Sheath-core composite fibers and multifilaments

The core-sheath composite fiber with controlled interfiber voids and polymer elution addresses the challenge of replicating natural silk's luxurious luster and texture, achieving a balanced light, flexible, and resilient fabric.

JP7585792B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020571859
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-28
Filing Date
2020-10-02
Publication Date
2024-11-19
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

Existing synthetic fibers struggle to replicate the luxurious luster, light, flexible, and resilient texture of natural silk, as previous methods either fail to create balanced interfiber voids or result in uneven distribution leading to impaired soft feel and flexibility.

Method used

A core-sheath composite fiber with a sheath component completely covering a multi-lobed core component, featuring a thickness ratio Smax/Smin of 5.0 or more and interfiber voids ranging from 5 to 30 μm, including fine voids of less than 5 μm and coarse voids of 10 μm or more, achieved by controlling the elution of polymers with different solubility and melting points.

Benefits of technology

The composite fiber achieves a well-balanced texture similar to natural silk, with luxurious luster, dry feel, and resilience, while maintaining flexibility and lightness, suitable for various textile applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585792000007
    Figure 0007585792000007
  • Figure 0007585792000008
    Figure 0007585792000008
  • Figure 0007585792000009
    Figure 0007585792000009
Patent Text Reader

Abstract

A sheath-core composite fiber which is composed of two or more polymers, wherein a core component having a multifoliate shape with three or more projections is completely covered by a sheath component in a fiber cross-section of the sheath-core composite fiber, while having a ratio of the maximum thickness Smax of the sheath component to the minimum thickness Smin of the sheath component, namely Smax / Smin of 5.0 or more; and a multifilament which is composed of the core component of this sheath-core composite fiber. The present invention provides a sheath-core composite fiber and a multifilament, which are suitable for the achievement of a good textile that is comparable to natural silk.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a core-sheath composite fiber and a multifilament suitable for obtaining a textile having a luxurious luster similar to that of natural silk, and being light, soft and resilient. [Background technology]

[0002] Synthetic fibers made of polyester, polyamide, etc. have excellent mechanical properties and dimensional stability, and are therefore widely used in a variety of applications, from clothing to non-clothing. However, as people's lives have become more diverse and they are seeking a better life in recent years, there is a demand for advanced textures and functions not found in conventional synthetic fibers in many applications, including clothing.

[0003] When we look back at the evolution of technological development related to synthetic fibers, it is no exaggeration to say that each elemental technology has evolved with the motivation of imitating the characteristics of natural materials. This is because natural fibers such as linen, wool, cotton, and silk have excellent texture and functionality, and humans find the complex luster and texture they create attractive and luxurious.

[0004] In the history of synthetic fibers that have imitated natural materials, there have been proposals for a wide range of fiber technologies, from polymer technology to silk-making technology such as designing fiber cross-sectional shapes and blending different fibers, particularly for silky materials that aim to achieve the characteristics of silk, the finest natural material (hereinafter referred to as natural silk).

[0005] For example, it is known that when the cross-sectional shape of a polyester fiber, which has a relatively high degree of light reflection, is made into a multi-lobed irregular cross-section, the irregularities of the multi-lobed shape amplify the light reflection, resulting in a fiber with high brightness like natural silk but with a mild luster, and this fiber is produced in large quantities as a representative example of a silky material. However, it may be difficult to achieve the texture of natural silk (dry feeling, lightness, softness, resilience, etc.) other than the luster by simply making the cross-sectional shape more complex, and various fiber technologies related to composite fibers that pursue the texture of natural silk, etc. have been disclosed.

[0006] Patent Document 1 proposes a composite fiber having a multi-lobed cross section, with easily soluble components arranged at the apexes of the multi-lobed shape in a tapered shape toward the inside of the fiber. In the composite fiber, grooves are arranged at the apexes of the multi-lobed shape when the easily soluble components are subjected to a dissolution treatment, and it is said that the light reflection by the multi-lobed shape and the increased frictional force by the grooves make it possible to reproduce a luxurious luster and dry touch like natural silk, as well as the silk sound that is a characteristic of textiles made of natural silk.

[0007] Patent Document 2 proposes a composite fiber in which an easily soluble component divides a less easily soluble component into a plurality of pieces in the fiber cross section. In this composite fiber, when the easily soluble component is subjected to a dissolution treatment, a single composite fiber is divided into a plurality of fibers with an irregular cross section, and the combined effect of the fine fiber diameter and the irregular cross section makes it possible to impart a luxurious luster and dry touch like natural silk, as well as a soft texture.

[0008] It is also known that silky woven or knitted fabrics can be obtained from multifilaments made of blended fibers with different shrinkage rates, and Patent Document 3 proposes a blended multifilament made of at least two fiber groups with different thermal shrinkage rates, produced by a blended spinning method. In the blended multifilament made of different shrinkage rates, one fiber is made of a copolymer polyester, and when heat is applied, a difference in yarn length occurs between the fiber groups due to the shrinkage difference, which gives the fabric a rich volume and makes it possible to make a silky material. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 57-5912 [Patent Document 2] JP 2010-222771 A [Patent Document 3] Japanese Patent Application Publication No. 2-19528 Summary of the Invention [Problem to be solved by the invention]

[0010] As in Patent Document 1, by forming a special cross-sectional shape using eluted components, light reflection and frictional force can be controlled to reproduce to some extent the luxurious luster, dry feel, and unique silk sound that are characteristic of natural silk. However, in Patent Document 1, the interfiber voids may be insufficient, and the fabric may be formed with single fibers densely packed together. As a result, when worn as clothing, the light and soft texture that is comfortable may be lacking.

[0011] On the other hand, as in Patent Document 2, a method of imparting flexibility to a fabric by reducing the bending stiffness of each single fiber through thinning the fiber diameter by dissolution division or the like is effective in terms of imparting flexibility. However, in Patent Document 2, the voids formed in the multifilament may be limited, and furthermore, due to the narrowing of the thread diameter, the single fibers tend to be closely packed depending on the structure of the fabric. For this reason, in order to achieve the light texture characteristic of natural silk, it is necessary to precisely design the fabric, which may restrict the development of the material.

[0012] In addition, as in Patent Document 3, a method of imparting volume to a fabric by blending fibers with different shrinkage is effective in terms of obtaining lightness due to the volume, but since different fibers are blended during drawing or yarn processing, fiber bias may occur. When fiber bias occurs in this way, for example, clogging occurs in areas where high shrinkage fibers are concentrated, and soft texture may be impaired.

[0013] As described above, various techniques have been proposed for silky materials that utilize synthetic fibers, but it is difficult to say that there exists a technique that can achieve a well-balanced expression of a light, flexible, and resilient texture while having a luxurious luster like that of natural silk. Therefore, the object of the present invention is to provide a core-sheath composite fiber and a multifilament that are suitable for obtaining good textiles that are close to those of natural silk by solving the problems of the conventional techniques described above. [Means for solving the problem]

[0014] The object of the present invention is achieved by the following means: A sheath-core composite fiber made of two or more types of polymers, in which a multi-lobed core component having three or more convex portions is completely covered by a sheath component in a fiber cross section, and the ratio Smax / Smin of the maximum thickness Smax of the sheath component to the minimum thickness Smin is 5.0 or more; A multifilament consisting of the core component of the above-described core-sheath composite fiber, A multifilament having a void structure in which the average inter-fiber void distance is 5 to 30 μm, and the ratio of inter-fiber void distances less than 5 μm is 10 to 50%. A fiber product partially containing the above-described core-sheath composite fiber or multifilament. It is. Effect of the Invention

[0015] By using the core-sheath composite fiber or multifilament of the present invention, a unique void structure like that of natural silk can be formed in the multifilament, in which fine interfiber voids of less than 5 μm and coarse interfiber voids of 10 μm or more are uniformly mixed between each individual fiber, and a textile that has a luxurious luster similar to that of natural silk and is light, flexible, and resilient can be obtained. [Brief description of the drawings]

[0016] [Figure 1] This is a schematic diagram of the cross-sectional structure of raw silk extracted from silkworm cocoons, which are the source of natural silk. [Diagram 2] 1(a) and 1(b) are schematic diagrams illustrating examples of the cross-sectional structure of a core-sheath composite fiber of the present invention. [Diagram 3] 1(a)(b)(c) are schematic diagrams of cross-sectional structures of conventional composite fibers. [Figure 4] 1(a)(b)(c) are schematic diagrams illustrating examples of the cross-sectional structure of a core-sheath composite fiber of the present invention. [Diagram 5] 1(a) and 1(b) are schematic diagrams illustrating examples of the cross-sectional structure of a core-sheath composite fiber of the present invention. [Figure 6] 1(a)(b) is a schematic diagram of a cross-sectional structure of a composite fiber according to the prior art; [Figure 7] 1 is an example of the crimp form of the crimpable fibers constituting the multifilament of the present invention. [Figure 8] 1A and 1B are schematic diagrams of cross-sectional structures of the multifilament of the present invention, in which (a) is a diagram for understanding the meaning of "uniformly intermingled," and (b) is a diagram for understanding a method for measuring an average interfiber gap distance. [Figure 9]1(a)(b) is a schematic diagram showing an example of the cross-sectional structure of a crimped fiber constituting the multifilament of the present invention. [Figure 10] 1(a)(b) is a schematic diagram showing a cross-sectional structure of an example of a core-sheath composite fiber from which the multifilament of the present invention can be produced. [Figure 11] FIG. 1 is a schematic diagram of a cross-sectional structure of an example of a composite fiber from which a multifilament of the prior art can be produced. [Figure 12] FIG. 2 is a cross-sectional view of a composite spinneret for illustrating a method for producing the core-sheath composite fiber and multifilament of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will be described in detail below together with preferred embodiments.

[0018] In pursuing the principles of how natural silk's texture is expressed, if we look back at the silk-reeling process of natural silk, we can see that when raw silk is taken from the silkworm cocoon that is the source of natural silk, it has a fiber cross-sectional shape in which two triangular cross-sections of fibroin (a in Figure 1), which is a component that is difficult to dissolve, are covered with sericin (b in Figure 1), which is a component that is easily dissolved. Natural silk has a unique silk-reeling process in which sericin is dissolved from this raw silk, and it is thought that the light and flexible texture unique to natural silk is created by the appearance of interfiber voids due to the dissolution of this sericin.

[0019] Conventional silky materials often use a technique in which the fibers are thinned using chemicals such as alkali to form interfiber voids. However, the present inventors focused on the process by which these interfiber voids are formed, and through detailed observation of natural silk fabrics and silky materials made using conventional techniques, they discovered that there are significant differences in the size and distribution of the interfiber voids that are formed between natural silk and conventional materials.

[0020] In other words, in the case of natural silk, there is a uniform mixture of fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more between each individual fiber, whereas with conventional materials, only inter-fiber voids of either less than 5 μm or more than 10 μm can be formed, and it was discovered that this difference in void formation has a significant impact on the properties of woven and knitted fabrics.

[0021] When the size of the interfiber voids is 10 μm or more, the fibers fixed at the binding points of the woven or knitted fabric can move, improving flexibility and lightness due to the reduction in apparent density at high void ratios, while when the size of the interfiber voids is 5 μm or more, the resilience decreases due to the reduction in bending rigidity, so in conventional materials where only interfiber voids of less than 5 μm or more than 10 μm can be formed, there is a trade-off between lightness, flexibility, and resilience. On the other hand, in natural silk, which has a uniform mixture of coarse interfiber voids of 10 μm or more that are responsible for lightness and flexibility, and fine interfiber voids of less than 5 μm that are responsible for resilience, this trade-off relationship is eliminated, and a light, flexible, and resilient texture can be expressed in a well-balanced manner.

[0022] The present invention is based on this idea, and in order to form the unique inter-fiber voids that natural silk exhibits as described above, it is important that in the composite fiber of the present invention, the core component having a multi-leaf shape with three or more convex portions is completely covered by the sheath component in the fiber cross section of the core-sheath composite fiber made of two or more types of polymers, and this is the first requirement of the present invention.

[0023] The term "core-sheath composite fiber" as used herein refers to a fiber that is composed of two or more types of polymers and has a cross-sectional shape in which the sheath component covers the core component in a cross section perpendicular to the fiber axis.

[0024] The core and sheath components of the core-sheath composite fiber of the present invention are excellent in processability when both are thermoplastic polymers, so that the polymer group constituting the fiber is preferably, for example, a polyester-based, polyethylene-based, polypropylene-based, polystyrene-based, polyamide-based, polycarbonate-based, polymethyl methacrylate-based, polyphenylene sulfide-based polymer group and copolymers thereof. In particular, from the viewpoint of being able to impart high interfacial affinity and obtaining a fiber without composite cross-section abnormalities, it is preferable that the thermoplastic polymers used in the core-sheath composite fiber are all the same polymer group and copolymers thereof. Furthermore, from the viewpoint of being able to obtain a bending rigidity close to that of natural silk and also obtaining good color development when dyed, a particularly preferred range is a polyester-based combination. In addition, various additives such as inorganic substances such as titanium oxide, silica, barium oxide, carbon black, colorants such as dyes and pigments, flame retardants, fluorescent whitening agents, antioxidants, and ultraviolet absorbers may be contained in the polymer.

[0025] In addition, as environmental issues are gaining attention, the use of plant-derived biopolymers and recycled polymers in the present invention is also preferable from the viewpoint of reducing the environmental load, and the polymers used in the present invention described above can be recycled polymers that have been recycled by any of the methods of chemical recycling, material recycling, and thermal recycling. Even when biopolymers and recycled polymers are used, polyester resins can accentuate the features of the present invention as their polymer properties, and recycled polyesters can be preferably used in the present invention from the viewpoint of obtaining bending rigidity and good color development close to those of natural silk, as described above.

[0026] Here, the core-sheath composite fiber of the present invention is intended to obtain a multifilament consisting of a core component by dissolving the sheath component after performing advanced processing such as weaving and knitting. For this reason, it is preferable that the core component is difficult to dissolve and the sheath component is easy to dissolve in the solvent used to dissolve the sheath component, and it is preferable to select the core component according to the application and then select the sheath component from the above-mentioned polymers in consideration of the solvent that can be used from the core component. In this case, the larger the dissolution rate ratio of the difficult to dissolve component (core component) to the easy to dissolve component (sheath component) in the solvent, the more preferable the combination, and it is recommended to select polymers with a dissolution rate ratio of up to 3000 times.

[0027] The sheath component is preferably selected from polymers that are melt moldable and more easily soluble than other components, such as polyesters and their copolymers, polylactic acid, polyamide, polystyrene and its copolymers, polyethylene, and polyvinyl alcohol. From the viewpoint of simplifying the elution process of the sheath component, the sheath component is preferably a copolymerized polyester, polylactic acid, polyvinyl alcohol, etc., which are easily soluble in aqueous solvents or hot water, etc. In particular, since they are easily soluble in aqueous solvents such as alkaline aqueous solutions while maintaining crystallinity, even in false twist processing in which rubbing is applied under heating, fusion between composite fibers does not occur, and from the viewpoint of passability through higher-level processing, particularly preferred polymers include polyesters copolymerized with 5 mol% to 15 mol% of 5-sodium sulfoisophthalic acid and polyesters copolymerized with 5 wt% to 15 wt% of polyethylene glycol having a weight average molecular weight of 500 to 3000 in addition to the above-mentioned 5-sodium sulfoisophthalic acid.

[0028] Generally, when the size of the inter-fiber voids is increased, the fibers fixed at the binding points of the woven or knitted fabric can move, improving flexibility and lightness due to a decrease in apparent density at a high void ratio, but it also reduces the resilience due to a decrease in bending rigidity as described above. To resolve this trade-off, it is important to have a mixture of coarse inter-fiber voids of 10 μm or more, which are responsible for improving lightness, and fine inter-fiber voids of less than 5 μm, which balance flexibility and resilience, and to achieve this, it is necessary that in the core-sheath composite fiber of the present invention, the sheath component completely covers the multi-lobal core component having three or more projections.

[0029] If the sheath component completely covers the core component of a multi-lobed shape having three or more convex parts, coarse inter-fiber voids of 10 μm or more are formed by sheath elution in the concave parts of the multi-lobed shape with a large sheath thickness, while fine inter-fiber voids of less than 5 μm can be formed in the convex parts with a small sheath thickness, so that a light and soft texture characteristic of natural silk can be achieved while also achieving a bouncy texture. Furthermore, the formation of convex parts on the fiber surface can also provide a light reflection amplification effect, so that not only can a luxurious luster such as high brightness and mild luster like natural silk be expressed, but also the formation of convex parts on the fiber surface can provide a dry tactile feel. From this perspective, the more convex parts there are, the greater the inter-fiber void formation, the luster effect, and the dry feel, so for example, a tri-lobed shape with three convex parts as shown in Figure 2(a) or a quadruple-lobed shape with four convex parts as shown in Figure 2(b) is preferable. However, if the number of concave-convex portions becomes too large, the spacing between the concave-convex portions becomes finer and the effect gradually approaches that of a round cross section, so the substantial upper limit for the number of convex portions of the multi-lobal shape of the core component in the present invention is six.

[0030] In the composite fiber of the present invention, from the viewpoint of forming fine inter-fiber gaps of less than 5 μm that are sufficient to allow movement between adjacent single fibers by dissolution of the sheath component, it is preferable that the composite fiber has a ratio Smin / D of the minimum thickness Smin of the sheath component to the fiber diameter D of 0.01 or more.

[0031] In the present invention, the fiber diameter D is obtained by embedding the multifilament made of the core-sheath composite fiber of the present invention in an embedding agent such as epoxy resin, and taking an image of the fiber cross section perpendicular to the fiber axis with a transmission electron microscope (TEM) at a magnification at which 10 or more fibers can be observed. In this case, if metal dyeing is applied, the contrast of the joint between the core component and the sheath component can be made clear by utilizing the dyeing difference between the polymers. The diameter of the fiber randomly sampled in each image is measured in μm units to the first decimal place, and the simple number average of the results of this operation for 10 randomly sampled fibers is calculated, and the value rounded off to the first decimal place is defined as the fiber diameter D (μm). Here, if the fiber cross section perpendicular to the fiber axis is not a perfect circle, its area is measured, and the value obtained by converting it into a circle is used.

[0032] The minimum thickness Smin of the sheath component in the present invention is calculated by drawing a straight line from the center of gravity G1 of the core component 1 present on the fiber cross section toward any fiber surface, measuring the distance S1-F between the intersection point S1 of the periphery of the core component 1 with the line and the intersection point F of the fiber surface with the line to the first decimal place, and calculating the minimum value among the obtained values. This operation was performed on 10 randomly selected fibers, and a simple number average was calculated, and the value rounded off to the first decimal place was determined as the minimum thickness Smin (μm) of the sheath component. Here, for example, as shown in Fig. 4(a) and Fig. 5(b), if a core component 2 different from the core component 1 whose center of gravity is taken exists on a line drawn from the center of gravity G1 of the core component 1 toward any fiber surface, the value measured is used as the distance S1-S2 between the intersection point S1 of the periphery of the core component 1 with the line and the intersection point S2 closest to S1 among the intersection points of the periphery of the core component 2 with the line. Regarding the symbols in the figure, for example, G1 is the center of gravity of core component 1, G2 is the center of gravity of core component 2, and G is a general term for them, and the same applies to the other symbols.

[0033] Furthermore, the ratio (Smin / D) of the obtained fiber diameter D to the minimum thickness Smin of the sheath component was simply averaged, and the value was rounded off to two decimal places to obtain Smin / D.

[0034] When the sheath components are arranged so that the ratio Smin / D of the minimum thickness Smin of the sheath components to the fiber diameter D is 0.01 or more, the resulting woven or knitted fabric can express fine inter-fiber voids of less than 5 μm that allow the fibers fixed at the binding points of the woven or knitted fabric to move due to sheath dissolution, and can impart a soft texture, which is preferable. From this perspective, the higher the Smin / D, the larger the size of the fine inter-fiber voids of less than 5 μm, making it easier for the fibers to move, so if Smin / D is 0.03 or more, it is possible to express the high drape characteristic of natural silk due to further increased flexibility, and this can be listed as a more preferable range. On the other hand, if the size of the inter-fiber voids becomes too large, the bending recovery property also decreases, and the resilience, which is one of the textures of natural silk, is impaired, so the substantial upper limit in the present invention is 0.1.

[0035] As mentioned above, in order to resolve the trade-off relationship between the increase in the size of interfiber voids and the decrease in resilience, it is important to form coarse interfiber voids of 10 μm or more due to sheath elution in the recesses of the multi-leaf shape with a large sheath thickness, while forming fine interfiber voids of less than 5 μm in the protrusions with a small sheath thickness, by making the core component multi-leaf. Furthermore, it is important to control the size of the maximum and minimum interfiber voids. As a result of intensive research by the present inventors, it was found that by setting the ratio of the maximum and minimum interfiber voids to a certain range or more, a sufficient difference is created between the two interfiber voids, and the light, flexible and resilient texture peculiar to natural silk can be accentuated. In other words, the second requirement is that the ratio Smax / Smin of the maximum thickness Smax to the minimum thickness Smin of the sheath component is 5.0 or more.

[0036] In the present invention, the maximum thickness Smax of the sheath component is calculated by drawing a straight line from the center of gravity G1 of the core component 1 present on the fiber cross section toward any fiber surface, measuring the distance S1-F between the intersection point S1 of the periphery of the core component 1 with the line and the intersection point F of the fiber surface with the line to the first decimal place, and calculating the maximum value among the obtained values. This operation was performed on 10 randomly selected fibers, and a simple number average was calculated, and the value rounded off to the first decimal place was determined as the minimum thickness Smax (μm) of the sheath component. Here, for example, as shown in FIG. 4(a) and FIG. 5(b), if a core component 2 different from the core component 1 whose center of gravity is taken exists on a line drawn from the center of gravity G1 of the core component 1 toward any fiber surface, the value measured is the distance S1-S2 between the intersection point S1 of the periphery of the core component 1 with the line and the intersection point S2 closest to S1 among the intersection points of the periphery of the core component 2 with the line.

[0037] Furthermore, the ratio (Smax / Smin) of the maximum thickness Smax of the sheath component to the minimum thickness Smin of the sheath component was simply averaged, and the ratio was rounded to one decimal place to obtain Smax / Smin.

[0038] In the core-sheath composite fiber of the present invention, if the ratio Smax / Smin of the maximum thickness Smax of the sheath component corresponding to the coarse inter-fiber voids of 10 μm or more and the minimum thickness Smin corresponding to the fine inter-fiber voids of less than 5 μm is 5.0 or more, the light, flexible and resilient texture characteristic of natural silk can be sufficiently emphasized. Furthermore, if Smax / Smin is 10.0 or more, the inter-fiber void size close to that characteristic of natural silk can be formed, and lightness closer to that of natural silk can be obtained, so this is a more preferable range. From the viewpoint of lightness, the higher the Smax / Smin, the more preferable, but if Smax / Smin is high, the irregularity of the irregular cross-section fiber obtained after the sheath component is dissolved increases, and high-level problems such as glare and streaks may occur when the fiber is made into a fabric, so the substantial upper limit of Smax / Smin is 30.0.

[0039] The area ratio of the sheath component in the core-sheath composite fiber of the present invention is preferably 10% to 50%. As the area occupied by the sheath component is increased, the effect of forming inter-fiber voids due to the elution of the sheath component is enhanced, so that the area ratio is preferably 10% or more, and more preferably 20% or more. In addition, while a higher area ratio of the sheath component is preferable from the viewpoint of inter-fiber voids, there is a possibility that excessive elution of the sheath component may cause a decrease in strength or a long elution treatment time, so that the practical upper limit is 50%.

[0040] In the core-sheath composite fiber of the present invention, the fiber cross section is a perfect circle or an ellipse, and the inscribed circle diameter R A (Diameter of A in Fig. 4(a)) and circumscribed circle diameter R B (The diameter of B in Fig. 4(a)) The relationship is 1.0≦R B / R A It is preferable that R is ≦2.5. B / R A represents the degree of deformation of the fiber.

[0041] In the sheath-core composite fiber of the present invention, it is important to mix different inter-fiber voids by forming a multi-lobal shape due to sheath elution, and it is preferable to use a sheath-core composite fiber having a perfect circle as shown in Figures 2(a) and (b), Figures 4(b) and (c), and Figure 5(a), or an elliptical shape as shown in Figures 4(a) and 5(b), with a multi-lobal core component, since this allows inter-fiber voids of 10 μm or more and inter-fiber voids of less than 5 μm to be mixed. B / R A 1.0≦R B / R A If the ratio is ≦2.5, the core-sheath composite fiber of the present invention is likely to be closely packed when present as a multifilament, and the inter-fiber voids obtained after dissolution into the sheath component can be made uniform without unevenness, which is preferable from the viewpoint of quality control.

[0042] In the sheath-core composite fiber of the present invention, from the viewpoint of emphasizing a dry touch after dissolution of the sheath component, it is preferable that the multi-lobal core component has grooves at the tips of the convex portions toward the center of gravity of the core component, and the ratio GN / GM of the distance GM from the center of gravity G of the core component to the groove bottom M and the distance GN from the center of gravity G of the core component to the tip N of the convex portion is 1.1 to 1.5.

[0043] The distance GM from the center of gravity G of the core component to the groove bottom M in the present invention is calculated by, for example, calculating the distance between the center of gravity G1 of the core component, which is the intersection of two arbitrary lines that halve the area of ​​the core component, and the groove bottom M1, which is the point on the groove surface closest to the center of gravity G1 of the core component, as shown in Figure 5(a). If there are two or more core components, the largest value among the values ​​calculated for each core component was used. This operation was performed on 10 randomly selected fibers, and the simple number average of the results was calculated and rounded off to the first decimal place to determine the distance GM (μm) from the center of gravity G of the core component to the groove bottom M.

[0044] The distance from the center of gravity G of the core component to the tip N of the protrusion, GN, in the present invention is calculated as the distance between the center of gravity G1 of the core component and the tip N1 of the protrusion, which is the farthest point from the center of gravity G1 of the core component on the groove surface, as shown in Fig. 5(a), for example. If there are two or more core components, the largest value among the values ​​calculated for each core component was used. This operation was performed on 10 randomly selected fibers, and the simple number average of the results was calculated and rounded off to the nearest tenth to obtain the distance GN (μm) from the center of gravity G of the core component to the tip N of the protrusion.

[0045] Furthermore, the ratio (GN / GM), which is the distance from the center of gravity G of the core component to the groove bottom M, GM, and the distance from the center of gravity G of the core component to the tip N of the convex portion, GN, was calculated as a simple number average and rounded off to two decimal places to obtain GN / GM. In this case, if the core component does not have a groove at the tip of the convex portion, GN / GM = 1.0.

[0046] In the present invention, it is preferable to have a groove at the tip of the convex portion with a depth such that GN / GM is 1.1 or more toward the center of gravity of the core component after the sheath component is dissolved, because the surface of the groove comes into contact with the skin at points, thereby improving the frictional force and emphasizing the dry tactile sensation. Furthermore, a groove depth of GN / GM of 1.3 or more not only provides a dry feeling, but also diffuses light, resulting in a milder gloss, and suppresses white blur due to regular reflection of light, improving color development when dyed, so this is a more preferable range. However, if the groove depth is made deeper, the frictional force may become too high, causing deterioration of abrasion resistance such as fibrillation, so the practical upper limit of GN / GM is 1.5.

[0047] From the viewpoint of pursuing the texture of natural silk by reproducing the interfiber gaps specific to natural silk in more detail, it is preferable that in the core-sheath composite fiber of the present invention, the core component is divided into two or more parts by the sheath component, and each divided core component has the multi-lobal shape described above.

[0048] At the stage of raw silk taken from silkworm cocoons, which are the source of natural silk, the cross-sectional shape of the fiber is composed of two triangular cross-sections of fibroin (a in FIG. 1), which is a component that is difficult to dissolve, covered with sericin (b in FIG. 1), which is a component that is easily dissolved. In other words, the gap between adjacent fibers after division is always controlled only by the rate of sericin elution, regardless of the arrangement of the single fibers in the multifilament, and this can be understood to create a state in which fine inter-fiber gaps of less than 5 μm are stably present between each single fiber, which is characteristic of natural silk. In the core-sheath composite fiber of the present invention, the core component is divided into two or more by the sheath component, and each divided core component preferably has a multi-leaf shape. The number of divisions is not particularly limited as long as it is two or more, and for example, as shown in FIG. 4(c), it may be divided into six core components. However, as the number of divisions increases, the inter-fiber gaps obtained become smaller and precise control of the cross section becomes difficult, so the practical upper limit of the number of divisions is 10.

[0049] In the present invention, in order to make the inter-fiber voids larger, it is preferable to arrange polymers with different melting points next to each other in the fiber cross section, and to cause the core-sheath composite fiber to have a crimped form due to the difference in shrinkage during heat treatment caused by the difference in melting points, or to cause a difference in yarn length to appear after the sheath component of the core-sheath composite fiber is dissolved. If the inter-fiber voids can be made larger, not only can the diffuse reflection of light be increased to obtain a luxurious luster and high color development, but the porosity is increased and the apparent density is reduced, thereby emphasizing the lightness.

[0050] That is, in the core-sheath composite fiber of the present invention, in the core component divided by the sheath component, it is preferable that adjacent core component 1 (e.g., c1 in Figures 4(a), (b) and (c)) and core component 2 (e.g., c2 in Figures 4(a), (b) and (c)) are made of polymers with different melting points.

[0051] In the present invention, the polymers with different melting points refer to a combination of polymers with melting points differing by 10° C. or more from a group of melt-moldable polymers and copolymers thereof, such as polyesters, polyethylenes, polypropylenes, polystyrenes, polyamides, polycarbonates, polymethyl methacrylates, and polyphenylene sulfide. In addition, in the core-sheath composite fiber of the present invention, the purpose is to utilize the shrinkage difference of the core component to create a crimped form in the core-sheath composite fiber, or to create a difference in fiber length after the sheath component of the core-sheath composite fiber is dissolved. Therefore, as a combination of polymers with different melting points for the core components, it is preferable to use a high shrinkage low melting point polymer as core component 1 and a low shrinkage high melting point polymer as core component 2. Examples of such combinations of low melting point polymers and high melting point polymers include, for example, polyester-based copolymers of polyethylene terephthalate / polyethylene terephthalate, polybutylene terephthalate / polyethylene terephthalate, polytrimethylene terephthalate / polyethylene terephthalate, thermoplastic polyurethane / polyethylene terephthalate, polyester-based elastomer / polyethylene terephthalate, and the like. Examples of combinations include ethylene terephthalate, polyester elastomer / polybutylene terephthalate, polyamide-based combinations such as nylon 66 / nylon 610, nylon 6-nylon 66 copolymer / nylon 6 or 610, PEG copolymerized nylon 6 / nylon 6 or 610, thermoplastic polyurethane / nylon 6 or 610, and polyolefin-based combinations such as ethylene-propylene rubber finely dispersed polypropylene / polypropylene and propylene-α-olefin copolymer / polypropylene. From the viewpoints of not only being able to achieve bending rigidity close to that of natural silk in the core-sheath composite fiber of the present invention, but also being able to obtain good color development when dyed, it is particularly preferable that the core component to be divided be a polyester-based combination.Furthermore, examples of copolymerization components in copolymerized polyethylene terephthalate include succinic acid, adipic acid, azelaic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, maleic acid, phthalic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid. From the viewpoint of maximizing the difference in shrinkage with polyethylene terephthalate, it is preferable to use polyethylene terephthalate in which 5 mol % to 15 mol % of isophthalic acid is copolymerized.

[0052] The area ratio of the core component 1, which is a low melting point polymer, to the core component 2, which is a high melting point polymer, in the sheath-core composite fiber of the present invention is preferably in the range of 70% / 30% to 30% / 70%, i.e., core component 1 / core component 2. If the ratio is in this range, the crimped form of the sheath-core composite fiber due to the shrinkage difference, or the yarn length difference after the sheath component of the sheath-core composite fiber is dissolved, can be fully expressed without being affected by hardening of the texture due to denseness when the low melting point polymer highly shrinks during heat treatment, and larger inter-fiber voids can be obtained.

[0053] The core-sheath composite fiber of the present invention is produced by first forming various sheet-like fiber structures such as woven or knitted fabrics, nonwoven fabrics, and paper, and then dissolving the sheath component to obtain a multifilament composed of the core component. The multifilament can have the texture of natural silk, such as a luxurious luster and a dry touch, which are manifested by the unique fiber cross-sectional shape and interfiber voids, and a light, flexible, and resilient texture.

[0054] In order to maximize the texture of natural silk, such as the luxurious luster and the light, flexible, and resilient texture described above, it is important to form a void structure in the multifilament in which fine interfiber voids of less than 5 μm and coarse interfiber voids of 10 μm or more are uniformly mixed between each fiber, as in natural silk. Therefore, it is important that the multifilament of the present invention has a void structure in which the average interfiber void distance is 5 to 30 μm, and the proportion of interfiber void distances less than 5 μm is 10 to 50%.

[0055] The inter-fiber gap distance in the present invention is obtained by taking an image of a cross section of a multifilament fabric perpendicular to the length direction of the fabric and perpendicular to the fiber axis direction of the multifilament with a scanning electron microscope (SEM) at a magnification where 10 or more fibers can be observed. For each of the taken images, a perfect circle that fits 10 fibers is drawn as shown in FIG. 8(b), and one arbitrary fiber is selected from the 10 fibers present inside the perfect circle, and the intersection points between the line connecting the center of gravity of the fiber and the adjacent fiber and the surface of each fiber are obtained, and the distance between the intersection points is measured in μm units to the first decimal place. The obtained value is rounded off to the first decimal place to determine the inter-fiber gap distance (μm). "Adjacent" here means that no other fiber is present on the line connecting the centers of gravity of any two fibers. This operation was performed on all adjacent fibers in the 10 fibers inside the perfect circle as shown in Figure 8(b), and the simple number average of the results was calculated and rounded off to the first decimal place to obtain the average inter-fiber gap distance (μm). The percentage of inter-fiber gap distances less than 5 μm was also calculated.

[0056] The longer the average inter-fiber gap distance, the more space is created for the fibers fixed at the binding points of the woven or knitted fabric to move, and the effect of improving flexibility is obtained, so the average inter-fiber gap distance must be 5 μm or more. Furthermore, if the average inter-fiber gap distance is 10 μm or more, the apparent density decreases when the fabric is made into a fabric by expressing bulkiness, and the effect of improving lightness is also added, so that a light and soft texture similar to that of natural silk can be expressed, which is a preferable range. From this point of view, while lightness and flexibility are improved, the effect of suppressing the decrease in bending rigidity at inter-fiber gaps of less than 5 μm uniformly mixed in the multifilament is small, and the resilience tends to decrease, so the actual upper limit of the average inter-fiber gap distance is 30 μm.

[0057] In addition to the above, in order to suppress the decrease in bending rigidity caused by an increase in the average gap distance and to maintain the resilience, it is necessary that the ratio of inter-fiber gap distances less than 5 μm is 10% or more. Furthermore, if the ratio of inter-fiber gap distances less than 5 μm is 20% or more, the trade-off relationship between lightness, flexibility, and resilience is eliminated, and a light, flexible, and resilient texture can be expressed in a well-balanced manner, which is considered to be a preferable range. From this perspective, if the ratio of inter-fiber gap distances less than 5 μm is increased, the resilience improves, but lightness and flexibility tend to decrease, so the practical upper limit of the ratio of inter-fiber gap distances less than 5 μm is 50%.

[0058] The multifilament of the present invention preferably has a void structure with a void ratio of 30 to 80%.

[0059] The void ratio as referred to in the present invention is determined by taking an image of a cross section of a multifilament fabric perpendicular to the length direction of the fabric and perpendicular to the fiber axis direction of the multifilament with a scanning electron microscope (SEM) at a magnification where 10 or more fibers can be observed. For each image taken, a perfect circle that fits 10 fibers is drawn as in Figure 8(b), and the total cross-sectional area of ​​the 10 fibers present inside the perfect circle is subtracted from the cross-sectional area of ​​the perfect circle to calculate the value. In this case, if 1 / 2 or more of the fiber is contained inside the perfect circle, it is counted as one fiber, and the cross-sectional area is expressed in μm 2 The measurement was made to the first decimal place. The obtained value was then divided by the cross-sectional area of ​​the perfect circle to calculate the porosity (%), which was then multiplied by 100 and rounded off to the nearest tenth.

[0060] It is preferable that the multifilament has a void structure with a void ratio of 30% or more, since this creates space sufficient for the fibers fixed at the binding points of the woven or knitted fabric to move, thereby improving flexibility.

[0061] Furthermore, a void structure with a void ratio of 50% or more is considered to be a more preferable range because the high void ratio reduces the apparent density when made into a fabric, and also improves lightness, allowing for a light and soft texture similar to that of natural silk to be expressed. From this perspective, the higher the average inter-fiber void distance and void ratio, the more improved the lightness and softness will be, but the effect of suppressing the decrease in bending rigidity will be smaller in inter-fiber voids of less than 5 μm uniformly mixed in the multifilament, and the resilience will tend to decrease, so a void structure with a void ratio of 80% is the practical upper limit.

[0062] In the multifilament of the present invention, it is preferable that the multifilament is made of two or more kinds of crimpable fibers composed of polymers with different melting points, and the crimpable fibers are uniformly mixed. Here, the crimpable fibers referred to in the present invention have a crimped form in which the fibers are twisted as shown in FIG.

[0063] Furthermore, in the present invention, "crimpable fibers are uniformly mixed" means that, in any crimpable fiber X in the multifilament, as shown in Figure 8(a), among all the crimpable fibers adjacent to the crimpable fiber X, there is at least one crimpable fiber Y composed of a polymer different from that of the crimpable fiber X. In addition, in the present invention, "adjacent" means that no other crimpable fiber is present on the straight line connecting the center of gravity of the crimpable fiber X and the center of gravity of any crimpable fiber. There are various methods for obtaining the void structure possessed by the multifilament of the present invention, such as a method of bundling a plurality of sheath-core composite fibers as shown in FIG. 2(a) or FIG. 5(a) and then dissolving the sheath component, and a method of bundling a plurality of sheath-core composite fibers in which core components made of polymers with different melting points are arranged side by side as shown in FIG. 4(a), (b), and (c), dissolving the sheath component, dividing the core components, and then expressing a difference in fiber length by heat treatment. However, from the viewpoint of more uniformly mixing fine inter-fiber voids of less than 5 μm and large inter-fiber voids of 10 μm or more in the multifilament, it is preferable to use a method of bundling a plurality of sheath-core composite fibers in which the fiber cross section is divided into two by the sheath component d, the core components c1 and c2 are made of polymers with different melting points, as shown in FIG. 10(a) and (b), and then expressing a crimped morphology by heat treatment, and then dissolving the sheath component and dividing the core components by polymer, thereby uniformly mixing crimpable fibers made of different polymers.

[0064] By using the above method, the core-sheath composite fiber is subjected to a heat treatment to develop a crimped form, and coarse inter-fiber gaps of 10 μm or more can be formed. Furthermore, since the sheath component exists between the core components, after the sheath component is dissolved, inter-fiber gaps of less than 5 μm can be more stably formed between adjacent crimpable fibers made of polymers with different melting points, so that fine inter-fiber gaps of less than 5 μm and coarse inter-fiber gaps of 10 μm or more can be more uniformly mixed in the multifilament. That is, in the multifilament of the present invention, it is preferable that the multifilament is made of two or more types of crimpable fibers made of polymers with different melting points, and the crimpable fibers are uniformly mixed, and this makes it possible to more prominently display the texture of natural silk, such as the luxurious luster and dry touch expressed by the unique fiber cross-sectional shape and void structure, and the light, soft and resilient texture.

[0065] In the multifilament of the present invention, the crimpable fiber preferably has a crimp peak count of 5 peaks / cm or more.

[0066] Within this range, the excluded volume effect between fibers can be fully exerted, and it is possible to form coarse interfiber gaps of several tens of μm. Furthermore, if it is 10 peaks / cm or more, the excluded volume effect between fibers is further increased, the size of the interfiber gaps can be further increased, and a light and soft texture similar to that of natural silk can be expressed, so this is considered to be a more preferable range. On the other hand, if the number of crimped peaks is increased, the steric hindrance effect due to the crimped form exceeds the excluded volume effect, causing entanglement between the fibers and impairing flexibility, so the upper limit of the number of crimped peaks is 100 peaks / cm.

[0067] In the multifilament of the present invention, the difference in yarn length between two or more kinds of crimpable fibers made of different polymers is preferably 3% or more. By making the difference in yarn length 3% or more, the number of crimp peaks of the crimpable fibers made of polymers with different melting points that exhibit a crimped morphology can be made 10 peaks / cm or more. However, if the difference in yarn length becomes too large, the number of crimp peaks also increases accordingly, and the steric hindrance effect due to the crimped morphology exceeds the excluded volume effect, causing entanglement between the fibers, which may impair flexibility, so the upper limit of the difference in yarn length is 20%.

[0068] In the multifilament of the present invention, it is preferable that the crimpable fiber is composed of a single polymer. If the crimpable fiber is composed of a single polymer, the core-sheath composite fiber composed of adjacent polymers with different melting points will develop a crimped form by heat treatment, and the crimp phase of adjacent crimpable fibers will be aligned, making it possible to form fine inter-fiber gaps of less than 5 μm. On the other hand, if the fiber is composed of two or more different polymers, the center of gravity of the polymer on the cross section will be different depending on the composite cross section, and the fibers composed of adjacent polymers with different melting points will become crimpable fibers with different crimp forms after the sheath component is dissolved, so the crimp phase will not be aligned, making it difficult to stably form fine inter-fiber gaps of less than 5 μm.

[0069] In the fibers constituting the multifilament of the present invention, it is preferable that the fiber cross section has a multi-lobal shape having three or more convex portions.

[0070] If the fiber cross section has a multi-lobed shape with three or more convex portions, the unevenness on the fiber surface will provide a light reflection amplification effect, and the complex reflection of light due to the presence of the large and small interfiber voids described above will result in a luxurious luster with high brightness and mild luster like natural silk. Furthermore, the unevenness on the fiber surface will improve friction, resulting in a dry feel to the touch. From this perspective, the more convex portions there are, the higher the luster effect and the dry feel will be, but if the number of convex portions is too large, the intervals between the convex portions will become finer, and the effect will gradually approximate that of a round cross section, so the practical upper limit of the convex portions that the fibers constituting the multifilament of the present invention have is six.

[0071] In the fibers constituting the multifilament of the present invention, the inscribed circle diameter R C (Diameter of C in Figure 9(a)) and circumscribed circle diameter R D (Diameter of D in Fig. 9(a)) is 1.5≦R D / R C It is preferable that R is ≦2.0. D / R C If the range is set in this way, the light reflected and amplified by the irregularities of the multi-lobed shape is reflected uniformly without glare, which is preferable from the viewpoint of quality control.

[0072] In the fibers constituting the multifilament of the present invention, from the viewpoint of emphasizing a dry touch, it is preferable that the fibers have grooves at the tips of the convex portions in the cross section of the fiber, and the ratio (MN / D) of the distance from the groove bottom M to the convex portion tip N, MN, to the fiber diameter D is 0.04 to 0.20.

[0073] The ratio (MN / D) of the distance from the groove bottom M to the convex tip N, MN, and the fiber diameter D, referred to in the present invention, can be determined by embedding the multifilament of the present invention in an embedding agent such as epoxy resin, and taking images of the fiber cross section perpendicular to the fiber axis with a scanning electron microscope (SEM) at a magnification such that 10 or more fibers can be observed. For fibers randomly extracted from each of the taken images within the same image, the distance MN between the groove bottom M, which is the closest point to the groove surface, and the convex tip N, which is the furthest point, from the center of gravity G, which is the intersection of any two straight lines that halve the cross-sectional area of ​​the crimped fiber in the fiber cross section, was calculated, as shown in Figure 9, for example.

[0074] The diameter of the fiber was measured in μm units to the first decimal place. If the fiber cross section perpendicular to the fiber axis was not a perfect circle, the area was measured and the value calculated as a circle was used as the fiber diameter.

[0075] The ratio (MN / D) of the distance MN from the groove bottom M to the protrusion tip N and the fiber diameter D was calculated to four decimal places, and this operation was performed on 10 randomly selected fibers to calculate a simple number average of the results, which was rounded off to three decimal places to obtain MN / D. In this case, if the crimpable fiber did not have a groove at the tip of the protrusion, MN / D=0.

[0076] In the fibers constituting the multifilament of the present invention, it is preferable to have grooves with a depth of 0.04 or more for MN / D, which enhances the dry touch by improving the frictional force caused by the groove surface contacting the skin at points. Furthermore, a groove depth of 0.10 or more for MN / D not only provides a dry feel, but also diffuses light, resulting in a milder luster, and suppresses white blurring due to regular reflection of light, improving color development when dyed, so this is a more preferable range. However, if the groove depth is made deeper, the frictional force may become too high, causing deterioration of abrasion resistance such as fibrillation, so the practical upper limit of MN / D is 0.20.

[0077] In the fibers constituting the multifilament of the present invention, the fiber diameter is preferably 15 μm or less from the viewpoint of making the texture softer. Furthermore, by making the fiber diameter 12 μm or less, the fiber diameter approaches the single yarn fineness of natural silk, which is about 10 μm, and a texture closer to that of natural silk can be obtained, which is a suitable range for general clothing applications such as innerwear, shirts, blouses, etc. that come into contact with the skin. However, if the fiber diameter is too small, the bending recovery is reduced, and not only the resilience, which is one of the textures of natural silk, but also the color development may be reduced, so the fiber diameter is preferably 8 μm or more.

[0078] In the sheath-core composite fiber and multifilament of the present invention, a unique void structure can be formed in which fine interfiber voids of less than 5 μm and coarse interfiber voids of several tens of μm are uniformly mixed between each fiber, as in natural silk. Therefore, when the sheath-core composite fiber or multifilament of the present invention is used as at least a part of a textile product, it is possible to reproduce the various textures peculiar to natural silk, and therefore, combined with the ease of handling unique to synthetic fibers, it can be suitably used in a wide range of textile products, from general clothing such as jackets, skirts, pants, underwear, and sports clothing, clothing materials, interior products such as carpets, sofas, and curtains, vehicle interior products such as car seats, cosmetics, cosmetic masks, wiping cloths, and health products for daily life.

[0079] An example of a method for producing the core-sheath composite fiber and multifilament of the present invention will be described in detail below.

[0080] The core-sheath composite fiber of the present invention, which is made of two or more polymers, can be produced by melt spinning, which is intended to produce continuous fibers, wet and dry-wet solution spinning, and melt-blowing and spunbonding methods suitable for obtaining a sheet-like fiber structure, but from the viewpoint of increasing productivity, melt spinning is preferred. In the melt spinning method, the fiber can be produced by using a composite spinneret, which will be described later, and the spinning temperature is set to a temperature at which the polymers used, mainly those with high melting points or high viscosity, exhibit fluidity. The temperature at which the fiber exhibits fluidity varies depending on the molecular weight, but stable production is possible when it is set between the melting point of the polymer and melting point + 60°C.

[0081] The spinning speed is preferably about 500 to 6000 m / min, and can be changed depending on the physical properties of the polymer and the purpose of use of the fiber. In particular, from the viewpoint of high orientation and improving mechanical properties, it is preferable to set the spinning speed to 500 to 4000 m / min and then draw the fiber, since this can promote uniaxial orientation of the fiber. In drawing, it is preferable to appropriately set the preheating temperature using the softening temperature, such as the glass transition temperature of the polymer, as a guide. The upper limit of the preheating temperature is preferably a temperature at which yarn path disturbance does not occur due to spontaneous elongation of the fiber during the preheating process. For example, in the case of PET, which has a glass transition temperature of about 70°C, the preheating temperature is usually set to about 80 to 95°C.

[0082] In addition, the sheath-core composite fiber of the present invention can be produced stably when the discharge amount per hole in the spinneret is about 0.1 to 10 g / min. After cooling and solidifying, the discharged polymer flow is given an oil agent and taken up by rollers set to a specified peripheral speed. Thereafter, it is stretched by heated rollers to become the desired sheath-core composite fiber.

[0083] Furthermore, in the core-sheath composite fiber of the present invention which is made of two or more types of polymers, it is preferable to set the melt viscosity ratio of the polymers used to less than 5.0 and the difference in solubility parameter values ​​to less than 2.0, since this makes it possible to stably form a composite polymer flow and obtain a fiber with a good composite cross section.

[0084] As the composite spinneret used in producing the core-sheath composite fiber of the present invention made of two or more types of polymers, it is preferable to use the composite spinneret described in JP 2011-208313 A. The composite spinneret shown in Fig. 12 of the present application is assembled in a spin pack in a laminated state of three major members, namely, from the top, a metering plate 1, a distribution plate 2, and a discharge plate 3, and is used for spinning. Incidentally, Fig. 12 shows an example in which three types of polymers, namely, polymer A, polymer B, and polymer C, are used. With conventional composite spinnerets, it is difficult to composite three or more types of polymers, and it is therefore preferable to use a composite spinneret utilizing fine flow paths as exemplified in Fig. 12.

[0085] In the spinneret member shown in FIG. 12, the metering plate 1 measures and introduces the amount of polymer per each discharge hole and each distribution hole, the distribution plate 2 controls the composite cross section and its cross-sectional shape in the cross section of the single fiber, and the discharge plate 3 compresses the composite polymer flow formed by the distribution plate 2 and discharges it.

[0086] In order to avoid confusing the explanation of the composite spinneret, it is not shown in the figure, but for the members to be stacked above the metering plate 1, a member with a flow path formed in accordance with the spinning machine and spinning pack may be used. By designing the metering plate 1 to match the existing flow path members, the existing spinning pack and its members can be used as they are. For this reason, it is not necessary to dedicate a spinning machine specifically for the spinneret. In addition, it is preferable to actually stack multiple flow path plates between the flow path and the metering plate or between the metering plate 1 and the distribution plate 2. The purpose of this is to provide a flow path through which the polymer is efficiently transported in the cross-sectional direction of the spinneret and the cross-sectional direction of the single fiber, and to configure it so that it is introduced into the distribution plate 2. The composite polymer flow discharged from the discharge plate 3 is cooled and solidified according to the above-mentioned manufacturing method, and is then given an oil agent and taken up by a roller with a specified peripheral speed. After that, it is stretched by a heated roller to become the desired core-sheath composite fiber.

[0087] When the sheath component is removed from the core-sheath composite fiber of the present invention to produce a multifilament consisting of the core component, it is necessary to dissolve the sheath component to obtain a fiber consisting of the core component, and for this purpose, the sheath component may be removed by immersing the core-sheath composite fiber in a solvent capable of dissolving the easily soluble component. When the easily soluble component is a copolymerized polyethylene terephthalate or polylactic acid in which 5-sodium sulfoisophthalic acid or polyethylene glycol is copolymerized, an alkaline aqueous solution such as an aqueous sodium hydroxide solution can be used. In this case, it is preferable to heat the alkaline aqueous solution to 50°C or higher, since this can accelerate the progress of hydrolysis. In addition, if a fluid dyeing machine or the like is used, it is preferable from an industrial point of view, since a large amount can be treated at once. EXAMPLES

[0088] The core-sheath composite fiber and multifilament of the present invention will be specifically described below with reference to examples.

[0089] The following evaluations were carried out for the Examples and Comparative Examples.

[0090] A. Melt Viscosity of Polymer The chip-shaped polymer was dried in a vacuum dryer to a moisture content of 200 ppm or less, and the melt viscosity was measured by a Toyo Seiki Capillograph while changing the strain rate stepwise. The measurement temperature was the same as the spinning temperature, and the measurement was started 5 minutes after the sample was put into the heating furnace under a nitrogen atmosphere. The shear rate was 1216 s -1 The value was evaluated as the melt viscosity of the polymer.

[0091] B. Melting point of the polymer The chip-shaped polymer was dried in a vacuum dryer to a moisture content of 200 ppm or less, and about 5 mg was weighed out. Using a TA Instruments differential scanning calorimeter (DSC) Q2000, the temperature was raised from 0°C to 300°C at a rate of 16°C / min, and then the temperature was held at 300°C for 5 minutes to perform DSC measurement. The melting point was calculated from the melting peak observed during the temperature rise process. Measurements were performed three times for each sample, and the average value was taken as the melting point. When multiple melting peaks were observed, the melting point was taken as the melting point of the melting peak with the highest temperature.

[0092] C. Fineness The weight of 100 m of the multifilament was measured, and the weight was multiplied by 100. This operation was repeated 10 times, and the average value was rounded off to one decimal place to obtain the fineness (dtex) of the multifilament.

[0093] D. Sectional parameters (R B / R A ) The core-sheath composite fiber was embedded in an embedding agent such as epoxy resin, and the fiber cross section perpendicular to the fiber axis was photographed with a Hitachi scanning electron microscope (SEM) at a magnification such that 10 or more fibers could be observed. The obtained image was analyzed using computer software WinROOF manufactured by Mitani Shoji, and the circumscribed circle diameter R of the fiber was calculated. B (For example, the diameter of B in Figure 4(a)) and the inscribed circle diameter R of the fiber A (For example, the diameter of A in Figure 4(a)) R B / R A In the present invention, the measurement was carried out three times for each filament, and the simple number average of the results for 10 filaments was calculated and rounded off to the third decimal place to obtain R B / R A It was decided.

[0094] E. Cross-sectional parameters (Smin / D, Smax / Smin) The core-sheath composite fibers were embedded in an embedding agent such as epoxy resin, and images of the fiber cross sections perpendicular to the fiber axis were taken with a transmission electron microscope (TEM) at a magnification where 10 or more fibers could be observed. In this case, by applying metal staining, the dyeing difference between the polymers can be utilized to clarify the contrast of the joints of the composite components. For the images taken, the ratio of the minimum thickness Smin of the sheath component to the fiber diameter D, Smin / D, and the ratio of the maximum thickness Smax of the sheath component to the minimum thickness Smin of the sheath component, Smax / Smin, were calculated.

[0095] However, in the present invention, the diameter of fibers randomly sampled within each captured image was measured in μm units to the first decimal place, and this operation was performed for 10 randomly sampled fibers to determine a simple number average of the results, which was rounded off to the first decimal place to determine the fiber diameter D (μm). Here, if the fiber cross section perpendicular to the fiber axis was not a perfect circle, its area was measured and the value calculated in terms of a circle was used.

[0096] 2(a) and 5(a), for example, a straight line is drawn from the center of gravity G1 of the core component 1 present on the cross section of a fiber randomly selected from each captured image to the surface of any fiber, and the distance S1-F between the intersection S1 of the periphery of the core component 1 and the line and the intersection F of the fiber surface and the line is measured to one decimal place, and the minimum value of the obtained values ​​is calculated. This operation is performed on 10 randomly selected fibers, and the simple number average of the results is calculated, and the value rounded off to one decimal place is defined as the minimum thickness Smin (μm) of the sheath component. Here, for example, as shown in Figures 4(a) and 5(b), if there is a core component 2 different from the core component 1 whose center of gravity is taken on a line drawn from the center of gravity G1 of core component 1 toward any fiber surface, the value measured for the distance S1-S2 between the intersection S1 of the outer periphery of core component 1 and the line and the intersection S2 of the outer periphery of core component 2 and the line that is closest to S1 was used.

[0097] The ratio (Smin / D) of the fiber diameter D and the minimum thickness of the sheath component Smin thus determined was simply averaged, and the value was rounded off to two decimal places to obtain Smin / D.

[0098] 2(a) and 5(a), for example, a straight line is drawn from the center of gravity G1 of the core component 1 present on the cross section of a fiber randomly selected from each captured image toward the surface of any fiber, and the distance S1-F between the intersection S1 of the periphery of the core component 1 and the line and the intersection F of the fiber surface and the line is measured to one decimal place, and the maximum value among the obtained values ​​is calculated. This operation is performed on 10 randomly selected fibers, and the simple number average of the results is calculated, and the value rounded off to the nearest decimal place is defined as the minimum thickness Smax (μm) of the sheath component. Here, for example, as shown in Figures 4(a) and 5(b), if there is a core component 2 different from the core component 1 whose center of gravity is taken on a line drawn from the center of gravity G1 of core component 1 toward any fiber surface, the value measured for the distance S1-S2 between the intersection S1 between the outer periphery of core component 1 and the line and the intersection S2 between the outer periphery of core component 2 and the line that is closest to S1 was used.

[0099] The maximum thickness of the sheath component, Smax, and the minimum thickness of the sheath component, Smin, were calculated, and the simple number average of the ratio (Smax / Smin) was calculated, and the value rounded to the second decimal place was used as Smax / Smin.

[0100] F. Sectional parameters (GN / GM) In the case of the sheath-core composite fiber observed in section E, when the core component of the multi-lobal shape has grooves at the tips of the protrusions toward the center of gravity of the core component, the ratio GN / GM, which is the distance from the center of gravity G of the core component to the groove bottom M, GM, and the distance from the center of gravity G of the core component to the tips N of the protrusions, GN, was calculated. In this case, when the core component does not have grooves at the tips of the protrusions, GN / GM=1.0.

[0101] In the present invention, the distance GM from the center of gravity G of the core component to the groove bottom M is calculated by, for example, calculating the distance between the center of gravity G1 of the core component, which is the intersection of two arbitrary straight lines that halve the area of ​​the core component, and the groove bottom M1, which is the point on the groove surface closest to the center of gravity G1 of the core component, as shown in Figure 5(a). If there are two or more core components, the largest value among the values ​​calculated for each core component was used. This operation was performed on 10 randomly selected fibers, and the simple number average of the results was calculated and rounded off to the first decimal place to determine the distance GM (μm) from the center of gravity G of the core component to the groove bottom M.

[0102] In the present invention, the distance from the center of gravity G of the core component to the tip N of the protrusion, GN, is calculated as the distance between the center of gravity G1 of the core component and the tip N1 of the protrusion, which is the point on the groove surface farthest from the center of gravity G1 of the core component, for example, as shown in Figure 5(a). If there are two or more core components, the largest value among the values ​​calculated for each core component is used. This operation was performed on 10 randomly selected fibers, and the simple number average of the results was calculated and rounded off to the first decimal place to determine the distance from the center of gravity G of the core component to the tip N of the protrusion, GN (μm).

[0103] The ratio (GN / GM), which is the distance from the center of gravity G of the core component to the bottom of the groove M (GM) and the distance from the center of gravity G of the core component to the tip of the convex portion N (GN), was calculated as a simple number average and rounded off to three decimal places to obtain GN / GM.

[0104] G. Mixed state of fibers in multifilament In a fabric made of multifilament, an image of the cross section of the fabric perpendicular to the length direction of the fabric and perpendicular to the fiber axis direction of the multifilament is taken with a scanning electron microscope (SEM) manufactured by Hitachi at a magnification where 10 or more fibers can be observed. The taken image is analyzed using computer software WinROOF manufactured by Mitani Shoji, and the number of fibers Y composed of a polymer different from fiber X present among all fibers in a state where no other fibers exist on a line connecting the center of gravity of fiber X and the center of gravity of the arbitrary fiber in the multifilament as shown in Figure 8 (a) is evaluated. This evaluation is performed on 10 fibers randomly extracted from one multifilament, and the simple number average of the results is calculated, and the mixed state is judged in two stages based on the following criteria from the value rounded off to the first decimal place.

[0105] A: Uniformly mixed (one or more fibers Y made of a different polymer than fiber X) C: Unevenly mixed (less than one fiber Y made of a different polymer than fiber X).

[0106] H.Number of crimped peaks (mountains / cm) In a fabric made of multifilament, the multifilament was pulled out from the fabric without plastic deformation, one end of the multifilament was fixed, and a load of 1 mg / dtex was applied to the other end for 30 seconds or more, and then markings were applied at any point where the distance between two points was 1 cm in the fiber axis direction of the multifilament. Then, the fibers were separated from the multifilament without plastic deformation, and the distance between the markings that had been applied in advance was adjusted to the original 1 cm, and the sample was fixed on a slide glass, and an image was taken with a Keyence VHX-2000 digital microscope at a magnification where a 1 cm marking could be observed. The number of crimped peaks between the markings was calculated in the captured image. This operation was performed on 10 fibers composed of the same polymer, and a simple number average was calculated, and the value rounded off to the first decimal place was taken as the number of crimped peaks (peaks / cm). If fibers made of different polymers were mixed, the number of crimp peaks was determined for each fiber made of each polymer, and the number of crimp peaks of the fiber made of the polymer with the largest number of crimp peaks was adopted.

[0107] I. Thread length difference In a fabric made of multifilament, the multifilament was pulled out from the fabric without plastic deformation, one end of the multifilament was fixed, and a load of 1 mg / dtex was applied to the other end for 30 seconds or more. After that, markings were applied at any point where the distance between two points was 1 cm in the fiber axis direction of the multifilament. Then, the fibers were separated from the multifilament without plastic deformation, and the distance between the pre-applied markings was adjusted to the original 1 cm and fixed on a slide glass. An image of this sample was taken with a Keyence VHX-2000 digital microscope at a magnification where a 1 cm marking could be observed. The obtained image was analyzed using computer software WinROOF manufactured by Mitani Shoji to measure the actual fiber length between the markings. This operation was performed on 10 fibers each made of different polymers, and the results were simply averaged. From the results, (maximum actual fiber length - minimum actual fiber length) / (minimum actual fiber length) x 100 was calculated, and the value rounded off to the first decimal place was used as the yarn length difference (%).

[0108] J. Interfiber gap distance In a fabric made of multifilaments, a cross section of the fabric perpendicular to the length direction of the fabric and perpendicular to the fiber axis direction of the multifilaments is photographed with a scanning electron microscope (SEM) manufactured by HITACHI at a magnification where 10 or more fibers can be observed. The photographed image is analyzed using computer software, WinROOF manufactured by Mitani Shoji, to draw a perfect circle in which 10 fibers fit, as shown in FIG. 8(b), and one fiber is selected from the 10 fibers present inside the perfect circle, and the intersection points between the line connecting the center of gravity of the fiber and the adjacent fiber and each fiber surface are obtained, and the distance between the intersection points is measured in μm units to the first decimal place. The obtained value is rounded off to the first decimal place to determine the interfiber gap distance (μm). "Adjacent" here means that no other fiber is present on the line connecting the centers of gravity of any two fibers. This operation was performed on all adjacent fibers in the 10 fibers inside the perfect circle as shown in Figure 8(b), and the simple number average of the results was calculated and rounded off to the first decimal place to obtain the average inter-fiber gap distance (μm). The percentage of inter-fiber gap distances less than 5 μm was also calculated.

[0109] K. Porosity In a fabric made of multifilament, a cross section of the fabric perpendicular to the length direction of the fabric and perpendicular to the fiber axis direction of the multifilament is photographed with a Hitachi scanning electron microscope (SEM) at a magnification where 10 or more fibers can be observed. The photographed image is analyzed using computer software, WinROOF, manufactured by Mitani Shoji, to draw a perfect circle that fits 10 fibers as shown in Figure 8(b), and the total cross-sectional area of ​​the 10 fibers present inside the perfect circle is subtracted from the cross-sectional area of ​​the perfect circle to calculate the value. In this case, if 1 / 2 or more of the fiber is contained inside the perfect circle, it is counted as one fiber, and the cross-sectional area is expressed in μm 2 The measurement was made to the first decimal place. The obtained value was then divided by the cross-sectional area of ​​the perfect circle to calculate the porosity (%), which was then multiplied by 100 and rounded off to the nearest tenth.

[0110] L. Fiber diameter of irregular cross-section fiber Using the image taken in section K, the diameter of fibers randomly sampled within the same image was measured in μm units to the first decimal place, and this operation was performed for 10 randomly sampled fibers. The largest fiber diameter among the results was rounded off to the first decimal place and recorded as the fiber diameter D (μm). If the fiber cross section perpendicular to the fiber axis was not a perfect circle, its area was measured and the value calculated in terms of a circle was used.

[0111] M. Sectional parameters (R D / R C ) The images taken in K. were analyzed using computer software, WinROOF (Mitsutani Shoji Co., Ltd.), to determine the circumscribed circle diameter R D (For example, the diameter of C in FIG. 9(a)) and the inscribed circle diameter R of the fiber C (For example, the diameter of C in Figure 9(a)) R D / R C In the present invention, the measurement was carried out three times for each filament, and the simple number average of the results for 10 filaments was calculated and rounded off to the second decimal place to obtain R D / R C It was decided.

[0112] N. Sectional parameter (MN / D) When the fiber observed in section K had a groove at the tip of the protrusion, the ratio of the distance from the groove bottom M to the tip N of the protrusion, MN, to the fiber diameter D, MN / D, was calculated. When the fiber did not have a groove at the tip of the protrusion, MN / D=0 was used.

[0113] The ratio (MN / D) of the distance from the groove bottom M to the convex tip N, MN, and the fiber diameter D, referred to in the present invention, is determined by embedding the multifilament in an embedding agent such as epoxy resin, and taking an image of the fiber cross section perpendicular to the fiber axis with a scanning electron microscope (SEM) manufactured by Hitachi at a magnification such that 10 or more fibers can be observed. Fibers randomly extracted from the captured image were analyzed using computer software, WinROOF manufactured by Mitani Shoji, to calculate the distance MN between the groove bottom M, which is the closest point to the groove surface, and the convex tip N, which is the furthest point, from the center of gravity G, which is the intersection of any two straight lines that halve the cross-sectional area of ​​the fiber cross section, as shown in Figure 9(b), for example.

[0114] The fiber diameter D was measured in μm units to the first decimal place. If the fiber cross section perpendicular to the fiber axis was not a perfect circle, its area was measured and the value calculated as a circle was used as the fiber diameter D.

[0115] The ratio (MN / D) of the distance MN from the bottom of the groove M to the tip of the convex portion N and the fiber diameter D was calculated to four decimal places, and this operation was performed on 10 randomly selected fibers to calculate the simple number average of the results. The value was rounded off to three decimal places to obtain MN / D.

[0116] O. Texture evaluation (gloss, lightness, flexibility, resilience, dryness) Eight pieces of satin fabric were made by adjusting the number of fibers so that the warp cover factor (CFA) was 800 and the weft cover factor (CFB) was 1200. Note that the CFA and CFB mentioned here are the warp density and weft density of the fabric measured in a 2.54 cm section in accordance with JIS-L-1096:2010 8.6.1, and CFA = warp density x (warp fineness). 1 / 2 , CFB = weft density x (weft fineness) 1 / 2 The five textures of the resulting woven fabrics, luster, lightness, flexibility, resilience, and dryness, were evaluated using the following methods.

[0117] The glossiness was measured by using an automatic variable angle photometer (GONIOPHOTOMETER GP-200 type) manufactured by Murakami Color Research Laboratory to shine light on each sample at an incident angle of 60°, and measuring the light intensity at reception angles of 0° to 90° in 0.1° increments using two-dimensional reflected light distribution measurement. The maximum light intensity (specular reflection) near a reception angle of 60° was divided by the minimum light intensity (diffuse reflection) near a reception angle of 0° to calculate the value. This operation was performed three times per location, and a simple number average was calculated for a total of 10 locations, and the value was rounded off to one decimal place to determine the contrast glossiness. From the obtained contrast glossiness, the glossiness was judged into three levels based on the following criteria.

[0118] S: Excellent gloss (contrast gloss <1.6) A: Good gloss (1.6≦contrast gloss<1.9) C: Poor gloss (contrast gloss level 1.9 or less).

[0119] The lightness was measured by measuring the thickness (cm) of a 20 cm x 20 cm piece of fabric using a Terotec constant pressure thickness gauge (PG-14J), calculating the volume of the fabric, and then dividing the weight (g) of the fabric by the volume to obtain the apparent density (g / cm 3 From the apparent density obtained, the lightness was judged into three levels based on the following criteria.

[0120] S: Excellent lightness (apparent density ≦0.33) A: Good lightness (0.34<apparent density≦0.39) C: Less light (0.4<apparent density).

[0121] The flexibility was measured using a pure bending tester (KES-FB2) manufactured by Kato Tech, with a 20cm x 20cm fabric held at an effective sample length of 20cm x 1cm, and the maximum curvature in the weft direction was ±2.5cm. -1 When bent under the conditions of 0.5 cm curvature -1 and 1.5cm -1 The difference in bending moment per unit width (gf cm / cm) is calculated as the curvature difference of 1 cm. ―1 Divided by the value and curvature -0.5cm -1 and -1.5cm -1The difference in bending moment per unit width (gf cm / cm) is calculated as the curvature difference of 1 cm. ―1 This operation was performed three times for each location, and the simple number average of the results was calculated for a total of 10 locations. The value was rounded off to the fourth decimal place and then divided by 100 to obtain the bending hardness B x 10 -2 (gf cm 2 / cm). The bending hardness obtained was B x 10 -2 The flexibility was assessed on a three-level scale based on the following criteria.

[0122] S: Excellent flexibility (bending hardness B x 10 -2 ≦1.0) A: Good flexibility (1.0 < bending hardness B × 10 -2 ≦1.9) C: Poor flexibility (1.9 < bending hardness B × 10 -2 ).

[0123] The resilience was measured using a pure bending tester (KES-FB2) manufactured by Kato Tech. A 20cm x 20cm woven fabric was held with an effective sample length of 20cm x 1cm and bent in the weft direction with a curvature of ±1.0cm. -1 This operation was performed three times at each location, and a simple number average was calculated for a total of 10 locations. The average was rounded to the fourth decimal place and then divided by 100 to obtain the bending recovery 2HB x 10 -2 (gf cm / cm). The bending recovery obtained was 2HB × 10 -2 The feeling of repulsion was judged on a three-point scale based on the following criteria.

[0124] S: Excellent resilience (bending recovery 2HB x 10 -2 ≦1.0) A: Good resilience (1.0 < bending recovery 2HB x 10 -2 ≦1.9) C: Poor resilience (1.9<bending recovery 2HB×10 -2 ).

[0125] The dry feeling was evaluated by applying a load of 50g to a 1cm x 1cm terminal wound with piano wire and sliding it over a 10cm x 10cm area of ​​a 20cm x 20cm woven fabric at a speed of 1.0mm / sec to obtain the average coefficient of friction MIU. This action was carried out three times per location, for a total of 10 locations, and the simple number average of the results was calculated and rounded off to the nearest tenth to obtain the coefficient of friction. The dry feeling was evaluated from the obtained coefficient of friction in three stages based on the following criteria.

[0126] S: Excellent dry feeling (friction coefficient 0.7 or less) A: Good dry feeling (0.3≦friction coefficient<0.7) C: Poor dry feeling (friction coefficient < 0.3).

[0127] P. Chromogenicity The number of fibers was adjusted so that the cover factor (CFA) in the warp direction was 800 and the cover factor (CFB) in the weft direction was 1200, and eight pieces of satin fabric were produced. The fabric obtained was dyed black using disperse dye Sumikaron Black S-3B (10% owf). The L value of the dyed fabric was evaluated by reflectance measurement using a Konica Minolta CM-3700A. This operation was performed three times per location, and the simple number average of the results was calculated for a total of 10 locations, and the value rounded off to the first decimal place was used as the black dyeing L value. The color development was evaluated in three stages based on the following criteria from the obtained black dyeing L value.

[0128] S: Excellent color development (black dyeing L value < 15) A: Good color development (15≦black dyeing L value<18) C: Poor color development (black staining L value ≦18).

[0129] Q. Abrasion resistance The number of fibers was adjusted so that the cover factor (CFA) in the warp direction was 1100 and the cover factor (CFB) in the weft direction was 1100, and a plain weave fabric was prepared. The obtained fabric was dyed black using the disperse dye Sumikaron Black S-3B (10% owf). The dyed fabric was cut into a circle with a diameter of 10 cm, moistened with distilled water, and attached to a disk. The fabric was further cut into a 30 cm square and fixed on a horizontal plate while still dry. The disk with the fabric moistened with distilled water was horizontally brought into contact with the fabric fixed on the horizontal plate, and the disk was moved circularly for 10 minutes at a load of 420 g and a speed of 50 rpm so that the center of the disk drew a circle with a diameter of 10 cm, causing friction between the two pieces of fabric. After leaving it for 4 hours after the end of the friction, the degree of discoloration of the fabric attached to the disk was graded from 1 to 5 in 0.5 grade increments using a gray scale for discoloration. From the results of the evaluation, the abrasion resistance was evaluated into three levels based on the following criteria.

[0130] S: Excellent abrasion resistance (grade: 4 or higher) A: Good abrasion resistance (grade: 3 or 3-4) C: Poor abrasion resistance (grade: less than grade 3).

[0131] [Example 1] Polymer 1 was prepared as polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233 °C), and polymer 2 was prepared as polyethylene terephthalate (PET, melt viscosity: 130 Pa s, 254 °C).

[0132] After these polymers were melted separately at 290°C, polymer 1 / polymer 2 were weighed out to a weight ratio of 30 / 70 and fed into a spin pack incorporating the composite spinneret shown in Figure 12, and the fed polymers were discharged from the discharge hole to form a composite structure in which the sheath component completely covers the core component having a groove at the tip of the convex part of the trilobal cross section, a true circular core-sheath composite fiber as shown in Figure 5(a). At this time, the sheath component was polymer 1 and the core component was polymer 2.

[0133] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-36 filaments.

[0134] The ratio of the minimum thickness to the fiber diameter of the obtained sheath component (Smin / D) was 0.03, and the ratio of the maximum thickness to the minimum thickness of the sheath component (Smax / Smin) was 16. In addition, the ratio (GN / GM) of the distance from the center of gravity G of the core component to the groove bottom M, GM, to the distance from the center of gravity G of the core component to the tip N of the convex portion, GN, was 1.42, confirming that it was a sheath-core composite fiber of the present invention.

[0135] The inscribed circle diameter R of the core-sheath composite fiber A and circumscribed circle diameter R B The ratio was 1.0, and when present as a multifilament, it was easy for the fibers to be closely packed, and therefore the interfiber voids obtained after dissolution into the sheath component could be made uniform without any unevenness.

[0136] The fabric woven from the obtained core-sheath composite fiber was treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, resulting in a fabric composed of multifilaments (fiber diameter 10 μm) consisting of the core component of the core-sheath composite fiber.

[0137] The fabric made of the multifilament has a void structure in which fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more exist uniformly between each fiber, like natural silk, due to the sheath component that completely covers the multi-leaf-shaped core component being eluted. This gives the fabric a good gloss (contrast gloss: 1.7) that is not dependent on the viewing angle, and a resilience (bending recovery 2HB: 0.6×10 -2 It has a dry feel (friction coefficient: 0.7) with a good lightness (apparent density: 0.40 g / cm 3 ) and flexibility (bending hardness B: 0.7×10 -2 gf cm 2 / cm), giving it a texture similar to that of natural silk.

[0138] In addition, when the woven fabric was dyed black, it exhibited excellent color development (black dyeing L value: 14) due to the uniform interfiber voids between the single fibers and the diffuse reflection of light at the grooves at the tips of the convex parts of the irregular cross-section fibers, and it was found to have good abrasion resistance (grade 3-4) without discoloration due to fibrillation at the grooves. The results are shown in Table 1-1.

[0139] [Examples 2 and 3] The same procedures as in Example 1 were repeated except that the weight ratio of polymer 1 / polymer 2 was changed to 20 / 80 (Example 2) and 10 / 90 (Example 3).

[0140] In Examples 2 and 3, the bending stiffness increased as the sheath component was reduced, and the woven fabric had a characteristic elastic feel while retaining a natural silk-like texture. In addition, the grooves at the tips of the protruding parts of the fibers in the multifilament became shallower, which resulted in excellent abrasion resistance. The results are shown in Table 1-1.

[0141] [Example 4] The same procedure as in Example 1 was repeated except that the composite structure of the core-sheath composite fiber was changed to that shown in FIG. 2(a).

[0142] In Example 4, the grooves at the tips of the protrusions of the fibers in the multifilament were eliminated, so that the diffuse reflection of light was reduced, the reflection intensity was increased, and the visibility of the gloss was improved. In addition, the abrasion resistance was also excellent. The results are shown in Table 1-1.

[0143] [Comparative Example 1] Polymer 1 was prepared as polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233 °C), and polymer 2 was prepared as polyethylene terephthalate (PET, melt viscosity: 130 Pa s, 254 °C).

[0144] After these polymers were melted separately at 290°C, polymer 1 / polymer 2 were weighed out to a weight ratio of 30 / 70 and fed into a spinning pack equipped with a composite spinneret as shown in Figure 12, and the fed polymers were discharged from the discharge hole to form a true circular core-sheath composite fiber as shown in Figure 3(a), with a simple composite structure in which a core component with a circular cross section is covered with a sheath component. At this time, the sheath component was polymer 1 and the core component was polymer 2.

[0145] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-36 filaments.

[0146] The fabric woven from the obtained core-sheath composite fiber was treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, resulting in a fabric composed of multifilaments (fiber diameter 10 μm) consisting of the core component of the core-sheath composite fiber.

[0147] Although the obtained woven fabric had large inter-fiber voids of 10 μm or more between each fiber in the multifilament, there were no fine inter-fiber voids of less than 5 μm, and the voids collapsed when the fabric was touched, so the fabric lacked lightness and resilience. In addition, since there were no convex or groove parts in the core component, the fabric also lacked a dry feel. The results are shown in Table 1-1.

[0148] [Comparative Example 2] The same procedure as in Comparative Example 1 was repeated except that the composite structure of the core-sheath composite fiber was changed to that shown in FIG. 3(b).

[0149] In Comparative Example 2, the core component had a trilobal cross section, which slightly improved the dry feel, but after the sheath component was dissolved out, there were no fine inter-fiber gaps of less than 5 μm between each fiber, and the product lacked lightness and resilience. The results are shown in Table 1-1.

[0150] [Comparative Example 3] Polymer 1 was prepared as polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233 °C), and polymer 2 was prepared as polyethylene terephthalate (PET, melt viscosity: 130 Pa s, 254 °C).

[0151] These polymers were melted separately at 290°C, and then weighed out so that the weight ratio of polymer 1 / polymer 2 was 5 / 95, and fed into a spinning pack incorporating a composite spinneret as shown in Figure 12. The fed polymers were discharged from the discharge holes so as to form a composite structure in which the easily soluble component was arranged tapering toward the inside of the fiber at the tip of the convex part of the trilobal, poorly soluble component as described in JP-A-57-5912, as shown in Figure 6(a). At this time, the easily soluble component was arranged as polymer 1, and the poorly soluble component was arranged as polymer 2.

[0152] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a composite fiber of 56 dtex-36 filaments.

[0153] The fabric woven from the obtained composite fiber was treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath components, resulting in a fabric composed of multifilaments (fiber diameter 12 μm) made of the difficult-to-dissolve components of the composite fiber.

[0154] In Comparative Example 3, the tip of the protruding portion of the trilobal modified cross section fiber had a deep groove tapering toward the inside of the fiber, which increased the friction coefficient and provided an excellent dry feel, but poor abrasion resistance. In addition, after the sheath component was dissolved, there were no large interfiber gaps of 10 μm or more between each fiber, resulting in a shiny luster that lacked a luxurious feel, and also lacking in lightness, flexibility, and resilience. The results are shown in Table 1-2.

[0155] [Examples 5 and 6] The same procedures as in Example 4 were carried out except that the extrusion rate was changed so that the fiber diameter of the modified cross section fiber consisting only of the core component of the core-sheath composite fiber was 14 μm (Example 5) or 17 μm (Example 6).

[0156] In Examples 5 and 6, by increasing the fiber diameter, the unevenness due to the trilobal cross section of the fiber in the multifilament obtained after sheath elution was emphasized, and the reflection intensity was further increased, and the visibility of the gloss of the obtained woven fabric was further increased. In addition, since the bending stiffness was increased, a characteristic elastic touch was obtained while retaining the natural silk-like texture. The results are shown in Table 1-2.

[0157] [Example 7] The same procedure as in Example 4 was repeated except that the composite structure of the core-sheath composite fiber was changed to that shown in FIG. 2(b).

[0158] In Example 7, the fiber cross section of the multifilament fiber changed from a trilobal cross section to a tetralobal cross section, which increased the diffuse reflection of light at the convex parts, and not only brought about a more luxurious luster, but also improved friction and a drier texture. The results are shown in Table 1-2.

[0159] [Comparative Example 4] Polymer 1 was prepared as polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233 °C), and polymer 2 was prepared as polyethylene terephthalate (PET, melt viscosity: 130 Pa s, 254 °C).

[0160] After these polymers were melted separately at 290°C, polymer 1 / polymer 2 were weighed out to a weight ratio of 20 / 80 and fed into a spinning pack incorporating a composite spinneret as shown in Figure 12, and the fed polymers were discharged from the discharge hole so as to form a composite structure in which the easily soluble component divides the poorly soluble component into multiple pieces as described in JP-A-2010-222771 as shown in Figure 3(c). At this time, the easily soluble component was polymer 1 and the poorly soluble component was polymer 2.

[0161] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a composite fiber of 56 dtex-18 filaments.

[0162] The fabric woven from the obtained composite fiber was treated in a 1 wt % aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath components, resulting in a fabric composed of multifilaments (fiber diameter 6 μm) made of the difficult-to-dissolve components of the composite fiber.

[0163] In Comparative Example 4, since the fibers in the multifilament have a fine fiber diameter, the luster and flexibility are excellent, but the fine inter-fiber gaps of less than 5 μm and the coarse inter-fiber gaps of 10 μm or more are not uniformly present between each fiber, and the fiber lacks lightness and resilience. In addition, since the fiber diameter is fine, it is difficult to dye with a dye, and the color development is also lacking. The results are shown in Table 1-2.

[0164] [Example 8] Polymer 1 was polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233°C). Polymer 2 was polyethylene terephthalate copolymerized with 7 mol% isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa s, melting point: 232°C). Polymer 3 was polyethylene terephthalate (PET, melt viscosity: 130 Pa s, melting point: 254°C).

[0165] These polymers were melted separately at 290°C, and then weighed out to give a weight ratio of polymer 1 / polymer 2 / polymer 3 of 30 / 35 / 35, and fed into a spin pack incorporating the composite spinneret shown in Figure 12. The fed polymers were discharged from the discharge hole to produce an elliptical core-sheath composite fiber as shown in Figure 5(b), in which the core component is completely coated with the sheath component, the core component is divided into two by the sheath component, and the divided core components 1 and 2 each have a groove at the tip of the convex part of the trilobal cross section. At this time, the sheath component was arranged to be polymer 1, core component 1 was polymer 2, and core component 2 was polymer 3.

[0166] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-18 filaments.

[0167] The ratio (Smin / D) of the minimum thickness to the fiber diameter of the obtained sheath component was 0.03, and the ratio (Smax / Smin) of the maximum thickness to the minimum thickness of the sheath component was 12. In addition, the ratio (GN / GM) of the distance from the center of gravity G of the core component to the groove bottom M, GM, to the distance from the center of gravity G of the core component to the tip N of the convex portion, GN, was 1.38, confirming that it was a sheath-core composite fiber of the present invention.

[0168] The inscribed circle diameter R of the core-sheath composite fiber A and circumscribed circle diameter R B The ratio was 1.8, and when present as a multifilament, it was easy for the fibers to be closely packed, so that the interfiber voids obtained after dissolution into the sheath component could be made uniform without any unevenness.

[0169] The fabric woven from the obtained core-sheath composite fiber was treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, and then heat-treated with wet heat at 130°C to obtain a fabric composed of multifilaments (fiber diameter 10 μm) consisting of the core component of the core-sheath composite fiber.

[0170] The fabric composed of the multifilament had a void structure in which fine interfiber voids of less than 5 μm and coarse interfiber voids of 10 μm or more were uniformly present between each fiber, like natural silk, due to the elution of the sheath component that completely covered the multi-leaf-shaped core component. Furthermore, since core component 1 and core component 2 have different shrinkage differences, a difference in thread length was generated by heat treatment after the elution of the sheath component, and the interfiber voids of 10 μm or more became coarse compared to Example 1, resulting in a void structure more similar to the interfiber voids of natural silk. Furthermore, the texture of the fabric had a luxurious luster that was not dependent on the viewing angle (relative gloss: 1.4) as well as excellent resilience (bending recovery 2HB: 0.8×10 -2 It has a dry feel (friction coefficient: 0.8) with a smooth surface (apparent density: 0.32 g / cm 3 ) and excellent flexibility (bending hardness B: 0.9×10 -2 gf cm 2 / cm), and the fabric had a texture almost like natural silk.

[0171] Furthermore, when the fabric was dyed black, the diffuse reflection of light was further enhanced, and excellent color development (black dyeing L value: 13) was demonstrated, and it was found that the fabric also had good abrasion resistance (grade 3-4) without discoloration due to fibrillation in the grooves. The results are shown in Table 2-1.

[0172] [Examples 9 and 10] The same procedures as in Example 8 were repeated except that polymer 2 was changed to polypropylene terephthalate (PPT) (Example 9) or polyethylene terephthalate (PET) (Example 10).

[0173] In Example 9, the rubber elasticity of PPT was combined to produce a fabric with a more flexible feel, and it also had a unique stretch function that natural silk does not have. In addition, since PPT has a lower refractive index than PET, the fabric obtained had excellent color development.

[0174] In Example 10, although there was no difference in the yarn length, the texture similar to that of natural silk was fully expressed, and since the core component was divided into two, fine interfiber voids of less than 5 μm and coarse interfiber voids of 10 μm or more were more uniformly present than in Example 1, and the texture of the obtained woven fabric was improved in terms of lightness, flexibility, and resilience. The results are shown in Table 2-1.

[0175] [Example 11] The same procedure as in Example 8 was repeated except that the composite structure of the core-sheath composite fiber was changed to that shown in FIG. 4(a).

[0176] In Example 11, the grooves at the tips of the protrusions of the modified cross section fiber were eliminated, so that the diffuse reflection of light was reduced, the reflection intensity was increased, and the visibility of the gloss was improved. In addition, the abrasion resistance was also excellent. The results are shown in Table 2-1.

[0177] [Examples 12 and 13] The composite structure of the core-sheath composite fiber is shown in FIG. 4(a), and the procedure of Example 8 was repeated except that the weight ratio of polymer 2 / polymer 3 was changed to 50 / 20 (Example 12) and 20 / 50 (Example 13).

[0178] In Examples 12 and 13, the higher the ratio of the high shrinkage component, polymer 2, the stronger the difference in yarn length and the lighter the resulting woven fabric became, and the higher the ratio of the low shrinkage component, polymer 3, the less diffuse reflection of light, the higher the reflection intensity and the more visible the gloss became. Not only did the high shrinkage rate of the high shrinkage component during wet heat treatment cause clogging, but the fabric also had excellent flexibility and resilience. The results are shown in Tables 2-1 and 2-2.

[0179] [Example 14] The composite structure of the core-sheath composite fiber is shown in Figure 4(a). B / R A The same procedures as in Example 8 were repeated except that 1.0 was changed to 3.0.

[0180] The greater the degree of irregularity of the core-sheath composite fiber, the greater the degree of irregularity of the core component. Therefore, the unevenness due to the trilobal cross section of the fiber in the multifilament obtained after sheath leaching was emphasized, further increasing the reflection intensity, and further increasing the visibility of the luster of the obtained woven fabric. The results are shown in Table 2-2. [Example 15] The composite structure of the core-sheath composite fiber is shown in Fig. 4(b). B / R A The procedure of Example 8 was repeated except that the following change was made:

[0181] The smaller the irregularity of the core-sheath composite fiber, the more easily it can be closely packed when present as a multifilament, and therefore the interfiber voids obtained after dissolving into the sheath component can be made uniform without unevenness, improving the quality of the resulting woven fabric. The results are shown in Table 2-2. [Example 16] The composite structure of the core-sheath composite fiber is shown in Fig. 4(c). B / R A The procedure of Example 8 was repeated except that the following change was made:

[0182] In Example 16, the core component was divided into six pieces by the sheath component, and the fiber diameter of the modified cross section fiber obtained after removing the sheath component became thinner, so that a woven fabric was obtained that not only had a milder and more luxurious luster, but also had excellent flexibility and texture. The results are shown in Table 2-2.

[0183] [Comparative Example 5] Polymer 1 was polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233°C). Polymer 2 was polyethylene terephthalate copolymerized with 7 mol% isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa s, melting point: 232°C). Polymer 3 was polyethylene terephthalate (PET, melt viscosity: 130 Pa s, melting point: 254°C).

[0184] After melting these polymers separately at 290°C, polymer 1 / polymer 2 / polymer 3 were weighed out to a weight ratio of 5 / 42.5 / 42.5 and fed into a spinning pack incorporating the composite spinneret shown in Figure 12, and the fed polymers were discharged from the discharge hole so that the difficult-to-dissolve component was composed of two types of polymers, a high shrinkage component and a low shrinkage component, in a composite structure in which the easily soluble component was arranged tapered toward the inside of the fiber at the tip of the convex part of the trilobal shaped difficult-to-dissolve component described in JP-A-2-145825, as shown in Figure 6(b). At this time, the easily soluble component was polymer 1, the high shrinkage component of the difficult-to-dissolve component was polymer 2, and the low shrinkage component was polymer 3.

[0185] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, and the stream was wound up at a spinning speed of 1500 m / min. The stream was then stretched between rollers heated to 90°C and 130°C to produce composite fibers of 56 dtex-36 filaments (high shrinkage: 28 dtex-18 filaments, low shrinkage: 28 dtex-18 filaments).

[0186] The fabric woven from the obtained composite fiber was treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath components, and then heat-treated with wet heat at 130°C to obtain a fabric composed of multifilaments (fiber diameter 12 μm) made of the difficult-to-dissolve components of the composite fiber.

[0187] In Comparative Example 5, the tip of the protruding portion of the trilobal modified cross section fiber had a deep groove tapering toward the inside of the fiber, which increased the friction coefficient and provided an excellent dry feel, but poor abrasion resistance. In addition, although lightness was obtained due to the expression of the crimp form caused by the difference in thermal shrinkage between the high shrinkage component and the low shrinkage component, fine inter-fiber voids of less than 5 μm and coarse inter-fiber voids of 10 μm or more were not uniformly present between each fiber, and clogging also occurred due to the high shrinkage rate of the high shrinkage component, resulting in a lack of flexibility and resilience. The results are shown in Table 2-2.

[0188] [Example 17] The following polymers were prepared: polymer 1 was polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233°C); polymer 2 was polyethylene terephthalate copolymerized with 7 mol% isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa s, melting point: 232°C); and polymer 3 was polyethylene terephthalate (PET, melt viscosity: 130 Pa s, melting point: 254°C).

[0189] These polymers were melted separately at 290°C, and then weighed out to give a weight ratio of polymer 1 / polymer 2 / polymer 3 of 30 / 35 / 35, and fed into a spin pack incorporating the composite spinneret shown in Figure 12. The fed polymers were discharged from the discharge hole to produce a core-sheath composite fiber as shown in Figure 10(b), in which the core is completely coated with the sheath, the core is divided into two by the sheath, and the divided core 1 and core 2 each have a groove at the tip of the convex part of the trilobal cross section. At this time, the sheath was polymer 1, core 1 was polymer 2, and core 2 was polymer 3.

[0190] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, the stream was wound up at a spinning speed of 1500 m / min, and stretched between rollers heated to 90°C and 130°C to produce a core-sheath composite fiber of 56 dtex-18 filaments.

[0191] The ratio (Smin / D) of the minimum thickness to the fiber diameter of the obtained sheath component was 0.03, and the ratio (Smax / Smin) of the maximum thickness to the minimum thickness of the sheath component was 12. In addition, the ratio (GN / GM) of the distance from the center of gravity G of the core component to the groove bottom M, GM, to the distance from the center of gravity G of the core component to the tip N of the convex portion, GN, was 1.38, confirming that it was a sheath-core composite fiber of the present invention.

[0192] The inscribed circle diameter R of the core-sheath composite fiber A and circumscribed circle diameter R BThe ratio was 1.8, and when present as a multifilament, it was easy for the fibers to be closely packed, so that the interfiber voids obtained after dissolution into the sheath component could be made uniform without any unevenness.

[0193] The fabric woven from the obtained core-sheath composite fiber was subjected to a wet heat treatment at 130°C, and then treated in a 1% by weight aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, resulting in a multifilament fabric in which crimpable fibers made of different polymers were uniformly mixed. The obtained crimpable fiber had a composite structure (irregularity: 1.6) with grooves (MN / D: 0.13) at the tips of the convex parts of the trilobal cross section, a fiber diameter of 10 μm, the number of crimped peaks was 14 peaks / cm, and the yarn length difference of the crimpable fibers made of polymers with different melting points was 7%.

[0194] In the multifilament woven fabric, not only were large interfiber voids of 10 μm or more formed between each fiber due to the excluded volume effect between fibers caused by the difference in thermal shrinkage between polymers with different melting points, but interfiber voids of less than 5 μm were formed between adjacent crimped fibers made of polymers with different melting points, and the multifilament had a void structure very similar to that of natural silk, in which fine interfiber voids of less than 5 μm and large interfiber voids of 10 μm or more were more uniformly mixed. When the void structure was evaluated, the average interfiber void distance was 10.5 μm, the proportion of interfiber void distances less than 5 μm was 25%, and the void ratio was 65%.

[0195] The fabric also has a luxurious luster (contrast gloss: 1.4) that is not dependent on viewing angle, and is very light (apparent density: 0.32 g / cm 3 ) and has a dry feel (friction coefficient: 0.8), while the inter-fiber gap distance is more stably formed to be less than 5 μm than in Example 8, resulting in a resilient feel (bending recovery 2HB: 0.7×10 -2 gf cm / cm) and flexibility (flexural hardness B: 0.8×10 -2 gf cm 2 / cm) and had a texture almost like natural silk.

[0196] Furthermore, when the woven fabric was dyed black, the diffuse reflection of light was emphasized by the coarse interfiber gaps of 10 μm or more that existed uniformly between the fibers, resulting in excellent color development (black dyeing L value: 13), and it was found that the fabric also had good abrasion resistance (grade 3-4) with no discoloration due to fibrillation in the grooves. The results are shown in Table 3.

[0197] [Examples 18 and 19] The same operations as in Example 17 were carried out except that the weight ratio of polymer 1 / polymer 2 / polymer 3 was changed to 20 / 40 / 40 (Example 18) and 10 / 45 / 45 (Example 19).

[0198] In Examples 18 and 19, the smaller the sheath component, the higher the ratio of inter-fiber gaps of less than 5 μm in the multifilament, and the greater the bending stiffness, resulting in a woven fabric with a characteristic elastic feel while retaining a natural silk-like texture. In addition, the shallower grooves at the tips of the convex parts of the crimped fibers provided excellent abrasion resistance. The results are shown in Table 3.

[0199] [Example 20] The same operations as in Example 17 were repeated except that polymer 2 was changed to polypropylene terephthalate (PPT, melt viscosity: 150 Pa·s, melting point: 233° C.).

[0200] In Example 20, the rubber elasticity of PPT was combined to produce a fabric with a more flexible feel, and it also had a unique stretch function that natural silk does not have. In addition, since PPT has a lower refractive index than PET, the fabric obtained also had excellent color development. The results are shown in Table 3.

[0201] [Example 21] The same procedures as in Example 17 were repeated except that polymer 2 was changed to polyethylene terephthalate having a high melt viscosity (high viscosity PET, melt viscosity: 250 Pa·s, melting point: 254° C.).

[0202] In Example 5, by expressing the crimp due to the viscosity difference rather than the melting point difference between polymer 3 and polymer 2, the number of crimp peaks of the crimpable fibers constituting the multifilament was also reduced, so that the diffuse reflection of light due to the void structure of the multifilament was suppressed and the visibility of the gloss was increased. Furthermore, the expression of the crimp form in the wet heat treatment was reduced, so that the ratio of the inter-fiber void distance of less than 5 μm was also increased, and the resilience was also excellent. The results are shown in Table 3.

[0203] [Comparative Example 6] The following polymers were prepared: polymer 1 was polyethylene terephthalate copolymerized with 8 mol% 5-sodium sulfoisophthalic acid and 9 wt% polyethylene glycol (SSIA-PEG copolymerized PET, melt viscosity: 100 Pa s, melting point: 233°C); polymer 2 was polyethylene terephthalate copolymerized with 7 mol% isophthalic acid (IPA copolymerized PET, melt viscosity: 140 Pa s, melting point: 232°C); and polymer 3 was polyethylene terephthalate (PET, melt viscosity: 130 Pa s, melting point: 254°C).

[0204] These polymers were melted separately at 290°C, and then weighed out to give a weight ratio of polymer 1 / polymer 2 of 2.5 / 47.5 and a weight ratio of polymer 1 / polymer 3 of 2.5 / 47.5, and fed into a spinning pack incorporating a composite spinneret as shown in Fig. 12, and the fed polymers were discharged so that composite fibers consisting of two components, a high shrinkage component and an easy-to-dissolve component, and composite fibers consisting of two components, a low shrinkage component and an easy-to-dissolve component, were discharged from separate discharge holes, in a composite structure in which a readily soluble component is disposed tapered toward the inside of the fiber at the tip of the convex part of a trilobal hardly soluble component as described in JP-A-2-145825, as shown in Fig. 11. At this time, the readily soluble component was polymer 1, the high shrinkage component was polymer 2, and the low shrinkage component was polymer 3.

[0205] The extruded composite polymer stream was cooled and solidified, after which an oil agent was added, and the stream was wound up at a spinning speed of 1500 m / min. The stream was then stretched between rollers heated to 90°C and 130°C to produce composite fibers of 56 dtex-36 filaments (high shrinkage: 28 dtex-18 filaments, low shrinkage: 28 dtex-18 filaments).

[0206] The fabric woven from the obtained composite fiber was subjected to a heat treatment using wet heat at 130°C, and then treated in a 1 wt% aqueous sodium hydroxide solution (bath ratio 1:50) heated to 90°C to remove more than 99% of the sheath component, thereby obtaining a fabric composed of multifilaments (fiber diameter 12 μm) made of the difficult-to-dissolve components of the composite fiber.

[0207] In Comparative Example 6, the tip of the convex part of the trilobal modified cross section fiber had a deep groove tapering toward the inside of the fiber, which increased the friction coefficient and provided an excellent dry feel, but poor abrasion resistance. In addition, while the difference in yarn length between the high shrinkage component and the low shrinkage component provided lightness, the fibers made of different polymers were unevenly mixed due to the blended spinning method, and the proportion of inter-fiber gap distances less than 5 μm was low, resulting in a lack of resilience. The results are shown in Table 3.

[0208] [Example 22] The same procedure as in Example 17 was repeated except that the composite structure of the core-sheath composite fiber was changed to that shown in FIG. 10(a).

[0209] In Example 22, the grooves at the tips of the convex parts of the crimped fibers in the multifilament were eliminated, reducing the diffuse reflection of light, increasing the reflection intensity, and increasing the visibility of the gloss. In addition, the abrasion resistance was also excellent. The results are shown in Table 4.

[0210] [Examples 23 and 24] The same procedures as in Example 17 were repeated except that the weight ratio of polymer 2 / polymer 3 was changed to 50 / 20 (Example 23) and 20 / 50 (Example 24).

[0211] In Examples 23 and 24, the higher the ratio of polymer 2, which is a high shrinkage component, the more the number of crimp peaks and the difference in yarn length of the crimped fibers in the multifilament are expressed, the higher the average inter-fiber gap distance in the void structure of the multifilament, and the lighter the resulting woven fabric is. Also, the higher the ratio of polymer 3, which is a low shrinkage component, the smaller the number of crimp peaks of the crimped fibers in the multifilament is, so that the diffuse reflection of light due to the void structure of the multifilament is suppressed, and not only does the visibility of the gloss increase, but the smaller the expression of the crimp form in the wet heat treatment is, so that the ratio of inter-fiber gap distances of less than 5 μm is also increased, and the resilience is also excellent. The results are shown in Table 4.

[0212] [Examples 25 and 26] The same procedures as in Example 17 were repeated except that the extrusion rate was changed so that the fiber diameter of the crimped fibers in the multifilament was 14 μm (Example 25) or 17 μm (Example 26).

[0213] In Examples 25 and 26, the increased fiber diameter emphasized the unevenness caused by the trilobal cross section of the crimped fibers in the multifilament, increasing the reflection intensity and further increasing the visibility of the gloss of the resulting fabric. In addition, the increased bending stiffness gave the fabric a characteristic elastic feel while retaining the texture of natural silk. The results are shown in Table 4. [Industrial Applicability]

[0214] The multifilament of the present invention has two or more types of crimped fibers composed of different polymers uniformly mixed in the multifilament, and thus can form a unique void structure in which fine interfiber voids of less than 5 μm and coarse interfiber voids of 10 μm or more are uniformly mixed between each fiber in the multifilament, like natural silk. Therefore, the textile product made of the multifilament of the present invention can reproduce the various textures unique to natural silk, and can be used not only in Western and Japanese clothing in which natural silk has been mainly used in the past, but also in a wide range of textile products, such as general clothing such as jackets, skirts, pants, and underwear, sports clothing, clothing materials, interior products such as carpets, sofas, and curtains, vehicle interior products such as car seats, cosmetics, cosmetic masks, wiping cloths, and health products, due to their ease of handling unique to synthetic fibers.

[0215] [Table 1-1]

[0216] [Table 1-2]

[0217] [Table 2-1]

[0218] [Table 2-2]

[0219] [Table 3]

[0220] [Table 4] [Explanation of symbols]

[0221] a Fibroin, a component that is difficult to dissolve in raw natural silk b Sericin, a readily soluble component of raw natural silk c Difficultly eluted components d Easily eluted components A: A perfect circle (inscribed circle) inscribed at two or more points in the cross section of a composite fiber B. A perfect circle (circumscribed circle) that circumscribes the cross section of the composite fiber at two or more points C A perfect circle inscribed at two or more points in the fiber cross section (inscribed circle) D A perfect circle that circumscribes the fiber cross section at two or more points (circumscribed circle) F: The intersection point of a line drawn from the intersection point (center of gravity) of two lines that bisect the cross-sectional area of ​​the fiber toward the surface of any fiber and the fiber surface G The intersection point (center of gravity) of any two lines that bisect the area of ​​the fiber cross section M is the closest point to the intersection (center of gravity) of any two straight lines that bisect the cross-sectional area of ​​the fiber on the groove surface at the tip of the convex part. N is the farthest point from the intersection (center of gravity) of any two straight lines that bisect the cross-sectional area of ​​the fiber on the groove surface at the tip of the convex part. S: The intersection point of a line drawn from the intersection of two lines that bisect the cross-sectional area of ​​the fiber toward the surface of any fiber and the outer periphery of the core component X Any fiber in the multifilament Y is a fiber that is composed of a polymer different from X and that has no other fibers on the line connecting its center of gravity with the center of gravity of X in the multifilament. 1 Weighing plate 2 Distribution Plate 3 Discharge plate

Claims

1. A core-sheath composite fiber made of a polymer in which the sheath component has a greater dissolution rate in a solvent than the core component, the cross-section of the fiber being a perfect circle or ellipse, the sheath component completely covers the multi-lobed core component having three or more convex portions, and the ratio Smax / Smin of the maximum thickness Smax of the sheath component to the minimum thickness Smin of the sheath component is 5.0 or greater.

2. 2. The sheath-core composite fiber according to claim 1, wherein the multi-lobal core component has grooves at the tips of the convex portions in the direction of the center of gravity of the core component, and the ratio GN / GM of the distance GM from the center of gravity G of the core component to the groove bottom M and the distance GN from the center of gravity G of the core component to the tip N of the convex portion is 1.1 to 1.

5.

3. 3. The core-sheath composite fiber according to claim 1, wherein the core component is divided into two or more parts by the sheath component, and each divided core component has a multi-lobal shape.

4. 4. The core-sheath composite fiber according to claim 3, wherein adjacent core components in the core component divided by the sheath component are made of polymers having different melting points.

5. A multifilament comprising a core component of the sheath-core composite fiber according to any one of claims 1 to 4, the multifilament having a void structure in which the average inter-fiber void distance is 10 to 30 µm, and the proportion of inter-fiber void distances of less than 5 µm is 10 to 50%.

6. The multifilament according to claim 5, having a void structure with a void ratio of 30 to 80%.

7. 7. The multifilament according to claim 5 or 6, which is made of two or more kinds of crimpable fibers composed of polymers having different melting points, and the crimpable fibers are uniformly mixed.

8. The multifilament according to any one of claims 5 to 7, which is composed of multi-lobal fibers having three or more convex portions in a fiber cross section.

9. The multifilament according to any one of claims 5 to 8, which is composed of fibers having grooves at the tips of the convex portions in a fiber cross section, and a ratio (MN / D) of a distance MN from a groove bottom M to a convex portion tip N to a fiber diameter D is 0.04 to 0.

20.

10. A textile product comprising, in part, the sheath-core composite fiber or multifilament according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • JP1971041408B1

  • JP1973033415A

  • JP1974017639A

  • Modified cross-section yarn and its production

    JP1982005912A

  • Production of blended fiber yarn

    JP1984088974A