Hollow carbon fiber material loaded with trace ruthenium as well as preparation method and application of hollow carbon fiber material
Through the hollow carbon fiber material loaded with trace amounts of ruthenium, a hollow structure with high specific surface area is formed by coaxial electrospinning and water immersion technology, which solves the problem of lack of active sites of carbon nanofiber materials, significantly improves the electrocatalytic hydrogen evolution performance and reduces the Hydrogen production cost.
Patent Information
- Application Number
- CN202411115612.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing carbon nanofiber materials have small specific surface area and lack of active sites, which leads to insufficient catalytic activity and stability of the electrocatalyst, affecting the efficiency and cost of electrolytic hydrogen production technology.
The preparation method of hollow carbon fiber material loaded with trace amount of ruthenium is used to form a hollow structure through coaxial electrospinning technology and water immersion, combining cobalt and trace amount of ruthenium metal nanoparticles, significantly increasing the specific surface area and active sites of the material.
It significantly improves the electrocatalytic hydrogen evolution performance (HER), reduces the cost of hydrogen production, and maximizes the control of production costs.
Smart Images

Figure CN119020889A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation, and in particular to a hollow carbon fiber material loaded with trace ruthenium, and a preparation method and application thereof. Background Art
[0002] At present, due to the increasing depletion of fossil fuels and their huge side effects on the environment, the development of renewable energy and clean energy is of vital importance to alleviate the urgent energy crisis and environmental challenges. Hydrogen energy is regarded as the most promising clean energy, and the development of hydrogen energy has become a research hotspot in today's energy field. Through the coupling of water electrolysis hydrogen production technology with renewable energy power generation technology, the construction of a new energy system with new energy as the main body can be realized. The water electrolysis hydrogen production technology mainly produces hydrogen gas by the oxygen evolution reaction at the anode and the hydrogen evolution reaction at the cathode under the action of external electricity. However, the development of water electrolysis hydrogen production technology is still restricted by high costs. The application of catalysts can reduce the reaction barrier and thus reduce the cost of hydrogen production. Therefore, the research on catalysts is of great significance to the development of hydrogen production technology.
[0003] As the core material of electrochemical devices such as water electrolysis to produce hydrogen, fuel cells, etc., the catalytic activity, selectivity, stability and price of electrocatalysts are key factors affecting their widespread application. At present, electrocatalysts mainly include precious metals, transition metals and their compounds, metal oxides, etc., but these materials have poor conductivity and are easily oxidized and corroded, resulting in a reduction in active sites or even loss of activity, which reduces the life of the catalyst. Therefore, the development of non-precious metal electrocatalysts with high stability, high activity and low cost has become a research hotspot. Carbon-based materials are one of the most widely studied electrocatalysts. Among them, carbon nanofiber (CNF) materials have attracted widespread attention due to their relatively high specific surface area, good conductivity and thermal stability, and chemical inertness. However, existing carbon nanofibers still have problems such as small specific surface area and lack of active sites. Summary of the invention
[0004] In view of this, the present invention provides a hollow carbon fiber material loaded with trace ruthenium and a preparation method and application thereof. The carbon nanofiber material has a hollow structure and a specific surface area of up to 390 m 2 / g, and the active sites on the surface of the material are significantly increased, which greatly improves the electrocatalytic hydrogen evolution performance (HER) of the material.
[0005] In order to solve the above technical problems, the first aspect of the present invention provides a method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium, the steps comprising:
[0006] S1, dissolving polyacrylonitrile in N,N-dimethylformamide or dimethyl sulfoxide containing a cobalt source and a ruthenium source to obtain a shell spinning solution, and dissolving polyvinyl pyrrolidone in N,N-dimethylformamide or dimethyl sulfoxide to obtain a core spinning solution;
[0007] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor;
[0008] S3, soaking the carbon fiber precursor in water to obtain a hollow carbon fiber precursor;
[0009] S4. The hollow carbon fiber precursor is sequentially dried, pre-oxidized and carbonized at high temperature to obtain a hollow carbon fiber material loaded with a trace amount of ruthenium.
[0010] The specific process of the preparation method of the hollow carbon fiber material loaded with trace ruthenium provided by the present invention is as follows Figure 1 As shown, by selecting specific raw materials, utilizing coaxial electrospinning technology, and adopting water immersion to remove the core layer material polyvinyl pyrrolidone, it is more convenient and quick to obtain a carbon fiber material with a special hollow structure, which greatly increases the specific surface area of the carbon fiber material. In addition, by loading cobalt and trace ruthenium metal nanoparticles to increase the active sites on the surface of the carbon fiber material, the problem of small specific surface area and lack of active sites of the carbon fiber material is effectively solved, thereby maximizing the specific surface area of the material, exposing more active sites, providing a larger existence space for active substances, and significantly improving the HER catalytic activity.
[0011] In combination with the first aspect, the cobalt source is selected from cobalt nitrate hexahydrate or cobalt acetate tetrahydrate, preferably cobalt acetate tetrahydrate.
[0012] In combination with the first aspect, the ruthenium source is ruthenium trichloride hydrate.
[0013] In combination with the first aspect, the mass proportion of the ruthenium source in the shell spinning solution is 0.02% to 0.24%. The present invention only needs to combine a trace amount of ruthenium and cobalt to significantly improve the HER catalytic activity of the hollow carbon fiber material, significantly reducing the production cost.
[0014] In combination with the first aspect, the mass proportion of the cobalt source in the shell spinning solution is 1.2% to 3.6%.
[0015] The content of the cobalt source in the shell spinning solution defined in the present invention can improve the HER performance of the carbon fiber as much as possible while ensuring the integrity of the carbon fiber. Moreover, the present invention only needs to add a very small amount of ruthenium source to significantly improve the HER catalytic activity, thereby controlling the production cost to the maximum extent while improving the catalytic activity.
[0016] Preferably, the mass proportion of the ruthenium source in the shell spinning solution is 0.12%.
[0017] Preferably, the mass proportion of the cobalt source in the shell spinning solution is 2.4%.
[0018] In combination with the first aspect, the concentration of polyacrylonitrile in the shell spinning solution is 10wt% to 20wt%, and the concentration of polyvinyl pyrrolidone in the core spinning solution is 10wt% to 20wt%.
[0019] The components of the shell spinning solution and the core spinning solution specified in the present invention are immiscible with each other and have different solubility in water. Therefore, a carbon fiber material with a hollow structure loaded with trace amounts of ruthenium can be formed by limiting the amount of cobalt source in the shell spinning solution and soaking it in water after coaxial electrospinning.
[0020] Preferably, the concentration of polyacrylonitrile in the shell spinning solution is 15 wt %, and the concentration of polyvinyl pyrrolidone in the core spinning solution is 12 wt %.
[0021] In combination with the first aspect, the loading voltage of the coaxial electrospinning is 12kV~26kV, the distance from the needle to the receiving tube is 15cm~20cm, the flow rate ratio of the outer shell spinning solution to the inner core spinning solution is 1.2~3:1, and the total liquid supply rate is 4.8mL / h~12.0mL / h.
[0022] Preferably, the loading voltage of the coaxial electrospinning is 18 kV, the distance from the needle to the receiving tube is 16 cm, the flow rate ratio of the shell spinning solution to the core spinning solution is 2:1, and the total liquid supply rate is 8.0 mL / h.
[0023] In combination with the first aspect, the immersion is immersion in water at a temperature of 25°C to 80°C for 6h to 36h. The immersion conditions specified in the present invention can not only ensure that the polyvinyl pyrrolidone is fully dissolved to form a hollow structure, but also avoid the inherent structure of the carbon fiber being destroyed due to excessively high temperature or excessively long immersion time.
[0024] Preferably, the soaking is soaking in water at a temperature of 50° C. for 12 hours.
[0025] In combination with the first aspect, the drying is performed at a temperature of 60° C. to 100° C. for 5 h to 20 h, preferably at a temperature of 80° C. for 12 h.
[0026] In combination with the first aspect, the pre-oxidation is oxidation at a temperature of 220°C to 260°C for 1 hour to 4 hours, preferably oxidation at a temperature of 250°C for 1.5 hours.
[0027] In combination with the first aspect, the high temperature carbonization is carried out in an inert atmosphere or a nitrogen atmosphere, heating the temperature to 600°C to 800°C at a heating rate of 2°C / min to 6°C / min and maintaining it for 1h to 3h, preferably heating the temperature to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and maintaining it for 2h.
[0028] A second aspect of the present invention provides a hollow carbon fiber material loaded with trace amounts of ruthenium, which is prepared according to the above-mentioned method for preparing the hollow carbon fiber material loaded with trace amounts of ruthenium.
[0029] In combination with the second aspect, the hollow carbon fiber material has a hollow diameter of 350nm to 700nm, a wall thickness of 60nm to 120nm, and a specific surface area of 380m 2 / g~390m 2 / g.
[0030] For example, the hollow diameter of the hollow carbon fiber material can be 350nm-450nm, 400nm-500nm or 600nm-700nm, the wall thickness can be 60nm-70nm, 90nm-100nm, 80nm-110nm or 80nm-120nm, and the specific surface area can be 380m 2 / g, 384m 2 / g, 386m 2 / g or 390m 2 / g.
[0031] The third aspect of the present invention provides an application of the above-mentioned hollow carbon fiber material loaded with trace amounts of ruthenium in the field of electrocatalytic materials.
[0032] The hollow carbon fiber material loaded with trace amounts of ruthenium provided by the present invention has excellent morphology, considerable wall thickness, hollow diameter and specific surface area, and provides sufficient active sites, thereby being able to provide a carrier area for active substances to a greater extent. When used in the field of electrocatalytic materials, the HER catalytic activity of the catalyst can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of a method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium provided in an embodiment of the present invention;
[0034] Figure 2 is a SEM image of a hollow carbon fiber material loaded with trace amounts of ruthenium provided in Example 1 of the present invention;
[0035] Figure 3 This is a SEM image of a carbon fiber material loaded with a trace amount of ruthenium provided in Comparative Example 1 of the present invention;
[0036] Figure 4This is a HER performance diagram of a hollow carbon fiber material loaded with a trace amount of ruthenium provided in Example 1 of the present invention;
[0037] Figure 5 This is a HER performance diagram of a hollow carbon fiber material loaded with a trace amount of ruthenium provided in Example 2 of the present invention;
[0038] Figure 6 This is a HER performance diagram of a hollow carbon fiber material loaded with a trace amount of ruthenium provided in Example 3 of the present invention;
[0039] Figure 7 This is a HER performance diagram of a hollow carbon fiber material loaded with a trace amount of ruthenium provided in Example 4 of the present invention;
[0040] Figure 8 This is a HER performance diagram of a carbon fiber material loaded with a trace amount of ruthenium provided in Comparative Example 1 of the present invention;
[0041] Fig. 9 This is a HER performance diagram of the hollow carbon nanofiber material provided in Comparative Example 2 of the present invention;
[0042] Fig.10 This is a HER performance diagram of the hollow carbon nanofiber material provided in Comparative Example 3 of the present invention;
[0043] Fig.11 This is a HER performance diagram of the hollow carbon nanofiber material provided in Comparative Example 4 of the present invention;
[0044] Fig.12 This is the HER performance diagram of the hollow carbon nanofiber material provided in Comparative Example 5 of the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0046] In view of the fact that existing carbon nanofibers still have problems such as small specific surface area and lack of active sites, the present invention provides a hollow carbon fiber material loaded with trace ruthenium and a preparation method thereof. The hollow carbon fiber material has a special hollow structure, which can not only ensure that the carbon fiber material has good conductivity, but also fully expose the catalytic active centers, thereby promoting the mass transfer of the catalytic material and improving its catalytic performance, which is of great significance for the development of new energy catalysts.
[0047] The hollow carbon fiber material loaded with trace amounts of ruthenium and the preparation method thereof provided by the present invention are described in more detail below through specific examples and comparative examples.
[0048] Example 1
[0049] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0050] S1. Prepare shell spinning solution and core spinning solution:
[0051] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide dissolved with 100 mg of C4H6CoO4·4H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.6 wt %;
[0052] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0053] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 18 kV, the distance from the needle to the receiving tube is 16 cm, the rate ratio of the shell spinning solution to the core spinning solution is 2:1, and the total liquid supply rate is 8.0 mL / h;
[0054] S3, soaking the carbon fiber precursor in deionized water at 50° C. for 12 hours to obtain a hollow carbon fiber precursor;
[0055] S4. Dry the hollow carbon fiber precursor at 80°C for 12 hours, and pre-oxidize it at 250°C for 1.5 hours; then, in a nitrogen atmosphere, heat it to 800°C at a heating rate of 5°C / min and keep it for 2 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0056] According to the test, the hollow diameter is 400nm-500nm, the wall thickness is 90nm-100nm, and the specific surface area is 390m 2 / g.
[0057] Example 2
[0058] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0059] S1. Prepare shell spinning solution and core spinning solution:
[0060] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide containing 50 mg of C4H6CoO4·4H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.7 wt %;
[0061] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0062] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 18 kV, the distance from the needle to the receiving tube is 18 cm, the rate ratio of the shell spinning solution to the core spinning solution is 2.5:1, and the total liquid supply rate is 5.0 mL / h;
[0063] S3, soaking the carbon fiber precursor in deionized water at 55° C. for 10 hours to obtain a hollow carbon fiber precursor;
[0064] S4. Dry the hollow carbon fiber precursor at 90°C for 16 hours, and pre-oxidize it at 220°C for 3.5 hours; then, in a nitrogen atmosphere, heat it to 750°C at a heating rate of 4°C / min and keep it for 2.5 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0065] The test results show that the hollow diameter is 400nm-500nm, the wall thickness is 80nm-110nm, and the specific surface area is 384m 2 / g.
[0066] Example 3
[0067] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0068] S1. Prepare shell spinning solution and core spinning solution:
[0069] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide dissolved with 150 mg of C4H6CoO4·4H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.4 wt %;
[0070] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0071] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 16 kV, the distance from the needle to the receiving tube is 15 cm, the rate ratio of the shell spinning solution to the core spinning solution is 1.2:1, and the total liquid supply rate is 4.8 mL / h;
[0072] S3, soaking the carbon fiber precursor in deionized water at 25° C. for 36 hours to obtain a hollow carbon fiber precursor;
[0073] S4. Dry the hollow carbon fiber precursor at 60°C for 20 hours, and pre-oxidize it at 240°C for 3.5 hours; then, in a nitrogen atmosphere, heat it to 600°C at a heating rate of 2°C / min and keep it for 3 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0074] According to the test, the hollow diameter is 600nm-700nm, the wall thickness is 80nm-120nm, and the specific surface area is 380m 2 / g.
[0075] Example 4
[0076] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0077] S1. Prepare shell spinning solution and core spinning solution:
[0078] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 4.3 mL of dimethyl sulfoxide containing 100 mg of C4H6CoO4·4H2O and 10 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.6 wt %;
[0079] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0080] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 20 kV, the distance from the needle to the receiving tube is 20 cm, the rate ratio of the shell spinning solution to the core spinning solution is 3:1, and the total liquid supply rate is 12.0 mL / h;
[0081] S3, soaking the carbon fiber precursor in deionized water at 80° C. for 6 hours to obtain a hollow carbon fiber precursor;
[0082] S4. Dry the hollow carbon fiber precursor at 100°C for 5 hours, and pre-oxidize it at 260°C for 1 hour; then, in a nitrogen atmosphere, heat it to 800°C at a heating rate of 6°C / min and keep it for 1 hour to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0083] The test results show that the hollow diameter is 350nm-450nm, the wall thickness is 60nm-70nm, and the specific surface area is 386m2 / g.
[0084] Comparative Example 1
[0085] This comparative example provides a method for preparing a carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0086] S1. Prepare shell spinning solution:
[0087] 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide dissolved with 100 mg of C4H6CoO4·4H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.4 wt%;
[0088] S2, electrospinning the shell spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the electrospinning is 18 kV, the distance from the needle to the receiving tube is 16 cm, the rate ratio of the shell spinning solution to the core spinning solution is 2:1, and the total liquid supply rate is 8.0 mL / h;
[0089] S3. Dry the carbon fiber precursor at 80°C for 12 hours, and pre-oxidize it at 250°C for 1.5 hours; then, in a nitrogen atmosphere, heat it to 800°C at a heating rate of 5°C / min and keep it for 2 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0090] After testing, its diameter is 300nm~400nm and its specific surface area is 120m 2 / g.
[0091] Comparative Example 2
[0092] This comparative example provides a method for preparing a hollow carbon fiber material, which is basically the same as the preparation method in Example 1, except that when preparing the shell spinning solution, only C4H6CoO4·4H2O is added but RuCl3·xH2O is not added, and the remaining steps are the same as in Example 1.
[0093] After testing, the hollow diameter is 400nm~500nm, and the wall thickness is 80nm~90nm.
[0094] Comparative Example 3
[0095] This comparative example provides a method for preparing a hollow carbon fiber material, which is basically the same as the preparation method in Example 1, except that when preparing the shell spinning solution, only RuCl3·xH2O is added but C4H6CoO4·4H2O is not added, and the remaining steps are the same as in Example 1.
[0096] After testing, the hollow diameter is 500nm~600nm, and the wall thickness is 100nm~120nm.
[0097] Comparative Example 4
[0098] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0099] S1. Prepare shell spinning solution and core spinning solution:
[0100] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide dissolved with 100 mg of Fe(No3)3·9H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.6 wt%;
[0101] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0102] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 18 kV, the distance from the needle to the receiving tube is 16 cm, the rate ratio of the shell spinning solution to the core spinning solution is 2:1, and the total liquid supply rate is 8.0 mL / h;
[0103] S3, soaking the carbon fiber precursor in deionized water at 50° C. for 12 hours to obtain a hollow carbon fiber precursor;
[0104] S4. Dry the hollow carbon fiber precursor at 80°C for 12 hours, and pre-oxidize it at 250°C for 1.5 hours; then, in a nitrogen atmosphere, heat it to 800°C at a heating rate of 5°C / min and keep it for 2 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0105] After testing, the hollow diameter is 400nm~500nm, and the wall thickness is 90nm~100nm.
[0106] Comparative Example 5
[0107] This embodiment provides a method for preparing a hollow carbon fiber material loaded with a trace amount of ruthenium, comprising the following steps:
[0108] S1. Prepare shell spinning solution and core spinning solution:
[0109] Preparation of shell spinning solution: 0.6 g of polyacrylonitrile was dispersed in 3.59 mL of N,N-dimethylformamide dissolved with 100 mg of Ni(NO3)3·6H2O and 5 mg of RuCl3·xH2O, and stirred evenly to obtain a shell spinning solution with a polyacrylonitrile concentration of 14.6 wt %;
[0110] Preparation of the core spinning solution: 0.6 g of polyvinyl pyrrolidone was dispersed in 4.4 g of N, N-dimethylformamide, and stirred evenly to obtain a core spinning solution with a concentration of 12 wt %;
[0111] S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; wherein the loading voltage of the coaxial electrospinning is 18 kV, the distance from the needle to the receiving tube is 16 cm, the rate ratio of the shell spinning solution to the core spinning solution is 2:1, and the total liquid supply rate is 8.0 mL / h;
[0112] S3, soaking the carbon fiber precursor in deionized water at 50° C. for 12 hours to obtain a hollow carbon fiber precursor;
[0113] S4. Dry the hollow carbon fiber precursor at 80°C for 12 hours, and pre-oxidize it at 250°C for 1.5 hours; then, in a nitrogen atmosphere, heat it to 800°C at a heating rate of 5°C / min and keep it for 2 hours to obtain a hollow carbon fiber material loaded with trace ruthenium.
[0114] After testing, the hollow diameter is 400nm~500nm, and the wall thickness is 90nm~100nm.
[0115] Test Example 1
[0116] The hollow carbon fiber materials loaded with trace amounts of ruthenium obtained in Example 1 and Comparative Example 1 were characterized by SEM, and the results were as follows: Figures 2-3 shown.
[0117] from Figure 2 It can be seen that the carbon nanofiber material prepared by the method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium provided in the embodiment of the present invention has an obvious hollow structure; Figure 3 It can be seen that the carbon nanofiber material obtained in Comparative Example 1 presents a solid structure, which leads to a smaller specific surface area of the carbon nanofiber material and affects its electrocatalytic performance.
[0118] Test Example 2
[0119] The hollow carbon fiber materials loaded with trace amounts of ruthenium prepared in Examples 1 to 4 and Comparative Examples 1 to 5 were tested for electrocatalytic hydrogen evolution (HER) performance in a typical three-electrode system. The results are as follows: Figures 4 to 12 shown.
[0120] from Figure 4 It can be seen that the overpotential of the carbon nanofiber material prepared in Example 1 is 144 mV. Figure 8 to Figure 12 It can be seen that the overpotentials of the carbon nanofiber materials prepared in Comparative Examples 1, 2, 3, 4 and 5 are 242mV, 230mV, 446mV, 266mV and 365mV, respectively. This shows that Comparative Example 1 has a solid structure inside its material, resulting in a small specific surface area of the carbon nanofiber material, and the active sites are not fully exposed, thereby reducing its catalytic activity; while Comparative Examples 2 and 3 lack ruthenium active sites and cobalt active sites on their material surfaces, which seriously affects their hydrogen evolution performance. Comparative Examples 4 and 5 replace cobalt with iron and nickel, respectively, and the performance shows a significant attenuation, which further illustrates that the interaction between cobalt and ruthenium can make the carbon fiber material have good hydrogen evolution performance.
[0121] The morphology of the hollow carbon fiber materials prepared in Examples 2 to 4 is basically consistent with that in Example 1, and the HER test results thereof are also basically consistent with the test results of Example 1, which will not be repeated here.
[0122] In summary, as long as the selection of solvent in the shell spinning solution, the selection of solvent in the core spinning solution, the immersion time, the concentration ratio, the flow rate ratio, the pre-oxidation treatment conditions, the high-temperature carbonization treatment conditions and the electrospinning conditions are all within the preferred range of the present invention, the technical effects basically the same as those of Examples 1 to 4 can be achieved.
[0123] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium, characterized in that the steps include: S1, dissolving polyacrylonitrile in N,N-dimethylformamide or dimethyl sulfoxide containing a cobalt source and a ruthenium source to obtain a shell spinning solution, and dissolving polyvinyl pyrrolidone in N,N-dimethylformamide or dimethyl sulfoxide to obtain a core spinning solution; S2, coaxially electrospinning the shell spinning solution and the core spinning solution to obtain a carbon fiber precursor; S3, soaking the carbon fiber precursor in water to obtain a hollow carbon fiber precursor; S4. The hollow carbon fiber precursor is sequentially dried, pre-oxidized and carbonized at high temperature to obtain a hollow carbon fiber material loaded with a trace amount of ruthenium.
2. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The cobalt source is selected from cobalt nitrate hexahydrate or cobalt acetate tetrahydrate; The ruthenium source is ruthenium trichloride hydrate.
3. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The mass proportion of the ruthenium source in the shell spinning solution is 0.02% to 0.24%.
4. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The loading voltage of the coaxial electrospinning is 12kV to 26kV, the distance from the needle to the receiving tube is 15cm to 20cm, the flow rate ratio of the outer shell spinning solution to the inner core spinning solution is 1.2 to 3:1, and the total liquid supply rate is 4.8mL / h to 12.0mL / h.
5. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The soaking is soaking in water with a temperature of 25° C. to 80° C. for 6 h to 36 h.
6. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The drying is performed at a temperature of 60°C to 100°C for 5h to 20h; and / or The pre-oxidation is carried out at a temperature of 220° C. to 260° C. for 1 h to 4 h.
7. The method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 1, characterized in that: The high temperature carbonization is carried out in an inert atmosphere or a nitrogen atmosphere, heating the temperature to 600° C. to 800° C. at a heating rate of 2° C. / min to 6° C. / min and maintaining the temperature for 1 hour to 3 hours.
8. A hollow carbon fiber material loaded with trace amounts of ruthenium, characterized in that: The hollow carbon fiber material is prepared according to the method for preparing a hollow carbon fiber material loaded with trace amounts of ruthenium according to any one of claims 1 to 7.
9. The hollow carbon fiber material loaded with trace amounts of ruthenium according to claim 8, characterized in that: The hollow carbon fiber material has a hollow diameter of 350nm to 700nm, a wall thickness of 60nm to 120nm, and a specific surface area of 380m 2 / g~390m 2 / g.
10. Use of the hollow carbon fiber material loaded with trace amounts of ruthenium as claimed in claim 8 or 9 in the field of electrocatalytic materials.
Citation Information
Cited By
Far infrared fiber thermal fabric and preparation method and application thereof
CN119711040A
Biomass-derived hollow thin-wall two-stage porous carbon fiber material, preparation method thereof and supercapacitor
CN120158843A
Biomass derived hemp rope type honeycomb briquette-shaped hollow porous carbon fiber material as well as preparation method and application thereof
CN120311353A