are filled with p +A p-type gate bottom protection region 4b is formed on the drift layer 2. + The first base bottom buried region 4c of the p type and the p type buried region between the first base bottom buried region 4c and the base region 6 + A second base bottom buried region 5b of a type is formed on the upper surface of the base region 6 so as to contact the trench 9a. + A p-type source region 7 and a p-type ... + A p-type base contact region 8 is formed on the bottom surface of the mesa groove 9b. Furthermore, an electric field relaxation region 20 is formed on the bottom surface of the mesa groove 9b. The electric field relaxation region 20 is a p-type + The main body 21a of the mold and the plurality of p + The mesa groove 9b has a JTE structure having a spatial modulation portion 21b of a type. At the outer end of the bottom of the mesa groove 9b, an n-type + A channel stopper 3c of the n type is formed. + The mold channel stopper 3c is made of the n ion-implanted layer 3q remaining after dry etching.

[0050] A field oxide film is deposited on the exposed surface after removing the carbon film by CVD or the like. A photoresist film is applied to the upper surface of the field oxide film, and the photoresist film is patterned by photolithography or the like. The patterned photoresist film is used as an etching mask to selectively remove the field oxide film. As a result, as shown in FIG. 15, a field oxide film 10 is formed, which extends from the bottom and side surfaces of the mesa groove 9b to the upper surface of the base contact region 8b.

[0051] A gate insulating film 11p such as a SiO2 film is formed on the bottom and side surfaces of the trench 9a and on the top surfaces of the source region 7 and the base contact region 8 by thermal oxidation or chemical vapor deposition (CVD) technology, as shown in Fig. 16. Next, a polysilicon layer (doped polysilicon layer) 12p doped with a high concentration of impurities such as phosphorus (P) or boron (B) is deposited by CVD technology, as shown in Fig. 16, so as to fill the trench 9a. The polysilicon layer 12p extends to cover the side and bottom surfaces of the mesa groove 9b.

[0052] Then, a part of the polysilicon layer 12p and a part of the gate insulating film 11p are selectively removed by photolithography and dry etching. As shown in FIG. 17, a pattern of the gate electrode 12a made of the gate insulating film 11 and the polysilicon layer is formed to form an insulated gate electrode structure (11, 12a). In addition, a wiring layer 12b electrically connected to the gate electrode 12a is formed on the upper surface of the field oxide film 10 in the vicinity of the mesa groove 9b. Next, an insulating film is deposited on the upper surface of the insulated gate electrode structure (11, 12a) made of the gate electrode 12a and the gate insulating film 11 by CVD or the like. As the insulating film, boron phosphorus glass (BPSG), NSG, or the like is used. Then, a part of the deposited insulating film is selectively removed by photolithography and dry etching. As a result, as shown in FIG. 17, a source electrode contact hole and a gate electrode pad contact hole are opened in the interlayer insulating film 13p. Although not shown, the gate contact hole is also opened in the interlayer insulating film 13p so that a part of the gate surface electrode connected to the gate electrode 12a is exposed at a location different from the source electrode contact hole.

[0053] The substrate on which the interlayer insulating film 13p is formed is subjected to a reflow process such as a heat treatment. The reflow process smooths the steep steps at the ends of the interlayer insulating film 13p. As a result, as shown in FIG. 18, the interlayer insulating film 13 is formed with smoothed openings of the source electrode contact hole and the gate electrode pad contact hole.

[0054] A metal layer such as a Ni film is deposited by sputtering or vapor deposition, and the metal layer is patterned by photolithography and RIE. Then, a source contact layer 14 is formed by rapid thermal annealing (RTA), for example, at about 1000° C. Next, a metal layer such as a TiN film is deposited by sputtering, and the metal layer is patterned by photolithography and RIE to form barrier metal layers 15a and 15b. As a result, as shown in FIG. 19, the source contact layer 14 is formed on the upper surfaces of the source region 7 and the base contact region 8, and the barrier metal layer 15a is formed so as to cover the interlayer insulating film 13. Also, the barrier metal layer 15b is formed on the upper surface of the wiring layer 12b so as to cover the interlayer insulating film 13. Next, a metal layer such as an Al film is deposited by sputtering. A metal layer such as an Al film is patterned using photolithography and RIE techniques to form patterns of the source electrode 16a, the gate electrode pad 16b, and the gate surface electrode (not shown). As a result, the patterns of the source electrode 16a and the gate surface electrode are separated, and the gate electrode pad 16b is electrically connected to the gate electrode 12a via the wiring layer 12b.

[0055] Furthermore, the bottom surface of the substrate 1p is polished by chemical mechanical polishing (CMP) or the like to adjust the thickness, thereby forming the drain region 1. Thereafter, a drain electrode 17 made of Au or the like is formed on the entire bottom surface of the drain region 1 by a sputtering method, a deposition method, or the like. In this manner, the trench gate type semiconductor device shown in FIG. 2 is completed.

[0056] According to the method for manufacturing a semiconductor device according to the embodiment, the trench and the mesa groove can be simultaneously etched to form the same groove depth. Therefore, the number of exposure masks used in the photolithography process can be reduced by one. In addition, the number of steps in the photolithography and dry etching of the trench and the mesa groove can be reduced, which makes it possible to reduce the cost of the semiconductor device.

[0057] (Other embodiments) As described above, the insulated gate semiconductor device according to the embodiment of the present invention has been described, but the description and drawings forming a part of this disclosure should not be understood as limiting the present invention. Various alternative embodiments, examples, and operating techniques will be apparent to those skilled in the art from this disclosure.

[0058] As described above, in the semiconductor device according to the embodiment, the JTE structure having the main body portion 21a and the spatial modulation portion 21b is used as the electric field relaxation region 20. However, the electric field relaxation region 20 may be a guard ring using the first base bottom buried region 4c. In the above description, the trench (first groove) 9a is a narrow groove of 1 μm or less, whereas the mesa groove (second groove) 9b is a wide groove of 5 μm or more and 400 μm or less. However, the width of the second groove 9b is not limited and may be 5 μm or less. For example, the second groove 9b may be a trench used for the gate of a trench-type MOSFET like the trench 9a, although the groove width is different from that of the trench 9a.

[0059] Thus, the present invention naturally includes various embodiments not described here, such as configurations in which the configurations described in the above embodiments and modifications are applied in any way. Therefore, the technical scope of the present invention is defined only by the invention-specifying matters according to the claims that are appropriate from the above description. [Explanation of symbols]

[0060] 1...Drain region (second main region) 1p,100...SiC semiconductor substrate (substrate) 2, 2p…Drift layer 3...Current diffusion layer 3c…Channel stopper 3p, 3q...n ion-implanted layers 4a, 4c...first base bottom buried region 4b…Gate bottom protection area 5a, 5b...Second base bottom buried region 5p, 5q…n ion-implanted layers 6, 6p...base region 7, 7p...Source region (first main region) 8, 8b, 8p…Base contact region 9a…Trench (first trench) 9b…Mesa groove (second groove) 10...Field oxide film 11, 11p...Gate insulating film (11, 12a)…Insulated gate electrode structure 12a...gate electrode 12b...Wiring layer 12p...Polysilicon layer (doped polysilicon layer) 13, 13p...Interlayer insulating film 14…Source contact layer 15a, 15b...Barrier metal layer 16a...Source electrode (first main electrode) 16b...gate electrode pad 17...Drain electrode (second main electrode) 20...Electric field relaxation region 21a…Main body 21b…Spatial modulation section 30...Substrate 31a, 31b...Mask 34a, 34b, 35a, 35b...opening 40,60,80,90...Oxide film 55...Epitaxial layer 101…Chip area 101a...Active part 101b...outer periphery 102…Dicing line

Claims

1. providing masks having different thicknesses on upper surfaces of a plurality of silicon carbide substrates; forming a first opening having a predetermined width and a second opening having a width greater than the first opening in each of the masks; simultaneously etching a first groove and a second groove in each of the plurality of substrates through the first opening and the second opening; acquiring a depth ratio between the first groove and the second groove for each of the plurality of substrates; obtaining a thickness of the mask that provides a desired depth ratio from a relationship between the thickness of the mask and the depth ratio; A method for adjusting groove depth comprising the steps of:

2. 2. The method for adjusting a groove depth according to claim 1, wherein the width of the first opening is 1 μm or less, and the width of the second opening is 5 μm or more and 400 μm or less.

3. 3. The method of claim 1, wherein the desired value of the depth ratio is 1±0.

05.

4. 4. The method for adjusting a groove depth according to claim 1, wherein the mask is made of silicon dioxide.

5. 5. The method for adjusting a groove depth according to claim 1, wherein the first groove and the second groove are formed by etching with plasma using a gas system including a fluorine-based gas.

6. obtaining a first width of a trench forming an insulated gate structure disposed in an active portion, and a second width of a mesa groove wider than the first width, disposed so as to surround the active portion in an outer periphery; obtaining a mask thickness that allows the trench having the first width and the mesa groove having the second width to be etched to the same depth by the groove depth adjustment method of claim 1; forming a base region of a second conductivity type on an upper surface side of a drift region of a first conductivity type of a target substrate made of silicon carbide; Selectively forming a source region of a first conductivity type having a higher impurity concentration than the drift region above the base region; forming a target mask on an upper surface of the source region and the base region to the mask thickness; forming a first opening having the first width and a second opening having the second width in the target mask; simultaneously forming the trench and the mesa groove in the target substrate by etching the target substrate through the first opening and the second opening; forming an insulated gate electrode structure inside the trench; 2. A method for manufacturing a semiconductor device comprising the steps of:

7. 7. The method for manufacturing a semiconductor device according to claim 6, wherein the first width is 1 [mu]m or less, and the second width is 5 [mu]m or more and 400 [mu]m or less.

8. 8. The method for manufacturing a semiconductor device according to claim 6, wherein the depth ratio is 1±0.

05.

9. 9. The method for manufacturing a semiconductor device according to claim 6, wherein the target mask is made of silicon dioxide.

10. 10. The method for manufacturing a semiconductor device according to claim 6, wherein the trench and the mesa groove are formed by etching with plasma using a gas system including a fluorine-based gas.

11. 11. The method for manufacturing a semiconductor device according to claim 6, further comprising the step of forming a channel stopper region prior to the step of simultaneously forming the trench and the mesa groove.

12. 12. The method for manufacturing a semiconductor device according to claim 6, further comprising forming an electric field relaxation region prior to a step of simultaneously forming the trench and the mesa groove.

Citation Information

Patent Citations

  • Load sensing proportioning valve

    JP1985099749A

  • Dry-etching method

    JP1992237124A

  • Manufacture of semiconductor substrate

    JP2000150632A

  • Semiconductor device

    JP2006186108A

  • Dry etching method

    JP2010245101A